Pseudoboehmite, its production method and uses

The integration of organic acid sources and cation exchange resins in pseudoboehmite production effectively reduces sodium content and wastewater, making it suitable for hydrogenation catalysts by eliminating washing steps and enhancing process efficiency.

JP7555930B2Active Publication Date: 2024-09-25CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021537874
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-28
Filing Date
2019-12-27
Publication Date
2024-09-25
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

Existing methods for producing pseudoboehmite result in high sodium content and require extensive washing, leading to wastewater generation and increased environmental impact.

Method used

A method involving the use of organic acid sources and cation exchange resins to capture and encapsulate metal ions, particularly sodium, during pseudoboehmite production, eliminating the need for washing steps and reducing sodium content.

Benefits of technology

Produces pseudoboehmite with low sodium content, suitable for hydrogenation catalysts, while minimizing wastewater and streamlining the manufacturing process through closed-loop recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555930000026
    Figure 0007555930000026
  • Figure 0007555930000001
    Figure 0007555930000001
  • Figure 0007555930000002
    Figure 0007555930000002
Patent Text Reader

Abstract

The present invention relates to pseudo-boehmite having a dry basis content of 55 to 85% by weight and containing phosphate ester groups, wherein the pseudo-boehmite has a sodium oxide content of 0.5% by weight or less and a phosphorus content (as calculated as phosphorus pentoxide) of 1.2 to 5.7% by weight, based on 100% by weight of the total weight of the pseudo-boehmite. The pseudo-boehmite is characterized by its extremely low sodium content. The present invention further relates to a method for producing pseudo-boehmite and its use in the production of alumina, hydrogenation catalysts, and the hydrogenation of oil products.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to pseudo-boehmite. The present invention also relates to a method for producing pseudo-boehmite, and the use of pseudo-boehmite in the preparation of alumina, the preparation of hydrogenation catalyst, and the hydrogenation of oil products. [Background technology]

[0002] Pseudo-boehmite, also known as alumina monohydrate and pseudoboehmite, can be a white colloid (wet product) or powder (dry product) with incomplete crystalline water molecules and spatial network structure, characterized by high crystal phase purity, good deflocculation performance, strong cohesiveness, high specific surface area, large pore volume, etc. Pseudo-boehmite is dehydrated at high temperature to prepare activated alumina. Activated alumina has excellent specific surface area and pore structure, especially gamma-Al2O3 has large specific surface area, adjustable pore structure, and excellent thermal stability, so activated alumina is widely used in the petrochemical industry and chemical fertilizer industry as catalyst carrier, desiccant, adsorbent, etc.

[0003] The manufacturing methods of pseudo-boehmite in industry mainly include the organic aluminum alkoxide method and inorganic neutralization treatment with different raw materials. Among these inorganic neutralization treatments, three manufacturing processes are commonly present in the industrial field: aluminum chloride treatment, aluminum sulfate treatment, and carbonization treatment. (1) Aluminum chloride treatment: neutralization reaction of aluminum salt and base, such as AlCl3+3NH4OH→Al(OH)3+3NH4Cl; (2) Aluminum sulfate treatment: metathesis reaction of aluminum salt and aluminate, such as Al2(SO4)3+6NaAlO2+12H2O→8Al(OH)3+3Na2SO4; (3) Carbonization treatment: neutralization reaction of aluminate and acid, such as 2NaAlO2+CO2+3H2O→2Al(OH)3+Na2CO3. In the above three processes, aluminum hydroxide is produced by neutralization method, and then sodium impurities are removed by washing treatment, which consumes a lot of washing water and generates a large amount of wastewater.

[0004] CN201610674763.3 discloses low-impurity pseudo-boehmite, its manufacturing method and manufacturing apparatus. The weight percent content of metal ion impurities in the low-impurity pseudo-boehmite is ≦0.1%. The method includes forming raw pseudo-boehmite into a slurry, acidifying the slurry to obtain acidified raw pseudo-boehmite, aging at a set time and temperature to obtain aged raw pseudo-boehmite, passing the aged pseudo-boehmite through a cation exchange resin at a set flow rate to remove metal ion impurities in the aged pseudo-boehmite, and drying the raw pseudo-boehmite from which the metal ion impurities have been removed to obtain low-impurity pseudo-boehmite, where the weight percent content of metal ion impurities is ≦0.1%. The apparatus includes a first container, a second container, a third container, and a dryer.

[0005] CN201110103785.1 discloses a method for producing ultrafine aluminum hydroxide and ultrafine alumina using pulverized fuel ash in a circulating fluidized bed as raw material. The method includes: a) grinding the pulverized fuel ash, performing wet magnetic separation on the ground pulverized fuel ash to remove iron, and then reacting the resulting product with hydrochloric acid to obtain a hydrochloric acid immersion liquid; b) passing the hydrochloric acid immersion liquid through a macroporous cationic resin column for adsorption, saturating the adsorption by the resin, and then eluting the resin with an eluent to obtain an elution liquid containing aluminum chloride and iron chloride; c) dissolving the elution liquid in an alkali for iron removal to obtain a sodium metaaluminate solution; d) adding a dispersant to the sodium metaaluminate solution and mixing uniformly to obtain a dispersion; and e) introducing carbon dioxide into the dispersion and performing separation to obtain ultrafine aluminum hydroxide. The ultrafine aluminum hydroxide is calcined at different temperatures to obtain gamma-alumina and alpha-alumina, respectively. Summary of the Invention

[0006] Through industrial research, the present inventors have found pseudo-boehmite and a method for producing pseudo-boehmite. Without being bound by any theory, the present inventors have concluded that the organic acid source, which is one of the reaction raw materials, can simultaneously exert the function of transferring metal ions and the function of protecting the adsorbent resin in the method for producing pseudo-boehmite of the present invention. This is the first finding in the technical field. Specifically, the organic acid source captures or replaces metal ions, especially sodium ions, contained or encapsulated in the pseudo-boehmite (which exists in a colloidal state) produced in the production process, and then transfers the metal ions to the cation exchange resin as another reaction raw material to be adsorbed and fixed by the cation exchange resin, thereby not only effectively promoting the separation of the pseudo-boehmite from the metal ions, but also forming protective micelles around the cation exchange resin to separate the cation exchange resin from the produced pseudo-boehmite, thereby effectively preventing the cation exchange resin from being embedded in the pseudo-boehmite to reduce the metal ion adsorption capacity. Therefore, according to the method for producing pseudo-boehmite of the present invention, pseudo-boehmite with a very low content of metal ions, especially sodium ions, can be obtained without introducing a washing process. The present invention was completed based on this finding.

[0007] Specifically, the present invention relates to the following aspects: 1. Pseudo-boehmite having a dry basis content of 55 to 85% by weight (preferably 65 to 75% by weight) relative to 100% by weight of the total weight of the pseudo-boehmite, containing a phosphate ester group, a sodium oxide content of 0.5% by weight or less (preferably 0.05% by weight or less, more preferably 0.03% by weight or less), and a phosphorus content (calculated as phosphorus pentoxide) of 1.2 to 5.7% by weight (preferably 1.4 to 4.2% by weight).

[0008] 2. Pseudo-boehmite according to the above-mentioned or below-mentioned embodiment, wherein the phosphate ester group is derived from a compound represented by the following structural formula (I):

[0009] [ka]

[0010] In structural formula (I), each A is the same or different and independently represents a hydrogen ion, an ammonium ion (NH + ), a metal ion (e.g. an alkali metal ion or an alkaline earth metal ion, especially a sodium ion) and a compound represented by the formula

[0011] [ka]

[0012] (preferably, at least one A is a hydrogen ion, more preferably, both of the two A's are hydrogen ions); R0 is a hydrogen atom, an optionally substituted C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl (preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 linear or branched alkyl, more preferably C9 linear or branched alkyl); The n groups R1 are identical or different and independently represent 1-6 Selected from linear or branched alkylene (preferably C 2-4 linear or branched alkylene, more preferably ethylene); n is a number in the range of 0 to 200 (preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20).

[0013] 3. Pseudo-boehmite according to any one of the preceding and following embodiments, having a gibbsite content of <3.0% by weight, based on 100% by weight of the total weight of the pseudo-boehmite.

[0014] 4. Pseudo-boehmite according to the above-mentioned or below-mentioned embodiment, further containing at least one auxiliary agent selected from Si, B and Ti, and the content of the at least one auxiliary agent (in terms of oxide) is 1 to 8 weight % (preferably 2 to 6 weight %) relative to 100 weight % of the total weight of the pseudo-boehmite.

[0015] 5. A method for producing pseudo-boehmite, comprising the steps of: An alkaline aluminum source (e.g., an aluminate, in particular a metaaluminate, more in particular sodium metalluminate), a cation exchange resin (in particular a strongly acidic cation exchange resin, preferably selected from at least one of a strongly acidic styrene-based cation exchange resin and a sulfonated styrene-based gel-type strongly acidic cation exchange resin, more preferably selected from at least one of a D001 macroporous strongly acidic styrene-based cation exchange resin, a D002 macroporous strongly acidic styrene-based cation exchange resin and a D61 macroporous strongly acidic styrene-based cation exchange resin, even more preferably selected from at least one of a D001 macroporous strongly acidic styrene-based cation exchange resin and a D61 macroporous strongly acidic styrene-based cation exchange resin) and an organic acid source (in particular a carboxylic acid, a salt of a carboxylic acid, an organic ester of a carboxylic acid, an organic ester / salt of a carboxylic acid, a phosphonic acid, a salt of a phosphonic acid, an organic ester of a phosphonic acid, an organic ester / salt of a phosphonic acid, a phosphonic acid salt, an organic ester of a phosphonic acid ... esters, organic esters / salts of physphingic acid, organic esters of carbonic acid, organic esters of carbonic acid, organic esters of phosphoric acid, organic esters of phosphoric acid, organic esters of phosphorous ... 15 -Alkyl ether phosphate ester, mono-C9-C 15 -Alkyl phosphate ester, di-C9-C 15-Alkyl phosphate esters, and di-C9-C 15- and at least one of the alkyl ether phosphate esters, more preferably mono-C9-C 15 a compound represented by the following structural formula (I) in the presence of water (particularly deionized water) to obtain a mixed solution, the organic acid source having an acidity coefficient pKa of 0 to 8 (preferably 2 to 8, more preferably 3 to 6), and separating the mixed solution to obtain pseudo-boehmite.

[0016] [ka]

[0017] In structural formula (I), each A is the same or different and independently represents a hydrogen ion, an ammonium ion (NH + ), a metal ion (e.g. an alkali metal ion or an alkaline earth metal ion, especially a sodium ion) and a compound represented by the formula

[0018] [ka]

[0019] (preferably, at least one A is a hydrogen ion, more preferably, both of the two A's are hydrogen ions); R0 is a hydrogen atom, an optionally substituted C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl (preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 linear or branched alkyl, more preferably C9 linear or branched alkyl); The n groups R1 are identical or different and independently represent 1-6 Linear or branched alkylene (preferably C 2-4linear or branched alkylene, more preferably ethylene); n is a number in the range of 0 to 200 (preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20).

[0020] 6. The mass ratio (in terms of alumina) of the alkaline aluminum source to the organic acid source is 1.2:1 to 24:1 (preferably 5:1 to 20:1), and / or the number of carbon atoms in the organic acid source is 30 or less (preferably 20 or less, more preferably 15 or less), and / or the HLB value of the organic acid source is 3 to 8 (preferably 3 to 6), and / or the particle size of the cation exchange resin is 20 to 150 mesh (preferably 40 to 80 mesh), and / or the organic system is represented by the structural formula:

[0021] [ka]

[0022] It refers to a group represented by R a is a hydrogen atom or an optionally substituted C 1-30 Hydrocarbyl (preferably C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl, preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 linear or branched alkyl), The n groups R1 are identical or different and independently represent 1-6 Linear or branched alkylene (preferably C 2-4 linear or branched alkylene, more preferably ethylene); The production method according to the above-mentioned or below-mentioned embodiment, wherein n is a number in the range of 0 to 200 (preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20), and / or the salt is selected from at least one of an alkali metal salt and an alkaline earth metal salt, preferably an alkali metal salt (e.g., a sodium salt).

[0023] 7. A method of manufacture according to any of the preceding or following embodiments, comprising the steps of: (1) reacting the alkaline aluminum source, the organic acid source, and a part of the total amount of the cation exchange resin in the presence of water to obtain a first mixed liquid; (2) After aging the first mixture, another part of the total amount of the cation exchange resin is added to obtain a second mixture; (3) separating the cation exchange resin from the second mixture to obtain a slurry; and (4) If necessary, the slurry is filtered and then dried to obtain the pseudo-boehmite.

[0024] 8. A production method according to the above-mentioned or below-mentioned embodiment, wherein the alkaline aluminum source is sodium metalluminate having a caustic ratio of 1.15 to 1.35 (preferably 1.20 to 1.30), and / or wherein in step (1), the reaction temperature is 45°C to 80°C (preferably 50°C to 75°C) and the pH value of the reaction system is 7.5 to 10 (preferably 8.0 to 9.5), and / or wherein in step (2), the aging temperature is 50 to 100°C (preferably 60 to 90°C) and the aging time is 0.5 to 3 hours (preferably 1 to 2 hours), and / or wherein in step (4), the drying temperature is 100 to 150°C and the drying time is 6 to 10 hours.

[0025] 9. A method of manufacture according to any of the preceding or following embodiments, comprising the steps of: (1) reacting the aqueous solution of the alkaline aluminum source, the aqueous solution of the organic acid source, and the suspension of the portion of the cation exchange resin (optionally in the presence of water, preferably by adding the aqueous solution of the alkaline aluminum source, the aqueous solution of the organic acid source, and the suspension of the cation exchange resin to water) to obtain the first mixed solution; (2) aging the first mixture, and then adding the suspension of the other part of the cation exchange resin to obtain the second mixture; (3) separating the cation exchange resin from the second mixture to obtain a slurry; (4) If necessary, the slurry is filtered and then dried to obtain the pseudo-boehmite.

[0026] 10. In step (1), the amount of water is 5 to 20% by volume (preferably 5 to 15% by volume) of the total volume of the reaction system (e.g., reactor), and / or in step (1), the concentration of the sodium metallominate solution is 20 to 100 g Al2O3 / L (preferably 30 to 70 g Al2O3 / L) calculated as oxide, and / or in step (1), the flow rate at which the sodium metallominate solution is added to the reaction system is 20 mL / min to 60 mL / min (preferably 30 mL / min to 50 mL / min), and / or in step (1), the concentration of the aqueous solution of the organic acid source is 0.05 to 0.5 g / mL, and / or in step (1), the flow rate at which the aqueous solution of the organic acid source is added to the reaction system is 5 mL / min to 10 mL / min, and / or in step (1), the solid content of the suspension of the cation exchange resin is 30 to 80% by weight. and / or in step (1), the flow rate of the suspension of the cation exchange resin added to the reaction system or the amount of the suspension of the cation exchange resin used is such that the pH value of the reaction system is maintained at 7.5 to 10 (preferably 8.0 to 9.5), and / or in step (2), the amount of the suspension of the cation exchange resin used is such that the pH value of the first mixed solution reaches 6.0 to 7.5 (preferably 6.5 to 7.0).

[0027] 11. A porous membrane having a phosphorus content of 0.3 to 5.0% by weight (preferably 0.5 to 4.5% by weight) (calculated as elemental phosphorus), a pore volume of 0.7 to 1.2 mL / g (preferably 0.8 to 1.1 mL / g, and more preferably 0.9 to 1.1 mL / g), and an acid amount per unit surface area of ​​0.001 to 0.002 mmol / m 2 (Preferably 0.0015 to 0.002 mmol / m 2 ) and alumina having a hydraulic hardness of 3 to 10 N / particle (preferably 5 to 10 N / particle).

[0028] 12. A method for producing alumina, comprising the steps of: Pseudo-boehmite is produced by the production method according to the embodiment described above or below, and the pseudo-boehmite is calcined to obtain alumina.

[0029] 13. A catalyst (particularly a hydrogenation catalyst) comprising a catalytically active component (particularly an active metal component, for example selected from at least one of the metals of Group VIB and Group VIII of the Periodic Table of the Elements, in particular selected from at least one of Mo, W, Ni and Co) and a support, wherein the support comprises an alumina according to any of the embodiments described hereinbefore or hereinafter, or an alumina prepared by a process according to any of the embodiments described hereinbefore or hereinafter.

[0030] 14. A method for producing a catalyst (particularly a hydrogenation catalyst), comprising the steps of: Producing pseudo-boehmite according to the production method according to any one of the above-mentioned or below-mentioned embodiments, The pseudo-boehmite is molded and optionally dried and calcined to obtain a carrier; The catalyst is obtained by supporting a catalytically active component (particularly an active metal component, for example at least one selected from Group VIB metals and Group VIII metals of the Periodic Table of Elements, particularly at least one selected from Mo, W, Ni and Co) on the support.

[0031] 15. A hydrogenation process comprising the step of hydrogenating an oil product (e.g., selected from at least one of diesel, vacuum gas oil, heavy oil and residual oil) in the presence of a hydrogenation catalyst according to any of the preceding or following embodiments, or produced by a process according to any of the preceding or following embodiments, under hydrogenation reaction conditions.

[0032] 16. The hydrogenation reaction conditions are: reaction pressure 5-20 MPaG, reaction temperature 350-500°C, and liquid hourly space velocity 0.1-2.0 h -1 and the hydrogen / oil volume ratio is 100 to 1000. Effect of the Invention

[0033] Compared with the prior art, the present invention can achieve at least one of the following advantages: (1) The pseudo-boehmite of the present invention has an extremely low sodium content even without washing treatment in the production process, and is particularly suitable as a support material for a hydrogenation catalyst.

[0034] (2) The pseudo-boehmite of the present invention has a low gibbsite content and is particularly suitable as a support material for a hydrogenation catalyst.

[0035] (3) According to the manufacturing process of pseudo-boehmite, the washing process in the conventional manufacturing method can be omitted under a suitable environment, the amount of wastewater can be greatly reduced, the manufacturing process flow can be shortened, the pseudo-boehmite with a low sodium content can be guaranteed to be obtained, and the surface acidity of the manufactured alumina product can be improved. Therefore, the filtered slurry can be recycled, thereby realizing the closed circulation of the manufacturing process and not discharging pollutants.

[0036] (4) According to the process for producing pseudo-boehmite of the present invention, the sodium content in the produced pseudo-boehmite can be further reduced by gradually adding a cation exchange resin in the synthesis reaction process, and a pseudo-boehmite product having a lower sodium content can be obtained.

[0037] (5) The alumina of the present invention has a large pore volume, a small impurity content, a large unit surface acid content, and high hydraulic properties, and is therefore particularly suitable for producing a hydrogenation catalyst support having excellent wear resistance. [Brief description of the drawings]

[0038] [Figure 1] 1 is an XRD spectrum of the pseudo-boehmite produced in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] Reference will now be made in detail to the present embodiments of the invention, with an understanding that the scope of the invention is not limited by the embodiments, but is defined by the appended claims.

[0040] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference in their entirety.Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this invention belongs.In case of discrepancy, the present specification, including definitions, shall prevail.

[0041] When this specification derives from materials, substances, processes, steps, apparatus, elements and the like by expressions such as "known to those skilled in the art," "prior art," or similar terms, it is intended that the subject matter so derived includes those conventionally used in the art at the time of the filing of this application, but also those that may no longer be in common use but which will become known in the art as suitable for similar purposes.

[0042] In the context of this specification, the term "substantially" means tolerating the presence of deviations that would be acceptable or considered reasonable by one of ordinary skill in the art, for example, deviations within ±10%, within ±5%, within ±1%, within ±0.5%, or within ±0.1%.

[0043] In the present context, the term "ester" includes monoesters and polyesters, depending on the type of acid.

[0044] In the present context, the expression "ester / salt" refers to a mixture of esters and salts.

[0045] In the context of this specification, the acidity coefficient pKa is determined in the non-salt form of the corresponding substance (especially the organic acid source), where the so-called non-salt form refers to the one obtained by replacing all metal or ammonium ions contained in the substance by hydrogen ions.

[0046] In the context of this specification, the phase structure and gibbsite content of pseudo-boehmite are characterized by XRD spectrum, where the XRD measurement conditions are as follows: X-ray diffraction analyzer model D / max2500 manufactured by Rigaku Corporation, Japan, operating voltage 40 kV, operating current 80 mA, scan range 10(°)-70(°), step difference 0.01(°), and scan speed 1(°)·min -1 It is.

[0047] In the context of this specification, hydraulicity refers to the property of reacting with water and gradually solidifying and hardening in a wet medium. For this purpose, alumina hydraulicity is defined as the strength of N / particle of a sample obtained by contacting alumina with sprayed water droplets to make it agglomerate, solidify into particles, and dry at 200°C for 3 hours. The specific measurement method includes the following: (1) Weigh 100g of the produced alumina sample, add 50g of water, spray small water droplets with a 100um nozzle in the atomizer, adsorb the small water droplets with alumina, gradually agglomerate, further crystallize, and solidify into pellets. Due to the different microscopic properties of alumina, the solidification and hardening times are different, and the hydraulicity of alumina in a short time is better than that in a long time. (2) Dry the solidified alumina pellets at 200 °C for 3 hours, screen the alumina pellets of 1.0-1.5 mm, and use an intelligence strength tester to test the pressure of 20 samples, the unit is N, and the unit of average strength is N / particle.

[0048] In the context of this specification, the method for determining the dry basis content includes weighing 10 g of pseudo-boehmite raw material and placing it into a muffle furnace for high temperature calcination: where the calcination conditions include 600°C and constant temperature for 3 hours, taking out a sample, and weighing the calcined sample. Divide the weight of the calcined sample by 10 g and then multiply by 100% to obtain the dry basis content of the sample.

[0049] In the present context, the pore volume and specific surface area of ​​alumina are analyzed by low-temperature nitrogen adsorption.

[0050] In the context of this specification, so-called numbers include integers and decimals.

[0051] In the context of this specification, the expression "optionally substituted" includes any of the following: halogen, hydroxy, mercapto, amino, aminocarbonyl, nitro, oxo, thio, cyano, C 1-6 Linear or branched (halo)alkane (oxy, thio, amino, carbonyl) groups, C 2-6 Linear or branched (halo)alkene (oxy, thio, amino, carbonyl) groups, C 2-6 Linear or branched (halo)alkyne (oxy, thio, amino, carbonyl) groups, C 3-20 Cycloalkyl, C 3-20 Cycloalkane (oxy, thio, amino) groups, C 3-20 Cycloalkyl C 1-6 Linear or branched (halo)alkane (oxy, thio, amino, carbonyl) groups, C 3-20 Cycloalkyl C 2-6 Linear or branched (halo)alkene (oxy, thio, amino, carbonyl) groups, C 3-20 Cycloalkyl C 2-6 Linear or branched (halo)alkyne (oxy, thio, amino, carbonyl) groups, C 3-20 Cycloalkenyl, C 3-20 Cycloalkyne (oxy, thio, amino) groups, C 3-20 Cycloalkenyl C 1-6 Linear or branched (halo)alkane (oxy, thio, amino, carbonyl) groups, C 3-20 Cycloalkenyl C 2-6 Linear or branched (halo)alkene (oxy, thio, amino, carbonyl) groups, C 3-20 Cycloalkenyl C 2-6 Linear or branched (halo)alkyne (oxy, thio, amino, carbonyl) groups, C 6-20 Aryl, C 6-20 Arene (oxy, thio, amino) groups, C 6-20 Aryl C1 -6 Linear or branched (halo)alkane (oxy, thio, amino, carbonyl) groups, C 6-20 Aryl C 2-6Linear or branched (halo)alkene (oxy, thio, amino, carbonyl) groups, C 6-20 Aryl C 2-6 Linear or branched (halo)alkyne (oxy, thio, amino, carbonyl) groups, C 4-20 Heteroaryl, C 4-20 Heteroarene (oxy, thio, amino) groups, C 4-20 Heteroaryl C 1-6 Linear or branched (halo)alkane (oxy, thio, amino, carbonyl) groups, C 4-20 Heteroaryl C 2-6 Linear or branched (halo)alkene (oxy, thio, amino, carbonyl) groups, C 4-20 Heteroaryl C 2-6 Linear or branched (halo)alkyne (oxy, thio, amino, carbonyl) groups, C 2-20 Heterocyclyl, C 2-20 Heterocyclic (oxy, thio, amino) groups, C 2-20 Heterocyclyl C 1-6 Linear or branched (halo)alkane (oxy, thio, amino, carbonyl) groups, C 2-20 Heterocyclyl C 2-6 Linear or branched (halo)alkene (oxy, thio, amino, carbonyl) groups and C 2-20 Heterocyclyl C 2-6 It represents that the compound is optionally substituted with one or more (e.g., 1 to 5, 1 to 4, 1 to 3, 1 to 2, or 1) substituents selected from linear or branched (halo)alkyne (oxy, thio, amino, carbonyl) groups. When a plurality of these substituents are present, two adjacent substituents (e.g., the molecular chain ends of two substituents) may be bonded to each other to form a divalent substituent structure. For example, two adjacent C 1-6 Linear or branched alkyl groups may be linked together to form the corresponding alkylene structure. Alternatively, two adjacent C 1-6 Linear or branched alkoxy groups can, for example, form related alkylenedioxy group structures, with two adjacent C 1-6 Linear or branched alkylamino groups can, for example, form related alkylenediamino structures, with two adjacent C 1-5Linear or branched alkylthio groups can, for example, form related alkylenedithio structures, etc. Preferred substituents include, for example, halogen or C 1-6 Here, the expression "(halo)alkane(oxy, thio, amino, carbonyl) group" means alkyl, haloalkyl, alkyloxy, alkylthio, alkylamino, alkylcarbonyl, haloalkyloxy, haloalkylthio, haloalkylamino, or haloalkylcarbonyl, and the expression "(halo)alkene(oxy, thio, amino, carbonyl) group" means alkenyl, haloalkenyl, alkenyloxy, alkenylthio, alkenylamino, alkenylcarbonyl, haloalkene, The term "(halo)alkyne (oxy, thio, amino, carbonyl) group" means alkynyl, haloalkynyl, alkynyloxy, alkynylthio, alkynylamino, alkynylcarbonyl, haloalkynyloxy, haloalkynylthio, haloalkynylamino, or haloalkynylcarbonyl, and the term "(oxy, thio, amino) group" means oxy, thio, or amino. Here, the term "halo" includes monohalo, dihalo, trihalo, or perhalo, etc.

[0052] Unless expressly indicated, all percentages, parts, ratios, etc. referred to herein are by weight and pressures are gauge pressures.

[0053] In the context of this specification, any two or more embodiments of the present invention can be combined in any combination, and the resulting technical solutions are part of the original disclosure of this specification and within the scope of the present invention.

[0054] According to one embodiment of the present invention, the present invention relates to pseudo-boehmite, wherein the pseudo-boehmite has a dry base content of 55-85% by weight, preferably 65-75% by weight, based on 100% by weight of the total weight of the pseudo-boehmite.

[0055] According to one embodiment of the present invention, the pseudo-boehmite contains a phosphate ester group. For this purpose, the presence of the phosphate ester group can be easily identified from the pseudo-boehmite by a person skilled in the art using analytical methods such as infrared absorption spectroscopy and mass spectroscopy. Specifically, for example, in an infrared absorption spectrum, the phosphate ester group is usually shown as a characteristic peak of groups such as P=O, PO, and O=P-OH, and more specifically, for example, in the infrared absorption spectrum of the phosphate ester group, the characteristic peaks of the P=O group and the PO group are usually shown at 900 to 1300 cm -1 The characteristic peak of the O=P-OH group is usually located at 2200-2800 cm -1 Located in.

[0056] According to one embodiment of the present invention, the phosphorus content of the pseudo-boehmite (calculated as phosphorus pentoxide) is generally 1.2 to 5.7% by weight, preferably 1.4 to 4.2% by weight, relative to 100% by weight of the total weight of the pseudo-boehmite.

[0057] According to one embodiment of the present invention, the phosphate ester group is from a compound represented by the following structural formula (I):

[0058] [ka]

[0059] According to one embodiment of the present invention, in structural formula (I), each A is the same or different from each other, and each A is independently a hydrogen ion, an ammonium ion (NH + ), a metal ion (e.g., an alkali metal ion or an alkaline earth metal ion, especially a sodium ion) and the structural formula

[0060] [ka]

[0061] Preferably, at least one A is a hydrogen ion, more preferably both A are hydrogen ions. R0 is a hydrogen atom, an optionally substituted C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl, preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 A linear or branched alkyl, more preferably a C9 linear or branched alkyl. In addition, the n groups R1 are the same or different from each other and are each independently selected from the group consisting of C 1-6 Selected from linear or branched alkylene, preferably C 2-4 It is a straight-chain or branched alkylene, more preferably ethylene. n represents the average degree of polymerization of the polyether group, and is generally a number in the range of 0 to 200, preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20.

[0062] According to one embodiment of the present invention, the sodium oxide content of the pseudo-boehmite is 0.5% by weight or less, preferably 0.05% by weight or less, and more preferably 0.03% by weight or less, based on 100% by weight of the total weight of the pseudo-boehmite.

[0063] According to one embodiment of the present invention, the gibbsite content of the pseudo-boehmite is <3.0 wt. % relative to 100 wt. % of the total weight of the pseudo-boehmite.

[0064] According to one embodiment of the present invention, the pseudo-boehmite further contains at least one auxiliary selected from Si, B, and Ti, where the content (in terms of oxide) of the at least one auxiliary is 1 to 8% by weight, preferably 2 to 6% by weight, based on 100% by weight of the total weight of the pseudo-boehmite.

[0065] According to one embodiment of the present invention, pseudo-boehmite can be produced by the production method of the present invention as described below. Here, the production method of pseudo-boehmite includes at least a contact step and a separation step.

[0066] According to one embodiment of the present invention, in the contacting step, an alkaline aluminum source, a cation exchange resin, and an organic acid source are contacted in the presence of water to obtain a mixed liquid.

[0067] According to one embodiment of the present invention, the alkaline aluminum source in the contact step may be any alkaline aluminum source conventionally used in the production of pseudo-boehmite in the above technical field, specifically, for example, an aluminate, particularly a metaaluminate, more specifically, sodium metalluminate, wherein the sodium metalluminate has a caustic ratio of preferably 1.15 to 1.35, more preferably 1.20 to 1.30.

[0068] According to one embodiment of the present invention, in the contact step, the cation exchange resin may be any cation exchange resin capable of adsorbing metal ions, particularly sodium ions, in an ion exchange manner, more specifically, may be a strongly acidic cation exchange resin. Here, the strongly acidic cation exchange resin is more preferably selected from at least one of macroporous strongly acidic styrene-based cation exchange resin and sulfonated styrene-based gel-type strongly acidic cation exchange resin, more preferably selected from at least one of D001 macroporous strongly acidic styrene-based cation exchange resin, D002 macroporous strongly acidic styrene-based cation exchange resin and D61 macroporous strongly acidic styrene-based cation exchange resin, and even more preferably selected from at least one of D001 macroporous strongly acidic styrene-based cation exchange resin and D61 macroporous strongly acidic styrene-based cation exchange resin.

[0069] According to one embodiment of the present invention, in the contact step, the particle size of the cation exchange resin is generally 20-150 mesh, preferably 40-80 mesh.

[0070] According to one embodiment of the present invention, in the contacting step, the so-called organic acid source refers to an acid or acid derivative containing an organic group in the molecular structure. Preferably, the organic group is represented by the structural formula

[0071] [ka]

[0072] In the polyether group, R a is a hydrogen atom or an optionally substituted C 1-30 Hydrocarbyl, preferably C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl, preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 In addition, the n groups R1 are the same or different and each independently represent one of the following: 1-6 Selected from linear or branched alkylene, preferably C 2-4 It is a straight-chain or branched alkylene, more preferably ethylene. n represents the average degree of polymerization of the polyether group, and is generally a number in the range of 0 to 200, preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20. In order to facilitate the production process of the present invention, the number of carbon atoms (meaning the total number of carbon atoms contained in the entire molecular structure) of the organic acid source is generally 30 or less, preferably 20 or less, more preferably 15 or less.

[0073] According to one embodiment of the present invention, in order to achieve the intended function of the organic acid source, it is desirable that the pKa of the organic acid source is higher than the pKa of the cation exchange resin and lower than the pKa of the alkaline aluminum source. Specifically, for example, the acidity coefficient pKa of the organic acid source is generally 0 to 8, preferably 2 to 8, more preferably 3 to 6.

[0074] According to one embodiment of the present invention, the organic acid source may be, more specifically, for example, a carboxylic acid, a salt of a carboxylic acid, an organic ester of a carboxylic acid, an organic ester / salt of a carboxylic acid, a phosphonic acid, a salt of a phosphonic acid, an organic ester of a phosphonic acid, an organic ester / salt of a phosphonic acid, physphinic acid, a salt of a physphinic acid, an organic ester of a physphinic acid, an organic ester / salt of a physphinic acid, an organic ester of a carbonic acid, an organic ester / salt of a carbonic acid, an organic ester of a phosphoric acid, an organic ester / salt of a phosphoric acid, an organic ester of a phosphorous acid, an organic ester of a phosphorous acid, an organic ester of a phosphorous acid. The organic ester is selected from at least one of organic esters of carbonic acid, organic esters of carbonic acid, organic esters of phosphoric acid, organic esters of phosphoric acid, organic esters of phosphorous acid, and organic esters of phosphorous acid, more preferably from at least one of organic esters of phosphoric acid and organic esters of phosphoric acid, and in particular from organic esters of phosphoric acid. Preferably, the organic ester is represented by the structural formula:

[0075] [ka]

[0076] In the polyether group, R a is a hydrogen atom or an optionally substituted C 1-30 Hydrocarbyl, preferably C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl, preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 In addition, the n groups R1 are the same or different and each independently represent one of the following: 1-6 Selected from linear or branched alkylene, preferably C 2-4It is a straight-chain or branched alkylene, more preferably ethylene. n represents the average degree of polymerization of the polyether group and is generally a number in the range of 0 to 200, preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20.

[0077] According to one embodiment of the present invention, the organic ester of phosphoric acid may be an organic monoester of phosphoric acid or an organic diester of phosphoric acid, more particularly selected from at least one of monoalkyl ether phosphate ester, dialkyl ether phosphate ester, monoalkyl phosphate ester and dialkyl phosphate ester, and more particularly selected from mono-C9-C 15 -Alkyl ether phosphate ester, mono-C9-C 15 -Alkyl phosphate ester, di-C9-C 15 -Alkyl phosphate esters and di-C9-C 15 -alkyl ether phosphate esters, more preferably mono-C9-C 15 -alkyl ether phosphate ester, more preferably mono-C9-alkyl ether phosphate ester.

[0078] According to one embodiment of the present invention, the organic ester of phosphoric acid is more particularly a compound represented by the following structural formula (I).

[0079] [ka]

[0080] According to one embodiment of the present invention, in structural formula (I), each A is the same or different from each other, and each A is independently a hydrogen ion, an ammonium ion (NH + ), a metal ion (e.g., an alkali metal ion or an alkaline earth metal ion, especially a sodium ion) and the structural formula

[0081] [ka]

[0082] Preferably, at least one A is a hydrogen ion, more preferably both A are hydrogen ions. R0 is a hydrogen atom, an optionally substituted C 1-30 Linear or branched alkyl and optionally substituted C 6-20 aryl, preferably C 5-20 is selected from linear or branched alkyl and phenyl, more preferably C 9-15 A linear or branched alkyl, more preferably a C9 linear or branched alkyl. In addition, the n groups R1 are the same or different from each other and are each independently selected from the group consisting of C 1-6 Linear or branched alkylene, preferably C 2-4 It is a linear or branched alkylene, more preferably ethylene. n represents the average degree of polymerization of the polyether group, and is generally a number in the range of 0 to 200, preferably a number in the range of 0 to 100, more preferably a number in the range of 5 to 50 or 5 to 20.

[0083] According to one embodiment of the present invention, in order to fully exert its intended function in the production method of the present invention, the HLB value of the organic acid source is generally 3 to 8, preferably 3 to 6. Here, after determining a specific chemical structure of the organic acid source, its corresponding HLB value can be measured or calculated by a conventionally known method, or can be determined by referring to known data.

[0084] According to one embodiment of the present invention, in the contact step, the weight ratio of the alkaline aluminum source (converted into alumina) to the organic acid source is generally 1.2:1 to 24:1, preferably 5:1 to 20:1.

[0085] According to one embodiment of the present invention, in the contacting step, the salt specifically includes, for example, at least one of an alkali metal salt and an alkaline earth metal salt, preferably an alkali metal salt, such as a sodium salt.

[0086] According to one embodiment of the present invention, in the separation step, the mixture is separated to obtain pseudo-boehmite. Here, the manner or method of separation is not particularly limited as long as it can separate pseudo-boehmite from the mixture, and specifically, for example, filtration and any of the embodiments described below in this specification can be mentioned.

[0087] According to one embodiment of the present invention, the manufacturing method preferably comprises the following steps: (1) reacting a part of the total amount of an alkaline aluminum source, an organic acid source, and a cation exchange resin (referred to as usage amount A) in the presence of water to obtain a first mixed solution; (2) aging the first mixture, and then adding another portion of the total amount of cation exchange resin (referred to as usage amount B) to the first mixture to obtain a second mixture; (3) separating the cation exchange resin from the second mixture to obtain a slurry; and (4) A step of filtering the slurry as necessary and then drying the slurry to obtain pseudo-boehmite.

[0088] According to one embodiment of the present invention, the weight ratio of the amount A to the amount B is generally 8:1 to 4:1.

[0089] According to one embodiment of the present invention, in step (1), the reaction temperature (which refers to the temperature of the reaction mixture in the reactor) is generally 45°C to 80°C, preferably 50°C to 75°C.

[0090] According to one embodiment of the present invention, in step (1), the pH value of the reaction system (meaning the pH value of the reaction mixture in the reactor) is maintained at 7.5 to 10, preferably 8.0 to 9.5, by controlling the amount A used.

[0091] According to one embodiment of the present invention, in step (2), the aging temperature is generally 50 to 100° C., preferably 60 to 90° C., and the aging time is generally 0.5 to 3 hours, preferably 1 to 2 hours.

[0092] According to one embodiment of the present invention, in step (4), the drying temperature is generally 100 to 150° C., and the drying time is generally 6 to 10 hours, but may not be limited thereto.

[0093] According to one embodiment of the present invention, the manufacturing method more preferably comprises the steps of: (1) reacting an aqueous solution of an alkaline aluminum source, an aqueous solution of an organic acid source, and the suspension of the portion of the cation exchange resin to obtain a first mixed solution; (2) aging the first mixture and adding the second suspension of the cation exchange resin to obtain a second mixture; (3) separating the cation exchange resin from the second mixture to obtain a slurry; and (4) A step of filtering the slurry as necessary and then drying the slurry to obtain pseudo-boehmite.

[0094] According to one embodiment of the present invention, in step (1), the aqueous solution of the alkaline aluminum source, the aqueous solution of the organic acid source, and the suspension of the cation exchange resin can be added to the reactor simultaneously in a simultaneous mode, or separately, preferably simultaneously in a simultaneous mode. In addition, when adding the solutions separately to the reactor, the order of addition of the multiple streams is not particularly limited, but preferably, the aqueous solution of the alkaline aluminum source and the aqueous solution of the organic acid source are added first, and then the suspension of the cation exchange resin is added.

[0095] According to one embodiment of the present invention, step (1) is optionally carried out in the presence of water, in particular deionized water, in which an aqueous solution of an alkaline aluminum source, an aqueous solution of an organic acid source and a suspension of a cation exchange resin are preferably added to the water.

[0096] According to one embodiment of the present invention, in step (1), the amount of water is 5 to 20% by volume, preferably 5 to 15% by volume, of the total volume of the reaction system (eg, reactor).

[0097] According to one embodiment of the present invention, in step (1), the concentration of the sodium metallominate solution is generally 20 to 100 g Al2O3 / L, preferably 30 to 70 g Al2O3 / L, calculated as oxide.

[0098] According to one embodiment of the present invention, in step (1), the flow rate at which the sodium methamthenate solution is added to the reaction system is 20 mL / min to 60 mL / min, and preferably 30 mL / min to 50 mL / min.

[0099] According to one embodiment of the present invention, in step (1), the concentration of the aqueous solution of the organic acid source is 0.05 to 0.5 g / mL.

[0100] According to one embodiment of the present invention, in the step (1), the aqueous solution of the organic acid source is added to the reaction system at a flow rate of 5 mL / min. -1 0mL / min.

[0101] According to one embodiment of the present invention, in step (1), the solid content of the suspension of the cation exchange resin is 30 to 80% by weight, preferably 50 to 80% by weight.

[0102] According to one embodiment of the present invention, in step (1), the flow rate at which the suspension of the cation exchange resin is added to the reaction system, or the amount of the suspension of the cation exchange resin added to the reaction system is such that the pH value of the reaction system is maintained at 7.5 to 10, preferably 8.0 to 9.5.

[0103] According to one embodiment of the present invention, a preferred embodiment of the step (1) is, for example, adding bottom water to a reactor, heating to a constant temperature under stirring, and then adding an aqueous solution of sodium metallate, the aqueous solution of the organic phosphate ester, and a suspension of the cation exchange resin to carry out the reaction. Preferably, the bottom water is deionized water, and the amount of the water added is 5 to 20%, preferably 5 to 15%, of the reactor volume.

[0104] According to one embodiment of the present invention, in step (1), the aqueous solution of sodium metallate can be specifically prepared by, for example, mixing and boiling aluminum hydroxide and sodium hydroxide to prepare a solution having a concentration of 300 to 400 g Al2O3 / L, and then diluting the solution with an aqueous solution containing 1 to 5 wt % NaOH to a required concentration.

[0105] According to one embodiment of the present invention, the amount of the cation exchange resin suspension added to the reaction system in step (2) is an amount that allows the pH value of the first mixture to reach 6.0 to 7.5, preferably 6.5 to 7.0.

[0106] According to one embodiment of the present invention, in step (3), the separation can specifically include, for example, a method of separating the cation exchange resin from the second mixed liquid with a 100 to 120 mesh screen, where the separated cation exchange resin can be regenerated and recycled for use.

[0107] According to one embodiment of the present invention, in step (4), the slurry is separated into a filter cake and a filtrate, for example by filtration, the filter cake is dried to obtain pseudo-boehmite, and the filtrate can be recycled for use.

[0108] According to one embodiment of the present invention, in step (4), the drying temperature is generally 100 to 150° C., and the drying time is generally 6 to 10 hours, but may not be limited thereto.

[0109] According to one embodiment of the present invention, in the manufacturing process, precursors of auxiliary agents, such as one or more of SiO2, B2O3 and TiO2, may be added according to actual requirements. For this purpose, these precursors are added to the reaction process of step (1) in the form of water-soluble inorganic salts. Specific examples of the inorganic salts include silicates, borates, sulfates, nitrates, etc. In addition, the amount of these auxiliary agents added can be arbitrarily adjusted according to the requirements of the subsequent catalyst, etc. In general, the weight content of these auxiliary agents in terms of oxide is generally 1-8 wt%, preferably 2-6 wt%, based on 100 wt% of the total weight.

[0110] According to one embodiment of the present invention, the present invention also relates to alumina produced by using pseudo-boehmite according to any of the preceding embodiments of the present invention. Of course, the alumina according to the present invention can be produced by other production methods and is not limited to the specific production method according to the present invention.

[0111] According to one embodiment of the present invention, the phosphorus content of the alumina is generally 0.3 to 5.0% by weight (calculated as elemental phosphorus), and preferably 0.5 to 4.5% by weight.

[0112] According to one embodiment of the present invention, the pore volume of the alumina is generally 0.7 to 1.2 mL / g, preferably 0.8 to 1.1 mL / g, and more preferably 0.9 to 1.1 mL / g.

[0113] According to one embodiment of the present invention, the unit surface acid amount of the alumina is generally 0.001 to 0.002 mmol / m 2 , preferably 0.0015 to 0.002 mmol / m 2 It is.

[0114] According to one embodiment of the present invention, the hydraulic hardness of the alumina is generally 3 to 10 N / particle, preferably 5 to 10 N / particle.

[0115] According to one embodiment of the present invention, the alumina may also contain auxiliary agents, which may be one or more of Si, B, and Ti. Furthermore, the weight content of these auxiliary agents, calculated as oxides, is generally 2-14% by weight, preferably 4-11% by weight, based on 100% by weight of the total weight of the alumina.

[0116] According to one embodiment of the present invention, the alumina can be obtained by calcining pseudo-boehmite according to any one of the preceding embodiments of the present invention, wherein the calcination temperature is generally 500-900° C. and the calcination time is generally 2-8 hours.

[0117] According to one embodiment of the present invention, the present invention also relates to a catalyst, particularly a hydrogenation catalyst. The catalyst contains a catalytically active component and a carrier. In the present specification, the carrier contains the alumina of any one of the preceding embodiments of the present invention. In addition, the catalytically active component may specifically be, for example, a catalytically active component conventionally used in the technical field of hydrogenation of hydrocarbon oils, particularly an active metal component, particularly, for example, at least one of Group VIB metals and Group VIII metals of the Periodic Table of Elements, particularly at least one of Mo, W, Ni and Co. Preferably, the Group VIB metal is preferably Mo and / or W, and the Group VIII metal is preferably Ni and / or Co. Here, the content of the Group VIB metal component is 1% by weight to 30% by weight, and the content of the Group VIII metal component is 1% by weight to 15% by weight, based on 100% by weight of the total weight of the hydrogenation catalyst.

[0118] According to one embodiment of the present invention, the hydrogenation catalyst is 120 to 250 m 2 / g specific surface area, 0.50 to 0.75 mL / g pore volume, and 0.30 to 0.55 mmol / g infrared acidity.

[0119] According to one embodiment of the present invention, the hydrogenation catalyst may contain an auxiliary, which may be one or more of Si, B, and Ti. Furthermore, the weight of these auxiliary agents in terms of oxide is generally 0.5 to 5% by weight relative to 100% by weight of the total weight of the hydrogenation catalyst.

[0120] According to one embodiment of the present invention, the catalyst can be produced by the inventive production method as described below, which thus comprises at least the steps of producing the support and loading it.

[0121] According to one embodiment of the present invention, the process for producing the carrier can specifically include, for example, a method for obtaining a catalyst carrier by molding, optionally drying and calcining the pseudo-boehmite according to any one of the preceding embodiments of the present invention.

[0122] According to one embodiment of the present invention, the catalyst support preferably has the following properties: a pore volume of 0.5 to 0.9 mL / g, preferably 0.6 to 0.9 mL / g, more preferably 0.6 to 0.8 mL / g; a specific surface area of ​​150 to 280 m 2 / g, phosphorus content is 0.3 wt% to 5.0 wt% (phosphorus element equivalent), preferably 0.5 wt% to 4.5 wt%, and unit surface acid amount is 0.001 to 0.004 mmol / m 2 , preferably 0.0015 to 0.003 mmol / m 2 , the wear index is less than 1.0%.

[0123] According to one embodiment of the present invention, the loading step specifically includes, for example, a method of loading a catalytically active component onto the support to obtain a catalyst.

[0124] According to one embodiment of the present invention, in a preferred embodiment of the process for preparing the hydrogenation catalyst, pseudo-boehmite and deionized water are mixed uniformly, and then the resulting mixture is further molded, dried and calcined to obtain a carrier, and the active metal component is introduced onto the resulting carrier as described above to obtain the catalyst.

[0125] According to one embodiment of the present invention, in the preparation process of the hydrogenation catalyst, additives can be added as necessary, and the additives include a pore expanding agent and / or an extrusion aid. The pore expanding agent is one or more of carbon black, ammonium phosphate, ammonium carbonate, polyethylene glycol, polyvinyl alcohol, methyl cellulose, and polyacrylamide.

[0126] According to one embodiment of the present invention, in the process for producing a hydrogenation catalyst, the support is dried at 80 to 200° C. for 2 to 20 hours, and calcined at 600 to 1000° C. for 1 to 8 hours.

[0127] According to one embodiment of the present invention, in the preparation process of the hydrogenation catalyst, the said forming technology is a conventional technology known to those skilled in the art, the specific forming operation can be selected by those skilled in the art according to the actual requirements, and the shape can be any shape, such as cylindrical strip shape, three-leaf clover shape, four-leaf clover shape, spherical shape, and flake-like shape.

[0128] According to one embodiment of the present invention, in the process for preparing a hydrogenation catalyst, the active metal component is one or more of a group VIB metal and / or a group VIII metal, where the group VIB metal is generally Mo and / or W and the group VIII metal is generally Ni and / or Co.

[0129] According to one embodiment of the present invention, in the preparation process of the hydrogenation catalyst, the step of introducing the active metal component can be any conventional method available in the technical field, such as impregnation method, mixing and kneading method, etc., and is preferably the impregnation method. The support carrying the active metal component by the impregnation method is prepared by a conventional impregnation method, and spray impregnation method, saturation impregnation method or supersaturation impregnation method can be used. When the method of loading the hydrogenation active metal component on the support is the impregnation method, the method includes blending a solution of a compound containing a hydrogenation active metal, impregnating the support with the solution, followed by drying and optionally calcination.

[0130] According to one embodiment of the present invention, in the process for producing a hydrogenation catalyst, the concentration of the compound containing a hydrogenation active metal in the solution and the amount of the solution used are, based on oxide conversion and catalyst, such that, in the final catalyst, the content of the Group VIB metal component is 1 wt % to 30 wt % and the content of the Group VIII metal component is 1 wt % to 15 wt % relative to 100 wt % of the total weight of the hydrogenation catalyst.

[0131] According to one embodiment of the present invention, in the process for producing a hydrogenation catalyst, the drying temperature is 20 to 120° C., and the drying time is 0.5 to 24 hours.

[0132] According to one embodiment of the present invention, in the process for producing a hydrogenation catalyst, the calcination temperature is 400 to 550° C., and the calcination time is 1 to 6 hours.

[0133] According to one embodiment of the present invention, in the preparation process of the hydrogenation catalyst, precursors of auxiliary agents, such as one or more of SiO2, B2O3 and TiO2, may be added according to actual requirements. Here, the precursors are added in the form of water-soluble inorganic salts in the preparation process of the catalyst. The inorganic salts specifically include, for example, silicates, borates, sulfates or nitrates. Furthermore, the added amounts of these auxiliary agents may depend on the requirements of the catalyst. Specifically, for example, the weight content of these auxiliary agents in terms of oxide is generally 0.5-5 wt%, preferably 0.5-3 wt%, based on 100 wt% of the total weight of the catalyst.

[0134] According to one embodiment of the present invention, the present invention also relates to a hydrogenation method comprising the step of hydrogenating an oil product under hydrogenation reaction conditions in the presence of the hydrogenation catalyst according to any of the preceding embodiments of the present invention, wherein the oil product may be at least one selected from diesel oil, light oil, heavy oil and residual oil.

[0135] According to one embodiment of the present invention, in the hydrogenation method, the hydrogenation reaction conditions are generally a reaction pressure of 5 to 20 MPaG, a reaction temperature of 350 to 500°C, and a liquid hourly space velocity of 0.1 to 2.0 h -1and the hydrogen / oil volume ratio is 100 to 1000. EXAMPLES

[0136] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0137] In the following examples and comparative examples, "wt%" refers to "mass%."

[0138] In the following examples and comparative examples of the present invention, the contents of sodium oxide and phosphorus pentoxide in the pseudo-boehmite were measured by a fluorescence method.

[0139] Example 1 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L; a C9 monoalkyl ether phosphate ester (pKa=4.3, HLB=7) solution with a concentration of 0.2 g / mL was prepared for later use; and 60 mesh D001 macroporous strong acidic styrene-based cation exchange resin was prepared as a suspension with a solids content of 50 wt% for later use.

[0140] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, and the above three streams were added to the reactor in a simultaneous mode, the flow rate of sodium metaaluminate was controlled at 30mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled at 6mL / min, the flow rate of D001 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor at 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the resulting slurry was aged at 90℃ for 2 hours, and then D001 macroporous strong acidic styrene-based cation exchange resin suspension was added and the pH value of the slurry was adjusted to 7.0. The cation exchange resin and the slurry were separated by a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate the filter cake and the filtrate, and the filtrate could be recycled for use. The obtained filter cake was dried at 120°C for 8 hours to produce the pseudo-boehmite a1 of the present invention, whose properties are shown in Table 1, and its XRD is shown in Figure 1.

[0141] Since there was no washing step, the pseudo-boehmite a1 produced in Example 1 inevitably contained phosphate ester groups from the C9 monoalkyl ether phosphate ester.

[0142] Example 2 Pseudo-boehmite a2 was produced under the same conditions as in Example 1, except that the sodium metaaluminate solution was adjusted to 65 g Al2O3 / L and the colloid formation temperature was adjusted to 70°C. The properties of the pseudo-boehmite a2 are shown in Table 1.

[0143] Example 3 Pseudo-boehmite a3 was produced in the same manner as in Example 1, except that the 60 mesh D001 macroporous strong acid styrene-based cation exchange resin was replaced with 80 mesh D61 macroporous strong acid styrene-based cation exchange resin, the colloid formation pH value was adjusted to 9.0, and the drying conditions were changed to drying at 150°C for 6 hours. The properties of the pseudo-boehmite a3 are shown in Table 1.

[0144] Example 4 Pseudo-boehmite a4 was produced under the same conditions as in Example 1, except that the C9 monoalkyl ether phosphate ester was replaced with a C9 alkyl phosphate ester (pKa=4.8, HLB=5) and the pH after aging was adjusted to 6.5. The properties of the pseudo-boehmite a4 are shown in Table 1.

[0145] Example 5 Pseudo-boehmite A5 was produced under the same conditions as in Example 1, except that the flow rate of sodium metallaminate was changed to 45 mL / min, the concentration of the C9 monoalkyl ether phosphate ester solution was changed to 0.1 g / mL, and the flow rate was changed to 8 mL / min. The properties of the pseudo-boehmite A5 are shown in Table 1.

[0146] Comparative Example 1 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution having a concentration of 345 g Al2O3 / L, and then the solution was diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution having a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L for later use; a C9 monoalkyl ether phosphate ester (pKa=4.3, HLB=7) solution having a concentration of 0.2 g / mL was prepared for later use.

[0147] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two liquids were added simultaneously, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled to 6mL / min, and the temperature of the slurry in the reactor was kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, the slurry was filtered to separate the filter cake and the filtrate, the filter cake was washed with distilled water to pH=7, and the obtained filter cake was dried at 120℃ for 8 hours to prepare comparative pseudo-boehmite b1 (its characteristics are shown in Table 2). Its XRD is shown in Figure 1.

[0148] Comparative Example 2 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L for further use; 60 mesh D001 macroporous strong acidic styrene-based cation exchange resin was prepared into a suspension with a solid content of 50 wt% for further use.

[0149] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two liquids were added to the reactor in simultaneous mode, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of D001 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and then the pH value of the slurry was adjusted to 7.0 with the cation exchange resin suspension. The cation exchange resin and the slurry were separated with a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate the filter cake and filtrate, and the filtrate could be reused, and the obtained filter cake was dried at 120℃ for 8 hours to produce comparative pseudo-boehmite b2. Its properties were shown in Table 2.

[0150] Comparative Example 3 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, and this solution was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 25 g Al2O3 / L for later use.

[0151] The sodium metaaluminate solution was added to a 5000 mL reactor, a mixed gas of CO2 and air was introduced into the reactor, the temperature of the slurry in the reactor was controlled to be constant at 22°C, and the reaction was terminated when the pH value of the slurry in the reactor reached 10.5. The resulting slurry was filtered, and the filter cake was washed with deionized water in an amount 60 times that of the pseudo-boehmite produced to neutralize it, and then dried at 120°C for 8 hours to produce comparative pseudo-boehmite b3. Its properties are shown in Table 2.

[0152] Comparative Example 4 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, and then the solution was diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 150 g Al2O3 / L for later use; an aluminum sulfate solution with a concentration of 50 g Al2O3 / L was prepared for later use.

[0153] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two solutions were added to the reactor in a simultaneous mode, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of aluminum sulfate solution was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and after the aging was completed, the slurry was filtered, and the filter cake was washed with deionized water that was 80 times the amount of the pseudo-boehmite produced to neutralize it, and dried at 120℃ for 8 hours to produce pseudo-boehmite b4 of the present invention. Its properties are shown in Table 2, and its XRD is shown in FIG.

[0154] [Table 1]

[0155] [Table 2]

[0156] As can be seen from the data in the tables and figures, the pseudo-boehmite prepared according to the present invention has a low gibbsite content, and the characteristic peak of gibbsite does not appear in the XRD diagram. The pseudo-boehmite prepared according to the present invention has a low content of impurity sodium, and is suitable for the preparation of hydrogenation catalysts.

[0157] In the following examples and comparative examples of the present invention, the P content in alumina was measured by spectrophotometry, and the Na content was measured by inductively coupled plasma emission spectroscopy (ICP). The unit surface acidity of alumina was measured by infrared spectroscopy, and the adsorbent used was pyridine.

[0158] Example 2-1 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L; a C9 monoalkyl ether phosphate ester (pKa=4.3, HLB=7) solution with a concentration of 0.2 g / mL was prepared for later use; and 60 mesh D001 macroporous strong acidic styrene-based cation exchange resin was prepared as a suspension with a solids content of 50 wt% for later use.

[0159] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, and the above three streams were added to the reactor in simultaneous mode, the flow rate of sodium metaaluminate was controlled at 30mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled at 6mL / min, the flow rate of D001 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and then the pH value of the slurry was adjusted to 7.0 with D001 macroporous strong acidic styrene-based cation exchange resin suspension. The cation exchange resin and the slurry were separated by a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate the filter cake and the filtrate, and the filtrate was reused. The filter cake was dried at 120°C for 8 hours and calcined at 600°C for 3 hours to produce alumina A1 of the present invention, whose properties are shown in Table 2-1.

[0160] Example 2-2 Alumina A2 was produced under the same conditions as in Example 1, except that the sodium metaaluminate solution was adjusted to 65 g Al2O3 / L and the colloid formation temperature was adjusted to 70°C. The properties of alumina A2 are shown in Table 2-1.

[0161] Example 2-3 Alumina A3 was produced in the same manner as in Example 1, except that the 60 mesh D001 macroporous strong acid styrene-based cation exchange resin was replaced with 80 mesh D61 macroporous strong acid styrene-based cation exchange resin, the colloid formation pH value was adjusted to 9.0, and the drying conditions were changed to drying at 150°C for 6 hours. The properties of alumina A3 are shown in Table 2-1.

[0162] Examples 2-4 Alumina A4 was produced under the same conditions as in Example 1, except that the C9 monoalkyl ether phosphate ester was replaced with a C9 alkyl phosphate ester (pKa=4.8, HLB=5) and the pH after aging was adjusted to 6.5. The properties of the alumina A4 are shown in Table 2-1.

[0163] Examples 2-5 Alumina A5 was produced under the same conditions as in Example 1, except that the flow rate of sodium metallaminate was 45 mL / min, the concentration of the C9 monoalkyl ether phosphate ester solution was 0.1 g / mL, and the flow rate was 8 mL / min. The properties of alumina A5 are shown in Table 2-1.

[0164] Comparative Example 2-1 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution having a concentration of 345 g Al2O3 / L, and then the solution was diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution having a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L for later use; a C9 monoalkyl ether phosphate ester (pKa=4.3, HLB=7) solution having a concentration of 0.2 g / mL was prepared for later use.

[0165] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two liquids were added simultaneously, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled to 6mL / min, and the temperature of the slurry in the reactor was kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, the slurry was filtered to separate the filter cake and the filtrate, the filter cake was washed with distilled water to pH=7, the obtained filter cake was dried at 120℃ for 8 hours, and calcined at 600℃ for 3 hours to produce comparative alumina B1. Its properties are shown in Table 2-2.

[0166] Comparative Example 2-2 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L for further use; 60 mesh D001 macroporous strong acidic styrene-based cation exchange resin was prepared into a suspension with a solid content of 50 wt% for further use.

[0167] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two liquids were added to the reactor in simultaneous mode, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of D001 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and then the pH value of the slurry was adjusted to 7.0 with the cation exchange resin suspension. The cation exchange resin and the slurry were separated with a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate the filter cake and filtrate, and the filtrate could be recycled and used, and the obtained filter cake was dried at 120℃ for 8 hours and calcined at 600℃ for 3 hours to obtain comparative alumina B2. Its properties were shown in Table 2-2.

[0168] Comparative Example 2-3 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, and this solution was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 25 g Al2O3 / L for later use.

[0169] The sodium metaaluminate solution was added to a 5000 mL reactor, a mixed gas of CO2 and air was introduced into the reactor, the temperature of the slurry in the reactor was controlled to a constant 22°C, and the reaction was terminated when the pH value of the slurry in the reactor reached 10.5. The resulting slurry was filtered, and the filter cake was washed with deionized water in an amount 60 times that of the pseudo-boehmite produced to neutralize it, dried at 120°C for 8 hours, and then calcined at 600°C for 3 hours to produce comparative alumina B3. Its properties are shown in Table 2-2.

[0170] Comparative Example 2-4 Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, and then the solution was diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 150 g Al2O3 / L for later use; an aluminum sulfate solution with a concentration of 50 g Al2O3 / L was prepared for later use.

[0171] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two solutions were added to the reactor in a simultaneous mode, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of aluminum sulfate solution was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and after the aging was completed, the slurry was filtered, and the filter cake was washed with deionized water in an amount 80 times that of the pseudo-boehmite produced to neutralize it, dried at 120℃ for 8 hours, and then calcined at 600℃ for 3 hours to produce alumina B4 of the present invention. Its properties are shown in Table 2-2.

[0172] [Table 3]

[0173] [Table 4]

[0174] In the following examples and comparative examples of the present invention, the P content and metal oxide content in the alumina were measured by spectrophotometry, and the Na content was measured by inductively coupled plasma emission spectroscopy (ICP). The total acid content of the alumina was measured by an infrared spectrometer, and the adsorbent used was pyridine. The wear index was measured using a flow state wear index meter and represented the wear rate of the sample per unit weight per unit time.

[0175] Example 3-1 (1) Production of pseudo-boehmite Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L; a C9 monoalkyl ether phosphate solution with a concentration of 0.2 g / mL (pKa=4.3, HLB=7) was prepared for later use; and 60 mesh D001 macroporous strong acidic styrene-based cation exchange resin was prepared as a suspension with a solids content of 50 wt% for later use.

[0176] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, and the above three streams were added to the reactor in simultaneous mode, the flow rate of sodium metaaluminate was controlled at 30mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled at 6mL / min, the flow rate of D001 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and then the pH value of the slurry was adjusted to 7.0 with D001 macroporous strong acidic styrene-based cation exchange resin suspension. The cation exchange resin and the slurry were separated by a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate a filter cake and a filtrate, and the filtrate could be recycled for use. The obtained filter cake was dried at 120°C for 8 hours to prepare the pseudo-boehmite a1 of the present invention.

[0177] (2) Preparation of hydrogenation catalyst C1 500 g of the pseudo-boehmite raw material a1 produced was taken, 10.5 g of sesbania powder and 7.0 g of methylcellulose were added, and the mixture was molded into a sphere. The sphere was then fired at 850°C for 5 hours to obtain carrier Z1 having a particle size of 0.3 to 0.8 mm. The properties of the carrier Z1 are shown in Table 3-1.

[0178] 57.12g of phosphoric acid was weighed out, 1800mL of distilled water was added, 155.16g of molybdenum oxide and 71.12g of basic nickel carbonate were added in sequence, and the mixture was heated and stirred until completely dissolved, and then diluted with distilled water to a constant volume of 2000mL to obtain solution L1. Support Z1 was saturated with solution L1, dried at 110°C for 2 hours, and then calcined at 550°C for 5 hours to produce catalyst C1. Its specific properties are shown in Table 3-3.

[0179] Example 3-2 Pseudoboehmite a-2, carrier Z-2 and catalyst C-2 were prepared under the same conditions as in Example 1, except that 60 mesh D001 macroporous strong acid styrene-based cation exchange resin was replaced with 80 mesh D002 macroporous strong acid styrene-based cation exchange resin, the pH value of the slurry in the reactor was changed to 8.5, and the obtained slurry was aged at 75°C for 3 hours. The specific properties of the carriers are shown in Table 1, and the specific properties of the catalysts are shown in Table 3-3.

[0180] Example 3-3 (1) Production of pseudo-boehmite Pseudoboehmite a3 was produced under the same conditions as in Example 1, except that the C9 monoalkyl ether phosphate ester was replaced with a C9 alkyl phosphate ester (pKa=4.8, HLB=5), the flow rate was changed to 8 mL / min, the flow rate of sodium metallaminate was changed to 50 mL / min, and the colloid formation temperature was adjusted to 70°C.

[0181] (2) Catalyst production 500g of the pseudo-boehmite raw material a3 produced was taken, 10.5g of sesbania powder and 17.5g of polyacrylamide were added, and the mixture was molded into a sphere. The spherical sample was calcined at 700 ° C for 3 hours to obtain carrier Z3 with a particle size of 0.8-1.2 mm. Its characteristics are shown in Table 1. 62.72g of phosphoric acid was added, 1800mL of distilled water was added, 221.48g of molybdenum oxide and 71.84g of cobalt hydroxide were added in sequence, and the mixture was heated and distilled until completely dissolved, and diluted to a constant amount of 2000mL of distilled water to obtain solution L2. The carrier Z3 was saturated with solution L2, dried at 110 ° C for 4 hours, and then calcined at 500 ° C for 5 hours to produce catalyst C3. Its specific characteristics are shown in Table 3-3.

[0182] Examples 3-4 (1) Production of pseudo-boehmite Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 360 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.25 and a concentration of 60 g Al2O3 / L; a C9 monoalkyl ether phosphate ester (pKa=4.3, HLB=7) solution with a concentration of 0.1 g / mL was prepared for later use; and 60 mesh D61 macroporous strong acidic styrene-based cation exchange resin was prepared as a suspension with a solids content of 70 wt% for later use.

[0183] 800mL of pure water was added to a 5000mL reactor, stirring and heating were started, the pure water was heated to 60℃, the above three liquids were added simultaneously, the flow rate of sodium metaaluminate was controlled to 20mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled to 8mL / min, and the flow rate of D61 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor to 8.5, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 80℃ for 2 hours, and then the pH value of the slurry was adjusted to 7.0 with the cation exchange resin suspension. The cation exchange resin and the slurry were separated with a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate the filter cake and the filtrate, and the filtrate could be recycled for use, and the obtained filter cake was dried at 150℃ for 6 hours to produce the pseudo-boehmite a4 of the present invention.

[0184] (2) Catalyst production 500 g of the pseudo-boehmite raw material a4 was taken, 7.0 g of sesbania powder and 10.5 g of ammonium bicarbonate were added, and the mixture was molded into a sphere. The mixture was then calcined at 650°C for 3 hours to obtain carrier Z4 with a particle size of 0.6 to 1.0 mm (the characteristics are shown in Table 1). The carrier Z4 was saturated with solution L1, dried at 110°C for 2 hours, and calcined at 480°C for 4 hours to produce catalyst C4. The specific characteristics are shown in Table 3-3.

[0185] Comparative Example 3-1 (1) Production of pseudo-boehmite Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution having a concentration of 345 g Al2O3 / L, and then the solution was diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution having a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L for later use; a C9 monoalkyl ether phosphate ester (pKa=4.3, HLB=7) solution having a concentration of 0.2 g / mL was prepared for later use.

[0186] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two liquids were added simultaneously, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of C9 monoalkyl ether phosphate ester solution was controlled to 6mL / min, and the temperature of the slurry in the reactor was kept constant. After the reaction was completed, the obtained slurry was aged at 80℃ for 2 hours, the slurry was filtered to separate the filter cake and the filtrate, the filter cake was washed with distilled water to pH=7, and the obtained filter cake was dried at 120℃ for 8 hours to produce pseudo-boehmite f1.

[0187] (2) Catalyst production 500 g of the produced pseudo-boehmite raw material f1 was taken, 10.5 g of sesbania powder and 7.0 g of methylcellulose were added, and the mixture was molded into a sphere. The sphere was then fired at 850°C for 5 hours to obtain a carrier F1 having a particle size of 0.3 to 0.8 mm. The properties of the carrier are shown in Table 3-2.

[0188] The carrier F1 was saturated with the solution L1, dried at 110° C. for 2 hours, and then calcined at 550° C. for 5 hours to produce the catalyst CF1. The specific properties are shown in Table 3-4.

[0189] Comparative Example 3-2 (1) Production of pseudo-boehmite Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, which was then diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 50 g Al2O3 / L for further use; 60 mesh D001 macroporous strong acidic styrene-based cation exchange resin was prepared into a suspension with a solid content of 50 wt% for further use.

[0190] 500mL of pure water was added to a 5000mL reactor as bottom water, stirring and heating were started, the pure water was heated to 50℃, the above two liquids were added to the reactor in simultaneous mode, the flow rate of sodium metaaluminate was controlled to 30mL / min, the flow rate of D001 macroporous strong acidic styrene-based cation exchange resin suspension was adjusted to control the pH value of the slurry in the reactor to 8.0, and the temperature and pH value of the slurry in the reactor were kept constant. After the reaction was completed, the obtained slurry was aged at 90℃ for 2 hours, and then the pH value of the slurry was adjusted to 7.0 with the cation exchange resin suspension. The cation exchange resin and the slurry were separated with a 100 mesh screen, and the separated cation exchange resin was regenerated and recycled for use. The slurry was filtered to separate the filter cake and filtrate, the filtrate could be reused, and the obtained filter cake was dried at 120℃ for 8 hours to produce pseudoboehmite f2.

[0191] (2) Catalyst production 500 g of the produced pseudo-boehmite raw material f2 was taken, 10.5 g of sesbania powder and 7.0 g of methylcellulose were added, and the mixture was molded into a sphere. The sphere was then fired at 850°C for 5 hours to obtain carrier F2 having a particle size of 0.3 to 0.8 mm. The properties of the carrier are shown in Table 3-2.

[0192] The carrier F2 was saturated with the solution L1, dried at 110°C for 2 hours, and then calcined at 550°C for 5 hours to produce the catalyst CF2, the specific properties of which are shown in Table 3-4.

[0193] Comparative Example 3-3 (1) Production of pseudo-boehmite Aluminum hydroxide and sodium hydroxide were mixed and boiled to prepare a solution with a concentration of 345 g Al2O3 / L, and then the solution was diluted with an aqueous solution containing 3.5 wt% NaOH to prepare a sodium metaaluminate solution with a caustic ratio of 1.20 and a concentration of 150 g Al2O3 / L for later use; an aluminum sulfate solution with a concentration of 50 g Al2O3 / L was prepared for later use.

[0194] Add 500mL of pure water as bottom water to a 5000mL reactor, start stirring and heating, heat the pure water to 50℃, add the above two solutions to the reactor in simultaneous mode, control the flow rate of sodium metaaluminate to 30mL / min, adjust the flow rate of aluminum sulfate solution to control the pH value of the slurry in the reactor to 8.0, and keep the temperature and pH value of the slurry in the reactor constant. After the reaction is completed, the obtained slurry is aged at 90℃ for 2 hours, and after the aging is completed, the slurry is filtered, and the filter cake is washed with deionized water 80 times the amount of the generated pseudo-boehmite to neutralize it, and dried at 120℃ for 8 hours to prepare pseudo-boehmite f3.

[0195] (2) Catalyst production 500 g of the produced pseudo-boehmite raw material f3 was taken, 10.5 g of sesbania powder and 7.0 g of methylcellulose were added, and the mixture was molded into a sphere. The sphere was then fired at 850°C for 5 hours to obtain carrier F3 having a particle size of 0.3 to 0.8 mm. The properties of the carrier are shown in Table 3-2.

[0196] The carrier F3 was saturated impregnated with the solution L1, dried at 110°C for 2 hours, and then calcined at 550°C for 5 hours to produce the catalyst CF3, the specific properties of which are shown in Table 3-4.

[0197] [Table 5]

[0198] [Table 6]

[0199] [Table 7]

[0200] [Table 8]

[0201] The activity of the above catalyst was evaluated in a continuous stirred high pressure autoclave (CSTR), the catalyst loading was 100mL, and the ebullated bed reactor was similar to the continuous stirred tank reactor (CSTR), both of which had good total backmixing performance and comparable reaction rate characteristics. Therefore, the CSTR could be used instead of the ebullated bed reactor for catalyst performance evaluation. The characteristics of the feedstock and the evaluation conditions were shown in Tables 3-5. The activity of Comparative Example 3 was 100, and the other activities were compared with Comparative Example 3, and the evaluation results were shown in Table 4.

[0202] [Table 9]

[0203] [Table 10]

[0204] As can be seen from Table 6, the hydrogenation catalyst prepared with the alumina in this study had increased impurity removal and conversion rates compared with the catalyst prepared in the comparative example, and was particularly suitable for use as an ebullated bed hydrogenation catalyst for heavy oil or residual oil.

Claims

1. The dry basis content is 55 to 85% by weight based on 100% by weight of the total weight of the pseudo-boehmite; Contains a phosphate ester group, Pseudo-boehmite having a sodium oxide content of 0.5% by weight or less and a phosphorus content calculated as phosphorus pentoxide of 1.2 to 5.7% by weight.

2. Based on 100% by weight of the total weight of pseudo-boehmite, the dry basis content being 65-75% by weight; and / or the sodium oxide content is less than or equal to 0.03% by weight; and / or The pseudo-boehmite according to claim 1, wherein the phosphorus content in terms of phosphorus pentoxide is 1.4 to 4.2% by weight.

3. The pseudo-boehmite according to claim 1, wherein the phosphate ester group is derived from a compound represented by the following structural formula (I): [Formula 1] In structural formula (I), each A is the same or different and independently represents a hydrogen ion, an ammonium ion (NH 4 + ), metal ions and structural formulas [chemical 2] is selected from the group represented by R 0 represents a hydrogen atom, a substituted or unsubstituted C 1-30 Linear or branched alkyl and substituted or unsubstituted C 6-20 aryl; n groups R 1 are the same or different from each other, and independently of each other, C 1-6 is selected from linear or branched alkylene; n is a number ranging from 0 to 200.

4. The pseudo-boehmite according to claim 3 , wherein the metal ion is an alkali metal ion or an alkaline earth metal ion.

5. At least one A is a hydrogen ion, and / or R 0 But, C 5-20 and / or selected from linear or branched alkyl and phenyl; n groups R 1 are the same or different from each other, and independently of each other, C 2-4 and / or selected from linear or branched alkylene; The pseudo-boehmite according to claim 3, wherein n is a number ranging from 0 to 100.

6. Both of the two A's are hydrogen ions, and / or R 0 C 9 and / or n groups R 1 are the same or different from one another and are, independently of one another, ethylene; and / or The pseudo-boehmite according to claim 3, wherein n is a number in the range of 5 to 20.

7. 2. The pseudo-boehmite of claim 1, having a gibbsite content of <3.0 wt.%, based on 100 wt.% of the total weight of the pseudo-boehmite.

8. The pseudo-boehmite according to claim 1, further comprising at least one auxiliary selected from the group consisting of Si, B and Ti, and the content of the at least one auxiliary in terms of oxide is 1 to 8 wt % relative to 100 wt % of the total weight of the pseudo-boehmite.

9. The pseudo-boehmite according to claim 8, wherein the content of the at least one auxiliary agent is 2 to 6% by weight, calculated as oxide, relative to 100% by weight of the total weight of the pseudo-boehmite.

10. A method for producing pseudo-boehmite, comprising the steps of: contacting an alkaline aluminum source, a cation exchange resin and an organic acid source in the presence of water to obtain a mixture, wherein the alkaline aluminum source is an aluminate, the cation exchange resin is selected from at least one of a macroporous strongly acidic styrene-based cation exchange resin and a sulfonated styrene-based gel-type strongly acidic cation exchange resin, and the organic acid source is selected from at least one of a mono-C9-C15-alkyl ether phosphate ester, a mono-C9-C15-alkyl phosphate ester, a di-C9-C15-alkyl phosphate ester, and a di-C9-C15-alkyl ether phosphate ester; and separating the mixed liquid to obtain pseudo-boehmite.

11. the alkaline aluminum source is sodium metaaluminate; and / or The cation exchange resin is selected from at least one of D001 macroporous strongly acidic styrenic cation exchange resin and D61 macroporous strongly acidic styrenic cation exchange resin, and / or The process of claim 10, wherein the organic acid source has an acidity coefficient pKa of 3 to 6.

12. The method according to claim 10, wherein the organic acid source is a compound represented by the following structural formula (I): [C3] In structural formula (I), each A is the same or different and independently represents a hydrogen ion, an ammonium ion (NH 4 + ), metal ions and structural formulas [C4] is selected from the group represented by R 0 represents a hydrogen atom, a substituted or unsubstituted C 1-30 Linear or branched alkyl and substituted or unsubstituted C 6-20 aryl; n groups R 1are the same or different from each other, and independently of each other, C 1-6 is selected from linear or branched alkylene; n is a number ranging from 0 to 200.

13. At least one A is a hydrogen ion, and / or R 0 But, C 5-20 and / or selected from linear or branched alkyl and phenyl; n groups R 1 are the same or different from each other, and independently of each other, C 2-4 and / or selected from linear or branched alkylene; The method according to claim 12, wherein n is a number ranging from 0 to 100.

14. Both of the two A's are hydrogen ions, and / or R 0 C 9 and / or n groups R 1 are each ethylene, and / or The method according to claim 12, wherein n is a number in the range of 5 to 20.

15. The method according to claim 12, wherein the metal ion is an alkali metal ion or an alkaline earth metal ion.

16. The method according to claim 10, wherein a mass ratio of the alkaline aluminum source to the organic acid source, calculated as alumina, is from 1.2:1 to 24:1, and / or the organic acid source has 30 or less carbon atoms, and / or the organic acid source has an HLB value of 3 to 8, and / or the cation exchange resin has a particle size of 20 to 150 mesh.

17. the mass ratio of the alkaline aluminum source to the organic acid source, calculated as alumina, is from 5:1 to 20:1; and / or the organic acid source has 15 or less carbon atoms; and / or the organic acid source has an HLB value of 3 to 6; and / or The method according to claim 16, wherein the particle size of the cation exchange resin is 40 to 80 mesh.

18. The method of claim 10, comprising the steps of: (1) reacting the alkaline aluminum source, the organic acid source, and a part of the total amount of the cation exchange resin in the presence of water to obtain a first mixed solution; (2) A step of aging the first mixed solution and then adding another part of the total amount of the cation exchange resin to obtain a second mixed solution; (3) separating the cation exchange resin from the second mixture to obtain a slurry; and (4) A step of drying the slurry after filtering the slurry or without filtering the slurry to obtain the pseudo-boehmite.

19. the alkaline aluminum source is sodium metaaluminate having a caustic ratio of 1.15 to 1.35; and / or In the step (1), the reaction temperature is 45° C. to 80° C., and the pH value of the reaction system is 7.5 to 10; and / or In the step (2), the aging temperature is 50 to 100° C. and the aging time is 0.5 to 3 hours, and / or The method according to claim 18, wherein in the step (4), the drying temperature is 100 to 150° C., and the drying time is 6 to 10 hours.

20. the alkaline aluminum source is sodium metaaluminate having a caustic ratio of 1.20 to 1.30; and / or In the step (1), the reaction temperature is 50° C. to 75° C., and / or the pH value of the reaction system is 8.0 to 9.5, and / or The method according to claim 19, wherein in the step (2), the aging temperature is 60 to 90° C. and / or the aging time is 1 to 2 hours.

21. 20. The method of claim 19, comprising the steps of: (1) reacting the aqueous solution of the alkaline aluminum source, the aqueous solution of the organic acid source, and the suspension of the portion of the cation exchange resin to obtain the first mixed solution; (2) aging the first mixture and then adding the suspension of the other part of the cation exchange resin to obtain the second mixture; (3) separating the cation exchange resin from the second mixture to obtain a slurry; and (4) After filtering the slurry or without filtering the slurry, the slurry is then dried to obtain the pseudo-boehmite; and / or the aqueous solution of alkaline aluminum source is an aqueous solution of sodium metaaluminate having a caustic ratio of 1.15 to 1.

35.

22. The step (1) is carried out in the presence of water, and / or 22. The method according to claim 21, wherein in the step (1), the aqueous solution of the alkaline aluminum source, the aqueous solution of the organic acid source, and the suspension of the cation exchange resin are added to water to obtain the first mixed solution.

23. In the step (1), the amount of water is 5 to 20% by volume of the total volume of the reaction system, and / or In the step (1), the concentration of the sodium metaaluminate solution is 20 to 100 g Al 2 O 3 / L, and / or In the step (1), the flow rate at which the sodium metaaluminate solution is added to the reaction system is 20 mL / min to 60 mL / min; and / or In the step (1), the concentration of the aqueous solution of the organic acid source is 0.05 to 0.5 g / mL, and / or In the step (1), the flow rate at which the aqueous solution of the organic acid source is added to the reaction system is 5 mL / min to 10 mL / min; and / or In step (1), the suspension of the cation exchange resin has a solids content of 30 to 80% by weight, and / or In the step (1), the flow rate of the suspension of the cation exchange resin added to the reaction system or the amount of the suspension of the cation exchange resin added to the reaction system is such that the pH value of the reaction system is maintained at 7.5 to 10; and / or In the step (2), the amount of the suspension of the cation exchange resin added to the reaction system is an amount such that the pH value of the first mixture reaches 6.0 to 7.5; The process of claim 21 , wherein the reaction system is a reactor.

24. In the step (1), the amount of water is 5 to 15% by volume of the total volume of the reaction system, and / or In the step (1), the concentration of the sodium metaaluminate solution is 30 to 70 g Al 2 O 3 / L, and / or In the step (1), the flow rate at which the sodium metaaluminate solution is added to the reaction system is 30 mL / min to 50 mL / min; and / or In step (1), the suspension of the cation exchange resin has a solids content of 50 to 80% by weight, and / or In the step (1), the flow rate of the suspension of the cation exchange resin added to the reaction system or the amount of the suspension of the cation exchange resin added to the reaction system is such that the pH value of the reaction system is maintained at 8.0 to 9.5, and / or The method according to claim 23, wherein in the step (2), an amount of the suspension of the cation exchange resin added to the reaction system is such that a pH value of the first mixture reaches 6.5 to 7.

0.

25. The phosphorus content is 0.3 to 5.0 wt.% in terms of elemental phosphorus, The pore volume is 0.7 to 1.2 mL / g; The amount of acid per unit surface area is 0.001 to 0.002 mmol / m 2 and Alumina with a hydraulic hardness of 3 to 10 N / particle.

26. The phosphorus content is 0.5 to 4.5% by weight in terms of elemental phosphorus, and / or and / or the pore volume is 0.9 to 1.1 mL / g; The amount of acid per unit surface area is 0.0015 to 0.002 mmol / m 2 and / or 26. Alumina according to claim 25, wherein said hydraulic property is between 5 and 10 N / particle.

27. A method for producing alumina, comprising the steps of: A step of producing pseudo-boehmite by the method according to claim 10; and A step of calcining the pseudo-boehmite to obtain alumina.

28. 26. A catalyst comprising a catalytically active component and a support, said support comprising the alumina of claim 25.

29. the catalyst is a hydrogenation catalyst; and / or 30. The catalyst of claim 28, wherein the catalytically active component is selected from at least one of Mo, W, Ni and Co.

30. A method for producing a catalyst, comprising the steps of: A step of producing pseudo-boehmite according to the production method of claim 10; forming the pseudo-boehmite into a shape and calcining it with or without drying to obtain a carrier; and A step of supporting a catalytically active component on the support to obtain the catalyst.

31. the catalyst is a hydrogenation catalyst; and / or The process of claim 30, wherein the catalytically active component is selected from at least one of Mo, W, Ni and Co.

32. 31. A process for hydrogenation comprising the step of hydrogenating an oil product in the presence of the hydrogenation catalyst of claim 28 or the hydrogenation catalyst produced by the process of claim 30 under hydrogenation reaction conditions.

33. 33. The hydrogenation process of claim 32, wherein the oil product is selected from at least one of diesel, vacuum gas oil, heavy oil and residual oil.

34. The hydrogenation reaction conditions are a reaction pressure of 5 to 20 MPaG, a reaction temperature of 350 to 500° C., and a liquid hourly space velocity of 0.1 to 2.0 h -1 and the hydrogen / oil volume ratio is 100 to 1000.

Citation Information

Patent Citations

  • Methods for preparing pseudoboehmite and amminium oxide by taking kaolin as raw material

    CN103274438A

  • Distillate oil hydrofining catalyst and preparation method and application ofdistillate oil hydrofining catalyst

    CN104624215A

  • Alumina in high hydrothermal stability, and preparation method

    CN1958456A

  • Method for producing beta-alumina

    JP2003335517A

  • Method for producing pseudocrystalline boehmite from inexpensive precursors

    JP2003507298A