Method for manufacturing bonded semiconductor wafer
The method addresses the issue of bonding material intrusion by using a passivation film and fluorine-based etching to enhance sacrificial layer etching, improving yield in semiconductor wafer manufacturing.
Patent Information
- Application Number
- JP2021176922
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing methods for transferring semiconductor functional layers face issues with bonding materials seeping into element isolation grooves, inhibiting sacrificial layer etching and reducing the yield of device manufacturing.
A method involving epitaxial growth of a sacrificial layer on a starting substrate, forming device isolation trenches, applying a passivation film, bonding with a flexible thermosetting material, and etching the sacrificial layer to separate the starting substrate, using a fluorine-based solution to prevent bonding material intrusion.
Prevents bonding material from entering element isolation grooves, ensuring effective etching of the sacrificial layer, thereby improving the yield of device manufacturing, particularly for micro LEDs.
Smart Images

Figure 0007556342000049 
Figure 0007556342000057 
Figure 0007556342000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a bonded semiconductor wafer. [Background technology]
[0002] The technology of separating only a semiconductor functional layer, such as an epitaxial functional layer, from a starting substrate and transferring it to another substrate is an important technology for alleviating constraints imposed by the physical properties of the starting substrate and increasing the design freedom of device systems.
[0003] To achieve this transfer, a technology is required to remove the starting substrate after bonding the epitaxial functional layer to the permanent substrate and then to achieve the transfer.
[0004] Patent Document 1 discloses a technique for thermocompression bonding a semiconductor epitaxial substrate and a temporary support substrate via a dielectric layer, and a technique for separating the temporary support substrate and the epitaxial functional layer by wet etching.
[0005] Patent Document 2 discloses a technique in which an element isolation groove is formed to expose a sacrificial layer, and then bonding is performed, and the sacrificial layer is etched to separate the starting substrate.
[0006] However, this technology requires that the bonding material be a solid material. If the bonding interface is formed with a soft or liquid material, the bonding layer will deform due to the pressure during bonding and will seep into the isolation trench. The seeped bonding material will fill the isolation trench, and as a result, the sacrificial layer, which is the purpose of forming the isolation trench, will be covered with the bonding material, preventing the etching of the sacrificial layer from proceeding. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2021-27301 [Patent Document 2] International Publication No. WO2014 / 020906 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a method for manufacturing a bonded semiconductor wafer in which element isolation grooves are formed in an epitaxial wafer and the epitaxial wafer is bonded to a bonded substrate via a flexible bonding material, which prevents the bonding material from seeping into the element isolation grooves and impeding sacrificial layer etching. [Means for solving the problem]
[0009] The present invention has been made to achieve the above-mentioned object, and provides a method for manufacturing a bonded semiconductor wafer, comprising the steps of epitaxially growing a sacrificial layer on a starting substrate, epitaxially growing an epitaxial layer having a semiconductor functional layer on the sacrificial layer to produce an epitaxial wafer, forming an element isolation groove by a selective etching method so that the sacrificial layer is exposed in a partial region of the epitaxial wafer, forming a passivation film on at least the surface of the element isolation groove where the sacrificial layer is exposed, bonding the epitaxial layer of the epitaxial wafer to a bonded substrate that is transparent to visible light via a thermosetting bonding material to produce a bonded substrate, etching and removing the passivation film of the bonded substrate, and supplying an etching liquid to the element isolation groove of the bonded substrate to etch the sacrificial layer, thereby separating the starting substrate and the epitaxial layer.
[0010] With this manufacturing method for bonded semiconductor wafers, a passivation (PSV) film is formed on at least the surface of the sacrificial layer in the element isolation groove during bonding, so that it is possible to prevent the bonding material from seeping into the element isolation groove and covering the surface of the sacrificial layer, which would hinder the etching of the sacrificial layer.
[0011] In this case, the bonded substrate is preferably made of any one of the following materials: sapphire, synthetic quartz, quartz (natural quartz), glass, SiC, LiTaO3, and LiNbO3.
[0012] Such a bonded substrate can be selected so as to have high transparency to lasers, and is suitable as a bonded substrate in the method for producing a bonded semiconductor wafer of the present invention.
[0013] The thermosetting bonding material is preferably one or more of the following materials: silicone resin, epoxy resin, benzocyclobutene, spin-on glass, polyimide, and fluororesin.
[0014] Such a thermosetting bonding material can be suitably used as a bonding material in a method for producing a bonded semiconductor wafer.
[0015] The thickness of the thermosetting bonding material is preferably 0.01 μm or more and 0.6 μm or less.
[0016] If the adhesive layer has such a thickness, uneven thickness caused by being too thick will not be a problem, and a thickness necessary and sufficient for adhesion can be ensured.
[0017] The thermosetting bonding material may not be thermoset.
[0018] In this way, if the thermosetting bonding material is not thermally cured, it can be easily peeled off when peeling is performed.
[0019] The passivation film is preferably a silicon oxide film.
[0020] In this way, if the passivation film used in the present invention is a silicon oxide film, it can be formed and removed relatively easily. In addition, the silicon oxide film removal etching can also serve as the sacrificial layer etching by using a fluorine-based solution.
[0021] In addition, the bonded semiconductor wafer is preferably used for a micro LED.
[0022] Thus, the method for producing a bonded semiconductor wafer of the present invention is particularly advantageous in producing small-sized elements such as those used in micro LEDs. Effect of the Invention
[0023] According to the method for producing a bonded semiconductor wafer of the present invention, in a method for producing a bonded semiconductor wafer in which an isolation groove is formed in an epitaxial wafer and the epitaxial wafer is bonded to a substrate via a flexible thermosetting bonding material, the presence of a passivation film can prevent the bonding material from seeping into the isolation groove and impeding the etching of the sacrificial layer, thereby improving the yield of device production in the bonded semiconductor wafer. [Brief description of the drawings]
[0024] [Figure 1] 1 is a schematic cross-sectional view showing a part of a first embodiment of a method for producing a bonded semiconductor wafer of the present invention. [Diagram 2] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Diagram 3] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 4] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Diagram 5] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 6] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 7] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 8]4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 9] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 10] 4 is a schematic cross-sectional view showing another part of the first embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 11] 1 is a schematic cross-sectional view of an example of a bonded semiconductor wafer obtained by a first embodiment of a method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 12] 4 is a schematic cross-sectional view showing a part of a second embodiment of a method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 13] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 14] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 15] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 16] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 17] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 18] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 19] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 20] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 21] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 22]4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Diagram 23] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 24] 4 is a schematic cross-sectional view showing another part of the second embodiment of the method for producing a bonded semiconductor wafer of the present invention. FIG. [Diagram 25] FIG. 2 is a schematic cross-sectional view of an example of a bonded semiconductor wafer obtained by a second embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 26] 4 is a schematic cross-sectional view showing a part of a third embodiment of a method for producing a bonded semiconductor wafer of the present invention. FIG. [Figure 27] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 28] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 29] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 30] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 31] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 32] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 33] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 34] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 35] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 36]FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 37] FIG. 4 is a schematic cross-sectional view showing another part of the third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 38] FIG. 2 is a schematic cross-sectional view of an example of a bonded semiconductor wafer obtained by a third embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 39] 10 is a schematic cross-sectional view showing a part of a fourth embodiment of a method for producing a bonded semiconductor wafer of the present invention. FIG. [Diagram 40] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 41] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 42] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 43] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 44] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 45] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 46] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 47] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 48] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 49] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 50]FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 51] FIG. 11 is a schematic cross-sectional view showing another part of the fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Figure 52] FIG. 11 is a schematic cross-sectional view of an example of a bonded semiconductor wafer obtained by a fourth embodiment of the method for producing a bonded semiconductor wafer of the present invention. [Diagram 53] 5 is a schematic cross-sectional view showing a part of a method for manufacturing a bonded semiconductor wafer of a comparative example. [Figure 54] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 55] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 56] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 57] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 58] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 59] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 60] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 61] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 62] 10 is a schematic cross-sectional view showing another part of the method for producing a bonded semiconductor wafer of the comparative example. [Figure 63] 1 is a schematic cross-sectional view of an example of a bonded semiconductor wafer obtained by a manufacturing method of a bonded semiconductor wafer according to a comparative example. [Figure 64] 1 is a graph showing the yields of Examples 1 to 4 and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention will be described in detail below, but the present invention is not limited thereto.
[0026] The present invention is a method for manufacturing a bonded semiconductor wafer, comprising the steps of epitaxially growing a sacrificial layer on a starting substrate, epitaxially growing an epitaxial layer having a semiconductor functional layer on the sacrificial layer to produce an epitaxial wafer, forming an element isolation groove by a selective etching method so that the sacrificial layer is exposed in a partial region of the epitaxial wafer, forming a passivation film on at least the surface of the element isolation groove where the sacrificial layer is exposed, bonding the epitaxial layer of the epitaxial wafer to a bonded substrate that is transparent to visible light via a thermosetting bonding material to produce a bonded substrate, etching and removing the passivation film of the bonded substrate, and supplying an etching solution to the element isolation groove of the bonded substrate to etch the sacrificial layer, thereby separating the starting substrate and the epitaxial layer.
[0027] Hereinafter, the present invention will be described by taking the first to fourth embodiments as examples. In each embodiment, similar components are denoted by the same reference numerals in the drawings. Also, some overlapping descriptions will be omitted.
[0028] [First embodiment] A first embodiment will be described. First, as shown in Fig. 1, epitaxial growth is performed in sequence on a starting substrate 11 to form each layer, and an epitaxial wafer 20 is produced. This produces an epitaxial layer having a sacrificial layer 12 and a semiconductor functional layer 18. More specifically, the epitaxial growth of each layer can be performed as follows.
[0029] As shown in FIG. 1, a sacrificial layer 12 is epitaxially grown on a starting substrate 11 made of, for example, GaAs of a first conductivity type. The sacrificial layer 12 can be formed, for example, by stacking a GaAs buffer layer of a first conductivity type, and then growing a GaInP first etch stop layer of a first conductivity type and a GaAs second etch stop layer of a first conductivity type. Furthermore, for example, an AlGaInP first cladding layer 13 of a first conductivity type, a non-doped AlGaInP active layer 14, an AlGaInP second cladding layer 15 of a second conductivity type, a GaInP intermediate layer of a second conductivity type (not shown), and a GaP window layer 16 of a second conductivity type are sequentially grown on the sacrificial layer 12 to prepare an epitaxial wafer 20 having a light emitting device structure as a semiconductor functional layer (epitaxial functional layer) 18. Here, the first cladding layer 13 to the second cladding layer 15 are referred to as a double hetero (DH) structure portion (FIG. 1). Note that the material of the semiconductor functional layer (epitaxial functional layer) 18 is not limited to these. The semiconductor functional layer 18 may have a light emitting element structure as described above, and in this case, the method for manufacturing a bonded semiconductor wafer of the present invention may be particularly suitably applied.
[0030] 2, a selective etching method is used to form an isolation trench 21 so as to expose the sacrificial layer 12 in a partial region of the epitaxial wafer 20. More specifically, a mask is formed by photolithography, and etching (selective etching) is performed from the GaP window layer 16 to at least the first cladding layer 13 to form the isolation trench 21 (FIG. 2).
[0031] 2 shows a state in which the sacrificial layer 12 is exposed (exposed portion 12a) and not etched, but the present invention is not limited to this state. For example, the sacrificial layer 12 may be etched across the element isolation pattern, and the depth of the etching groove may reach the starting substrate 11. Even in this state, the sacrificial layer 12 is exposed as a part of the side surface of the element isolation pattern. The present invention can also be applied in this case.
[0032] Next, as shown in Fig. 3, a passivation film 22 is formed on at least the surface (exposed portion 12a) of the element isolation trench 21 where the sacrificial layer 12 is exposed. More specifically, as shown in Fig. 3, a passivation (PSV) film 22 such as SiO2 (silicon oxide film) can be formed on the surface constituting the outermost surface of the wafer (the surface of the window layer 16 in the case of Fig. 3) and inside the element isolation trench 21 (Fig. 3).
[0033] Next, as shown in FIG. 4, a PSV pattern substrate is prepared in which the passivation film 22 in the region other than the inside of the element isolation trench 21 is removed (FIG. 4).
[0034] By forming the passivation film 22 in the element isolation groove 21 in this manner, it is possible to prevent the bonding material from seeping into the element isolation groove 21 when bonding a bonded substrate (bonded wafer) via the bonding material, as described below, and to prevent the groove from being blocked by the bonding material, thereby preventing the etching of the sacrificial layer.
[0035] Next, as shown in FIGS. 5 and 6, the epitaxial layer having the semiconductor functional layer 18 of the epitaxial wafer 20 and the bonded substrate 31 transparent to visible light are bonded via a thermosetting bonding material 24 to produce a bonded substrate 30. More specifically, first, as shown in FIG. 5, benzocyclobutene (BCB) is spin-coated as a thermosetting bonding material on the epitaxial wafer (FIG. 5). Next, as shown in FIG. 6, the epitaxial wafer is stacked against a bonded substrate 31, such as a sapphire wafer, and bonded by thermocompression to produce a bonded substrate (epitaxial bonded substrate) 30 in which the epitaxial wafer 20 and the sapphire wafer 31 are bonded via the thermosetting bonding material 24 (BCB) (FIG. 6). When applying the thermosetting bonding material (BCB) by spin-coating, it is preferable that the designed film thickness is 0.01 μm or more and 0.6 μm or less. The thermosetting bonding material 24 may not be thermally cured. If the thermosetting bonding material 24 is not thermally cured, it can be easily peeled off when peeling is performed.
[0036] The bonded substrate 31 is not limited to sapphire, and any material can be selected as long as it is flat and has a low absorptivity of the excimer laser light. In addition to sapphire, synthetic quartz, quartz (natural quartz), glass, SiC, LiTaO3, and LiNbO3 can be selected.
[0037] The thermosetting bonding material 24 is not limited to BCB, and any material having thermosetting properties can be selected. In addition to BCB, silicone resin, epoxy resin, spin-on-glass (SOG), polyimide (PI), fluororesin, etc. may be used. As the fluororesin, amorphous fluororesin such as Cytop (registered trademark) can be used.
[0038] Next, as shown in Fig. 7, the passivation film 22 of the bonded substrate 30 is removed by etching. More specifically, the passivation film 22 can be etched with, for example, a fluorine-based solution (Fig. 7). In the example of Fig. 7, the etching solution is supplied from a direction nearly perpendicular to the paper surface. This etching removes the passivation film 22, revealing the element isolation grooves 21.
[0039] Next, as shown in FIG. 8, an etching solution is supplied to the element isolation groove 21 of the bonded substrate 30 to etch the sacrificial layer 12, thereby separating the starting substrate 11 from the epitaxial layer (having the semiconductor functional layer 18). More specifically, the starting substrate 11 can be peeled off by etching the sacrificial layer 12 with a fluorine-based solution (FIG. 8). Although the passivation film removal step and the sacrificial layer etching step are described as separate steps as shown in FIG. 7 and FIG. 8, they can be performed as a series of steps by selecting materials that can be selectively etched with a fluorine-based solution for both the passivation film 22 and the sacrificial layer 12. The material that can be selectively etched with a fluorine-based solution as the passivation film 22 is, for example, SiO2 as described above. The material that can be selectively etched with a fluorine-based solution as the sacrificial layer 12 is, for example, GaInP or GaAs as described above.
[0040] In this manner, a bonded semiconductor wafer 35 can be manufactured. The bonded semiconductor wafer 35 shown in Fig. 8 can be used for a micro LED. Furthermore, electrodes and the like of each element can be formed subsequently as follows.
[0041] First, as shown in FIG. 9, a part of the second cladding layer 15 is exposed by photolithography (FIG. 9).
[0042] Next, as shown in FIG. 10, a passivation (PSV) film 42 such as SiO2 is formed on the surface to cover the ends of the element isolation trenches 21 and the sides of the exposed active layer 14, and a PSV pattern film is produced that is processed so that parts of the first cladding layer 13 and the second cladding layer 15 are exposed (FIG. 10).
[0043] Next, as shown in FIG. 11, an electrode 44 is formed on the exposed portion of the passivation film 42, and a heat treatment is performed to realize an ohmic contact (FIG. 11).
[0044] [Second embodiment] Next, a second embodiment of the present invention will be described. First, similarly to the first embodiment, epitaxial growth is performed in sequence on a starting substrate 11 to form each layer, and an epitaxial wafer 20 having an epitaxial layer including a sacrificial layer 12 and a semiconductor functional layer 18 is produced. More specifically, the epitaxial growth of each layer can be performed as follows.
[0045] First, as shown in FIG. 12, a sacrificial layer 12 is epitaxially grown on a starting substrate 11 made of, for example, GaAs of a first conductivity type. The sacrificial layer 12 can be formed, for example, by stacking a GaAs buffer layer of a first conductivity type, and then growing a GaInP first etch stop layer of a first conductivity type and a GaAs second etch stop layer of a first conductivity type. Furthermore, for example, an AlGaInP first cladding layer 13 of a first conductivity type, a non-doped AlGaInP active layer 14, an AlGaInP second cladding layer 15 of a second conductivity type, a GaInP intermediate layer of a second conductivity type (not shown), and a GaP window layer 16 of a second conductivity type are sequentially grown on the sacrificial layer 12 to prepare an epitaxial wafer 20 having a light emitting device structure as a semiconductor functional layer (epitaxial functional layer) 18. Here, the first cladding layer 13 to the second cladding layer 15 are referred to as a double hetero (DH) structure portion (FIG. 12). Note that the material of the semiconductor functional layer (epitaxial functional layer) 18 is not limited to these. The semiconductor functional layer 18 may have a light emitting element structure as described above.
[0046] Next, as shown in Fig. 13, a selective etching method is used to form an isolation trench 21 so that the sacrificial layer 12 is exposed in a partial region of the epitaxial wafer 20. More specifically, a mask is formed by photolithography, and etching (selective etching) is performed from the GaP window layer 16 to at least the first cladding layer 13 to form the isolation trench 21 (Fig. 13). As a result, the sacrificial layer 12 is exposed (exposed portion 12a).
[0047] Next, as shown in FIG. 14, for example, benzocyclobutene (BCB) is spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material (FIG. 14), and heat is applied at 250° C. for 1 hour to harden the BCB film (in the figure, the hardened thermosetting bonding material is shown as hardened bonding material 25).
[0048] Next, as shown in FIG. 15, a part of the hardened bonding material (hardened BCB portion) 25 in the element isolation trench 21 is removed by photolithography to form an opening 26, thereby exposing the exposed portion 12a of the sacrificial layer 12 (FIG. 15).
[0049] Next, a passivation (PSV) film 22 such as SiO2 is formed on the surface as shown in FIG. 16 (FIG. 16), and a PSV pattern substrate is produced in which the passivation film 22 in areas other than the element isolation grooves 21 is removed as shown in FIG. 17 (FIG. 17).
[0050] Next, as shown in FIG. 18, benzocyclobutene (BCB) is spin-coated onto the epitaxial wafer as a thermosetting bonding material 24 (FIG. 18).
[0051] 19, the epitaxial wafer 20 and the sapphire wafer 31 are placed face to face with each other and bonded together by thermocompression to produce a bonded substrate (epitaxial bonded substrate) 50 in which the epitaxial wafer 20 and the sapphire wafer 31 are bonded together via a thermosetting bonding material 24 (BCB) (FIG. 19). When applying the thermosetting bonding material (BCB) by spin coating, the designed thickness is preferably 0.01 μm or more and 0.6 μm or less.
[0052] The bonded substrate 31 is not limited to sapphire, and any material can be selected as long as it is flat and has a low absorptivity of the excimer laser light. In addition to sapphire, synthetic quartz, quartz (natural quartz), glass, SiC, LiTaO3, and LiNbO3 can be selected.
[0053] The thermosetting bonding material 24 is not limited to BCB, and any material having thermosetting properties may be selected. In addition to BCB, silicone resin, epoxy resin, spin-on-glass (SOG), polyimide (PI), fluororesin, etc. may be used.
[0054] Next, as shown in Fig. 20, the passivation film 22 of the bonded substrate 50 is removed by etching. More specifically, for example, the passivation film 22 can be etched with a fluorine-based solution (Fig. 20). In the example of Fig. 20, the etching solution is supplied from a direction nearly perpendicular to the paper surface. This etching removes the passivation film 22, and the element isolation grooves 21 appear.
[0055] Next, as shown in Fig. 21, an etching solution is supplied to the element isolation groove 21 of the bonded substrate 50 to etch the sacrificial layer 12, thereby separating the starting substrate 11 from the epitaxial layer (having the semiconductor functional layer 18). More specifically, as shown in Fig. 21, the sacrificial layer 12 is etched with a fluorine-based solution to peel off the starting substrate 11 (Fig. 21). Note that, as shown in Figs. 21 and 22, the passivation film removal step and the sacrificial layer etching step are described as separate steps, but by selecting materials that are selectively etched with a fluorine-based solution for both the passivation film 22 and the sacrificial layer 12, these steps can be performed as a series of steps.
[0056] In this manner, a bonded semiconductor wafer 55 can be manufactured. The bonded semiconductor wafer 55 shown in Fig. 21 can be used for a micro LED. Furthermore, electrodes and the like of each element can be formed subsequently as follows.
[0057] First, a part of the second cladding layer 15 is exposed by photolithography as shown in Fig. 22. Then, as shown in Fig. 23, the spike-shaped hardened bonding material 25 (BCB hardened portion) is physically removed by a method such as lift-off (Fig. 23). Here, the hardened bonding material is subjected to a pressure of 5 kgf / cm. 2The spike-shaped hardened bonding material 25 (BCB hardened portion) can be removed with a liquid flow of about 1000 psi, but this method is not limited to this, and an ashing method or an RIE (reactive ion etching) method may also be used. In the ashing method or RIE method, the hardened bonding material 25 (BCB hardened film) is isotropically corroded, but the spike-shaped BCB hardened portion is corroded faster than the film-shaped BCB hardened portion, so if the time conditions are right, it is possible to remove only the spike-shaped BCB hardened portion.
[0058] Next, as shown in Figure 24, a passivation (PSV) film 42 such as SiO2 is formed on the surface to cover the exposed side of the active layer 14, and a PSV pattern film is produced that is processed so that parts of the first cladding layer 13 and second cladding layer 15 are exposed (Figure 24).
[0059] Next, as shown in FIG. 25, an electrode 44 is formed on the exposed portion of the passivation film 42, and a heat treatment is performed to realize an ohmic contact (FIG. 25).
[0060] [Third embodiment] Next, a third embodiment of the present invention will be described. First, similarly to the first and second embodiments, epitaxial growth is performed in sequence on a starting substrate 11 to form each layer, and an epitaxial wafer 20 having an epitaxial layer including a sacrificial layer 12 and a semiconductor functional layer 18 is produced. More specifically, the epitaxial growth of each layer can be performed as follows.
[0061] First, as shown in FIG. 26, a sacrificial layer 12 is epitaxially grown on a starting substrate 11 made of, for example, GaAs of a first conductivity type. The sacrificial layer 12 can be formed, for example, by stacking a GaAs buffer layer of a first conductivity type, and then growing a GaInP first etch stop layer of a first conductivity type and a GaAs second etch stop layer of a first conductivity type. Furthermore, for example, an AlGaInP first cladding layer 13 of a first conductivity type, a non-doped AlGaInP active layer 14, an AlGaInP second cladding layer 15 of a second conductivity type, a GaInP intermediate layer of a second conductivity type (not shown), and a GaP window layer 16 of a second conductivity type are sequentially grown on the sacrificial layer 12 to prepare an epitaxial wafer 20 having a light emitting device structure as a semiconductor functional layer (epitaxial functional layer) 18. Here, the first cladding layer 13 to the second cladding layer 15 are referred to as a double hetero (DH) structure portion (FIG. 26). Note that the material of the semiconductor functional layer (epitaxial functional layer) 18 is not limited to these. The semiconductor functional layer 18 may have a light emitting element structure as described above.
[0062] Next, as shown in Fig. 27, a selective etching method is used to form an isolation trench 21 so that the sacrificial layer 12 is exposed in a partial region of the epitaxial wafer 20. More specifically, a mask is formed by photolithography, and etching (selective etching) is performed from the GaP window layer 16 to at least the first cladding layer 13 to form the isolation trench 21 (Fig. 27). As a result, the sacrificial layer 12 is exposed (exposed portion 12a).
[0063] Next, as shown in Fig. 28, for example, benzocyclobutene (BCB) is spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material (Fig. 28), and heat is applied at 250°C for 1 hour to harden the BCB film (in the figure, the hardened thermosetting bonding material is shown as hardened bonding material 25). Note that, as a general tendency, when the aspect ratio of the width, depth, etc. of the element isolation trench 21 is greater than 0.1 (deep), the BCB does not reach the bottom of the element isolation trench, and a part of the DH structure and the sacrificial layer 12 are exposed at the bottom of the element isolation trench 21.
[0064] Next, as shown in FIG. 29, a part of the hardened bonding material 25 (hardened BCB portion) in the element isolation trench 21 is removed by photolithography to form an opening 26, thereby exposing the sacrificial layer 12 (FIG. 29).
[0065] Next, as shown in Figure 30, a passivation (PSV) film 22 such as SiO2 is formed on the surface (Figure 30), and then, as shown in Figure 31, the passivation film 22 in areas other than the element isolation grooves 21 is removed to produce a PSV pattern substrate (Figure 31).
[0066] Next, as shown in Fig. 32, for example, benzocyclobutene (BCB) is spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material 24 (Fig. 32), and then, as shown in Fig. 33, a bonded substrate 31, for example, a sapphire wafer, is placed face-to-face and thermocompressed to produce a bonded substrate (epitaxial bonded substrate) 60 in which the epitaxial wafer 20 and the sapphire wafer 31 are bonded via the thermosetting bonding material (BCB). When applying the thermosetting bonding material (BCB) by spin-coating, the designed film thickness is preferably 0.01 μm or more and 0.6 μm or less (Fig. 33).
[0067] The bonded substrate 31 is not limited to sapphire, and any material can be selected as long as it is flat and has a low absorptivity of excimer laser light. In addition to sapphire, synthetic quartz, quartz (natural quartz), glass, SiC, LiTaO3, and LiNbO3 can be selected.
[0068] The thermosetting bonding material 24 is not limited to BCB, and any material having thermosetting properties may be used. In addition to BCB, silicone resin, epoxy resin, spin-on-glass (SOG), polyimide (PI), fluororesin, etc. may be used.
[0069] Next, as shown in Fig. 34, the passivation film 22 of the bonded substrate 60 is removed by etching. More specifically, the passivation film 22 can be etched with, for example, a fluorine-based solution (Fig. 34). In the example of Fig. 34, the etching solution is supplied from a direction nearly perpendicular to the paper surface. This etching removes the passivation film 22, revealing the element isolation grooves 21.
[0070] Next, as shown in Fig. 35, an etching solution is supplied to the element isolation groove 21 of the bonded substrate 60 to etch the sacrificial layer 12, thereby separating the starting substrate 11 from the epitaxial layer (having the semiconductor functional layer 18). More specifically, as shown in Fig. 35, the sacrificial layer 12 is etched with a fluorine-based solution to peel off the starting substrate 11 (Fig. 35). Note that, as shown in Figs. 34 and 35, the passivation film removal step and the sacrificial layer etching step are described as separate steps, but by selecting materials that are selectively etched with a fluorine-based solution for both the passivation film 22 and the sacrificial layer 12, these steps can be performed as a series of steps.
[0071] In this manner, a bonded semiconductor wafer 65 can be manufactured. The bonded semiconductor wafer 65 shown in Fig. 35 can be used for a micro LED. Furthermore, electrodes and the like of each element can be formed subsequently as follows.
[0072] First, as shown in FIG. 36, a part of the second cladding layer 15 is exposed by photolithography (FIG. 36).
[0073] Next, as shown in FIG. 37, a passivation (PSV) film 42 such as SiO2 is formed on the surface to cover the ends of the element isolation trenches 21 and the side surfaces of the exposed active layer 14, and a PSV pattern film is fabricated so that parts of the first cladding layer 13 and the second cladding layer 15 are exposed (FIG. 37).
[0074] Next, as shown in FIG. 38, an electrode 44 is formed on the exposed portion of the passivation film 42, and a heat treatment is performed to realize an ohmic contact (FIG. 38).
[0075] [Fourth embodiment] Next, a fourth embodiment of the present invention will be described. First, similarly to the first to third embodiments, epitaxial growth is sequentially performed on a starting substrate 11 to form each layer, and an epitaxial wafer 20 having an epitaxial layer including a sacrificial layer 12 and a semiconductor functional layer 18 is produced. More specifically, the epitaxial growth of each layer can be performed as follows.
[0076] First, as shown in FIG. 39, a sacrificial layer 12 is epitaxially grown on a starting substrate 11 made of, for example, GaAs of a first conductivity type. The sacrificial layer 12 can be formed, for example, by stacking a GaAs buffer layer of a first conductivity type, and then growing a GaInP first etch stop layer of a first conductivity type and a GaAs second etch stop layer of a first conductivity type. Furthermore, for example, an AlGaInP first cladding layer 13 of a first conductivity type, a non-doped AlGaInP active layer 14, an AlGaInP second cladding layer 15 of a second conductivity type, a GaInP intermediate layer of a second conductivity type (not shown), and a GaP window layer 16 of a second conductivity type are sequentially grown on the sacrificial layer 12 to prepare an epitaxial wafer 20 having a light emitting device structure as a semiconductor functional layer (epitaxial functional layer) 18. Here, the first cladding layer 13 to the second cladding layer 15 are referred to as a double hetero (DH) structure portion (FIG. 39). Note that the material of the semiconductor functional layer (epitaxial functional layer) 18 is not limited to these. The semiconductor functional layer 18 may have a light emitting element structure as described above.
[0077] Next, as shown in Fig. 40, a selective etching method is used to form an isolation trench 21 so that the sacrificial layer 12 is exposed in a partial region of the epitaxial wafer 20. More specifically, a mask is formed by photolithography, and etching (selective etching) is performed from the GaP window layer 16 to at least the first cladding layer 13 to form the isolation trench 21 (Fig. 40). As a result, the sacrificial layer 12 is exposed (exposed portion 12a).
[0078] Next, as shown in FIG. 41, benzocyclobutene (BCB) is spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material (FIG. 41), and heat is applied at 250° C. for 1 hour to harden the BCB film (in the figure, the hardened thermosetting bonding material is shown as hardened bonding material 25).
[0079] Generally, when the aspect ratio of the width or depth of the element isolation trench 21 is greater than 0.1 (is deep), the element isolation trench is not completely filled with BCB.
[0080] Next, as shown in FIG. 42, a part of the hardened bonding material 25 (hardened BCB portion) in the element isolation trench 21 is removed by photolithography to form an opening 26, thereby exposing the sacrificial layer 12 (FIG. 42).
[0081] Next, as shown in Figure 43, a passivation (PSV) film 22 such as SiO2 is formed on the surface (Figure 43), and a PSV pattern substrate is produced in which the passivation film is removed from areas other than the element isolation grooves 21 as shown in Figure 44 (Figure 44).
[0082] Next, as shown in Fig. 45, for example, benzocyclobutene (BCB) is spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material 24 (Fig. 45), and then, as shown in Fig. 46, the epitaxial wafer 20 and the sapphire wafer, which is the substrate to be bonded, are placed face-to-face and thermocompressed to produce a bonded substrate (epitaxial bonded substrate) 70 in which the epitaxial wafer 20 and the sapphire wafer 31 are bonded via the thermosetting bonding material (BCB). When applying the thermosetting bonding material (BCB) by spin-coating, the designed film thickness is preferably 0.01 μm or more and 0.6 μm or less (Fig. 46).
[0083] The bonded substrate 31 is not limited to sapphire, and any material can be selected as long as it is flat and has a low absorptivity of excimer laser light. In addition to sapphire, synthetic quartz, quartz (natural quartz), glass, SiC, LiTaO3, and LiNbO3 can be selected.
[0084] The thermosetting bonding material 24 is not limited to BCB, and any material having thermosetting properties may be selected. In addition to BCB, silicone resin, epoxy resin, spin-on-glass (SOG), polyimide (PI), fluororesin, etc. may be used.
[0085] Next, as shown in Fig. 47, the passivation film 22 of the bonded substrate 70 is removed by etching. More specifically, the passivation film 22 can be etched with, for example, a fluorine-based solution (Fig. 47). In the example of Fig. 47, the etching solution is supplied from a direction nearly perpendicular to the paper surface. This etching removes the passivation film 22, revealing the element isolation trenches 21.
[0086] Next, as shown in Fig. 48, an etching solution is supplied to the element isolation groove 21 of the bonded substrate 70 to etch the sacrificial layer 12, thereby separating the starting substrate 11 from the epitaxial layer (having the semiconductor functional layer 18). More specifically, as shown in Fig. 48, the sacrificial layer 12 is etched with a fluorine-based solution to peel off the starting substrate 11 (Fig. 48). Note that, as shown in Figs. 47 and 48, the passivation film removal step and the sacrificial layer etching step are described as separate steps, but by selecting materials that are selectively etched with a fluorine-based solution for both the passivation film 22 and the sacrificial layer 12, these steps can be performed as a series of steps.
[0087] In this manner, a bonded semiconductor wafer 75 can be manufactured. The bonded semiconductor wafer 75 shown in Fig. 48 can be used for a micro LED. Furthermore, electrodes and the like of each element can be formed subsequently as follows.
[0088] First, as shown in FIG. 49, a part of the second cladding layer 15 is exposed by photolithography (FIG. 49).
[0089] Next, as shown in FIG. 50, the hardened bonding material 25 (BCB hardened portion) in the shape of a spike is physically removed by a method such as lift-off (FIG. 50). In the present embodiment, the spike-shaped BCB hardened portion can be removed by a liquid flow with a pressure of about 5 kgf / cm 2 although it is needless to say that the present invention is not limited to this method. An ashing method or an RIE method may be used. In the ashing method or the RIE method, the hardened bonding material 25 (BCB hardened film) is isotropically attacked. However, since the erosion rate of the spike-shaped BCB hardened portion is higher than that of the film-shaped BCB hardened portion, it is possible to remove only the spike-shaped BCB hardened portion by adjusting the time conditions.
[0090] Next, as shown in FIG. 51, a passivation (PSV) film 42 such as SiO2 is formed on the surface to cover the side surface of the exposed active layer 14, and a PSV pattern film is fabricated by processing so that a part of the first cladding layer 13 and the second cladding layer 15 is exposed (FIG. 51).
[0091] Next, as shown in FIG. 52, an electrode 44 is formed on the exposed portion of the passivation film 42, and heat treatment is performed to realize an ohmic contact (FIG. 52).
Example
[0092] Hereinafter, the present invention will be described in detail with reference to examples and comparative examples, but these do not limit the present invention.
[0093] (Example 1) First, as shown in FIG. 1, on a first-conductivity-type GaAs starting substrate 11, after laminating a first-conductivity-type GaAs buffer layer, a first-conductivity-type Ga x In 1-x P (0.4 ≦ x ≦ 0.6) first etch stop layer was epitaxially grown to 0.3 μm, and a first-conductivity-type GaAs second etch stop layer was epitaxially grown to 0.3 μm to form a sacrificial layer 12. Further, a first-conductivity-type (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) first cladding layer 13 was grown to 1.0 μm, and an undoped (Aly Ga 1-y ) x In 1-x P (0.4 ≤ x ≤ 0.6, 0 ≤ y ≤ 0.6) active layer 14, a second conductivity type (Al y Ga 1-y ) x In 1-x P (0.4 ≤ x ≤ 0.6, 0 < y ≤ 1) second cladding layer 15 was grown to a thickness of 1.0 μm, a second conductivity type GaInP intermediate layer (not shown) was grown to a thickness of 0.1 μm, and a second conductivity type GaP window layer 16 was grown to a thickness of 4 μm in sequence to prepare an epitaxial wafer 20 having a light-emitting element structure as a semiconductor functional layer (epitaxial functional layer) 18 (FIG. 1).
[0094] Next, a resist mask was formed by photolithography, and dry etching using chlorine-based plasma was performed to etch from the first cladding layer 13 to the GaP window layer 16 to form element isolation grooves 21 in an element isolation step (FIG. 2).
[0095] Next, an SiO2 film was formed as a passivation film 22 on the surface of the window layer 16 and inside the element isolation grooves 21 (FIG. 3), and the passivation film 22 (SiO2 film) in the region other than the element isolation grooves 21 was removed (FIG. 4).
[0096] Next, benzocyclobutene (BCB) was spin-coated as a thermosetting bonding material 24 on the epitaxial wafer 20 (FIG. 5), and it was overlapped with a sapphire wafer as a substrate to be bonded 31 and thermocompression bonded to bond the epitaxial wafer 20 and the sapphire wafer 31 via the BCB 24 to produce a bonded substrate (epitaxial bonded substrate) 30. When applying BCB by spin coating, the designed film thickness was 0.6 μm (FIG. 6). After reaching the temperature of 150 °C which is the softening point of BCB, the temperature was lowered to room temperature for bonding. Next, the SiO2 film inside the element isolation grooves 21 was etched with a fluorine-based solution (FIG. 7). Next, the sacrificial layer 12 was etched with a fluorine-based solution to peel off the GaAs starting substrate 11 (FIG. 8). Next, a resist mask was formed by photolithography, and a part of the second cladding layer 15 was exposed by dry etching using chlorine-based plasma (FIG. 9).
[0097] Next, an SiO2 film was formed as the passivation film 42 on the surface to cover the ends of the element isolation grooves 21 and the sides of the exposed active layer 14, and it was processed so that a part of the first cladding layer 13 and the second cladding layer 15 was exposed (FIG. 10).
[0098] Next, an AuBe alloy layer was provided as the electrode 44 in a region 0.1 μm near the P-type layer and an AuGe alloy layer was provided in a region 0.2 μm near the N-type layer on the exposed portion of the SiO2 film which is the passivation film 42. Heat treatment was performed to achieve ohmic contact (FIG. 11).
[0099] (Example 2) First, as shown in FIG. 12, on a first-conductivity-type GaAs starting substrate 11, after laminating a first-conductivity-type GaAs buffer layer, a first-conductivity-type Ga x In 1-x P (0.4 ≦ x ≦ 0.6) first etch stop layer of 0.3 μm and a first-conductivity-type GaAs second etch stop layer of 0.3 μm were epitaxially grown to form the sacrificial layer 12. Further, a first-conductivity-type (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) first cladding layer 13 of 1.0 μm, an undoped (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 ≦ y ≦ 0.6) active layer 14, a second-conductivity-type (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) second cladding layer 15 of 1.0 μm, a second-conductivity-type GaInP intermediate layer (not shown) of 0.1 μm, and a second-conductivity-type GaP window layer 16 of 4 μm were sequentially grown to prepare an epitaxial wafer 20 having a light-emitting element structure as a semiconductor functional layer (epitaxial functional layer) 18 (FIG. 12).
[0100] Next, a resist mask was formed by photolithography, and a device isolation process was performed in which the first cladding layer 13 to the GaP window layer 16 were etched by dry etching using chlorine-based plasma to form device isolation grooves 21 (FIG. 13).
[0101] Next, benzocyclobutene (BCB) was spin-coated onto the epitaxial wafer 20 to supply BCB to the surface and inside the element isolation trenches 21 (FIG. 14), and heat was applied at 250° C. for 1 hour to harden the BCB film (hardened bonding material 25).
[0102] Next, a part of the hardened bonding material 25 (hardened BCB portion) in the element isolation trench 21 was removed by photolithography to expose the sacrificial layer 12 (FIG. 15).
[0103] Next, a SiO2 film was formed as a passivation film 22 on the surface of the window layer 16 and inside the element isolation trench 21 (FIG. 16), and the passivation film 22 (SiO2 film) in the region other than the element isolation trench 21 was removed (FIG. 17).
[0104] Next, benzocyclobutene (BCB) was spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material 24 (FIG. 18), and then the epitaxial wafer 20 was placed face-to-face with a sapphire wafer, which was a substrate to be bonded 31, and then thermocompression-bonded to produce a bonded substrate (epitaxially bonded substrate) 50 in which the epitaxial wafer 20 and the sapphire wafer 31 were bonded via the BCB 24. When applying BCB by spin-coating, the designed film thickness was 0.6 μm (FIG. 19).
[0105] Next, the passivation film 22 (SiO2 film) inside the element isolation trench 21 was etched with a fluorine-based solution (FIG. 20).
[0106] Next, the sacrificial layer 12 was etched with a fluorine-based solution to peel off the GaAs starting substrate 11 (FIG. 21). A resist mask was formed by photolithography, and a part of the second cladding layer 15 was exposed by dry etching using chlorine-based plasma (FIG. 22).
[0107] Next, the spike-shaped cured bonding material 25 (BCB cured portion) was removed with a liquid flow at a pressure of about 5 kgf / cm 2 (Fig. 23).
[0108] An SiO2 film was formed as a passivation film 42 on the surface to cover the side surfaces of the exposed active layers 14, and the processing was performed such that a part of the first cladding layer 13 and the second cladding layer 15 was exposed (Fig. 24).
[0109] Next, an AuBe alloy layer was provided in a region 0.1 μm near the P-type layer and an AuGe alloy layer was provided in a region 0.2 μm near the N-type layer as electrodes 44 on the exposed portion of the SiO2 film which is the passivation film 42. Heat treatment was performed to realize ohmic contact (Fig. 25).
[0110] (Example 3) First, as shown in Fig. 26, on a first-conductivity-type GaAs starting substrate 11, after laminating a first-conductivity-type GaAs buffer layer, a first-conductivity-type Ga x In 1-x P (0.4 ≦ x ≦ 0.6) first etch stop layer of 0.3 μm and a first-conductivity-type GaAs second etch stop layer of 0.3 μm were epitaxially grown to form a sacrificial layer 12. Further, a first-conductivity-type (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) first cladding layer 13 of 1.0 μm, an undoped (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 ≦ y ≦ 0.6) active layer 14, a second-conductivity-type (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) second cladding layer 15 of 1.0 μm, a second-conductivity-type GaInP intermediate layer (not shown) of 0.1 μm, and a second-conductivity-type GaP window layer 16 of 4 μm were sequentially grown to prepare an epitaxial wafer 20 having a light-emitting element structure as a semiconductor functional layer (epitaxial functional layer) 18 (Fig. 26).
[0111] A resist mask was formed by photolithography, and a device isolation process was carried out in which the first cladding layer 13 to the GaP window layer 16 were etched by dry etching using chlorine-based plasma to form device isolation grooves 21 (FIG. 27).
[0112] Benzocyclobutene (BCB) was spin-coated onto the epitaxial wafer 20 to supply BCB to the surface and to a portion of the inside of the element isolation trench 21 (Figure 28), and the BCB film was hardened by applying heat at 250°C for 1 hour (hardened bonding material 25).
[0113] A resist mask was formed by photolithography, and a part of the hardened bonding material 25 (hardened BCB portion) in the element isolation trench 21 was removed by dry etching using fluorine-based plasma to expose the sacrificial layer 12 (FIG. 29).
[0114] Next, a SiO2 film was formed as a passivation film 22 on the surface of the window layer 16 and inside the element isolation trench 21 (FIG. 30), and the passivation film 22 (SiO2 film) in the region other than the element isolation trench 21 was removed (FIG. 31).
[0115] Next, benzocyclobutene (BCB) was spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material 24 (FIG. 32), and then the epitaxial wafer 20 was placed face-to-face with a sapphire wafer, which was a substrate to be bonded 31, and then thermocompression-bonded to produce a bonded substrate (epitaxially bonded substrate) 60 in which the epitaxial wafer 20 and the sapphire wafer 31 were bonded via the BCB 24. When applying BCB by spin-coating, the designed film thickness was 0.6 μm (FIG. 33).
[0116] Next, the passivation film 22 (SiO2 film) inside the element isolation trench 21 was etched with a fluorine-based solution (FIG. 34).
[0117] Next, the sacrificial layer 12 was etched with a fluorine-based solution to remove the GaAs starting substrate 11 (FIG. 35).
[0118] Next, a resist mask was formed, and a part of the second cladding layer 15 was exposed by a dry etching method using chlorine-based plasma (Fig. 36).
[0119] An SiO2 film was formed as a passivation film 42 on the surface, covering the end of the element isolation groove 21 and the side surface of the exposed active layer 14, and processing was performed so that a part of the first cladding layer 13 and the second cladding layer 15 was exposed (Fig. 37).
[0120] Next, an AuBe alloy layer was provided in a region 0.1 μm near the P-type layer and an AuGe alloy layer was provided in a region 0.2 μm near the N-type layer as the electrode 44 on the exposed portion of the SiO2 film which is the passivation film 42. Heat treatment was performed to realize an ohmic contact (Fig. 38).
[0121] (Example 4) First, as shown in Fig. 39, on a GaAs starting substrate 11 of the first conductivity type, after laminating a GaAs buffer layer of the first conductivity type, Ga x In 1-x P (0.4 ≦ x ≦ 0.6) first etch stop layer of 0.3 μm and a GaAs second etch stop layer of the first conductivity type of 0.3 μm were epitaxially grown to form a sacrificial layer 12. Further, (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) first cladding layer 13 of 1.0 μm, undoped (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 ≦ y ≦ 0.6) active layer 14, (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) second cladding layer 15 of 1.0 μm, a second conductivity type GaInP intermediate layer (not shown) of 0.1 μm, and a second conductivity type GaP window layer 16 of 4 μm were sequentially grown to prepare an epitaxial wafer having a light-emitting element structure as a semiconductor functional layer (epitaxial functional layer) 18 (Fig. 39).
[0122] A resist mask was formed by photolithography, and a device isolation process was carried out in which the first cladding layer 13 to the GaP window layer 16 were etched by dry etching using chlorine-based plasma to form device isolation grooves 21 (FIG. 40).
[0123] Benzocyclobutene (BCB) was spin-coated onto the epitaxial wafer 20 to supply BCB to the surface and the inside (wall surface) of the element isolation trench 21 (Figure 41), and heat was applied at 250°C for 1 hour to harden the BCB film (hardened bonding material 25).
[0124] A resist mask was formed by photolithography, and a part of the hardened bonding material 25 (hardened BCB portion) in the element isolation trench was removed by dry etching using fluorine-based plasma to expose the sacrificial layer 12 (FIG. 42).
[0125] Next, a SiO2 film was formed as a passivation film 22 on the surface of the window layer 16 and on the element isolation trench 21 so as to cover the sacrificial layer 12 (Figure 43), and the passivation film 22 (SiO2 film) in the area other than the element isolation trench 21 was removed (Figure 44).
[0126] Next, benzocyclobutene (BCB) was spin-coated onto the epitaxial wafer 20 as a thermosetting bonding material 24 to supply BCB to the surface and part of the inside of the element isolation groove 21 (FIG. 45), and then the epitaxial wafer 20 was placed face-to-face with a sapphire wafer, which was the substrate to be bonded 31, and bonded by thermocompression to produce a bonded substrate (epitaxial bonded substrate) 70 in which the epitaxial wafer 20 and the sapphire wafer 31 were bonded via the BCB 24. When applying BCB by spin-coating, the designed film thickness was 0.6 μm (FIG. 46).
[0127] Next, the passivation film 22 (SiO2 film) inside the element isolation trench 21 was etched with a fluorine-based solution (FIG. 47).
[0128] Next, the sacrificial layer 12 was etched with a fluorine-based solution to remove the GaAs starting substrate 11 (FIG. 48).
[0129] Next, a resist mask was formed, and a part of the second cladding layer 15 was exposed by a dry etching method using chlorine-based plasma (Fig. 49).
[0130] The spiky BCB cured part was removed by a liquid flow with a pressure of about 5 kgf / cm 2 (Fig. 50).
[0131] An SiO2 film was formed as a passivation film 42 on the surface to cover the side surface of the exposed active layer, and it was processed so that a part of the first cladding layer 13 and the second cladding layer 15 was exposed (Fig. 51).
[0132] Next, an AuBe alloy layer was provided in a region 0.1 μm near the P-type layer and an AuGe alloy layer was provided in a region 0.2 μm near the N-type layer as the electrode 44 on the exposed part of the SiO2 film which is the passivation film 42. Heat treatment was performed to achieve ohmic contact (Fig. 52).
[0133] (Comparative Example) As shown in Fig. 53, on a GaAs starting substrate 111 of the first conductivity type, after laminating a GaAs buffer layer of the first conductivity type, a first conductivity type Ga x In 1-x P (0.4 ≦ x ≦ 0.6) first etch stop layer of 0.3 μm and a first conductivity type GaAs second etch stop layer of 0.3 μm were epitaxially grown to form a sacrificial layer 112. Further, a first conductivity type (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) first cladding layer 113 of 1.0 μm, a non-doped (Al y Ga 1-y ) x In 1-x P (0.4 ≦ x ≦ 0.6, 0 ≦ y ≦ 0.6) active layer 114, a second conductivity type (Al y Ga 1-y ) x In 1-xAn epitaxial wafer 120 having a light-emitting element structure as a semiconductor functional layer (epitaxial functional layer) 118 in which a second cladding layer 115 of P(0.4 ≦ x ≦ 0.6, 0 < y ≦ 1) was grown by 1.0 μm, a second-conductivity-type GaInP intermediate layer (not shown) was grown by 0.1 μm, and a second-conductivity-type GaP window layer 116 was grown by 4 μm in sequence was prepared (Fig. 53).
[0134] A device isolation step of forming a resist mask by photolithography and etching from the first cladding layer 113 to the GaP window layer 116 by a dry etching method using chlorine-based plasma to form a device isolation groove 121 was performed (Fig. 54). As a result, the surface 112a of the sacrificial layer 112 was exposed.
[0135] Next, BCB 122 was spin-coated on the sapphire wafer 131 (Fig. 55), and it was superposed so as to face the epitaxial wafer on which the device isolation groove 121 was formed, and heat-bonded to fabricate an epitaxial bonded substrate in which the epitaxial wafer and the sapphire wafer were bonded via BCB. When applying BCB by spin coating, the designed film thickness was 0.6 μm (Fig. 56).
[0136] At the time of bonding, since the amount of the BCB bonding agent 122 that enters the device isolation groove 121 cannot be controlled, there is a partially filled portion, while there is also a region where the BCB bonding agent 122 fills up to the exposed surface of the sacrificial layer 112 (see Fig. 56).
[0137] The sacrificial layer 112 was removed by wet etching to separate the GaAs starting substrate 111 and the epitaxial layer. Since the sacrificial layer etchant does not enter the portion where the BCB bonding agent 122 filled the device isolation groove 121, the sacrificial layer 112 was not etched and remained partially (Fig. 57). The partially remaining sacrificial layer is indicated by reference numeral 162.
[0138] When the GaAs starting substrate 111 was peeled off from the epitaxial layer, a part of the GaAs starting substrate 111 at the portion where the sacrificial layer 112 was not etched remained (Fig. 58). A part of the starting substrate that remained partially is indicated by reference numeral 161.
[0139] Next, a part of the BCB 122 filling the element isolation trench 121 was removed to form an isolation trench (FIG. 59).
[0140] A portion of the first cladding layer 113 and the active layer 114 was removed to expose the second cladding layer 115 (FIG. 60). After the second cladding layer 115 was exposed, the spike-shaped BCB bonding agent 122 was selectively removed by a lift-off technique (FIG. 61). Next, a SiO2 film was formed on the surface as a passivation film 42 to cover the element isolation edge and the side surface of the exposed active layer 114, and processing was performed so that a portion of the first cladding layer 113 and the second cladding layer 115 was exposed (FIG. 62). At this time, a portion 192 of the SiO2 film was attached to the remaining starting substrate 161.
[0141] Next, an AuBe alloy layer was provided in a region 0.1 μm from the P-type layer and an AuGe alloy layer was provided in a region 0.2 μm from the N-type layer as an electrode 144 on the exposed SiO2 film. An ohmic contact was achieved by heat treatment (FIG. 63). At this time, a part 194 of the electrode material was attached to the remaining starting substrate 161.
[0142] (Comparison between Examples and Comparative Examples) After etching the sacrificial layer, the area where the starting substrate (GaAs) does not adhere to the epitaxial layer and the epitaxial layer and the starting substrate are completely separated is defined as the non-defective area, and the ratio to the designed area is the yield. Figure 64 shows a comparison between the embodiment and the comparative example.
[0143] figure 64 As can be seen from the graph, in the cases of the examples, the peeled non-defective area is 90% or more. On the other hand, in the comparative example, the yield is significantly reduced. This difference in yield is also due to the difference in the sacrificial layer etching time due to the presence of an element isolation groove. In all of the examples in which an isolation groove is provided, the sacrificial layer etching time is within one hour. On the other hand, in the comparative example, the sacrificial layer etching time takes several tens of hours at room temperature.
[0144] In the embodiment, since the etching solution easily penetrates through the element isolation trenches, etching proceeds simultaneously over the entire surface of the wafer, so that uneven distribution of stress during the etching of the sacrificial layer is small and the epitaxial layer is not easily damaged, resulting in a good yield after etching the sacrificial layer.
[0145] On the other hand, in the comparative example, since etching proceeds from the outer periphery of the wafer, uneven stress during the sacrificial layer etching process is likely to be applied to the epitaxial layer, which makes the epitaxial layer prone to cracks and the like, resulting in a decrease in yield.
[0146] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0147] 11...Starting substrate, 12...sacrificial layer; 12a...exposed surface of sacrificial layer; 13...first cladding layer, 14...active layer, 15...second cladding layer, 16...window layer, 18...semiconductor functional layer, 20...epitaxial wafer, 21: element isolation groove; 22: passivation film; 24: thermosetting bonding material; 25...hardened bonding material; 26...opening of thermosetting bonding material; 30...bonded substrate, 31...substrate to be bonded, 35...bonded semiconductor wafer 42...passivation film, 44...electrode, 50...bonded substrate, 55...bonded semiconductor wafer, 60...bonded substrate, 65...bonded semiconductor wafer, 70...bonded substrate, 75...bonded semiconductor wafer.
Claims
1. epitaxially growing a sacrificial layer on a starting substrate; producing an epitaxial wafer by epitaxially growing an epitaxial layer having a semiconductor functional layer on the sacrificial layer; forming an isolation trench by selective etching in a portion of the epitaxial wafer such that the sacrificial layer is exposed; forming a passivation film on at least a surface of the element isolation trench where the sacrificial layer is exposed; a step of bonding the epitaxial layer of the epitaxial wafer to a bonded substrate that is transparent to visible light via a thermosetting bonding material to produce a bonded substrate; removing the passivation film of the bonding substrate by etching; supplying an etching solution to the element isolation groove of the bonded substrate to etch the sacrificial layer, thereby separating the starting substrate from the epitaxial layer; A method for producing a bonded semiconductor wafer, comprising the steps of:
2. The substrate to be bonded is made of sapphire, synthetic quartz, quartz, glass, SiC, LiTaO 3 , LiNbO 3 2. The method for producing a junction type semiconductor wafer according to claim 1, wherein the material is any one of the materials listed above.
3. 3. The method for producing a bonded semiconductor wafer according to claim 1, wherein the thermosetting bonding material is one or more of the following materials: silicone resin, epoxy resin, benzocyclobutene, spin-on glass, polyimide, and fluororesin.
4. 4. The method for producing a bonded semiconductor wafer according to claim 1, wherein the thickness of the thermosetting bonding material is 0.01 μm or more and 0.6 μm or less.
5. 5. The method for producing a bonded semiconductor wafer according to claim 1, wherein the thermosetting bonding material is not heat-cured.
6. 6. The method for producing a junction type semiconductor wafer according to claim 1, wherein the passivation film is a silicon oxide film.
7. 7. The method for producing a junction type semiconductor wafer according to claim 1, wherein the junction type semiconductor wafer is used for a micro LED.
Citation Information
Patent Citations
Method for manufacturing semiconductor device
JP2013004632A
Temporary bonding method of semiconductor substrate
JP2021027301A
Method for manufacturing composite substrate and method for manufacturing semiconductor crystal layer formation substrate
WO2014020906A1
Method for provisionally bonding semiconductor substrate
WO2021024768A1