Anode active material, anode, and secondary battery
A mixed silicon oxide powder composition with varying particle sizes and a carbon material addresses the inefficiencies of pre-doped silicon oxide in lithium-ion batteries, achieving improved initial efficiency and discharge capacity retention.
Patent Information
- Application Number
- JP2020215189
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-25
- Filing Date
- 2020-12-24
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Existing silicon-based negative electrode materials for lithium-ion secondary batteries face challenges in achieving high initial efficiency and maintaining discharge capacity and cycle characteristics, particularly when pre-doped with alkali or alkaline earth metals.
A combination of a first silicon oxide powder doped with an alkali or alkaline earth metal and a second undoped silicon oxide powder, along with a carbon material, is used to form a negative electrode active material, where the first powder has larger particle sizes and the second powder has smaller particle sizes, with specific weight ratios to optimize performance.
This approach enhances both the initial efficiency and discharge capacity retention rate of the battery, improving upon the limitations of using pre-doped silicon oxide alone.
Smart Images

Figure 0007556779000005 
Figure 0007556779000006 
Figure 0007556779000004
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to a negative electrode active material, a negative electrode, and a secondary battery. [Background technology]
[0002] With the increasing technological development and demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among such secondary batteries, lithium-ion secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, are commercially available and widely used. Currently, research is being actively conducted to increase the capacity of such lithium-ion secondary batteries.
[0003] Silicon-based materials such as silicon alloys and silicon oxide have a theoretical capacity density greater than that of carbon-based materials such as graphite, which are currently mainstream, and are therefore expected to be used as negative electrode materials to improve the energy density of lithium-ion secondary batteries. For example, SiO x The discharge capacity on the first discharge is 1700mAh / g or more, which is about five times that of graphite.
[0004] However, SiO x When silicon-based materials such as these are used as the negative electrode active material, there is a problem that the initial efficiency of the battery (i.e., the ratio of the discharge capacity to the charge capacity at the first charge and discharge) is lower than that of graphite. On the other hand, it is known that the initial efficiency is improved when silicon oxide powder pre-doped with Li or Mg is used as the negative electrode active material. However, there is a problem that such pre-doping may deteriorate the discharge capacity and cycle characteristics. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-114820 A
[0006] [Patent Document 2] International Publication No. 2015 / 059859
[0007] [Patent Document 3] JP 2017-188319 A
[0008] [Patent Document 4] JP 2012-33317 A Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a negative electrode active material for a secondary battery, a negative electrode, and a secondary battery that can achieve both high initial efficiency and excellent discharge capacity and capacity retention rate. [Means for solving the problem]
[0010] According to one aspect of the present invention, a first silicon oxide powder doped with at least one of an alkali metal and an alkaline earth metal; an undoped silicon dioxide powder; Including, The second silicon oxide powder is amorphous. A negative electrode active material for a secondary battery is provided.
[0011] In the negative electrode active material according to the above embodiment, the average particle size of the particles constituting the first silicon oxide powder may be larger than the average particle size of the particles constituting the second silicon oxide powder.
[0012] In the negative electrode active material according to the above embodiment, the particles constituting the first silicon oxide powder may have an average particle size of 3 μm or more and 15 μm or less, and the particles constituting the second silicon oxide powder may have an average particle size of 0.5 μm or more and 2 μm or less.
[0013] In the negative electrode active material according to the above embodiment, the weight ratio of the second silicon oxide powder to the first silicon oxide powder may be 0.2 or more.
[0014] In the negative electrode active material according to the above embodiment, the weight ratio of the second silicon oxide powder to the first silicon oxide powder may be less than 10.
[0015] In the negative electrode active material according to the above embodiment, the first silicon oxide powder may contain silicon microcrystals having a crystallite size of 5 nm or more and 30 nm or less.
[0016] In the negative electrode active material according to the above embodiment, the first silicon oxide powder may contain at least one of Li2SiO3, Li2Si2O5, Li4SiO4, and Mg2SiO4.
[0017] The negative electrode active material according to the above embodiment may further contain a carbon material powder containing one or a mixture of two or more of natural graphite, artificial graphite, graphitized carbon fiber, and amorphous carbon.
[0018] According to another aspect of the present invention, there is provided a negative electrode for a secondary battery, in which a negative electrode active material layer containing the negative electrode active material according to the above aspect is formed on a negative electrode current collector.
[0019] According to another aspect of the present invention, there is provided a secondary battery comprising the negative electrode according to the above aspect. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a diagram in which the initial capacity, initial efficiency, and capacity retention rate are plotted against the weight ratio of the first silicon oxide powder A to the second silicon oxide powder B for Example 1, Example 2, Comparative Example 1, and Comparative Example 2. [Diagram 2] FIG. 1 is a graph in which the initial capacity, initial efficiency, and capacity retention rate are plotted against the weight ratio of the first silicon oxide powder A to the second silicon oxide powder B for Example 3, Comparative Example 3, and Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto.
[0022] In this specification, the term "average particle size" refers to the particle size at 50% of the cumulative value in the particle size distribution measured by a laser diffraction scattering method, i.e., the median diameter (D 50 ). In this specification, the term "silicon oxide powder" refers to a powder containing silicon oxide (which may contain elements other than silicon and oxygen) and in which the total content of silicon and oxygen is 80% by weight or more. In this specification, the symbol "~" is used to mean both ends of the range indicated by the description. For example, the description "1~2" means "1 or more and 2 or less."
[0023] SiO as a negative electrode active material to increase the capacity of lithium-ion secondary batteries x When silicon-based materials such as SiO are used, the initial efficiency tends to be lower than when graphite is used. The reason for this is presumed to be as follows. x During the initial charge, SiO can form a Li-Si alloy, which is a reversible component from which Li can be re-released, and can also form lithium silicate (lithium silicate) of one or more phases, which is an irreversible component from which Li cannot be re-released. Although this lithium silicate has the effect of suppressing the expansion of the silicon component in the negative electrode active material, such an irreversible component does not contribute to charge and discharge, which can lead to a decrease in initial efficiency. This leads to the formation of a Li-Si alloy, which is a reversible component from which Li can be re-released, and can also form lithium silicate of one or more phases, which is an irreversible component from which Li cannot be re-released. x The initial efficiency of SiO is about 65% to 70%, which is very low compared to the initial efficiency of graphite (about 90% to 95%). x When used alone as the negative electrode active material, it may be possible that the balance with the positive electrode active material is not achieved, resulting in wasteful consumption of the positive electrode active material, resulting in a decrease in energy density.
[0024] On the other hand, SiO x When silicon-based materials such as SiO 2 are pre-doped with Li or Mg, the initial efficiency improves as the amount of pre-doping increases, but the discharge capacity and cycle characteristics may deteriorate compared to when pre-doping is not performed. The reason for this is presumed to be as follows. When pre-doping is performed, the amount of Li or Mg in the undoped SiO 2 is reduced. xIn addition to the inherent irreversible components that occur when using SiO, complex silicon compounds such as lithium silicate phases may be formed, and excess lithium compounds may be formed on the surface of the particles of the negative electrode active material. This can result in a discharge capacity per unit weight that is greater than that of undoped SiO x In addition, the doping process can be significantly reduced compared to SiO x It is believed that the increased crystallinity of the silicon microcrystals contained therein leads to the occurrence of cracks on the particle surface or inside the particle and an increase in the expansion rate of the material due to repeated charging and discharging, making the material more susceptible to cycle degradation.
[0025] The present inventors have found that by using a mixture of a first silicon oxide powder pre-doped with an alkali metal or an alkaline earth metal and a second silicon oxide powder not doped as a negative electrode active material, it is possible to achieve both high initial efficiency and excellent discharge capacity. The present inventors have also found that by mixing the first silicon oxide powder and the second silicon oxide powder as described above, cycle characteristics are improved more than expected. Furthermore, the present inventors have found that by further adding a carbon material to the first silicon oxide powder and the second silicon oxide powder as described above, initial efficiency is improved more than expected.
[0026] [Nonaqueous electrolyte secondary battery] One embodiment of the present invention relates to a non-aqueous electrolyte secondary battery. The non-aqueous electrolyte secondary battery according to this embodiment includes a negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and a non-aqueous electrolyte. A specific example of the secondary battery is a lithium ion secondary battery having advantages such as high energy density, discharge voltage, and output stability.
[0027] The following description will be given mainly by taking a lithium ion secondary battery as an example, however, the present invention is not limited to lithium ion secondary batteries and can be applied to various non-aqueous electrolyte secondary batteries.
[0028] A lithium ion secondary battery according to an embodiment of the present invention includes a negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and a non-aqueous electrolyte. The lithium ion secondary battery may also include a battery case that houses an electrode assembly including the negative electrode, the positive electrode, and the separator, and a sealing member that seals the battery case.
[0029] [Negative electrode] The negative electrode includes a negative electrode current collector and a negative electrode active material layer formed on one or both surfaces of the negative electrode current collector. The negative electrode active material layer may be formed on the entire surface of the negative electrode current collector, or may be formed only on a portion of the surface.
[0030] (Negative electrode current collector) The negative electrode current collector used in the negative electrode is not particularly limited as long as it does not induce chemical changes in the battery and has electrical conductivity. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or the like, or an aluminum-cadmium alloy.
[0031] The negative electrode current collector may have a thickness of 3 μm to 500 μm. Fine irregularities may be formed on the surface of the negative electrode current collector to enhance adhesion to the negative electrode active material. The negative electrode current collector may have various forms, such as a film, a sheet, a foil, a net, a porous body, a foam, or a nonwoven fabric.
[0032] (Negative electrode active material layer) The negative electrode active material layer can be formed, for example, by applying a negative electrode active material slurry, in which a mixture of a negative electrode active material, a binder, and a conductive agent is dissolved or dispersed in a solvent, to a negative electrode current collector, followed by drying and rolling, or by casting the above-mentioned negative electrode active material slurry on another support, and then peeling the resulting film from the support and laminating it on the negative electrode current collector. The above-mentioned mixture can further contain a dispersant, a filler, and other optional additives, as necessary.
[0033] The negative electrode active material may be contained in an amount of 80% by weight or more and 99% by weight or less based on the total weight of the negative electrode active material layer.
[0034] (Negative electrode active material) In the lithium ion secondary battery according to the embodiment, the negative electrode active material may include a first silicon oxide powder A doped with at least one of an alkali metal and an alkaline earth metal and a second silicon oxide powder B not doped. Further, the negative electrode active material may further include a carbon material powder.
[0035] The first silicon oxide powder A is one in which at least one of an alkali metal and an alkaline earth metal is doped into the silicon oxide powder. That is, the particles constituting the first silicon oxide powder A may contain at least one of the doped alkali metal element and alkaline earth metal element. The first silicon oxide powder A includes, for example, silicon oxide SiO x (0 < x < 2), elemental silicon Si, elemental doped metal, silicate of doped metal, other silicon compounds, and compounds of doped metals, etc. may be included.
[0036] The silicon oxide powder used as the raw material before doping is, for example, a powder of SiO x . SiO x may have a structure in which Si fine particles are dispersed in an amorphous silicon oxide matrix in the form of microcrystals or amorphous. The ratio x of oxygen to silicon is 0 < x < 2, preferably 0.5 ≦ x ≦ 1.6, more preferably 0.8 ≦ x ≦ 1.5. For example, the raw material silicon oxide powder may be SiO (x = 1). Further, the raw material silicon oxide powder may contain only SiO x having a specific value of x, or may be a mixture of two or more SiO x powders having different x values.
[0037] The raw silicon oxide powder may have an amorphous structure that does not contain a crystalline phase, except for microcrystals such as silicon dispersed in the structure. The dispersed microcrystals may be of a size that does not appear as a diffraction peak in an X-ray diffraction (XRD) pattern, and the XRD pattern of the raw silicon oxide powder may not have a diffraction peak derived from a crystalline phase. In this specification, even if a material contains microcrystals microscopically, if no diffraction peaks are observed in the XRD pattern, it is described as "amorphous". Note that the XRD pattern of the raw silicon oxide powder may include a diffraction peak derived from the dispersed microcrystals.
[0038] The metal element to be doped is not particularly limited as long as it is an alkali metal or an alkaline earth metal. For example, one or more of lithium, sodium, potassium, magnesium, and calcium may be doped into the raw material silicon oxide powder, but is not limited thereto.
[0039] For example, when doped with lithium, the first silicon oxide powder A may contain fine particles of silicon or lithium silicate in its structure. For example, the first silicon oxide powder A may have a structure in which silicon or lithium silicate is dispersed in a microcrystalline or amorphous form in an amorphous silicon oxide matrix. Examples of lithium silicate include, but are not limited to, Li2SiO3, Li2Si2O5, and Li4SiO4. The structure of the first silicon oxide powder A may contain various components such as lithium-based materials, silicon-based materials, and lithium silicon compounds other than those mentioned above.
[0040] Similarly, when doped with magnesium, the first silicon oxide powder A may have a structure in which fine particles of silicon or magnesium silicate (such as MgSiO3 or Mg2SiO4) are dispersed in an amorphous silicon oxide matrix. When doped with calcium, the first silicon oxide powder A may have a structure in which fine particles of silicon or calcium silicate (such as CaSiO3 or Ca2SiO4) are dispersed in an amorphous silicon oxide matrix. The same applies to the case where other alkali metals or alkaline earth metals are doped.
[0041] The total doping amount of alkali metal or alkaline earth metal in the first silicon oxide powder A may be, for example, 0.1 weight % or more and 20 weight % or less, preferably 0.5 weight % or more and 15 weight % or less, and more preferably 1 weight % or more and 10 weight % or less, based on the entire first silicon oxide powder A.
[0042] The XRD pattern of the first silicon oxide powder A may have one or more diffraction peaks derived from microcrystals in the silicon oxide matrix. Even if no diffraction peaks are observed in the XRD pattern of the raw silicon oxide powder, new diffraction peaks may appear in the XRD pattern of the first silicon oxide powder A due to the progress of crystallization or the generation of a new crystalline phase by the doping treatment.
[0043] In the first silicon oxide powder A, the size of the silicon crystallites in the silicon oxide matrix (hereinafter, the size of such tiny single crystals is referred to as "crystallite size". In this specification, "crystallite size" refers to the value of D calculated using the following Scherrer formula (1)) can be, for example, 5 nm or more and 30 nm or less, preferably 5 nm or more and 20 nm or less, and more preferably 5 nm or more and 10 nm or less. The crystallite size of such crystallites can be calculated using the following Scherrer formula (1), which is well known in the art, from the line width of the peak derived from each crystallite on the XRD pattern of the first silicon oxide powder A. D(nm)=Kλ / Bcosθ ……(1) where D is the crystallite size of the crystallites, B is the full width at half maximum (rad) of the peak of interest in the XRD pattern, θ is the diffraction angle in the XRD pattern, K=0.9, λ=0.154 nm (for CuKα).
[0044] For example, in the case of silicon, a diffraction peak of the (111) plane is observed at approximately 2θ=28.4°, and the crystallite size D of the silicon microcrystals in the first silicon oxide powder A can be estimated from the full width at half maximum of this (111) peak and the diffraction angle θ.
[0045] The average particle size of the particles constituting the first silicon oxide powder A used as the negative electrode active material is, for example, 1 μm or more and 20 μm or less, preferably 3 μm or more and 15 μm or less, and more preferably 4 μm or more and 10 μm or less.
[0046] By using the negative electrode active material containing the first silicon oxide powder A, the initial efficiency can be improved as compared with the negative electrode active material containing only undoped silicon oxide powder. The reason for this is that in the undoped silicon oxide powder, a large amount of silicate phase, which is an irreversible component that does not contribute to charge and discharge, is generated during the first charge and discharge, whereas in the first silicon oxide powder A, such a silicate phase is formed in advance, so it is presumed that the decrease in the first discharge capacity with respect to the first charge capacity can be relatively suppressed.
[0047] The second silicon oxide powder B is a powder of undoped silicon oxide. Here, "undoped" means that, excluding inevitable impurities, no metal elements and non-metal elements other than silicon and oxygen are doped. That is, the particles constituting the second silicon oxide powder B can be those that do not contain metal elements and non-metal elements other than silicon and oxygen, excluding inevitable impurities. For example, the second silicon oxide powder B is a powder of SiO x The powder of SiO x can have a structure in which Si fine particles are dispersed in the form of microcrystals or amorphous in an amorphous silicon oxide matrix, for example. The ratio x of oxygen to silicon is 0 < x < 2, preferably 0.5 ≤ x ≤ 1.6, and more preferably 0.8 ≤ x ≤ 1.5. For example, the second silicon oxide powder B can be SiO (x = 1). Also, the second silicon oxide powder B may contain only SiO x having a specific value of x, or may be a mixture of two or more kinds of SiO x powders having different values of x.
[0048] The second silicon oxide powder B may have an amorphous structure that does not include a crystalline phase, except for microcrystals of silicon etc. dispersed in the structure. For example, the XRD pattern of the second silicon oxide powder B may have substantially no diffraction peaks derived from a crystalline phase when the dispersed microcrystals are large enough not to appear as diffraction peaks in the XRD pattern.
[0049] The average particle size of the particles constituting the second silicon oxide powder B used in the negative electrode active material can be, for example, smaller than the average particle size of the particles constituting the first silicon oxide powder A. The average particle size of the particles constituting the second silicon oxide powder B can be, for example, 0.1 μm or more and 5 μm or less, preferably 0.3 μm or more and 3 μm or less, and more preferably 0.5 μm or more and 2 μm or less.
[0050] By using a negative electrode active material containing the second silicon oxide powder B, the discharge capacity and cycle characteristics can be improved compared to a negative electrode active material containing only silicon oxide powder doped with an alkali metal or an alkaline earth metal. The reason for this is that the SiO x The diffusion of metal ions in the particles of the fine powder of is faster than that of doped silicon oxide, and the SiO x It is believed that the occurrence of cracks and expansion / contraction during charging / discharging is suppressed because the silicon oxide is amorphous, compared to highly crystalline doped silicon oxide. However, such a mechanism is merely an exemplary speculation and does not limit the present invention in any way.
[0051] The weight ratio A:B of the first silicon oxide powder A to the second silicon oxide powder B in the negative electrode active material may be, for example, 1:9 to 9:1, preferably 3:7 to 9:1, more preferably 4:6 to 9:1, and most preferably 5:5 to 8:2. When the weight ratio is expressed as B / A, the weight ratio B / A may be, for example, 0.1 or more, preferably 0.2 or more, and more preferably 0.25 or more. The weight ratio B / A may be, for example, less than 10, preferably less than 5, and more preferably less than 2. When the weight ratio is within the above range, it is possible to achieve both high initial efficiency and excellent discharge capacity and cycle characteristics.
[0052] When the carbon material powder is included in the negative electrode active material, the carbon material powder may include any carbon material that can generally be used as a negative electrode active material for non-aqueous electrolyte secondary batteries. For example, the carbon material powder may include one or a mixture of two or more of natural graphite, artificial graphite, graphitized carbon fiber, and amorphous carbon, but is not limited thereto. A composite with an element other than carbon can also be used. The carbon material may be low-crystalline carbon or high-crystalline carbon. Typical low-crystalline carbons are soft carbon and hard carbon, and typical high-crystalline carbons are amorphous, plate-like, scaly, spherical, or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesocarbon microbeads, mesophase pitch, and high-temperature fired carbon such as petroleum- or coal-based coke.
[0053] The average particle size of the particles constituting the powder of the carbon material may be, for example, 1 μm or more and 50 μm or less, and preferably 10 μm or more and 20 μm or less.
[0054] When the negative electrode active material contains a carbon material powder in addition to the first silicon oxide powder A and the second silicon oxide powder B, the weight ratio of the silicon material (i.e., the first silicon oxide powder A and the second silicon oxide powder B) to the carbon material in the negative electrode active material may be, for example, 1:99 to 50:50, preferably 5:95 to 30:80, and more preferably 8:92 to 20:80.
[0055] When the negative electrode active material contains a carbon material powder, the carbon material tends to exhibit better initial efficiency and cycle characteristics than a silicon material, and therefore even better initial efficiency and cycle characteristics can be obtained compared to when the negative electrode active material contains only the first silicon oxide powder A and the second silicon oxide powder B.
[0056] The negative electrode active material may contain other materials in addition to the first silicon oxide powder A, the second silicon oxide powder B, and the carbon material powder.
[0057] (binder) The binder is added as a component that promotes the bonding between the active material and the conductive agent, the bonding with the current collector, etc. Examples of binders include polyvinylidene fluoride (PVdF), polyvinyl alcohol (PVA), polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), polyacrylic acid, acrylamide, polyimide, fluororubber, various copolymers thereof, and the like, and one or a mixture of two or more of these may be used, but the binder is not limited to these.
[0058] The content of the binder may be 0.1% by weight or more and 30% by weight or less based on the total weight of the negative electrode active material layer. The content of the binder may be preferably 0.5% by weight or more and 20% by weight or less, and more preferably 1% by weight or more and 10% by weight or less. When the content of the binder polymer satisfies the above range, it is possible to provide sufficient adhesive strength within the electrode while preventing a decrease in the capacity characteristics of the battery.
[0059] (Conductive agent) The conductive agent is not particularly limited as long as it is an electrically conductive material that does not induce chemical changes. Examples of the conductive agent include carbon-based materials such as artificial graphite, natural graphite, carbon nanotubes, graphene, carbon black, acetylene black, ketjen black, denka black, thermal black, channel black, furnace black, lamp black, and carbon fibers; metal powders and metal fibers such as aluminum, tin, bismuth, silicon, antimony, nickel, copper, titanium, vanadium, chromium, manganese, iron, cobalt, zinc, molybdenum, tungsten, silver, gold, lanthanum, ruthenium, platinum, and iridium; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive polymers such as polyaniline, polythiophene, polyacetylene, polypyrrole, and polyphenylene derivatives, and the like, and a mixture of one or more of these may be used, but are not limited thereto.
[0060] The content of the conductive agent may be 0.1% by weight or more and 30% by weight or less based on the total weight of the negative electrode active material layer. The content of the conductive agent may be preferably 0.5% by weight or more and 15% by weight or less, more preferably 0.5% by weight or more and 10% by weight or less. When the content of the conductive agent satisfies the above range, it is advantageous in that sufficient conductivity can be imparted and the amount of the negative electrode active material is not reduced, thereby ensuring the battery capacity.
[0061] (Thickener) The negative electrode active material slurry may further include a thickener. Specifically, the thickener may be a cellulose-based compound such as carboxymethyl cellulose (CMC). The thickener may be included in an amount of, for example, 0.5% by mass to 10% by mass based on the total weight of the negative electrode active material layer.
[0062] (solvent) The solvent used in the negative electrode active material slurry is not particularly limited as long as it is generally used in the production of the negative electrode. Examples of the solvent include N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), isopropyl alcohol, acetone, water, etc., and one or a mixture of two or more of these can be used, but it is not limited thereto.
[0063] [Method for manufacturing negative electrode] The method for manufacturing a negative electrode for a lithium-ion secondary battery according to the embodiment may include: (1) a step of obtaining a negative electrode active material; (2) a step of obtaining a negative electrode active material slurry from the negative electrode active material; and (3) a step of obtaining a negative electrode from the negative electrode active material slurry.
[0064] (1) Step of obtaining negative electrode active material The first silicon oxide powder A is obtained, for example, by a thermal doping method. More specifically, the first silicon oxide powder A is obtained, for example, by mixing a raw material silicon oxide powder and a doping metal source powder and performing high-temperature firing in an inert atmosphere such as an argon atmosphere or a nitrogen atmosphere. If necessary, the obtained first silicon oxide powder A can be pulverized by a bead mill or the like to adjust the particle size.
[0065] As the raw material silicon oxide powder, for example, commercially available SiO x (0 < x < 2) powder or the like can be used. Here, the ratio x of oxygen to silicon is 0 < x < 2, preferably 0.5 ≦ x ≦ 1.6, and more preferably 0.8 ≦ x ≦ 1.5. Examples of the doping metal source include metallic lithium Li, lithium hydride LiH, etc. when doping with lithium, magnesium hydride MgH2 when doping with magnesium, calcium hydride CaH2 when doping with calcium, etc., but it is not limited thereto. The firing temperature is, for example, 650 ° C or higher and 850 ° C or lower.
[0066] As the second silicon oxide powder B, for example, commercially available SiO x (0 < x < 2) can be used. The SiO used xThe powder is the SiO 2 powder used as the raw material for the first silicon oxide powder A. x The second silicon oxide powder B may be the same as or different from the powder B. If necessary, the particle size of the second silicon oxide powder B may be adjusted by pulverizing the second silicon oxide powder B using a bead mill or the like.
[0067] The first silicon oxide powder A and the second silicon oxide powder B are mixed, if necessary, with other materials such as a carbon material to obtain a negative electrode active material.
[0068] (2) Obtaining a negative electrode active material slurry from the negative electrode active material A solvent is added to the negative electrode active material obtained in the above (1). At this time, a conductive agent, a binder, a thickener, etc. may be added as necessary. The negative electrode active material, the conductive agent, the binder, the thickener, etc. are dissolved or dispersed in the solvent to obtain a negative electrode active material slurry.
[0069] (3) Obtaining a negative electrode from the negative electrode active material slurry The negative electrode active material slurry is applied to a negative electrode current collector, and then dried and rolled to produce a negative electrode in which a negative electrode active material layer is formed on the negative electrode current collector.
[0070] As another method, for example, the negative electrode may be produced by casting the above-mentioned negative electrode active material slurry on another support, peeling it off from the support, and laminating the resulting film on the negative electrode current collector. Also, the negative electrode active material layer may be formed on the negative electrode current collector by any other method.
[0071] [Positive electrode] In the lithium ion secondary battery according to the embodiment, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on one or both surfaces of the positive electrode current collector. The positive electrode active material layer may be formed on the entire surface of the positive electrode current collector, or may be formed only on a portion of the surface.
[0072] (Positive electrode current collector) The positive electrode current collector used in the positive electrode is not particularly limited as long as it does not induce chemical changes in the battery and has electrical conductivity.For example, as the positive electrode current collector, stainless steel; aluminum; nickel; titanium; baked carbon; aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used.
[0073] The positive electrode current collector may have a thickness of 3 μm to 500 μm. Fine irregularities may be formed on the surface of the positive electrode current collector to enhance adhesion to the positive electrode active material. The positive electrode current collector may have various forms, such as a film, a sheet, a foil, a net, a porous body, a foam, or a nonwoven fabric.
[0074] (Cathode active material layer) The positive electrode active material layer can be formed, for example, by applying a positive electrode active material slurry, in which a mixture of a positive electrode active material, a conductive agent, and a binder is dissolved and dispersed in a solvent, to a positive electrode current collector, followed by drying and rolling. The mixture can further contain a dispersant, a filler, and other optional additives, as necessary.
[0075] The positive electrode active material may be contained in an amount of 80% by weight or more and 99% by weight or less based on the total weight of the positive electrode active material layer.
[0076] (Cathode active material) As the positive electrode active material, a compound capable of reversible insertion (intercalation) and deintercalation (deintercalation) of lithium can be used. Specific examples include lithium metal composite oxides containing lithium and one or more metals such as cobalt, manganese, nickel, copper, vanadium, and aluminum. More specifically, such lithium metal composite oxides include lithium-manganese oxides (e.g., LiMnO2, LiMnO3, LiMn2O3, LiMn2O4, etc.); lithium-cobalt oxides (e.g., LiCoO2, etc.); lithium-nickel oxides (e.g., LiNiO2, etc.); lithium-copper oxides (e.g., Li2CuO2, etc.); lithium-vanadium oxides (e.g., LiV3O8, etc.); lithium-nickel-manganese oxides (e.g., LiNi1-z Mn z O2 (0 < z < 1), LiMn 2-z Ni z O4 (0 < z < 2), etc.); lithium-nickel-cobalt-based oxides (e.g., LiNi 1-y Co y O2 (0 < y < 1), etc.); lithium-manganese-cobalt-based oxides (e.g., LiCo 1-z Mn z O2 (0 < z < 1), LiMn 2-y Co y O4 (0 < y < 2), etc.); lithium-nickel-manganese-cobalt-based oxides (e.g., Li(Ni x Co y Mn z )O2 (0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1), Li(Ni x Co y Mn z )O4 (0 < x < 2, 0 < y < 2, 0 < z < 2, x + y + z = 2), etc.); lithium-nickel-cobalt-metal (M) oxides (e.g., Li(Ni x Co y Mn z M w )O2 (M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, 0 < x < 1, 0 < y < 1, 0 < z < 1, 0 < w < 1, x + y + z + w = 1), etc.); compounds in which the transition metal elements in these compounds are partially substituted with one or two or more other metal elements, etc. The positive electrode active material layer can contain any one or two or more of these compounds. However, it is not limited to only these.
[0077] In particular, in terms of improving the capacity characteristics and stability of the battery, LiCoO2, LiMnO2, LiMn2O4, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.4 Mn 0.3 Co 0.3)O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, Li(Ni 0.8 Mn 0.1 Co 0.1 )O2), lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.) are preferred.
[0078] (Binder and conductive agent) The types and contents of the binder and conductive agent used in the positive electrode active material slurry may be the same as those described for the negative electrode.
[0079] (solvent) The solvent used in the positive electrode active material slurry is not particularly limited as long as it is generally used in the manufacture of a positive electrode. Examples of the solvent include amine solvents such as N,N-dimethylaminopropylamine, diethylenetriamine, and N,N-dimethylformamide (DMF), ether solvents such as tetrahydrofuran, ketone solvents such as methyl ethyl ketone, ester solvents such as methyl acetate, amide solvents such as dimethylacetamide and 1-methyl-2-pyrrolidone (NMP), and dimethylsulfoxide (DMSO), and one or a mixture of two or more of these may be used, but are not limited thereto.
[0080] The amount of the solvent used is sufficient as long as it is capable of dissolving or dispersing the positive electrode active material, conductive material, and binder and has a viscosity that allows excellent thickness uniformity to be exhibited when applied to the positive electrode current collector, taking into consideration the coating thickness of the slurry and the production yield.
[0081] [Cathode manufacturing method] A manufacturing method of a positive electrode for a lithium ion secondary battery according to the embodiment may include a step of obtaining a positive electrode active material slurry by dissolving or dispersing a positive electrode active material together with a binder, a conductive agent, a thickener, and the like as necessary in a solvent, and a step of forming a positive electrode active material layer on a positive electrode current collector by applying the positive electrode active material slurry onto the positive electrode current collector in a manner similar to the manufacturing method of a negative electrode, thereby obtaining a positive electrode.
[0082] [Separator] In the lithium ion secondary battery according to the embodiment, the separator separates the negative electrode and the positive electrode to provide a path for lithium ions to move, and any separator that is generally used as a separator in a lithium ion secondary battery can be used without any particular limitation. In particular, a separator that has a small resistance to ion movement of the electrolyte and has an excellent moisture-absorbing ability of the electrolyte is preferable. For example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used as the separator. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber or polyethylene terephthalate fiber, can also be used. In addition, a separator coated with a ceramic component or a polymeric substance to ensure heat resistance or mechanical strength may be used.
[0083] [Non-aqueous electrolyte] In the non-aqueous electrolyte secondary battery according to this embodiment, examples of the non-aqueous electrolyte include organic liquid electrolytes and inorganic liquid electrolytes that can be used in the manufacture of secondary batteries, but are not limited thereto.
[0084] The non-aqueous electrolyte may contain an organic solvent and a lithium salt, and may further contain additives as necessary. Hereinafter, the liquid electrolyte may also be referred to as an "electrolytic solution."
[0085] The organic solvent may be used without particular limitation as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Examples of organic solvents include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitrile-based solvents such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amide-based solvents such as dimethylformamide; dioxolane-based solvents such as 1,3-dioxolane; and sulfolane-based solvents. These may be used alone or in mixtures of two or more kinds, but are not limited thereto. In particular, carbonate-based solvents are preferred, and mixtures of cyclic carbonates (e.g., ethylene carbonate, propylene carbonate, etc.) having high ionic conductivity and high dielectric constant capable of enhancing the charge / discharge performance of batteries and low-viscosity linear carbonate-based compounds (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) are more preferred. In this case, when the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to 1:9, excellent electrolyte performance can be exhibited.
[0086] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium ion secondary battery. Examples of the lithium salt include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, and the like, and one or a mixture of two or more of these can be used, but are not limited thereto. The lithium salt can be contained in the electrolyte at a concentration of, for example, 0.1 mol / L or more and 2 mol / L or less. When the concentration of the lithium salt is within this range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0087] Additives can be used as necessary for the purpose of improving battery life characteristics, suppressing the decrease in battery capacity, and improving battery discharge capacity. Examples of additives include haloalkylene carbonate compounds such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC), pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride, and one or a mixture of two or more of these can be used, but are not limited thereto. The additives can be contained in an amount of, for example, 0.1% by weight to 15% by weight based on the total weight of the electrolyte.
[0088] In particular, fluoroethylene carbonate and difluoroethylene carbonate can act as a film-forming agent that forms a film at the interface between the electrode and the electrolyte. For example, when at least one of fluoroethylene carbonate and difluoroethylene carbonate is included, a good SEI film is formed in the process of alloying the silicon-based material and lithium in the negative electrode using the negative electrode active material containing the silicon-based material, so that stable charging and discharging can be performed. The content of the film-forming agent can be, for example, 0.1% by weight or more and 15% by weight or less, preferably 0.5% by weight or more and 10% by weight or less, and more preferably 1% by weight or more and 7% by weight or less, based on the total weight of the electrolyte. The film-forming agent can include at least one of fluoroethylene carbonate and difluoroethylene carbonate.
[0089] [Method of manufacturing non-aqueous electrolyte secondary battery] The nonaqueous electrolyte secondary battery according to the embodiment may be manufactured by interposing a separator (e.g., a separator membrane) and an electrolyte between the negative electrode manufactured as described above and the positive electrode manufactured as described above. More specifically, a separator is disposed between the negative electrode and the positive electrode to form an electrode assembly, and the electrode assembly is placed in a battery case such as a cylindrical battery case or a prismatic battery case, and then an electrolyte is injected to manufacture the nonaqueous electrolyte secondary battery. Alternatively, the electrode assemblies may be stacked, and the resulting product obtained by impregnating the electrode assemblies with an electrolyte is placed in a battery case and sealed to manufacture the battery.
[0090] The battery case may be one commonly used in the art, and may have, for example, a cylindrical shape using a can, a rectangular shape, a pouch shape, or a coin shape.
[0091] The lithium ion secondary battery according to the embodiment can be used not only as a power source for a small device, but also as a unit battery of a medium- to large-sized battery module including a large number of battery cells, etc. Preferred examples of such medium- to large-sized devices include, but are not limited to, electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems. EXAMPLES
[0092] Examples and comparative examples are described below, but the present invention is not limited thereto. The mechanisms described below are merely exemplary speculations to aid in understanding the present application, and do not limit the present invention in any way.
[0093] [Example 1] (Production of negative electrodes) A silicon oxide powder was prepared by thermally doping an amorphous SiO powder with lithium (first silicon oxide powder A). The average particle size of the particles constituting the first silicon oxide powder A was 7.0 μm. The lithium content measured by inductively coupled plasma optical emission spectroscopy was 6 wt% based on the total weight of the first silicon oxide powder A. When the first silicon oxide powder A was subjected to X-ray diffraction (XRD) measurement, a diffraction peak of the (111) plane of silicon Si was observed near 2θ=28.4°. The crystallite size of the silicon microcrystals calculated from the (111) peak using the Scherrer equation was about 9 nm. In addition, peaks mainly attributed to Li2SiO3 and Li2Si2O5 were observed in the XRD pattern.
[0094] Amorphous SiO powder (Sigma Aldrich) was pulverized in a bead mill to prepare an undoped silicon oxide powder (silicon dioxide powder B). The particles constituting silicon dioxide powder B had an average particle size of 1.6 μm, a lower limit of the particle size distribution of 0.3 μm, and an upper limit of the particle size distribution of 6.0 μm. When the XRD pattern of silicon dioxide powder B was measured, no diffraction peaks indicating a crystalline phase were observed.
[0095] The first silicon oxide powder A and the second silicon oxide powder B were mixed in a weight ratio of 5:5 to obtain a negative electrode active material powder. 5 parts by weight of carbon black as a conductive agent and 10 parts by weight of polyacrylic acid as a binder were added to 85 parts by weight of the negative electrode active material powder, and pure water was added as a solvent and mixed to obtain a negative electrode active material slurry. This negative electrode active material slurry was applied to a copper foil, vacuum dried, and pressed to a predetermined density to obtain a negative electrode.
[0096] (Battery manufacturing) Metallic lithium was used as a counter electrode (i.e., positive electrode) to the obtained negative electrode to prepare a coin battery (half cell).
[0097] [Example 2] A coin battery was produced in the same manner as in Example 1, except that the weight ratio of the first silicon oxide powder A to the second silicon oxide powder B was 8:2.
[0098] [Example 3] As in Example 1, the first silicon oxide powder A and the second silicon oxide powder B were mixed in a weight ratio of 5:5 to obtain a mixed powder. Natural graphite was added to this mixed powder so that the weight ratio of the mixed powder to the natural graphite was 1:9, and a negative electrode active material powder was obtained (i.e., the weight ratio of the first silicon oxide powder A, the second silicon oxide powder B, and the natural graphite was 0.5:0.5:9). 1.0 part by weight of carbon black as a conductive agent, 1.5 parts by weight of styrene butadiene rubber (SBR) as a binder, and 1.5 parts by weight of carboxymethyl cellulose (CMC) as a thickener were added to 96 parts by weight of the negative electrode active material powder, and pure water was added as a solvent and mixed to obtain a negative electrode active material slurry. This negative electrode active material slurry was applied to copper foil, vacuum dried, and pressed to a predetermined density to obtain a negative electrode. Metallic lithium was used as the counter electrode (i.e., the positive electrode) of this negative electrode, and a coin battery was manufactured.
[0099] [Example 4] A coin battery was produced in the same manner as in Example 1, except that the first silicon oxide powder A was prepared so as to have an average particle size of 4.2 μm.
[0100] [Example 5] A coin battery was produced in the same manner as in Example 1, except that the second silicon oxide powder B was prepared so that its average particle size was 0.8 μm.
[0101] [Comparative Example 1] A coin battery was manufactured in the same manner as in Example 1, except that no second silicon oxide powder B was used and only first silicon oxide powder A was used (i.e., the weight ratio of first silicon oxide powder A to second silicon oxide powder B was 10:0).
[0102] [Comparative Example 2] A coin battery was manufactured in the same manner as in Example 1, except that no first silicon oxide powder A was used and only second silicon oxide powder B was used (i.e., the weight ratio of first silicon oxide powder A to second silicon oxide powder B was 0:10).
[0103] [Comparative Example 3] A coin battery was manufactured in the same manner as in Example 3, except that no second silicon oxide powder B was used and only the first silicon oxide powder A was mixed with natural graphite (i.e., the weight ratio of the first silicon oxide powder A to the second silicon oxide powder B to the natural graphite was 1:0:9).
[0104] [Comparative Example 4] A coin battery was manufactured in the same manner as in Example 3, except that no first silicon oxide powder A was used and only second silicon oxide powder B was mixed with natural graphite (i.e., the weight ratio of first silicon oxide powder A to second silicon oxide powder B to natural graphite was 0:1:9).
[0105] [Comparative Example 5] A coin battery was produced in the same manner as in Example 1, except that the first silicon oxide powder A was prepared so as to have an average particle size of 18 μm.
[0106] [Comparative Example 6] A coin battery was produced in the same manner as in Example 1, except that the second silicon oxide powder B was prepared so that its average particle size was 5 μm.
[0107] [Evaluation example 1: Initial charge / discharge characteristics] The coin batteries manufactured in each Example and Comparative Example were charged and discharged at a constant current of 0.2 C with a cutoff voltage of 1.5 V. The "initial capacity" is defined as the value obtained by dividing the discharge capacity in this initial charge / discharge process by the weight (g) of the negative electrode active material powder used in each Example and Comparative Example, as follows:
number
[0108] The charge / discharge efficiency in this initial charge / discharge process (hereinafter referred to as "initial efficiency") is defined by the following equation.
number
[0109] [Evaluation Example 2: Capacity Retention Rate] For the coin batteries manufactured according to each Example and Comparative Example, following the first charge / discharge cycle carried out in Evaluation Example 1, charge / discharge was carried out once more under the same conditions, and then similar charge / discharge cycles were repeated 48 times at a constant current of 0.5 C. That is, a total of 50 charge / discharge cycles were repeated, including the first and second charge / discharge cycles. The capacity retention rate during this repeated charge / discharge cycle is defined by the following formula.
number
[0110] The initial capacity, initial efficiency, and capacity retention rate calculated for each coin battery manufactured in each Example and Comparative Example were as follows: In addition, the weight ratio of the first silicon oxide powder A to the second silicon oxide powder B (columns "A:B" and "B / A") and the weight ratio of the silicon oxide powder to natural graphite (column "Silicon oxide:graphite") are also shown in the table below. [Table 1]
[0111] First, Example 1, Example 2, Comparative Example 1, and Comparative Example 2, which did not use natural graphite, are compared. The initial capacity was smallest (1355 mAh / g) in Comparative Example 1, which used only the first silicon oxide powder A, and increased as the ratio of the second silicon oxide powder B to the first silicon oxide powder A increased. On the other hand, the initial efficiency was smallest (75.4%) in Comparative Example 2, which used only the second silicon oxide powder B, and increased as the ratio of the second silicon oxide powder B to the first silicon oxide powder A decreased. In addition, when comparing the capacity retention rate, it was smallest (71.3%) in Comparative Example 1, which used only the first silicon oxide powder A, as in the initial capacity, and increased as the ratio of the second silicon oxide powder B to the first silicon oxide powder A increased.
[0112] Thus, in Comparative Example 1, in which only the first silicon oxide powder A was used, the initial efficiency was high, but the initial capacity and capacity retention rate were small. In Comparative Example 2, in which only the second silicon oxide powder B was used, the initial capacity and capacity retention rate were high, but the initial efficiency was low. For this reason, in Comparative Example 1 and Comparative Example 2, in which only either the first silicon oxide powder A or the second silicon oxide powder B was used, it was not possible to achieve both high initial efficiency and excellent discharge capacity and capacity retention rate.
[0113] In contrast, in Examples 1 and 2 containing the first silicon oxide powder A and the second silicon oxide powder B, none of the initial capacity, initial efficiency, or capacity retention rate was extremely poor, and a good balance was achieved between high initial efficiency and excellent discharge capacity and capacity retention rate.
[0114] FIG. 1 is a plot of the initial capacity (◯), initial efficiency (△), and capacity retention rate (□) versus the weight ratio (A:B) of the first silicon oxide powder A and the second silicon oxide powder B for Example 1, Example 2, Comparative Example 1, and Comparative Example 2, in which natural graphite was not used. As shown in FIG. 1, the graphs of the initial capacity (◯) and initial efficiency (△) versus A:B were almost linear. That is, the initial capacity increased almost linearly as the A:B ratio changed from 10:0 to 0:10, and the initial efficiency decreased almost linearly as the A:B ratio changed from 10:0 to 0:10. On the other hand, the graph (□) of the capacity retention rate versus A:B did not show a simple proportional relationship, but was a convex curve. That is, the capacity retention rate was drastically improved from Comparative Example 1, in which only the silicon oxide powder A was used as the negative electrode active material, even when a small amount of the second silicon oxide powder B was added to the first silicon oxide powder A. For example, Example 1, in which the weight ratio A:B was 5:5, showed a capacity retention rate of 96%, which is far higher than the capacity retention rate (71%) of Comparative Example 1, in which only the first silicon oxide powder A was used as the negative electrode active material, even though the first silicon oxide powder A, which may cause cycle deterioration, accounted for half of the negative electrode active material. This result suggests that by mixing the first silicon oxide powder A and the second silicon oxide powder B, some kind of synergistic effect was achieved, achieving a capacity retention rate higher than expected.
[0115] The above synergistic effect may be caused, for example, by the following mechanism. However, the following is merely an exemplary speculation for aiding understanding of the present application and is not intended to limit the present invention in any way.
[0116] In each example, the first silicon oxide powder A and the second silicon oxide powder B are mixed. Compared to the first silicon oxide powder A doped with lithium, the undoped second silicon oxide powder B has a higher lithium absorption capacity, and is therefore presumed to be able to absorb lithium quickly and form an alloy. It is believed that this alloying reduces the resistance of the second silicon oxide powder B, and that lithium diffuses smoothly from the second silicon oxide powder B to the adjacent first silicon oxide powder A. In this way, the surface resistance of the first silicon oxide powder A is substantially reduced, which is presumed to smooth the charge and discharge process and contribute to improving the life characteristics.
[0117] In addition, when the average particle size of the particles constituting the second silicon oxide powder B is smaller than that of the particles constituting the first silicon oxide powder A, the small second silicon oxide powder B can easily enter the gaps between the large first silicon oxide powder A. This can increase the density of the entire negative electrode active material, and therefore the charge / discharge capacity per weight. Furthermore, it is believed that the substantial contact area between the first silicon oxide powder A and the second silicon oxide powder B increases, making lithium diffusion, i.e., the charging and discharging of the battery, smoother, and improving the life characteristics.
[0118] Next, Example 3, Comparative Example 3, and Comparative Example 4, which used natural graphite, are compared. As in the case where natural graphite was not used, the initial capacity and capacity retention rate were smallest (464 mAh / g, 92.7%) in Comparative Example 3, which used only the first silicon oxide powder A, and increased as the ratio of the second silicon oxide powder B to the first silicon oxide powder A increased. On the other hand, the initial efficiency was smallest (86.9%) in Comparative Example 4, which used only the second silicon oxide powder B, and increased as the ratio of the second silicon oxide powder B to the first silicon oxide powder A decreased.
[0119] FIG. 2 is a plot of the initial capacity (◯), initial efficiency (△), and capacity retention rate (□) against the weight ratio (A:B) of the first silicon oxide powder A and the second silicon oxide powder B for Example 3, Comparative Example 3, and Comparative Example 4 using natural graphite, similar to FIG. 1. As in the case where natural graphite was not used, the graph of the initial capacity (◯) against A:B was almost a straight line. That is, the initial capacity increased almost linearly as the A:B ratio changed from 10:0 to 0:10. On the other hand, the graph of the capacity retention rate (□) against A:B was not a simple proportional relationship, but was a convex curve, similar to the case where natural graphite was not used. That is, the capacity retention rate was drastically improved by the addition of the second silicon oxide powder B from Comparative Example 3 in which only the silicon oxide powder A was used as the negative electrode active material. Therefore, even when natural graphite was used, the capacity retention rate was improved more than expected by mixing the first silicon oxide powder A and the second silicon oxide powder B.
[0120] Furthermore, unlike the case where natural graphite was not used, the graph of the initial efficiency (△) versus A:B did not show a simple proportional relationship, but instead showed a convex curve. That is, the initial efficiency did not decrease linearly versus A:B when the second silicon oxide powder B was added to the first silicon oxide powder A, but showed a more gradual decrease. In other words, the initial efficiency was drastically improved by adding the first silicon oxide powder A to the second silicon oxide powder B, compared to Comparative Example 4, in which only the second silicon oxide powder B was used as the negative electrode active material. This result suggests that a further synergistic effect was achieved by mixing the first silicon oxide powder A and the second silicon oxide powder B in the presence of a carbon material, resulting in an initial efficiency higher than expected.
[0121] The above-mentioned effect due to the presence of a carbon material may be caused, for example, by the following mechanism. However, the following is merely an exemplary speculation for aiding understanding of the present application and does not limit the present invention in any way.
[0122] The reason why the addition of carbon materials resulted in high initial efficiency is believed to be that by mixing carbon materials such as graphite, which has a smaller volume change due to charging and discharging than silicon oxide, the volume change of the electrode during the first charge, which is the largest change due to charging, is smaller than when silicon oxide alone is used as the negative electrode active material. In addition, the improvement in capacity retention is believed to be due to the ease of deformation and high electronic conductivity of the carbon material. That is, silicon oxide is hard and does not deform even when the electrode is pressed, so when the negative electrode active material is only silicon oxide, even when the first silicon oxide powder A and the second silicon oxide powder B, which have different particle sizes, are mixed, voids that interrupt the conductive path are likely to occur in part of the electrode. In contrast, when graphite, which is soft and easily deformed by pressing, especially natural graphite, is mixed, it is presumed that the above-mentioned voids are significantly reduced. In addition, it is presumed that natural graphite, which has high electronic conductivity, adheres closely to silicon oxide, which has relatively low electronic conductivity, and natural graphite plays a role in facilitating the insertion and removal of lithium ions into and from silicon oxide. For this reason, it is believed that the addition of a carbon material can improve not only the initial charging time but also the life characteristics, that is, the capacity retention rate.
[0123] Note that, the types of binders and thickeners used are different between Example 1, Example 2, Comparative Example 1, and Comparative Example 2, which did not use natural graphite, and Example 3, Comparative Example 3, and Comparative Example 4, which used natural graphite, but this is simply because appropriate binders and thickeners were selected depending on whether or not natural graphite was used. This difference does not have a significant effect on the initial capacity, initial efficiency, and capacity retention rate of the battery.
[0124] As with Example 1, Examples 4 and 5 are also better than Comparative Example 1 in terms of initial capacity and life (capacity retention rate), but the initial efficiency is somewhat reduced due to the smaller particle sizes of A and B. When the particle size of A becomes large as in Comparative Example 5, electrode collapse due to expansion occurs from the first charge / discharge, so that even if B is added, a conductive path between the particles cannot be obtained, and the life characteristics are significantly reduced. When the particle size of B becomes large as in Comparative Example 6, it becomes difficult to uniformly fill the gaps between the particles, and at the same time, electrode deterioration due to the expansion of B itself becomes greater than in Example 1, so life deterioration occurs.
Claims
1. A first silicon oxide powder doped with at least one of an alkali metal and an alkaline earth metal; undoped silicon dioxide powder; Including, The second silicon oxide powder is amorphous, The average particle size of the particles constituting the first silicon oxide powder is larger than the average particle size of the particles constituting the second silicon oxide powder, The average particle size of the particles constituting the first silicon oxide powder is 3 μm or more and 15 μm or less, and the average particle size of the particles constituting the second silicon oxide powder is 0.5 μm or more and 2 μm or less. Negative electrode active material for secondary batteries.
2. 2. The negative electrode active material according to claim 1, wherein a weight ratio of the second silicon oxide powder to the first silicon oxide powder is 0.2 or more.
3. 3. The negative electrode active material according to claim 1, wherein a weight ratio of the second silicon oxide powder to the first silicon oxide powder is less than 10.
4. 4. The negative electrode active material according to claim 1, wherein the first silicon oxide powder contains silicon microcrystals having a crystallite size of 5 nm or more and 30 nm or less.
5. The first silicon oxide powder is Li 2 SiO 3 , Li 2 S 2 O 5 , Li 4 SiO 4 , and Mg 2 SiO 4 The negative electrode active material according to any one of claims 1 to 4, comprising at least one of the following:
6. The negative electrode active material according to any one of claims 1 to 5, further comprising a carbon material powder containing one or a mixture of two or more of natural graphite, artificial graphite, graphitized carbon fiber, and amorphous carbon.
7. 7. A negative electrode for a secondary battery, comprising: a negative electrode active material layer comprising the negative electrode active material according to claim 1 formed on a negative electrode current collector.
8. A secondary battery comprising the negative electrode according to claim 7.
Citation Information
Patent Citations
Negative electrode material for secondary battery, and its manufacturing method
JP2010170943A
Cathode material for nonaqueous electrolytic secondary battery and method of manufacturing the same, and lithium ion secondary battery
JP2012033317A
Silicon oxide powder, lithium ion secondary battery negative electrode material including the same, lithium ion secondary battery including the material, and method for producing silicon oxide powder for lithium ion secondary battery negative electrode material
JP2013114820A
Negative electrode active substance, mixed negative electrode active substance material, and method for manufacturing negative electrode active substance
JP2017188319A
Negative electrode active material, mixed negative electrode active material material, and method for producing negative electrode active material
JP2017195015A