Multi-element doped porous carbon and preparation method thereof, silicon-carbon negative electrode material and preparation method and application of silicon-carbon negative electrode material

By using a combination technology of multi-element doped porous carbon and nano-silicon particles in silicon-carbon negative electrode materials, the problem of volume expansion of silicon-carbon materials during the lithiation process is solved, its specific capacity and cycle stability are improved, and high efficiency is achieved. electrochemical properties.

CN118851172AActive Publication Date: 2024-10-29YANTAI ADVANCED MATERIALS & GREEN MFG SHANDONG PROVINCIAL LAB +1

Patent Information

Application Number
CN202410939174.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The volume expansion of existing silicon-carbon anode materials during the lithiation process leads to cracking, crushing or falling off, which reduces the cycle life, and there is still room for improvement in its specific capacity, first Coulombic efficiency and cycle stability.

Method used

Multi-element doped porous carbon is used as the substrate, and N, S, F and Li elements are introduced into the phenolic resin to form a porous structure, and chemical vapor deposition is used to deposit nano silicon particles on it to form silicon carbon micron particles, and conduct Carbon coating to enhance the performance of the anode material.

Benefits of technology

Significantly improves the first Coulombic efficiency and specific capacity of the silicon carbon anode material, and maintains high capacity stability during long cycles. The first specific capacity is >2500mAh/g, the capacity retention rate is >90% after 1000 cycles, and the first Coulombic efficiency reaches 95%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851172A_ABST
    Figure CN118851172A_ABST
Patent Text Reader

Abstract

The invention provides multi-element doped porous carbon and a preparation method thereof, a silicon-carbon negative electrode material and a preparation method and application thereof, and relates to the technical field of lithium batteries. According to the invention, a porous carbon matrix with uniform aperture and particle size is prepared through an in-situ heteroelement doping technology of resin-based porous carbon. Wherein the heteroelement atoms are beneficial to stabilizing the silicon particles and improving the silicon loading capacity, and participate in forming an SEI film at the same time, so that the first coulombic efficiency and the long cycle stability of the silicon-carbon negative electrode are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a multi-element doped porous carbon and a preparation method thereof, a silicon-carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] With the development of the electric vehicle market, the improvement of energy density has become the main goal of lithium-ion battery development. Silicon anode material has a very high theoretical specific capacity (4200mAh / g), and is expected to replace graphite as the anode material for the next generation of lithium-ion batteries.

[0003] However, there are still huge challenges in the practical application of silicon negative electrodes. During the lithiation process, silicon materials will undergo volume expansion (about 400%), causing them to crack, shatter or fall off the current collector, thereby significantly reducing the cycle life. Therefore, silicon negative electrode materials usually need to be carbon-coated to prepare silicon-carbon composite materials to improve their conductivity and inhibit the volume expansion effect. The new generation of silicon-carbon materials uses porous carbon as a substrate, and nano-silicon particles are loaded inside the porous carbon pores by silane deposition, providing a buffer space for the expansion of silicon particles, thereby improving the cycle stability. In this material system, increasing the loading amount and loading stability of silicon particles becomes a key issue.

[0004] The Chinese patent with publication number CN 117658096A discloses a heteroatom-doped hierarchical mesoporous carbon material and its preparation method. The heteroatom-doped hierarchical mesoporous carbon material prepared by the hard template method has a developed mesoporous structure and high mechanical strength, and is used for the preparation of silicon-carbon negative electrode materials and lithium-ion batteries. The obtained lithium-ion battery has excellent electrochemical performance, the first reversible specific capacity is greater than 1800mAh / g; the first coulombic efficiency is higher than 85%, and can reach up to 93%; the capacity retention rate after 100 cycles is ≥88%, and can reach up to 94%; the capacity retention rate after 500 cycles is ≥80%, and can reach up to 90%. The patent has achieved good cycle stability, with both high reversible specific capacity and first coulombic efficiency, but from its public data, its specific capacity, first coulombic efficiency and cycle stability still need to be further improved. Summary of the invention

[0005] The purpose of the present invention is to provide a multi-element doped porous carbon and a preparation method thereof, a silicon-carbon negative electrode material and a preparation method and application thereof. The multi-element doped porous carbon provided by the present invention is used as a substrate to prepare a silicon-carbon negative electrode material with high first coulombic efficiency, high specific capacity, and good long-term cycle stability.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a multi-element doped porous carbon, wherein the doping elements include N, S, F and Li elements; in the multi-element doped porous carbon, the molar content of the N element is 2.1-9.5%, the molar content of the S element is 1.0-3.6%, the molar content of the F element is 1.0-3.3%, and the molar content of the Li element is 1.0-3.3%.

[0008] Preferably, the specific surface area of ​​the multi-element doped porous carbon is 1400-1950 m 2 / g, average pore diameter of 0.8-5nm, particle size of 2-15μm, pore volume of 0.5-1.2cm 3 / g, and the micropore volume accounts for 65-80%.

[0009] Preferably, the method comprises the following steps:

[0010] A nitrogen source, a sulfur source, lithium fluoride, phenol, formaldehyde, a catalyst and water are mixed, and the obtained mixture is heated and cured to obtain a multi-element doped phenolic resin; the mass of the nitrogen source is 3-15% of the mass of the phenol; the mass of the sulfur source is 2-7.5% of the mass of the phenol; the mass of the lithium fluoride is 2.5-5% of the mass of the phenol;

[0011] Under a protective atmosphere, subjecting the multi-element doped phenolic resin to a carbonization heat treatment to obtain a multi-element doped carbon material;

[0012] The multi-element doped carbon material is etched in a water vapor-inert gas mixture to form a porous structure, thereby obtaining multi-element doped porous carbon.

[0013] Preferably, the nitrogen source is one or more of urea, melamine, ethylenediamine, dicyandiamide, n-butylamine, ethanolamine, imidazole and pyridine;

[0014] The sulfur source is one or more of sublimated sulfur, oxidized thiourea, thiophene, ammonium thiocyanate and ammonium persulfate.

[0015] Preferably, the carbonization heat treatment includes: first heating to 90-110°C and keeping warm for 50-70 min, second heating to 500-550°C and keeping warm for 50-70 min, and third heating to 800-1000°C and keeping warm for 120-240 min.

[0016] Preferably, the etching conditions include: a temperature of 450-550° C., a holding time of 60-120 min; a water vapor flow rate of 1-5 L / min, and an inert gas flow rate of 1-15 L / min.

[0017] The present invention provides a silicon-carbon negative electrode material, comprising silicon-carbon micron particles and a carbon layer coated on the surface of the silicon-carbon micron particles; the silicon-carbon micron particles comprise multi-element doped porous carbon, and nano-silicon particles located in the pores and / or the surface of the multi-element doped porous carbon;

[0018] The mass content of Si in the silicon-carbon negative electrode material is 50-65%, and the mass content of C is 30-50%;

[0019] The multi-element doped porous carbon is the multi-element doped porous carbon described in the above scheme or the multi-element doped porous carbon prepared by the preparation method described in the above scheme.

[0020] Preferably, the average particle size of the silicon-carbon negative electrode material is 2 to 15 μm, and the specific surface area is 0.5 to 5 m 2 / g, wherein the size of the nano silicon particles is 1 to 3 nm.

[0021] The present invention provides a method for preparing the silicon-carbon negative electrode material described in the above scheme, comprising the following steps:

[0022] Depositing silicon nanoparticles on multi-element doped porous carbon by cracking silane using chemical vapor deposition to obtain silicon carbon micron particles;

[0023] The silicon-carbon micron particles are carbon-coated to obtain the silicon-carbon negative electrode material.

[0024] The present invention provides the use of the silicon-carbon negative electrode material described in the above scheme or the silicon-carbon negative electrode material prepared by the preparation method described in the above scheme in a lithium ion battery.

[0025] The present invention provides a multi-element doped porous carbon, wherein the doping elements include N, S, F and Li elements; in the multi-element doped porous carbon, the molar content of the N element is 2.1-9.5%, the molar content of the S element is 1.0-3.6%, the molar content of the F element is 1.0-3.3%, and the molar content of the Li element is 1.0-3.3%.

[0026] In the porous carbon provided by the present invention, N and S heteroatoms can serve as binding sites for silicon source gas deposition, guide the uniform deposition of silane in the pores, increase the amount of silicon particle deposition (the mass proportion of silicon particles in the silicon-carbon negative electrode material reaches more than 50%) and stabilize silicon nanoparticles, thereby improving the capacity (the first specific capacity>2500mAh / g) and preventing the particles from falling off due to volume expansion during charging and discharging; the fluorine F element can help form the SEI film during the charging and discharging process, improve the capacity stability, and avoid capacity decay (the capacity retention rate after 1000 cycles>90%); the introduced Li element can form a lithium-silicon alloy when the silicon particles are deposited, reduce the lithium ions consumed by the first charging of the silicon-carbon negative electrode, improve the first coulomb efficiency (95%), and improve the utilization rate of the negative electrode material.

[0027] The present invention provides a method for preparing the multi-element doped porous carbon described in the above scheme, by adding a heteroelement source during the synthesis of a phenolic resin precursor, and realizing nitrogen, sulfur, fluorine, and lithium doping of the porous carbon by an in-situ doping method. The doping method is simple and easy, and the prepared porous carbon has uniform pore size and particle size. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the first charge and discharge curve of the silicon-carbon negative electrode material of Example 1;

[0029] Figure 2 This is a cycle performance diagram of the silicon-carbon negative electrode material of Example 1. DETAILED DESCRIPTION

[0030] The present invention provides a multi-element doped porous carbon, wherein the doping elements include N, S, F and Li elements; in the multi-element doped porous carbon, the molar content of the N element is 2.1 to 9.5%, preferably 2.5 to 9.0%, and more preferably 3.0 to 8.8%. In an embodiment of the present invention, it is specifically 3.4%, 4.6% or 8.7%.

[0031] In the multi-element doped porous carbon provided by the present invention, the molar content of the S element is 1.0-3.6%, preferably 1.5-3.5%. In the embodiments of the present invention, it is specifically 2.5%, 3.2% or 3.6%.

[0032] In the multi-element doped porous carbon provided by the present invention, the molar content of the F element is 1.0-3.3%, preferably 1.3-3.0%. In the embodiments of the present invention, it is specifically 1.3%, 1.9% or 3.3%.

[0033] In the multi-element doped porous carbon provided by the present invention, the molar content of Li element is 1.0-3.3%, preferably 1.3-3.0%. In the embodiments of the present invention, it is specifically 1.3%, 1.9% or 3.3%.

[0034] In the porous carbon provided by the present invention, N and S heteroatoms can serve as binding sites for silicon source gas deposition, guide the uniform deposition of silane in the pores, increase the amount of silicon particle deposition (the mass proportion of silicon particles in the silicon-carbon negative electrode material reaches more than 50%) and stabilize silicon nanoparticles, thereby improving the capacity (the first specific capacity>2500mAh / g) and preventing the particles from falling off due to volume expansion during charging and discharging; the fluorine F element can help form the SEI film during the charging and discharging process, improve the capacity stability, and avoid capacity decay (the capacity retention rate after 1000 cycles>90%); the introduced Li element can form a lithium-silicon alloy when the silicon particles are deposited, reduce the lithium ions consumed by the first charging of the silicon-carbon negative electrode, improve the first coulomb efficiency (95%), and improve the utilization rate of the negative electrode material.

[0035] In the present invention, the specific surface area of ​​the multi-element doped porous carbon is preferably 1400 to 1950 m 2 / g, more preferably 1600 to 1930 m 2 / g, in the embodiment of the present invention, specifically 1682m 2 / g, 1760m 2 / g or 1923m 2 / g.

[0036] In the present invention, the average pore diameter of the multi-element doped porous carbon is preferably 0.8-5 nm, more preferably 2-4 nm, and in the embodiments of the present invention, specifically 2.6 nm, 2.9 nm or 3.1 nm.

[0037] In the present invention, the particle size of the multi-element doped porous carbon is preferably 2 to 15 μm, more preferably 5 to 13 μm, and further preferably 6 to 10 μm; the pore volume of the multi-element doped porous carbon is preferably 0.5 to 1.2 cm 3 / g, more preferably 0.6 to 1.18 cm 3 / g, in the embodiment of the present invention, specifically 0.81cm 3 / g, 0.97cm 3 / g or 1.16cm 3 / g; wherein the micropore volume ratio is preferably 65-80%, more preferably 66-75%, and in the embodiments of the present invention, specifically 65%, 69% or 70%.

[0038] The present invention provides a method for preparing the multi-element doped porous carbon described in the above scheme, comprising the following steps:

[0039] A nitrogen source, a sulfur source, lithium fluoride, phenol, formaldehyde, a catalyst and water are mixed, and the obtained mixture is heated and cured to obtain a multi-element doped phenolic resin;

[0040] Under a protective atmosphere, subjecting the multi-element doped phenolic resin to a carbonization heat treatment to obtain a multi-element doped carbon material;

[0041] The multi-element doped carbon material is etched in a water vapor-inert gas mixture to form a porous structure, thereby obtaining multi-element doped porous carbon.

[0042] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.

[0043] The invention mixes a nitrogen source, a sulfur source, lithium fluoride, phenol, formaldehyde, a catalyst and water, and heats and solidifies the obtained mixture to obtain a multi-element doped phenolic resin.

[0044] In the present invention, the nitrogen source is preferably one or more of urea, melamine, ethylenediamine, dicyandiamide, n-butylamine, ethanolamine, imidazole and pyridine; the mass of the nitrogen source is 3-15% of the mass of phenol, preferably 5-13%, more preferably 8-10%.

[0045] In the present invention, the sulfur source is preferably one or more of sublimed sulfur, oxidized thiourea, thiophene, ammonium thiocyanate and ammonium persulfate; the mass of the sulfur source is 2-7.5% of the mass of phenol, preferably 3-7%, more preferably 4-6%. In the present invention, the ammonium thiocyanate and ammonium persulfate serve as both sulfur sources and nitrogen sources.

[0046] In the present invention, the mass of the lithium fluoride is 2.5-5% of the mass of the phenol, preferably 3-4.5%, and more preferably 3.5-4%.

[0047] In the present invention, the catalyst is preferably ammonia water, and the mass concentration of the ammonia water is preferably 15%. The mass of the catalyst is preferably 2.5-10% of the mass of phenol, more preferably 4-8%, and further preferably 5-6%.

[0048] In the present invention, the mass of the formaldehyde is preferably 45 to 110% of the mass of the phenol, more preferably 50 to 100%, and even more preferably 60 to 90%.

[0049] In the present invention, the mass of the phenol is preferably 5-20% of the mass of water, more preferably 8-16%, and further preferably 10-14%; and the water is preferably deionized water.

[0050] In the present invention, the mixing of the nitrogen source, the sulfur source, lithium fluoride, phenol, formaldehyde, the catalyst and water preferably comprises: mixing phenol and water, adding the nitrogen source, the sulfur source and lithium fluoride to the obtained mixed solution, heating and stirring, adding formaldehyde to the obtained mixed solution, performing a first heating reflux, adding the catalyst to the obtained reflux liquid, performing a second heating reflux, and obtaining a mixture.

[0051] In the present invention, the heating and stirring time is preferably 60-70°C, more preferably 65°C; the heating and stirring time is preferably 1-3h, more preferably 2h. In the present invention, the temperature of the first heating reflux is preferably 60-70°C, more preferably 65°C; the first heating reflux time is preferably 15-30min, more preferably 20-25min; the temperature of the second heating reflux is preferably 60-70°C, more preferably 65°C; the first heating reflux time is preferably 1-3h, more preferably 2h.

[0052] After obtaining the mixture, the present invention heats and solidifies the mixture to obtain a multi-element doped phenolic resin.

[0053] In the present invention, the temperature of the heating and curing is preferably 150 to 160° C., and the time of the heating and curing is preferably 0.5 to 1 hour.

[0054] After obtaining the multi-element doped phenolic resin, the present invention performs carbonization heat treatment on the multi-element doped phenolic resin under a protective atmosphere to obtain the multi-element doped carbon material.

[0055] Before the carbonization heat treatment, the present invention preferably further comprises ball milling the multi-element doped phenolic resin; the rotation speed of the ball milling is preferably 60 to 600 r / min, and the time of the ball milling is preferably 30 to 900 min. The particle size of the phenolic resin powder obtained after ball milling is preferably 2 to 20 μm.

[0056] In the present invention, the protective atmosphere is preferably a nitrogen atmosphere or an argon atmosphere; the flow rate of the protective gas is preferably 1 to 20 L / min, more preferably 5 to 15 L / min.

[0057] In the present invention, the carbonization heat treatment preferably includes: first heating to 90-110°C and keeping warm for 50-70 min, second heating to 500-550°C and keeping warm for 50-70 min, and third heating to 800-1000°C and keeping warm for 120-240 min.

[0058] As a further preferred solution, the temperature after the first heating (i.e., the first heat preservation) is more preferably 95-105° C., and more preferably 100° C.; the first heat preservation time is more preferably 55-65 min, and more preferably 60 min;

[0059] The temperature after the second heating (i.e., the second heat preservation) is more preferably 510-540°C, and more preferably 520-530°C; the second heat preservation time is more preferably 55-65 minutes, and more preferably 60 minutes;

[0060] The temperature after the third heating (ie the third insulation) is more preferably 850-950° C., and further preferably 880-930° C.; the time of the third insulation is more preferably 150-210 min, and further preferably 170-190 min.

[0061] In the carbonization heat treatment process of the present invention, the phenolic resin is carbonized to form a carbon material, thereby obtaining a multi-element doped carbon material.

[0062] After obtaining the multi-element doped carbon material, the present invention etches the multi-element doped carbon material in a water vapor-inert gas mixture to form a porous structure, thereby obtaining multi-element doped porous carbon.

[0063] In the present invention, the etching conditions include: the temperature is preferably 450-550°C, more preferably 480-520°C; the holding time is preferably 60-120min, more preferably 80-100min; the water vapor flow rate is preferably 1-5L / min, more preferably 2-4L / min; the inert gas flow rate is preferably 1-15L / min, more preferably 5-10L / min.

[0064] In the present invention, the inert gas is preferably nitrogen or argon.

[0065] If only water vapor is used for etching, the etching will be severe and the reaction will be difficult to control; the present invention uses a water vapor-inert gas mixture for etching, and the etching is gentler and easier to control.

[0066] After being etched, the carbon material of the present invention forms a porous structure to obtain multi-element doped porous carbon.

[0067] The present invention adopts an in-situ doping method to prepare multi-element doped porous carbon. Not only is the doping method simple and easy, but the prepared porous carbon has uniform pore size and particle size, which is conducive to more uniform deposition of nano silicon particles.

[0068] The present invention provides a silicon-carbon negative electrode material, comprising silicon-carbon micron particles and a carbon layer coated on the surface of the silicon-carbon micron particles; the silicon-carbon micron particles comprise the multi-element doped porous carbon described in the above scheme, and nano-silicon particles located in the pores and / or surface of the multi-element doped porous carbon.

[0069] In the present invention, the mass content of Si in the silicon-carbon negative electrode material is 50-65%, preferably 52-63%, more preferably 55-60%; the mass content of C is 30-50%, preferably 32-45%, more preferably 33-41%. The molar content of N element in the silicon-carbon negative electrode material is preferably 0.5-3.0%, the molar content of S element is preferably 0.3-1.1%, the molar content of F element is preferably 0.3-1.1%, and the molar content of Li element is preferably 0.3-1.1%.

[0070] In the present invention, the average particle size of the silicon-carbon negative electrode material is preferably 2 to 15 μm, more preferably 5 to 13 μm, and further preferably 6 to 10 μm; the specific surface area is preferably 0.5 to 5 m 2 / g, more preferably 1 to 4.5 m 2 / g, more preferably 1.5 to 4 m 2 / g.

[0071] In the present invention, the size of the nano silicon particles is preferably 1-3 nm; the nano silicon particles preferably include crystalline nano silicon and amorphous nano silicon.

[0072] The present invention provides a method for preparing the silicon-carbon negative electrode material described in the above scheme, comprising the following steps:

[0073] Depositing silicon nanoparticles on multi-element doped porous carbon by cracking silane using chemical vapor deposition to obtain silicon carbon micron particles;

[0074] The silicon-carbon micron particles are carbon-coated to obtain the silicon-carbon negative electrode material.

[0075] In the present invention, the deposition of silicon nanoparticles on multi-element doped porous carbon by cracking silane using chemical vapor deposition preferably includes the following steps: under the protection of an inert atmosphere, the multi-element doped porous carbon is heated to a target temperature, a mixed gas including silane gas and an inert gas is introduced, chemical vapor deposition is performed, and silicon-carbon nanoparticles are obtained.

[0076] In the present invention, the silane gas is preferably one or more of monosilane, dimethylsilane, chlorosilane, chloromethylsilane and dichlorosilane; the intake rate of the silane gas is preferably 1-5 L / min; the temperature of the chemical vapor deposition is preferably 450-750°C, more preferably 500-700°C; the time of the chemical vapor deposition is preferably 60-120 min, more preferably 80-100 min; the inert gas is preferably nitrogen; the inlet flow rate of the inert gas is preferably 1-10 L / min.

[0077] After obtaining the silicon-carbon micron particles, the present invention performs carbon coating on the silicon-carbon micron particles to obtain the silicon-carbon negative electrode material.

[0078] In the present invention, the carbon coating preferably includes: cooling the silicon-carbon micron particles to a carbon coating temperature, and then introducing a mixture of a carbon source gas and an inert gas to perform carbon coating.

[0079] In the present invention, the temperature of the carbon coating is preferably 400-600°C, more preferably 450-550°C; the time of the carbon coating is preferably 60-120min, more preferably 80-100min; the flow rate of the carbon source gas is preferably 1-5L / min; the inert gas is preferably argon; the flow rate of the inert gas is preferably 1-10L / min.

[0080] The present invention provides the use of the silicon-carbon negative electrode material described in the above scheme or the silicon-carbon negative electrode material prepared by the preparation method described in the above scheme in a lithium ion battery.

[0081] The multi-element doped porous carbon and its preparation method, silicon-carbon negative electrode material and its preparation method and application provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0082] Example 1

[0083] S101 introduces nitrogen source, sulfur source and fluorine source into phenolic resin to obtain multi-element doped phenolic resin:

[0084] Phenol and deionized water are mixed, and the mass content of phenol in the mixed solution is 5%; urea, thiophene and lithium fluoride are added to the mixed solution, and the mass fractions are 4%, 2.5% and 2.5% of phenol respectively, and the solution is continuously stirred at 65°C for 2 hours; the mixed liquid is added to formaldehyde, the mass of formaldehyde is 60% of phenol, and the first heating reflux is carried out at a temperature of 65°C for 20 minutes; ammonia water with a mass fraction of 15% is introduced, and the amount of ammonia water added is 5% of the mass of phenol, and the second heating reflux reaction is carried out at a temperature of 65°C for 2 hours; then the temperature is raised to 150°C and cured for 0.5 hours to obtain a multi-element doped phenolic resin.

[0085] S102 calcined and carbonized the multi-element doped phenolic resin and etched it:

[0086] The multi-element doped phenolic resin is ball-milled at a speed of 550r / min for 30min, and the ball milling is repeated three times; the phenolic resin is placed in a high-temperature rotary furnace, nitrogen is introduced at 5L / min, and the temperature is first raised to 90°C and maintained for 60min; then the temperature is raised to 500°C and maintained for 60min; then the temperature is raised to 800°C and maintained for 120min to obtain a multi-element doped porous carbon precursor. After the porous carbon precursor is cooled to 450°C in the rotary furnace, the gas introduced is switched to a mixed gas of water vapor and nitrogen at flow rates of 2L / min and 8L / min, respectively, for 60min and then cooled to obtain a multi-element doped porous carbon.

[0087] The specific surface area of ​​the multi-element doped porous carbon is 1682 m 2 / g, pore volume is 0.81cm 3 / g, the micropore volume accounts for 65%, the average pore diameter is 2.9nm, and the XPS test shows that the molar content of nitrogen is 3.4%, the molar content of sulfur is 2.5%, the molar content of fluorine is 1.3%, and the molar content of lithium is 1.3%.

[0088] S103 deposits silane on porous carbon to obtain a silicon-carbon intermediate product (i.e., silicon-carbon micron particles) loaded with nano-silicon:

[0089] The porous carbon was placed in a high-temperature rotary furnace and argon gas was introduced for protection at a flow rate of 10 L / min; the temperature was raised to 550°C, and monosilane gas was introduced at 3 L / min for 60 min, and a silicon-carbon intermediate product loaded with nano-silicon was obtained after vapor deposition.

[0090] S104 performs carbon coating treatment on the silicon-carbon intermediate product to obtain a silicon-carbon negative electrode material:

[0091] When the temperature of the rotary furnace drops to 400°C, switch the gas flow to 3 L / min of acetylene and 10 L / min of argon, the coating time is 60 min, and cool to obtain the silicon-carbon negative electrode material.

[0092] The silicon-carbon negative electrode material has a silicon mass content of 52%, a carbon mass content of 41%, and the remainder is doped impurities, an average particle size of 7.2 μm, and a specific surface area of ​​3.6 m 2 / g.

[0093] Electrochemical performance test:

[0094] The electrochemical properties of the silicon-carbon negative electrode material prepared in this embodiment were tested. The silicon-carbon negative electrode material was used as an active substance, mixed evenly with conductive carbon black (SuperP) and polyacrylic acid binder (PAA) in a mass ratio of 96:1:3, and ultrapure water was used as a dispersant to coat the slurry on the surface of the copper foil.

[0095] The electrode sheet was dried in a vacuum drying oven at 120°C for 12 h, and then rolled and punched to obtain a silicon-carbon negative electrode sheet with an active material content of 2.0 mg / cm 2 ; A metal lithium sheet was used as the counter electrode, and 1 mol / L LiPF6 (ethylene carbonate EC: diethyl carbonate DEC = 1:1 (volume ratio)) was used as the electrolyte. The above silicon-carbon negative electrode sheets were assembled into button cells in a glove box, and the charge and discharge performance tests were carried out. The test steps were 0.1C, 0.05C, 0.02C, and 0.01C variable rate discharge to 0V, 0.1C charge to 2V, and cycled 1000 times.

[0096] The initial specific capacity of the silicon-carbon negative electrode is 2622mAh / g, the initial efficiency is 95.8%, and the capacity retention rate after 1000 cycles is 93.5%. The initial charge and discharge curve is as follows Figure 1 As shown, the long cycle performance is Figure 2 shown.

[0097] Example 2

[0098] S201 introduces nitrogen source, sulfur source and fluorine source into phenolic resin to obtain multi-element doped phenolic resin:

[0099] Phenol and deionized water are mixed, and the mass ratio of phenol in the mixed solution is 5%; ethylenediamine, ammonium thiocyanate and lithium fluoride are added to the mixed solution, and the mass fractions are 3%, 5% and 3% of phenol respectively, and the mixture is stirred continuously at 65°C for 2 hours; the mixed liquid is added to formaldehyde, the mass of formaldehyde is 80% of phenol, and the first heating reflux is carried out at 65°C for 20 minutes; ammonia water with a mass fraction of 15% is introduced, and the amount of ammonia water added is 7.5% of the mass of phenol, and the second heating reflux reaction is carried out at 65°C for 2 hours. Then the temperature is raised to 155°C and cured for 0.5 hours to obtain a multi-element doped phenolic resin.

[0100] S202 calcined and carbonized the multi-element doped phenolic resin and etched it:

[0101] The multi-element doped phenolic resin is ball-milled at a rotation speed of 550 r / min for 30 min, and the ball milling is repeated three times; then it is placed in a high-temperature rotary furnace, nitrogen is introduced at 5 L / min, the temperature is first raised to 100°C and maintained for 60 min; then the temperature is raised to 550°C and maintained for 50 min; then the temperature is raised to 850°C and maintained for 180 min to obtain a multi-element doped porous carbon precursor; after the porous carbon precursor is cooled to 480°C in the rotary furnace, the gas introduced is switched to a mixed gas of water vapor and nitrogen at flow rates of 3 L / min and 10 L / min respectively, which is maintained for 60 min and then cooled to obtain multi-element doped porous carbon.

[0102] The specific surface area of ​​the multi-element doped porous carbon is 1760 m 2 / g, pore volume is 0.97cm 3 / g, the micropore volume accounts for 70%, the average pore diameter is 2.6nm, the molar content of nitrogen is 4.6%, the molar content of sulfur is 3.2%, the molar content of fluorine is 1.9%, and the molar content of lithium is 1.9%.

[0103] S203 deposits silane on porous carbon to obtain a silicon-carbon intermediate product loaded with nano-silicon:

[0104] The porous carbon was placed in a high-temperature rotary furnace and argon gas was introduced for protection at a flow rate of 12 L / min; the temperature was raised to 600°C, and dimethylsilane gas was introduced at 3.5 L / min for 90 minutes. After vapor deposition, a silicon-carbon intermediate product loaded with nano-silicon was obtained.

[0105] S204 performs carbon coating treatment on the silicon-carbon intermediate product to obtain a silicon-carbon negative electrode material:

[0106] When the temperature of the rotary furnace drops to 450°C, switch the gas flow to cyclohexane at 2 L / min and argon at 8 L / min, the coating time is 90 min, and cool to obtain the silicon-carbon negative electrode material.

[0107] The silicon-carbon negative electrode material has a silicon mass content of 62%, a carbon mass content of 33%, an average particle size of 6.6 μm, and a specific surface area of ​​2.8 m 2 / g.

[0108] Electrochemical performance test:

[0109] Refer to the test method in Example 1.

[0110] The first specific capacity of the silicon-carbon negative electrode in this embodiment is 2737 mAh / g, the first efficiency is 96.3%, and the capacity retention rate after 1000 cycles is 92.2%.

[0111] Example 3

[0112] S301 introduces nitrogen source, sulfur source and fluorine source into phenolic resin to obtain multi-element doped phenolic resin:

[0113] Phenol and deionized water are mixed, and the mass ratio of phenol in the mixed solution is 17.5%; ethanolamine, thiourea oxide, and lithium fluoride are added to the mixed solution, and the mass fractions are 12%, 6%, and 5% of phenol, respectively, and stirred continuously at 65°C for 2 hours; the mixed liquid is added to formaldehyde, the mass of formaldehyde is 50% of phenol, and the first heating reflux is carried out at a temperature of 65°C for 20 minutes; ammonia water with a mass fraction of 15% is introduced, and the amount of ammonia water added is 10% of the mass of phenol, and the second heating reflux reaction is carried out at a temperature of 65°C for 2 hours. Then the temperature is raised to 160°C and cured for 0.5 hours to obtain a multi-element doped phenolic resin.

[0114] S302 calcined and carbonized the multi-element doped phenolic resin and etched it:

[0115] The multi-element doped phenolic resin is ball-milled at a rotation speed of 550 r / min for 30 min, and the ball milling is repeated three times; the phenolic resin is placed in a high-temperature rotary furnace, and nitrogen is introduced at 20 L / min. The temperature is first raised to 110° C. and maintained for 70 min; then the temperature is raised to 550° C. and maintained for 70 min; then the temperature is raised to 1000° C. and maintained for 240 min to obtain a multi-element doped porous carbon precursor; after the porous carbon precursor is cooled to 550° C. in the rotary furnace, the gas introduced is switched to a mixed gas of water vapor and nitrogen at flow rates of 5 L / min and 15 L / min, respectively, for 60 min and then cooled to obtain the multi-element doped porous carbon.

[0116] The specific surface area of ​​the multi-element doped porous carbon is 1923 m 2 / g, pore volume is 1.16cm 3 / g, the micropore volume accounts for 69%, the average pore diameter is 3.1nm, the molar content of nitrogen element is 8.7%, the molar content of sulfur element is 3.6%, the molar content of fluorine element is 3.3%, and the molar content of lithium element is 3.3%.

[0117] S303 deposits silane on porous carbon to obtain a silicon-carbon intermediate product loaded with nano-silicon:

[0118] The porous carbon was placed in a high-temperature rotary furnace and argon gas was introduced for protection at a flow rate of 15 L / min; the temperature was raised to 750°C, and chlorosilane gas was introduced at 5 L / min for 120 min. After vapor deposition, a silicon-carbon intermediate product loaded with nano-silicon was obtained.

[0119] S304 performs carbon coating treatment on the silicon-carbon intermediate product to obtain a silicon-carbon negative electrode material:

[0120] When the temperature of the rotary furnace drops to 500°C, switch the gas flow to 5 L / min of ethylene and 10 L / min of argon, the coating time is 120 min, and cool to obtain the silicon-carbon negative electrode material.

[0121] The silicon-carbon negative electrode material has a silicon mass content of 65%, a carbon mass content of 30%, an average particle size of 8.2 μm, and a specific surface area of ​​1.9 m 2 / g.

[0122] Electrochemical performance test:

[0123] Refer to the test method in Example 1.

[0124] In this embodiment, the first specific capacity of the silicon-carbon negative electrode is 2793 mAh / g, the first efficiency is 95.3%, and the capacity retention rate after 1000 cycles is 92.0%.

[0125] Comparative Example 1

[0126] S401 synthesizes phenolic resin without element doping as follows:

[0127] Phenol and deionized water are mixed, and the mass ratio of phenol in the solution is 5%; the mixed liquid is added to formaldehyde, the mass of formaldehyde is 60% of the mass of phenol, and the first heating reflux is carried out at a temperature of 65°C for 20 minutes; ammonia water with a mass fraction of 15% is introduced, and the amount of ammonia water added is 5% of the mass of phenol, and the second heating reflux reaction is carried out at a temperature of 65°C for 2 hours. Then the temperature is raised to 150°C and cured for 0.5 hours to obtain phenolic resin.

[0128] S402 calcined and carbonized the phenolic resin and etched it to obtain porous carbon:

[0129] Refer to the treatment method in Example 1.

[0130] The specific surface area of ​​the porous carbon obtained is 1043m 2 / g, pore volume is 0.44cm 3 / g, the micropore volume accounts for 36%, the average pore diameter is 6.3nm, and the molar content of nitrogen, sulfur, fluorine and lithium elements is 0%.

[0131] S403 deposits silane on porous carbon to obtain a silicon-carbon intermediate product loaded with nano-silicon:

[0132] Refer to the treatment method in Example 1.

[0133] S404 performs carbon coating treatment on the silicon-carbon intermediate product to obtain a silicon-carbon negative electrode material:

[0134] Refer to the treatment method in Example 1.

[0135] The silicon-carbon negative electrode material of this embodiment has a silicon mass content of 42%, a carbon mass content of 51%, an average particle size of 7.2 μm, and a specific surface area of ​​8.6 m 2 / g.

[0136] Electrochemical performance test:

[0137] Refer to the test method in Example 1.

[0138] The first specific capacity of the silicon-carbon negative electrode in this comparative example is 1613 mAh / g, the first efficiency is 82.4%, and the capacity retention rate after 1000 cycles is 53.3%. Compared with Example 1, the data of this comparative example show that the absence of impurity doping in porous carbon will reduce the silicon loading capacity, and the first coulombic efficiency and cycle stability of the obtained silicon-carbon negative electrode are lower.

[0139] Comparative Example 2

[0140] S501 introduces nitrogen source and sulfur source into phenolic resin to obtain N and S doped phenolic resin:

[0141] Phenol and deionized water are mixed, and the mass ratio of phenol in the solution is 17.5%; ethanolamine and thiourea oxide are added to the mixed solution, and the mass fractions are 12% and 6% of phenol respectively, and the mixture is stirred continuously at 65°C for 2 hours; the mixed liquid is added to formaldehyde, the mass of formaldehyde is 50% of phenol, and the first heating reflux is carried out at 65°C for 20 minutes; ammonia water with a mass fraction of 15% is introduced, and the amount of ammonia water added is 10% of the mass of phenol, and the second heating reflux reaction is carried out at 65°C for 2 hours. Then the temperature is raised to 160°C and cured for 0.5 hours to obtain N and S doped phenolic resin.

[0142] S502 calcined and carbonized N and S doped phenolic resin and etched to obtain porous carbon:

[0143] Refer to the treatment method in Example 1.

[0144] The specific surface area of ​​the porous carbon is 1706 m 2 / g, pore volume is 0.98cm 3 / g, the micropore volume accounts for 64%, the average pore diameter is 3.2nm, the molar content of nitrogen is 13%, the molar content of sulfur is 7%, and the molar content of fluorine and lithium is 0%.

[0145] S403 deposits silane on porous carbon to obtain a silicon-carbon intermediate product loaded with nano-silicon:

[0146] Refer to the treatment method in Example 1.

[0147] S404 performs carbon coating treatment on the silicon-carbon intermediate product to obtain a silicon-carbon negative electrode material:

[0148] Refer to the treatment method in Example 1.

[0149] The silicon-carbon negative electrode material has a silicon mass content of 50%, a carbon mass content of 45%, an average particle size of 7.5 μm, and a specific surface area of ​​6.2 m 2 / g.

[0150] Electrochemical performance test:

[0151] Refer to the test method in Example 1.

[0152] The first specific capacity of the silicon-carbon negative electrode in Comparative Example 2 is 2213 mAh / g, the first efficiency is 82.4%, and the capacity retention rate after 1000 cycles is 78.7%. Compared with Example 1, the data of this comparative example show that the fluorine and lithium elements in the porous carbon are related to the formation of SEI; the silicon-carbon negative electrode made of porous carbon without fluorine and lithium elements has lower first coulombic efficiency and cycle stability.

[0153] Comparative Example 3

[0154] S601 synthesizes F and Li doped phenolic resin as follows:

[0155] Phenol and deionized water are mixed, wherein the mass ratio of phenol in the solution is 17.5%; lithium fluoride is added to the mixed solution, wherein the mass fraction is 5% of the phenol, and the solution is continuously stirred at 65°C for 2 hours; the mixed liquid is added to formaldehyde, wherein the mass of the formaldehyde is 50% of the phenol, and the solution is heated and refluxed for the first time at 65°C for 20 minutes; ammonia water with a mass fraction of 15% is introduced, wherein the amount of ammonia water added is 10% of the mass of the phenol, and the solution is heated and refluxed for the second time at 65°C for 2 hours, and then the temperature is raised to 160°C and cured for 0.5 hours to obtain F and Li doped phenolic resin.

[0156] S502: F and Li doped phenolic resin is calcined and etched to obtain porous carbon:

[0157] Refer to the treatment method in Example 1.

[0158] The specific surface area of ​​the porous carbon is 1365 m 2 / g, pore volume is 0.51cm 3 / g, the micropore volume accounts for 57%, the average pore diameter is 4.2nm, the molar content of nitrogen and sulfur elements is 0, and the molar content of fluorine and lithium elements is 3.7%.

[0159] S403 deposits silane on porous carbon to obtain a silicon-carbon intermediate product loaded with nano-silicon:

[0160] Refer to the treatment method in Example 1.

[0161] S404 performs carbon coating treatment on the silicon-carbon intermediate product to obtain a silicon-carbon negative electrode material:

[0162] Refer to the treatment method in Example 1.

[0163] The silicon-carbon negative electrode material has a silicon mass content of 48%, a carbon mass content of 46%, an average particle size of 6.9 μm, and a specific surface area of ​​3.2 m 2 / g.

[0164] Electrochemical performance test:

[0165] Refer to the test method in Example 1.

[0166] The first specific capacity of the silicon-carbon negative electrode in Comparative Example 3 is 2013 mAh / g, the first efficiency is 93.4%, and the capacity retention rate after 1000 cycles is 95.5%. Compared with Example 1, the data of this comparative example show that the sulfur and nitrogen elements in the porous carbon are related to the silicon loading; the silicon content of the silicon-carbon negative electrode made of porous carbon without doping sulfur and nitrogen elements is lower, so the specific capacity is lower.

[0167] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A multi-element doped porous carbon, It is characterized in that The doping elements include N, S, F and Li elements; in the multi-element doped porous carbon, the molar content of the N element is 2.1-9.5%, the molar content of the S element is 1.0-3.6%, the molar content of the F element is 1.0-3.3%, and the molar content of the Li element is 1.0-3.3%.

2. The multi-element doped porous carbon according to claim 1, It is characterized in that The specific surface area of ​​the multi-element doped porous carbon is 1400 to 1950 m 2 / g, average pore diameter of 0.8-5nm, particle size of 2-15μm, pore volume of 0.5-1.2cm 3 / g, and the micropore volume accounts for 65-80%.

3. The method for preparing the multi-element doped porous carbon according to claim 1 or 2, It is characterized in that The following steps are involved: A nitrogen source, a sulfur source, lithium fluoride, phenol, formaldehyde, a catalyst and water are mixed, and the obtained mixture is heated and cured to obtain a multi-element doped phenolic resin; the mass of the nitrogen source is 3-15% of the mass of the phenol; the mass of the sulfur source is 2-7.5% of the mass of the phenol; the mass of the lithium fluoride is 2.5-5% of the mass of the phenol; Under a protective atmosphere, subjecting the multi-element doped phenolic resin to a carbonization heat treatment to obtain a multi-element doped carbon material; The multi-element doped carbon material is etched in a water vapor-inert gas mixture to form a porous structure, thereby obtaining multi-element doped porous carbon.

4. The preparation method according to claim 3, It is characterized in that The nitrogen source is one or more of urea, melamine, ethylenediamine, dicyandiamide, n-butylamine, ethanolamine, imidazole and pyridine; The sulfur source is one or more of sublimated sulfur, oxidized thiourea, thiophene, ammonium thiocyanate and ammonium persulfate.

5. The preparation method according to claim 3, It is characterized in that The carbonization heat treatment includes: first heating to 90-110° C. and keeping warm for 50-70 min, second heating to 500-550° C. and keeping warm for 50-70 min, and third heating to 800-1000° C. and keeping warm for 120-240 min.

6. The preparation method according to claim 3, It is characterized in that The etching conditions include: a temperature of 450-550° C., a heat preservation time of 60-120 min; a water vapor flow rate of 1-5 L / min, and an inert gas flow rate of 1-15 L / min.

7. A silicon-carbon negative electrode material, It is characterized in that It comprises silicon-carbon micron particles and a carbon layer coated on the surface of the silicon-carbon micron particles; the silicon-carbon micron particles comprise multi-element doped porous carbon, and nano-silicon particles located in the pores and / or the surface of the multi-element doped porous carbon; The mass content of Si in the silicon-carbon negative electrode material is 50-65%, and the mass content of C is 30-50%; The multi-element doped porous carbon is the multi-element doped porous carbon according to claim 1 or 2 or the multi-element doped porous carbon prepared by the preparation method according to any one of claims 3 to 6.

8. The silicon-carbon negative electrode material according to claim 7, It is characterized in that The average particle size is 2-15 μm, and the specific surface area is 0.5-5 m 2 / g, wherein the size of the nano silicon particles is 1 to 3 nm.

9. The method for preparing the silicon-carbon negative electrode material according to claim 7 or 8, It is characterized in that The following steps are involved: Depositing silicon nanoparticles on multi-element doped porous carbon by cracking silane using chemical vapor deposition to obtain silicon carbon micron particles; The silicon-carbon micron particles are carbon-coated to obtain the silicon-carbon negative electrode material.

10. Use of the silicon-carbon negative electrode material according to claim 7 or 8 or the silicon-carbon negative electrode material prepared by the preparation method according to claim 9 in lithium-ion batteries.

Citation Information

Patent Citations

  • Negative electrode material, preparation method thereof and lithium ion battery

    CN115706211A

  • Negative electrode material and preparation method thereof, battery and terminal

    CN116190596A

  • Easily separated nickel and boron doped carbon nitride catalyst and preparation method thereof

    CN116328814A

Cited By

  • Silicon-carbon negative electrode material and preparation method and application thereof

    CN119153671A

  • Silicon-carbon material and preparation method thereof, porous carbon substrate, negative electrode material and battery

    CN119812286A

  • Silicon-carbon material, method of making the same, porous carbon substrate, negative electrode material, and battery

    CN119812286B

  • Silicon-carbon negative electrode material and preparation method thereof, negative electrode plate and secondary battery

    CN119864392A

  • Resin material with high carbon formation rate as well as preparation method and application thereof

    CN120289785A