Flame-retardant resin composition

A resin composition with modified polyphenylene ether and aryloxycyclic phosphazene compound addresses the challenges of high dielectric loss and flame retardancy in high-frequency applications, ensuring excellent dielectric properties and thermal stability.

JP7557119B2Active Publication Date: 2024-09-27FUSHIMI PHARMA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020005239
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-16
Publication Date
2024-09-27
Estimated Expiration
2040-01-16

AI Technical Summary

Technical Problem

Existing resin compositions used in high-frequency signal applications, such as those in 5G communication systems, face challenges with high dielectric loss, poor thermal stability, and inadequate flame retardancy, particularly when using conventional flame retardants that can degrade over time or impair mechanical and dielectric properties.

Method used

A resin composition comprising a modified polyphenylene ether compound with carbon-carbon unsaturated double bonds and an aryloxycyclic phosphazene compound as a flame retardant, which maintains excellent dielectric properties and thermal stability while providing high glass transition temperature.

Benefits of technology

The composition achieves superior dielectric properties, flame retardancy, and thermal stability, making it suitable for high-frequency applications without compromising mechanical strength or long-term reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557119000011
    Figure 0007557119000011
  • Figure 0007557119000018
    Figure 0007557119000018
  • Figure 0007557119000005
    Figure 0007557119000005
Patent Text Reader

Abstract

To provide a resin composition which exhibits excellent dielectric characteristics, has flame retardancy and thermal stability, and also has a high glass transition temperature.SOLUTION: A flame-retardant resin composition contains (A) a modified polyphenylene ether compound terminal-modified with a substituent having a carbon-carbon unsaturated double bond, (B) a compound having a carbon-carbon unsaturated double bond in the molecule, and (C) a flame retardant. The flame retardant (C) is an aryloxy cyclic phosphazene compound represented by the following formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, in particular, a flame-retardant resin composition. [Background technology]

[0002] Systems that handle high-frequency signals are being put into practical use in industrial fields related to automobiles, ITS (Intelligent Transport Systems), IoT (Internet of Things), 5th generation mobile communication systems (5G), etc. Accordingly, the signal transmission speed in the electrical and electronic devices essential to these systems, such as electronic components such as semiconductors and printed wiring boards on which these components are mounted, is becoming extremely high, with frequencies reaching several tens of GHz.

[0003] Conventionally, resins such as phenolic resin, epoxy resin, and polyimide resin have been used for printed wiring boards. Although these resins have a well-balanced variety of performance, they have a large dielectric loss in the high frequency range, and alternative materials are desired.

[0004] On the other hand, polyphenylene ether resins are known to have low relative dielectric constants and dielectric loss tangents in the high frequency range, and are therefore suitable for use in printed wiring boards for electronic devices that operate in the high frequency range.

[0005] In order to increase the signal transmission speed and reduce transmission loss, printed wiring boards are required to have excellent dielectric properties (low relative dielectric constant and dielectric tangent, i.e., small transmission loss), as well as mechanical properties, thermal stability, and flame retardancy, and flame retardants are used as necessary.

[0006] Flame retardants used for resins of printed wiring boards are generally broadly divided into inorganic flame retardants and organic flame retardants. Examples of inorganic flame retardants include metal hydroxides such as aluminum hydroxide and magnesium hydroxide, antimony compounds such as red phosphorus, antimony trioxide and antimony pentoxide, and boron compounds. On the other hand, examples of organic flame retardants include halogen compounds such as chlorinated paraffin, bis(pentabromophenyl)ethane, brominated polystyrene, and tetrabromobisphenol A, phosphorus compounds such as triphenyl phosphate (TPP), tricresyl phosphate (TCP), and bisphenol A bis(diphenyl phosphate) (BDP), and halogenated phosphorus compounds such as tris(chloroethyl)phosphate (TCEP) and tris(β-chloropropyl)phosphate (TCPP).

[0007] Inorganic flame retardants generally have excellent dielectric properties and are unlikely to impair the dielectric properties of resins, but because they are water absorbent and hydrolyzable, their use is likely to cause deterioration over time of the mechanical and dielectric properties of resin molded bodies, making them unsuitable as flame retardants for resin materials for electrical and electronic devices that require long-term reliability. On the other hand, the use of organic flame retardants, especially halogen-based compounds, is limited from the perspective of the demand for halogen-free environmental compatibility. On the other hand, phosphorus-based compounds have plasticity, so increasing the amount added to the resin to increase flame retardancy may impair the mechanical strength of the resin molded body. In addition, because they are easily hydrolyzed, their use leads to deterioration over time of the dielectric properties of the resin molded body.

[0008] Therefore, phosphazene compounds, which are organic-inorganic hybrid materials, have been attracting attention as flame retardants to be used in resins. Phosphazene compounds are phosphorus-containing compounds, but because they have a higher phosphorus content than other organic phosphorus compounds, such as organic phosphate esters, it is possible to impart the required flame retardancy to resin molded products by reducing the amount added to the resin material. In addition, because they have low plasticity and hydrolysis, they are less likely to cause a decrease in the mechanical properties and dielectric properties of resin molded products or to deteriorate over time.

[0009] Patent Document 1 discloses a phosphazene compound substituted with 2,2'-biphenol and an epoxy resin composition containing the same, and describes that the epoxy resin molded body is preferably used as a substrate material in the applications of electric, electronic, and communication devices. However, the relative dielectric constant and dielectric loss tangent of a thermosetting resin composition such as an epoxy resin are high, and the use is limited in applications that handle high-frequency signals. On the other hand, Patent Documents 2 to 4 disclose a composition of a phosphazene compound substituted with 2,2'-biphenol and an imide-based resin and a molded body thereof, and describes that the use is preferably used as a substrate material in the applications of electric, electronic, and communication devices. However, although the relative dielectric constant and dielectric loss tangent of the imide-based resin molded body are lower than those of the epoxy resin, the use is limited in industrial fields such as the fifth generation mobile communication system (5G) that handles high-frequency signals. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2019 / 198766 [Patent Document 2] China Patent Publication No. 110204862 [Patent Document 3] Taiwan Patent Publication No. 201940589 [Patent Document 4] International Publication No. 2020 / 004440 Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present invention is to provide a resin composition which exhibits excellent dielectric properties, as well as flame retardancy, thermal stability, and a high glass transition temperature. [Means for solving the problem]

[0012] The resin composition used in the present invention is a flame-retardant resin composition comprising: (A) a modified polyphenylene ether compound terminally modified with a substituent having a carbon-carbon unsaturated double bond; (B) a compound having a carbon-carbon unsaturated double bond in its molecule; and (C) a flame retardant, wherein the flame retardant (C) is an aryloxy cyclic phosphazene compound represented by the following formula (1).

[0013] [ka]

[0014] In formula (1), n ​​represents an integer of 3 to 8, and the R group is an aryloxy group represented by the following formula (2) or (3).

[0015] [ka]

[0016] [ka]

[0017] In formula (2) and formula (3), R 1 and R 4 represents a single bond, an oxygen atom, or a methylene group; R 2 , R 3 , R 5 and R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and p, q, r and s each independently represent an integer of 1 to 4.

[0018] In the modified polyphenylene ether compound used in the present invention, the substituent having a carbon-carbon unsaturated double bond is at least one type of substituent selected from the group consisting of a vinylphenyl group, a vinylbenzyl group, an acryloyl group and a methacryloyl group.

[0019] The aryloxy cyclic phosphazene compound used in the present invention is a compound of formula (1) in which n is 3 or 4, or a mixture containing 95% by weight or more of compounds of formula (1) in which n is 3 and 4.

[0020] The aryloxy cyclic phosphazene compound used in the present invention preferably has an acid value of 0.05 mgKOH / g or less.

[0021] Furthermore, the aryloxy cyclic phosphazene compound used in the present invention preferably has a water content of 100 mg / kg or less as measured by the Karl Fischer method.

[0022] Another aspect of the present invention relates to a resin molded article made of a flame-retardant resin composition.

[0023] A further aspect of the present invention relates to an electric / electronic component including a resin molded article. Effect of the Invention

[0024] Since the flame-retardant resin composition according to the present invention uses a specific aryloxy cyclic phosphazene compound, it is possible to form a resin molded article which exhibits excellent dielectric properties, as well as flame retardancy and thermal stability and a high glass transition temperature.

[0025] The electric / electronic part according to the present invention contains the resin molded article according to the present invention, and therefore exhibits excellent dielectric properties, as well as excellent flame retardancy and thermal stability, and has a high glass transition temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The resin composition of the present invention is a resin composition comprising: (A) a modified polyphenylene ether compound terminally modified with a substituent having a carbon-carbon unsaturated double bond; (B) a compound having a carbon-carbon unsaturated double bond in its molecule; and (C) a flame retardant, wherein the flame retardant (C) contains an aryloxy cyclic phosphazene compound represented by the following formula (1):

[0027] [ka]

[0028] Hereinafter, each component of the resin composition according to this embodiment will be specifically described.

[0029] The (A) modified polyphenylene ether compound used in the present invention, which has been terminally modified with a substituent having a carbon-carbon unsaturated double bond, is, but is not particularly limited to, a compound having a polyphenylene ether structure in the compound, the terminal of which has been modified with a vinylphenyl group, a vinylbenzyl group, an acryloyl group or a methacryloyl group.

[0030] The (A) modified polyphenylene ether compound used in the present invention, which is terminally modified with a substituent having a carbon-carbon unsaturated double bond, is not particularly limited as long as it has a polyphenylene ether structure, and can be represented, for example, as a compound of the following formula (4).

[0031] [ka]

[0032] In formula (4), X represents a divalent group represented by the following formula (5).

[0033] [ka]

[0034] In formula (5), R 7 and R 8 each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group having 1 to 6 carbon atoms, or a phenyl group. a and b each independently represent an integer of 1 to 4, and l and m each independently represent an integer of 1 to 30. B represents a divalent group represented by the following formula (6) or (7).

[0035] [ka]

[0036] [ka]

[0037] In formula (6), R 9 each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group having 1 to 6 carbon atoms, or a phenyl group; and c represents an integer of 1 to 4.

[0038] In formula (7), R 10 and R 11 each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group having 1 to 6 carbon atoms, or a phenyl group, and d and e each independently represent an integer of 1 to 4. A represents a single bond, an oxygen atom, or a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms. Examples of A include -CH2-, -CHCH3- and -C(CH3)2-.

[0039] Furthermore, in formula (4), the group represented by Z is a substituent having a carbon-carbon unsaturated double bond, and can be represented by the following formula (8) or formula (9).

[0040] [ka]

[0041] [ka]

[0042] In formula (8), R 12 and R 13each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Each g independently represents an integer of 1 to 4, and h represents 0 or 1. Specific examples include a vinylphenyl group and a vinylbenzyl group.

[0043] In addition, in formula (9), R 14 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. Specific examples include an acryloyl group and a methacryloyl group.

[0044] The component (B) of the present invention is not particularly limited as long as it is a compound having a carbon-carbon unsaturated double bond in the molecule, but it may be any compound capable of reacting with a modified polyphenylene ether compound whose terminal is modified by a substituent having a carbon-carbon unsaturated double bond. The compound is preferably a compound having two or more carbon-carbon double bonds.

[0045] Examples of the compound used as component (B) include a polyfunctional methacrylate compound having two or more methacrylic groups in the molecule, a polyfunctional acrylate compound having two or more acrylic groups in the molecule, a polyfunctional vinyl compound having two or more vinyl groups in the molecule such as polybutadiene, a vinylbenzyl compound such as divinylbenzene having a vinylbenzyl group in the molecule, and a polyfunctional maleimide compound having two or more maleimide groups in the molecule. In addition, styrene-butadiene copolymers, trialkenyl isocyanurate compounds such as triallyl isocyanurate (TAIC), trialkenyl cyanurates such as triallyl cyanurate (TAC), and the like are suitable examples. By using such compounds, a resin composition having excellent thermal stability and without impairing dielectric properties can be obtained. These compounds may be used alone or in combination of two or more.

[0046] Next, the aryloxy cyclic phosphazene compound which is the flame retardant of the component (C) of the present invention will be described. The flame retardant used in this embodiment contains an aryloxy cyclic phosphazene compound represented by the following formula (1).

[0047] [ka]

[0048] In formula (1), n ​​represents an integer of 3 to 8, and the R group is an aryloxy group represented by the following formula (2) or (3).

[0049] [ka]

[0050] [ka]

[0051] In formula (2) and formula (3), R 1 and R 4 represents a single bond, an oxygen atom, or a methylene group; R 2 , R 3 , R 5 and R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and p, q, r and s each independently represent an integer of 1 to 4.

[0052] In formula (1), n ​​represents an integer of 3 to 8. Thus, the aryloxy cyclic phosphazene compound represented by formula (1) is an aryloxycyclotriphosphazene compound (trimer) in which n is 3, an aryloxycyclotetraphosphazene compound (tetramer) in which n is 4, an aryloxycyclopentaphosphazene compound (pentamer) in which n is 5, an aryloxycyclohexaphosphazene compound (hexamer) in which n is 6, an aryloxycycloheptaphosphazene compound (septamer) in which n is 7, or an aryloxycyclooctaphosphazene compound (octamer) in which n is 8.

[0053] These aryloxy cyclic phosphazene compounds with smaller n are more likely to realize resin molded articles with excellent dielectric properties when used in the composition of the present invention, so n is preferably an integer of 3 to 6, and particularly preferably 3 or 4. The aryloxy cyclic phosphazene compounds may be a mixture of two or more compounds with different n, but this mixture with a higher content of aryloxy cyclic phosphazene compounds with smaller n is more likely to realize resin molded articles with excellent dielectric properties when used in the composition of the present invention. Therefore, as the mixture of aryloxy cyclic phosphazene compounds with different n, a mixture containing 95% by weight or more of cyclic phosphazene compounds with n of 3 to 6 is preferred, and a mixture containing 95% by weight or more of cyclic phosphazene compounds with n of 3 and 4 is particularly preferred.

[0054] Cyclic phenoxyphosphazene compounds, such as hexaphenoxycyclotriphosphazene, are generally soluble in the resin component (a mixture of the above-mentioned component (A) and the above-mentioned component (B)). However, the aryloxy cyclic phosphazene compound of the present invention has a high melting point and is poorly soluble or insoluble in the above-mentioned resin component. This makes it possible to obtain a flame-retardant resin composition that is excellent in flame retardancy and thermal stability and has a high glass transition temperature without impairing the dielectric properties of the resin.

[0055] The melting point of the aryloxy cyclic phosphazene compound is obtained by measuring with differential thermal analysis. In the differential thermal curve obtained by heating a measurement sample in a temperature range from room temperature to 600°C at 10°C / min under a nitrogen atmosphere, the melting point is defined as the temperature at the apex of an endothermic peak at which melting can be confirmed at the beginning of heating. The melting point of the aryloxy cyclic phosphazene compound is preferably equal to or higher than the temperature at which the resin molded product is used. The melting point of the aryloxy cyclic phosphazene compound is preferably 300°C, more preferably 330°C, and even more preferably 350°C or higher.

[0056] On the other hand, a useful index of thermal stability can be obtained by measuring the 5% weight loss temperature by thermogravimetric analysis. The temperature at which a measurement sample loses 5% of its initial weight under a nitrogen atmosphere is defined as the 5% weight loss temperature. The 5% weight loss temperature of the aryloxy cyclic phosphazene compound is preferably equal to or higher than the temperature at which the resin molded product is used. The 5% weight loss temperature of the aryloxy cyclic phosphazene compound is preferably 360°C, more preferably 380°C, and even more preferably 400°C or higher.

[0057] The acid value of the aryloxy cyclic phosphazene compound represented by formula (1) used in the flame retardant resin composition of the present invention is preferably 0.15 mg KOH / g or less, more preferably 0.10 mg KOH / g or less, and particularly preferably 0.01 mg KOH / g or less. If the acid value of the aryloxy cyclic phosphazene compound exceeds 0.15 mg KOH / g, the dielectric properties may be impaired. The acid value of the aryloxy cyclic phosphazene compound can be measured, for example, according to JIS K0070 "Testing method for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products".

[0058] The moisture content of the aryloxy cyclic phosphazene compound used in the flame retardant resin composition of the present invention is preferably 1,000 mg / kg or less, more preferably 500 mg / kg or less, and particularly preferably 100 mg / kg or less. The aryloxy cyclic phosphazene compound represented by formula (1) may have a deteriorated dielectric property if the moisture content exceeds 1,000 mg / kg. The moisture content of the aryloxy cyclic phosphazene compound can be measured, for example, by the Karl Fischer method according to JIS K0068 "Method for measuring moisture content in chemical products".

[0059] In the flame-retardant resin composition of the present invention, two or more of the above-mentioned aryloxy cyclic phosphazene compounds may be used in combination.

[0060] The flame-retardant resin composition of the present invention may be used as a resin varnish prepared by mixing with a solvent capable of dissolving the resin component. Such a resin varnish can be prepared, for example, as follows.

[0061] First, the modified polyphenylene ether compound (A) whose terminals have been modified by a substituent having a carbon-carbon unsaturated double bond and the compound (B) whose molecule has a carbon-carbon unsaturated double bond are dissolved in an organic solvent. At this time, heating may be performed as necessary. Then, the aryloxy cyclic phosphazene compound (C) which is a component that is not soluble in an organic solvent is added, and dispersed using a disperser, ball mill, bead mill, planetary mixer, roll mill, or the like to prepare a varnish-like resin composition. At this time, various additives described later may be added. The organic solvent used here is not particularly limited as long as it dissolves the modified polyphenylene ether compound (A) whose terminals have been modified by a substituent having a carbon-carbon unsaturated double bond and the compound (B) whose molecule has a carbon-carbon unsaturated double bond and does not inhibit the reaction between them. Specifically, toluene, methyl ethyl ketone, cyclohexanone, and the like can be mentioned. These may be used alone or in combination of two or more.

[0062] The resin varnish used in the present invention preferably further contains a polymerization initiator. In the case of reacting by heating, examples of the polymerization initiator that can be used include peroxides such as benzoyl peroxide, dicumyl peroxide, and diisopropyl peroxydicarbonate, azo compounds such as 2,2-azobisisobutyronitrile (AIBN), azobis-2,4-dimethylvaleronitrile, azobiscyclohexylnitrile, azobiscyanovaleric acid, and 2,2-azobis(2-methylbutyronitrile), and acid generators such as aromatic sulfonates.

[0063] The content of the aryloxy cyclic phosphazene compound in the flame-retardant resin composition of the present invention can be appropriately set according to various conditions such as the type of resin component and the use of the composition of the present invention, but it is usually set to 0.1 to 200 parts by weight, more preferably 0.5 to 100 parts by weight, and particularly preferably 1 to 50 parts by weight, relative to 100 parts by weight of the resin component in terms of solid content. If the content of the aryloxy cyclic phosphazene compound is less than 0.1 parts by weight, it may be difficult to obtain a resin molded product that exhibits sufficient flame retardancy. On the other hand, if the content of the aryloxy cyclic phosphazene compound exceeds 200 parts by weight, the inherent properties of the resin component may be impaired, and it may be difficult to obtain a resin molded product that exhibits the properties due to the resin component.

[0064] In addition, in the case where the reaction is caused by irradiation with energy rays, examples of the polymerization initiator that can be used include acetophenone-based photopolymerization initiators, benzophenone-based photopolymerization initiators, benzoin-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, sulfonium-based photopolymerization initiators, and iodonium-based photopolymerization initiators, etc. In this case, a sensitizer such as a tertiary amine can be used in combination as necessary.

[0065] The flame-retardant resin composition of the present invention may contain a glass substrate in addition to the above-mentioned components (A), (B) and (C), thereby making it possible to suppress defects during processing such as cracking, dimensional changes and warping, and to improve dimensional stability and mechanical strength after processing.

[0066] The glass substrate to be used is not particularly limited, but it is preferable to use a glass substrate having a low relative dielectric constant. More specifically, it is preferable to set the relative dielectric constant of the glass substrate so that the relative dielectric constant of the resin molded body at 10 GHz is 4.0 or less.

[0067] As such a glass substrate, a commercially available glass substrate can be used, and for example, "E glass (relative dielectric constant 6.8)" or "NE glass (relative dielectric constant 4.8)" manufactured by Nitto Boseki Co., Ltd. can be preferably used.

[0068] The flame-retardant resin composition of the present invention can be blended with various additives within a range that does not impair the intended physical properties depending on the application, the type of resin component, etc. Examples of additives that can be used include inorganic fillers such as natural silica, calcined silica, synthetic silica, amorphous silica, white carbon, alumina, aluminum hydroxide, magnesium hydroxide, calcium silicate, calcium carbonate, zinc borate, zinc stannate, titanium oxide, zinc oxide, molybdenum oxide, zinc molybdate, natural mica, synthetic mica, aerosil, kaolin, clay, talc, calcined kaolin, calcined clay, calcined talc, wollastonite, glass short fiber, glass fine powder, hollow glass, and potassium titanate fiber, nanocarbons such as nanocarbon tubes, graphene, and fullerene, organic fibers such as aramid fiber and polyparaphenylene benzobisoxazole fiber, surface treatment agents for fillers such as silane coupling agents, waxes, fatty acids and their metal salts, release agents such as acid amides and paraffin, chlorinated Examples of flame retardants include phosphorus-based flame retardants such as paraffin, phosphate ester, condensed phosphate ester, phosphoric acid amide, phosphoric acid amide ester, phosphinate, phosphinate salt, ammonium phosphate, and red phosphorus; nitrogen-based flame retardants such as melamine, melamine cyanurate, melam, melem, melon, and succinoguanamine; flame retardants such as silicone-based flame retardants and bromine-based flame retardants; flame retardant assistants such as antimony trioxide; dripping inhibitors such as polytetrafluoroethylene (PTFE); ultraviolet absorbers such as benzotriazole; antioxidants such as hindered phenols and styrenated phenols; photopolymerization initiators such as thioxanthone-based initiators; fluorescent brightening agents such as stilbene derivatives; curing agents, dyes, pigments, colorants, light stabilizers, photosensitizers, thickeners, lubricants, defoamers, leveling agents, gloss agents, polymerization inhibitors, thixotropy-imparting agents, plasticizers, and antistatic agents.

[0069] The resin molded article formed using the flame-retardant resin composition of the present invention has excellent flame retardancy and thermal stability, and has a high glass transition temperature, and can therefore be used for a variety of applications and purposes in various industrial fields. In particular, the resin molded article has excellent dielectric properties due to its low relative dielectric constant and dielectric loss, and is useful in electrical and electronic parts. For example, the resin molded article is useful as an electrical and electronic part for semiconductor sealing or circuit board applications (particularly, metal-clad laminates, substrates for printed wiring boards, adhesives for printed wiring boards, adhesive sheets for printed wiring boards, insulating circuit protection films for printed wiring boards, conductive pastes for printed wiring boards, sealants for multilayer printed wiring boards, circuit protection agents, coverlay films or cover inks). EXAMPLES

[0070] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these in any way.

[0071] In the following, the "unit" in "unit mol" means the smallest structural unit of a cyclic phosphazene compound, for example, (NPO2R) in the case of formula (1). In the case of a chlorocyclophosphazene compound, the "unit" is (NPCl2) and 1 unit mol is 115.87 g. In the following, unless otherwise specified, "%" and "parts" mean "% by weight" and "parts by weight", respectively.

[0072] Flame retardants used in the examples The flame retardants used in the examples are as follows. Various cyclic phosphazene compounds prepared as flame retardants for the examples are as follows: 1 H- and 31 The identification was based on the results of P-NMR and TOF-MS.

[0073] The dielectric properties were measured using a cavity resonator for powder measurement manufactured by AET Corporation, measuring the relative permittivity and dielectric loss tangent at a temperature of 25°C and a frequency of 10 GHz. Thermal stability was also measured using a thermogravimetric measuring device (model number "STA7200" manufactured by Hitachi High-Technologies Corporation) to measure the 5% weight loss temperature in thermogravimetry when heated at 10°C / min in a temperature range from room temperature to 600°C in a nitrogen atmosphere. The melting point was measured by differential thermal analysis. Higher 5% weight loss temperature and melting point indicate better thermal stability.

[0074] Synthesis Example 1 (Flame Retardant A: Production of 2,2'-biphenylenedioxy cyclic phosphazene compound) In a 1L four-neck flask equipped with a thermometer, stirrer, and condenser, 248.8g (1.80mol) of potassium carbonate, 122.9g (0.66mol) of 2,2'-biphenol, 500mL of tetrahydrofuran, and 69.5g (0.60unit mol) of hexachlorocyclotriphosphazene were charged under nitrogen flow and reacted for 24 hours under reflux. After cooling the reaction mixture to room temperature, it was washed twice with 500mL of ion-exchanged water and then with 300mL of methanol. The precipitated crystals were dried to obtain 126.4g of product. (Yield: 91.9%). The analytical results of this product were as follows.

[0075] ◎ 1 H-NMR spectrum (in deuterated chloroform, δ, ppm): 7.2~7.6(24H) ◎ 31 P-NMR spectrum (in deuterated chloroform, δ, ppm): 26.3 Trimer (P=N)3 TOF-MS: 687

[0076] From the above analysis results, it was confirmed that this product was a 2,2'-biphenylenedioxy cyclic phosphazene compound with the composition [N3P3(OC6H4C6H4O)3]. This product was used as flame retardant A.

[0077] Synthesis Example 2 (Flame Retardant B: Production of 2,2'-methylenediphenoxy cyclic phosphazene compound) In a 500mL four-neck flask equipped with a thermometer, stirrer, and condenser, 35.8g (0.26mol) of potassium carbonate, 19.0g (0.095mol) of 2,2'-dihydroxybiphenylmethane, 200mL of tetrahydrofuran, and 10.0g (0.086unit mol) of hexachlorocyclotriphosphazene were charged under nitrogen flow and reacted for 24 hours under reflux. After cooling to room temperature, the reaction mixture was washed twice with 1000mL of ion-exchanged water, and then washed with 500mL of methanol. The precipitated crystals were dried to obtain 17.9g of product. (Yield: 85.9%). The analytical results of this product were as follows.

[0078] ◎ 1 H-NMR spectrum (in deuterated chloroform, δ, ppm): 4.0(6H), 7.0~7.3(24H) ◎ 31 P-NMR spectrum (in deuterated chloroform, δ, ppm): 7.6 Trimer (P=N)3 TOF-MS: 729

[0079] From the above analysis results, it was confirmed that this product was a 2,2'-methylenediphenoxy cyclic phosphazene compound with the composition [N3P3(OC6H4CH2C6H4O)3]. This product was used as flame retardant B.

[0080] Synthesis Example 3 (Flame Retardant C: Production of 1,1'-methylenedi-2-naphthoxy cyclic phosphazene compound) In a 500mL four-neck flask equipped with a thermometer, stirrer, and condenser, 57.2g (0.41mol) of potassium carbonate, 45.6g (0.15mol) of 1,1'-methylenedi-2-naphthol, 200mL of tetrahydrofuran, and 16.0g (0.14unit mol) of hexachlorocyclotriphosphazene were charged under nitrogen flow and reacted for 24 hours under reflux. After cooling to room temperature, the reaction mixture was washed twice with 500mL of ion-exchanged water, and then washed with 300mL of methanol. The precipitated crystals were dried to obtain 42.6g of product. (Yield: 89.8%). The analytical results of this product were as follows.

[0081] ◎ 1 H-NMR spectrum (in deuterated chloroform, δ, ppm): 4.9(6H), 7.0~7.1(6H), 7.4~7.5(18H), 7.7~7.8(6H), 8.1~8.2(6H) ◎ 31 P-NMR spectrum (in deuterated chloroform, δ, ppm): 10.9 Trimer (P=N)3 TOF-MS: 1029

[0082] From the above analysis results, the composition of this product is [N3P3(OC 10 H6CH2C 10 The product was identified as a 1,1'-methylenedi-2-naphthoxy cyclic phosphazene compound of formula (H6O)3. This product was used as flame retardant C.

[0083] Synthesis Example 4 (Flame Retardant D: Production of 1,1'-bi-2-naphthoxy cyclic phosphazene compound) In a 1L four-neck flask equipped with a thermometer, stirrer, and condenser, 62.2g (0.45mol) of potassium carbonate, 47.2g (0.16mol) of 1,1'-binaphthol, 200mL of tetrahydrofuran, and 17.4g (0.15unit mol) of hexachlorocyclotriphosphazene were charged under nitrogen flow and reacted for 24 hours under reflux. After cooling to room temperature, the reaction mixture was washed twice with 500mL of ion-exchanged water, and then with 300mL of methanol. The precipitated crystals were dried to obtain 44.5g of product. (Yield: 90.0%). The analytical results of this product were as follows.

[0084] ◎ 1 H-NMR spectrum (in deuterated chloroform, δ, ppm): 7.2~8.2(36H) ◎ 31 P-NMR spectrum (in deuterated chloroform, δ, ppm): 27.4 Trimer (P=N)3 TOF-MS: 987

[0085] From the above analysis results, the composition of this product is [N3P3(OC 10 The product was confirmed to be a 1,1'-bi-2-naphthoxy cyclic phosphazene compound of the formula [H6O]3. This product was used as phosphorus-based flame retardant D.

[0086] Synthesis Example 5 (Flame Retardant E: Production of Fully Phenoxy-Substituted Cyclic Phosphazene Compound) According to the method described in PHOSPHORUS-NITROGEN COMPOUNDS, by HRALLCOCK, published in 1972, p. 151, published by ACADEMIC PRESS, a white solid hexaphenoxycyclotriphosphazene [N3P3(OC6H5)6] was produced from hexachlorocyclotriphosphazene, and this was used as flame retardant E.

[0087] (Flame retardant F: phosphate ester) A phosphoric acid ester, trade name "CR-741" manufactured by Daihachi Chemical Industry Co., Ltd., was obtained and used as flame retardant F.

[0088] (Flame retardant G: metal phosphinate) A metal phosphinic acid salt, Clariant's product name "Exolit OP935", was obtained and used as flame retardant G.

[0089] (Flame retardant H: phosphine oxide) Phosphine oxide, trade name "PQ-60" manufactured by Shinichi Chemical Co., Ltd. of Taiwan, was obtained and used as flame retardant H.

[0090] In this example, the components used in preparing the resin varnish will be described.

[0091] The following materials were used in the examples below. Component A: A modified polyphenylene ether compound that is end-modified with a substituent having a carbon-carbon unsaturated double bond. Methacrylic end-modified polyphenylene ether compound: "Product name: SA-9000" (manufactured by SABIC Innovative Plastics) Terminal vinylbenzyl modified polyphenylene ether compound: "Product name: OPE-2St2200" (manufactured by Mitsubishi Gas Chemical Company, Inc.)

[0092] Component B: A compound that has a carbon-carbon unsaturated double bond in the molecule Styrene butadiene random copolymer: "Product name: RICON181" (manufactured by CRAY VALLEY) Triallyl isocyanurate (TAIC): Reagents (Tokyo Chemical Industry Co., Ltd.)

[0093] C component: flame retardant The above synthesized or obtained flame retardants A to H

[0094] Polymerization initiator Dicumyl peroxide: "Product name: Percumil D" (manufactured by Nippon Oil & Fats Co., Ltd.)

[0095] Glass Substrate "NE Glass", #1078 type (manufactured by Nitto Boseki Co., Ltd.)

[0096] Examples 1 to 8 (Method of preparing resin varnish) (A) A modified polyphenylene ether compound, which was terminally modified by a substituent having a carbon-carbon unsaturated double bond, was mixed with toluene, and the mixture was heated to 60°C to obtain a 50% by weight toluene solution of (A). (B) A compound having a carbon-carbon unsaturated double bond in the molecule was added to the obtained toluene solution of (A) in the ratio shown in Table 3, and then the mixture was stirred for 30 minutes to completely dissolve the compound. Then, (C) A flame retardant was added and the mixture was stirred with a disperser to obtain a varnish-like resin composition (resin varnish).

[0097] (Preparation of prepregs) A glass cloth (NE Glass "#1078" manufactured by Nitto Boseki Co., Ltd.) was used as the substrate, and the resin varnish prepared above was impregnated into the glass cloth at room temperature, and then the glass cloth was heated at 130°C for about 5 minutes to dry and remove the solvent in the varnish, and the resin composition was semi-cured to prepare a prepreg. The resin content of the prepreg was adjusted to 60% by weight.

[0098] (Preparation of Molded Body) Four sheets of the obtained prepreg were stacked together and cured under vacuum in stages at 120°C for 30 minutes, 150°C for 30 minutes, and 200°C for 100 minutes, under pressure to obtain a molded product of a size suitable for evaluation.

[0099] Comparative Examples 1 to 8 The same procedures as in Examples 1 to 8 were carried out except that flame retardants E to H were used instead of flame retardants A to D, to obtain molded bodies having a size suitable for the evaluation described below.

[0100] Evaluation of molded bodies obtained in the examples and comparative examples The flame retardancy, dielectric properties, and glass transition temperature were evaluated for the molded articles obtained in Examples 1 to 8 and Comparative Examples 1 to 8. The evaluation methods were as follows.

[0101] <Flame retardancy> Molded products measuring 125 mm in length, 12.5 mm in width and 1.5 mm in thickness were classified into four flame retardancy classes, V-0, V-1, V-2 and HB, based on the total burning time when exposed to flame 10 times and whether or not cotton ignited due to dripping during burning, based on the UL-94 vertical burning test by Underwriter's Laboratories Inc. V-0 is the highest rating, followed by V-1, V-2 and HB in descending order.

[0102] <Dielectric properties (relative permittivity and dielectric tangent)> The dielectric constant and dielectric loss tangent of a molded body with a length of 80 mm, width of 3 mm and thickness of 1.0 mm were measured by the cavity resonance perturbation method. The measurements were performed using an AET Corporation cavity resonator and a Keysight Corporation network analyzer "E5063A", and the dielectric properties were measured at 25°C and a frequency of 10 GHz.

[0103] <Glass transition temperature (Tg)> The glass transition temperature (Tg) of the molded body was measured by dynamic mechanical analysis (DMA), and the maximum value of tan δ (loss modulus / storage modulus) was taken as Tg. The measurement was performed using a dynamic mechanical analysis device (PerkinElmer Japan, "DMA8000") with a tensile module at a temperature rise rate of 5°C / min.

[0104] Table 1 shows the dielectric properties (dielectric constant, dielectric tangent), 5% weight loss temperature and melting point of each flame retardant.

[0105] [Table 1]

[0106] As is clear from the results shown in Table 1, it was shown that the aryloxy cyclic phosphazene compounds of flame retardants A to D exhibit superior dielectric properties and thermal stability as compared with the flame retardants E to H.

[0107] The evaluation results of the molded bodies of each of Examples 1 to 8 and Comparative Examples 1 to 8 are shown in Tables 2 and 3.

[0108] [Table 2]

[0109] [Table 3]

[0110] As is clear from the results shown in Tables 2 and 3, the molded bodies of Examples 1 to 8 exhibited excellent dielectric properties (dielectric constant, dielectric tangent), as well as flame retardancy, thermal stability, and a high glass transition temperature.

Claims

1. (A) a modified polyphenylene ether compound whose terminals are modified with a substituent having a carbon-carbon unsaturated double bond; (B) a compound having at least one carbon-carbon unsaturated double bond in the molecule, selected from the group consisting of a styrene-butadiene copolymer, a trialkenyl isocyanurate compound, and a trialkenyl cyanurate compound; A resin component which is a mixture of (C) a flame retardant; and The present invention is characterized in that it contains The flame retardant (C) is one or more aryloxy cyclic phosphazene compounds represented by the following formula (1): Flame-retardant resin composition. 【Chemistry 1】 In formula (1), n ​​is an integer of 3 to 8, and the R group is an aryloxy group represented by the following formula (2) or (3). 【Chemistry 2】 【Chemistry 3】 In formula (2) and formula (3), R 1 and R 4 represents a single bond, an oxygen atom or a methylene group; R 2 , R 3 , R 5 and R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and p, q, r, and s each independently represent an integer of 1 to 4.

2. 2. The flame-retardant resin composition according to claim 1, wherein the substituent having a carbon-carbon unsaturated double bond in the modified polyphenylene ether compound (A) is at least one substituent selected from the group consisting of a vinylphenyl group, a vinylbenzyl group, an acryloyl group, and a methacryloyl group.

3. The flame-retardant resin composition according to claim 1 or 2, wherein the aryloxy cyclic phosphazene compound is a compound of formula (1) in which n is 3 or 4, or a mixture containing 95% by weight or more of compounds of formula (1) in which n is 3 and 4.

4. 4. The flame-retardant resin composition according to claim 1, wherein the aryloxy cyclic phosphazene compound has an acid value of 0.05 mg KOH / g or less.

5. 4. The flame-retardant resin composition according to claim 1, wherein the aryloxy cyclic phosphazene compound has a water content of 100 mg / kg or less as measured by the Karl Fischer method.

6. A resin molded product comprising the flame-retardant resin composition according to any one of claims 1 to 5.

7. An electric / electronic part comprising the resin molded article according to claim 6.

Citation Information

Patent Citations

  • Resin composition, prepreg, laminated board, metal foil-coated laminated board and printed circuit board

    CN110204862A

  • Polyphenylene ether resin composition, prepreg, metal-clad laminate, and printed wiring board

    JP2017128718A

  • Resin composition, prepreg, laminate, metal foil-clad laminate, and printed circuit board having excellent dielectric properties, high flame retardancy, good heat resistance, low water absorption, low coefficient of thermal expansion, and high adhesion to a conductor after curing

    TW201940589A

  • Resin composition, prepreg, resin sheet, metal-foil-clad laminated plate, and printed wiring board

    WO2015133292A1

  • Epoxy resin composition and molded body thereof

    WO2019198766A1