Clamping tool, method for manufacturing the same, and cleaning device
The clamping jig, composed of ceramics with high surface resistance and a DLC film, addresses substrate damage from electrostatic discharge in cleaning apparatuses by gradually dissipating charge, ensuring effective and durable cleaning of semiconductor substrates.
Patent Information
- Application Number
- JP2022571515
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-23
- Filing Date
- 2021-12-21
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-12-21
AI Technical Summary
Conventional cleaning apparatuses using hydrofluoric acid for semiconductor substrates face issues with substrate damage due to sudden electrostatic discharge, leading to decreased acid concentration and potential peripheral damage.
A clamping jig made of ceramics with silicon carbide, silicon carbonitride, or boron carbide, featuring a substrate contacting surface with high surface resistance and a DLC film, designed to gradually dissipate electrostatic charge, reducing peripheral damage.
The clamping jig effectively prevents peripheral damage from electrostatic discharge by gradually releasing charge, maintaining the integrity of the substrate contacting surface and enhancing cleaning efficiency.
Smart Images

Figure 0007557547000003 
Figure 0007557547000004 
Figure 0007557547000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a clamping jig, a method for manufacturing a clamping jig, and a cleaning device. [Background technology]
[0002] Conventionally, cleaning devices have been used to clean semiconductor substrates with cleaning liquids such as predetermined chemical solutions or pure water in order to remove contaminants such as particles, organic contaminants, and metal impurities adhering to the semiconductor substrates, as well as polymers remaining after etching processes.
[0003] As an example of a liquid processing apparatus including such a cleaning device, Patent Document 1 discloses a liquid processing apparatus equipped with a holding means for holding a substrate horizontally, the holding means having a claw portion for holding an edge surface of the substrate. As a holding means for holding a substrate horizontally, Patent Document 2 discloses a clamper for pressing down the substrate from above, and describes that the material of the clamper is silicon carbide. Furthermore, Cited Document 3 describes a clamping jig having an anti-adhesion layer (conductive layer) on the contact surface side that comes into contact with the substrate to suppress adhesion of resist material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5726686 [Patent Document 2] Japanese Patent Application Publication No. 4-130627 [Patent Document 3] JP 2014-154866 A Summary of the Invention [Means for solving the problem]
[0005] The clamping jig according to the present disclosure includes a support portion, a gripping portion located at one end of the support portion for gripping the outer periphery of a substrate, and a base portion located at the other end of the support portion for supporting the support portion. The support portion, the gripping portion, and the base portion include ceramics containing silicon carbide, silicon carbonitride, or boron carbide as a main component. The substrate contact surface of the gripping portion and at least one surface selected from the group consisting of the outer surface of the gripping portion, the outer surface of the support portion, the substrate facing surface of the support portion, and the surface of the support portion opposite to the substrate facing surface are conductive, and the substrate contact surface of the gripping portion has the highest surface resistance.
[0006] The manufacturing method of a clamping jig according to the present disclosure includes the steps of: attaching at least one powder selected from the group consisting of graphite, graphene, carbon nanotubes, fullerene, and amorphous carbon to at least one portion of a molded body formed by pressure molding granules, selected from the group consisting of a portion corresponding to the outer surface of the gripping portion, a portion corresponding to the outer surface of the support portion, a portion corresponding to the substrate-facing surface of the support portion, and a portion corresponding to the surface opposite to the portion corresponding to the substrate-facing surface of the support portion; sintering the molded body to which the powder is attached to obtain a sintered body; polishing the portion of the sintered body that corresponds to the substrate contact surface of the gripping portion; and forming a film mainly composed of DLC on the polished portion corresponding to the substrate contact surface of the gripping portion.
[0007] Furthermore, the cleaning apparatus according to the present disclosure includes a plurality of the clamping jigs. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic diagram showing a schematic configuration of a cleaning device equipped with a clamping jig according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is an enlarged view of a clamping jig according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] As described above, when a conventional cleaning device uses an acid containing hydrofluoric acid as a cleaning solution, the concentration of hydrofluoric acid decreases as the number of times the substrate is cleaned increases. As a result, a large current flows instantaneously toward the contact surface, and the periphery of the contact surface may be damaged by the impact.
[0010] An object of the present disclosure is to provide a clamping jig in which the peripheral portion of the substrate contact surface of the gripping portion is less likely to be damaged even if a sudden electrostatic discharge occurs and current flows instantaneously toward the substrate contact surface.
[0011] As described above, in the clamping jig according to the present disclosure, the substrate contact surface of the gripping part and at least one surface selected from the group consisting of the outer surface of the gripping part, the outer surface of the support part, the substrate facing surface of the support part, and the surface opposite to the substrate facing surface of the support part are conductive. Furthermore, the substrate contact surface of the gripping part has the highest surface resistance value. As a result, even if a sudden electrostatic discharge occurs and a current flows instantaneously toward the substrate contact surface, the clamping jig according to the present disclosure can gradually release the charge through the substrate contact surface of the gripping part, the outer surface of the gripping part, and the outer surface of the support part. Therefore, in the clamping jig according to the present disclosure, the peripheral portion of the substrate contact surface of the gripping part is less likely to be damaged.
[0012] Hereinafter, a clamping jig according to the present disclosure will be described in detail with reference to Figures 1 and 2. Figure 1 is a schematic diagram showing a schematic configuration of a cleaning device 30 equipped with a clamping jig 22 according to an embodiment of the present disclosure.
[0013] A cleaning apparatus 30 shown in FIG. 1 includes a housing 1 and a chamber 2 that provides a space inside the housing 1 for cleaning various substrates W such as semiconductor wafers and liquid crystal display (LCD) substrates.
[0014] The housing 1 has a first window 3 for loading and unloading the substrate W into and from the housing 1. The first window 3 is opened and closed by a first shutter 4. A transport arm 5 carries the substrate W and loads and unloads the substrate W into and from the housing 1 through the first window 3. The first window 3 is closed by the first shutter 4 except when the substrate W is being loaded or unloaded. The first shutter 4 is installed inside the housing 1 and opens and closes the first window 3 from inside the housing 1.
[0015] The chamber 2 has a second window 6 for loading and unloading the substrate W into and from the chamber 2. The second window 6 is opened and closed by a second shutter 7. The transport arm 5 enters and exits the chamber 2 through the second window 6 to deliver the substrate W to and from a rotating chuck 8 installed inside the chamber 2. The second shutter 7 is installed inside the chamber 2 and opens and closes the second window 6 from inside the chamber 2.
[0016] A gas supply unit 9 that supplies a dry gas such as nitrogen into the chamber 2 is provided on the top plate of the chamber 2. The gas supply unit 9 supplies the dry gas downward to prevent the chamber 2 from filling up due to evaporation of a cleaning liquid (e.g., an acid containing fluorine such as hydrofluoric acid or hypofluorous acid) supplied to the substrate W held by the rotating chuck 8. When the dry gas is supplied downward, watermarks, which are contaminants, are less likely to occur on the surface of the substrate W.
[0017] Within the chamber 2 are a processing cup 10 for accommodating the substrate W, a rotating chuck 8 for holding the substrate W within the processing cup 10, an underplate 11 positioned away from the back surface of the substrate W, and a top plate 16 positioned away from the front surface of the substrate W.
[0018] Processing cup 10 has an inclined portion at its top and a drain 10a at its bottom. Processing cup 10 can be raised and lowered between a position where the upper portion where the inclined portion of processing cup 10 is formed is located above substrate W held by rotating chuck 8 (the position shown by the solid line in FIG. 1; hereinafter, may be referred to as the "processing position") and a position where the upper portion is below substrate W held by rotating chuck 8 (the position shown by the two-dot chain line in FIG. 1; hereinafter, may be referred to as the "retracted position").
[0019] When the substrate W is transferred between the transport arm 5 and the rotating chuck 8, the processing cup 10 is held in a retracted position so as not to impede the entry or exit of the transport arm 5. On the other hand, when the substrate W held by the rotating chuck 8 is cleaned, the processing cup 10 is held in a processing position. The processing cup 10 held in the processing position prevents the cleaning liquid supplied to the substrate W from splashing to the surrounding area, and further guides the cleaning liquid used in cleaning the substrate W to a drain 10a.
[0020] The drain 10a is connected to a cleaning liquid recovery line and an exhaust duct (neither of which are shown in the figures). The drain 10a is adapted to discard mist and the like generated in the processing cup 10 and to recover the cleaning liquid in the chamber 2.
[0021] The rotary chuck 8 has a disk-shaped rotary plate 12 and a cylindrical body 13 connected to the rotary plate 12. A support (not shown) for supporting the substrate W and a clamping jig 22 for fixing the substrate W are attached to the outer periphery of the rotary plate 12. The support is disposed at at least three positions at equal intervals along the circumferential direction, and supports the substrate W from the back surface side.
[0022] The clamping jigs 22 are disposed at at least three positions at equal intervals along the circumferential direction and fix the substrate W from the outer circumferential surface side. A belt 14 is wound around the outer circumferential surface of the cylinder 13. By driving the belt 14 by a motor 15, the cylinder 13 and the rotating plate 12 are rotated, and the substrate W fixed by the clamping jigs 22 can be rotated.
[0023] The underplate 11 is connected to a first shaft 24 that penetrates the center of the rotating plate 12 and the inside of the cylinder 13. The first shaft 24 is fixed to a horizontal plate 25, and the horizontal plate 25 can be raised and lowered together with the first shaft 24 by a first lifting mechanism 26 such as an air cylinder. The underplate 11 and the first shaft 24 are provided with a first flow path 23 that supplies a cleaning liquid and a drying gas toward the substrate W.
[0024] A disk-shaped top plate 16 located near the top plate of the chamber 2 is connected to the lower end of a cylindrical second shaft 17. The top plate 16 is rotatable by a motor 19 provided on a horizontal plate 18. The second shaft 17 is rotatably supported on the lower surface of the second horizontal plate 18. This second horizontal plate 18 can be raised and lowered in the vertical direction by a second lifting mechanism 20 such as an air cylinder fixed to the top plate of the chamber 2. A second flow path 21 for supplying a cleaning liquid or a drying gas is provided inside each of the top plate 16 and the second shaft 17 along the axial direction.
[0025] When the substrate W is transferred between the rotating chuck 8 and the transfer arm 5, the top plate 16 is held in a position close to the ceiling of the chamber 2 so as not to collide with the transfer arm 5. When the surface (upper surface) of the substrate W is cleaned, the top plate 16 is lowered to a position close to the surface of the substrate W held by the clamping jig 22. A cleaning liquid and the like are supplied toward the substrate W through the second flow path 21.
[0026] When the front and back surfaces (top and bottom surfaces) of the substrate W are cleaned simultaneously, the back surface of the substrate W is cleaned using the underplate 11 and the first flow path 23 at the same time as the above-mentioned cleaning of the front surface of the substrate W. Examples of the method for cleaning the back surface of the substrate W include the following method. First, the underplate 11 is brought close to the back surface of the substrate W. Next, a cleaning liquid is supplied from the first flow path 23 between the substrate W and the underplate 11 to form a cleaning liquid layer. This is held for a predetermined time to perform a cleaning liquid process. Next, pure water or the like is supplied from the first flow path 23 between the substrate W and the underplate 11 to flush out the chemical solution and perform a rinsing process. Next, the substrate W is rotated at high speed while a dry gas is supplied from the first flow path 23 between the substrate W and the underplate 11.
[0027] The cleaning liquid may be, for example, an acid containing fluorine, such as hydrofluoric acid or hypofluorous acid.
[0028] The substrate W is cleaned after being held by the clamping jig 22. At this time, the processing cup 10 is raised and then the used chemicals, pure water, etc. are drained from the drain 10a.
[0029] When cleaning of the substrate W is completed, the processing cup 10 and the underplate 11 are lowered. With the top plate 16 raised, the substrate W is transferred from the clamping jig 22 to the support. Next, the first shutter 4 and the second shutter 7 are opened, and the transport arm 5 is advanced into the chamber 2. In this state, the substrate W is transferred from the rotating chuck 8 to the transport arm 5 in the reverse procedure to the procedure for transferring the substrate W from the transport arm 5 to the rotating chuck 8 described above, and the substrate W is unloaded from the cleaning apparatus 30.
[0030] Next, a clamping jig 22 according to an embodiment of the present disclosure will be described. As shown in Fig. 2, the clamping jig 22 includes a support portion 22a, a gripping portion 22b located at one end of the support portion 22a for gripping the outer periphery of the substrate W, and a base portion 22c located at the other end of the support portion 22a for supporting the support portion 22a.
[0031] The clamping jig 22 according to an embodiment of the present disclosure includes ceramics mainly composed of silicon carbide, silicon carbonitride, or boron carbide. Specifically, the support portion 22a, the gripping portion 22b, and the base portion 22c of the clamping jig 22 according to an embodiment of the present disclosure are formed of ceramics mainly composed of silicon carbide, silicon carbonitride, or boron carbide. In this specification, the main component means a component that occupies 80 mass% or more of the total 100 mass% of the components constituting the ceramic. The ceramics mainly composed of silicon carbonitride refers to a composite ceramics containing silicon carbide, silicon nitride, and silicon carbonitride, and the total content of these components is 80 mass% or more. Whether the main component is silicon carbide, silicon carbonitride, or boron carbide, components other than the main component may include, for example, boron, free carbon, etc.
[0032] The components constituting the ceramics can be identified by an X-ray diffractometer using CuKα radiation. The content of each component can be determined, for example, by an ICP (Inductively Coupled Plasma) emission spectrometer or a fluorescent X-ray analyzer.
[0033] The support 22a is a member for connecting the gripping portion 22b and the base 22c, which will be described later. The gripping portion 22b is a member for gripping the outer periphery of the substrate W with the substrate contact surface 22b1. The gripping portion 22b is located at one end of the support 22a. Although not specifically shown in FIG. 2, the gripping portion 22b is processed into a shape that makes it easy to grip the outer periphery of the substrate W. Specifically, a slit, a groove, or the like is formed in the gripping portion 22b. The substrate contact surface 22b1 shown in FIG. 2 is flat, but the shape of the substrate contact surface 22b1 may be a curved surface or a bent surface. The gripping portion 22b is composed of the substrate contact surface 22b1 and a portion located on the outer periphery side of the substrate contact surface 22b1.
[0034] The base 22c is located at the other end of the support 22a, that is, on the opposite side to the position of the gripping part 22b. The clamping jig 22 has an insertion hole for inserting a metallic pin 221, for example, and the pin 221 is inserted into the insertion hole. If the pin 221 is made of metal, even if a sudden static electricity discharge occurs as described below, the electric charge can be gradually released through the pin 221. As a result, the peripheral part of the substrate contact surface 22b1 of the gripping part 22b is less likely to be damaged.
[0035] In the clamping jig 22 according to one embodiment, at least one surface selected from the group consisting of the substrate contact surface 22b1 of the gripping portion 22b, the outer side surface 22b2 of the gripping portion 22b, the outer side surface 22a2 of the support portion 22a, the substrate facing surface 22a1 of the support portion 22a, and the surface 22a3 of the support portion 22a opposite to the substrate facing surface 22a1, is conductive. In this specification, "conductive" means that the surface resistance at 20±2°C is 10 4 This means that the resistance is less than or equal to Ω.
[0036] Among these surfaces, in the clamping jig 22 according to one embodiment, the substrate contact surface 22b1 of the gripping portion 22b has the highest surface resistance. If the substrate contact surface 22b1 of the gripping portion 22b has the highest surface resistance, even if a sudden electrostatic discharge occurs and a current flows instantaneously toward the substrate contact surface 22b1 of the gripping portion 22b, the electric charge can be gradually released from the substrate contact surface 22b1 of the gripping portion 22b through at least one surface selected from the group consisting of the outer surface 22b2 of the gripping portion 22b, the outer surface 22a2 of the support portion 22a, the substrate facing surface 22a1 of the support portion 22a, and the surface 22a3 opposite to the substrate facing surface 22a1 of the support portion 22a. As a result, the peripheral portion of the substrate contact surface 22b1 of the gripping portion 22b is less likely to be damaged.
[0037] In particular, the difference between the surface resistance of the substrate contact surface 22b1 of the gripping portion 22b and the surface resistance of at least one surface selected from the group consisting of the outer surface 22b2 of the gripping portion 22b, the outer surface 22a2 of the support portion 22a, the substrate-facing surface 22a1 of the support portion 22a, and the surface 22a3 of the support portion 22a opposite to the substrate-facing surface 22a1 is preferably 50 Ω or more.Furthermore, the difference is preferably 90 Ω or more.
[0038] For example, it is preferable that the surface resistance of the substrate contact surface 22b1 of the gripping portion 22b is about 100Ω or more and 1000Ω or less, and the surface resistance of at least one surface selected from the group consisting of the outer surface 22b2 of the gripping portion 22b, the outer surface 22a2 of the support portion 22a, the substrate facing surface 22a1 of the support portion 22a, and the surface 22a3 opposite to the substrate facing surface 22a1 of the support portion 22a is about -10Ω or more and 10Ω or less. If the surface resistance of each surface is in such a range, the peripheral portion of the substrate contact surface 22b1 of the gripping portion 22b is more unlikely to be damaged. Here, the surface resistance values are measured at 20±2°C for all surfaces.
[0039] The maximum surface resistance (RS max ) for the minimum value (RS min ) percentage (RS min / RS max ) should be between 0.82 and 0.99. min / RS max If the surface resistance value of each surface is within this range, the difference between the surfaces is small, and the charge can be gradually and substantially uniformly released with little difference between the surfaces. The surface resistance value can be measured, for example, using a surface resistance meter (for example, Hioki E.E. Corporation, HiTester 3127-10).
[0040] In order to set the surface resistance of each surface within the above range, for example, the substrate contact surface 22b1 of the gripping portion 22b is preferably coated with a film mainly composed of diamond-like carbon (DLC). Diamond-like carbon (DLC) is an amorphous carbon having sp2 bonds, which are the structure of graphite, and sp3 bonds, which are the structure of diamond.
[0041] In this specification, the term "film mainly composed of diamond-like carbon (DLC)" refers to a film having a wave number of 1500 to 1640 cm in Raman spectroscopy. -1 The G band is observed in the range of 1300 to 1400 cm -1 The film has a D band observed in the range of 1500 to 1640 cm -1 The strongest peak intensity among the peaks present in H G , wave number 1300~1400cm -1 The highest peak intensity among the peaks present in the range is H D Then, H G >H D If this relationship is satisfied, the denseness of the film can be maintained.
[0042] The film may contain, other than diamond-like carbon (DLC), for example, Fe at 0.05 mass ppm or less and Ni at 0.01 mass ppm or less. The thickness of the film mainly composed of DLC is, for example, 0.1 μm or more and 1 μm or less, and in particular, 0.4 μm or more and 0.8 μm or less.
[0043] The surface of the film may be at least on the substrate contact surface 22b1 side of the outer surface 22b2 of the gripping portion 22b, and may decrease with increasing distance from the substrate contact surface 22b1. The surface of the film may be at least on the outer surface 22b2 side of the gripping portion 22b of the outer surface 22a2 of the support portion 22a, and may decrease with increasing distance from the outer surface 22b2 of the gripping portion 22b.
[0044] At least one surface selected from the group consisting of outer surface 22b2 of gripping portion 22b, outer surface 22a2 of support portion 22a, substrate-facing surface 22a1 of support portion 22a, and surface 22a3 opposite substrate-facing surface 22a1 of support portion 22a preferably contains at least one material selected from the group consisting of graphite, graphene, carbon nanotubes, fullerene, and amorphous carbon.
[0045] On the substrate contact surface 22b1 of the gripping portion 22b, the average value of the cut level difference (Rδc), which represents the difference between the cut level at a load length ratio of 25% on the roughness curve of the substrate contact surface 22b1 of the gripping portion 22b and the cut level at a load length ratio of 75% on the roughness curve, is preferably, for example, 0.01 μm or more and 0.06 μm or less.
[0046] If the average value of the cutting level difference (Rδc) is 0.01 μm or more, the contact angle of pure water and ultrapure water with respect to the substrate contact surface 22b1 of the gripping part 22b becomes small, and the substrate contact surface 22b1 of the gripping part 22b exhibits hydrophilicity. Therefore, when the gripping part 22b is washed with pure water after washing with acid, adhesion of air bubbles is further reduced. As a result, adhesion of minute dirt contained in the air bubbles can be further suppressed. Here, the acid is an acid containing fluorine such as hydrofluoric acid and hypofluorous acid. The contact angle of pure water or ultrapure water with respect to the substrate contact surface 22b1 can be obtained by the sessile drop method described in JIS R 3257:1999. The contact angle may be measured, for example, using a contact angle meter (CA-X150 type manufactured by Kyowa Interface Science Co., Ltd.). On the other hand, if the average value of the cutting level difference (Rδc) is 0.06 μm or less, the anchor effect of fluorine with respect to the substrate contact surface 22b1 of the gripping part 22b becomes smaller. As a result, adhesion of fluorine to the substrate contact surface 22b1 of the gripping portion 22b is suppressed.
[0047] The cut level difference (Rδc) can be measured using a laser microscope (Keyence Corporation, ultra-deep color 3D shape measuring microscope (VK-X1000 or its successor model)) in accordance with JIS B 0601:2001. The measurement conditions are as follows: illumination method is coaxial epi-illumination, measurement magnification is 480x, cutoff value λs is none, cutoff value λc is 0.08mm, cutoff value λf is none, end effect is corrected, and the measurement range per location is 710μm×533μm. The measurement ranges are set from a total of two locations on the substrate contact surface 22b1 of the gripper 22b.
[0048] For each measurement range, four lines to be measured are drawn at approximately equal intervals along the longitudinal direction, and line roughness measurements are performed. The length of each line to be measured is 560 μm. The average value of the cut level difference (Rδc) can be calculated using the cut level differences (Rδc) obtained from a total of eight lines to be measured.
[0049] In the substrate contact surface 22b1 of the gripping part 22b, the average value of the root mean square slope (RΔq) in the roughness curve is preferably, for example, 0.12 or less. If the average value of the root mean square slope (RΔq) is 0.12 or less, the unevenness of the substrate contact surface 22b1 of the gripping part 22b becomes smaller. Therefore, even if the substrate W comes into contact with the substrate W, the substrate W is less likely to be scratched. The measurement conditions for the root mean square slope (RΔq) are the same as the measurement conditions for the cut level difference (RΔc).
[0050] Next, an embodiment of a method for manufacturing a clamping jig according to the present disclosure will be described. The method for manufacturing a clamping jig according to an embodiment includes the following steps (a) to (d). (a) A step of adhering at least one type of powder selected from the group consisting of graphite, graphene, carbon nanotubes, fullerene, and amorphous carbon to at least one portion selected from the group consisting of a portion corresponding to the outer side of the gripping portion, a portion corresponding to the outer side of the support portion, a portion corresponding to the substrate-facing surface of the support portion, and a portion corresponding to the surface opposite to the portion corresponding to the substrate-facing surface of the support portion in a molded body mainly composed of silicon carbide. (b) A step of sintering the green body with the powder attached thereto to obtain a sintered body. (c) A step of polishing a portion of the sintered body that corresponds to the substrate contact surface of the gripping portion. (d) A process of forming a film mainly composed of DLC (hereinafter, the film mainly composed of DLC may be referred to as a "DLC film") on the portion of the polished gripping portion that corresponds to the substrate contact surface.
[0051] First, one embodiment of a method for manufacturing a clamping jig including ceramics containing silicon carbide as a main component will be described. In step (a), granules mainly composed of silicon carbide are prepared, for example, by the following procedure. Coarse powder and fine powder are prepared as silicon carbide powder, and ion-exchanged water and, if necessary, a dispersant are mixed and ground for 40 to 60 hours by a ball mill or a bead mill to form a slurry. The mass ratio of the fine powder to the coarse powder may be, for example, 85% by mass or more and 94% by mass or less of the fine powder, and 6% by mass or more and 15% by mass or less of the coarse powder. The particle sizes of the fine powder and the coarse powder after the grinding and mixing are 0.4 μm to 4 μm and 11 μm to 34 μm, respectively. The coarse powder and the fine powder may be either α type or β type.
[0052] Next, a sintering aid consisting of boron carbide powder and amorphous carbon powder or phenol resin, and a binder are added to the obtained slurry, mixed, and then spray-dried to obtain granules containing silicon carbide as the main component. Examples of the binder include acrylic emulsion, polyvinyl alcohol, polyethylene glycol, and polyethylene oxide.
[0053] RS min / RS max To adjust the amount of nitrogen, a nitrogen source may be added to the slurry, and a resol type phenolic resin containing nitrogen may be used as the phenolic resin. min / RS maxIn order to obtain a clamping jig having a refractive index of 0.82 or more and 0.99 or less, for example, the nitrogen content per 100 parts by mass of silicon carbide powder may be set to 0.0001 parts by mass or more and 0.0015 parts by mass or less.
[0054] The resulting granules are then filled into a mold and pressed at a pressure of, for example, 49 MPa to 147 MPa to obtain a molded body. Next, in the resulting molded body, at least one powder selected from the group consisting of graphite, graphene, carbon nanotubes, fullerene, and amorphous carbon is attached to at least one portion selected from the group consisting of a portion corresponding to the outer surface of the gripping portion, a portion corresponding to the outer surface of the support portion, and a portion corresponding to the substrate-facing surface of the support portion.
[0055] Specifically, the IPA solution containing these powders is sprayed using a spray coating device. When graphite powder is selected, the average particle size may be, for example, 10 μm or more and 100 μm or less. The content of the graphite powder relative to 100 parts by mass of the IPA solution may be, for example, 1 part by mass or more and 5 parts by mass or less.
[0056] The green body with the powder attached thereto is subjected to step (b). Specifically, the green body with the powder attached is degreased by holding it in a nitrogen atmosphere at a temperature of 450°C to 650°C for 2 hours to 10 hours to obtain a degreased body. Next, this degreased body is held in a reduced pressure atmosphere of an inert gas such as argon at a temperature of 1800°C to 2200°C for 3 hours to 6 hours to obtain a sintered body.
[0057] An embodiment of a method for manufacturing a clamping jig containing ceramics whose main component is silicon carbonitride will be described.
[0058] Silicon carbide powder having an average particle size of 0.5 μm to 10 μm, ion-exchanged water, and optionally a dispersant are pulverized and mixed by a ball mill or a bead mill for 40 hours to 60 hours to obtain a slurry. The silicon carbide powder may be either α-type or β-type. The content of inevitable impurities in 100% by mass of the silicon carbide powder is preferably 200 ppm by mass or less, particularly 150 ppm by mass or less.
[0059] Next, the mixture is mixed, spray-dried, molded, sprayed with powder such as graphite, and degreased in the same manner as described above, and then the nitriding treatment is performed. The nitriding treatment is performed at a temperature of 1500°C to 1950°C under a nitrogen partial pressure of 1 MPa to 100 MPa. This nitriding treatment causes some of the silicon carbide in the molded body to react with nitrogen to generate silicon nitride and free carbon, and the silicon carbide becomes a nitride that is firmly bonded by the silicon nitride. Some of the silicon carbide dissolves nitrogen and becomes silicon carbonitride. As silicon nitride is generated, densification progresses. However, when silicon nitride and free carbon are generated, a concentration difference may occur between the surface and the inside of the ceramic. To reduce this concentration difference, the nitrogen partial pressure in the nitriding treatment should be 1 MPa to 50 MPa and the temperature should be 1550°C to 1950°C.
[0060] In particular, by making silicon nitride 28% by mass or more and free carbon 7% by mass or more out of a total of 100% by mass of the components constituting the ceramic, the relative density of the ceramic can be made 80% or more. To obtain ceramics with 28% by mass or more of silicon nitride and 7% by mass or more of free carbon, for example, the nitriding time may be set to 3 hours or more and 5 hours or less.
[0061] By subjecting the degreased body to a calcination treatment at 1600°C to 2100°C, particularly at 1700°C to 2000°C and below at 1333 Pa or less, the content of unavoidable impurities in the degreased body can be further reduced, and the longer the calcination treatment time, the higher the purity. In practice, the calcination treatment time should be 0.5 hours to 12 hours. When the content of unavoidable impurities in 100 mass% of silicon carbide powder is 200 mass ppm or less, the content of unavoidable impurities in the ceramic can be reduced to 50 mass ppm or less by performing the calcination treatment.
[0062] An embodiment of a method for manufacturing a clamping jig including ceramics based on boron carbide will be described.
[0063] First, if the composition formula is, for example, B x A boron carbide powder represented by C (x=3.5 to 10) is prepared. The average particle size of the boron carbide powder is 0.5 μm or more and 2 μm or less. Graphite powder and silicon carbide powder are added to this boron carbide powder. The amount of graphite powder added relative to 100 parts by mass of the boron carbide powder is, for example, 1 part by mass or more and 20 parts by mass or less, and the amount of silicon carbide powder added is, for example, 0.1 parts by mass or more and 10 parts by mass or less. The graphite powder is, for example, highly oriented pyrolytic graphite (HOPG) powder.
[0064] Furthermore, as a sintering aid, at least one of borides of elements selected from Groups 4, 5, and 6 of the periodic table and oxides of elements selected from Group 3 of the periodic table may be added to promote sintering. Examples of the borides to be added include zirconium boride (ZrB2), titanium boride (TiB2), and chromium boride (CrB2). Examples of the oxide to be added include yttrium oxide (Y2O3).
[0065] Next, the mixture is mixed, spray-dried, molded, sprayed with powder such as graphite, and degreased in the same manner as described above. The degreased body is then fired in a reduced pressure atmosphere of an inert gas such as argon or in a vacuum atmosphere. The firing process includes a melting step in which the temperature is held in a first reference temperature range of 2100°C to 2300°C for 10 minutes to 10 hours to melt the graphite, and a precipitating step in which the temperature is raised to a second reference temperature of 2200°C to 2350°C at a heating rate of 1000°C / hour to 1200°C / hour, the temperature is held in the second reference temperature range for 10 minutes to 20 hours, and then the temperature is lowered to precipitate the melted graphite.
[0066] In order to further promote densification, pressure may be applied with high-pressure gas when the open porosity becomes 5% or less as the sintering progresses. For example, high-pressure GPS (Gas Pressure Sintering) method or hot isostatic pressing (HIP) method may be used, and the gas pressure may be set to 1 MPa or more and 300 MPa or less. By setting the gas pressure within this range, the relative density of the ceramics will be 95% or more. If necessary, sintering may be performed while applying mechanical pressure, such as with the hot press method or SPS (Spark Plasma Sintering) method.
[0067] The obtained sintered body is then subjected to step (c). Specifically, the portion of the obtained sintered body that corresponds to the substrate contact surface of the gripping portion (hereinafter, this portion may be referred to as the portion corresponding to the substrate contact surface) is polished. The polishing process may be, for example, buff polishing. The base material of the buff is not limited, and may be, for example, felt, cotton strip, cotton strip, etc. Examples of the abrasive include diamond powder and green carborundum (GC) powder. These abrasives may be added to oils and fats and used in a paste state.
[0068] The average particle size of the abrasive is, for example, 0.5 μm or more and 6 μm or less. The outer diameter of the base material is 150 mm, and the rotation speed is, for example, 28 m / min or more and 170 m / min or less. The polishing time is, for example, 0.5 minutes or more and 5 minutes or less. In order to obtain a clamping jig having an average value of 0.01 μm or more and 0.06 μm or less of cut level difference (Rδc) representing the difference between the cut level at a load length ratio of 25% in the roughness curve of the substrate contact surface of the gripping part and the cut level at a load length ratio of 75% in the roughness curve, the average particle size of the abrasive may be set to 0.5 μm or more and 6 μm or less.
[0069] In order to obtain a clamping jig having an average value of the root mean square slope (RΔq) of the roughness curve of the substrate contact surface of the gripping part of 0.12 or less, the polishing time should be 3 minutes or more.
[0070] Next, the polished sintered body is subjected to step (d). Specifically, a DLC film is formed on the portion of the polished sintered body that corresponds to the substrate contact surface. The DLC film is formed, for example, by the following procedure.
[0071] First, the sintered body is placed at a predetermined position in a plasma processing vessel, and after exhausting the air, the sintered body is heated to 100°C or higher and 450°C or lower in a non-oxidizing gas atmosphere such as argon gas or nitrogen gas or in a high vacuum. Next, high-frequency power and a negative bias voltage are supplied to the sintered body in a non-oxidizing gas atmosphere or an inert gas atmosphere to generate a discharge plasma, and ions are irradiated onto the portion corresponding to the substrate contact surface of the gripping part. This ion irradiation can remove the oxide film and deposits on the portion corresponding to the substrate contact surface. A raw material gas for forming a DLC film is supplied into the plasma processing vessel to generate a discharge plasma, and a DLC film is formed on the portion corresponding to the substrate contact surface. The raw material gas for forming a DLC film is, for example, a hydrocarbon gas such as methane, acetylene, or toluene, and hydrogen may be added as necessary.
[0072] In the clamping jig of the present disclosure obtained by the above-mentioned manufacturing method, the substrate contact surface of the gripping part and at least one surface selected from the group consisting of the outer surface of the gripping part, the outer surface of the support part, the substrate facing surface of the support part, and the surface opposite to the substrate facing surface of the support part are conductive. Furthermore, the substrate contact surface of the gripping part has the highest surface resistance value. As a result, even if a sudden electrostatic discharge occurs and a current flows instantaneously toward the substrate contact surface, the clamping jig of the present disclosure can gradually release the electric charge through the substrate contact surface of the gripping part, the outer surface of the gripping part, and the outer surface of the support part. Therefore, the clamping jig of the present disclosure is less likely to be damaged in the periphery of the substrate contact surface of the gripping part. EXAMPLES
[0073] Example 1 Coarse powder and fine powder were prepared as silicon carbide powder, and the silicon carbide powder and ion-exchanged water were milled and mixed in a ball mill for 50 hours to form a slurry. The mass ratio of the fine powder to the coarse powder was 89.5 mass% for the fine powder and 10.5 mass% for the coarse powder. After milling and mixing, the particle size range of the fine powder was 0.4 μm to 4 μm, and the particle size range of the coarse powder was 11 μm to 34 μm.
[0074] Next, the obtained slurry was mixed with a sintering aid consisting of boron carbide powder and amorphous carbon powder or phenol resin, and a binder. The mixture was then spray-dried to obtain granules containing silicon carbide as the main component. The binder used was an acrylic emulsion, polyvinyl alcohol, polyethylene glycol, or polyethylene oxide.
[0075] The granules obtained were then filled into a mold and pressed at a pressure of 98 MPa to obtain a molded body. In the molded body, an IPA solution containing graphite powder was sprayed onto the portions of the molded body corresponding to the outer surface of the gripping portion, the outer surface of the support portion, and the substrate-facing surface of the support portion using a spray coating device. The average particle size of the graphite powder was 50 μm. The content of the graphite powder per 100 parts by mass of the IPA solution was 3 parts by mass.
[0076] The graphite powder compact was degreased by holding it in a nitrogen atmosphere at 550°C for 6 hours to obtain a degreased body, which was then held in a reduced pressure argon gas atmosphere at 2000°C for 5 hours to obtain a sintered body.
[0077] The sintered body was subjected to buff polishing on the surface corresponding to the substrate contact surface. Felt was used as the base material for the buff. Diamond powder with the average particle size shown in Table 1 was used as the abrasive, and this diamond powder was added to oils and fats and used in a paste state. The outer diameter of the base material was 150 mm, and the rotation speed was 100 m / min. The polishing time was 2 minutes.
[0078] First, the sintered body, the portion of the gripper that corresponds to the substrate contact surface, was buffed and placed at a predetermined position in a plasma processing vessel. After evacuation, the sintered body was heated to 300°C in an argon gas atmosphere. Next, high-frequency power and a negative bias voltage were supplied to the sintered body in the argon gas to generate discharge plasma, and the portion that corresponds to the substrate contact surface was irradiated with ions. Acetylene was supplied into the plasma processing vessel to generate discharge plasma, and a DLC film was formed on the portion that corresponds to the substrate contact surface, to obtain samples No. 1 to 6, which are clamping jigs. Sample No. 7 was a clamping jig in which the portion that corresponds to the substrate contact surface of the sintered body was buffed but no DLC film was formed on the portion that corresponds to the substrate contact surface.
[0079] The surface resistance of each sample was measured for the substrate contact surface of the gripping part, the outer surface of the gripping part, the outer surface of the support part, the substrate facing surface of the support part, the substrate facing surface of the support part, and the surface opposite the substrate facing surface. The surface resistance was measured using a surface resistance meter (Hioki E.E. Corporation, HiTester 3127-10) and the temperature of the measurement environment was set to 20±2°C.
[0080] The cut level difference (Rδc) of the substrate contact surface of each sample was measured using a laser microscope (Keyence Corporation, ultra-deep color 3D shape measuring microscope (VK-X1000 or its successor model)) in accordance with JIS B 0601:2001. The measurement conditions were as follows: illumination method: coaxial incident light, measurement magnification: 480x, cutoff value λs: none, cutoff value λc: 0.08mm, cutoff value λf: none, end effect correction: yes, measurement range per location: 710μm×533μm, and the measurement range was set from a total of two locations on the substrate contact surface of the gripping part.
[0081] For each measurement range, four lines were drawn at approximately equal intervals along the longitudinal direction to measure the line roughness. The length of each line was 560 μm. The average cut level difference (Rδc) was calculated using the cut level difference (Rδc) obtained from a total of eight lines to be measured.
[0082] The contact angle of pure water with respect to the substrate contact surface was measured by the sessile drop method described in JIS R 3257:1999 using a contact angle meter (Model CA-X150 manufactured by Kyowa Interface Science Co., Ltd.). Each sample was immersed in hydrofluoric acid for 48 hours, then removed, washed with water, and ultrasonically cleaned with pure water. The presence or absence of fluorine on the substrate contact surface of each sample after ultrasonic cleaning was detected by elemental analysis using an energy dispersive X-ray analyzer (EDS). The measurement results of each sample obtained by the above-mentioned method are shown in Table 1.
[0083] [Table 1]
[0084] As shown in Table 1, in samples Nos. 1 to 6, the substrate contact surface of the gripper, the outer side surface of the gripper, the outer side surface of the support, the substrate-facing surface of the support, and the surface opposite the substrate-facing surface of the support are conductive, and the substrate contact surface of the gripper has the highest surface resistance. As a result, in samples Nos. 1 to 6, even if a sudden static electricity discharge occurs and a current flows instantaneously toward the substrate contact surface, the charge can be gradually released from the substrate contact surface of the gripper through the outer side surface of the gripper, the outer side surface of the support, the substrate-facing surface of the support, and the surface opposite the substrate-facing surface of the support.
[0085] In particular, samples No. 2 to No. 5 have an average cutting level difference (Rδc) of 0.01 μm or more and 0.06 μm or less, a small contact angle with pure water, and are hydrophilic. Therefore, when the sample is washed with pure water after washing with acid, adhesion of air bubbles is further reduced, and adhesion of minute dirt contained in the air bubbles can be further suppressed. Furthermore, no fluorine was observed in samples No. 2 to No. 5, which is good.
[0086] Example 2 The substrate contact surface of the gripping part of the sintered body prepared by the same method as that shown in Sample No. 4 of Example 1 was subjected to buffing. The buffing method was the same as that shown in Example 1, except for the buffing time. The buffing time for each sample is shown in Table 2.
[0087] In the same manner as in Example 1, a DLC film was formed on the portion of the gripping part corresponding to the surface that contacts the substrate, to obtain Samples Nos. 8 to 11, which are clamping jigs.
[0088] The root mean square slope (RΔq) of the substrate contact surface of each sample was measured, and the average value was calculated. The average values are shown in Table 2. The measurement conditions for the root mean square slope (RΔq) were the same as those for the measurement conditions for the cut level difference (Rδc) shown in Example 1. Using each sample, a disk-shaped substrate was supported at three points along the circumferential direction, and the substrates were replaced while observing the presence or absence of scratches on the outer edge of the substrate every time 100 substrates were supported. Observation was performed using an optical microscope at a magnification of 100 times. The presence or absence of scratches after supporting 2000 substrates is shown in Table 2.
[0089] [Table 2]
[0090] As shown in Table 2, it is understood that samples Nos. 9 to 11, which have an average value of the root mean square slope (RΔq) of 0.12 or less, are unlikely to scratch the substrate W even when they come into contact with the substrate. [Explanation of symbols]
[0091] 1. Housing 2 Chamber 3 First window 4 First Shutter 5. Transport arm 6 Second window 7 Second Shutter 8 Rotating Chuck 9 Gas Supply Section 10 Processing Cup 11 Underplate 12 Rotating plate 13 Cylinder 14 Belt 15 Motor 16 Top Plate 17 Second Axis Body 18 Second horizontal plate 19 Motor 20 Second lifting mechanism 21 Second flow path 22 Clamping fixture 22a Strut part 22a1 Board facing surface 22a2 outer surface 22a3 Surface opposite to the substrate 22b Grip part 22b1 Board contact surface 22b2 External surface 22c base 221 Pin 23 First Channel 24 First Axis Body 25 Horizontal board 26 First lifting mechanism 30 Cleaning Equipment
Claims
1. A support portion and a gripping portion located at one end of the support portion for gripping an outer periphery of the substrate; a base portion located at the other end of the support portion and configured to support the support portion; Including, the support portion, the grip portion, and the base portion each include a ceramic containing silicon carbide, silicon carbonitride, or boron carbide as a main component; the substrate contact surface of the gripping portion and at least one surface selected from the group consisting of an outer surface of the gripping portion, an outer surface of the support portion, a substrate facing surface of the support portion, and a surface of the support portion opposite to the substrate facing surface are conductive, and the substrate contact surface of the gripping portion has the highest surface resistance value; Clamping fixture.
2. 2. The clamping jig according to claim 1, wherein the gripping portion comprises a film mainly composed of DLC, and at least a part of a surface of the film facing the substrate is a substrate contact surface.
3. 3. The clamping jig according to claim 1 or 2, wherein at least one surface selected from the group consisting of an outer surface of the gripping portion, an outer surface of the support portion, a substrate-facing surface of the support portion, and a surface of the support portion opposite to the substrate-facing surface, comprises at least one material selected from the group consisting of graphite, graphene, carbon nanotubes, fullerenes, and amorphous carbon.
4. The average value of the cut level difference (Rδc) representing the difference between the cut level at a load length rate of 25% in the roughness curve of the substrate contact surface of the gripping portion and the cut level at a load length rate of 75% in the roughness curve is 0.01 μm or more and 0.06 μm or less. The clamping jig according to any one of claims 1 to 3.
5. 5. The clamping jig according to claim 1, wherein an average value of the root mean square slope (RΔq) of a roughness curve of the substrate contact surface of said gripping portion is 0.12 or less.
6. A method for manufacturing the clamping jig according to any one of claims 1 to 5, comprising the steps of: a step of adhering at least one powder selected from the group consisting of graphite, graphene, carbon nanotubes, fullerene, and amorphous carbon to at least one portion selected from the group consisting of a portion corresponding to the outer surface of the gripping portion, a portion corresponding to the outer surface of the support portion, a portion corresponding to the substrate-facing surface of the support portion, and a portion corresponding to the surface opposite to the portion corresponding to the substrate-facing surface of the support portion in a compact obtained by pressure-molding the granules; sintering the green body to which the powder is attached to obtain a sintered body; polishing a portion of the sintered body corresponding to a substrate contact surface of the gripping portion; forming a film mainly composed of DLC on a portion of the polished gripping portion corresponding to a substrate contact surface; A method for manufacturing a clamping jig, comprising:
7. A cleaning device comprising a plurality of clamping jigs according to any one of claims 1 to 5.
Citation Information
Patent Citations
Preparation of indole derivative
JP1982026686A
Plasma etching device
JP1992130627A
Substrate holding mechanism, substrate processing apparatus using the same and substrate processing method
JP2003092343A
Liquid treatment device and liquid treatment method
JP2003229399A
Substrate holding mechanism, and substrate treatment apparatus and substrate treatment method using the same
JP2005285798A