Integrated dry process for irradiation photoresist patterning

The integrated dry process for EUV photoresist patterning addresses the challenges of EUV lithography by using a cluster of reaction chambers with metal-containing EUV resists, enhancing etch resistance and reducing line edge roughness through dry development, thereby improving throughput and precision.

JP7557569B2Active Publication Date: 2024-09-27LAM RES CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023063868
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-07
Filing Date
2023-04-11
Publication Date
2024-09-27
Estimated Expiration
2041-07-02

AI Technical Summary

Technical Problem

Current photolithography processes face challenges in creating small features with conventional organic chemically amplified resists (CARs) due to low power output, low absorption coefficients, and pattern collapse issues in extreme ultraviolet (EUV) lithography, particularly with high aspect ratios and line edge roughness.

Method used

An integrated dry process for EUV photoresist patterning using a cluster of reaction chambers, including deposition, post-application bake, post-exposure bake, development, and cleaning, utilizing metal-containing EUV resists with dry development techniques to enhance etch resistance and absorption.

Benefits of technology

The dry process improves etch resistance, reduces line edge roughness, and increases throughput by avoiding wet development limitations, enabling precise control over film thickness and reducing line collapse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557569000007
    Figure 0007557569000007
  • Figure 0007557569000002
    Figure 0007557569000002
  • Figure 0007557569000013
    Figure 0007557569000013
Patent Text Reader

Abstract

To provide a method and a system for an integrated process for forming patterned photoresist.SOLUTION: A Method for forming a thin film on a patternable semiconductor substrates using EUV includes: depositing an organometallic polymer-like material onto a surface of a semiconductor substrate; exposing the surface to the EUV to form a pattern; and developing the pattern for subsequent transfer to underlying layers. The deposition processes include a chemical vapor deposition (CVD) method, an atomic layer deposition (ALD), and an ALD with CVD component, for example, a discontinuous ALD-like process in which a metal precursor and a counter-reactant are separated in either time or space can be used.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] <Incorporated by Reference> The PCT application form is filed concurrently herewith as part of this application. Each application to which this application claims benefit or priority identified in the concurrently filed PCT application form is incorporated herein by reference in its entirety for all purposes. [Background technology]

[0002] The background art description provided herein is intended to provide a general description of the background to the present technology. Work by the currently named inventors, as well as aspects of the description that may not otherwise be considered prior art at the time of filing, are not admitted, expressly or impliedly, as prior art against the present technology to the extent described in this background art section.

[0003] The fabrication of semiconductor devices, such as integrated circuits, is a multi-step process that involves photolithography. Generally, this process involves depositing material on a wafer and patterning the material by lithographic techniques to form the structural features (e.g., transistors and circuits) of the semiconductor device. Typical photolithography process steps known in the art include providing a substrate, applying a photoresist, such as by spin coating, exposing the photoresist to light in a desired pattern to render the exposed areas of the photoresist somewhat soluble in a developer, applying and developing a developer to remove either the exposed or unexposed areas of the photoresist, and then forming features in the areas of the substrate where the photoresist was removed, such as by etching or material deposition.

[0004] Advances in semiconductor design have driven the need for, and the ability to, create ever-smaller features on semiconductor substrate materials. This technological advancement has been characterized by "Moore's Law," which states that transistor density in high-density integrated circuits doubles every two years. Indeed, advances in chip design and manufacturing have enabled modern microprocessors to contain billions of transistors and other circuit features on a single chip. Individual features on such chips can be approximately 22 nanometers (nm) or smaller, and in some cases, less than 10 nm.

[0005] One of the challenges in fabricating devices with such small features is the ability to reliably and reproducibly create photolithography masks with sufficient resolution. Current photolithography processes typically use 193 nm ultraviolet (UV) light to expose photoresists. This light has a wavelength significantly larger than the size of the desired features to be created on the semiconductor substrate, which presents unique challenges. Achieving feature sizes smaller than the wavelength of light requires complex resolution enhancement techniques, such as multi-patterning. Therefore, there has been considerable interest and research into developing photolithography techniques using shorter wavelength light, such as extreme ultraviolet radiation (EUV), which has a wavelength of 10 to 15 nm, e.g., 13.5 nm. However, EUV photolithography processes can suffer from challenges such as low power output and light loss during patterning. Conventional organic chemically amplified resists (CARs), similar to those used in 193 nm UV lithography, have potential drawbacks for use in EUV lithography, particularly their low absorption coefficient in the EUV region, which can lead to blurring or line-edge roughness due to diffusion of photoactivated species. Furthermore, achieving the etch resistance required to pattern underlying device layers can result in small features patterned with conventional CAR materials having high aspect ratios, posing a risk of pattern collapse. Therefore, there remains a need for improved EUV photoresist materials with properties such as higher absorbance and etch resistance, which can be reduced in thickness. Summary of the Invention

[0006] Disclosed herein are methods and systems for an integrated process for forming patterned photoresist. One aspect of the disclosed embodiments provides an integrated lithography system. The integrated lithography system includes a plurality of reaction chambers in a cluster, the plurality of reaction chambers including a photoresist (PR) deposition chamber, a post-apply bake (PAB) chamber, a post-exposure bake (PEB) chamber, a development chamber, and a controller including one or more processors and one or more memory devices, the one or more memory devices storing computer-executable instructions for receiving a substrate in the PR deposition chamber; depositing PR on a surface of the substrate in the PR deposition chamber; receiving the substrate with the PR in the PAB chamber; and processing the PR in the PAB chamber. receiving the substrate in the PEB chamber after processing the PR, where a portion of the PR has been chemically altered by exposure to radiation to create a patterned PR; treating the patterned PR in the PEB chamber to alter a material property of the patterned PR; and controlling the one or more processors to dry develop the patterned PR in the develop chamber by removing either exposed or unexposed portions of the patterned PR by a dry develop process including exposure to a compound to form a PR mask.

[0007] In some embodiments, the PR is a metal-containing PR. In some embodiments, the PR is an EUV PR. In some embodiments, the plurality of reaction chambers further include a substrate cleaning chamber, and the computer-executable instructions, prior to the computer-executable instructions for receiving the substrate having the PR in the PAB chamber, further include instructions for controlling the one or more processors to receive the substrate having the PR in the cleaning chamber; and perform a dry cleaning process to remove PR from a bevel edge and / or a backside of the substrate. In some embodiments, the plurality of reaction chambers further include an underlayer deposition chamber, and the computer-executable instructions, prior to the computer-executable instructions for depositing PR, further include instructions for controlling the one or more processors to deposit an underlayer on the front surface of the substrate by a dry process, the underlayer increasing adhesion of the PR to the substrate. In some embodiments, the underlayer deposition chamber is the PR deposition chamber.

[0008] In some embodiments, the plurality of reaction chambers further include a pretreatment chamber, and the computer-executable instructions further include instructions for controlling the one or more processors to treat the surface of the substrate via a dry process to generate more exposed hydroxyl groups on the surface of the substrate prior to the computer-executable instructions for depositing a metal-containing photoresist. In some embodiments, each of the plurality of reaction chambers is at subatmospheric pressure, and the photoresist may be at subatmospheric pressure until the dry development process is completed. In some embodiments, an ambient environment of the substrate may be controlled to reduce exposure of the photoresist to moisture before the patterned photoresist is dry-developed. In some embodiments, the computer-executable instructions further include computer-executable instructions for depositing the photoresist via a dry process comprising mixing a water vapor flow of an organometallic precursor with a water vapor flow of a counter-reactant. In some embodiments, the processes performed by the plurality of reaction chambers are all dry processes. In some embodiments, the processes performed by the plurality of reaction chambers include wet and dry processes.

[0009] In some embodiments, the cluster includes multiple PR deposition chambers. In some embodiments, the PAB chamber and the PEB chamber are the same chamber. In some embodiments, the computer-executable instructions further include instructions for controlling the one or more processors to perform a dry cleaning process to remove PR from a bevel edge and / or backside of the substrate in the PAB chamber. In some embodiments, the multiple reaction chambers further include a lithography scanner, and the computer-executable instructions, prior to the computer-executable instructions for receiving the substrate in the PEB chamber, further include instructions for controlling the one or more processors to receive the substrate with the lithography scanner; and expose a portion of the PR to radiation to create a patterned PR. In some embodiments, the multiple substrate processing environments further include a thermal treatment processing environment, and the one or more memory devices further include computer-executable instructions for controlling the one or more processors to thermally treat the metal-containing PR in the thermal treatment processing environment before and / or after a portion of the metal-containing PR is chemically altered by exposure to radiation to create a patterned PR.

[0010] Another aspect of the embodiments disclosed herein provides an integrated substrate processing system, the system including a plurality of substrate processing environments, the plurality of substrate processing environments including a metal-containing photoresist (PR) deposition environment, one or more other separate integrated processing environments selected from the group consisting of: an additional metal-containing photoresist (PR) deposition environment, a metal-containing PR development environment, and a thermal processing environment, and a controller including one or more processors and one or more memory devices, the one or more memory devices including computer-executable instructions for controlling the one or more processors to receive a substrate in the metal-containing PR deposition environment, deposit a metal-containing PR on a surface of the substrate in the metal-containing PR deposition environment, and perform additional PR processing operations in the one or more other separate integrated processing environments.

[0011] In some embodiments, the plurality of substrate processing environments further include a PR dry development processing environment, and the one or more memory devices further store computer-executable instructions for controlling the one or more processors to chemically alter a portion of the metal-containing PR by exposing it to radiation to create a patterned PR, and then dry-develop the patterned PR in the development environment to form a PR mask by removing either the exposed or unexposed portions of the patterned PR by a dry development process including exposure to a compound. In some embodiments, the plurality of substrate processing environments further include a scanner environment, and the one or more memory devices further store computer-executable instructions for controlling the one or more processors to expose a portion of the metal-containing PR to radiation in the scanner environment to chemically alter the exposed portions.

[0012] In some embodiments, the plurality of substrate processing environments are different process chambers within a cluster. In some embodiments, the plurality of substrate processing environments are different stations within a chamber. In some embodiments, the plurality of substrate processing environments include three metal-containing PR deposition environments. In some embodiments, the plurality of substrate processing environments include two metal-containing PR deposition environments and a metal-containing PR development environment, and the one or more memory devices further store computer-executable instructions for controlling the one or more processors to develop the patterned PR via a dry process after portions of the metal-containing PR are chemically altered by exposure to radiation to create patterned PR.

[0013] In some implementations, the plurality of substrate processing environments include a metal-containing PR deposition environment, a thermal treatment processing environment, and a metal-containing PR development environment, and the one or more memory devices further store computer-executable instructions for controlling the one or more processors to: heat-treat the metal-containing PR in the thermal treatment processing environment before and / or after a portion of the metal-containing PR is chemically altered by exposure to radiation to create a patterned PR; and develop the patterned PR via a dry process after heat-treating the metal-containing PR in the thermal treatment processing environment. In some implementations, the plurality of substrate processing environments include a metal-containing PR deposition environment, a first thermal treatment processing environment, a second thermal treatment processing environment, and a metal-containing PR development environment, and the one or more memory devices further store computer-executable instructions for controlling the one or more processors to: heat-treat the metal-containing PR in the first thermal treatment processing environment before a portion of the metal-containing PR is chemically transformed by exposure to radiation to create a patterned PR; heat-treat the metal-containing PR in the second thermal treatment processing environment after a portion of the metal-containing PR is chemically transformed by exposure to radiation to create a patterned PR; and develop the patterned PR via a dry process after heat-treating the metal-containing PR in the second thermal treatment processing environment.

[0014] These and other features of the disclosed embodiments are described in detail below with reference to the associated drawings. [Brief explanation of the drawings]

[0015] [Figure 1] FIG. 1 shows a process flow diagram in one exemplary embodiment.

[0016] [Figure 2] FIG. 2 shows an exemplary chemical reaction scheme of the present technology.

[0017] [Figure 3A]FIG. 3A illustrates a representative process flow for one exemplary embodiment. [Figure 3B] FIG. 3B illustrates a representative process flow for one exemplary embodiment. [Figure 3C] FIG. 3C illustrates a representative process flow for one exemplary embodiment. [Figure 3D] FIG. 3D illustrates a representative process flow for one exemplary embodiment. [Figure 3E] FIG. 3E illustrates a representative process flow for one exemplary embodiment.

[0018] [Figure 4] FIG. 4 is a schematic diagram illustrating an example process chamber for performing methods according to disclosed embodiments. [Figure 5] FIG. 5 is a schematic diagram illustrating an example process chamber for performing methods according to disclosed embodiments. [Figure 6] FIG. 6 is a schematic diagram illustrating an example process chamber for performing methods according to disclosed embodiments. [Figure 7] FIG. 7 is a schematic diagram illustrating an example process chamber for performing methods according to disclosed embodiments. [Figure 8] FIG. 8 is a schematic diagram illustrating an example process chamber for performing methods according to disclosed embodiments. [Figure 9] FIG. 9 is a schematic diagram illustrating an example process chamber for performing methods according to disclosed embodiments.

[0019] [Figure 10A] FIG. 10A is a schematic diagram of various process cluster configurations in the disclosed embodiments. [Figure 10B] FIG. 10B is a schematic diagram of various process cluster configurations in the disclosed embodiments. [Figure 10C] FIG. 10C is a schematic diagram of various process cluster configurations in disclosed embodiments. [Figure 10D]FIG. 10D is a schematic diagram of various process cluster configurations in disclosed embodiments. [Figure 10E] FIG. 10E is a schematic diagram of various process cluster configurations in disclosed embodiments. [Figure 10F] FIG. 10F is a schematic diagram of various process cluster configurations in disclosed embodiments.

[0020] [Figure 11] FIG. 11 illustrates various example tool architectures that may be used to perform methods according to the disclosed embodiments. [Figure 12] FIG. 12 illustrates various example tool architectures that may be used to perform methods according to the disclosed embodiments. [Figure 13A] FIG. 13A illustrates various example tool architectures that may be used to perform methods according to the disclosed embodiments. [Figure 13B] FIG. 13B illustrates various example tool architectures that may be used to perform methods according to the disclosed embodiments. DETAILED DESCRIPTION OF THE INVENTION

[0021] The present disclosure relates generally to the field of semiconductor processing. In particular aspects, the present disclosure is directed to methods and apparatus for processing EUV photoresists (e.g., EUV-sensitive metal and / or metal oxide-containing resist films) in conjunction with EUV patterns and EUV-patterned film development to form patterning masks.

[0022] Reference will be made in detail herein to specific embodiments of the present disclosure. Examples of specific embodiments are illustrated in the accompanying drawings. While the present disclosure will be described in connection with these specific embodiments, the present disclosure is not limited to such specific embodiments. On the contrary, the present disclosure also covers alternatives, modifications, and equivalents that may be included within the scope of the present disclosure. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the present disclosure. The present disclosure may be practiced without some or all of the following specific features. In other instances, well-known process operations are omitted in detail to avoid unnecessarily obscuring the present disclosure.

[0023] Patterning thin films in semiconductor processing is often a critical step in semiconductor manufacturing. Patterning involves lithography. In conventional photolithography, such as 193 nm photolithography, pattern printing involves emitting photons from a photon source onto a mask, printing a pattern onto a light-sensitive photoresist, causing a chemical reaction in the photoresist, and after development, removing specific portions of the photoresist to form the pattern.

[0024] Advanced technology nodes (as defined by the International Technology Roadmap for Semiconductors) include the 22 nm, 16 nm, and beyond. For example, at the 16 nm node, the width of a typical via or line in a damascene structure is typically about 30 nm or less. The scaling of features on advanced semiconductor integrated circuits (ICs) and other devices is driving further improvements in lithographic resolution.

[0025] Extreme ultraviolet (EUV) lithography can extend lithography technology by moving to imaging source wavelengths smaller than those achievable with conventional photolithography methods. EUV sources with wavelengths of approximately 10-20 nm or 11-14 nm, e.g., 13.5 nm, can be used in cutting-edge lithography tools, also known as scanners. EUV radiation is strongly absorbed by a wide range of solid and fluid materials, including quartz and water vapor, and therefore operates in a vacuum.

[0026] EUV lithography utilizes patterned EUV resist to form a mask for use in etching underlying layers. The EUV resist may be a polymer-based chemically amplified resist (CAR) fabricated by a liquid-based spin-on technique. As an alternative to CAR, direct photopatternable metal oxide-containing films, such as those available from Inpria, Corvallis, Oregon, and described in U.S. Patent Publications US2017 / 0102612, US2016 / 021660, and US2016 / 0116839, the disclosures of which are incorporated herein by reference, at least for their disclosure of photopatternable metal oxide-containing films, can be used. Such films can be fabricated by spin-on techniques or dry deposition. Metal oxide-containing films can be directly patterned (i.e., without the use of a separate photoresist) by EUV exposure in a vacuum environment, where patterning resolution of less than 30 nm is possible, as disclosed, for example, in U.S. Pat. No. 9,996,004 (EUV PHOTOPATTERNING OF VAPOR-DEPOSITED METAL OXIDE-CONTAINING HARD MASKS, issued June 12, 2018) and / or U.S. Patent Application No. PCT / US19 / 31618 (METHODS FOR MAKING EUV PATTERNABLE HARD MASKS, filed May 9, 2019), the disclosures of which are incorporated herein by reference, at least with respect to the composition, deposition, and patterning of directly photopatternable metal oxide films to form EUV resist masks. Generally, patterning involves exposing an EUV resist to EUV radiation to form a photopattern in the resist, followed by development to remove portions of the resist according to the photopattern to form the mask.

[0027] While this disclosure relates to lithographic patterning techniques and materials exemplified for EUV lithography, it should also be understood that it is applicable to other next-generation lithography technologies. In addition to EUV, which includes the standard 13.5 nm EUV wavelength currently in use and under development, DUV (deep-UV), which generally refers to the use of 248 nm or 193 nm excimer laser sources, X-ray, formally including EUV in the lower energy range in the X-ray range, and electron beam, which covers a wide energy range, are the radiation sources most relevant to such lithography. Specific methods may depend on the specific materials and applications used in the semiconductor substrate and final semiconductor device. Accordingly, the methods described herein are merely exemplary of methods and materials that may be used in the present technology.

[0028] Direct photopatternable EUV resists may consist of or contain metals and / or metal oxides mixed within an organic component. Metals / metal oxides hold great promise for enhancing EUV photon absorption, further generating secondary electrons, and / or improving etch selectivity relative to underlying film and device layers. To date, these resists have been developed using a wet (solvent) approach, which requires moving wafers in a track where they are exposed to a developing solvent, dried, and baked. Wet development not only limits productivity but also causes line collapse due to surface tension effects during solvent evaporation between fine features.

[0029] To address these issues, dry development techniques have been proposed to address substrate delamination and interface defects. Compared with wet development, dry development has its own challenges, such as etch selectivity between EUV-exposed and unexposed resist materials, resulting in higher size-to-dose requirements for effective resist exposure. If the selectivity is suboptimal, longer exposure under etching gases can also cause rounding of PR corners, which can lead to larger line critical dimension (CD) variations in the subsequent transfer etching process.

[0030] 1 illustrates a flow diagram of an exemplary method for performing dry chamber cleaning when depositing and developing photoresist, in some embodiments. The operations of process 100 may be performed in a different order and / or with different, fewer, or more operations. One or more operations of process 100 may be performed using various apparatus described herein. In some embodiments, the operations of process 100 may be implemented, at least in part, according to software stored on one or more non-transitory computer-readable media.

[0031] At block 102 of process 100, a layer of photoresist is deposited. The deposition can be either a dry deposition process, such as an evaporation process, or a wet process, such as a spin-on deposition process. The photoresist can be an EUV resist or a metal-containing EUV resist. Figure 2 shows an exemplary process for forming a polymerized organometallic material and depositing a metal-containing EUV resist.

[0032] Referring back to FIG. 1 , in addition to depositing a metal-containing EUV resist film on a semiconductor substrate in block 102 of process 100, a metal-containing EUV resist material can be formed on the interior surfaces of the process chamber. The interior surfaces can include the chamber walls, floor, and ceiling of the process chamber. Other interior surfaces can include the showerhead, nozzle, and substrate support surface. The metal-containing EUV resist material can be formed as a result of a dry deposition process, such as a CVD or ALD process. The thickness of the metal-containing EUV resist material formed on the interior surfaces can increase over time as a result of additional processing (e.g., deposition) operations being performed in the process chamber. The metal-containing EUV resist material has a tendency to flake off, generate particles, or flake off the interior surfaces of the process chamber, which can contaminate subsequent semiconductor substrates during processing.

[0033] In block 150 of process 100, a dry chamber clean operation of the present disclosure can be performed as a subsequent step to depositing a metal-containing EUV resist film on a semiconductor substrate in block 102 of process 100. This allows deposition and dry clean to be performed in the same process chamber. However, it should be apparent that the dry chamber clean can be performed in a different process chamber than the deposition operation in some embodiments. In fact, the dry chamber clean can be performed after bevel and / or backside clean, bake, develop, or etch operations.

[0034] The dry-deposited metal-containing EUV photoresist films being removed are typically composed of Sn, O, and C, but the same cleaning method can be applied to films of other metal oxide resists and materials, and the method can also be used for film strip and PR rework.

[0035] In block 104 of process 100, an optional cleaning process cleans the backside and / or bevel edge of the semiconductor substrate. Backside and / or bevel edge cleaning can non-selectively etch the EUV resist film to equally remove films that are oxidized or crosslinked to various degrees on the backside and bevel edge of the substrate. During application of the EUV patternable film, either wet or dry deposition processes can result in unintentional deposition of resist material on the bevel edge and / or backside of the substrate. This unintentional deposition can induce particles that can subsequently migrate to the top surface of the semiconductor substrate and cause particle defects. This bevel edge and backside deposition can also cause problems in downstream processing, including contamination of patterning (scanner) and development tools. Traditionally, removal of this bevel edge and backside deposition is accomplished by wet cleaning techniques. For spin-coated photoresist materials, this process is called edge bead removal (EBR) and is accomplished by directing a flow of solvent from above and below the bevel edge while the substrate is rotating. The same process can be applied to soluble organotin oxide-based resists deposited by evaporation techniques. The bevel edge and / or backside cleaning of the substrate can be a dry cleaning process.

[0036] In block 150 of process 100, the dry chamber cleaning operation of the present disclosure may be performed after the bevel edge cleaning and / or backside cleaning operations. This allows the bevel cleaning and / or backside cleaning and the dry chamber cleaning to be performed in the same process chamber. However, it should be apparent that in some embodiments, the dry chamber cleaning can be performed in a different process chamber than the bevel edge cleaning and / or backside cleaning operations.

[0037] In block 106 of process 100, an optional post-apply bake (PAB) is performed after deposition of the EUV patternable film and before EUV exposure. The PAB process can include a combination of thermal treatment, chemical exposure, and moisture to increase the EUV sensitivity of the EUV patternable film, allowing patterns to be developed in the EUV patternable film with reduced EUV doses.

[0038] In block 150 of process 100, the dry chamber clean operation of the present disclosure may be performed after the PAB process. This allows the bake and dry chamber clean to be performed in the same process chamber. However, it should be apparent that in some embodiments, the dry chamber clean can be performed in a different process chamber than the PAB process operation.

[0039] In block 108 of process 100, the metal-containing EUV resist film is exposed to EUV radiation to develop a pattern. Generally, exposure to EUV changes the chemical composition and cross-linking of the metal-containing EUV resist film, providing etch selectivity contrast for subsequent development. After exposing the metal-containing EUV resist film to EUV light, a photopatterned metal-containing EUV resist is obtained. The photopatterned metal-containing EUV resist includes EUV-exposed and unexposed regions.

[0040] An optional post-exposure bake (PEB) is performed in block 110 of process 100 to further increase the contrast in etch selectivity of the photopatterned metal-containing EUV resist. The photopatterned metal-containing EUV resist may be thermally treated in the presence of various chemical species to promote crosslinking of the EUV-exposed regions of the photopatterned metal-containing EUV resist, or may simply be baked on a hotplate in air.

[0041] In block 150 of process 100, the dry chamber clean operation of the present disclosure may be performed after the PEB process. This allows the bake and dry chamber clean to be performed in the same process chamber. However, it should be apparent that in some embodiments, the dry chamber clean can be performed in a different process chamber than the PEB process operation.

[0042] In block 112 of process 100, the photopatterned metal-containing resist is developed to form a resist mask. In various embodiments, either the exposed regions are removed (positive tone) or the unexposed regions are removed (negative tone). In some embodiments, development can include selective deposition of the photopatterned metal-containing resist onto either the exposed or unexposed regions, followed by an etching operation. In various embodiments, these processes can be dry or wet processes. An example development process includes subjecting an organotin oxide-containing EUV-sensitive photoresist thin film (e.g., 10-30 nm thick, e.g., 20 nm thick) to an EUV exposure dose and a post-exposure bake, followed by development. The photoresist film can be deposited based on a gas-phase reaction of an organotin precursor, such as isopropyl(tris)(dimethylamino)tin, with water vapor, or can be a spin-on film containing tin clusters in an organic matrix. The photopatterned metal-containing resist is developed by exposure to a development chemistry. In some embodiments, the development chemistry comprises a halide-containing chemistry.

[0043] In block 150 of process 100, a dry chamber clean operation of the present disclosure can be performed after development. This allows development and dry chamber clean to be performed in the same process chamber. However, it will be apparent that in some embodiments, the dry chamber clean can be performed in a different process chamber than the development operation. Furthermore, it will be apparent that in some embodiments, the dry chamber clean can be performed in the same or a different process chamber than the etching operation. An etching operation may also be performed to etch an underlying substrate layer of the semiconductor substrate.

[0044] Each of operations 102-112 is described in more detail below. In various embodiments, the method of the present technology combines all dry steps of film formation by vapor deposition, (EUV) lithography photopatterning, and dry development. In other embodiments, the method of the present technology includes wet deposition and dry development, or dry deposition and wet development. In some processes, after photopatterning in an EUV scanner, the substrate can be placed directly into a dry development / etching chamber. Such a process can avoid the material and production costs associated with wet development. Alternatively, a post-exposure bake step can be performed in the development chamber or a separate chamber to further crosslink the exposed regions and form a denser SnO-like network.

[0045] In some embodiments, the substrate may be placed in various processing environments to perform each of operations 102-112. Examples include a PR deposition environment, one or more thermal treatment environments for PAB and / or PEB, a wafer cleaning environment, a scanning environment, and a PR development environment. As described below, in some embodiments, one or more of these environments may be stations / pedestals within a chamber, a chamber with one or more pedestals, and / or a multi-chamber cluster tool with one or more chambers. In some embodiments, multiple operations may be performed in a single processing environment. For example, the thermal treatment environment and the wafer cleaning environment may be the same processing environment, in which case both operations may be performed sequentially without moving the wafer to a different pedestal, chamber, or tool. In some embodiments, multiple processing environments may be within the same chamber or tool; for example, the thermal treatment environment and the wafer cleaning environment may be in different stations within a quad-station module chamber. In some embodiments, multiple processing environments of the same type may be provided within the same tool, for example, to enhance or optimize throughput in multi-operation wafer processing situations where some processing operations are much slower than others. It should be understood that other combinations of environments as defined above are also within the scope of the present disclosure.

[0046] The dry process of the present technology does not limit the mechanism, function, or utility of the technology, but may offer various advantages over wet development processes known to those skilled in the art. For example, the dry deposition techniques described herein can deposit thinner, defect-free films than can be achieved using wet spin-coating techniques, and the exact thickness of the deposited film can be adjusted and controlled by simply extending or shortening the length of the deposition step or sequence. Thus, dry processes may offer greater tunability and provide better critical dimension (CD) control and scum removal. Dry development may offer improved performance (e.g., preventing line collapse due to surface tension in wet development) and enhanced throughput (e.g., avoiding wet development tracks). Other advantages may include the elimination of the need for organic solvent-based developers, reduced susceptibility to adhesion, the elimination of the need for wet resist application and removal (e.g., avoiding scum and pattern distortion), improved line edge roughness, the ability to pattern directly on device topography, the ability to tailor hard mask chemistries for specific substrates and semiconductor device designs, and the absence of other solubility-based limitations.

[0047] In some cases, it may be appropriate or optimal to combine wet and dry processing. For example, where a significant capital investment has been made in wet wafer processing equipment, performance may be improved by integrating dry processing and its associated equipment with the wet processing equipment for some operations in a multi-operation process.

[0048] Thus, the present disclosure provides processes and apparatus configured to dry develop EUV photopatterned metal and / or metal oxide-containing resist as part of an EUV resist mask formation process. Various embodiments include combining all dry operations of deposition film formation, (EUV) lithography photopatterning, and dry development. Various other embodiments include effectively combining the dry processing operations described herein with wet processing operations; for example, spin-on EUV photoresist (wet process) available from Inpria may be combined with dry development or other wet or dry processes described herein. In various embodiments, wafer cleaning may be a wet process as described herein, while other processes are dry. In further embodiments, a wet development process may be performed in combination with PR film (dry) deposition.

[0049] Lithography Processing: 3A-3E illustrate another exemplary process flow for forming a metal photoresist hard mask. In general, a metal-containing film that is sensitive to a patterning agent, such as photons, electrons, protons, ions, or neutral species, and that can be patterned by exposure to any of these species, is deposited on a semiconductor substrate. The metal-containing film is then patterned by exposure to a patterning agent in a vacuum environment to form a metal mask. This description primarily refers to metal-containing films, particularly those patterned by extreme ultraviolet lithography (EUV lithography (EUVL)), particularly when the metal is Sn, using an EUV source with excited Sn droplets. Hereinafter, such films are referred to as EUV-sensitive films. However, it should be understood that other implementations (e.g., different metal-containing films and patterning agents / techniques) are possible.

[0050] 3A shows a semiconductor substrate 100 to be patterned. In a typical example, the semiconductor substrate 100 is a silicon wafer having integrated circuits formed in part thereof.

[0051] FIG. 3B shows a metal-containing film 102 that is sensitive to a patterning agent deposited on a semiconductor substrate 100. The metal-containing film may be a metal salt (e.g., a metal halide) or an organometallic compound that is sensitive to exposure to a patterning agent so that the metal-containing film can be decomposed into a base material and be sensitive to a subsequent development process. Suitable patterning agents may be photons, electrons, protons, ions, or neutral species, and the metal-containing film 102 can be patterned by being exposed to one of these species and decomposed into a base material, or be sensitive to a subsequent development process. Typically, prior to deposition, the semiconductor substrate 100 is placed in a reactor chamber, and metal-containing film deposition occurs under vacuum.

[0052] A blanket of metal-containing film 102 can be formed by condensation from appropriate precursors (e.g., in a non-plasma CVD reactor such as an Altus® CVD tool or an Aether® GP CVD tool, available from Lam Research Corporation, Fremont, California). Suitable process conditions for this deposition by condensation include a deposition temperature between about 0°C and 250°C, e.g., between ambient temperature (e.g., about 23°C) and 150°C, and a reactor pressure of less than 20 Torr (e.g., pressure maintained between 0.5 and 2 Torr at 60°C). The deposition rate can be controlled by maintaining a precursor flow rate between about 100 and 1000 sccm.

[0053] The Sn-containing film is deposited and transferred in a vacuum environment to prevent degradation by water vapor. The deposited film is then transferred to an EUV patterning tool and patterned by direct exposure without the use of photoresist, as shown in Figures 3C-3D.

[0054] It should be noted that EUVL tools typically operate at higher vacuums than deposition tools, and in this case it is desirable to increase the vacuum environment of the substrate during transfer from deposition to the patterning tool, and to degas the substrate and deposited metal-containing film before loading into the patterning tool to prevent contamination of the optics of the patterning tool by outgassing the substrate.

[0055] As shown in FIG. 3C, this patterning results in exposed metal-containing film regions 102a of the formed metal mask and unexposed regions 102b of material that are removed by pattern development.

[0056] As shown in FIG. 3D, the pattern can then be developed. Development is described in more detail elsewhere herein. In some embodiments, pattern development can occur by simply heating the substrate to volatilize the unexposed regions 102b of the metal-containing film, leaving only the exposed regions 102a as a fully formed metal mask. Note that this pattern development operation does not require vacuum integration, as it produces a thermally and environmentally stable patterned metal mask. Additionally, pattern development is preferably performed outside the tool to avoid contamination of the patterning tool's optics with incompatible byproducts of metal-containing film decomposition.

[0057] As shown in FIG. 3E, pattern amplification can be performed as an optional step. For example, selective ALD or electroless deposition (ELD) may be performed on the patterned substrate after the operations shown in FIGS. 3C and / or 3D to further increase the thickness of the metal mask by selectively depositing additional metal 106. This may reduce the optical transmission of the mask or enhance its mechanical strength. Such amplification may be achieved by application of electroless deposition processes, such as those described in U.S. Pat. Nos. 6,911,067, 6,794,288, 6,902,605, and 4,935,312, which are incorporated herein by reference for their disclosures in this regard.

[0058] For example, an initial 1 nm seed can be amplified to 10 nm in this manner. This operation does not require vacuum integration, as a thermally and environmentally stable patterned metal mask can be formed prior to amplification, as in the pattern development described with reference to Figure 3D.

[0059] One advantage of all-dry or partially dry deposition is that the dry operation can be a one-pass adjustable process. The operation can be optimized by varying various process conditions, as described below. For example, the dry process for PR deposition and underlayer requires only two passes, whereas a wet process may require a rinse and bake operation before the PR film deposition. On the other hand, a wet process may require the use of premixed solutions according to process parameters, or additional passes for heat treatment, cooling, and spin drying. A dry process can eliminate the drying step of the solution, reducing PR delamination and line tilt / collapse.

[0060] Another advantage of all-dry or partial-dry deposition is greater control over the processing environment. Wet spin-on processes use pre-formulated solutions and can be performed at ambient pressure. Dry processes can be performed under vacuum, with control over, for example, pressure, humidity, oxygen, temperature, etc. In embodiments where integrated processes are performed in the same tool, chamber, or station, the vacuum can be maintained between dry processes, which is advantageous for controlling the wafer environment during and between processing operations. Additionally, integrated processes can reduce wait times because the processes are performed in the same tool, chamber, or station.

[0061] Photoresist (PR) deposition: As noted above, the present disclosure provides methods for fabricating imaging layers on semiconductor substrates that can be patterned using EUV or other next-generation lithography techniques. Exemplary methods include forming polymerized organometallic materials in water vapor and depositing them onto the substrate. In other embodiments, spin-on methods may be used.

[0062] This technology provides a method for depositing EUV-sensitive thin films onto substrates to act as resists for subsequent EUV lithography and processing. These EUV-sensitive films are composed of materials that undergo changes upon EUV irradiation, such that bulky pendant substituents bonded to metal atoms in low-density M-OH-rich materials are lost, allowing crosslinking to occur to higher-density M-OH-bonded metal oxide materials. EUV patterning can create film regions with altered physical and chemical properties relative to unexposed regions. These properties can be exploited in subsequent processing, such as dissolving the unexposed and exposed regions or selectively depositing materials in the exposed and unexposed regions. In some embodiments, under the conditions in which such subsequent processing occurs, the unexposed film has a hydrophobic surface, while the exposed film has a hydrophilic surface (it is recognized that the hydrophilic properties of exposed and unexposed regions are relative to each other). For example, differences in the chemical composition, density, and crosslinking of the films can be exploited to effect material removal. Removal can be achieved by wet or dry processes, as further described below.

[0063] The thickness of the EUV-patternable film formed on the substrate surface can vary depending on the surface characteristics, materials used, and processing conditions. In various embodiments, the film thickness can range from 0.5 nm to 100 nm, preferably thick enough to absorb a majority of the EUV light under EUV patterning conditions. For example, the overall absorption of the resist film can be 30% or less (e.g., 10% or less, 5% or less) so that the resist material at the bottom of the resist film is fully exposed. In some embodiments, the film thickness is 10-20 nm. While not limiting the mechanism, function, or utility of the present disclosure, the disclosed process, unlike conventional wet spin-coating processes, has fewer constraints on substrate surface adhesion and is therefore believed to be applicable to a wider variety of substrates. Furthermore, as discussed above, deposited films can closely conform to surface features, providing advantages when forming masks on substrates, such as substrates with inherent features, without "filling" or planarizing the features.

[0064] substrate : Substrates useful in the methods of the present technology can include any material composition suitable for lithographic processing, particularly for the fabrication of integrated circuits and other semiconductor devices. In some embodiments, the substrate is a silicon wafer. The substrate can also be a silicon wafer having features formed thereon with irregular surface topography ("intrinsic topographical features"). (As used herein, "surface" refers to the surface onto which the film of the present technology is deposited or the surface that is exposed to EUV light during processing.) Such inherent topographical features can include areas from which material has been removed (e.g., by etching) or added (e.g., by deposition) during processing prior to performing the methods of the present technology. Such prior processing can include the methods of the present technology or other processing methods in an iterative process in which two or more feature layers are formed on the substrate. Without limiting the mechanism, function, or utility of the present technology, it is believed that in some embodiments, the methods of the present technology can offer advantages over art-known methods of depositing photolithographic films onto the surface of a substrate using spin-casting. It is believed that these advantages result from the ability of the present technology's films to conform to underlying features without "filling" or planarizing the features, and from the ability to deposit films on a wide variety of material surfaces.

[0065] In some embodiments, the incoming wafer is provided with a substrate surface of the desired material, with the topmost material being the layer to which the resist pattern will be transferred. The choice of material will depend on the integration level, but it is generally desirable to select a material that can be etched with high selectivity (i.e., faster etching) to the EUV resist and imaging layers. Examples of suitable substrate materials include various carbon-based films (e.g., ashing hard masks (AHMs), silicon-based films (e.g., SiOx, SiOxNy, SiOxCyNz), a-Si:H, poly-Si, or SiN), or other (typically sacrificial) films applied to facilitate the patterning process.

[0066] In some embodiments, the substrate is a hard mask, which is used in the lithographic etching of the underlying semiconductor material. Hard masks include amorphous carbon (aC), SnO x ,SiO2,SiO x N y ,SiO x C, Si3N4, TiO2, TiN, W, W-doped C, WO x, The substrate may be made of any of a variety of materials, such as HfO2, ZrO2, and Al2O3. For example, the substrate may be made of a SnO2 substrate. x In various embodiments, the layer can be from 1 nm to 100 nm thick, or from 2 nm to 10 nm thick.

[0067] In some embodiments, the substrate includes an underlayer. The underlayer may be deposited on a hard mask or other layer and is generally located below the imaging layer, as described herein. The underlayer can be used to enhance the sensitivity of the photoresist, increase EUV absorption, and / or enhance the patterning performance of the photoresist. When the substrate to be patterned has significant topography due to device features, another important function of the underlayer is to overcoat and planarize the existing topography, allowing subsequent patterning steps to be performed on a flat surface with focus on the entire area of ​​the pattern. In such applications, the underlayer (or at least one of multiple underlayers) may be applied using a spin-coating technique. When the photoresist material employed has a significant inorganic component, e.g., a predominantly metal oxide framework, the underlayer may advantageously be a carbon-based film applied by either spin-coating or a dry vacuum-based deposition process. This layer may include various ashing hardmask (AHM) films having carbon and hydrogen-based compositions, and may be doped with additional elements such as tungsten, boron, nitrogen, or fluorine. Methods and apparatus useful in such processes are described in U.S. Patent Application No. 62,909,430, filed October 2, 2019, which is incorporated herein by reference for its method and apparatus disclosure.

[0068] Film deposition: In various embodiments, the EUV patternable film is formed by deposition on the substrate using deposition equipment and processes known in the art, in which a polymerized organometallic material is formed in the vapor phase or in situ on the substrate surface.

[0069] Typically, a water vapor stream of an organometallic precursor is mixed with a water vapor stream of a counter-reactant to form a polymerized organometallic material, which is then deposited on the surface of a semiconductor substrate. As one skilled in the art will appreciate, the mixing and deposition in this process may be simultaneous in a substantially continuous process. Methods and apparatus useful in such processes are described in publications PCT / US2019 / 031618, filed May 9, 2019, and PCT / US2019 / 060742, filed November 11, 2019, which are incorporated herein by reference for their method and apparatus disclosures, particularly regarding various organometallic precursors.

[0070] EUV-sensitive thin films can be deposited on semiconductor substrates, and these films can be used as resists for subsequent EUV lithography and processing. These EUV-sensitive thin films are composed of materials that undergo changes upon EUV irradiation, such that bulky pendant substituents bonded to metal atoms in low-density M-OH-rich materials are eliminated, allowing crosslinking to occur to higher-density M-OH-bonded metal oxide materials. EUV patterning can create film regions with altered physical and chemical properties relative to unexposed regions. These properties can be exploited in subsequent processing, such as dissolving the unexposed and exposed regions or selectively depositing materials in the exposed and unexposed regions. In some embodiments, the unexposed film has a more hydrophobic surface than the exposed film under the conditions under which such subsequent processing will occur. For example, differences in the chemical composition, density, and crosslinking of the films can be exploited to effect material removal. Removal can be accomplished by wet or dry processes, as further described below.

[0071] In various embodiments, the thin film is an organometallic material, such as an organotin material including tin oxide, or other metal oxide material / moiety. The organometallic compound can be produced by the vapor-phase reaction of an organometallic precursor with a counter-reactant. In various embodiments, the organometallic compound is formed by mixing a specific combination of organometallic precursors having bulky alkyl or fluoroalkyl groups with a counter-reactant and polymerizing the mixture in the vapor phase to produce a low-density EUV-sensitive material that is deposited on the semiconductor substrate.

[0072] In various embodiments, the organometallic precursors contain at least one alkyl group on each metal atom that can survive gas-phase reaction, while other ligands or ions coordinated to the metal atoms can be replaced by counter reactants. Organometallic precursors include those represented by the general formula (1): M a R b L c (General formula 1) where M is a metal with a large EUV absorption cross section; R is C n H 2n+1 (preferably n≧2); L is a ligand, ion, or other moiety reactive with a counter reactant; a≧1; b≧1; and c≧1.

[0073] In various embodiments, M is 1x10 7 cm 2 / mol. M can be, for example, selected from the group consisting of tin, hafnium, tellurium, bismuth, indium, antimony, germanium, and combinations thereof. In some embodiments, M is tin. R can be fluorinated, for example, a compound of formula C n F x H (2n+1)In various embodiments, R has at least one β-hydrogen or β-fluorine. For example, R can be selected from the group consisting of ethyl, i-propyl, n-propyl, t-butyl, i-butyl, n-butyl, sec-butyl, n-pentyl, i-pentyl, t-pentyl, sec-pentyl, and mixtures thereof. L can be any moiety that is readily displaced by a counter reactant to generate an M-OH moiety, such as a moiety selected from the group consisting of an amine (dialkylamino, monoalkylamino, etc.), an alkoxy, a carboxylate, a halogen, and mixtures thereof.

[0074] Counter-reactants have the ability to chemically bond at least two metal atoms by displacing a reactive moiety, ligand, or ion (e.g., L in Formula 1 above). Examples of counter-reactants include water, peroxides (e.g., hydrogen peroxide), di- or polyhydroxy alcohols, fluorinated di- or polyhydroxy alcohols, fluorinated glycols, and other sources of hydroxyl moieties. In various embodiments, the counter-reactant reacts with the organometallic precursor by forming an oxygen bridge between adjacent metal atoms.

[0075] Other potential counter reactants include hydrogen sulfide and hydrogen disulfide, which can bridge metal atoms via sulfur bridges. In another example, Te-containing precursors can be used as counter reactants, together with or instead of water, to form, for example, Te-Sn-Te-Sn bridges. Tellurium coreactants suitable for use with Sn(NMe2)x-type precursors include RTeH, RTeD (D = deuterium), and R2Te precursors (R = alkyl group, particularly t-butyl or isopropyl), such as t-butylTeD. For example, bis(trimethylsilyl)Te can be used with M(OR)x-type precursors.

[0076] In addition to the organometallic precursor and counter-reactant, the thin film can include optional materials to modify the chemical or physical properties of the film, such as altering the film's sensitivity to EUV or improving its etch resistance. Such optional materials can be introduced, for example, by doping during vapor deposition, before semiconductor substrate deposition, after film deposition, or both. In some embodiments, a gentle remote H plasma can be introduced to replace some Sn-L bonds with Sn-H, thereby increasing the reactivity of the resist under EUV.

[0077] In various embodiments, the EUV-patternable film is formed by deposition on a semiconductor substrate using deposition equipment and processes known in the art. In such processes, a polymerized organometallic material is formed on the surface of the semiconductor substrate in the gas phase or in situ. Suitable processes include, for example, chemical vapor deposition (CVD), atomic layer deposition (ALD), and ALD with a CVD component, e.g., discontinuous ALD-like processes in which the metal precursor and counter-reactant are separated in either time or space.

[0078] Generally, a water vapor flow of an organometallic precursor is mixed with a water vapor flow of a counter-reactant to form a polymerized organometallic material, which is then deposited on the surface of a semiconductor substrate. In some embodiments, two or more organometallic precursors are included in the water vapor flow. In some embodiments, two or more counter-reactants are included in the water vapor flow. As one skilled in the art will appreciate, the mixing and deposition in this process may be simultaneous in a substantially continuous process.

[0079] In one example of a continuous CVD process, two or more gas streams of organometallic precursor and counter-reactant sources are introduced into a deposition chamber of a CVD apparatus via separate inlet paths, where they mix and react in the gas phase to form a coagulated polymeric material (e.g., via metal-oxygen-metal bond formation). The gas streams can be introduced, for example, using separate inlets or a dual-plenum showerhead. The apparatus is configured so that the organometallic precursor and counter-reactant gas streams mix within the chamber, where they react to form a polymerized organometallic material. Without limiting the mechanism, function, or utility of this technology, it is believed that the product from such a gas-phase reaction will have a larger molecular weight as the metal atoms are crosslinked by the counter-reactant and then condensed or deposited onto a semiconductor substrate. In various embodiments, the steric hindrance of the bulky alkyl groups prevents the formation of a densely packed network, producing a smooth, amorphous, low-density film.

[0080] CVD processes are typically carried out under reduced pressure, such as between 10 milliTorr and 10 Torr (1333.22 mPa and 1333.22 Pa). In some embodiments, the process is carried out at between 0.5 and 2 Torr (66.6612 and 266.645 Pa). In some embodiments, the temperature of the semiconductor substrate is equal to or less than the temperature of the reactant stream. For example, the substrate temperature may be between 0°C and 250°C, or between ambient temperature (e.g., 23°C) and 150°C. In various processes, deposition of polymerized organometallic material onto the substrate occurs at a rate that is inversely proportional to the surface temperature.

[0081] The thickness of the EUV-patternable film formed on the surface of a semiconductor substrate can vary depending on the surface characteristics, materials used, and processing conditions. In various embodiments, the film thickness can range from 0.5 nm to 100 nm and can be thick enough to absorb a majority of the EUV light under EUV patterning conditions. The EUV-patternable film can accommodate absorption of 30% or more, resulting in significantly fewer EUV photons available toward the bottom of the EUV-patternable film. Higher EUV absorption results in more crosslinking and densification near the top of the EUV-exposed film compared to the bottom of the EUV-exposed film. While more efficient utilization of EUV photons is possible with EUV-patternable films having higher total absorption, it can be appreciated that in some instances, the EUV-patternable film may have an absorption less than about 30%. By comparison, the maximum overall absorption of most other resist films is less than 30% (e.g., 10% or less, or 5% or less), thereby ensuring sufficient exposure of the resist material at the bottom of the resist film. In some embodiments, the film thickness is 5 nm to 40 nm or 10 nm to 20 nm. Without limiting the mechanism, function, or utility of the present disclosure, it is believed that the process of the present disclosure, unlike wet spin-coating processes of the art, places fewer constraints on substrate surface adhesion and is therefore applicable to a wider variety of substrates. Furthermore, as noted above, deposited films can closely conform to surface features, providing advantages when forming masks on substrates, such as substrates with underlying properties, without "filling" or planarizing the features.

[0082] Another way that EUV sensitivity in PR films can be further improved in some embodiments of the technology described herein is by creating films with a vertically graded film composition, resulting in depth-dependent EUV sensitivity. A uniform PR with a high absorption coefficient requires a higher EUV dose to fully expose the bottom because the light intensity decreases throughout the film's depth. Increasing the density of atoms with high EUV absorption at the bottom of the film relative to the top (i.e., creating a gradient of increasing EUV absorption) allows for more efficient utilization of available EUV photons and distributes the absorption (and secondary electron effects) more uniformly at the bottom of the highly absorbing film.

[0083] The method for manipulating the vertical composition gradient of PR films is particularly applicable to dry deposition processes such as CVD and ALD, and can be achieved by adjusting the flow ratios between different reactants during deposition. Examples of manipulable composition gradients include the ratio between different highly absorbing metals, the proportion of metal atoms with EUV-decomposable bulky groups, the proportion of counter-reactants or bulky groups containing highly absorbing elements (e.g., Te and I), and combinations thereof. Further discussion of vertical gradient films is provided in PCT Publication PCT / US20 / 70172, filed June 24, 2020, which is incorporated herein by reference for its disclosure of these methods and apparatus.

[0084] Backside / Bevel Cleaning: When applying an EUV photoresist film to a substrate, either by conventional wet, e.g., spin-on, processing, or by dry deposition as described herein, unintentional deposition of resist material can occur on the bevel edge and / or backside of the wafer. This bevel edge and backside deposition can cause problems in downstream processing, including contamination of patterning (scanner) and development tools. Traditionally, removal of this bevel edge and backside deposition is accomplished by wet cleaning techniques.

[0085] The latest technology for cleaning spin-coated organometallic photoresists is the wet cleaning process. Edge bead removal (EBR) is performed on both the front and back sides of the wafer by placing a nozzle over the edge of the wafer and spraying a solvent onto the wafer while it is spinning. The organic solvent (e.g., PGME, PGMEA, 2-heptanone) dissolves the photoresist on the edge and cleans the bevel edge area. If the backside is contaminated, the wafer must be sent to a separate wet cleaning station for backside cleaning. With spin coating, the wafer area in contact with the chuck generally remains clean, and a separate backside clean is not always performed. Additional cleaning, such as dilute hydrofluoric acid (dHF), dilute hydrochloric acid (dHCl), dilute sulfuric acid, or standard clean 1 (SC-1), may be required to reduce metal contamination. A backside scrub is typically performed before the EUV scanner.

[0086] The solvents used in wet cleaning processes inherently have high acquisition and disposal costs. These solvents can be hazardous to the environment and pose potential health risks. Wet cleaning processes can be limited by the uniformity of EUV resist material removal on the bevel edge region; surface tension and water vapor often result in wavy removal, resulting in insufficient EUV resist material removal at the bevel edge region. Furthermore, backsplash using organic solvents can cause defects on the front side of the wafer. Wet cleaning processes are typically performed in separate tools / chambers, requiring wafers to be transferred between tools / chambers after deposition. This can contaminate the tools / chambers used for backside and / or bevel edge cleaning.

[0087] This document describes a cleaning process for cleaning the backside and / or bevel edge of a semiconductor substrate. Backside and / or bevel edge cleaning involves non-selective etching of an EUV resist film, thereby equally removing films that are oxidized or crosslinked to various degrees on the backside and bevel edge of the substrate. During application of an EUV-patternable film, either wet or dry deposition processes can result in unintentional deposition of resist material on the bevel edge and / or backside of the substrate. This unintentional deposition can induce particles that can subsequently migrate to the top surface of the semiconductor substrate and cause particle defects. This bevel edge and backside deposition can also cause problems in downstream processing, including contamination of patterning (scanner) and development tools. Traditionally, removal of this bevel edge and backside deposition is accomplished by wet cleaning techniques. For spin-coated photoresist materials, this process, called edge bead removal (EBR), is accomplished by directing a solvent flow from above and below the bevel edge while the substrate is rotating. The same process can also be applied to soluble organotin oxide-based resists deposited by vapor deposition techniques.

[0088] The bevel edge and / or backside cleaning of the substrate can also be performed using a dry cleaning process. In some embodiments, the dry cleaning process uses water vapor and / or plasma with one or more of the following gases: HBr, HCl, HI, BCl3, SOCl2, Cl2, BBr3, H2, O2, PCl3, CH4, methanol, ammonia, formic acid, NF3, and HF. In some embodiments, the dry cleaning process can use the same chemistry as the dry development process described herein. For example, the bevel edge and backside cleaning can use a hydrogen halide development chemistry. In the backside and bevel edge cleaning process, the water vapor and / or plasma must be limited to only certain areas of the substrate to ensure that only the backside and bevel are removed, avoiding degradation of the film on the frontside of the substrate.

[0089] Process conditions may be optimized for bevel edge and backside cleaning. In some embodiments, higher temperatures, higher pressures, and / or higher reactant flow rates can increase the etch rate. Suitable process conditions for dry bevel edge and backside cleaning include reactant flow rates of 100-10,000 sccm (e.g., 500 sccm of HCl, HBr, HI, or H2 and Cl2 or Br2, BCl3, or H2), temperatures of 20-140°C (e.g., 80°C), pressures of 20-1,000 mTorr (e.g., 100 mTorr), plasma powers of 0-500 W at high frequency (e.g., 13.56 MHz), and times of 10-20 seconds, depending on the photoresist film, composition, and properties. These conditions are suitable for some processing reactors, such as the Kiyo etch tool available from Lam Research Corporation, Fremont, California; however, a wider range of process conditions may be applicable depending on the capabilities of the processing reactor.

[0090] Further discussion of bevel edges and backside cleaning is provided in publication PCT / US20 / 70187, filed June 25, 2020, and / or publication PCT / US20 / 39615, filed June 25, 2020, which are incorporated herein by reference for all purposes.

[0091] PR Rework : Alternatively, the dry cleaning operation can be extended to complete photoresist removal or photoresist "rework." Photoresist rework is the removal of applied EUV photoresist and preparing the semiconductor substrate for reapplication of photoresist, such as when the original photoresist is damaged or otherwise defective. Because photoresist rework must be performed without damaging the underlying semiconductor substrate, oxygen-based etches should be avoided. Alternatively, variations on halide-containing chemistries, such as those described herein, can be used. Photoresist rework operations can be applied at any stage of process 100. Thus, photoresist rework can be performed after photoresist deposition, bevel edge and backside cleaning, PAB processing, EUV exposure, PEB processing, or development. In some embodiments, photoresist rework can be performed non-selectively in exposed and unexposed regions of the photoresist, but can also be selective to underlying layers.

[0092] In some embodiments, the photoresist rework process uses water vapor and / or plasma with one or more of the following gases: HBr, HCl, HI, BCl3, Cl2, BBr3, H2, PCl3, CH4, methanol, ammonia, formic acid, NF3, and HF. In some embodiments, the photoresist rework process can use the same chemistry as the dry development process described herein. For example, the photoresist rework can use a hydrogen halide development chemistry.

[0093] Process conditions may be optimized for photoresist rework. In some embodiments, higher temperatures, higher pressures, and / or higher reactant flow rates can increase the etch rate. Suitable process conditions for photoresist rework include reactant flow rates of 100-500 sccm (e.g., 500 sccm of HCl, HBr, HI, BCl3 or H2 and Cl2 or Br2), temperatures of 20-140°C (e.g., 80°C), pressures of 20-1000 mTorr (e.g., 300 mTorr), plasma powers of 300-800 W (e.g., 500 W) at high frequency (e.g., 13.56 MHz), and voltages of 0-200 V. b Conditions sufficient to completely remove EUV photoresist include a wafer bias of 1000 Å (higher biases are used with harder underlying substrate materials) and a time of 20 seconds to 3 minutes, which depend on the photoresist film, composition, and properties. These conditions are suitable for some processing reactors, such as the Kiyo etch tool available from Lam Research Corporation, Fremont, California, but a wider range of process conditions may be applicable depending on the capabilities of the processing reactor.

[0094] Further discussion of bevel edges and backside cleaning or PR rework is set forth in publication PCT / US20 / 39615, filed June 25, 2020, which is incorporated herein by reference for all purposes.

[0095] PAB / Soft Bake: Photolithography processes typically include one or more bake steps to promote the chemical reactions necessary to create chemical contrast between exposed and unexposed areas of the photoresist. For high volume manufacturing (HVM), such bake steps are typically performed on a track, where wafers are baked on a hotplate at a preset temperature in air or, in some cases, under a stream of N2. During these bake steps, more careful control of the bake atmosphere and the introduction of additional reactive gas components into the atmosphere can further reduce dose and / or improve pattern fidelity.

[0096] According to various aspects of the present disclosure, one or more post-treatments of metal and / or metal oxide-based photoresists after deposition (e.g., post-apply bake (PAB)) and / or after exposure (e.g., post-exposure bake (PEB)) can increase the difference in material properties between exposed and unexposed photoresists, thereby reducing dose-to-size (DtS), improving PR profiles, and improving line edge and line width roughness (LER / LWR) after subsequent dry development. The PAB treatment can include a combination of thermal treatment, chemical exposure, and moisture to increase the EUV sensitivity of the EUV-patternable film, reducing the EUV dose and developing a pattern in the EUV-patternable film. The PAB treatment temperature can be adjusted and optimized to increase the sensitivity of the EUV-patternable film. For example, the treatment temperature can be between about 90°C and about 200°C or between about 150°C and about 190°C. In some embodiments, the PAB treatment can be performed at a pressure between atmospheric pressure and vacuum for a treatment time of about 1 to 15 minutes, e.g., about 2 minutes. In some embodiments, the PAB treatment can be performed at a temperature between about 100°C and 200°C for about 1 to 2 minutes.

[0097] In block 108 of process 100, the metal-containing EUV resist film is exposed to EUV radiation to develop a pattern. Generally, exposure to EUV changes the chemical composition and cross-linking of the metal-containing EUV resist film, providing etch selectivity contrast for subsequent development.

[0098] The metal-containing EUV resist film is then patterned by exposing a region of the film to EUV light, typically under relatively high vacuum. EUV devices and imaging methods useful herein include those known in the art. In particular, as described above, exposed regions of the film are formed as regions with altered physical and chemical properties relative to unexposed regions due to EUV patterning. For example, in the exposed regions, cleavage of metal-carbon bonds can occur via β-hydride elimination, resulting in reactive, accessible metal hydride functionality that can be converted to hydroxide and bridged metal oxide moieties via metal-oxygen bridges during a subsequent post-exposure bake (PEB) step. This process can be used to create chemical contrast for development as a negative-tone resist. Generally, a higher number of β-H groups in the alkyl group results in a more sensitive film. This can also be explained as more branched and weaker Sn-C bonds. After exposure, the metal-containing EUV resist film can be baked to induce further crosslinking of the metal oxide film. The difference in properties between the exposed and unexposed regions can be exploited in subsequent processing, such as to dissolve the unexposed regions or to deposit material onto the exposed regions. For example, the pattern can be developed using dry processes to form a metal oxide-containing mask.

[0099] In particular, in various embodiments, hydrocarbon-terminated tin oxide present on the surface is converted to hydrogen-terminated tin oxide in the exposed regions of the imaging layer, particularly when the exposure is performed in a vacuum using EUV. However, removal of the exposed imaging layer from vacuum to air or the controlled introduction of oxygen, ozone, HO, or water can oxidize the surface Sn—H to Sn—OH. The difference in properties between the exposed and unexposed regions can be exploited in subsequent processing, for example, by reacting the irradiated regions, the unirradiated regions, or both, with one or more reagents to selectively add or remove material from the imaging layer.

[0100] Although the mechanism, function, or utility of the present technology is not limited, for example, 10 mJ / cm 2 ~100mJ / cm 2 EUV exposure at a dose of 1000 s leads to the cleavage of Sn-C bonds and loss of alkyl substituents, which relieves steric hindrance and leads to the collapse of low-density films. Furthermore, reactive metal-H bonds generated in the β-hydride elimination reaction react with neighboring active groups, such as hydroxyls, in the film, leading to further crosslinking and densification, and creating a chemical contrast between exposed and unexposed regions.

[0101] After exposing the metal-containing EUV resist film to EUV light, a photopatterned metal-containing EUV resist is obtained, which includes EUV-exposed areas and non-exposed areas.

[0102] In some embodiments, a post-exposure bake (PEB) is performed to further increase the contrast in etch selectivity of the photopatterned metal-containing EUV resist. The photopatterned metal-containing EUV resist may be thermally treated in the presence of various chemical species to promote crosslinking of the EUV-exposed regions, or simply baked on a hotplate in air, for example, at 150°C-250°C for 1-5 minutes (e.g., 190°C for 2 minutes).

[0103] In various embodiments, the bake process involves carefully controlling the bake environment, the introduction of reactive gases, and / or the ramp rate of the bake temperature. Examples of useful reactive gases include air, HO, HO, water vapor, CO, CO, O, O, CH, CHOH, N, H, NH, NO, NO, alcohol, acetylacetone, formic acid, Ar, He, or mixtures thereof. The PEB process (1) completely evaporates organic fragments generated during EUV exposure, (2) oxidizes Sn-H, Sn-Sn, or Sn radical species generated by EUV exposure to metal hydroxides, and (3) promotes cross-linking between adjacent Sn-OH groups to form a more densely cross-linked SnO-like network. The bake temperature is carefully selected to achieve optimal performance in EUV lithography. A PEB temperature that is too low results in insufficient cross-linking, resulting in low chemical contrast during development at a given dose. Furthermore, excessively high PEB temperatures can have adverse effects, such as severe oxidation and film shrinkage in unexposed regions (in this example, regions removed by development of the patterned film to form the mask), as well as undesirable interdiffusion at the interface between the photopatterned metal-containing EUV resist and the underlying layer, all of which contribute to a loss of chemical contrast and an increase in the density of defects due to insoluble scum. The PEB treatment temperature can be between about 100°C and about 300°C, between about 170°C and about 290°C, or between about 200°C and about 240°C. In some embodiments, the PEB treatment can be performed at a pressure between atmospheric and vacuum, and for a treatment time of about 1 minute to 15 minutes, e.g., about 2 minutes. In some embodiments, the PEB thermal treatment can be repeated to further enhance etch selectivity.

[0104] Additionally, the bake temperature ramp rate in either the PAB or PEB process is also a useful process parameter that can be manipulated to fine-tune the crosslinking / etch selectivity results. Alternatively, the PAB and PEB thermal treatments can be performed in a single run or multiple runs, using different process conditions such as ambient gas or mixture, temperature, and pressure for each run, to adjust the PR characteristics and, consequently, different etch selectivities.

[0105] In alternative embodiments, either or both of the post-apply and post-exposure treatments may include a remote plasma process in addition to or instead of a thermal treatment to generate radicals to react with the metal-containing photoresist and modify its material properties. In such implementations, the radicals may be generated from the same or different gas species.

[0106] In various embodiments, the treatment performed on the metal-containing photoresist to modify its material properties precedes and follows treatment of exposing the metal-containing photoresist to EUV lithography (e.g., PAB and PEB). Further discussion of PAB and PEB operations is found in U.S. patent application Ser. No. 62 / 970,020, filed February 4, 2020, and publication PCT / US20 / 70171, filed June 24, 2020, which publications are incorporated herein by reference for all purposes.

[0107] EUV scanner: Extreme ultraviolet (EUV) lithography can extend lithography techniques beyond their optical limits by moving to smaller image source wavelengths than achievable with current photolithography methods, enabling the patterning of features with small critical dimensions. EUV sources with wavelengths of approximately 13.5 nm can be used in cutting-edge lithography tools, also known as scanners. EUV radiation is strongly absorbed by a wide range of solid and fluid materials, including quartz and water vapor, and therefore operates in a vacuum.

[0108] The present technology also provides methods for patterning an imaging layer by exposing certain regions of the imaging layer to radiation, such as EUV, DUV, or an electron beam. Such patterning involves concentrating the radiation on one or more regions of the imaging layer. The exposure is typically performed so that the imaging layer film has one or more unexposed regions. The resulting imaging layer has multiple exposed and unexposed regions, resulting in a pattern consistent with the creation of transistors or other features of a semiconductor device formed by the addition or removal of material from the substrate during subsequent substrate processing. EUV, DUV, and electron beam radiation methods and radiation devices useful herein include those known in the art.

[0109] This specification discloses a vacuum-integrated metal hardmask process and associated vacuum-integrated hardware that combines film formation (deposition / condensation) with optical lithography, resulting in significantly improved Extreme Ultraviolet Lithography (EUVL) performance (e.g., reduced line edge roughness).

[0110] In various embodiments herein, a deposition process such as condensation (e.g., ALD or MOCVD performed in a PECVD tool such as a Lam Vector®) can be used to form a thin film of a metal-containing film (e.g., a photosensitive metal salt or a metal-containing organic compound (organometallic compound)) that is highly absorbing in EUV (e.g., wavelengths of about 10-20 nm), for example, at the wavelength of an EUVL light source (e.g., 13.5 nm = 91.8 eV). This film photolyzes upon EUV exposure to form a metal mask that serves as a pattern transfer layer for subsequent etching (e.g., in a conductor etching tool such as a Lam 2300® Kiyo®).

[0111] Following deposition, the EUV-patternable thin film is exposed to a beam of EUV light, typically under a relatively high vacuum, to form a pattern. For EUV exposure, the metal-containing film may be deposited in a chamber integrated with the lithography platform (e.g., a wafer stepper such as the TWINSCAN NXE:3300B platform offered by ASML, Veldhoven, The Netherlands) and transferred under vacuum to prevent reaction prior to exposure. EUVL also requires significant reduced pressure with strong optical absorption of incident photons by ambient gases such as HO and O, facilitating integration with lithography tools. In other embodiments, photosensitive metal film deposition and EUV exposure may be performed in the same chamber.

[0112] It should be noted that while this disclosure refers to EUVL as the primary patterning technique, in alternative embodiments, patterns can be written directly onto a blanket mask using a focused beam of electrons, ions, or neutral species. These processes are also performed in vacuum. In the event that by-products condense on the reflective optics of the EUVL system, in situ chamber cleaning may be used.

[0113] In particular, as discussed above, EUV patterning creates regions of the film with altered physical and chemical properties relative to unexposed regions. For example, in exposed regions, metal-carbon bonds can be cleaved by β-hydride elimination, resulting in metal-oxygen bridges that create reactive and accessible metal hydride functionality that can be converted to hydroxide and bridged metal oxide moieties. This creates chemical contrast for use as a template for negative resists or hard masks. In general, the greater the number of β-H groups in the alkyl group, the more sensitive the film. After exposure, the film can be baked to further crosslink the metal oxide film.

[0114] Although the mechanism, function, or utility of the present technology is not limited, for example, 10 mJ / cm 2 ~100mJ / cm 2EUV exposure at doses of 1000 nm can relieve steric hindrance, creating spaces for the collapse of low-density films. Furthermore, reactive metal-H bonds generated in β-hydride elimination reactions can react with neighboring active groups, such as hydroxyls, in the film, leading to further crosslinking and densification, creating chemical contrast between exposed and unexposed regions.

[0115] The vacuum integration of the film deposition and lithography process and equipment described herein provides for the deposition of EUV-sensitive metal films and their subsequent patterning by direct EUV exposure, which occurs in a vacuum environment to avoid decomposition or alteration. EUVL is performed in a vacuum to avoid alteration of the incident 13.5 nm light flux due to light absorption by ambient gases. The advantages of the described vacuum-integrated hard mask process include the vacuum operation of the EUV system, which opens up the possibility of using oxygen- and humidity-sensitive compounds, and the use of these materials is made possible by the vacuum integration of the deposition and EUV systems. Photodecomposition of metal precursors creates a nonlinear reaction, and photodecomposition is enhanced by increased adsorption of the metal film. Metals exhibit better thermalization of high-energy secondary electrons than photoresists, thereby enhancing contrast or LER. Using metal films as a direct mask or with pattern amplification allows for the formation of much thinner films and reduces the required exposure time. Metal films are more desirable hard masks for etching, reducing the required thickness in terms of masking. Additionally, further development and optimization of materials compatible with EUV vacuum and optics, organometallic precursors with suitable dose thresholds for metal deposition, and nucleation films with multiple photolysis events to remove spatially defined nucleation sites can proceed according to the processes described herein.

[0116] Further discussion regarding the operation of lithographic exposure is provided in U.S. patent application Ser. No. 14 / 610,038, filed Jan. 30, 2015, which is incorporated herein by reference for all purposes.

[0117] Post-exposure bake: As noted above, photolithography processes typically include one or more bake steps to promote the chemical reactions necessary to create chemical contrast between exposed and unexposed areas of the photoresist. The bake can be performed after deposition of the imaging layer / before EUV exposure (e.g., post-apply bake (PAB)) and / or after EUV exposure (e.g., post-exposure bake (PEB)).

[0118] In various embodiments, the bake method involves careful control of the bake environment, introduction of reactive gases, and / or careful control of the bake temperature ramp rate. In some embodiments, the PEB method described above may be used. Such methods are particularly useful for metal oxide-based EUV photoresists (PRs).

[0119] In a typical EUV lithography workflow, spin-on metal oxide resist materials typically undergo two bake steps: 1) a post-resist application bake to evaporate any residual solvent absorbed into the film, and 2) a post-EUV exposure bake. The second bake, commonly referred to as PEB, is designed to serve multiple purposes: 1) completely evaporate organic fragments generated during EUV exposure; 2) oxidize metal hydride species (another product of the β-H elimination reaction during EUV exposure) to metal hydroxides; and 3) promote cross-linking between adjacent -OH groups to form a cross-linked metal oxide network. The bake temperature is carefully selected to achieve optimal EUV lithography performance. A PEB temperature that is too low can result in insufficient removal of organic fragments and insufficient cross-linking, resulting in low chemical contrast during development at a given dose. Also, excessively high PEB temperatures can have adverse effects, such as severe oxidation and film shrinkage in unexposed areas (in this example, areas that will be removed by developing the patterned film to form the mask), as well as undesirable interdiffusion at the interface between the PR and the underlying layer, all of which contribute to a loss of chemical contrast and an increase in density defects due to insoluble scum. Since only the bake temperature and bake time can be controlled, tunability and process window are often very limited.

[0120] As described herein, careful control of the bake environment and introduction of reactive gas species during the PEB process allows for additional chemical control to fine-tune the crosslinking process. The ability to tailor the kinetics of crosslinking behavior in PR materials can minimize interdiffusion and other related defect formation mechanisms, providing a wide process window that allows for further optimization of lithographic performance. Furthermore, control of the bake temperature ramp rate and pressure (subatmospheric) are also useful process parameters that can be manipulated to fine-tune the crosslinking process.

[0121] Further discussion of PAB and PEB operations is set forth in U.S. patent application Ser. No. 62 / 970,020, filed February 4, 2020, and publication PCT / US20 / 70171, filed June 24, 2020, which are incorporated herein by reference for all purposes.

[0122] Pattern development after EUV exposure: After EUV exposure and, optionally, PEB, the selectivity between the exposed and unexposed regions of the imaging layer can be exploited by dry development, wet development, or area-selective ALD. For example, a dry or wet development process can be used to remove the unexposed regions while leaving the exposed regions. Processing of the imaging layer after EUV exposure depends on the substrate material and the desired characteristics of the semiconductor device to be formed using the substrate. For example, features can be formed on the substrate by various lithographic techniques, such as by making either the exposed (positive tone) or unexposed (negative tone) regions of the film selectively soluble in dry or liquid developers, as defined by a patterned exposure tool.

[0123] Dry development offers the potential for improved performance (e.g., preventing line collapse due to surface tension in wet development) and enhanced throughput (e.g., avoiding the use of wet development tracks). Other potential advantages of dry development and / or all-dry processing include the elimination of organic solvent developers, reduced sensitivity to adhesion issues, increased EUV absorption for improved dose efficiency, and no solubility-based limitations.

[0124] EUV photoresist dry development: As described above, EUV patterning results in exposed regions of a film with altered physical and chemical properties relative to unexposed regions. For example, in exposed regions, metal-carbon bonds can be cleaved by β-hydride elimination, resulting in metal-oxygen bridges that generate reactive and accessible metal hydride functionality that can be converted to hydroxide and bridged metal oxide moieties. This creates chemical contrast for use as a negative resist or hard mask template. In general, the greater the number of β-H groups in the alkyl group, the more sensitive the film. After exposure, the film can be baked to further crosslink the metal oxide film.

[0125] The difference in properties between the exposed and unexposed regions can be exploited in subsequent processing to dissolve the unexposed regions or deposit material onto the exposed regions. For example, the pattern can be developed using a dry process to form a metal oxide-containing mask. Methods and apparatus useful in such processes are described in publications PCT / US2019 / 067540, filed December 19, 2019; PCT / US20 / 39615, filed June 25, 2020; and U.S. patent application Ser. No. 62 / 912,330, filed October 8, 2019, which are incorporated herein by reference for their method and apparatus disclosures.

[0126] In a thermal development process, the photopatterned metal-containing EUV resist is exposed to a development chemistry at an optimal temperature in terms of etch selectivity between exposed and unexposed regions. Lower temperatures can result in higher etch selectivity contrast, while higher temperatures can result in lower etch selectivity contrast. In some embodiments, the temperature can be between about −60° C. and about 120° C., between about −20° C. and about 60° C., or between about −20° C. and about 20° C., e.g., about −10° C. The chamber pressure can be adjustable and can affect the etch selectivity between exposed and unexposed regions during development. In some embodiments, the chamber pressure is relatively low and no dilution is involved, and the chamber pressure may be between about 0.1 mTorr (about 13.3322 mPa) and about 300 mTorr (about 39996.7 mPa), between about 0.2 mTorr (about 26.6645 mPa) and about 100 mTorr (about 13332.2 mPa), or between about 0.5 mTorr (about 66.6612 mPa) and about 50 mTorr (6666.12 mPa). In some embodiments, the chamber pressure can be between about 20 mTorr (about 2666.45 mPa) and about 800 mTorr (about 106658 mPa), or between about 20 mTorr (about 2666.45 mPa) and about 500 mTorr (about 66661.2 Pa), for example, about 300 mTorr (about 3999.67 mPa). In some embodiments, the chamber pressure can be relatively high with high flow rate and dilution, and the chamber pressure can be between about 100 Torr (about 13332.2 Pa) and about 760 Torr (about 101325 Pa), or between about 200 Torr (26664.5 Pa) and about 760 Torr (about 101325 Pa). The flow rates of the reactants can be adjusted, and the flow rates of the reactants can affect the etch selectivity between exposed and unexposed regions during development. In some embodiments, the reactant flow can be between about 50 sccm and about 2000 sccm, between about 100 sccm and about 2000 sccm, or between about 100 sccm and about 1000 sccm, for example, about 500 sccm. For high flow rates, the reactant flow rate can be between about 1 L and about 10 L. The exposure duration can be adjusted in the thermal development process.The duration of exposure can depend on the amount of resist desired to be removed, the development chemistry, the amount of cross-linking in the resist, the composition and properties of the resist, etc. In some embodiments, the duration of exposure can be between about 5 seconds and about 5 minutes, between about 10 seconds and about 3 minutes, or between about 10 seconds and about 1 minute.

[0127] In a thermal development process, the photopatterned metal-containing EUV resist may be subjected to a specific halide-containing chemical reaction in the gas or liquid phase. In some embodiments, the development chemistry comprises hydrogen halides, hydrogen and halogen gas, boron trichloride, organic halides, acyl halides, carbonyl halides, thionyl halides, or mixtures thereof. Hydrogen halides can include, but are not limited to, HF, HCl, HBr, HI, etc. For example, the hydrogen halide can be HCl or HBr. Hydrogen and halogen gases can include, but are not limited to, hydrogen gas (H2) mixed with F2, Cl2, Br2, or I2. Boron trichloride (BCl3) can be used in combination with any of the aforementioned hydrogen halides or hydrogen and halogen gases. Organic halides include C x H y F z ,C x H y Cl z ,C x H y Br z , and C x H y I z(x, y, z are values ​​greater than or equal to 0). Acyl halides can include, but are not limited to, CH3COF, CH3COCl, CH3COBr, and CH3COI. Carbonyl halides can include, but are not limited to, COF2, COCl2, COBr2, and COI2. Thionyl halides can include, but are not limited to, SOF2, SOCl2, SoBr2, and SOI2. In some embodiments, halide-containing chemical reactions can be carried out with or without inert / carrier gases such as He, Ne, Ar, Xe, and N2.

[0128] The thermal development process may be performed without the use of plasma. By applying a non-plasma thermal approach, multiple wafers can be developed simultaneously in a batch in a low-cost thermal vacuum chamber / oven, significantly increasing productivity. However, in some embodiments, the thermal development process may be followed by exposure to plasma. Subsequent exposure to plasma may be performed for desorption, descumming, smoothing, or other processing operations.

[0129] In a plasma development process, the photopatterned metal-containing EUV resist is exposed to a development chemistry containing radicals / ions of one or more gases. The process chamber for semiconductor substrate processing may be a plasma generation chamber or may be coupled to a plasma generation chamber separate from the process chamber. In some embodiments, dry development may be performed by a remote plasma. The plasma generation chamber may be an inductively coupled plasma (ICP) reactor, a transformer coupled plasma (TCP) reactor, or a capacitively coupled plasma (CCP) reactor, using equipment and techniques known in the art. An electromagnetic field acts on one or more gases to generate plasma within the plasma generation chamber. Ions and / or radicals from the remote plasma may interact with the photopatterned metal-containing EUV resist. In some embodiments, a vacuum line is coupled to the process chamber for pressure control, and a development chemistry line is coupled to the plasma generation chamber to enable delivery of one or more gases into the plasma generation chamber. The process chamber may include one or more heaters for temperature control, such as a heater coupled to a substrate support within the process chamber for substrate temperature control. In some embodiments, the interior of the process chamber may be coated with a corrosion-resistant film, such as an organic polymer or an inorganic coating. One such coating is polytetrafluoroethylene (PTFE), e.g., Teflon® 1M. Such materials can be used in the thermal processes of the present disclosure without risk of removal by plasma exposure.

[0130] In the plasma development process, the photopatterned metal-containing EUV resist is exposed to a remote plasma under conditions optimized for etch selectivity between exposed and unexposed regions. These conditions can be optimized for the generation of a gentle plasma, which can be achieved by high pressure and low power. The chamber pressure can be adjustable and can affect the etch selectivity between exposed and unexposed regions during development. In some embodiments, the chamber pressure can be about 5 mTorr (about 666.612 mPa) or greater, or about 15 mTorr (about 1999.84 mPa) or greater. In some embodiments, the chamber pressure can be relatively high with high flow and dilution, and the chamber pressure can be between about 100 Torr (about 13332.2 Pa) and about 760 Torr (about 101325 Pa), or between about 200 Torr (about 26664.5 Pa) and about 760 Torr (about 101325 Pa). The RF power level can be adjusted, and the RF power can affect etch selectivity, roughness, scum removal, and other development characteristics. In some embodiments, the RF power can be about 1000 W or less, about 800 W or less, or about 500 W or less. The temperature can be adjusted, and the temperature can affect various aspects of development, such as etch selectivity. In some embodiments, the temperature can be between about −60° C. and about 300° C., between about 0° C. and about 300° C., or between about 30° C. and about 120° C. The gas flow rate can be adjusted, and the gas flow rate can affect the etch selectivity between exposed and unexposed regions during development. In some embodiments, the gas flow rate can be between about 50 sccm and about 2000 sccm, between about 100 sccm and about 2000 sccm, or between about 200 sccm and about 1000 sccm, such as about 500 sccm. The exposure duration can be adjusted in the plasma development process. The exposure duration can depend on the amount of resist desired to be removed, the development chemistry, the amount of cross-linking in the resist, the composition and properties of the resist, and other factors, hi some embodiments, the exposure duration can be between about 1 second and about 50 minutes, between about 3 seconds and about 20 minutes, or between about 10 seconds and about 6 minutes.

[0131] In a plasma development process, the photopatterned metal-containing EUV resist may be exposed to radicals of a specific halide-containing gas. In some embodiments, the radicals are generated from a remote plasma source. For example, in plasma development, the photopatterned metal-containing EUV resist may be exposed to radicals of a hydrogen-halide gas generated from a remote plasma source. In some embodiments, the halide-containing gas includes hydrogen halide, hydrogen-halogen gas, boron trichloride, organic halide, acyl halide, carbonyl halide, thionyl halide, or mixtures thereof. Hydrogen halides may include, but are not limited to, hydrogen fluoride (HF), hydrogen chloride (HCl), hydrogen bromide (HBr), and hydrogen iodide (HI). For example, the hydrogen halide may be HCl or HBr, and the hydrogen-halogen gas may include, but is not limited to, hydrogen gas (H2) mixed with fluorine gas (F2), chlorine gas (Cl2), bromine gas (Br2), or iodine gas (I2). Organic halides include, but are not limited to, C x H y F z ,C x H y Cl z ,C x H y Br z , and C x H y I z (x, y, z are values ​​equal to or greater than 0). Acyl halides can include, but are not limited to, CH3COF, CH3COCl, CH3COBr, and CH3COI. Carbonyl halides can include, but are not limited to, COF2, COCl2, COBr2, and COI2. Thionyl halides can include, but are not limited to, SOF2, SOCl2, SoBr2, and SOI2. In some embodiments, the halide-containing gas can be supplied with or without an inert / carrier gas such as He, Ne, Ar, Xe, and N2.

[0132] Descumming / Smoothing / Curing: In some cases, there may be scum (material in the open, unexposed areas of the EUV resist after development, e.g., clusters, likely to have a high metal concentration) or roughness (the same composition on the sidewalls of etched features in the developed pattern). Both of these problems are primarily due to a non-optimal Gaussian or stochastic distribution of light, resulting in partially or fully exposed material in areas where the resist should remain unexposed. The reverse can also occur.

[0133] The process conditions for the descumming and smoothing operations may be controlled during or after development. In some embodiments, the reactant flow rate may be between about 50 sccm and about 1000 sccm, or between about 100 sccm and about 500 sccm, e.g., about 500 sccm He. In some embodiments, the temperature may be between about -60°C and about 120°C, between about -20°C and about 60°C, or between about 20°C and about 40°C, e.g., about 20°C. In some embodiments, the chamber pressure can be between about 1 mTorr (about 133.322 mPa) and about 300 mTorr (about 39996.7 mPa), between about 5 mTorr (about 666.612 mPa) and about 100 mTorr (about 13332.2 mPa), between about 5 mTorr (about 666.612 mPa) and about 20 mTorr (about 2666.45 mPa), for example, about 10 mTorr (about 1333.22 mPa). Even with high ion energy, the plasma power can be relatively low. In some embodiments, the plasma power can be between about 50 W and about 1000 W, between about 100 W and about 500 W, or between about 100 W and about 300 W, for example, about 300 W. In some embodiments, the wafer bias can be between about 10 V and about 500 V, between about 50 V and about 300 V, for example, about 200 V. The plasma can be generated using a high RF frequency. In some embodiments, the RF frequency is 13.56 MHz. The exposure time to the inert gas plasma can be relatively short to avoid excessive exposure to ultraviolet light during the plasma exposure. In some embodiments, the exposure duration is between about 0.5 seconds and about 5 seconds, between about 1 second and about 3 seconds, for example, about 2 seconds.

[0134] He desorption scumming and cleaning of unexposed resist residue can have the additional benefit of hardening the exposed resist, thereby enhancing its hard mask function in subsequent operations to etch the underlying substrate. This resist hardening is achieved by exposing the EUV-exposed resist to UV generated by a He plasma and can continue after the bias is turned off and descumming / smoothing is complete. He plasma hardening may be performed instead if descumming / smoothing is not required or will not be performed.

[0135] In some embodiments, to improve results, He plasma scum removal / smoothing can be performed cyclically with dry development, as described above. In this way, for example, most of the organic components in the unexposed areas of the pattern can be removed by dry development, followed by a short He plasma run to remove some of the metal concentrated at the surface, providing access to the remaining underlying organic material, which can then be removed in the next dry development run / cycle. Another cycle of He plasma can be used to remove all residual metal, resulting in a clean, smooth feature surface. This cycle can be continued until all or substantially all of the residual scum and roughness has been removed, resulting in a clean, smooth feature surface.

[0136] In some embodiments, He desorption scumming and smoothing can be performed in conjunction with a wet development process. Wet development is known to have very high selectivity and exhibit clear on / off behavior. However, as a result, the wet development process cannot remove inadvertently partially or completely exposed areas. Such residues remain after the wet development process, resulting in scum formation and high line edge and line width roughness. Interestingly, in the dry development process, the etch rate and selectivity can be adjusted based on multiple control factors (e.g., time, temperature, pressure, gas / flow rate), so such an adjustable dry development process can also be applied to scum removal and smoothing of metal-containing resist lines by removing such partially exposed residues.

[0137] Device: Current EUV resist coating techniques typically use spin-on resists that are applied in an atmospheric environment, but this technique allows for the application of only one chemical mixture throughout the entire film stack, without the need for atmospheric control or influence.

[0138] The chamber, shown in Figures #AW and #AX below, incorporates a number of elements to enable dry deposition of EUV resist, including a four-zone electrostatic chuck for wafer substrate temperature control to + / - 0.5C, and a four-precursor water vapor delivery system plumbed to a dual plenum gas distribution plate.

[0139] In various embodiments, the chamber, gas distribution plate, and associated delivery piping are all heated to prevent condensation of any of the precursors.

[0140] Various embodiments also incorporate a gas box for supplying the necessary gas components to the chamber.

[0141] In various embodiments, the ESC is powered by RF power to enhance cleaning of the chamber.

[0142] In various embodiments, the gate valve and all internal chamber components are heated to prevent or minimize deposition other than on the wafer surface.

[0143] In various embodiments, a gas exclusion ring is used around the periphery of the wafer to prevent deposition on the backside and topside edge bevel.

[0144] The innovation in these designs is the combination of different technology elements into one chamber to achieve the desired deposition performance: wafer temperature uniformity, chemical gradient distribution via a gas distribution plate, deposition exclusion ring, and heated chamber surfaces all work together in various embodiments to achieve outstanding film properties.

[0145] In some embodiments, a dual plenum fractal (DPF) showerhead may be used during operation as described herein. The dual plenum fractal showerheads described herein may be configured to uniformly distribute process gases to a process volume above a semiconductor wafer in a semiconductor processing chamber. As a result, the entire surface of the wafer is generally exposed to such process gases simultaneously, unlike showerheads in which process gases flow from the center of the showerhead for a period of time and then from the periphery, which may promote more uniform wafer processing. Further details of DPF showerheads are described in U.S. Patent Application No. 62 / 914,616, entitled "DUAL PLENUM SHOWERHEAD," the disclosure of which, at least with respect to the configuration of the process chamber, is incorporated herein.

[0146] FIG. 4 is a schematic diagram of one embodiment of a process station 400 having a process chamber body 402 for maintaining a low-pressure environment suitable for the dry development, cleaning, rework, descumming, and smoothing implementations described above. Multiple process stations 400 may be included in a common low-pressure process tool environment. For example, FIG. 5 illustrates one embodiment of a multi-station processing tool 500, such as a VECTOR® processing tool available from Lam Research Corporation of Fremont, California. In some embodiments, one or more hardware parameters of the process stations 400, including those discussed in detail below, may be programmably adjusted by one or more computer controllers 450.

[0147] The process stations may be configured as modules in a cluster tool. Figure 7 illustrates a semiconductor process cluster tool configuration having a vacuum-integrated deposition and patterning module suitable for implementing embodiments described herein. Such a cluster process tool configuration may include resist deposition, resist exposure (EUV scanner), resist dry development, and etching modules, as described above and further below with reference to Figures 6 and 7.

[0148] In some embodiments, certain processing functions, such as dry developing and etching, can be performed sequentially in the same module.Embodiments of the present disclosure relate to methods and apparatus for receiving a wafer, including a photo-patterned thin EUV resist film disposed on a layer or stack to be etched, into a dry developing / etching chamber after photo-patterning in an EUV scanner, dry developing the photo-patterned thin EUV resist film, and then etching the underlying layer using the patterned EUV resist as a mask, as described herein.

[0149] 4, the process station 400 is in fluid communication with a reactant delivery system 401a for delivering process gases to a distribution showerhead 406. The reactant delivery system 401a optionally includes a mixing vessel 404 for mixing and / or conditioning process gases for delivery to the showerhead 406. One or more mixing vessel inlet valves 420 can control the introduction of process gases into the mixing vessel 404. If plasma exposure is performed, the plasma may be supplied to the showerhead 406 or may be generated in the process station 400. As mentioned above, in at least some embodiments, non-plasma thermal exposure is preferred.

[0150] 4 includes an optional vaporization point 403 for vaporizing a liquid reactant supplied to the mixing vessel 404. In some embodiments, a liquid flow controller (LFC) may be provided upstream of the vaporization point 403 to control the mass flow of the liquid for vaporization and delivery to the process station 400. For example, the LFC may include a thermal mass flow meter (MFM) located downstream of the LFC. A plunger valve of the LFC may be adjusted in response to a feedback control signal from a proportional-integral-derivative (PID) controller in electrical communication with the MFM.

[0151] 4, the substrate 412 is located below the showerhead 406 and rests on a pedestal 408. The showerhead 406 may have any suitable shape and may have ports for delivering process gases to the substrate 412, and the ports may be arranged in any suitable number and configuration.

[0152] In some embodiments, the pedestal 408 may be raised or lowered to expose the substrate 412 to the volume between the substrate 412 and the showerhead 406. In some embodiments, the height of the pedestal may be programmatically adjusted by a suitable computer controller 450.

[0153] In some embodiments, the pedestal 408 may be temperature controlled via a heater 410. In some embodiments, the pedestal 408 may be heated to temperatures above 0° C. up to 300° C. or higher, such as 50-120° C., e.g., about 65-80° C., during non-plasma thermal exposure of the photopatterned resist to dry development chemistries such as HBr, HCl, or BCl3, as described in the disclosed embodiments.

[0154] Additionally, in some embodiments, the pressure of the process station 400 may be controlled by a butterfly valve 418. As shown in the embodiment of Figure 4, the butterfly valve 418 throttles the vacuum provided from a downstream vacuum pump (not shown). However, in some embodiments, pressure control of the process station 400 may also be adjusted by varying the flow rate of one or more gases introduced to the process station 400.

[0155] In some embodiments, the position of the showerhead 406 can be adjusted relative to the pedestal 408 to vary the volume between the substrate 412 and the showerhead 406. Additionally, the vertical position of the pedestal 408 and / or the showerhead 406 can be varied by any suitable mechanism within the scope of the present disclosure. In some embodiments, the pedestal 408 can include a rotation axis for rotating the orientation of the substrate 412. In some embodiments, one or more of these exemplary adjustments can be performed programmatically by one or more suitable computer controllers 450.

[0156] Where plasma may be used, for example, in gentle plasma-based dry development embodiments and / or etching operations performed in the same chamber, the showerhead 406 and pedestal 408 are in electrical communication with a radio frequency (RF) power source 414 and matching network 416 for powering the plasma. In some embodiments, the plasma energy may be controlled by controlling one or more of the process station pressure, gas concentration, RF source power, RF source frequency, and plasma power pulse timing. For example, the RF power source 414 and matching network 416 may be operated at any suitable power to form a plasma having a desired radical species composition. An example of a suitable power is about 500 W or less.

[0157] In some embodiments, instructions to the controller 450 may be provided through input / output control (IOC) sequence instructions. As an example, instructions for setting conditions for a process phase may be included in a corresponding recipe phase of a process recipe. In some cases, the phases of a process recipe are arranged sequentially, with all instructions for a process phase being executed simultaneously with that process phase. In some embodiments, instructions for setting one or more reactor parameters may be included in a recipe phase. For example, a recipe phase may include instructions for setting the flow rate of a reactant gas, such as HBr or HCl, for a dry development chemistry, or instructions for a time delay for a recipe phase. In some embodiments, the controller 450 may include any of the features associated with the system controller 550 of FIG. 5, described below.

[0158] As noted above, a multi-station processing tool can include one or more process stations. FIG. 5 is a schematic diagram of one embodiment of a multi-station processing tool 500 having an inbound load lock 502 and an outbound load lock 504, either or both of which may include a remote plasma source. An atmospheric pressure robot 506 is configured to move wafers from a cassette loaded via a pod 508 to the inbound load lock 502 through an atmospheric port 510. The robot 506 places the wafer on a pedestal 512 in the inbound load lock 502, closes the atmospheric port 510, and pumps down the load lock. If the inbound load lock 502 includes a remote plasma source, the wafer can be subjected to a remote plasma treatment in the load lock for silicon nitride surface treatment before being introduced into the processing chamber 514. Additionally, the wafer may also be heated in the inbound load lock 502 to remove moisture and adsorbed gases, for example. The chamber transfer port 516 to the processing chamber 514 is then opened and another robot (not shown) places the wafer into the reactor on a pedestal in the first station shown in the reactor for processing. While the embodiment shown in Figure 5 includes a load lock, in some embodiments, the wafer can be fed directly into the process station.

[0159] The illustrated processing chamber 514 includes four process stations, numbered 1 through 4 in the embodiment shown in FIG. 5 . Each station has a heated pedestal (shown as 518 for station 1) and a gas line inlet. In some embodiments, each process station can have different or multiple purposes. For example, in some embodiments, a process station may be switchable between a dry development process mode and an etch process mode. Additionally, or alternatively, in some embodiments, the processing chamber 514 may include one or more matched pairs of dry development and etch process stations. While the illustrated processing chamber 514 includes four stations, a processing chamber according to the present disclosure may have any suitable number of stations. For example, in some embodiments, a processing chamber may have five or more stations, while in other embodiments, a processing chamber may have three or fewer stations.

[0160] FIG. 5 illustrates one embodiment of a wafer handling system 590 for transferring wafers within the processing chamber 514. In some embodiments, the wafer handling system 590 can transport wafers between various process stations and / or between process stations and load locks. Any suitable wafer handling system can be used. Non-limiting examples include a wafer carousel or a wafer handling robot. FIG. 5 also illustrates one embodiment of a system controller 550 used to control the process conditions and hardware status of the process tool 500. The system controller 550 can include one or more memory devices 556, one or more mass storage devices 554, and one or more processors 552. The processor 552 can include a CPU or computer, analog and / or digital input / output connections, a stepper motor control board, etc.

[0161] In some embodiments, the system controller 550 controls all activity of the process tool 500. The system controller 550 executes system control software 558 stored on mass storage device 554, loaded into memory device 556, and executed by processor 552. Alternatively, control logic may be hard-coded into the controller 550. For these applications, application-specific integrated circuits, programmable logic devices (e.g., field-programmable gate arrays or FPGAs), and the like may be used. In the following description, "software" or "code" may be substituted with functionally equivalent hard-coded logic. The system control software 558 may include instructions that control the timing, mixture of gases, gas flow rates, chamber and / or station pressure, chamber and / or station temperature, wafer temperature, target power levels, RF power levels, substrate pedestal, chuck and / or susceptor position, and other parameters of a particular process performed by the process tool 500. The system control software 558 may be configured in any suitable format. For example, various process tool component subroutines or controls may be written to control operation of the process tool components necessary to perform various process tool operations. System control software 558 may be coded in any suitable computer-readable programming language.

[0162] In some embodiments, the system control software 558 includes input / output control (IOC) sequence instructions for controlling the various parameters described above. In some embodiments, other computer software and / or programs stored on the mass storage device 554 and / or memory device 556 associated with the system controller 550 may be employed. Examples of such programs or portions of programs include a substrate positioning program, a process gas control program, a pressure control program, a heater control program, a plasma control program, etc.

[0163] The substrate positioning program may include program code for process tool components used to load the substrate onto the pedestal 518 and control the spacing between the substrate and other parts of the process tool 500 .

[0164] The process gas control program may include code for controlling various gas compositions (e.g., HBr or HCl gas as described herein) and flow rates, and optionally for flowing gases to one or more process stations prior to deposition to stabilize the pressure within the process station. The pressure control program may include code for controlling the pressure within the process station, for example, by regulating throttle valves in the exhaust systems of the process stations, gas flow rates to the process stations, etc.

[0165] The heater control program may include code for controlling current to a heater to heat the substrate, and may control the delivery of a heat carrier gas (such as helium) to the substrate.

[0166] The plasma control program may include code for setting RF power levels applied to process electrodes of one or more process stations according to embodiments herein.

[0167] The pressure control program may include code for maintaining pressure within a reaction chamber according to embodiments herein.

[0168] In some embodiments, there may be a user interface associated with the system controller 550. The user interface may include a display screen, a graphical software representation of equipment and / or process conditions, and user input devices such as a pointing device, keyboard, touch screen, microphone, etc.

[0169] In some embodiments, the parameters adjusted by the system controller 550 may relate to process conditions. Non-limiting examples include process gas composition and flow rates, temperature, pressure, plasma conditions (such as RF bias power levels), etc. These parameters may be provided to the user as a recipe or may be entered using a user interface.

[0170] Signals for monitoring the process may be provided from various process tool sensors through analog and / or digital input connections of the system controller 550. Signals for controlling the process may be output to analog and digital output connections of the process tool 500. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (such as vacuum gauges), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain process conditions.

[0171] The system controller 550 may provide program instructions for carrying out the deposition processes described above. The program instructions may control various process parameters such as DC power levels, RF bias power levels, pressure, temperature, etc. These instructions may control parameters for operating the dry development and / or etching processes according to various embodiments described herein.

[0172] The system controller 550 typically includes one or more memory devices and one or more processors configured to execute instructions to cause the devices to perform methods according to the disclosed embodiments. A machine-readable medium containing instructions for controlling process operations according to the disclosed embodiments may be coupled to the system controller 550.

[0173] In some implementations, the system controller 550 is part of a system that may be part of the examples described above. The system may include semiconductor processing equipment, including one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (such as a wafer pedestal, gas flow system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after semiconductor wafer or substrate processing. The electronics may also be referred to as a "controller" that allows control of various components or subparts of one or more systems. The system controller 550 may be programmed to control any of the processes disclosed herein, including process gas delivery, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and motion settings, wafer transfer into and out of tools and other transfer tools and / or load locks connected or interfaced to the particular system, depending on the processing conditions and / or type of system.

[0174] Generally, the system controller 550 can be defined as electronic equipment having various integrated circuits, logic, memory, and / or software to receive and issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips in firmware format that store program instructions, digital signal processors (DSPs), chips defined as application-specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions may be instructions communicated to the system controller 550 in the form of various individual settings (or program files) that define operational parameters for performing a particular process on or in connection with a semiconductor wafer or system. In some embodiments, the operational parameters may be part of a recipe defined by a process engineer to accomplish one or more processing steps during the fabrication of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.

[0175] In some implementations, the system controller 550 may be part of or coupled to a computer integrated or coupled with the system, or networked to the system, or a combination thereof. For example, the system controller 550 may perform wafer processing remotely in the “cloud” or as part of a fab host computer system. The computer may provide remote access to the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance metrics from multiple manufacturing operations, modify parameters of a current process, configure processing steps to follow a current process, or initiate a new process. In some examples, a remote computer (e.g., a server) can provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows entry or programming of parameters and / or settings, which are then communicated to the system from the remote computer. In some examples, the system controller 550 receives instructions in the form of data, which specify parameters for each of the processing steps to be performed during one or more operations. The parameters may be specific to the type of process being performed and the type of tool that the system controller 550 is configured to interface with or control. Thus, as noted above, the system controller 550 may be distributed, such as using one or more discrete controllers that are networked together and operate toward a common purpose, such as the processes and controls described herein. One example of a distributed controller for such purposes is one or more integrated circuits on the chamber that communicate with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer) and coupled to control the process on the chamber.

[0176] Non-limiting examples of systems may include a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a clean chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an ALD chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry development chamber or module, and any other semiconductor processing system related to or usable in the fabrication and / or manufacturing of semiconductor semiconductor wafers.

[0177] As noted above, depending on the process step or steps performed by the tool, the system controller 550 may communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport to bring containers of wafers to or from tool locations and / or loading ports in a semiconductor fabrication factory.

[0178] In the following, in certain embodiments, an inductively coupled plasma (ICP) reactor is described that may be suitable for etching operations suitable for implementation of some embodiments. Although an ICP reactor is described herein, in some embodiments, a capacitively coupled plasma reactor may also be used.

[0179] 6 shows a cross-sectional schematic of an inductively coupled plasma apparatus 600 suitable for performing certain embodiments or implementations, such as dry development and / or etching, such as a Kiyo® reactor manufactured by Lam Research Corporation of Fremont, Calif. In other embodiments, other tools or tool types capable of performing the dry development and / or etching processes described herein may be used in the implementation.

[0180] The inductively coupled plasma apparatus 600 includes an overall process chamber 624 structurally defined by a chamber wall 601 and a window 611. The chamber wall 601 can be made of stainless steel or aluminum. The window 611 can be made of quartz or other dielectric material. An optional internal plasma grid 650 divides the overall process chamber into an upper subchamber 602 and a lower subchamber 603. In most embodiments, the plasma grid 650 can be removed to allow access to the chamber space consisting of the subchambers 602 and 603. A chuck 617 is located within the lower subchamber 603 near the bottom inner surface. The chuck 617 is configured to receive and hold a semiconductor wafer 619 on which etching and deposition processes are performed. The chuck 617 can be an electrostatic chuck for supporting the wafer 619, when present. In some embodiments, an edge ring (not shown) surrounds the chuck 617 and has a top surface that is substantially planar with the upper surface of the wafer 619 when the wafer 619 is present on the chuck 617. The chuck 617 also includes an electrostatic electrode for chucking and dechucking the wafer 619. For this purpose, a filter and DC clamp power supply (not shown) may be provided. Other control systems may be provided for lifting the wafer 619 from the chuck 617. The chuck 617 can be charged using an RF power supply 623. The RF power supply 623 is connected to a matching network 621 via connection 627. The matching network 621 is connected to the chuck 617 via connection 625. In this manner, the RF power supply 623 is connected to the chuck 617. In various embodiments, the bias power of the electrostatic chuck is set to approximately 50 V or can be set to a different bias power depending on the process being performed in accordance with the disclosed embodiments. For example, the bias power can be between about 20V and about 100V, or between about 30V and about 150V.

[0181] The elements for plasma generation include a coil 633 positioned above the window 611. In some embodiments, a coil is not used in the disclosed embodiments. The coil 633 is made of a conductive material and includes at least one full turn. The example coil 633 shown in FIG. 6 includes three turns. A cross section of the coil 633 is indicated by symbols, with coils with an "x" having their turns extending into the page and coils with a "●" having their turns extending toward the page. The elements for plasma generation also include an RF power supply 641 configured to provide RF power to the coil 633. Typically, the RF power supply 641 is connected to a matching network 639 via connection 645. The matching network 639 is connected to the coil 633 via connection 643. In this manner, the RF power supply 641 is connected to the coil 633. An optional Faraday shield 649a is positioned between the coil 633 and the window 611. The Faraday shield 649a can be maintained at a distance from the coil 633. In some embodiments, the Faraday shield 649a is positioned immediately above the window 611. In some embodiments, the Faraday shield 649b is located between the window 611 and the chuck 617. In some embodiments, the Faraday shield 649b is not maintained at a distance from the coil 633. For example, the Faraday shield 649b can be immediately below the window 611 with no distance. The coil 633, the Faraday shield 649a, and the window 611 are each configured to be substantially parallel to one another. The Faraday shield 649a can prevent metals or other species from depositing on the window 611 of the process chamber 624.

[0182] Process gases can flow into the process chamber through one or more main gas inlets 660 and / or one or more side gas inlets 670 located in the upper subchamber 602. Similarly, although not shown, similar gas inlets can be used to supply process gases to a capacitively coupled plasma processing chamber. A vacuum pump (e.g., a single-stage or two-stage mechanical dry pump and / or a turbomolecular pump 640) can be used to evacuate the process gases from the process chamber 624 and maintain the pressure therein. For example, a vacuum pump can be used to evacuate the lower subchamber 603 during an ALD purge operation. A valve-controlled conduit fluidly connecting the vacuum pump to the process chamber 624 can be used to selectively control the application of the vacuum environment provided by the vacuum pump. This can be achieved using a closed-loop controlled flow restriction device, such as a throttle valve (not shown) or a pendulum valve (not shown), during plasma processing operations. Similarly, a vacuum pump and valve-controlled fluid connection to a capacitively coupled plasma processing chamber can also be used.

[0183] During operation of the apparatus 600, one or more process gases may be supplied through the gas inlet 660 and / or the gas inlet 670. In certain embodiments, process gases may be supplied only through the main gas inlet 660 or only through the side gas inlet 670. In some examples, the gas inlets shown in the figures may be replaced with more complex gas inlets, such as one or more showerheads. The Faraday shield 649a and / or the optional grid 650 may include internal passages and holes that allow delivery of process gases to the process chamber 624. Either or both of the Faraday shield 649a and the optional grid 650 may function as showerheads for delivery of process gases. In some embodiments, a liquid vaporization / delivery system may be installed upstream of the process chamber 624 so that once a liquid reactant or precursor is vaporized, the vaporized reactant or precursor is introduced into the process chamber 624 via the gas inlet 660 and / or the gas inlet 670.

[0184] Radio frequency power is supplied from RF power supply 641 to coil 633, causing RF current to flow through coil 633. The RF current flowing through coil 633 generates an electromagnetic field centered about coil 633. The electromagnetic field generates an induced current within upper subchamber 602. Physical and chemical interactions of the various generated ions and radicals with wafer 619 etch features on wafer 619 and selectively deposit layers on wafer 619.

[0185] If a plasma grid 650 is used such that both the upper subchamber 602 and the lower subchamber 603 are present, the induced current acts on the gas present in the upper subchamber 602 to generate an electron-ion plasma in the upper subchamber 602. The optional internal plasma grid 650 limits the amount of thermal electrons in the lower subchamber 603. In some embodiments, the apparatus 600 is designed and operated such that the plasma present in the lower subchamber 603 is an ion-ion plasma.

[0186] Both the upper electron-ion plasma and the lower ion-ion plasma contain positive and negative ions, but the ion-ion plasma has a greater ratio of negative ions to positive ions. Volatile etching and / or deposition byproducts can be removed from the lower subchamber 603 through port 622. The chuck 617 disclosed herein can operate at elevated temperatures ranging from about 10°C to about 250°C. The temperature depends on the process operation and the specific recipe.

[0187] The tool 600 may be coupled to equipment (not shown) when installed in a clean room or manufacturing facility. The equipment includes plumbing to provide process gases, vacuum, temperature control, and environmental particle control. These equipment will be coupled to the tool 600 when installed in the target manufacturing facility. The tool 600 may also be coupled to a transfer chamber that allows robotic equipment to transfer semiconductor wafers into and out of the tool 600 using conventional automation.

[0188] In some embodiments, a system controller 630 (which may include one or more physical or logical controllers) controls the operation of some or all of the process chamber 624. The system controller 630 may include one or more memory devices and one or more processors. In some embodiments, the apparatus 600 includes a switching system for controlling flow rates and durations when the disclosed embodiments are implemented. In some embodiments, the apparatus 600 may have a switching time of up to about 600 ms, or up to about 750 ms. The switching time may depend on the flow reaction, the selected recipe, the reactor configuration, and other factors.

[0189] In some implementations, the system controller 630 is part of a system that may be part of the examples described above. The system may include semiconductor processing equipment, including one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (such as a wafer pedestal, a gas flow system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after processing of semiconductor wafers or substrates. The electronics may be integrated into the system controller 630, which may control various parts or subcomponents of one or more systems. The system controller may be programmed to control any of the processes disclosed herein, including process gas delivery, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and motion settings, wafer transfer into and out of tools and other transfer tools and / or load locks connected or interfaced to the particular system, depending on the process parameters and / or type of system.

[0190] Generally, the system controller 630 can be defined as electronic equipment having various integrated circuits, logic, memory, and / or software to receive and issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips in firmware format that store program instructions, digital signal processors (DSPs), chips defined as application-specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions may be instructions communicated to the controller in the form of various individual settings (or program files) that define operational parameters for performing a particular process on or in connection with a semiconductor wafer or system. In some embodiments, the operational parameters may be part of a recipe defined by a process engineer to accomplish one or more processing steps during the fabrication or removal of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or die of a wafer.

[0191] In some implementations, the system controller 630 may be part of or coupled to a computer that is integrated with or connected to the system, or networked to the system, or a combination thereof. For example, the controller may perform wafer processing remotely in the “cloud” or as part of a fab host computer system. The computer may provide remote access to the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance metrics from multiple manufacturing operations, modify parameters of a current process, configure processing steps to follow a current process, or initiate a new process. In some examples, a remote computer (e.g., a server) can provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows entry or programming of parameters and / or settings, which are then communicated to the system from the remote computer. In some examples, the system controller 630 receives instructions in the form of data, which specify parameters for each of the processing steps to be performed during one or more operations. The parameters can be specific to the type of process being performed and the type of tool the controller is configured to interface with or control. Thus, as noted above, the system controller 630 may be distributed, such as using one or more discrete controllers that are networked together and operate toward a common purpose, such as the processes and controls described herein. One example of a distributed controller for such purposes is one or more integrated circuits on the chamber that communicate with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer) and coupled to control the process on the chamber.

[0192] Non-limiting examples of systems may include a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a clean chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an ALD chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry development chamber or module, and any other semiconductor processing system related to or usable in the fabrication and / or manufacturing of semiconductor semiconductor wafers.

[0193] As described above, depending on the process step or steps being performed by the tool, the controller may communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport to carry containers of wafers to or from tool locations and / or loading ports in a semiconductor fabrication factory.

[0194] EUVL patterning can be performed using any suitable tool, often referred to as a scanner, such as, for example, the TWINSCAN NXE:3300B® platform provided by ASML (Veldhoven, The Netherlands). The EUVL patterning tool can be a standalone device that loads and unloads substrates for deposition and etching as described herein. Alternatively, as described below, the EUVL patterning tool can be a module on a larger, multi-component tool. Figure 7 illustrates a semiconductor process cluster tool architecture with vacuum-integrated deposition, EUV patterning, and dry develop / etch modules interfaced with a vacuum transfer module, suitable for implementing the processes described herein. While the processes can be performed without such vacuum-integrated equipment, such equipment may be advantageous in some implementations.

[0195] 7 illustrates a semiconductor process cluster tool architecture having vacuum-integrated deposition and patterning modules interfaced with a vacuum transfer module suitable for implementing the processes described herein. The arrangement of transfer modules for "transferring" wafers between multiple containment facilities and processing modules may be referred to as a "cluster tool architecture" system. The deposition and patterning modules are vacuum-integrated according to the requirements of the particular process. Other modules, such as for etching, may also be included in the cluster.

[0196] A vacuum transfer module (VTM) 738 interfaces with four processing modules 720a-720d, which may be individually optimized to perform various manufacturing processes. By way of example, processing modules 720a-720d may be implemented to perform deposition, evaporation, ELD, dry develop, etch, strip, and / or other semiconductor processes. For example, module 720a may be an ALD reactor that can be operated to perform the non-plasma thermal atomic layer deposition described herein, such as a Vector tool available from Lam Research Corporation of Fremont, California. And module 720b may be a PECVD tool, such as a LAM Vector®. Note that the figures are not necessarily to scale.

[0197] Airlocks (also known as load locks or transfer modules) 742 and 746 interface with VTM 738 and patterning module 740. For example, as mentioned above, a suitable patterning module may be the TWINSCAN NXE:3300B® platform provided by ASML (Veldhoven, The Netherlands). This tool architecture allows workpieces, such as semiconductor substrates or wafers, to be transferred in a vacuum to prevent reaction prior to exposure. The fact that EUVL also requires significant reduced pressure with strong optical absorption of incident photons by ambient gases such as HO and O facilitates integration of the deposition module with the lithography tool.

[0198] As noted above, this integrated architecture is only one possible embodiment of a tool for implementing the described processes. These processes can also be implemented using more conventional standalone EUVL scanners and deposition reactors, such as a Lam Vector tool, either standalone or modularly integrated with other etch, strip, etc. tools (e.g., a Lam Kiyo or Gamma tool) in a cluster architecture, as described, for example, with reference to FIG. 7 (although without the integrated patterning module).

[0199] Airlock 742 may be an "outgoing" load lock, referring to the transfer of substrates from the VTM 738 that serves deposition module 720a to the patterning module 740, and airlock 746 may be an "incoming" load lock, referring to the transfer of substrates from the patterning module 740 to the VTM 738. The incoming load lock 746 may also provide an interface outside the tool for accessing and removing substrates. Each process module has a facet that interfaces the module with the VTM 738. For example, deposition process module 720a has facet 736. Within each facet, sensors are used to sense the passage of wafer 726 as it moves between stations, such as sensors 1-18 in the figure. Patterning module 740, airlocks 742, and 746 may similarly include additional facets and sensors not shown.

[0200] A main VTM robot 722 transfers wafers 726 between modules, including airlocks 742 and 746. In one embodiment, robot 722 has one arm, and in another embodiment, robot 722 has two arms. Each arm has an end effector 724 to pick up wafers, such as wafer 726, for transfer. A front-end robot 744 is used to transfer wafers 726 from the output airlock 742 to the patterning module 740 and from the patterning module 740 to the input airlock 746. The front-end robot 744 may also transfer wafers 726 between the input load lock and outside the substrate access and removal tool. The input airlock module 746 can accommodate environments between atmosphere and vacuum, allowing wafers 726 to move between the two pressure environments without damage.

[0201] It should be noted that EUVL tools typically operate at higher vacuums than deposition tools. In this case, it may be desirable to elevate the vacuum environment of the substrate during transfer from the deposition to the EUVL tool and degas the substrate before loading into the patterning tool. This function may be achieved by having the unload airlock 742 hold the transferred wafer at a pressure below the pressure of the patterning module 740 during the degassing process, to prevent contamination of the optics of the patterning tool 740 by outgassing from the substrate. A suitable pressure for the unload degassing airlock is 1E-8 Torr or less.

[0202] Figure 8 shows an alternative semiconductor process cluster tool architecture to Figure 7 without the patterning module 740. Instead, a front-end robot 832 in an atmospheric transfer module (ATM) 840 is used to transfer wafers 826 from front-opening unified pods (FOUPs) 834 or cassettes in a load port module (LPM) 842 to an airlock 830. A module center 828 in a process module 820 is one location for placing the wafer 826. An aligner 844 in the ATM 840 is used to align the wafer.

[0203] In the exemplary processing method, a wafer is placed into one of the FOUPs 834 in the LPM 842. The front-end robot 832 transports the wafer from the FOUP 834 to an aligner 844, which allows the wafer 826 to be properly centered before being etched or processed. After the wafer 826 is aligned, it is moved by the front-end robot 832 to the airlock 830. The airlock module can match the environment between the ATM and the VTM, allowing the wafer 826 to move between the two pressure environments without damage. The wafer 826 is moved by the robot 822 from the airlock module 830 through the VTM 838 to one of the process modules 820a-d. To accomplish this wafer movement, the robot 822 uses an end effector 824 on each arm. Once processed, the wafer 826 is moved by the robot 822 from process modules 820a-d to the airlock 830. From here, the wafer 826 can be moved by the front-end robot 832 to one of a plurality of FOUPs 834 or to an aligner 844 .

[0204] As described above, a multi-station processing tool can include one or more process stations. FIG. 9 is a schematic diagram of one embodiment of a multi-station processing tool 900 having an inbound load lock 902 and an outbound load lock 904, either or both of which may include a remote plasma source. An atmospheric pressure robot 906 is configured to move a substrate or wafer from a cassette loaded via a pod 908 to the inbound load lock 902 through an atmospheric port 910. The robot 906 places the substrate on a pedestal 912 in the inbound load lock 902, closes the atmospheric port 910, and pumps down the load lock. If the inbound load lock 902 includes a remote plasma source, the substrate can be subjected to remote plasma processing in the load lock before being introduced into the processing chambers 914A-C. The substrate may also be subjected to heating in the inbound load lock 902, for example, to remove moisture or adsorbed gases. The chamber transfer port 916 to one of the processing chambers 914A-C is then opened, and another robot (not shown) places the substrate in the reactor on a pedestal in the first station shown within the reactor for processing. While the embodiment shown in FIG. 9 includes a load lock, in some embodiments, the substrate may be delivered directly to the process station. In various embodiments, a soak gas is introduced into the station as the substrate is placed on the pedestal 912 by the robot 906.

[0205] The illustrated processing chamber 914B includes four process stations, numbered 1 through 4 in the embodiment shown in FIG. 9 . Each station has a heated pedestal (shown as 918 for station 1) and a gas line inlet. In some embodiments, each process station can have different or multiple purposes. For example, in some embodiments, a process station may be switchable between ALD and PEALD process modes. Additionally, or alternatively, in some embodiments, the processing chamber 914 may include one or more matched pairs of ALD and plasma-enhanced ALD process stations. While the illustrated processing chamber 914 includes four stations, a processing chamber according to the present disclosure may have any suitable number of stations. For example, in some embodiments, a processing chamber may have five or more stations, while in other embodiments, a processing chamber may have three or fewer stations. Also, while FIG. 5A shows a multi-station processing tool 900 with three process chambers, in some embodiments, a multi-station processing tool may have four process chambers, as shown in FIG. 9B . In some embodiments, the multi-station processing tool may have four or more process chambers, while in other embodiments, the multi-station processing tool may have one, two, or three process chambers.

[0206] FIG. 9 illustrates one embodiment of a wafer handling system 990 for transferring substrates within a processing chamber 914. In some embodiments, the wafer handling system 990 can transfer substrates between various process stations and / or between a process station and a load lock. Any suitable wafer handling system can be used. Non-limiting examples include a wafer carousel or a wafer handling robot. FIG. 9 also illustrates one embodiment of a system controller 950 used to control the process conditions and hardware status of the processing tool 900. The system controller 950 can include one or more memory devices 956, one or more mass storage devices 954, and one or more processors 952. The processor 952 can include a CPU or computer, analog and / or digital input / output connections, a stepper motor control board, etc. In some embodiments, the system controller 950 includes machine-readable instructions for performing operations such as those described herein.

[0207] In some embodiments, a system controller 950 controls the activities of the process tool 900. The system controller 950 executes system control software 958 stored on a mass storage device 954, loaded into a memory device 956, and executed by a processor 952. Alternatively, the control logic may be hard-coded into the system controller 950. For these applications, application-specific integrated circuits, programmable logic devices (e.g., field-programmable gate arrays or FPGAs), and the like may be used. In the following description, references to "software" or "code" may be substituted with functionally equivalent hard-coded logic. The system control software 958 may include instructions that control the timing, mixture of gases, gas flow rates, chamber and / or station pressure, chamber and / or station temperature, substrate temperature, target power levels, RF power levels, substrate pedestal, chuck and / or susceptor position, and other parameters of a particular process being performed by the process tool 900. The system control software 958 may be configured in any suitable format. For example, various process tool component subroutines or control objects may be written to control operation of the process tool components necessary to perform the operations of the various process tools. System control software 958 may be coded in any suitable computer-readable programming language.

[0208] In various embodiments, the chambers 914A-C can perform the same or different operations. Also, while three chambers 914A-C are shown, some embodiments may have four or more chambers or three or fewer chambers. In some embodiments, each of the chambers 914A-C may perform a dry deposition process to deposit a photolithographic layer. In some embodiments, one or more of the chambers 914A-C may be used for a dry deposition process, while a different one or more of the chambers 914A-C may be used for a dry development process described herein. In some embodiments, one chamber may be used for a dry deposition process, one chamber may be used for a PAB process, and one chamber may be used for a dry development process. In some embodiments, a chamber used for a PAB process may also be used for a PEB process, or alternatively, a PEB process. In an embodiment having four chambers, one chamber can be used for the dry deposition process, one chamber for the PAB process, one chamber for the PEB process, and one chamber for the dry development process. In some embodiments, variations in process time can be addressed by changing module ratios (e.g., if the PR deposition time is twice the PAB time, the tool can be configured with twice as many PR deposition modules as PAB modules).

[0209] In some embodiments, the multi-station processing tool 900 may include different modules in each chamber to facilitate the embodiments described herein. For example, a VECTOR® processing module may be used for deposition processes, and a KIYO® processing module may be used for PAB, PEB, and dry development processes. In some embodiments, there may be different numbers of each type of module. For example, there may be one VECTOR module and one or more KIYO modules.

[0210] In some embodiments, multiple operations may be implemented on different pedestals within the same module of the same tool. In some embodiments, the VECTOR module may be integrated into the same module as the KIYO module. For example, pedestals 1 and 3 of chamber 914 may be used for dry deposition processes, while pedestals 2 and 4 may be used for different processes, such as wafer cleaning, PAB, PEB, and dry development processes. A wafer may be processed on one pedestal to deposit a PR film, after which a robot may move the wafer to another pedestal within the chamber for subsequent processes, such as those described herein. In this way, maintaining vacuum and indexing wafers from pedestal to pedestal is faster than transporting wafers between process modules. This results in increased efficiency (throughput), controlled and minimized cross-contamination, and superior film properties without substantially sacrificing technical performance.

[0211] Furthermore, each station / pedestal can be configured or optimized for each operation, and pedestals can be separated from one another by other station-specific barriers, such as gas curtains or gas seals, to reduce or minimize cross-contamination / crosstalk between deposition, cleaning, baking, irradiating, or developing processes. Examples of these are described, for example, in U.S. Patent Application Publication Nos. 2015 / 0004798 and 2017 / 0101710, which are incorporated herein by reference for their disclosures in this regard. Each pedestal process can be set to a different temperature and pressure without departing from the scope of the invention. Additionally, the temperature of each station's pedestal, showerhead, wall, etc. can be independently optimized for each process and does not need to be cycled. Gas distribution can be separate for each station. Pressures can be maintained independently by adding multiple throttle valves. In some embodiments, the exhaust for each station can be localized rather than shared, maintaining independent exhaust without cross-mixing / contamination of gases.

[0212] In some embodiments, integrated operations may be performed on the same pedestal, for example, wafer cleaning and PAB / PEB operations may be performed on the same pedestal, which can improve throughput by reducing transfer or wait times between wafer cleaning and bake operations.

[0213] 10A-10E illustrate various embodiments for performing processing operations in different chambers within a tool, along with process flow charts. The process flow charts illustrate operations that can be performed on-tool or off-tool. In various embodiments, the operations illustrated in FIGS. 10A-10E may be the same as those described in FIG. 1 above (as indicated by the use of the same reference numerals). Although cleaning operations are not illustrated in FIGS. 10A-10E, in some embodiments, cleaning operations may be performed. As will be further described with reference to FIG. 1, some operations may not be performed. In the embodiment illustrated in FIG. 10A(i), each chamber in the cluster tool performs a dry deposition process as illustrated in the process flow of FIG. 10A(ii). Other operations in the lithography process, such as PAB, EUV exposure, PEB, and development processes, may be performed on different tools or clusters.

[0214] In the embodiment of Figure 10B(i), the dry deposition and dry development processes can be performed in a single tool, as shown in the process flow of Figure 10B(ii). In various embodiments, two chambers can be used for the dry deposition process, while the dry development process uses a single chamber. The other operations can be performed on different tools.

[0215] In the embodiment of FIG. 10C(i), dry deposition, PAB, and dry development are each performed in a single tool, as shown in the process flow of FIG. 10C(ii). In various embodiments, one chamber can be used for each process. In some embodiments, the substrate may have a wait time between processes. In some embodiments, the wait time may involve waiting outside the tool, for example, in a FOUP or other controlled environment. In other embodiments, the wafer may move directly from the dry EUV deposition chamber to the PAB chamber without a wait time, or may wait in either process chamber for the wait time. This can be advantageous for reducing wait time and / or maintaining vacuum, both of which can improve the quality of the resulting PR film.

[0216] In the embodiment of FIG. 10D(i), the dry deposition, PEB, and dry develop processes are performed in a single tool, as shown in the process flow of FIG. 10D(ii). In some embodiments, the PAB chamber and the PEB chamber may be the same chamber, while in other embodiments, they may be different chambers. As noted above, in some embodiments, the wait time may occur outside the tool in a controlled environment, and in other embodiments, the wafer may be transferred directly from the PEB chamber to the develop chamber. This can be advantageous for reducing wait time and / or maintaining vacuum, both of which can improve the quality of the resulting PR film.

[0217] In the embodiment of FIG. 10E(i), dry deposition, PAB, PEB, and dry develop are performed within a single tool, as shown in the process flow of FIG. 10E(ii). In some embodiments, radiation exposure may occur off-tool in a separate scanner chamber. As noted above, in some embodiments, the wait time may occur off-tool in a controlled environment, and in other embodiments, the substrate may be moved directly from the dry deposition chamber to the PAB chamber or from the PEB chamber to the dry develop chamber. In such embodiments, the wait time may occur on-tool. Moving the substrate between chambers on the same tool for different operations can be advantageous to reduce wait time and maintain vacuum / environment control.

[0218] In the embodiment of FIG. 10F(i), a scanner may be integrated with a deposition chamber and / or a wet or dry development chamber. An organometallic tin precursor ampoule 1000 and an EUV deposition module 1010 may be used to dry-deposit an EUV PR. An EUV exposure module 1020 may be used to expose portions of the EUV PR to radiation and chemically alter the exposed portions. An EUV development module 1030 may remove portions of the EUV PR using a wet or dry process, allowing the PR to be treated as a negative or positive resist. A pattern transfer module 1040 may then transfer the pattern of the EUV PR to an underlying layer, for example, by an etching process that forms lines based on the developed EUV PR pattern. In some embodiments, byproducts from various processing environments may be shared or may flow to a single or multiple exhaust abatement systems 1050. In some embodiments, the process flow shown in FIG. 10F(ii) may be performed in the tool shown in FIG. 10F(i).

[0219] In some embodiments, a system controller (which may include one or more physical or logical controllers) controls the operation of some or all of the cluster tool and / or its separate modules. The controller may be local to the cluster structure or may be located outside the cluster structure, either at the manufacturing site or at a remote location, and may be connected to the cluster structure via a network. The system controller may include one or more memory devices and one or more processors. The processor may include a central processing unit (CPU) or computer, analog and / or digital input / output connections, stepper motor control boards, and other similar components. Instructions for performing appropriate control operations are executed by the processor. These instructions may be stored in a memory device coupled to the controller or provided over a network. In certain embodiments, the system controller executes system control software.

[0220] The system control software may include instructions for controlling the application timing and / or magnitude of any aspect of tool or module operation. The system control software may be configured in any suitable format. For example, various process tool component subroutines or control objects may be written to control operation of the process tool components necessary to perform various process tool operations. The system control software may be coded in any suitable computer-readable programming language. In some embodiments, the system control software includes input / output control (IOC) sequencing instructions for controlling the various parameters described above. For example, each phase of a semiconductor manufacturing process may include one or more instructions for execution by the system controller. Instructions for setting process conditions for condensation, deposition, evaporation, patterning, and / or etching phases may be included in the corresponding recipe phase, for example.

[0221] In various embodiments, an apparatus for forming a negative pattern mask is provided. The apparatus can include process chambers for patterning, deposition, and etching, and a controller including instructions for forming the negative pattern mask. The instructions can include code for, in the process chamber, patterning features in a chemically amplified (CAR) resist on a semiconductor substrate by EUV exposure to expose a surface of the substrate, dry developing the photopatterned resist, and etching an underlying layer or stack using the patterned resist as a mask.

[0222] The controller that controls the movement of the wafers can be local to the cluster structure, or can be located outside the cluster structure, either at the manufacturing site or at a remote location, and connected to the cluster structure via a network. A controller such as that described above with reference to Figure 6 or Figure 7 can be implemented in any of Figures 4, 5, 6, 7, 8, 9, or 10A-10F, as well as the tool structures described in Figures 11, 12, and 13.

[0223] 11, 12, and 13A and 13B illustrate alternative processing tool structural configurations, such as may be implemented at least in part in EOS or Sens.i products available from Lam Research Corporation of Fremont, California, that may be used in some embodiments.

[0224] The multi-station processing tool 1100 illustrated in FIG. 11 may include an equipment front-end module (EFEM) for receiving substrates via any FOUP. As shown in FIG. 12, a cross-sectional view of the multi-station processing tool 1100, an EFEM robot 1204 can move substrates from the EFEM 1104 via a load port 1206. The substrates can be moved via one or more shuttles 1208, which can move the substrates on linear tracks 1214 or lifters 1212. The substrates can then be moved by a wafer handling robot 1210 to the process chambers 1108 (eight chambers are shown in FIG. 12 for a total of 16 process chambers in the multi-station processing tool 1100). Each process chamber can be switchable between various process modes as described herein.

[0225] 11 , the multi-station processing tool 1100 may also include a fluid delivery system (FDS) 1112 for delivering process gases and other fluids to each process chamber, along with FDS controls 1114. Fan filter units 1102 and 1106 may be used to ensure a clean environment in the process chambers and passageways, respectively. In some embodiments, a resist processing track such as those shown in FIGS. 11 and 12 may be used to perform wet development of dry-deposited EUV PR.

[0226] Figure 13A shows a top view of another multi-station processing tool 1300 having a robot 1304 configured to move wafers from a loaded cassette via a pod 1308. A second robot 1306 can move the wafer to one of various process chambers 1302 for performing the operations described herein. Figure 13B shows a side view of the multi-station processing tool 1300. Various embodiments described herein can be performed using a cluster architecture such as those shown in Figures 11, 12, and 13.

[0227] Conclusion: Although the foregoing embodiments have been described in detail for clarity of understanding, it will be apparent that certain changes and modifications are possible within the scope of the appended claims. The embodiments described herein can be practiced without some or all of the following specific components. In other instances, well-known process operations have not been described in detail to avoid unnecessarily obscuring the present disclosure. Furthermore, although the disclosed embodiments are described in connection with specific embodiments, the disclosed embodiments are not limited to such specific embodiments. It should be noted that there are many alternative ways of implementing the processes, systems, and apparatus of the present embodiments. Therefore, the present embodiments should be considered as illustrative and not restrictive, and are not limited to the details set forth herein. For example, the present disclosure can be realized in the following forms. [Form 1] An integrated lithography system comprising: a plurality of reaction chambers in a cluster, the plurality of reaction chambers comprising: photoresist (PR) deposition chamber; Post-apply bake (PAB) chamber; Post-exposure bake (PEB) chamber; a development chamber; and a controller including one or more processors and one or more memory devices; The one or more memory devices store computer-executable instructions that cause the one or more processors to: receiving a substrate within the PR deposition chamber; depositing PR on the surface of the substrate in the PR deposition chamber; receiving the substrate having the PR in the PAB chamber; treating the PR in the PAB chamber to modify material properties of the PR; receiving the substrate in the PEB chamber after processing the PR, wherein a portion of the PR has been chemically altered by exposure to radiation to create patterned PR; treating the patterned PR in the PEB chamber to modify material properties of the patterned PR; dry developing the patterned PR in the developing chamber to form a PR mask by removing either the exposed or unexposed portions of the patterned PR by a dry developing process including exposure to a compound; An integrated lithography system that controls the [Form 2] 2. The system of claim 1, wherein the PR is a metal-containing PR. [Form 3] 2. The system of claim 1, wherein the PR is EUV PR. [Form 4] 10. The system of claim 1, wherein the plurality of reaction chambers further includes a substrate cleaning chamber, and the computer-executable instructions further include, prior to the computer-executable instructions for receiving the substrate having the PR in the PAB chamber, causing the one or more processors to: receiving the substrate having the PR in the cleaning chamber; performing a dry cleaning process to remove PR from the bevel edge and / or backside of said substrate; The method further includes an instruction to control the [Form 5] 10. The system of claim 1, wherein the plurality of reaction chambers further comprises an underlayer deposition chamber, and the computer-executable instructions further cause the one or more processors to, prior to the computer-executable instructions for depositing a PR, depositing an underlayer on the surface of the substrate by a dry process, which increases the adhesion of the PR to the substrate; The system further includes instructions for controlling the [Form 6] 6. The system of claim 5, wherein the underlayer deposition chamber is the PR deposition chamber. [Form 7] 10. The system of claim 1, wherein the plurality of reaction chambers further comprises a pre-treatment chamber, and the computer-executable instructions further cause the one or more processors to, prior to the computer-executable instructions for depositing the PR: treating the surface of the substrate by a dry process to generate more chemical functional groups on the surface of the substrate to enhance PR adhesion to the substrate; The system further includes instructions for controlling the [Form 8] A system as described in form 1, wherein the computer-executable instructions further include instructions for controlling the one or more processors to perform a dry cleaning process to remove PR from the bevel edge and / or backside of the substrate in the PAB chamber. [Form 9] 10. The system of claim 1, wherein the plurality of reaction chambers further comprises a lithography scanner, and the computer-executable instructions further cause the one or more processors to, prior to receiving the substrate in the PEB chamber: receiving the substrate with the lithography scanner; exposing a portion of said PR to radiation to create a patterned PR; The system further includes instructions for controlling the [Form 10] 10. The system according to any one of claims 1 to 9, wherein each of the reaction chambers is at or below atmospheric pressure, and the PR remains at or below atmospheric pressure until the dry development process is completed. [Form 11] 10. A system as described in any one of claims 1 to 9, wherein the system controls the ambient environment of the substrate to reduce exposure of the photoresist to moisture before the patterned PR is dry developed. [Form 12] 10. The system of any one of claims 1 to 9, wherein the computer-executable instructions further comprise computer-executable instructions for depositing the PR by a dry process comprising mixing a water vapor flow of an organometallic precursor with a water vapor flow of a counter-reactant. [Form 13] 10. A system according to any one of aspects 1 to 9, wherein the processes carried out by the plurality of reaction chambers are all dry processes. [Form 14] 10. A system according to any one of claims 1 to 9, wherein the processes carried out by the plurality of reaction chambers include wet and dry processes. [Form 15] 10. The system of any one of claims 1 to 9, wherein the cluster comprises a plurality of PR deposition chambers. [Form 16] 10. The system according to any one of claims 1 to 9, wherein the PAB chamber and the PEB chamber are the same chamber. [Form 17] an integrated substrate processing system including a plurality of substrate processing environments; The plurality of substrate processing environments include: a metal-containing photoresist (PR) deposition environment; and A group consisting of: an additive metal-containing photoresist (PR) deposition environment; Metal-containing PR development environment; Heat treatment processing environment; one or more other separate integrated processing environments selected from: a controller including one or more processors and one or more memory devices; Including, The one or more memory devices include computer-executable instructions that cause the one or more processors to: receiving a substrate within said metal-containing PR deposition environment; depositing a metal-containing PR on the surface of the substrate in the metal-containing PR deposition environment; performing additional PR processing operations in said one or more other separate integrated processing environments; A system that stores instructions for controlling the [Form 18] 18. The system of claim 17, wherein the plurality of substrate processing environments further includes a PR dry development processing environment; The one or more memory devices may configure the one or more processors to: chemically altering a portion of the metal-containing PR by exposing it to radiation to create a patterned PR, and then dry-developing the patterned PR in the development environment to form a PR mask by removing either the exposed or unexposed portions of the patterned PR by a dry-development process that includes exposure to a compound; The system further stores computer-executable instructions for controlling the [Form 19] 18. The system of claim 17, wherein the plurality of substrate processing environments further includes a thermal processing environment, and the one or more memory devices configure the one or more processors to: heat treating the metal-containing PR in the heat treatment processing environment before and / or after a portion of the metal-containing PR is chemically altered by exposure to radiation to create patterned PR; The system further stores computer-executable instructions for controlling the [Form 20] 18. The system of claim 17, wherein the plurality of substrate processing environments further includes a scanner environment, and wherein the one or more memory devices configure the one or more processors to: exposing a portion of said metal-containing PR to radiation in a scanner environment to chemically alter said exposed portion; The system further stores computer-executable instructions for controlling the [Form 21] 18. The system of claim 17, wherein the plurality of substrate processing environments are different process chambers within a cluster. [Form 22] 18. The system of claim 17, wherein the plurality of substrate processing environments are different stations within a chamber. [Form 23] 18. The system of claim 17, wherein the plurality of substrate processing environments includes three metal-containing PR deposition environments. [Form 24] 18. The system of claim 17, wherein the plurality of substrate processing environments includes two metal-containing PR deposition environments and a metal-containing PR development environment; The one or more memory devices may configure the one or more processors to: a portion of the metal-containing PR is chemically altered by exposure to radiation to create a patterned PR, and then the patterned PR is developed via a dry process; The system further stores computer-executable instructions for controlling the [Form 25] 18. The system of claim 17, wherein the plurality of substrate processing environments includes a metal-containing PR deposition environment, a thermal processing environment, and a metal-containing PR development environment; The one or more memory devices may configure the one or more processors to: heat treating the metal-containing PR in the heat treatment processing environment before and / or after a portion of the metal-containing PR is chemically altered by exposure to radiation to create patterned PR; heat-treating the metal-containing PR in the heat-treating processing environment, and then developing the patterned PR via a dry process; The system further stores computer-executable instructions for controlling the [Form 26] 18. The system of claim 17, wherein the plurality of substrate processing environments comprises the metal-containing PR deposition environment, a first thermal treatment processing environment, a second thermal treatment processing environment, and a metal-containing PR development environment; The one or more memory devices may configure the one or more processors to: heat treating the metal-containing PR in the first heat treatment processing environment before a portion of the metal-containing PR is chemically altered by exposure to radiation to create patterned PR; heat treating the metal-containing PR in the second heat treatment processing environment after a portion of the metal-containing PR has been chemically altered by exposure to radiation to create patterned PR; heat-treating the metal-containing PR in the second heat-treatment processing environment, and then developing the patterned PR via a dry process; The system further stores computer-executable instructions for controlling the

Claims

1. 1. An integrated lithography system comprising: a plurality of reaction chambers in a cluster, the plurality of reaction chambers comprising: Photoresist (PR) deposition chamber; Post-apply bake (PAB) chamber; Lithography scanner; Post Exposure Bake (PEB) chamber; A development chamber; and a substrate deposition chamber; a controller including one or more processors and one or more memory devices, the one or more memory devices storing computer executable instructions that cause the one or more processors to: receiving a substrate within the PR deposition chamber; depositing PR on a surface of the substrate in the PR deposition chamber; receiving the substrate having the PR in the PAB chamber; treating the PR in the PAB chamber to modify material properties of the PR; receiving the substrate with the lithography scanner after the PR process; exposing a portion of the PR to radiation to create a patterned PR; receiving the substrate in the PEB chamber, a portion of the PR being chemically altered by exposure to radiation to create the patterned PR; treating the patterned PR in the PEB chamber to modify material properties of the patterned PR; dry developing the patterned PR in the developing chamber to form a PR mask by removing either the exposed or unexposed portions of the patterned PR by a dry developing process including exposure to a compound; The computer-executable instructions further include instructions for controlling the one or more processors to deposit, prior to the computer-executable instructions for depositing a PR, an underlayer on the surface of the substrate that increases adhesion of the PR to the substrate; The PAB chamber and the PEB chamber are the same chamber. Integrated lithography system.

2. The system of claim 1 , wherein the PR is a metal-containing PR.

3. The system of claim 1 , wherein the PR is an EUV PR.

4. The system of claim 1 , wherein the underlayer is deposited by a dry process.

5. 10. The system of claim 1, wherein the plurality of reaction chambers further comprises a pre-treatment chamber, and the computer-executable instructions further comprise: prior to the computer-executable instructions for depositing the PR, causing the one or more processors to: treating the surface of the substrate by a dry process to generate more chemical functional groups on the surface of the substrate to enhance PR adhesion to the substrate; The system further includes instructions for controlling the

6. 2. The system of claim 1, wherein the computer executable instructions further include instructions for controlling the one or more processors to perform a dry cleaning process to remove PR from a bevel edge and / or backside of the substrate in the PAB chamber.

7. 10. The system of claim 1, wherein a reaction chamber of the plurality of reaction chambers is configured to perform a wafer cleaning process, a post apply bake process, a post exposure bake process, a dry develop process, or a combination thereof.

8. 10. The system of claim 1, wherein the development chamber, the PR deposition chamber, the PAB chamber, the PEB chamber, the underlayer deposition chamber, or a combination thereof, is the same chamber.

9. 9. The system of claim 1, wherein each of the reaction chambers is at subatmospheric pressure, and the PR is at subatmospheric pressure until the dry development process is completed.

10. 9. The system of claim 1, wherein dry developing the patterned PR is performed at a pressure between about 100 Torr and about 760 Torr.

11. 9. The system of claim 1, wherein the ambient environment of the substrate is controlled to reduce exposure of the patterned PR to moisture before the patterned PR is dry developed.

12. 9. The system of claim 1, wherein the computer-executable instructions further comprise computer-executable instructions for depositing the PR by a dry process comprising mixing a water vapor flow of an organometallic precursor with a water vapor flow of a counter reactant.

13. 9. The system of claim 1, wherein depositing the PR comprises a wet spin-on process.

14. 9. The system of claim 1, wherein the processes performed by the multiple reaction chambers include wet and dry processes.

15. 9. The system of claim 1, wherein the cluster comprises a plurality of PR deposition chambers.

16. 1. An integrated lithography system comprising: a plurality of reaction chambers in a cluster, the plurality of reaction chambers comprising: Photoresist (PR) deposition chamber; Post-apply bake (PAB) chamber; Post Exposure Bake (PEB) chamber; A development chamber; and a pre-treatment chamber; a controller including one or more processors and one or more memory devices, the one or more memory devices storing computer executable instructions that cause the one or more processors to: receiving a substrate within the PR deposition chamber; depositing PR on a surface of the substrate in the PR deposition chamber; receiving the substrate having the PR in the PAB chamber; treating the PR in the PAB chamber to modify material properties of the PR; receiving the substrate in the PEB chamber after processing of the PR, where a portion of the PR has been chemically altered by exposure to radiation to create a patterned PR; treating the patterned PR in the PEB chamber to modify material properties of the patterned PR; dry developing the patterned PR in the developing chamber to form a PR mask by removing either the exposed or unexposed portions of the patterned PR by a dry developing process including exposure to a compound; The computer-executable instructions further include instructions for controlling the one or more processors to treat the surface of the substrate by a dry process prior to the computer-executable instructions for depositing a PR to enhance adhesion of the PR to the substrate; The PAB chamber and the PEB chamber are the same chamber. Integrated lithography system.

17. 17. The system of claim 16, wherein the PR is a metal-containing PR.

18. 17. The system of claim 16, wherein the PR is an EUV PR.

19. 17. The system of claim 16, wherein the computer executable instructions further include instructions for controlling the one or more processors to perform a dry cleaning process to remove PR from a bevel edge and / or backside of the substrate in the PAB chamber.

20. 17. The system of claim 16, wherein the plurality of reaction chambers further comprises a lithography scanner, and the computer executable instructions further comprise, prior to the computer executable instructions for receiving the substrate in the PEB chamber, causing the one or more processors to: receiving the substrate with the lithography scanner; exposing a portion of the PR to radiation to create a patterned PR; The system further includes instructions for controlling the

21. 20. The system of claim 16, wherein a reaction chamber of the plurality of reaction chambers is configured to perform a wafer cleaning process, a post apply bake process, a post exposure bake process, a dry develop process, or a combination thereof.

22. 20. The system of claim 16, wherein the development chamber, the PR deposition chamber, the PAB chamber, the PEB chamber, the pre-treatment chamber, or a combination thereof, is the same chamber.

23. 23. The system of claim 16, wherein each of the plurality of reaction chambers is at subatmospheric pressure, and the PR is at subatmospheric pressure until the dry development process is completed.

24. 23. The system of any of claims 16 to 22, wherein dry developing the patterned PR is performed at a pressure between about 100 Torr (about 13332.2 Pa) and about 760 Torr (about 101325 Pa).

25. 23. A system according to any of claims 16 to 22, wherein the ambient environment of the substrate is controlled to reduce exposure of the patterned PR to moisture before the patterned PR is dry developed.

26. 23. The system of any of claims 16 to 22, wherein the computer-executable instructions further comprise computer-executable instructions for depositing the PR by a dry process comprising mixing a water vapor flow of an organometallic precursor with a water vapor flow of a counter reactant.

27. 23. The system of any of claims 16 to 22, wherein depositing the PR comprises a wet spin-on process.

28. 23. The system of any of claims 16 to 22, wherein the processes carried out in the multiple reaction chambers include wet and dry processes.

29. 23. The system of any of claims 16 to 22, wherein the cluster comprises a plurality of PR deposition chambers.

Citation Information

Patent Citations

  • Manufacture of integrated circuit

    JP1983108744A

  • [bakiyu[bakiyu][muchiyatsuku[muchiyatsuku] -

    JP1986012653U

  • Dry-etching device for semiconductor wafer

    JP1994037050A

  • Semiconductor device and manufacture thereof

    JP1994169021A

  • Semiconductor processing device and processing method

    JP1998041206A