Crosslinkable reactive silicone organic copolymer dispersions
Miniemulsion polymerization of ethylenically unsaturated monomers with ethylenically functionalized silicone polymers addresses the instability of silicone-organic polymer bonds, resulting in a stable, crosslinkable copolymer dispersion that forms durable films with enhanced properties on diverse substrates.
Patent Information
- Application Number
- JP2022537457
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-12-18
AI Technical Summary
Existing methods for forming chemical bonds between silicone and organic polymers in aqueous latexes result in unstable, phase-separated products due to the incompatibility of silicone and organic polymers, leading to hydrolyzable Si-O-C bonds and limited copolymerization, which affects the stability and application of silicone resin masonry coatings.
A method involving miniemulsion polymerization of ethylenically unsaturated monomers with ethylenically functionalized silicone polymers, using a combination of water-soluble and oil-soluble initiators to form a stable, crosslinkable reactive silicone organic copolymer dispersion with hydrolytically stable Si-C bonds, allowing for uniform copolymerization and small particle sizes.
The method produces a stable, finely divided copolymer dispersion with hydrolytically stable Si-C bonds, enabling robust crosslinking and forming films with improved durability, corrosion resistance, and other beneficial properties on various substrates.
Smart Images

Figure 0007559068000001
Abstract
Description
[Technical field]
[0001] The present invention relates to crosslinkable reactive silicone-organic copolymers of ethylenically unsaturated monomers and ethylenically functionalized silicone polymers in the form of aqueous dispersions, and to their preparation and use. [Background technology]
[0002] Silicone polymers, such as silicone resins, are used as binders for chemical modification of organic polymers or for coatings. For use as coating compositions, EP943634A1 describes aqueous latexes prepared by copolymerizing ethylenically unsaturated monomers in the presence of silicone resins containing silanol groups. In this case, interpenetrating networks (IPNs) are formed between polymer chains and polysiloxane chains.
[0003] The silicone resin emulsion polymers obtainable by these methods, and the otherwise known physical mixtures of silicone resin emulsions and organic polymer dispersions, are known for the fact that silicone resins and organic polymers are almost exclusively present in the form of physical blends, for example for use in the area of silicone resin masonry coatings.All constructions of chemical bonds between silicone components and organic components are accidental and include Si-OC bonds that are susceptible to hydrolysis.In this case, Si-OC bonds are always in competition with the formation of Si-O-Si bridges by condensation between silanol groups.
[0004] The copolymerization of double bond functionalized silicones with organic monomers to form C-C bonds should result in a more defined attachment of the silicone building blocks to the organic polymer. This type of approach using linear ethylenically unsaturated polyorganosiloxanes has been described in various specifications. For example, EP 1 308 468 A1 teaches hydrophobically modified copolymers obtained by copolymerizing linear silicones with up to two polymerizable groups with organic monomers in emulsion. A similar approach is pursued by EP 352 339 A1, in which vinyl-terminated linear polydimethylsiloxanes are copolymerized with (meth)acrylate monomers.
[0005] EP771826A2 describes the emulsion polymerization of (meth)acrylic esters and vinyl aromatic compounds, in which a difunctional silicone containing an acrylic or vinyl group is added for crosslinking. US5,618,879A similarly pursues this approach, but describes reactive aqueous copolymer dispersions limited to graft copolymers formed from organopolysiloxanes with two different functional groups, at least one of which is ethylenically unsaturated, and ethylenically unsaturated monomers. The graft copolymers are obtained by radical emulsion or microsuspension polymerization of ethylenically unsaturated monomers in the presence of functional organopolysiloxanes. US5,618,879A allows, in principle, both linear polyorganosiloxanes and silicone resins, but the proportion of highly crosslinked Q segments in the polyorganosiloxane reactant is limited to less than 30% in US5,618,879A.
[0006] However, the mere presence of silicone resin during radical polymerization of organic monomers does not mean that chemical bonds are actually created between the silicone and the resulting organic polymer. To understand this, it is necessary to look more closely at the known mechanisms of radical polymerization in an aqueous environment. Given the known incompatibility of silicone polymers with organic polymers, it is obvious to assume the formation of a two-phase product consisting of a silicone phase and an organic polymer phase without chemical bonds between the two phases. In particular, it is noted that in the standard method of radical emulsion polymerization, the polymerization reaction of the organic monomers begins in the aqueous phase, where micelles that grow further are formed, and the micelles are fed with further monomers via the aqueous phase, and copolymerization between hydrophobic silicone oligomers or silicone polymers that are inaccessible to water by the normal route of radical emulsion polymerization seems rather unlikely unless special measures are taken to push for true copolymerization. However, in the aforementioned specification, no such measures are taken. In the standard method of radical emulsion polymerization, the emulsion droplets that are mainly formed during emulsion preparation are otherwise depleted in the organic monomer, and eventually only the silicone remains, which can polymerize with itself and thus form a separate phase. When this type of dispersion is dried by evaporation of the water, the result is a silicone phase and an organic polymer phase that are not bonded to each other. Since phase separation occurs during the polymerization process, the assumption of an interpenetrating network structure of the product obtained by this route is unfounded.
[0007] Appropriate measures to promote or bring about copolymerization between silicone and organic monomer components must in any event exclude exclusive or predominant polymerization involving migration of reactants through the aqueous phase. In other words, polymerization must occur in droplets of reactants or monomers, as in suspension polymerization with oil-soluble initiators. Suspension polymerization is particularly common in the manufacture of vinyl chloride polymers. Suspension polymerization results in significantly larger particles than emulsion polymerization (suspension polymerization ≧50 μm, emulsion polymerization <1 μm) and a significantly larger particle size distribution. Also, lower molecular weights are achieved in suspension polymerization than in emulsion polymerization. As a result, the products of suspension polymerization are in different application areas than those of emulsion polymerization.
[0008] To obtain relatively small particle sizes with suspension polymerization (which in this respect can be considered as bulk polymerization in water), the possibility exists in fine suspension polymerization, which allows particle sizes of ≧1 μm in conjunction with the expected wide particle size distribution of the suspended polymer, thus already moving into the upper range of emulsion polymerization. Smaller particle sizes with narrower distributions are thus only possible with emulsion polymerization.
[0009] Small particle copolymer dispersions of silicones containing particles and silicone resins with organic polymers prepared by radical polymerization are taught by US 7,674,868 B2 and US 2018 / 0305576 A1. In both cases, the copolymerization between the silicone resin and the organic polymer component is achieved by mini-emulsion polymerization. Particle sizes in the range of less than 100 nm are obtained. The organic monomers are polymerized in the presence of an olefinically unsaturated silicone resin. The combination of water-soluble and oil-soluble initiators ensures that the polymerization occurs both in the monomer droplets and in the aqueous phase.
[0010] Miniemulsion polymerization also offers advantages over solution polymerization where the handling of hazardous organic solvents poses environmental and safety risks, as well as the inconvenience and cost of needing to remove the organic solvent for many applications, e.g., in water-based coatings. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] European Patent Application Publication No. 943634 [Patent Document 2] European Patent Application Publication No. 1308468 [Patent Document 3] European Patent Application Publication No. 352339 [Patent Document 4] European Patent Application Publication No. 771826 [Patent Document 5] U.S. Pat. No. 5,618,879 [Patent Document 6] U.S. Pat. No. 7,674,868 [Patent Document 7] US Patent Application Publication No. 2018 / 0305576 Summary of the Invention [Problem to be solved by the invention]
[0012] The object of the present invention was to improve upon the prior art by providing stable, in particular storage-stable, finely divided crosslinkable reactive silicone-organic copolymers in the form of their aqueous dispersions, in which the silicone polymer is bonded to an organic polymer component, the bonds in question being Si-C bonds which are hydrolytically stable, and the copolymers additionally contain crosslinkable reactive groups which are capable of forming a film on a substrate by post-crosslinking with themselves or in the presence of an additional crosslinking agent. [Means for solving the problem]
[0013] This object is achieved by the present invention.
[0014] The subject of the present invention is an ethylenically unsaturated monomer and an ethylenically functionalized silicone polymer, Crosslinkable reactive silicone-organic copolymers. - 1. An aqueous dispersion comprising: (A) one or more ethylenically unsaturated organic monomers, preferably monomers from the group comprising vinyl esters, (meth)acrylic esters, vinyl aromatics, olefins, 1,3-dienes, vinyl ethers and vinyl halides, more preferably methacrylic esters or acrylic esters, in an aqueous medium, (B) in the presence of at least one silicone polymer, preferably a silicone resin, functionalized with ethylenically unsaturated radically polymerizable groups and consisting of siloxane units of the general formula: [R 1 p (OR 2 ) z SiO (4-p-z) / 2] (I), [In the formula, R 1 are in each occurrence identical or different and are a group R* or E, in which R* is the same or different in each occurrence and is a hydrogen atom or a cyclic alkyl group having 1 to 18 carbon atoms, preferably C 1 ~C 18 Alkyl, C 6 ~C 18 Cycloalkyl or C 6 ~C 18 an optionally substituted hydrocarbon group having an aryl group, E is a group of the formula -(CR 5 2 ) m -X, preferably -(CH 2 ) 3 -X is an ethylenically unsaturated group, m is an integer from 1 to 10, preferably 3; R 2 are in each case identical or different and are a hydrogen atom or a hydrocarbon radical having 1 to 18 carbon atoms, preferably C 1 ~C 18 Alkyl group or C 6 ~C 18 is a cycloalkyl group, R 5 is a hydrogen atom, C 1 ~C 12 Alkyl group or C 6 ~C 18 an aryl group, preferably a hydrogen atom; X is an ethylenically unsaturated organic group; R 1 is an ethylenically unsaturated group E in at least 1 mol % and at most 50 mol % of all siloxane units (I), p is 0, 1, 2 or 3; z is 0, 1, 2 or 3; where the sum p+z has a value of 0, 1, 2 or 3; with the proviso that for at least 20 mol % of all siloxane units of formula (I) in silicone polymer (B), the sum p+z is 1 or 0, p is 1 or 0, and z is 0; and (C) in the presence of at least one compound having an ethylenically unsaturated group and at least one additional functional group that is not free-radically polymerizable but is capable of crosslinking, in an amount of 6 to 50% by weight, preferably 10 to 40% by weight, more preferably 10 to 20% by weight, based on the total weight of (A); It can be obtained by radical initiated miniemulsion polymerization, Miniemulsion polymerization involves, in a first step, preparing a solution of at least one silicone polymer (B) in one or more ethylenically unsaturated monomers to obtain a silicone-in-monomer solution, In a second step, the silicone monomer solution obtained is emulsified in water using an emulsifier, optionally a hydrophobic co-emulsifier and optionally a polymerization inhibitor to prevent premature radical emulsion polymerization in such a way as to give a miniemulsion having a particle size D(50) of less than or equal to 350 nm, preferably less than or equal to 300 nm, more preferably less than or equal to 250 nm, very preferably less than or equal to 200 nm, provided that compound (C) is added during the preparation of the silicone monomer solution in the first step or during the emulsification to form a mini-emulsion in the second step; In a third step, the miniemulsion obtained is subjected to a radical emulsion polymerization, in which the miniemulsion polymerization is carried out using a water-soluble or oil-soluble polymerization initiator or a mixture of water-soluble and oil-soluble polymerization initiators.
[0015] A further subject of the present invention is ethylenically unsaturated monomers and an ethylenically functionalized silicone polymer, Crosslinkable reactive silicone-organic copolymers. - 1. A method for preparing an aqueous dispersion comprising the steps of: (A) one or more ethylenically unsaturated organic monomers, preferably monomers from the group comprising vinyl esters, (meth)acrylic esters, vinyl aromatics, olefins, 1,3-dienes, vinyl ethers and vinyl halides, more preferably methacrylic esters or acrylic esters, in an aqueous medium, (B) in the presence of at least one silicone polymer, preferably a silicone resin, functionalized with ethylenically unsaturated radically polymerizable groups and consisting of siloxane units of the general formula: [R 1 p (OR 2 ) z SiO (4-p-z) / 2 ] (I), [In the formula, R 1 is in each occurrence identical or different and is a group R* or E, in which R* is the same or different in each occurrence and is a hydrogen atom or a cyclic alkyl group having 1 to 18 carbon atoms, preferably C 1 ~C 18 Alkyl, C 6 ~C 18 Cycloalkyl or C 6 ~C 18 an optionally substituted hydrocarbon group having an aryl group, E is a group of the formula -(CR 5 2 ) m -X group, preferably -(CH 2 ) 3 -X is an ethylenically unsaturated group, m is an integer from 1 to 10, preferably 3; R 2 are in each case identical or different and are a hydrogen atom or a hydrocarbon radical having 1 to 18 carbon atoms, preferably C 1 ~C 18 Alkyl group or C 6 ~C 18 is a cycloalkyl group, R 5 is a hydrogen atom, C 1 ~C 12 Alkyl group or C6 ~C 18 an aryl group, preferably a hydrogen atom; X is an ethylenically unsaturated organic group; R 1 is an ethylenically unsaturated group E in at least 1 mol % and at most 50 mol % of all siloxane units (I), p is 0, 1, 2 or 3; z is 0, 1, 2 or 3; where the sum p+z has a value of 0, 1, 2 or 3; with the proviso that for at least 20 mol % of all siloxane units of formula (I) in silicone polymer (B), the sum p+z is 1 or 0, p is 1 or 0, and z is 0; and (C) in the presence of at least one compound having an ethylenically unsaturated group and at least one additional functional group that is not free-radically polymerizable but is capable of crosslinking, in an amount of 6 to 50% by weight, preferably 10 to 40% by weight, more preferably 10 to 20% by weight, based on the total weight of (A); The aqueous dispersion is prepared by radical initiated miniemulsion polymerization; In a first step, a solution of at least one silicone polymer (B) is prepared in one or more ethylenically unsaturated monomers to obtain a silicone inmonomer solution; In a second step, the silicone monomer solution obtained is emulsified in water with an emulsifier, optionally a hydrophobic co-emulsifier, and optionally a polymerization inhibitor to prevent premature radical emulsion polymerization, in such a way as to give a miniemulsion having a particle size D(50) of less than or equal to 350 nm, preferably less than or equal to 300 nm, more preferably less than or equal to 250 nm, very preferably less than or equal to 200 nm, provided that compound (C) is added during the preparation of the silicone monomer solution in the first step or during the emulsification to form a mini-emulsion in the second step; In a third step, the miniemulsion obtained is subjected to a radical emulsion polymerization, in which the miniemulsion polymerization is carried out using a water-soluble polymerization initiator, or an oil-soluble polymerization initiator, or a mixture of water-soluble and oil-soluble polymerization initiators. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The ethylenically unsaturated monomers (A) used are vinyl esters, preferably vinyl esters of carboxylic acids having 1 to 15 carbon atoms. Preferred are vinyl acetate, vinyl propionate, vinyl butyrate, vinyl 2-ethylhexanoate, vinyl laurate, 1-methylvinyl acetate, vinyl pivalate and vinyl esters of α-branched monocarboxylic acids having 9 to 11 carbon atoms, such as VeoVa9® or VeoVa10® (trade names of Resolution). Particularly preferred is vinyl acetate.
[0017] Suitable monomers from the group of acrylic or methacrylic esters are esters of unbranched or branched alcohols having 1 to 15 carbon atoms. Preferred methacrylic or acrylic esters are methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, 2-ethylhexyl acrylate, and norbornyl acrylate. Particularly preferred are methyl acrylate, methyl methacrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, and norbornyl acrylate.
[0018] Preferred vinyl aromatic compounds are styrene, alpha-methylstyrene, the isomeric vinyltoluenes and vinylxylenes, and divinylbenzene. Particularly preferred is styrene.
[0019] Vinyl halide compounds include vinyl chloride, vinylidene chloride, as well as tetrafluoroethylene, difluoroethylene, hexylperfluoroethylene, 3,3,3-trifluoropropene, perfluoropropyl vinyl ether, hexafluoropropylene, chlorotrifluoroethylene, and vinyl fluoride. Vinyl chloride is particularly preferred.
[0020] An example of a preferred vinyl ether is methyl vinyl ether.
[0021] Preferred olefins are ethene, propene, 1-alkylethenes, and polyunsaturated alkenes, and preferred dienes are 1,3-butadiene and isoprene. Particularly preferred are ethene and 1,3-butadiene.
[0022] Particularly preferred as monomer (A) are one or more monomers from the group: vinyl acetate, vinyl esters of α-branched monocarboxylic acids having 9 to 11 carbon atoms, vinyl chloride, ethylene, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, 2-ethylhexyl acrylate, styrene and 1,3-butadiene. Also particularly preferred as comonomers (A) are mixtures of vinyl acetate and ethylene, mixtures of vinyl acetate, ethylene and a vinyl ester of an α-branched monocarboxylic acid having 9 to 11 carbon atoms, mixtures of n-butyl acrylate and 2-ethylhexyl acrylate and / or methyl methacrylate, mixtures of styrene and one or more monomers from the group methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, mixtures of vinyl acetate and one or more monomers from the group methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, optionally with ethylene, and mixtures of 1,3-butadiene and styrene and / or methyl methacrylate, the mixtures described optionally further comprising one or more of the aforementioned auxiliary monomers.
[0023] Examples of compounds (C) that can be used are the following monomers (C): ethylenically unsaturated alcohols, preferably hydroxyalkyl (meth)acrylates, more preferably 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate and glycerol 1-allyl ether, ethylenically unsaturated mono- and dicarboxylic acids and their salts, preferably crotonic acid, acrylic acid, methacrylic acid, fumaric acid and maleic acid, ethylenically unsaturated sulfonic acids and their salts, preferably vinylsulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid, ethylenically unsaturated primary, secondary or tertiary amines, preferably 2-dimethylaminoethyl methacrylate, 2-tert-butylaminoethyl methacrylate, allyl N-(2-aminoethyl)carbamate hydrochloride, allyl N-(6-aminohexyl)carbamate hydrochloride, allyl N-(3-aminopropyl)hydrochloride, allylamine and vinylpyridine, ethylenically unsaturated amides, preferably 3-dimethylaminopropyl methacrylamide and 3-trimethylammoniumpropyl methacrylamide chloride; ethylenically unsaturated phosphonic acids and their salts, preferably vinylphosphonic acid, - ethylenically unsaturated epoxides, preferably glycidyl methacrylate (GMA), ethylenically unsaturated isocyanates, preferably 1-(isocyanato-1-methyl)-3-(methylethyl)benzene, ethylenically unsaturated anhydrides, preferably maleic anhydride, ethylenically unsaturated monomers containing reactive carbonyl groups, such as acrolein, methacrolein, diacetone acrylamide, diacetone methacrylamide, 2-butanone methacrylate, formyl styrene, diacetone acrylate, diacetone methacrylate, acetonitrile acrylate, acetoacetoxyethyl methacrylate, acetoacetoxyethyl acrylate and vinyl acetoacetate, Ethylenically unsaturated organosilanes containing reactive groups, preferably methacryloyloxypropyltrimethoxysilane and vinyltrimethoxysilane.
[0024] Particularly preferred monomers (C) are ethylenically unsaturated alcohols, more preferably hydroxyalkyl (meth)acrylates, especially 2-hydroxyethyl methacrylate and 2-hydroxyethyl acrylate.
[0025] Thus, aqueous dispersions of crosslinkable reactive silicone-organic copolymers having hydroxyalkyl groups as the crosslinkable functional groups are preferred.
[0026] The crosslinkable reactive silicone organic copolymer can be crosslinked with itself or with other organic or inorganic compounds as crosslinkers. Crosslinking can be effected with or without the aid of stimulants such as catalysts or initiators, heat, electron beam radiation or UV radiation. Drying can also activate the crosslinked polymer through changes in pH, oxygen content, solvent or carrier evaporation, or other changes that cause a reaction. The particular method of achieving crosslinking in the binder polymer is not critical to the present invention. A variety of chemistries are known in the art for producing crosslinks in latexes.
[0027] The crosslinkable reactive silicone-organic copolymer can crosslink with itself if two crosslinkable functional monomers (C) are selected, for example an ethylenically unsaturated primary, secondary, or tertiary amine, such as 2-aminoethyl methacrylate, and an ethylenically unsaturated anhydride, such as methacrylic anhydride, or an ethylenically unsaturated epoxide, such as glycidyl methacrylate, and an ethylenically unsaturated anhydride, such as methacrylic anhydride.
[0028] A crosslinking agent can also be used for crosslinking.
[0029] A further subject of the invention is (1) an aqueous dispersion of a crosslinkable reactive silicone-organic copolymer of the present invention having crosslinkable functional groups; and (2) Crosslinking agent A crosslinkable composition comprising:
[0030] The crosslinker (2) has functional groups capable of reacting with the functional groups of the copolymer (1).
[0031] Preferably, (1) an aqueous dispersion of a crosslinkable reactive silicone-organic copolymer of the present invention having functional groups, preferably hydroxyalkyl groups, that can be crosslinked by reacting with isocyanate groups; and (2) An organic compound having two or more isocyanate groups as a crosslinking agent A crosslinkable composition comprising:
[0032] Examples of organic compounds having two or more isocyanate groups are diisocyanates and polyisocyanates.
[0033] Preferred examples of diisocyanates are hexamethylene 1,6-diisocyanate, isophorone diisocyanate, tolylene 2,4-diisocyanate, tolylene 2,6-diisocyanate, phenylene 1,3-diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), 4,4'-methylenebis(phenyl isocyanate) and dimethylphenyl diisocyanate.
[0034] Examples of polyisocyanates with more than two isocyanate groups include polymethylene polyphenyl polyisocyanates and esters of lysine triisocyanate. Mixtures of di / polyisocyanates can be used, as can di / polyisocyanates modified by the introduction of urethane, allophanate, urea, biuret, uretonimine, urethdion or isocyanurate residues.
[0035] Further non-limiting examples of crosslinkers are phenolic resins, amino resins, epoxy resins, beta-hydroxy(alkyl)amide resins, alkylated carbamate resins, isocyanates, polyacids, anhydrides, organometallic acid-functional materials, polyamines, polyamides, aminoplasts, and mixtures thereof.
[0036] Non-limiting examples of aminoplasts include condensates of amines and / or amides with aldehydes. The most common amines or amides are melamine, urea, or benzoguanamine. For example, condensates of melamine with formaldehyde are suitable aminoplasts. However, condensates of other amines or amides can be used, such as aldehyde condensates of glycoluril. The aldehyde used is most often formaldehyde, but other aldehydes such as acetaldehyde, crotonaldehyde, and benzaldehyde may also be used. Aminoplasts contain methylol groups, and at least a portion of these groups can be etherified with an alcohol to modify the curing reaction. Any monohydric alcohol can be used for this purpose, including methanol, ethanol, butanol, and hexanol. Non-limiting examples of commercially available aminoplasts that can be used include CYMELR 303, CYMELR 322, CYMEL® 327, CYMEL® 380, and CYMEL® 1130 (available from CYTEK Industries and / or ALLNEX).
[0037] Further non-limiting examples of crosslinking agents are polyamine compounds. Particularly suitable compounds of this type are the dihydrazides and trihydrazides of aliphatic and aromatic dicarboxylic acids with 2 to 20 carbon atoms. Representative useful polyamines include ethylenediamine, isophoronediamine, diethylenetriamine, and dibutylenetriamine. In one embodiment of the present invention, it is useful to utilize polyhydrazides as the polyamine compounds. Representative useful polyhydrazides include oxalic acid dihydrazide, adipic acid dihydrazide, succinic acid dihydrazide, malonic acid dihydrazide, glutaric acid dihydrazide, phthalic acid dihydrazide or terephthalic acid dihydrazide, and itaconic acid dihydrazide. In addition, water-soluble hydrazines such as ethylene-1,2-dihydrazine, propylene-1,3-dihydrazine, and butylene-1,4-dihydrazine can also be used as one of the crosslinking agents.
[0038] Further non-limiting examples of crosslinking agents are polyaziridines, polycarbodiimides, organosilanes, such as alkoxysilanes, which can form crosslinks through a condensation reaction with the hydroxyl, silanol or carboxylic acid functional groups of the copolymer, and polyfunctional aldehydes, such as glyoxal or furaldehyde.
[0039] The crosslinking agent (2) for reaction with the crosslinkable functional groups in (1) need only be present in an amount necessary to achieve the desired degree of cure. It is preferred that the crosslinking agent (2) be used in an amount that provides at least 0.1 equivalent of functional groups in (2) for each equivalent of crosslinkable functional groups in the copolymer (1).
[0040] More preferably, the crosslinking agent (2) is used in an amount to provide 0.2 to 2.0 equivalents of functional groups in (2) for each equivalent of crosslinkable functional groups in the copolymer (1).
[0041] The aqueous dispersions of the crosslinkable reactive silicone-organic copolymers of the present invention having functional groups are reactive in such a way that they form a film after application onto a substrate by crosslinking either through reaction with itself or with a crosslinker having functional groups capable of reacting with the functional groups of the copolymer.
[0042] The film on the substrate can be formed by applying an aqueous dispersion of the crosslinkable reactive silicone-organic copolymers of the present invention having functional groups (which are capable of crosslinking with themselves on the substrate) and then crosslinking them.
[0043] A further subject of the invention is a process for forming a film on a substrate by applying the crosslinkable compositions of the invention onto the substrate and then crosslinking them.
[0044] Examples of substrates are metal substrates, wood substrates, plastic substrates or mineral substrates.
[0045] The aqueous dispersion of crosslinkable reactive silicone organic copolymer of the present invention can be used as binder for coating composition, for example in the field of industrial coating or decorative coating, where the copolymer dispersion mainly forms film by crosslinking reaction involving different functional groups.The cured film provides advantages such as corrosion resistance, hardness, flexibility, toughness, durability, gloss, temperature resistance, dirt repellency, UV resistance, microbial resistance, anti-blocking properties, chemical resistance and waterproofing.
[0046] Coatings based on the aqueous dispersions of the present invention can be applied to a wide variety of substrates known in the coatings industry. For example, the coatings of the present invention can be applied to automotive substrates, industrial substrates, packaging substrates, wood flooring and furniture, clothing, cookware, bakeware, electronic devices including housings and circuit boards, glass and transparent films, or sporting goods including golf balls.
[0047] These substrates can be, for example, metallic or non-metallic. Metallic substrates include, but are not limited to, steel, including tin, electrogalvanized steel, cold rolled steel and hot-dip galvanized steel, aluminum, aluminum alloys, zinc-aluminum alloys, zinc-aluminum alloy coated steel, and aluminum plated steel.
[0048] Non-metallic substrates include polymers, plastics, polyesters, polyolefins, polyamides, cellulose, polystyrene, polyacrylic, poly(ethylene naphthalate), polypropylene, polyethylene, nylon, EVOH, polylactic acid, other "green" polymer substrates, poly(ethylene terephthalate) (PET), polycarbonate, polycarbonate acrylobutadiene styrene (PC / ABS), polyamides, wood, veneers, wood composites, particle board, medium density fiberboard, cement, stone, glass, paper, cardboard, textiles, and both synthetic and natural leather.
[0049] In certain embodiments, the coating of the present invention may be applied to coils. For example, in some of these embodiments, the coating based on the present invention may be applied to metal coils, including, but not limited to, galvanized steel coils and aluminum coils.
[0050] Coatings based on the aqueous dispersions of the present invention can be applied by any means standard in the art such as electrocoating, spraying, electrostatic spraying, dipping, rolling or brushing. Coatings of the present invention can be applied to a dry film thickness of 0.2 to 600 μm, for example, 12 μm to 26 μm or 21 μm to 25 μm.
[0051] The coating composition based on the aqueous dispersion of the present invention can also include any other material well known in the art of formulating coatings. For example, the coating composition of the present invention can also include a colorant. As used herein, "colorant" refers to any substance that imparts color and / or other opacity and / or other visual effect to the composition. The colorant can be added to the coating in any suitable form, such as discrete particles, dispersions, solutions, and / or flakes. A single colorant or a mixture of two or more colorants can be used in the coating of the present invention.
[0052] Examples of colorants include pigments (organic or inorganic), dyes and kezo dyes, such as pigments used in the paint industry and / or pigments listed in the Dry Color Manufacturers Association (DCMA), and special effect compositions. Colorants can include, for example, finely divided solid powders that are insoluble but wettable under the conditions of use. Colorants can be organic or inorganic and can be agglomerated or non-agglomerated. Colorants can be incorporated into the coating by the use of grinding vehicles, such as acrylic grinding vehicles, the use of which is familiar to those skilled in the art.
[0053] Examples of pigments and / or pigment compositions include, but are not limited to, carbazole dioxazine crude pigments, azo, monoazo, diazo, naphthol AS, salt type (flake), benzimidazolone, isoindolinone, isoindoline and polycyclic phthalocyanine, quinacridone, perylene, perinone, diketopyrrolopyrrole, thioindigo, anthraquinone, indanthrone, anthrapyrimidine, flavanthrone, pyranthrone, anthanthrone, dioxazine, arylcarbonium, quinophthalone pigments, diketopyrrolopyrrole red ("DPPBO red"), titanium dioxide, carbon black, and mixtures thereof. The terms "pigment" and "colored filler" can be used interchangeably.
[0054] Examples of dyes include, but are not limited to, solvent and / or aqueous based, such as phthalo green or blue, iron oxides, bismuth vanadate, anthraquinones, and perylenes and quinacridones.
[0055] Examples of hair dyes include, but are not limited to, pigments dispersed in water-based or water-miscible carriers such as AQUA-CHEM 896 available from Degussa, Inc., CHARISMA COLORANTS and MAXITONER INDUSTRIAL COLORANTS available from the Accurate Dispersions Division of Eastman Chemical, Inc.
[0056] Other non-limiting examples of materials that can be used with coating compositions based on the aqueous dispersions of the present invention include plasticizers, wear-resistant particles, corrosion-resistant particles, corrosion-resistant additives, fillers (including, but not limited to, mica, talc, clays, and inorganic minerals), antioxidants, hindered amine light stabilizers, UV light absorbers and stabilizers, surfactants, flow and surface control agents, thixotropic agents, organic co-solvents, reactive diluents, catalysts, reaction inhibitors, and other customary adjuvants.
[0057] In certain embodiments, the coating composition comprises pigment particles, which may comprise 20-70 wt.%, or 30-60 wt.%, based on the total weight of the coating composition. In some of these embodiments, the pigment particles are inorganic pigment particles.
[0058] The selection of the monomer (A) or the weight proportions of the monomers (A) and (C) here is generally made so as to result in a glass transition temperature Tg of the crosslinkable reactive silicone-organic copolymer preferably below 60° C., more preferably between 50° C. and +60° C., very preferably between −30° C. and +50° C., more particularly between 0° C. and 30° C. The glass transition temperature Tg of the polymer can be determined in known manner by differential scanning calorimetry (DSC). Tg may also be approximately calculated beforehand using the Fox equation: according to Fox TG, Bull. Am. Physics Soc. 1, 3, p. 123 (1956), 1 / Tg=x1 / Tg1+x2 / Tg2+··+xn / Tgn, where xn is the mass proportion of monomer n (wt.% / 100) and Tgn is the glass transition temperature in Kelvin of a homopolymer of monomer n. Tg values for homopolymers can be found in numerous reference and standard works in polymer technology and in tabular works searchable on the internet, such as those from Aldrich under the heading "Polymer Properties, Thermal Transitions of Homopolymers" (https: / / www.sigmaaldrich.com / content / dam / sigma-aldrich / docs / Aldrich / General_Information / thermal_transitions_of_homopolymers.pdf).
[0059] The proportion of monomers (A) and (C) in the construction of the copolymer of the invention is in each case preferably at least 20% by weight, more preferably between 30 and 95% by weight, based on the total weight of (A), (C) and the functionalized silicone polymer (B). This means that the proportion of (B) is preferably less than 80%, more specifically between 5 and 70% by weight, based on the total weight of (A), (C) and the functionalized silicone polymer (B).
[0060] Particularly preferred silicone polymers (B) have the following general formula: [R 1 p (OR 2 ) z SiO (4-p-z) / 2 ] (I) In the formula (I), p and z have the definition p=0 or 1 and z=0, 1 or 2, and for at least 20 mol% of all siloxane units of formula (I), p=1 and z=0 or p=0 and z=0, and this condition is preferably satisfied for at least 30 mol%, more preferably at least 35 mol%, more preferably at least 40 mol% of all siloxane units (I) for p=1 and z=0. It is also preferred that the siloxane units (I) contain 50 mol% or less of so-called Q units with p=0 and z=0.
[0061] Furthermore, also suitable are M units (R 3 SiO 1 / 2 ), D units (R 2 SiO 2 / 2 ), T units (RSiO 3 / 2 ), and Q units (SiO 4 / 2 ), where R is a group R 1 Or group -OR 2 and R 1 and R 2 have the definitions given above for them, except that for formula (I) where p=1 and z=0 or p=0 and z=0, T or Q units are always present in at least 20 mol %.
[0062] The most preferred silicone resins (B) are essentially composed of T or Q and D units, with the molar ratio of T / D units being preferably greater than 50 / 50, more particularly greater than 70 / 30, and particularly preferred are those that are composed of only T units, without any D units, with the molar ratio of T / D units being up to 20 / 80.Moreover, the most preferred silicone resins are those that are mainly composed of T units, more particularly those that are composed of T units to an extent of at least 80 mol%, and very particularly those that are composed of T units to an extent of at least 90 mol%.Also preferred silicone resins are those that have a small amount of silicon-bonded alkoxy groups.Since the synthesis method used is tolerant of hydrolyzable alkoxy groups, the alkoxy groups are not substantially hydrolyzed.In other words, essentially no hydroxyl groups are generated from the alkoxy groups, which are removed by condensation in the form of water, leaving Si-O-Si units.Nevertheless, if the functional silicone resin used is R 2 R having the definition given above according to formula (I) 2 It is preferred to have a low content of O-type groups. The more alkoxy groups present, the lower the degree of condensation of the silicone resin. A high degree of condensation is preferred, since for a given substitution pattern a high degree of condensation generally corresponds to a high glass transition temperature. The higher the glass transition, the less the silicone resin component of the copolymer tends to soften, which is an advantage in construction coatings, since a lower tendency to stain can be achieved in conjunction with a relatively high service temperature.
[0063] At least 1 mol %, preferably at most 50 mol %, preferably at most 40 mol %, of all siloxane units of formula (I) contain an ethylenically unsaturated group E as group R1.
[0064] The group X is linear, branched or cyclic. In addition to the double bond, further functional groups may also be present, which are generally inert to olefin polymerization, examples being halogens, carboxyl groups, sulfinato groups, sulfonato groups, amino groups, azido groups, nitro groups, epoxy groups, alcohol groups, ether groups, ester groups, thioether groups and thioester groups, as well as aromatic homocyclic and heterocyclic groups. Preferred examples of the group X are monounsaturated C 2 ~C 10 The most preferred groups for the group X are acrylic and methacrylic groups.
[0065] The hydrocarbon radical R* that does not contain multiple aliphatic C-C bonds can be, for example, an alkyl radical, a cycloalkyl radical or an aryl radical. Thus, examples of radicals R* are alkyl radicals, for example methyl radicals, ethyl radicals, n-propyl radicals, isopropyl radicals, n-butyl radicals, isobutyl radicals, tert-butyl radicals, n-pentyl radicals, isopentyl radicals, neopentyl radicals, tert-pentyl radicals, hexyl radicals such as n-hexyl radicals, heptyl radicals such as n-heptyl radicals, octyl radicals such as n-octyl radicals and isooctyl radicals such as 2,2,4-trimethylpentyl radicals, nonyl radicals such as n-nonyl radicals, n-decyl radicals, etc. decyl groups, dodecyl groups such as n-dodecyl groups, hexadecyl groups, and octadecyl groups such as n-octadecyl groups, cycloalkyl groups such as cyclopentyl, cyclohexyl, cycloheptyl, and methylcyclohexyl groups, aryl groups such as phenyl, naphthyl, anthryl, and phenanthryl groups, alkaryl groups such as tolyl, xylyl, ethylphenyl, and aralkyl groups such as benzyl and β-phenylethyl groups. Particularly preferred radicals R* are methyl, isooctyl, propyl, and phenyl groups. This description is merely illustrative and should not be understood as imposing any restrictions.
[0066] When the groups R* are substituted, they may further contain one or more identical or different heteroatoms selected from O, S, Si, Cl, F, Br, P or N atoms.
[0067] The examples of groups R* are fully valid for group R2.
[0068] Examples of alkyl groups R* having 1 to 12 carbon atoms and aryl groups R* having 6 to 18 carbon atoms are C 1 ~C 12 Alkyl group and C 6 ~C 18 Aryl group R 5 is perfectly valid.
[0069] In one preferred embodiment of the present invention, there are two different groups R* present in the silicone resin composed of siloxane units (I).
[0070] Examples of preferred combinations of radicals R* are phenyl and methyl, n-butyl and ethyl, n-butyl and methyl, ethyl and methyl, n-octyl and methyl, isooctyl and methyl, isooctyl and phenyl, n-octyl and phenyl, n-octyl and ethyl, phenyl and ethyl, isooctyl and ethyl, with the combinations phenyl and methyl, ethyl and methyl, isooctyl and methyl, ethyl and isooctyl, and phenyl and isooctyl being particularly advantageous. The combinations of methyl and isooctyl, and methyl and phenyl as two different radicals R* have proven to be particularly effective. These combinations of the two radicals allow the best control and setting of the two properties of compatibility in the polymer matrix and a high glass transition temperature. They also ideally meet the requirements of availability and economy.
[0071] It is preferred, and has proven to be particularly advantageous, that the siloxane units (I) with more carbon-rich substituents are present in less than 75 mol% of the total siloxane units of formula (I).This means that the siloxane units (I) with less carbon-rich substituents are present in more than 25 mol% of the total siloxane units of formula (I).In one particularly preferred embodiment of the present invention, the siloxane units of formula (I) with less carbon-rich substituents are present in the majority, i.e., more than 50 mol% of the total siloxane units of formula (I), and thus the carbon-rich substituents are present in the minority, i.e., less than 50 mol% of the total siloxane units of formula (I).
[0072] The carbon-rich substituent R* is a carbon-hydrogen group such as an alkyl group, a cycloalkyl group or an aryl group having 4 to 18 carbon atoms, preferably 6 to 18 carbon atoms, more preferably an isooctyl group and a phenyl group, and the carbon-poor substituent R* is an alkyl group having 1 to 3 carbon atoms, preferably a methyl group.
[0073] All ratio values given are normalized to 100 mol % as the sum of units of formula (I) bearing different carbon-rich Si-C bonded groups.
[0074] In the case of a combination of isooctyl and methyl groups, it is preferable that the number of siloxane units of formula (I) having methyl groups is greater than the number of siloxane units of formula (I) having isooctyl groups. The ratio of the number of siloxane units of formula (I) having methyl groups to the number of siloxane units of formula (I) having isooctyl groups is preferably 51:49 to 99:1, more preferably 55:45 to 98:2, and more specifically 60:40 to 98:2.
[0075] Ratios which have proven particularly effective are 60:40, 70:30, 90:10, and 95:5.
[0076] All these values are normalized to 100 as the sum of the units of formula (I) bearing a methyl group and the units of formula (I) bearing an isooctyl group.
[0077] In the case of a combination of a phenyl group and a methyl group, the ratio of the number of siloxane units of formula (I) having a methyl group to the number of siloxane units of formula (I) having a phenyl group is preferably 51:49 to 99:1, more preferably 55:45 to 98:2, and more specifically 60:40 to 98:2.
[0078] Ratios which have proven particularly effective are 60:40, 70:30, 80:20, 90:10, and 95:5.
[0079] All these numbers are normalized to 100 as the sum of the units of formula (I) bearing a methyl group and the units of formula (I) bearing a phenyl group.
[0080] Combinations of more than two different groups are also possible and are within the scope of the present invention. In that case, the above-mentioned preferred ratios for the combinations of two different groups apply mutatis mutandis, if the more carbon-rich substituted siloxane units are counted together and placed in ratio to the siloxane units with the smallest or least carbon-rich substituent. In this context, a distinction is made in the above-mentioned manner between combinations that contain aromatic substituents and combinations that do not contain aromatic substituents.
[0081] Even when more than two different siloxane units of formula (I) are present, preferred combinations are those of methyl, n-propyl, phenyl, n-butyl, n-octyl and isooctyl groups, more particularly those of methyl, n-propyl, phenyl and isooctyl groups, and particularly preferred are those of methyl, phenyl, n-propyl and isooctyl groups.
[0082] The ethylenically unsaturated group can be attached to the silicone polymer S through condensation of the silane of formula (II) with the silicone polymer S. (R 3 O) 3-n (R 4 ) n Si-(CR 5 2 ) m -X (II) In the formula, R 3 is a hydrogen atom, C 1 ~C 6 Alkyl group or C 6 ~C 18 is an aryl group, R 4 is a hydrogen atom, C 1 ~C 12 Alkyl group or C 6 ~C 18 is an aryl group, R 5 and m has the meaning given above, n is 0, 1 or 2.
[0083] The preparation of the silicone polymer (B) is disclosed in US2018 / 305576A1 (incorporated by reference) at paragraphs
[0083] on page 6 to
[0089] on page 7.
[0084] It has been found that readily available gamma-silane (m=3) is very suitable for carrying out the present invention, despite the low reactivity of gamma-silane compared to alpha-silane.It has been found that the present invention is in principle possible with small amounts of gamma-silane used for functionalization of the silicone polymer, as little as 1.0% by weight of silane, based on the total amount of silicone polymer used, but for the purpose of more complete incorporation of the silicone resin, it is advantageous to use at least 1.5% by weight of gamma-silane, preferably at least 2.0% by weight, more preferably at least 2.5% by weight of gamma-silane, more specifically at least 3.0% by weight of gamma-silane, the most preferred amount being between 4 and 8% by weight, since it is in this range that the best balance between efficiency and economy is obtained.
[0085] In miniemulsion polymerization, optionally, a hydrophobic co-emulsifier may also be present, which is present in an amount of up to 3% by weight, based on the total weight of component (A) and functionalized component (B).In this case, silicone polymers often take on the function of co-emulsifier.Further examples of co-emulsifiers are hexadecane, cetyl alcohol, oligomeric cyclosiloxanes, such as octamethylcyclotetrasiloxane, or vegetable oils, such as rapeseed oil, sunflower oil or olive oil.Also suitable are organic or inorganic polymers with number average molecular weight Mn of less than 10,000.
[0086] Specifically preferred hydrophobic co-emulsifiers according to the invention are the silicone polymer to be polymerized itself and hexadecane.
[0087] The copolymers are prepared in a heterophase manner by the known technique of miniemulsion polymerization. Miniemulsion polymerization differs from emulsion polymerization in a number of important ways. See the paper "Non-aqueous emulsion polymerizations" presented by Kevin Mueller, Mainz 2008, pp. 17-20, and the references cited therein. In contrast to emulsion polymerization, where the size of the polymer latex particles is essentially determined by kinetic processes and the stability of the lattice, the basis of miniemulsion polymerization is that the monomers before polymerization are entirely present within the micelles and therefore there is no longer any need to diffuse from the monomer droplets to the micelles during polymerization. In other words, the latex particles formed can therefore be considered as polymerized copies of the monomer droplets present at the starting point. As a result, the size of the latex particles is determined exclusively by the dispersion method and by the stability of the monomer-filled micelles. Since there is no need for transport of the monomer through the continuous phase, it is possible in this way to use monomers that are completely insoluble in the continuous phase as well. To increase the stability of the monomer droplets, it is necessary to suppress the Ostwald ripening that occurs. Thus, during the miniemulsion polymerization of the dispersed monomer phase, a hydrophobe, or, in the case of an inverse miniemulsion, an oleophobe, is added.
[0088] Among the species that can act as hydrophobes are optionally hydrophobic monomers suitable for that purpose, such as silicone components.
[0089] Here, miniemulsion polymerization differs from suspension polymerization in two ways. First, the polymer particles produced in the miniemulsion process are much smaller (50-500 nm) than those in suspension polymerization (1 μ-1 mm). Second, the number of groups per growing particle in suspension polymerization, 10, is significantly higher than that in miniemulsion polymerization (statistically, there are 0.5 groups per growing particle in the reaction).
[0090] To carry out radical miniemulsion polymerization, it is first necessary to build a miniemulsion of vinyl monomers in a continuous phase that is immiscible with the vinyl monomer. For this purpose, the monomers are dispersed in water together with emulsifiers and hydrophobic substances, for example using a high-pressure homogenizer or by input of energy using ultrasound. Here, the combination of emulsifiers and hydrophobic substances delays the occurrence of Ostwald ripening and the coalescence of the monomer droplets. In a second stage, the monomer droplets thus formed are polymerized. This is triggered either by a water-soluble initiator that is added after the preparation of a stable miniemulsion, or by an oil-soluble initiator that may be present in the monomer phase immediately after initiation, or by a combination of both.
[0091] The monomer droplets formed in the miniemulsion have a size of approximately 50-500 nm. This small size is the result of the homogenization of the miniemulsion, achieved by the input of a large amount of energy. The migration of the monomer between the individual droplets is suppressed by a certain type of stabilization.
[0092] Also, in parallel with the small monomer droplets, free micelles are no longer present in miniemulsions. In contrast to conventional emulsion polymerization, it is therefore mainly the droplets that are the site of nucleation (droplet nucleation). During miniemulsion polymerization, therefore, only very little diffusion of the monomer is observed. Within miniemulsion polymerization, each dispersed monomer droplet can then be described as an individual reactor operated at the nanoscopic level. As a result, in contrast to traditional emulsion and suspension polymerization, this method offers many advantages, which are highlighted below.
[0093] · Even monomers that are completely insoluble in water can be polymerized in miniemulsions, since the monomers do not need to be transported through a continuous phase, usually the water phase.
[0094] The size of the latex particles usually corresponds to the size of the preformed monomer droplets and can be adjusted with considerable precision by the nature and amount of emulsifier used.
[0095] Each monomer droplet is homogeneous in composition. Therefore, especially in the case of copolymerization, the monomer ratio in each droplet is the same, and there is no difference in the diffusion of the monomers.
[0096] · Lesser amounts of emulsifiers are used because miniemulsions are only kinetically and not thermodynamically stabilized.
[0097] The essential step of the process, namely that of preparing a finely divided miniemulsion, is carried out in the present case as follows:
[0098] In the first step, one or more silicone polymers, preferably silicone resins, composed of siloxane units of formula (I) are dissolved in one or more ethylenically unsaturated monomers to obtain a silicone resin-in-monomer solution. What is characteristic here is the fact that the silicone resins composed of siloxane units of formula (I) are soluble in the respective monomer mixtures. Insoluble components are separated by filtration if necessary and appropriate. The only silicone resin-in-monomer solutions according to the present invention are those that do not contain insoluble silicone components.
[0099] The silicone resin-in-monomer solution is optionally mixed with a hydrophobic co-emulsifier, examples of which are set forth above.
[0100] In a second step, the silicone resin-in monomer solution is emulsified with water and at least one emulsifier, and optionally further auxiliaries such as polymerization inhibitors to prevent premature radical emulsion polymerization, preferably by applying high shear forces, to obtain emulsions with particle sizes D(50) of 350 nm or less, known as miniemulsions. High shear forces in this context can be generated by suitable emulsifying devices such as conventional rotor-stator systems, or other methods that are common knowledge in the art of comparable emulsification, for example by high-pressure homogenizers, dissolver disks, ultrasonic devices, or equivalent emulsifying devices that exert high shear forces that allow the generation of small particle sizes of 200 nm or less, giving miniemulsions with particle sizes D(50) of 350 nm or less. For commercially available rotor-stator systems, rotation speeds of 4000-12000, preferably 5000-11000, more particularly 6000-10000, have proven to be particularly advantageous. Both continuous and discontinuous embodiments are suitable. In the case of high pressure homogenizers, pressures of preferably 300 bar to 1000 bar, more preferably 350 bar to 900 bar, more particularly 400 bar to 800 bar have proven to be advantageous. Since the preparation is polymerizable, effective temperature monitoring is important: the temperature of the miniemulsion should preferably not exceed 60°C, more preferably not exceed 55°C, more particularly not exceed 50°C, and in such circumstances should be rapidly cooled below these temperatures.
[0101] The silicone resin monomer solution of the present invention has a viscosity of 2 to 20,000 mPas at 25° C., preferably 5 to 15,000 mPas at 25° C., more specifically 7 to 10,000 mPas at 25° C. The mini-emulsion of the present invention has a viscosity of 2 to 5,000 mPas at 25° C., specifically 3 to 4,500 mPas at 25° C., more specifically 5 to 4,000 mPas at 25° C.
[0102] The amount of water in the miniemulsion of the present invention is between 80 and 20 weight percent, preferably between 75 and 20, and more specifically between 70 and 25 weight percent.
[0103] The particle size D(50) in the miniemulsion of the invention is less than or equal to 350 nm, preferably less than or equal to 300 nm, more preferably less than or equal to 250 nm, very preferably less than or equal to 200 nm, and also at least 20 nm, preferably at least 30 nm, more preferably at least 50 nm.
[0104] The miniemulsions of the present invention consist of a continuous aqueous phase and a dispersed organic phase.
[0105] The organic phase of the mini-emulsion is polymerized by radical emulsion polymerization method. In this case, in the third step, the dispersed silicone resin-in-monomer solution is subjected to free radical polymerization. This radical emulsion polymerization is preferably carried out by metering the mini-emulsion into an initial charge that includes water and a part of the catalyst. Further metered feeds include a polymerization initiator, which can optionally include a plurality of components, each of which is metered separately into the initial charge or included in the initial charge according to their interaction and function in the polymerization procedure.
[0106] Once the miniemulsion polymerization is complete, the resulting dispersion is adjusted to the desired pH, if necessary, optionally filtered and then ready for the respective use.
[0107] The reaction temperature in the miniemulsion polymerization is preferably 0°C to 100°C, more preferably 5°C to 80°C, and most preferably 30°C to 70°C.
[0108] The pH of the dispersion medium is between 2 and 9, preferably between 4 and 8. In one particularly preferred embodiment, it is between 4.5 and 7.5. The pH can be adjusted before the start of the reaction using hydrochloric acid or aqueous sodium hydroxide. The polymerization can be carried out batchwise or continuously, with all or individual components of the reaction mixture in the initial charge, with individual components of the reaction mixture partially in the initial charge and subsequently metered in partially or not in the initial charge, by metering methods. All metered feeds are preferably carried out at the rate at which the components in question are consumed.
[0109] The polymerization is initiated by a conventional water-soluble initiator or a combination of redox initiators, preferably the latter. Examples of initiators are sodium, potassium and ammonium salts of peroxodisulfate, hydrogen peroxide, tert-butyl peroxide, tert-butyl hydroperoxide, potassium peroxodiphosphate, tert-butyl peroxopivalate, cumene hydroperoxide, isopropylbenzene monohydroperoxide and azobisisobutyronitrile. The above initiators are preferably used in an amount of 0.01 to 4.0% by weight, based on the total weight of the monomers. As a combination of redox initiators, the initiators identified above are used together with a reducing agent. Suitable reducing agents are sulfites and bisulfites of monovalent cations, examples being sodium sulfite or derivatives of sulfoxylic acid such as zinc or alkali metal formaldehyde sulfoxylates, e.g. sodium hydroxymethanesulfinate, and ascorbic acid. The amount of reducing agent is preferably 0.15 to 3% by weight of the amount of monomers used. In addition, small amounts of metal compounds can be introduced which are soluble in the polymerization medium and whose metal component is redox active under the polymerization conditions, said compounds being based, for example, on iron or vanadium. One particularly preferred initiator system containing the aforementioned components is the system tert-butyl hydroperoxide / sodium hydroxymethanesulfinate / Fe(EDTA) 2+ / 3+ It is.
[0110] According to the miniemulsion polymerization method, it is also possible to use mainly oil-soluble initiators such as cumene hydroperoxide, isopropylbenzene monohydroperoxide, dibenzoyl peroxide or azobisisobutyronitrile. Preferred initiators for miniemulsion polymerization are potassium persulfate, ammonium persulfate, azobisisobutyronitrile, and dibenzoyl peroxide.
[0111] The size of the silicone domains in the copolymer after copolymerization is preferably in the range of 5 nm to 150 nm, more particularly 10 nm to 140 nm, particularly preferably 15 nm to 125 nm, which can be determined, for example, by scanning or transmission electron microscopy of the polymer dispersions or the polymer films obtained therefrom. EXAMPLES
[0112] <Preparation Example> In this document, materials are characterized by reporting data obtained by instrumental analysis. The underlying measurements are performed according to publicly available standards or are determined using specially developed techniques. To ensure clarity of the teachings given, the methods used are specified below.
[0113] In all examples, unless otherwise specified, all parts and percentages are by weight.
[0114] <Viscosity> Viscosity, unless otherwise specified, is determined by measurement using rotational viscometry according to DIN EN ISO 3219. All viscosity values relate to 25° C. and atmospheric pressure of 1013 mbar, unless otherwise specified.
[0115] <Molecular composition> The molecular composition is determined by nuclear magnetic resonance spectroscopy (for terminology, see ASTM E 386: High-Resolution Nuclear Magnetic Resonance Spectroscopy (NMR): terms and symbols), measuring 1H and 29Si nuclei.
[0116] 1 H NMR measurement explanation Solvent: CDCl 3 , 99.8%d Sample concentration: Approximately 50 mg / 1 ml of CDCl in a 5 mm NMR tube 3 Measurement without TMS, CDCl at 7.24 ppm3 Residual CHCl in 3 Referencing the spectrum by Spectrometer:Bruker Avance 400 Sample head: 5mm BBO sample head or SMART sample head (Bruker) Measurement parameters: Pulprog=zg30 TD=64k NS=64 or 128 (depending on the sensitivity of the sample head) SW=20.6ppm AQ=3.17 seconds D1=5 seconds SFO1=500.13MHz O1=6.175ppm Processing parameters: SI=32k WDW=EM LB=0.3Hz
[0117] Depending on the type of spectrometer used, individual adjustments of the measurement parameters may be necessary.
[0118] 29 Explanation of Si NMR measurements Solvent: C6D6 99.8%d / CCl4 1:1v / v with 1wt% Cr(ac)3 as a relaxation agent Sample concentration: Approximately 2g / 1.5ml of solvent in a 10mm NMR tube Spectrometer:Bruker Avance 400 Sample head: 10mm 1H / 13C / 15N / 29Si glass-free QNP sample head (manufactured by Bruker) Measurement parameters: Pulprog=zgig60 TD=64k NS=1024 (depending on the sensitivity of the sample head) SW=200ppm AQ=2.75 seconds D1=4 seconds SFO1=300.13MHz O1=-50ppm Processing parameters: SI=64k WDW=EM LB=0.3Hz
[0119] Depending on the type of spectrometer used, individual adjustments of the measurement parameters may be necessary.
[0120] <Molecular weight distribution> Molecular weight distribution is determined as weight average Mw and number average Mn using the method of gel permeation chromatography (GPC or size exclusion chromatography (SEC)) using polystyrene standards and a refractive index detector (RI detector). Unless otherwise specified, THF is used as the eluent and DIN 55672-1 is used. Polydispersity is the quotient Mw / Mn.
[0121] <Glass transition temperature> The glass transition temperature is determined by differential scanning calorimetry (DSC) according to DIN 53765, perforated crucible, heating rate 10 K / min.
[0122] <Determination of particle size> Particle size was measured by the method of dynamic light scattering (DLS) along with the determination of the zeta potential. The Z-average particle size was measured with a Malvern Zetasizer Nano ZS particle size analyzer. The polydispersity of particle size (PDI) indicates the width of the particle size distribution.
[0123] <MEKダブルラブ(Rub)テスト> This test method is used to determine the degree of cure of a film by its resistance to a specified solvent. Methyl ethyl ketone (MEK) is used as the solvent.
[0124] The MEK double rub test is performed according to ASTM D5402. The higher the MEK double rub test value, the better the cure, i.e., crosslinking, of the film.
[0125] Ethoxy-functional phenyl silicone resin and methacryloxypropyltrimethoxysilane (CH 3 O) 3 Si(CH2 ) 3 OC(=O)C(CH 3 )=CH 2 Preparation of ethylenically unsaturated phenyl silicone resin B1 by condensation with
[0126] Into a 1 L 4-neck flask equipped with a reflux condenser, thermometer, nitrogen inlet, and overhead stirrer was added 150 g of methanol, 20.45 g of 3-methacryloxypropyltrimethoxysilane, and 60 mol% PhSiO 3 / 2 Unit (=T Ph (units), 36 mol% MeSiO 3 / 2 unit (=T unit), and 4 mol% Me 2 SiO 2 / 2 319.4 g of silicone resin consisting of units (=D units), with 14.2% by weight of MeO groups statistically distributed among the T units, with a molecular weight Mw of 1800 g / mol and a viscosity of 440 mPa.s at 25° C. are charged. The mixture is heated to 40° C., then 0.40 g of a 37% aqueous solution of hydrochloric acid in 10 g of deionized water is added over 5 minutes. The mixture is refluxed at 65° C. for 2 hours with stirring, then neutralized by adding a solution of 0.69 g of 30% sodium methoxide in methanol diluted in 3.50 g of methanol. The solution obtained is distilled at 20 mbar and 55° C. to remove all volatile components. This gives 297 g of a slightly turbid liquid with the following characteristics:
[0127] Molecular weight and heterogeneity: M w =4577g / mol M n =1526g / mol PD=3.00
[0128] 1 H NMR and 29 Molecular composition from Si NMR: Me 2 SiO 2 / 2 : 7.02mol% (Ph)SiO 3 / 2 :58.65mol% ((CH 2 )3 OC(=O)C(CH 3 )=CH 2 )SiO 3 / 2 : 2.47mol% MeO-Si: 31.36 mol%
[0129] Ethoxy-functional silicone resin and methacryloxypropyltrimethoxysilane (CH 3 O) 3 Si(CH 2 ) 3 OC(=O)C(CH 3 )=CH 2 Preparation of ethylenically unsaturated silicone resin B2 by condensation with
[0130] A 3 L, four-neck flask equipped with a reflux condenser, thermometer, nitrogen inlet, and overhead stirrer is charged with 900 g of tetraethylsilicate oligomer, 366 g of hexamethyldisiloxane, 60 g of 3-methacryloxypropyltrimethoxysilane, and 313.20 g of low viscosity OH-terminated polydimethylsiloxane having an average of 45 siloxane units. To this mixture is added a solution of 1.10 g of 37% hydrochloric acid in 220.5 g of deionized water. The mixture is heated to 60°C, at which point the reaction begins to exotherm and heats itself to 75°C. Heat is reapplied to bring the temperature to 79°C, where the reaction is held at reflux with stirring for 60 minutes. The reaction mixture is cooled to below 50°C and transferred to a rotary evaporator flask. While heating at 55°C, a vacuum is gradually applied until 300 g of ethanol is removed, then 2.18 g of a 30% solution of sodium methoxide in methanol is added to neutralize the reaction mixture. 400 g of 2-ethylhexyl acrylate (2-EHA) is added along with 0.400 g of butylated hydroxytoluene (BHT) and the mixture is filtered using gravity through a 100 μm filter. Distillation is resumed at 60°C and 20 mbar to remove remaining volatiles. This produces 1433 g of a clear silicone resin solution in 2-ethylhexyl acrylate (2-EHA), consisting of 28.65% by weight of 2-EHA and 71.35% by weight of a silicone resin having the following characteristics:
[0131] Molecular weight and heterogeneity (using toluene as eluent): Mw=2370g / mol Mn=1447g / mol PD=1.64
[0132] 1 H NMR and 29 Molecular composition from Si NMR: Me 3 SiO 1 / 2 : 17.49mol% Me 2 SiO 2 / 2 :33.80mol% ((CH 2 ) 3 OC(=O)C(CH 3 )=CH 2 )SiO 3 / 2 : 1.25mol% SiO 4 / 2 :28.30mol% EtO-Si: 4.63 mol% MeO-Si: 0.26 mol%
[0133] Preparation of ethylenically unsaturated phenyl silicone resin CB1
[0134] A 3 L four-neck flask equipped with a reflux condenser, thermometer, nitrogen inlet, and overhead stirrer is charged with 623.7 g of absolute ethanol, 41.6 g of deionized water, 0.62 g of 37 wt % hydrochloric acid, 74.85 g of phenyltriethoxysilane, 47.77 g of 3-methacryloxypropyltrimethoxysilane, and 673.5 g of methyltriethoxysilane oligomer containing about 30 wt % silicon-bonded ethoxy groups (available under the trade name TRASIL®, WACKER Chemie AG). These components are mixed and refluxed at 80° C. for 2 hours, after which the mixture is neutralized by adding 1.15 g of a 30% solution of sodium methoxide in methanol. 330 g of ethanol is removed by distillation, and then the reaction is filtered through a 100 μm filter. The resulting solution is distilled at 80° C. and 20 mbar for 2 hours to remove volatile components, resulting in 522 g of a cloudy, highly viscous silicone resin.
[0135] Molecular weight and heterogeneity (using toluene as eluent): Mw=3401g / mol Mn=1126g / mol PD=3.02
[0136] Ethoxy-functional silicone resin and methacryloxypropyltrimethoxysilane (CH 3 O) 3 Si(CH 2 ) 3 OC(=O)C(CH 3 )=CH 2 Preparation of ethylenically unsaturated silicone resin CB2 by condensation with
[0137] A 3 L, 4-neck flask equipped with a reflux condenser, thermometer, nitrogen inlet, and overhead stirrer is charged with 900 g of tetraethylsilicate oligomer, 366 g of hexamethyldisiloxane, 60 g of 3-methacryloxypropyltrimethoxysilane, and 313.20 g of low viscosity OH-terminated polydimethylsiloxane having an average of 45 siloxane units. To this mixture is added a solution of 1.10 g of 37% hydrochloric acid in 220.5 g of deionized water. The mixture is heated to 60°C, at which point the reaction begins to exotherm and heats itself to 75°. Heating is resumed to bring the temperature to 79°C, where the reaction is held at reflux with stirring for 60 minutes. The reaction mixture is cooled to below 50°C and transferred to a rotary evaporator flask. While heating at 55°C, a vacuum is gradually applied until 315 g of ethanol has been removed, then 3.01 g of a 30% solution of sodium methoxide in methanol is added to neutralize the reaction. 400 g of butyl acrylate is added along with 0.400 g of butylated hydroxytoluene (BHT) and the mixture is filtered using gravity through a 100 μm filter. Distillation is resumed at 60°C and 20 mbar to remove remaining volatiles. This produces 1255 g of a clear silicone resin solution in butyl acrylate, consisting of 17.67% by weight butyl acrylate and 82.33% by weight silicone, with the following properties:
[0138] Molecular weight and heterogeneity: Mw=7100g / mol Mn=3130g / mol PD=2.27
[0139] 1 H NMR and 29 Molecular composition from Si NMR: Me 3 SiO 1 / 2 : 16.70mol% Me 2 SiO 2 / 2 : 47.50mol% ((CH 2 ) 3 OC(=O)C(CH 3 )=CH 2 )SiO 3 / 2:0.46mol% SiO 4 / 2 :20.87mol% EtO-Si: 4.51 mol% MeO-Si: 0.14 mol%
[0140] [Invention Example 1: Preparation of copolymer dispersion E1 from silicone resin B1]
[0141] Step 1: Preparation of mini-emulsion: The miniemulsion is prepared by dissolving the silicone resin B1 in a mixture of (meth)acrylic monomers (the monomer combination includes 2-hydroxyethyl methacrylate, which has a hydroxy group in addition to the radically polymerizable methyl methacrylate group) and then homogenizing at high pressure. The aim of homogenization is to achieve a z-average particle size of ≦200 nm. Below is an example of using an IKA® HPH 2000 / 5 high pressure homogenizer to prepare the miniemulsion.
[0142] The following ingredients are added to a sealable container and mixed on an orbital shaker. Silicone resin B1 260.00g Butyl acrylate 250.40g Methyl methacrylate 202.88g Hexadecane 3.51g Total 716.79g
[0143] The resulting mixture is combined with the solutions of the following ingredients and mixed on an orbital shaker for approximately 1 hour. Sodium dodecyl sulfate (SDS) 24.44g Hydroquinone Monomethyl Ether (2% aqueous solution) 3.77g 455.00g deionized water
[0144] The following ingredients are added to the above mixture in 20 g portions over 1 hour and mixed on an orbital shaker until a stable pre-emulsion is formed. 2-Hydroxyethyl methacrylate (HEMA) 100.00g Total 1300.00g
[0145] The pre-emulsion is passed through a high-pressure homogenizer at a pressure of 400-800 bar to obtain a mini-emulsion with a z-average particle size of 101 nm (PDI = 0.16).
[0146] Step 2: Polymerization A 3 L polymerization vessel equipped with an anchor stirrer, reflux condenser, thermometer, and nitrogen inlet is charged with 0.108 g of ethylenediaminetetraacetic acid (EDTA) disodium salt, 0.108 g of ferric ammonium sulfate hexahydrate, 250.17 g of deionized water, and 72 g of the miniemulsion prepared in step 1 as an initial charge and heated to 50° C. In one sealable vessel (feed 1), a solution of 4.62 g of tertiary butyl hydroperoxide (TBHP) in 38.58 g of deionized water is prepared. In a second sealable vessel (feed 2), a solution of 2.31 g of formaldehyde-free reducing agent (Bruggolite® FF6 M) in 43.86 g of deionized water is prepared. In a third vessel (feed 3), 828 g of miniemulsion is placed. Feeds 1 and 2 are started at a rate of 230 μL / min followed by feed 3 at a rate of 5.0 mL / min and are metered continuously over 165 minutes. Feeds 1 and 2 are continued for an additional 40 minutes after the end of feed 3, after which the reaction is held at 50° C. for an additional 90 minutes. After cooling to room temperature, the product is adjusted to pH 8 with aqueous ammonia and filtered through a 100 μm filter to give a dispersion with the following characteristics: Specific gravity: 1.068, Glass transition temperature: 17.0℃, Solids: 42.97%, Total Residual Free Monomer: <200ppm Z-average particle size: 173nm (PDI=0.20)
[0147] [Example 2: Preparation of copolymer dispersion E2 from silicone resin B2]
[0148] Step 1: Preparation of miniemulsion A miniemulsion is prepared by dissolving the ethylenically unsaturated silicone resin B2 in a mixture of (meth)acrylic monomers (the monomer combination includes 2-hydroxyethyl methacrylate, which has a hydroxy group in addition to the radically polymerizable methyl methacrylate group) and then homogenizing at high pressure. The aim of homogenization is to achieve a z-average particle size of ≦200 nm. Below is an example of the preparation of a miniemulsion using an IKA® HPH 2000 / 5 high pressure homogenizer.
[0149] Preparation of Silicone Resin and (Meth)Acrylate Monomer Mixture: The following ingredients are added to a sealable container and mixed on an orbital shaker. Silicone resin in 2-EHA (B2) 364.40g Butyl acrylate 150.00g Methyl methacrylate 198.88g Hexadecane 3.51g Total 716.79g
[0150] The resulting mixture is combined with the solutions of the following ingredients and mixed on an orbital shaker for approximately 1 hour. Sodium dodecyl sulfate (SDS) 24.44g Hydroquinone Monomethyl Ether (2% aqueous solution) 3.77g 455.00g deionized water
[0151] The following ingredients are added to the above mixture in 20 g portions over 1 hour and mixed on an orbital shaker until a stable pre-emulsion is formed. 2-Hydroxyethyl methacrylate 100.00g Total 1300.00g
[0152] The pre-emulsion is passed through a high-pressure homogenizer at a pressure of 400-800 bar to produce a mini-emulsion with a z-average particle size of 130 nm (PDI = 0.11).
[0153] Step 2: Polymerization A 3 L polymerization vessel equipped with an anchor stirrer, reflux condenser, thermometer, and nitrogen inlet is charged with 0.108 g of ethylenediaminetetraacetic acid (EDTA) disodium salt, 0.108 g of ferric ammonium sulfate hexahydrate, 250.17 g of deionized water, and 72 g of the miniemulsion prepared in step 1 as an initial charge and heated to 50° C. In one sealable vessel (feed 1), a solution of 4.62 g of tertiary butyl hydroperoxide (TBHP) in 38.58 g of deionized water is prepared. In a second sealable vessel (feed 2), a solution of 2.31 g of formaldehyde-free reducing agent (Bruggolite® FF6 M) in 43.86 g of deionized water is prepared. In a third vessel (feed 3), 828 g of miniemulsion is placed. Feeds 1 and 2 are started at a rate of 230 μL / min, followed by feed 3 at a rate of 5.0 mL / min and metered continuously for 165 minutes. Feeds 1 and 2 are continued for an additional 40 minutes after the end of feed 3, after which the reaction is held at 50° C. for an additional 90 minutes. After cooling to room temperature, the product is adjusted to pH 8 with aqueous ammonia and filtered through a 100 μm filter to give a dispersion with the following characteristics: Specific gravity: 1.058, Glass transition temperature: 16.5℃, Solids: 45.14%, Total Residual Free Monomer: <200ppm Z-average particle size: 173nm (PDI=0.20)
[0154] Comparative Example 1: Preparation of copolymer dispersion CE1 from ethylenically unsaturated phenyl silicone resin CB1
[0155] Step 1: Preparation of miniemulsion A miniemulsion is prepared by dissolving the ethylenically unsaturated silicone resin CB1 in a mixture of (meth)acrylic monomers (the monomer combination does not include 2-hydroxyethyl methacrylate) followed by homogenization at high pressure. The aim of homogenization is to achieve a z-average particle size of ≦200 nm. Below is an example of using an IKA® HPH 2000 / 5 high pressure homogenizer to prepare a miniemulsion.
[0156] Preparation of Silicone Resin and (Meth)Acrylate Monomer Mixture: The following ingredients are added to a sealable container and mixed on an orbital shaker. Silicone resin CB1 260.00g Butyl acrylate 253.24g Methyl methacrylate 170.30g Butyl methacrylate 74.64g Styrene 42.57g Methacrylic acid 11.61g Hexadecane 3.87g Total 816.23g
[0157] The resulting mixture is combined with the solutions of the following ingredients and mixed on an orbital shaker for approximately 1 hour until a stable pre-emulsion is formed. Sodium dodecyl sulfate (SDS) 24.44g Hydroquinone Monomethyl Ether (2% aqueous solution) 3.77g 455.00g deionized water Total 1300.00g
[0158] The pre-emulsion is passed through a high-pressure homogenizer at a pressure of 400-800 bar to produce a mini-emulsion with a z-average particle size of 156 nm (PDI = 0.16).
[0159] Step 2: Polymerization A 3 L polymerization vessel equipped with an anchor stirrer, reflux condenser, thermometer and nitrogen inlet is charged with 250.17 g of deionized water and 72 g of the miniemulsion prepared in step 1 as an initial charge and heated to 50° C. In one sealable vessel (feed 1), a solution of 4.62 g of tertiary butyl hydroperoxide (TBHP) in 38.34 g of deionized water is prepared. In a second sealable vessel (feed 2), a solution of 2.31 g of formaldehyde-free reducing agent (Bruggolite® FF6 M) in 43.86 g of deionized water is prepared. In a third vessel (feed 3), 828 g of miniemulsion is placed. Feeds 1 and 2 are started at a rate of 230 μL / min, followed by feed 3 at a rate of 5.0 mL / min, and are metered continuously over a period of 165 minutes. Feeds 1 and 2 are continued for an additional 45 minutes after the end of Feed 3, after which the reaction is held at 50° C. for an additional 90 minutes. After cooling to room temperature, the product is adjusted to pH 8 with aqueous ammonia and filtered through a 100 μm filter to give a dispersion having the following characteristics: Specific gravity: 1.070, Glass transition temperature: 17.0℃, Solids: 46.58%, Total Residual Free Monomer: <300ppm Z-average particle size: 151nm (PDI=0.18)
[0160] Comparative Example 2: Preparation of copolymer dispersion CE2 from ethylenically unsaturated phenyl silicone resin CB2
[0161] Step 1: Preparation of miniemulsion The miniemulsion is prepared by dissolving the silicone resin in a mixture of (meth)acrylic monomers (the monomer combination does not include 2-hydroxyethyl methacrylate) and then homogenizing at high pressure. The aim of homogenization is to achieve a z-average particle size of ≦200 nm. Below is an example of using an IKA® HPH 2000 / 5 high pressure homogenizer to prepare the miniemulsion.
[0162] The following ingredients are added to a sealable container and mixed on an orbital shaker. Silicone resin CB2 154.74g Butyl acrylate 306.29g Methyl methacrylate 350.32g Hexadecane 5.45g Total 816.80g
[0163] The resulting mixture is combined with the solutions of the following ingredients and mixed on an orbital shaker for approximately 1 hour until a stable pre-emulsion is formed. Sodium dodecyl sulfate (SDS) 24.46g Hydroquinone Monomethyl Ether (2% aqueous solution) 3.74g 455.00g deionized water Total 1300.00g
[0164] The pre-emulsion is passed through a high-pressure homogenizer at a pressure of 400-800 bar to produce a mini-emulsion with an average particle size of 206 nm (PDI = 0.22).
[0165] Step 2: Polymerization A 3 L polymerization vessel equipped with an anchor stirrer, reflux condenser, thermometer and nitrogen inlet is charged with 0.108 g of ethylenediaminetetraacetic acid (EDTA) disodium salt, 0.108 g of ferric ammonium sulfate hexahydrate, 250.17 g of deionized water and 72 g of the miniemulsion prepared in step 1 as an initial charge and heated to 50° C. In one sealable vessel (Feed 1), a solution of 4.62 g of tertiary butyl hydroperoxide (TBHP) in 38.58 g of deionized water is prepared. In a second sealable vessel (Feed 2), a solution of 2.31 g of formaldehyde-free reducing agent (Bruggolite® FF6 M) in 43.86 g of deionized water is prepared. In a third vessel (Feed 3), 828 g of miniemulsion is placed. Feeds 1 and 2 are started at a rate of 230 μL / min, followed by feed 3 at a rate of 5.0 mL / min and metered continuously for 165 minutes. Feeds 1 and 2 are continued for an additional 40 minutes after the end of feed 3, after which the reaction is held at 50° C. for an additional 90 minutes. After cooling to room temperature, the product is adjusted to pH 8 with aqueous ammonia and filtered through a 100 μm filter to give a dispersion with the following characteristics: Specific gravity: 1.054, Glass transition temperature: 11.7℃, Solids: 45.44%, Total Residual Free Monomer: <100ppm Z-average particle size: 131nm (PDI=0.16)
[0166] <Application in industrial coating formulations> The copolymer dispersions were used in industrial water-based coating formulations containing the polyisocyanate-based hardener Bayhydur® XP 2547 (a polyisocyanate based on hexamethylene diisocyanate, available from Covestro). In a typical formulation, the isocyanate hardener was mixed with the copolymer dispersion using a Cowles blade at 1000 rpm for approximately 30 seconds. After application of the formulations using a bird bar to aluminum Q-panels, the films (between approximately 23 and 27 μm dry thickness) were evaluated at room temperature and 50-55% relative humidity. The durability of the films was measured after one week using the MEK double rub test (ASTM D5402). The higher the value, the more durable the film. The formulation composition and test results are shown in Table 1.
[0167] [Table 1]
[0168] According to Table 1, formulations F1 and F2 of inventive dispersions E1 and E2 based on inventive copolymers having crosslinkable HO functionality (due to the use of 2-hydroxyethyl methacrylate as monomer (C)) showed better MEK double rub test values compared to formulations C1 and C2 of non-inventive dispersions CE1 and CE2 based on non-inventive copolymers not having crosslinkable HO functionality (without using 2-hydroxyethyl methacrylate), which indicates good durability of films formed from copolymer dispersions having reactive functional groups that form crosslinks with the isocyanate groups of the curing agent during curing.
[0169] The non-inventive copolymer of the non-inventive dispersion CE1 does not have crosslinkable HO functional groups (no 2-hydroxyethyl methacrylate is used), but does contain small amounts of crosslinkable functional groups (-COOH) because a small amount of 2.1% by weight of methacrylic acid was used, based on the ethylenically unsaturated monomer (A), by free radical polymerization. These small amounts of crosslinkable functional groups do not lead to crosslinking with the isocyanate groups of the curing agent.
Claims
1. 1. A process for preparing an aqueous dispersion of a crosslinkable reactive silicone-organic copolymer of an ethylenically unsaturated monomer and an ethylenically functionalized silicone resin, comprising the steps of: (A) in an aqueous medium of one or more (meth)acrylic acid ester monomers, (B) in the presence of at least one silicone resin functionalized with ethylenically unsaturated radically polymerizable groups and consisting of siloxane units of the general formula: [R 1 p (OR 2 ) z SiO (4-p-z)/2 ] (I)、 [In the formula, R 1 is in each case identical or different and is a group R* or E, in which R*, which is the same or different in each occurrence, is a hydrogen atom or an optionally substituted hydrocarbon group which does not contain multiple aliphatic C-C bonds and has 1 to 18 carbon atoms; E is a group represented by the formula -(CR 5 2 ) m -X is an ethylenically unsaturated group, m is an integer from 1 to 10, R 2 is the same or different in each occurrence and is a hydrogen atom or a hydrocarbon radical having 1 to 18 carbon atoms, R 5 is a hydrogen atom, C 1 ~C 12 Alkyl group or C 6 ~C 18 is an aryl group, X is an ethylenically unsaturated organic group; R 1 is an ethylenically unsaturated group E in at least 1 mol % and at most 50 mol % of all siloxane units (I), p is 0, 1, 2 or 3; z is 0, 1, 2 or 3; where the sum p+z has a value of 0, 1, 2 or 3; provided that for at least 20 mol % of all siloxane units of formula (I) in silicone resin (B), the sum p+z is 1 or 0, p is 1 or 0, and z is 0; and (C) in the presence of at least one compound having an ethylenically unsaturated group and at least one additional functional group that is not free radically polymerizable but is capable of crosslinking, in an amount of 6 to 50% by weight, based on the total weight of (A); The aqueous dispersion is prepared by radical initiated miniemulsion polymerization; the proportion of (B) being 5 to 70% by weight, based on the total weight of (A), (C) and the functionalized silicone resin (B); In a first step, a solution of at least one silicone resin (B) is prepared in one or more (meth)acrylic acid esters (A) to obtain a silicone inmonomer solution, In a second step, the silicone monomer solution obtained is emulsified in water with an emulsifier, optionally a hydrophobic co-emulsifier, and optionally a polymerization inhibitor to prevent premature radical emulsion polymerization, in such a way as to give a miniemulsion with a particle size D(50) of less than or equal to 350 nm; provided that compound (C) is added during the preparation of the silicone monomer solution in the first step or during the emulsification to form a mini-emulsion in the second step; A process in which in a third step the miniemulsion obtained is subjected to a radical emulsion polymerization, wherein the miniemulsion polymerization is carried out using a water-soluble polymerization initiator or an oil-soluble polymerization initiator or a mixture of a water-soluble polymerization initiator and an oil-soluble polymerization initiator.
2. E is a group represented by the formula -(CH 2 ) 3 2. The method of claim 1, characterized in that the moiety is a group of formula -X, where X is an ethylenically unsaturated organic group.
3. 3. The method according to claim 1, wherein X is an acrylic or methacrylic group.
4. 4. The method of claim 1, 2 or 3, characterized in that the sum p + z is 1 or 0, p is 1 or 0, and z is 0 for at least 30 mol % of all siloxane units of formula (I) in silicone resin (B).
5. 5. The process according to claim 1, characterized in that the group R* is at least two different groups selected from the group of carbon-rich hydrocarbon groups having 6 to 18 carbon atoms and carbon-poor groups having 1 to 3 carbon atoms.
6. The process according to any one of claims 1 to 5, characterized in that the compound (C) is a monomer selected from the group consisting of: - ethylenically unsaturated alcohols, - ethylenically unsaturated mono- and dicarboxylic acids and their salts, - ethylenically unsaturated sulfonic acids and their salts, - ethylenically unsaturated primary, secondary or tertiary amines, - ethylenically unsaturated amides, - ethylenically unsaturated phosphonic acids and their salts, - ethylenically unsaturated epoxides, - ethylenically unsaturated isocyanates, - ethylenically unsaturated anhydrides, - ethylenically unsaturated monomers containing reactive carbonyl groups, and - ethylenically unsaturated organosilanes containing reactive groups.
7. (1) an aqueous dispersion of a crosslinkable reactive silicone-organic copolymer prepared as described in any one of claims 1 to 6 having crosslinkable functional groups; and (2) Crosslinking agent A method for producing a crosslinkable composition by mixing
8. (1) an aqueous dispersion of a crosslinkable reactive silicone-organic copolymer prepared as described in any one of claims 1 to 6, which has a functional group capable of reacting with an isocyanate group to crosslink; and (2) An organic compound having two or more isocyanate groups as a crosslinking agent 8. The method of claim 7, wherein the crosslinkable composition is prepared by mixing:
9. 9. A method for forming a film on a substrate by applying crosslinkable compositions prepared as claimed in claim 7 or 8 to the substrate and then allowing them to crosslink.
10. A method for forming a film on a substrate by applying an aqueous dispersion of a crosslinkable reactive silicone-organic copolymer having functional groups capable of crosslinking by reaction with itself, prepared as described in any one of claims 1 to 6, and then allowing them to crosslink.
Citation Information
Patent Citations
Coating composition
EP0352339A1
Silicone / organic copolymer emulsions
EP0771826A2
Silicone resin-containing emulsion compositions, their preparation, use and corresponding products
EP0943634A1
Hydrophobically modified copolymers
EP1308468A1
Graft copolymer, its production and coating composition consisting essentially of same copolymer
JP1991281516A