Electromagnetic wave shielding composition, electromagnetic wave shielding sheet, electromagnetic wave shielding sintered body, and electronic component device
The use of metal particles with varying melting points and transitional liquid phase sintering in an electromagnetic shielding composition addresses the limitations of conventional materials, resulting in a sintered body with enhanced electromagnetic shielding and conductivity for electronic components.
Patent Information
- Application Number
- JP2020035275
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-02
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-03-02
AI Technical Summary
Conventional electromagnetic shielding materials face challenges in reducing volume resistivity, as using flat metal particles has limitations, and increasing the amount of metal particles also has constraints, making it difficult to achieve desired electromagnetic shielding properties.
A composition utilizing metal particles A, B, and C with varying melting points, enabling transitional liquid phase sintering to form a sintered body with improved electrical conductivity and reduced volume resistivity, comprising Cu, Sn, and optionally Bi, In, Zn, Cd, or Cu alloy particles, with specific ratios and particle sizes.
The composition forms a sintered body with excellent electromagnetic shielding effects, achieving lower volume resistivity and superior conductivity, suitable for electronic component devices.
Smart Images

Figure 0007559330000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electromagnetic wave shielding composition, an electromagnetic wave shielding sheet, an electromagnetic wave shielding sintered body, and an electronic component device. [Background technology]
[0002] When unwanted external electromagnetic waves enter electronic devices, they can malfunction. Therefore, electromagnetic shielding materials are used in electronic devices to block unwanted external electromagnetic waves.
[0003] Many electromagnetic wave shielding materials are made of metal and shield electronic devices from electromagnetic waves by reflecting them.
[0004] Conventional electromagnetic wave shielding materials include metal plating, metal housings, metal paints, etc. However, metal plating takes a long time to process and tends to be expensive. In addition, as electronic devices become smaller, metal housings need to be made smaller, and processing metal housings tends to be difficult.
[0005] On the other hand, metal paint contains metal particles, resin, and solvent, and conducts electricity through contact between the metal particles. The lower the volume resistivity of a coating film formed with a metal paint, the more the coating film tends to improve its electromagnetic wave shielding properties. Therefore, it is desirable to use flat metal particles to increase the contact points between the metal particles and reduce the volume resistivity of the coating film (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-150837 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, even if flat metal particles are used, there is a limit to how much the volume resistivity of the coating film can be reduced. Another method for reducing the volume resistivity of the coating film is to increase the amount of metal particles added to increase the number of contacts between the metal particles, but there is a limit to the amount of metal particles that can be added, and it may be difficult to achieve the required characteristics.
[0008] The present disclosure has been made in consideration of the above-mentioned conventional circumstances, and has an object to provide an electromagnetic shielding composition capable of forming an electromagnetic shielding sintered body having excellent electromagnetic shielding effect, as well as an electromagnetic shielding sheet, an electromagnetic shielding sintered body, and an electronic component device that use this electromagnetic shielding composition. [Means for solving the problem]
[0009] Specific means for achieving the above object are as follows. <1> An electromagnetic wave shielding composition comprising metal particles A, metal particles B having a melting point lower than that of metal particles A, metal particles C which are alloy particles containing a metal component contained in metal particles B and having a melting point lower than that of metal particles B, and a resin, wherein transitional liquid phase sintering is possible between metal particles A, metal particles B, and metal particles C. <2> The melting point of the metal particles B is 300° C. or less. <1> Electromagnetic wave shielding composition according to claim 1. <3> The metal particles A contain Cu, the metal particles B contain Sn, and the metal particles C contain Sn. <1> or <2> Electromagnetic wave shielding composition according to claim 1. <4> The ratio of the Cu content to the Sn content (Cu content / Sn content) based on mass of the metal particles A, the metal particles B and the metal particles C as a whole is 0.25 to 0.70. <3> Electromagnetic wave shielding composition according to claim 1. <5> The metal particles C contain at least one metal component X selected from the group consisting of Bi, In, Zn, Cd, Pb, Ag, and Cu. <1> ~ <4> 13. The electromagnetic wave shielding composition according to claim 12, <6> The proportion of the metal component X in the entire metal particles C is 3% by mass to 80% by mass. <5> Electromagnetic wave shielding composition according to claim 1. <7> The ratio of the metal particles B to the metal particles C (metal particles B / metal particles C) is 10 / 90 to 90 / 10 by mass. <1> ~ <6> 13. The electromagnetic wave shielding composition according to claim 12, <8> The average particle size of the metal particles A is 0.1 μm to 2 μm. <1> ~ <7> 13. The electromagnetic wave shielding composition according to claim 12,
[0010] <9> <1> ~ <8> 13. An electromagnetic wave shielding sheet having a resin composition layer containing the electromagnetic wave shielding composition according to any one of claims 1 to 12. <10> <1> ~ <8> or <9> 2. A sintered body for electromagnetic shielding, which is a sintered body of the electromagnetic shielding sheet according to claim 1. <11> <10> 2. An electronic component device having a region covered with the electromagnetic wave shielding sintered body according to claim 1. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide an electromagnetic shielding composition capable of forming an electromagnetic shielding sintered body having excellent electromagnetic shielding effect, as well as an electromagnetic shielding sheet, an electromagnetic shielding sintered body, and an electronic component device that use this electromagnetic shielding composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to the numerical values and their ranges, and do not limit the present disclosure.
[0013] In the present disclosure, a numerical range indicated using "~" includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of corresponding substances. When multiple substances corresponding to each component are present in the composition, the content of each component means the total content of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the particles corresponding to each component may include multiple types of particles. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In the present disclosure, the terms "layer" and "film" include cases where the layer or film is formed over the entire area when the area in which the layer or film is present is observed, as well as cases where the layer or film is formed over only a portion of the area. In the present disclosure, the average thickness of a layer or film is defined as the arithmetic mean value of thicknesses measured at five points on the layer or film of interest. The thickness of the layer or film can be measured using a micrometer or the like. In the present disclosure, when the thickness of the layer or film can be measured directly, it is measured using a micrometer. On the other hand, when the thickness of one layer or the total thickness of multiple layers is measured, it may be measured by observing the cross section of the measurement target using an electron microscope.
[0014] <Electromagnetic wave shielding composition> The electromagnetic shielding composition of the present disclosure contains metal particles A, metal particles B having a melting point lower than that of metal particles A, metal particles C which are alloy particles containing a metal component contained in metal particles B and having a melting point lower than that of metal particles B, and a resin, and is capable of transient liquid phase sintering between the metal particles A, the metal particles B, and the metal particles C. The electromagnetic shielding composition of the present disclosure may contain other components in addition to the above components.
[0015] According to the electromagnetic shielding composition of the present disclosure, a sintered body of metal particles A, B, and C can be formed by heating, utilizing the transition liquid phase sintering that occurs between metal particles A, B, and C. The formed sintered body tends to have lower interface resistance and better electrical conductivity than when metal particles are in contact with each other. As a result, it is presumed that the electromagnetic shielding sintered body formed using the electromagnetic shielding composition of the present disclosure has a low volume resistivity and a good electromagnetic shielding effect.
[0016] Furthermore, when the electromagnetic shielding composition contains metal particles C that are alloy particles, the volume resistivity may increase due to the metal components contained in the metal particles C. In the electromagnetic shielding composition of the present disclosure, the relative amount of metal particles C in the composition can be reduced by the amount of metal particles B contained therein. As a result, the increase in volume resistivity caused by the metal components contained in the metal particles C can be suppressed.
[0017] In the electromagnetic wave shielding composition of the present disclosure, transitional liquid phase sintering is possible between metal particles A, metal particles B, and metal particles C. In this disclosure, "transient liquid phase sintering" is also called Transient Liquid Phase Sintering (TLPS), and refers to a phenomenon in which a component with a relatively low melting point (low melting point component) among metals and alloys with different melting points transitions to a liquid phase by heating at the particle interface, and a component with a relatively high melting point (high melting point component) reacts and diffuses into the liquid phase, causing the formation of a metal compound (alloying) by both components. By utilizing this phenomenon, a sintered body that can be sintered at a low temperature and has a high melting point after sintering can be obtained. In the "transient liquid phase sintering" of the present disclosure, it is sufficient that at least some of the metal components contained in metal particles A, metal particles B, and metal particles C are sinterable, and it is not necessary that all of the metal components are sinterable. For example, metal particles C may contain a metal component, such as Bi, that does not contribute to the reaction during sintering.
[0018] In the electromagnetic shielding composition of the present disclosure, the melting points decrease in the order of metal particles A, metal particles B, and metal particles C. Therefore, for example, metal particles C, or metal particles B and metal particles C, which are components with a relatively low melting point, undergo transition to a liquid phase due to heating at the particle interface, and metal particles A and metal particles B, or metal particles A, which are components with a relatively high melting point, undergo reactive diffusion into the liquid phase, resulting in transient liquid phase sintering.
[0019] The components constituting the electromagnetic shielding composition of the present disclosure will be described in detail below.
[0020] (metal particles) The electromagnetic wave shielding composition of the present disclosure contains metal particles A, metal particles B having a melting point lower than that of metal particles A, and metal particles C which are alloy particles containing the metal components contained in metal particles B and having a melting point lower than that of metal particles B. The metal components contained in metal particles A, metal particles B, and metal particles C are not particularly limited as long as metal particles A, metal particles B, and metal particles C satisfy the above-mentioned conditions and are metal components that enable transitional liquid phase sintering between metal particles A, metal particles B, and metal particles C.
[0021] There is no particular limitation on the specific form of the metal particles A and the metal particles B. For example, the metal particles A and the metal particles B may each be in a state of a simple metal, or one or both of the metal particles A and the metal particles B may be in a state of an alloy. In addition, there is no particular limitation on the specific form of the metal particles C, so long as they are alloy particles. In a preferred embodiment, metal particle B is in a simple metal state, and metal particle C is in a state of an alloy of the metal contained in metal particle B and another metal such as metal component X described below. In a more preferred embodiment, metal particle A and metal particle B are in a simple metal state, and metal particle C is in a state of an alloy of the metal contained in metal particle B and another metal such as metal component X described below.
[0022] The metal particles A are preferably metal particles containing at least one selected from the group consisting of Cu, Au, Ag, Co, Ni and Fe. The metal particles B are preferably metal particles containing at least one selected from the group consisting of Sn, Zn, and In. The metal particles C are preferably alloy particles containing at least one selected from the group consisting of Sn, Zn and In as the metal component contained in the metal particles B, and a metal component X described below. In addition, when the metal component X contains In, the metal particles B are preferably metal particles that do not contain In and contain at least one of Sn and Zn, and the metal particles C are preferably metal particles that contain, together with the metal component X, at least one of Sn and Zn as a metal component contained in the metal particles B. Furthermore, when the metal component X contains Zn, the metal particles B are preferably metal particles that do not contain Zn and contain at least one of Sn and In, and the metal particles C are preferably metal particles that contain, in addition to the metal component X, at least one of Sn and In as a metal component contained in the metal particles B.
[0023] Examples of combinations of metal particles A, metal particles B having a melting point lower than that of metal particles A, and metal particles C having a melting point lower than that of metal particles B (metal particles A, metal particles B, metal particles C) include (metal particles containing Cu, metal particles containing Sn, metal particles containing Sn), (metal particles containing Cu, metal particles containing Zn, metal particles containing Zn), (metal particles containing Au, metal particles containing In, metal particles containing In), (metal particles containing Co, metal particles containing Sn, metal particles containing Sn), (metal particles containing Ni, metal particles containing Sn, metal particles containing Sn), and (metal particles containing Cu, metal particles containing Sn, metal particles containing Bi). Among these, a configuration in which metal particles A contain Cu, metal particles B contain Sn, and metal particles C contain Bi is preferred.
[0024] From the viewpoint of bonding strength after sintering, the melting point of the metal particles A is preferably higher than 300° C., more preferably higher than 500° C., and even more preferably higher than 800° C. The electromagnetic shielding composition of the present disclosure may contain two or more types of metal particles A, for example, two or more types of metal particles A each having a melting point higher than 300° C.
[0025] From the viewpoint of promoting the transition to a liquid phase during sintering, the melting point of metal particles B is preferably 300° C. or lower, more preferably 270° C. or lower, and even more preferably 250° C. or lower. The electromagnetic shielding composition of the present disclosure may contain two or more types of metal particles B, for example, two or more types of metal particles B each having a melting point of 300° C. or lower.
[0026] The melting point of the metal particles C is not particularly limited as long as it is lower than the melting point of the metal particles B, and from the viewpoint of promoting the transition to a liquid phase during sintering, it is preferably 250° C. or lower, more preferably 200° C. or lower, and even more preferably 150° C. or lower. The electromagnetic shielding composition of the present disclosure may contain two or more types of metal particles C, for example, two or more types of metal particles C each having a melting point of 250° C. or lower.
[0027] From the viewpoint of lowering the temperature at which transitional liquid phase sintering is possible, the metal particles C preferably contain at least one metal component X selected from the group consisting of Bi, In, Zn, Cd, Pb, Ag, and Cu, and more preferably contain a metal component other than the metal component X as a metal component contained in the metal particles B, and further preferably contain Sn as a metal component contained in the metal particles B, and contain the metal component X. Moreover, from the viewpoint of suitably lowering the volume resistivity of the electromagnetic wave shielding sintered compact, it is preferable that the metal particles B do not contain the metal component X.
[0028] The metal component X more preferably contains at least one selected from the group consisting of Bi, In, Zn, Cd, Ag, and Cu, and from the viewpoint of further lowering the temperature at which transient liquid phase sintering is possible, it is even more preferable that the metal component X contains at least one selected from the group consisting of Bi, In, Zn, and Cd.
[0029] From the viewpoint of lowering the temperature at which transitional liquid phase sintering is possible and from the viewpoint of suitably lowering the volume resistivity of the electromagnetic shielding sintered body, the proportion of the metal component X in the entire metal particles C is preferably 3 mass % to 80 mass %, more preferably 5 mass % to 15 mass %, 20 mass % to 30 mass %, or 50 mass % to 60 mass %.
[0030] In one embodiment, it is preferred that metal particles A are Cu (melting point: 1085°C) particles, metal particles B are Sn (melting point: 232°C) particles, and metal particles C are an alloy containing Sn (melting point: less than 232°C, for example, 138°C). Cu and Sn produce a copper-tin metal compound (Cu6Sn5) by sintering. This reaction proceeds at around 150°C, so sintering can be performed using general equipment such as a reflow furnace.
[0031] Examples of the metal particles C in the state of an alloy containing Sn include SnBi alloy, SnIn alloy, SnZn alloy, SnPb alloy, SnCd alloy, etc. Among them, SnBi alloy is preferable from the viewpoint of lowering the temperature at which transitional liquid phase sintering is possible. When SnBi alloy is used, Bi does not contribute to the reaction during sintering, so the volume resistivity of the sintered body for electromagnetic shielding tends to increase. On the other hand, in the electromagnetic shielding composition of the present disclosure, the relative amount of Bi in the composition can be reduced by using Sn as metal particles B together with SnBi alloy, so that the increase in volume resistivity caused by Bi tends to be suppressed favorably.
[0032] The composition of the SnBi alloy is not particularly limited, and an example thereof is Sn-Bi58, which is an alloy containing Sn and containing 58 mass% of element Bi. The melting point (liquid phase transition temperature) of the alloy represented by Sn-Bi58 is about 138°C.
[0033] When metal particles A contain Cu, metal particles B contain Sn, and metal particles C contain Sn, the ratio of the Cu content to the Sn content (Cu content / Sn content) on a mass basis in metal particles A, metal particles B, and metal particles C as a whole is preferably 0.25 to 0.70, more preferably 0.30 to 0.60, and even more preferably 0.40 to 0.50, from the viewpoints of volume resistivity and volume shrinkage.
[0034] The proportion of metal particles A in the total of metal particles A, metal particles B and metal particles C is preferably 10% by mass to 30% by mass, and more preferably 15% by mass to 25% by mass.
[0035] The ratio of metal particles B to metal particles C (metal particles B / metal particles C) is preferably 10 / 90 to 90 / 10 by mass, more preferably 20 / 80 to 80 / 20, and even more preferably 30 / 70 to 70 / 30. When metal particles B / metal particles C is 10 / 90 or more, the volume resistivity of the electromagnetic shielding sintered compact tends to be suitably reduced. When metal particles B / metal particles C is 90 / 10 or less, the temperature at which transient liquid phase sintering is possible tends to be reduced.
[0036] Metal particles A and metal particles B may each be composed of only one type of metal or two or more types of metals. When metal particles A or metal particles B are composed of two or more types of metals, the metal particles may be a combination (mixture) of metal particles containing each of the two or more types of metals, or the two or more types of metals may be contained in the same metal particle, or a combination thereof.
[0037] The configuration of metal particles containing two or more kinds of metals in the same metal particle is not particularly limited. For example, metal particles may be made of an alloy of two or more kinds of metals, or may be made of two or more kinds of simple metals. Metal particles consisting of two or more simple metals can be obtained, for example, by forming a layer containing one metal on the surface of a metal particle containing the other metal by plating, deposition, or the like. In addition, metal particles containing two or more kinds of metals in the same metal particle can also be obtained by a method in which a particle containing one metal is applied to the surface of a metal particle containing one metal in a dry manner using a force mainly consisting of an impact force in a high-speed airflow to combine the two.
[0038] The average particle size of the metal particles A, metal particles B, and metal particles C is not particularly limited.
[0039] For example, the average particle size of the metal particles A is preferably 0.05 μm to 10 μm, more preferably 0.1 μm to 2 μm, and even more preferably 0.15 μm to 1 μm. In particular, when the average particle size of the metal particles A is 2 μm or less, the amount of the metal particles A that is not liquid phase sintered after the transient liquid phase sintering can be reduced, and as a result, the volume resistivity of the electromagnetic shielding sintered compact tends to be suitably reduced.
[0040] The average particle size of the metal particles B is preferably from 0.01 μm to 4 μm, and more preferably from 0.05 μm to 1 μm or from 2 μm to 3 μm, from the viewpoint of the metal filling rate.
[0041] The average particle size of the metal particles C is preferably from 0.01 μm to 4 μm, and more preferably from 0.05 μm to 1 μm or from 2 μm to 3 μm, from the viewpoint of the metal filling rate.
[0042] In the present disclosure, the average particle size of metal particles refers to the volume average particle size measured by a laser diffraction particle size distribution analyzer (for example, Beckman Coulter, Inc., LS 13 320 type laser scattering diffraction particle size distribution analyzer). Specifically, metal particles are added in the range of 0.01% by mass to 0.3% by mass to 125 g of a solvent (terpineol) to prepare a dispersion. Approximately 100 ml of this dispersion is poured into a cell and measured at 25°C. The particle size distribution is measured with the refractive index of the solvent set to 1.48.
[0043] The total content of metal particles A, metal particles B, and metal particles C in the electromagnetic shielding composition is not particularly limited. For example, the total mass ratio of metal particles A, metal particles B, and metal particles C to the entire solid content of the electromagnetic shielding composition is preferably 96 mass% or less, more preferably 95 mass% or less, and even more preferably 94 mass% or less. Furthermore, the total mass ratio of metal particles A, metal particles B, and metal particles C to the entire solid content of the electromagnetic shielding composition may be 65 mass% or more.
[0044] (resin) The electromagnetic shielding composition of the present disclosure contains a resin. When the electromagnetic shielding composition contains a resin, voids in the sintered body of metal particles A, metal particles B, and metal particles C are filled with the resin, which tends to improve stress relaxation properties and adhesive strength.
[0045] The resin contained in the electromagnetic wave shielding composition may be a thermoplastic resin, a thermosetting resin, or a combination of these. In addition, the resin may be in the form of a monomer having a functional group capable of undergoing a polymerization reaction by heating, or in the form of an already polymerized polymer.
[0046] From the viewpoint of heat resistance, the electromagnetic shielding composition preferably contains a thermosetting resin as the resin, such as a resin having a functional group, such as an epoxy group, an acryloyl group, a methacryloyl group, a hydroxyl group, a vinyl group, a carboxyl group, an amino group, a maleimide group, an acid anhydride group, a thiol group, or a thionyl group.
[0047] Specific examples of the thermosetting resin include epoxy resins, oxazine resins, bismaleimide resins, phenol resins, unsaturated polyester resins, silicone resins, etc. Among these, epoxy resins are preferred.
[0048] Specific examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, naphthalene type epoxy resins, biphenol type epoxy resins, biphenyl novolac type epoxy resins, and cyclic aliphatic epoxy resins. The resins may be used alone or in combination of two or more.
[0049] The content of the resin in the electromagnetic shielding composition is not particularly limited. For example, the proportion of the resin in the total solid content of the electromagnetic shielding composition is preferably 0.1 mass % to 10 mass %, more preferably 0.5 mass % to 6 mass %, and even more preferably 1 mass % to 5 mass %. Furthermore, the proportion of the resin in the solid content of the electromagnetic shielding composition excluding metal particles A, metal particles B, and metal particles C is preferably 5 mass% to 50 mass%, more preferably 7 mass% to 30 mass%, and even more preferably 10 mass% to 20 mass%.
[0050] (hardening agent) When the resin is a thermosetting resin, the electromagnetic wave shielding composition may contain a curing agent that cures the thermosetting resin. The type of the curing agent is not particularly limited, and is appropriately selected depending on the type of the thermosetting resin.
[0051] When the thermosetting resin is an epoxy resin, the curing agent may be an amine-based curing agent, a phenol-based curing agent, an acid anhydride-based curing agent, etc. The curing agent may be either liquid or solid. The curing agent may be used alone or in combination of two or more kinds.
[0052] Examples of the amine-based curing agent include chain aliphatic amines, cyclic aliphatic amines, aliphatic aromatic amines, and aromatic amines. Specific examples of the amine-based curing agent include aromatic amine curing agents having one aromatic ring, such as m-phenylenediamine, 1,3-diaminotoluene, 1,4-diaminotoluene, 2,4-diaminotoluene, 3,5-diethyl-2,4-diaminotoluene, 3,5-diethyl-2,6-diaminotoluene, and 2,4-diaminoanisole; 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 4,4'-methylenebis(2-ethylaniline), 3,3'-diethyl-4,4'-diaminodiphenylmethane, and 3, Examples of such curing agents include aromatic amine curing agents having two aromatic rings, such as 3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane and 3,3',5,5'-tetraethyl-4,4'-diaminodiphenylmethane; hydrolysis condensates of aromatic amine curing agents; aromatic amine curing agents having a polyether structure, such as polytetramethylene oxide di-p-aminobenzoate and polytetramethylene oxide di-p-aminobenzoate; condensation products of aromatic diamines and epichlorohydrin; and reaction products of aromatic diamines and styrene.
[0053] Examples of acid anhydride curing agents include phthalic anhydride, maleic anhydride, methyl himic anhydride, himic anhydride, succinic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, chlorendic anhydride, methyl tetrahydrophthalic anhydride, 3-methylhexahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, trialkyl tetrahydrophthalic anhydride maleic anhydride adduct, benzophenone tetracarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, hydrogenated methyl nadic anhydride, trialkyl tetrahydrophthalic anhydride having multiple alkyl groups obtained by Diels-Alder reaction from maleic anhydride and diene compounds, and various cyclic acid anhydrides such as dodecenyl succinic anhydride.
[0054] Examples of the phenol-based curing agent include novolak resins obtained by condensing or co-condensing at least one selected from the group consisting of phenol compounds (e.g., phenol, cresol, xylenol, resorcin, catechol, bisphenol A, and bisphenol F) and naphthol compounds (e.g., α-naphthol, β-naphthol, and dihydroxynaphthalene) with an aldehyde compound (e.g., formaldehyde, acetaldehyde, propionaldehyde, benzaldehyde, and salicylaldehyde) under an acid catalyst; phenol-aralkyl resins; biphenyl-aralkyl resins; naphthol-aralkyl resins; and the like.
[0055] The ratio of the equivalent number of the functional group of the curing agent (for example, an amino group in the case of an amine-based curing agent, a phenolic hydroxyl group in the case of a phenol-based curing agent, and an acid anhydride group in the case of an acid anhydride-based curing agent) to the equivalent number of the epoxy resin (equivalent number of curing agent / equivalent number of epoxy resin) is preferably set in the range of 0.6 to 1.4, more preferably in the range of 0.7 to 1.3, and even more preferably in the range of 0.8 to 1.2.
[0056] (Cure accelerator) When the electromagnetic shielding composition contains a thermosetting resin, the electromagnetic shielding composition may contain a curing accelerator that accelerates the curing reaction of the thermosetting resin or the curing reaction between the thermosetting resin and a curing agent. The type of curing accelerator is not particularly limited, and is appropriately selected depending on the types of thermosetting resin and curing agent.
[0057] Specific examples of the curing accelerator include cycloamidine compounds such as 1,8-diaza-bicyclo[5.4.0]undecene-7, 1,5-diaza-bicyclo[4.3.0]nonene, and 5,6-dibutylamino-1,8-diaza-bicyclo[5.4.0]undecene-7; compounds having intramolecular polarization obtained by adding a compound having a π bond such as maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone to a cycloamidine compound; compounds having intramolecular polarization obtained by adding a compound having a π bond such as diazophenylmethane and a phenol resin to a cycloamidine compound; benzyldimethylamine, triethanolamine, and the like. Examples of the curing accelerator include tertiary amine compounds such as dimethylamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; derivatives of tertiary amine compounds; imidazole compounds such as imidazole, 2-methylimidazole, 2-phenylimidazole, and 2-phenyl-4-methylimidazole; derivatives of imidazole compounds; tetraphenylborate salts such as tetraphenylphosphonium tetraphenylborate, triphenylphosphonium tetraphenylborate, 2-ethyl-4-methylimidazolium tetraphenylborate, and N-methylmorpholinium tetraphenylborate; derivatives of tetraphenylborate salts; triphenylborane complexes such as triphenylphosphine-triphenylborane complex and morpholine-triphenylborane complex; and the like. One type of curing accelerator may be used alone, or two or more types may be used in combination.
[0058] The content of the curing accelerator is preferably 0.1% by mass to 15% by mass based on the total amount of the thermosetting resin and the curing agent.
[0059] (Flux components) The electromagnetic shielding composition of the present disclosure may contain a flux component. In the present disclosure, the flux component means an organic compound capable of exerting a fluxing action (action of removing an oxide film), and the type thereof is not particularly limited. The flux component may function as a curing agent for an epoxy resin, which is a thermosetting resin. In the present disclosure, a component that functions both as a flux component and as a curing agent for an epoxy resin is referred to as a flux component. Specific examples of the flux component include rosin, an activator, a thixotropic agent, an antioxidant, etc. The flux component may be used alone or in combination of two or more kinds.
[0060] Specific examples of rosins include dehydroabietic acid, dihydroabietic acid, neoabietic acid, dihydropimaric acid, pimaric acid, isopimaric acid, tetrahydroabietic acid, palustric acid, and 2,2-bis(hydroxymethyl)propionic acid (BHPA). Specific examples of the activator include aminodecanoic acid, pentane-1,5-dicarboxylic acid, triethanolamine, diethanolamine, ethanolamine diphenylacetic acid, sebacic acid, phthalic acid, benzoic acid, dibromosalicylic acid, anisic acid, iodosalicylic acid, and picolinic acid. Specific examples of the thixotropic agent include 12-hydroxystearic acid, 12-hydroxystearic acid triglyceride, ethylene bisstearic acid amide, hexamethylene bisoleic acid amide, and N,N'-distearyl adipic acid amide. Specific examples of the antioxidant include hindered phenol-based antioxidants, phosphorus-based antioxidants, and hydroxylamine-based antioxidants.
[0061] When the electromagnetic shielding composition contains a flux component, the flux component preferably contains at least one of rosin and an activator. In this case, the rosin preferably contains BHPA, and the activator preferably contains triethanolamine. As the flux component, it is more preferable to use BHPA and triethanolamine in combination.
[0062] When the electromagnetic shielding composition contains a flux component, the proportion of the flux component in the total solid content of the electromagnetic shielding composition is, for example, preferably 1 mass % to 20 mass %, more preferably 3 mass % to 15 mass %, and even more preferably 5 mass % to 10 mass %. The proportion of the flux component in the solid content of the electromagnetic shielding composition excluding metal particles A, metal particles B, and metal particles C is preferably 50 mass% to 95 mass%, more preferably 70 mass% to 95 mass%, and even more preferably 80 mass% to 90 mass%.
[0063] (solvent) The electromagnetic shielding composition of the present disclosure may contain a solvent. From the viewpoint of sufficiently dissolving the resin, the solvent is preferably a polar solvent, from the viewpoint of preventing the electromagnetic shielding composition from drying when applied, the solvent preferably has a boiling point of 200° C. or higher, and from the viewpoint of preventing the generation of voids during sintering, the solvent more preferably has a boiling point of 300° C. or lower.
[0064] Examples of solvents include terpineol, stearyl alcohol, tripropylene glycol methyl ether, diethylene glycol, diethylene glycol monoethyl ether (also known as ethoxyethoxyethanol), diethylene glycol monohexyl ether (also known as hexylcarbitol), diethylene glycol monomethyl ether, dipropylene glycol-n-propyl ether, dipropylene glycol-n-butyl ether, tripropylene glycol-n-butyl ether, 1,3-butanediol, 1,4-butanediol, Examples of the solvent include alcohols such as propylene glycol phenyl ether and 2-(2-butoxyethoxy)ethanol; esters such as tributyl citrate, 4-methyl-1,3-dioxolan-2-one, γ-butyrolactone, diethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, diethylene glycol monobutyl ether acetate, and glycerin triacetate; ketones such as isophorone; lactams such as N-methyl-2-pyrrolidone; nitriles such as phenylacetonitrile; etc. The solvent may be used alone or in combination of two or more.
[0065] The proportion of the solvent in the electromagnetic wave shielding composition is preferably an amount that gives the electromagnetic wave shielding composition a viscosity suitable for application methods such as screen printing and spray coating. The proportion of the solvent in the electromagnetic wave shielding composition is, for example, preferably 0.1 to 5 mass %, more preferably 0.2 to 3 mass %, and even more preferably 0.3 to 1 mass %.
[0066] (Method of manufacturing the composition for electromagnetic shielding) The method for producing the electromagnetic shielding composition of the present disclosure is not particularly limited. The electromagnetic shielding composition can be obtained by mixing the components constituting the composition, and further performing processing such as stirring, dissolving, and dispersing. The device for mixing, stirring, dispersing, and the like is not particularly limited, and a three-roll mill, a planetary mixer, a planetary mixer, a rotation-revolution type stirring device, a mortar mixer, a twin-screw kneader, a thin layer shear disperser, and the like can be used. In addition, these devices may be used in appropriate combination. During the above processing, heating may be performed as necessary. After the treatment, the maximum particle size of the electromagnetic shielding composition may be adjusted by filtration. The filtration can be performed using a filtering device. Examples of filters for filtration include metal mesh, metal filters, and nylon mesh.
[0067] <Electromagnetic wave shielding sheet> The electromagnetic shielding sheet of the present disclosure has a resin composition layer containing the electromagnetic shielding composition of the present disclosure. The electromagnetic shielding sheet of the present disclosure may further include a release film, as necessary.
[0068] The resin composition layer can be produced, for example, by applying a varnish-like electromagnetic shielding composition (hereinafter also referred to as "resin varnish") prepared by adding a solvent to the electromagnetic shielding composition of the present disclosure onto a release film such as a polyethylene terephthalate film or a polyimide film, and drying it.
[0069] The application of the resin varnish can be carried out by a known method. Specifically, methods such as comma coating, die coating, lip coating, gravure coating, and methods using an applicator can be mentioned. Methods of applying the resin varnish to form a resin composition layer with a predetermined thickness include a comma coating method in which the coated object is passed through a gap, and a die coating method in which the resin varnish is applied from a nozzle with an adjusted flow rate. When the thickness of the resin composition layer before drying is 50 μm to 500 μm, it is preferable to use the comma coating method.
[0070] The drying method is not particularly limited as long as it can remove at least a part of the organic solvent contained in the resin varnish, and can be appropriately selected from commonly used drying methods. The drying method may be drying by leaving at room temperature (e.g., 25°C), drying by heating, or drying under reduced pressure. For drying by heating or drying under reduced pressure, a hot plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far-infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, or the like may be used. The temperature and time for drying can be appropriately adjusted depending on the type and amount of the solvent used. For example, drying at 40° C. to 180° C. for 1 minute to 120 minutes is preferable.
[0071] The average thickness of the resin composition layer is preferably from 3 μm to 300 μm, more preferably from 5 μm to 100 μm, and further preferably from 10 μm to 50 μm.
[0072] <Sintered body for electromagnetic wave shielding> The electromagnetic shielding sintered body of the present disclosure is a sintered body of the electromagnetic shielding composition of the present disclosure or the electromagnetic shielding sheet of the present disclosure. The shape of the electromagnetic shielding sintered body is not particularly limited, and may be a layer provided on a support member or a sheet.
[0073] The electromagnetic shielding sintered body of the present disclosure can be produced by heating the electromagnetic shielding composition of the present disclosure or the electromagnetic shielding sheet of the present disclosure to cause transient liquid phase sintering of metal particles A and metal particles B contained in the electromagnetic shielding composition. The transient liquid phase sintering may be carried out by a heat treatment or a heat and pressure treatment. For the heat treatment, a hot plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far-infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, or the like can be used. The heating and pressurizing treatment may be carried out using a hot plate press or the like, or the above-mentioned heating treatment may be carried out while applying pressure. The heating temperature in the transient liquid phase sintering depends on the type of metal particles, but is preferably 140° C. or higher, may be 190° C. or higher, or may be 220° C. or higher. The upper limit of the heating temperature is not particularly limited, but is, for example, 300° C. or lower. The heating time in transient liquid phase sintering depends on the type of metal particles, but is preferably from 5 seconds to 10 hours, more preferably from 1 minute to 30 minutes, and even more preferably from 3 minutes to 10 minutes. The transient liquid phase sintering is preferably carried out in an atmosphere with a low oxygen concentration, which means a state in which the volumetric oxygen concentration is 1000 ppm or less, and preferably 500 ppm or less.
[0074] When the electromagnetic shielding sintered body is in the form of a layer or sheet, the average thickness of the electromagnetic shielding sintered body is preferably 3 μm to 30 μm, more preferably 4 μm to 20 μm, and even more preferably 5 μm to 10 μm.
[0075] <Electronic component equipment> The electronic component device of the present disclosure has a region covered with the electromagnetic shielding sintered body of the present disclosure. Examples of electronic component devices include devices in which electronic components such as active elements (e.g., semiconductor chips, transistors, diodes, thyristors) and passive elements (e.g., capacitors, resistors, resistor arrays, coils, switches) are mounted on a support member (e.g., a lead frame, a pre-wired tape carrier, a wiring board, glass, a silicon wafer, etc.). By covering the parts of the electronic component and the supporting member that generate electromagnetic waves or are susceptible to the effects of electromagnetic waves with the electromagnetic wave shielding sintered body of the present disclosure, the electronic component device of the present disclosure can be obtained. A method for covering an electronic component or a supporting member with an electromagnetic shielding sintered body includes a method in which a varnish-like electromagnetic shielding composition is applied to the area to be covered with the electromagnetic shielding sintered body, followed by drying and heating. Examples of the application method include a screen printing method and a spray coating method. The drying conditions and drying method are the same as those used in producing the electromagnetic shielding sheet described above. The heating conditions and heating method are the same as those used in producing the electromagnetic shielding sintered body described above. Alternatively, the electromagnetic shielding sheet of the present disclosure may be placed at a location to be covered with the electromagnetic shielding sintered compact, and then heated. The heating conditions and method for the electromagnetic shielding sheet are the same as those for producing the electromagnetic shielding sintered compact described above.
[0076] The electronic component device of the present disclosure may include a support member, an electronic component disposed on the support member, a cured product of a sealing material that seals the electronic component, and an electromagnetic shielding sintered body of the present disclosure disposed on a surface of the cured product of the sealing material. When the electromagnetic shielding sintered body is disposed on the surface of the cured product of the sealing material, the electromagnetic shielding sintered body may be formed on the surface of the cured product of the sealing material after the sealing material is cured, or an electromagnetic shielding composition or an electromagnetic shielding sheet may be disposed on the surface of the sealing material before it is cured, and the sealing material may be cured and the electromagnetic shielding sintered body may be formed at the same time.
[0077] The electronic component device may further include a housing that houses the electronic components and the supporting member. When the electronic components and the supporting member are housed in the housing, at least one of the inner surface and the outer surface of the housing is covered with the electromagnetic shielding sintered body of the present disclosure, thereby obtaining the electronic component device of the present disclosure. The method for covering the inner or outer surface of the housing with the electromagnetic shielding sintered body is the same as the method for covering an electronic component or a supporting member with the electromagnetic shielding sintered body.
[0078] In the area of an electronic component device covered with the electromagnetic shielding sintered body, it is preferable that no gaps such as voids are generated at the interface between the electromagnetic shielding sintered body and the member (coating member) covered by the electromagnetic shielding sintered body, such as an electronic component, a supporting member, or a housing, from the viewpoint of adhesive strength. In the present disclosure, when observing the interface between a covering member and the electromagnetic shielding sintered compact in a region covered with the electromagnetic shielding sintered compact, the proportion of the length of the portion where the covering member and the electromagnetic shielding sintered compact are not bonded to the length of the interface in the observed region (hereinafter, this may be referred to as porosity) is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. The length of the interface in the observation area and the length of the portion of the interface in the observation area where the covering member and the electromagnetic shielding sintered compact are not bonded can be determined from an image of the cross section of the area covered with the electromagnetic shielding sintered compact taken at 3000x magnification using a scanning electron microscope (SEM). EXAMPLES
[0079] The present disclosure will be described more specifically below with reference to examples, but the present disclosure is not limited to the following examples.
[0080] [Example 1] Resin varnish 1 was prepared by mixing 20 parts by mass of Cu particles (product name: 1400YM, Mitsui Mining & Smelting Co., Ltd., average particle size: 0.2 μm) as metal particles A, 28 parts by mass of Sn particles (product name: Sn100, STC-3, Mitsui Mining & Smelting Co., Ltd., average particle size: 3 μm) as metal particles B, 41 parts by mass of Sn-Bi58 particles (product name: SnBi58, STC-3, Mitsui Mining & Smelting Co., Ltd., average particle size: 3 μm) as metal particles C, 1.1 parts by mass of epoxy resin as resin, 2.0 parts by mass of BHPA as rosin, 7.5 parts by mass of triethanolamine as an activator, 0.1 parts by mass of imidazole as a curing accelerator, and 0.3 parts by mass of hexyl carbitol as a solvent. Resin varnish 1 was applied to a polyimide film using an applicator with a gap set to 50 μm to produce a coating. It was then dried at 100°C for 30 minutes and heat-treated in a reflow furnace in a nitrogen atmosphere at 150°C for 10 minutes to obtain a sintered body. The average thickness of the sintered body was 15 μm. A part of this sintered body was joined to the ground to prepare a test piece.
[0081] [Examples 2 and 3] A sintered body and a test piece were obtained in the same manner as in Example 1, except that the amounts of metal particles A, metal particles B, and metal particles C were changed to the values shown in Table 1.
[0082] [Comparative Example 1] Resin varnish 2 was prepared by mixing 15 parts by mass of Cu particles (product name: 1400YM, Mitsui Mining & Smelting Co., Ltd., average particle size: 0.2 μm) as metal particles A, 73 parts by mass of Sn-Bi58 particles (product name: SnBi58, STC-3, Mitsui Mining & Smelting Co., Ltd., average particle size: 3 μm) as metal particles C, 1.1 parts by mass of epoxy resin as resin, 2.5 parts by mass of BHPA as rosin, 8.0 parts by mass of triethanolamine as an activator, 0.1 parts by mass of imidazole as a curing accelerator, and 0.3 parts by mass of hexyl carbitol as a solvent. Resin varnish 2 was applied to a polyimide film using an applicator with a gap set to 50 μm to produce a coating. It was then dried at 100°C for 30 minutes and heat-treated in a reflow furnace in a nitrogen atmosphere at 150°C for 10 minutes to obtain a sintered body. The average thickness of the sintered body was 15 μm. A part of this sintered body was joined to the ground to prepare a test piece.
[0083] [Comparative Example 2] Resin varnish 3 was prepared by mixing 61 parts by mass of silver-coated copper powder (product name: 1400YP, Mitsui Mining & Smelting Co., Ltd., average particle size: 10 μm) as metal particles, 32 parts by mass of epoxy resin as resin, 4 parts by mass of imidazole as a curing accelerator, and 230 parts by mass of butyl acetate as a solvent. Resin varnish 3 was applied to a polyimide film using an applicator with a gap set to 200 μm to produce a coating. It was then dried at 50°C for 1 hour and heat-treated at 150°C for 1 hour to obtain a sintered body. The average thickness of the sintered body was 15 μm. A part of this sintered body was joined to the ground to prepare a test piece.
[0084] (Volume resistivity) The volume resistivity (Ω·cm) of the obtained sintered body was measured in an environment of 25°C by the following method. A square plate sample with a side length of 15 mm was cut out from the sheet-like electromagnetic shielding sintered compact, and four probes of a high-precision resistivity meter Loresta-GP (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) were pressed against the center of the plate sample. The volume resistivity ρ (Ω·cm) was calculated from the obtained surface resistivity and film thickness. Five plate samples were measured, and the average value was taken as the volume resistivity of the electromagnetic shielding sintered compact. Table 1 shows the relative values when the volume resistivity of the sintered body obtained in Comparative Example 2 is taken as 1.0.
[0085] JPEG0007559330000001.jpg73164
[0086] As shown in Table 1, the sintered bodies produced in Examples 1 to 3 had lower volume resistivities than the sintered bodies produced in Comparative Examples 1 and 2, and were found to have a high electromagnetic wave shielding effect.
Claims
1. The present invention comprises metal particles A, metal particles B having a melting point lower than that of the metal particles A, metal particles C which are alloy particles containing a metal component contained in the metal particles B and having a melting point lower than that of the metal particles B, and a resin, Transient liquid phase sintering is possible between the metal particles A, the metal particles B, and the metal particles C; The metal particles A contain Cu, the metal particles B contain Sn, and the metal particles C contain Sn, a ratio of the metal particles A to the total of the metal particles A, the metal particles B, and the metal particles C is 10% by mass to 30% by mass, The metal particles A are Cu particles, the metal particles B are Sn particles, and the metal particles C are an alloy containing Sn, The electromagnetic wave shielding composition has a ratio of the metal particles B to the metal particles C (metal particles B / metal particles C) of 28 / 41 to 40 / 27 by mass.
2. 2. The electromagnetic shielding composition according to claim 1, wherein the metal particles B have a melting point of 300° C. or lower.
3. 3. The electromagnetic shielding composition according to claim 1, wherein the ratio of the Cu content to the Sn content (Cu content / Sn content) based on mass of the metal particles A, the metal particles B and the metal particles C as a whole is 0.25 to 0.
70.
4. 4. The electromagnetic shielding composition according to claim 1, wherein the metal particles C contain at least one metal component X selected from the group consisting of Bi, In, Zn, Cd, Pb, Ag, and Cu.
5. 5. The electromagnetic shielding composition according to claim 4, wherein the proportion of the metal component X in the entire metal particles C is 3% by mass to 80% by mass.
6. The electromagnetic shielding composition according to any one of claims 1 to 5, wherein the average particle size of the metal particles A is 0.1 µm to 2 µm.
7. 7. An electromagnetic wave shielding sheet having a resin composition layer containing the electromagnetic wave shielding composition according to any one of claims 1 to 6.
8. 8. A sintered body for electromagnetic shielding, which is a sintered body of the electromagnetic shielding composition according to any one of claims 1 to 6 or the electromagnetic shielding sheet according to claim 7.
9. An electronic component device having a region covered with the electromagnetic wave shielding sintered body according to claim 8.
Citation Information
Patent Citations
Conductive paste
JP2002150837A
Conductive jointing material, method of jointing conductor, and method of manufacturing semiconductor
JP2012174332A
Preparation of metallurgical network composition and method of using the same