Narrow gap gas shielded arc welding method
The three-electrode welding method with controlled current values and gas composition suppresses hot cracking in multi-layer welding of steel plates, enhancing efficiency and reducing costs for structures.
Patent Information
- Application Number
- JP2024534721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2044-03-18
AI Technical Summary
Existing narrow-gap gas-shielded arc welding methods face issues with hot cracking during multi-electrode welding of steel plates, particularly in subsequent layers, which hinder high welding efficiency and increase construction costs.
A three-electrode welding method is employed with current values for the first and second electrodes ranging from 260A to 360A, and the current value for the third electrode controlled by the width of the previous weld bead, using a mixed gas containing at least 20% CO2, and specific electrode arrangements to suppress hot cracking.
The method achieves high welding efficiency with suppressed hot cracking, resulting in lower manufacturing costs and improved joint quality for structures like buildings and bridges.
Smart Images

Figure 0007560002000002 
Figure 0007560002000003 
Figure 0007560002000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas-shielded arc welding method, and in particular to a narrow-gap gas-shielded arc welding method applicable to steel plates with a thickness of 22 mm or more. The term "narrow gap" used here means that the groove angle is 25° or less and the width of the minimum groove gap between the steel plates to be welded (base metal) is 50% or less of the thickness of the steel plates. [Background technology]
[0002] Gas-shielded arc welding, which is used in welding steel plates, generally uses a consumable electrode system in which CO2 gas alone or a mixture of Ar and CO2 gas is used to shield the molten area, and is widely used in the manufacturing fields of automobiles, construction, bridges, electrical equipment, etc.
[0003] In recent years, as steel structures have become larger and thicker, the amount of deposition in welding during the manufacturing process, particularly in butt welding of steel plates, has increased, and the welding work requires more time, resulting in increased construction costs.
[0004] One possible way to improve this is to apply narrow-gap gas-shielded arc welding, which uses arc welding to multi-layer welds to weld gaps that are small relative to the plate thickness. This narrow-gap gas-shielded arc welding has a smaller cross-sectional area of the weld than regular gas-shielded arc welding, so it is expected to achieve high welding efficiency and energy savings, and ultimately reduce construction costs.
[0005] Furthermore, recently, a technology has been proposed for performing this narrow-gap gas-shielded arc welding method using multiple electrodes. With multi-electrode welding, the amount of deposited metal (metal that adheres to the inside of the gap after the welding wire melts) for filling the gap can be increased by the number of electrodes, making it possible to obtain higher welding efficiency than with single-electrode welding, and it is an effective means for increasing the efficiency of welding.
[0006] For example, Patent Document 1 discloses a narrow-gap gas-shielded arc welding method for joining steel plates by narrow-gap multi-layer welding. In Patent Document 1, the first layer welding is performed by multi-electrode welding with two or more electrodes, with the first and second electrodes positioned along a predetermined parallel weld line, and the distance between the tips of the welding wires of the first and second electrodes is controlled to a range of 5 mm to 16 mm. In addition, the angle of the straight line connecting the tips of the welding wires of the first and second electrodes with respect to the perpendicular direction of the weld line is controlled to a range of 45° or less. Furthermore, the fusion depth perpendicular to the weld line at the bottom of the steel plate is set to 1.5 mm or more. It is described that these methods provide the effect of preventing the occurrence of welding defects and improving welding construction efficiency even when groove processing such as gas cutting or plasma cutting is performed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6137053 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the technology described in Patent Document 1 is limited to the first layer welding, and in the second layer and subsequent layers, hot cracks C may occur on the weld bead surface as shown in FIG. 3, and therefore the technology is insufficient as a technology for preventing hot cracks.
[0009] An object of the present invention is to solve the problems of the conventional technique and to provide a multi-electrode narrow gap gas-shielded arc welding method which can achieve high welding efficiency and suppress hot cracking. [Means for solving the problem]
[0010] In order to achieve the above object, the present inventors have conducted extensive research into a welding method for suppressing hot cracking, focusing on three-electrode welding. As a result, in welding the second and subsequent layers, the current values of the first and second electrodes are set to a range of 260A to 360A, and the current value of the third electrode is controlled according to the width of the weld bead formed by the previous layer welding, which becomes the groove gap for the next weld. It has been found that this makes it possible to suppress hot cracking.
[0011] The present invention has been completed based on these findings and through further investigation. [1] A narrow-gap gas-shielded arc welding method to be applied to the second and subsequent layers in narrow-gap multi-layer welding in which the plate thickness t is 22 mm or more, the groove angle θ is 25° or less, and the bottom groove gap G0 is 7 mm to 18 mm, the multi-layer welding is performed using three electrodes, the current values I1 and I2 of the first and second electrodes are in the range of 260 A to 360 A, and the current value I3 of the third electrode in the i-th layer is i A narrow gap gas shielded arc welding method in which [A] is in a range that satisfies the following formula (1). I3 i ≦30×G i-1 -10 ··· (1) Here, I3 i : Current value of the third electrode of the i-th layer [A], G i-1 : Width [mm] of the weld bead formed by welding the layer before the i-th layer (i-1th layer), where i is a natural number greater than or equal to 2. [2] The narrow gap gas-shielded arc welding method according to [1], wherein one of the first electrode and the second electrode is a negative wire (positive polarity) and the other is a positive wire (reverse polarity), the distance a between the tips of the welding wire supplied from the power feed tips at the tip of the welding torch of each of the first electrode and the second electrode is in the range of 5 mm to 16 mm, the angle α of a straight line connecting the tips of the welding wire of the first electrode and the second electrode with respect to a direction perpendicular to the welding line is 60° or less, the diameter of the welding wire of all of the electrodes is in the range of 1.0 mm to 1.6 mm, and the distance b between the tips of the welding wire supplied from the power feed tips at the tip of the welding torch of each of the second electrode and the third electrode is in the range of 10 mm to 100 mm. [3] The narrow gap gas-shielded arc welding method according to [1] or [2], wherein the third electrode is positioned in the center of the groove behind the first electrode and the second electrode. [4] The narrow gap gas-shielded arc welding method according to any one of the above [1] to [3], wherein a mixed gas containing 20 volume % or more of CO2 gas is used as the shielding gas. [5] In any one of the narrow gap gas-shielded arc welding methods described above in [1] to [4], at least one of the welding wires used for the positive electrode contains 0.005% by mass to 0.060% by mass of REM (rare earth element). Effect of the Invention
[0012] According to the present invention, in the second and subsequent layers of the gas-shielded arc welding method for narrow-gap multi-layer welding with high welding efficiency, it is possible to perform the welding while suppressing hot cracking. Furthermore, the narrow-gap gas-shielded arc-welded joint obtained by this method has a significantly reduced manufacturing cost compared to conventional welded joints, and is therefore extremely useful for application to general structures such as buildings, bridges, and ships. [Brief description of the drawings]
[0013] [Figure 1] 1 is an explanatory diagram showing a schematic diagram of the groove shape targeted in the present invention, in which (a) is an example in which the weld metal surface is flat, (b) is an example in which the surface is convex, and (c) is an example in which the surface is concave. [Diagram 2] Fig. 2 is an explanatory diagram showing the procedure for welding with three electrodes, (a) being a front view and (b) being a top view. [Diagram 3] FIG. 3 is an explanatory diagram that typically shows an example of hot cracking that occurs in a weld metal layer. [Figure 4] FIG. 4 is an explanatory diagram showing the relationship between the width of the weld bead and the current value range of the third electrode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be specifically described below.
[0015] The present invention is a narrow-gap gas-shielded arc welding method for joining steel plates with a plate thickness t of 22 mm or more by narrow-gap multi-layer welding with a groove angle θ of 25° or less and a bottom groove gap G0 of 7 mm to 18 mm. Note that the "steel plate" referred to here includes thick steel materials, thick plate steel materials, etc.
[0016] [Steel plate thickness: 22mm or more] The plate thickness t of the steel plate 1 is 22 mm or more. If the plate thickness t is less than 22 mm, in a conventional R-shaped groove, the groove angle is increased to reduce the groove gap, which may result in a smaller groove cross-sectional area than the groove targeted by the present invention, and the R-shaped groove may result in a highly efficient welding with a smaller deposition amount. Preferably, the plate thickness t is 30 mm or more.
[0017] Furthermore, since the plate thickness of steel structures, including special structures, is 200 mm or less, in the present invention, it is preferable that the upper limit of the plate thickness t of the steel plate is set to 200 mm.
[0018] The present invention can be applied to various steel plates ranging from mild steel plates to high-tensile steel plates of 780 MPa class. It is also possible to weld high-tensile steel plates of 590 MPa class without preheating.
[0019] [Bevel angle θ: 25° or less] The groove shape used in the present invention is a V-shaped groove (including an I-shaped groove (θ=0°)) having a gap at the bottom, and is a narrow groove. An example of the groove shape is shown in FIG. 1. Here, 1 is a steel plate (base material) and 2 is a groove surface. The smaller the groove cross-sectional area of the groove part of the steel plate, the faster and more efficient welding is possible, but defects such as poor fusion are more likely to occur. In addition, when the groove angle θ of the groove part exceeds 25°, it can be carried out even with a conventional construction method. For this reason, the present invention targets a narrow groove with a groove angle θ of 25° or less, which is difficult to carry out with the conventional construction method and is expected to be even more efficient. In addition, when the groove angle θ of a V-shaped groove is 0°, it is called an I-shaped groove, and in terms of the amount of deposition, this 0° case is the most efficient. However, since the groove may close during welding due to welding heat distortion, it is preferable to set the groove angle θ according to the plate thickness t in anticipation of this. When the plate thickness t exceeds 100 mm, the upper limit of the suitable range is preferably 10°.The groove angle θ is more preferably 5° to 10°.
[0020] [Bottom Groove Gap G0: 7mm~18mm] The smaller the groove of the steel plate, the faster and more efficient the welding can be performed, but defects such as incomplete fusion are more likely to occur. In addition, welding in which the bottom groove gap G0, which is the gap (groove width) between the bottoms of the groove before welding begins, exceeds 18 mm can be performed with conventional construction methods. For this reason, the present invention targets a bottom groove gap G0 of 18 mm or less, which is expected to be even more efficient than conventional construction methods. On the other hand, if the bottom groove gap G0 is less than 7 mm, welding with three electrodes may be difficult. Therefore, the bottom groove gap G0 is in the range of 7 mm to 18 mm. Preferably, it is in the range of 8 mm to 12 mm.
[0021] [Multi-layer welding] In the present invention, the first layer and each layer after the second layer are joined by multi-layer welding using three electrodes using the narrow groove described above, and a welding method is provided that is particularly suitable for welding the second layer and after. Here, if the number of layers in the multi-layer welding is n, each layer is individually the first layer (first layer) to the nth layer (last layer), and if an intermediate layer is the ith layer, the layer immediately before that is the i-1th layer.
[0022] [Electrode current value] First, the current value I1 of the first electrode and the current value I2 of the second electrode are set to the range of 260A to 360A. If the current values I1 and I2 of the first and second electrodes are less than 260A, the groove face cannot be melted sufficiently, and there is a high possibility of incomplete fusion. On the other hand, if the current exceeds 360A, the height of the weld bead increases and the bead becomes elongated, increasing the risk of hot cracking. Therefore, the ranges of the current value I1 of the first electrode and the current value I2 of the second electrode are both set to 260A to 360A. Preferably, they are 270A to 340A.
[0023] Next, the current value I3 of the third electrode is controlled for each layer of the multi-layer welding based on the relationship with the width of the weld bead of each layer. The inventors have found that this makes it possible to suppress hot cracks occurring in each weld layer, which is the object of the present invention. Specifically, the current value I3 of the third electrode for the i-th layer i is set to a range that satisfies the following formula (1). I3 i ≦30×G i-1 -10 ··· (1) Here, I3 i : Current value of the third electrode of the i-th layer [A], G i-1 : Width [mm] of the weld bead formed by welding the layer before the i-th layer (i-1th layer), where i is a natural number greater than or equal to 2.
[0024] Current value I3 of the third electrode i When the weld bead width G becomes larger, the height of the weld bead becomes larger and the bead becomes longer, which increases the risk of hot cracking. i is the width G of the weld bead formed by welding one layer before (i-1th layer) i-1As the number of layers increases, the width also increases. Based on this, we investigated the relationship between the width of the weld bead and the current value of the third electrode, and found that the range shown in Figure 4 is favorable, from which we derived the above formula (1). In other words, within the range that satisfies formula (1), it is possible to prevent the weld bead from becoming elongated, and an excellent effect of preventing hot cracking can be obtained.
[0025] [First layer welding conditions] The narrow gap gas shielded arc welding method according to the present invention is characterized in that the current value for each electrode is controlled as described above as a condition to be applied in the second layer and thereafter. Therefore, the conditions for the first layer welding in the welding method according to the present invention are not particularly limited. However, the welding conditions for the second layer and thereafter that are applied in the present invention can be applied as they are to the welding conditions for the first layer. Furthermore, the current value I3 of the third electrode in the first layer welding is 1 may be set to the same range (260 A to 360 A) as the current value I1 of the first electrode and the current value I2 of the second electrode.
[0026] The following describes the preferred welding conditions for the second and subsequent layers. The following conditions are also preferred for the first layer.
[0027] [Electrode polarity] If the first electrode and the second electrode have the same polarity (for example, both the first electrode and the second electrode are wire positive), the mutual arcs are directed inward by the electromagnetic force of attraction, and heat is concentrated at the center of the groove. As a result, sufficient melting cannot be obtained at the groove surface. On the other hand, if one of the first electrode and the second electrode is wire negative (positive polarity) and the other is wire positive (negative polarity), and the arrangement of the first electrode and the second electrode is appropriately controlled, the magnetic fields due to the welding currents of each electrode generate strong outward electromagnetic forces, and the arcs repel each other. As a result, it is possible to obtain a sufficient melting depth at the groove surface. For the above reasons, in the present invention, it is preferable that one of the first electrode and the second electrode is wire negative (positive polarity) and the other is wire positive (negative polarity). The polarity of the third electrode 5 is not particularly limited, and may be either wire negative (positive polarity) or wire positive (negative polarity).
[0028] [Arrangement of the first and second electrodes] In narrow gap multi-pass welding, when one pass is performed per layer, the welding heat tends to concentrate at the center of the groove with one electrode, which causes insufficient melting at the groove surface of the steel plate, and defects due to incomplete fusion (cold lap) and spatter and slag inclusion on the groove surface are likely to occur. In particular, in the first layer welding, the temperature of the steel plate is low and the melting depth is small, so defects due to incomplete fusion are likely to occur. Therefore, in the present invention, as shown in Figure 2, it is preferable to position the first electrode 3 and the second electrode 4 of the three electrodes along a predetermined parallel welding line 8. Note that 6 is a backing material, 7 is a molten pool, M1 is the first layer (first layer) of the weld metal, and M2 is the second layer of the weld metal.
[0029] [Distance between the tips of the welding wires of the first and second electrodes a: 5mm~16mm] The distance a between the tips of the welding wires 3b, 4b supplied from the power feed tips 3a, 4a at the tip of each welding torch of the first electrode 3 and the second electrode 4 (hereinafter also referred to simply as the "first-second electrode distance"; see FIG. 2(b)) is preferably adjusted to a range of 5 mm to 16 mm. Note that the "distance between the welding wire tips" here refers to the distance between the centers of the welding wire tips of each electrode.
[0030] If the first-second electrode distance a is less than 5 mm, the current (electrons) flows between the electrodes, reducing the heat of the arc itself, and sufficient melting of the groove surface 2 cannot be obtained. On the other hand, if the first-second electrode distance a exceeds 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance, and the arc repulsion force to overcome the inward electromagnetic force generated by the current flowing through the groove surface 2 is not obtained, and the arcs turn inward, causing heat to concentrate at the center of the groove. As a result, sufficient melting of the groove surface 2 cannot be obtained. In addition, in narrow gap welding, suppressing welding defects caused by the adhesion of spatter to the groove surface 2 is an issue. However, the first electrode 3 and the second electrode 4 are arranged along predetermined parallel welding lines 8, 8, one of them is wire negative (positive polarity) and the other is wire positive (reverse polarity), and the first-second electrode distance a is adjusted to a range of 5 mm to 16 mm. As a result, the spatter is absorbed by the molten metals and adhesion of the spatter to the groove faces is suppressed, so that a sound weld can be obtained. For these reasons, it is preferable to adjust the distance a between the first and second electrodes to a range of 5 mm to 16 mm.
[0031] [Angle α of the straight line connecting the tips of the welding wires of the first and second electrodes: 60° or less] In the present invention, the repulsion of the arc is utilized to ensure melting of the groove surface. However, if the angle α of the straight line connecting the welding wire tips of the first electrode 3 and the second electrode 4 with respect to the direction perpendicular to the welding line exceeds 60°, a sufficient repulsive force of the arc cannot be obtained, and sufficient melting cannot be obtained at the groove surface. Therefore, the angle α of the straight line connecting the welding wire tips of the first electrode 3 and the second electrode 4 with respect to the direction perpendicular to the welding line 8 (hereinafter also simply referred to as the "first-second electrode arrangement angle", see FIG. 2(b)) is preferably 60° or less. More preferably, it is 55° or less. The first-second electrode arrangement angle α may be 0°.
[0032] [Welding wire diameter: 1.0mm~1.6mm] Welding wires for narrow-gap gas-shielded arc welding are generally manufactured with diameters in the range of 0.6 mm to 2.0 mm. When welding with the same current, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, in order to realize highly efficient welding, it is preferable to select a relatively thin wire diameter. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making the welding unstable. Therefore, the diameter of the welding wire used in the present invention is preferably in the range of 1.0 mm to 1.6 mm.
[0033] [Distance between the tips of the welding wires of the second and third electrodes b: 10mm~100mm] The distance b between the tips of welding wires 4b, 5b supplied from power feed tips 4a, 5a at the tips of the welding torches of second electrode 4 and third electrode 5 (hereinafter also simply referred to as the "second-third electrode distance"; see FIG. 2(b)) is preferably in the range of 10 mm to 100 mm. This is because hot cracking resistance is improved by setting the distance b in this range. More preferably, the distance b is 12 mm to 80 mm.
[0034] [Placement of the third electrode] If the weld build-up height exceeds the bottom groove gap G0 in the first layer welding, the risk of hot cracking increases. To avoid this, it is effective to position the third electrode 5 in the center of the groove behind the first electrode 3 and the second electrode 4. This also makes it possible to further reduce the number of layers, greatly reducing the risk of stacking defects in multi-layer welding. Note that the "center of the groove" here allows a range of ±10% of the bottom groove gap G0 from the center of the groove.
[0035] [Shielding gas: mixed gas containing 20% or more CO2 gas by volume] Since the amount of oxygen in the weld metal is also greatly affected by the shielding gas composition, it is preferable to use a mixed gas containing 20 volume % or more of CO2 gas and the remainder of an inert gas such as Ar as the shielding gas used in narrow gap gas-shielded arc welding according to the present invention. More preferably, it is a single gas of 100 volume % CO2 gas. In the present invention, it is preferable to increase the oxygen concentration in the weld metal, which controls the flow of the weld metal, and direct the convection of the weld metal from the center outward to stably deepen the molten depth at the bottom of the thick steel plate in the groove.
[0036] [REM content of welding wire: 0.005% by mass to 0.060% by mass] REM (rare earth elements) are elements effective in refining inclusions in weld metal and improving toughness during welding. In addition, when welding is performed by supplying a welding wire containing REM to a positive electrode, it is possible to refining droplets and stabilizing transfer. This refining of droplet transfer suppresses the generation of spatter and enables stable gas shielded arc welding even in positive polarity. For these reasons, in the present invention, it is preferable to supply a steel wire containing 0.005% to 0.060% by mass of REM (rare earth elements) to a positive electrode. Note that elements other than REM (rare earth elements) are included in the appropriate amounts normally contained according to the grade (steel type) of the welding wire, as specified in JIS Z 3312.
[0037] If the REM (rare earth element) content is less than 0.005% by mass, it is difficult to achieve the above-mentioned fine droplets and stable transfer. On the other hand, if the REM (rare earth element) content exceeds 0.060% by mass, cracks will occur during the wire manufacturing process, making it difficult to manufacture the welding wire. For this reason, the REM (rare earth element) content is preferably in the range of 0.005% to 0.060% by mass. More preferably, it is 0.010% to 0.055% by mass.
[0038] [Other welding conditions] In the present invention, the welding conditions other than those described above do not need to be particularly limited and may be in accordance with established methods, such as a welding voltage of 32 V to 37 V, a welding speed of 30 cm / min to 90 cm / min, a welding wire extension length of 15 mm to 30 mm, and a welding heat input per pass of 10 kJ / cm to 50 kJ / cm.
[0039] In addition, by satisfying the other welding conditions shown below, hot cracking can be further suppressed and welding can be performed more efficiently.
[0040] [Welding wire feed angle φ to the bottom groove: 0° to 15° to the perpendicular] Arcs have directionality and tend to point in the direction that the tip of the electrode (welding wire) is pointing. To effectively utilize the directivity of this arc to melt the groove surface, it is advantageous to point the electrode tip toward the groove surface, and the direction that the electrode tip points varies greatly depending on the feed angle φ of the welding wire supplied from the power contact tip at the tip of the welding torch. The feed angle φ of the welding wire supplied from the power contact tip at the tip of the welding torch with respect to the bottom groove is shown in Figure 2(a).
[0041] When the feed angle φ of the welding wires 3b and 4b supplied from the power feed tips 3a and 4a at the tip of the welding torch to the bottom groove is less than 0° with respect to the perpendicular line, the current flows through a path with less resistance. As a result, the arc creeps up the wire electrode (arc creeping up), making it difficult to maintain the targeted fusion at the groove surface 2, especially at the bottom. On the other hand, when the feed angle φ of the welding wire supplied from the power feed tip to the bottom groove exceeds 15° with respect to the perpendicular line, the arc is too directed toward the groove surface 2, so the weld bead shape becomes convex, and the melting by the arc in the welding after the first layer becomes insufficient, which makes it easy to cause welding defects. For this reason, the feed angle φ of the welding wires 3b and 4b of the first electrode 3 and the second electrode 4 to the bottom groove is preferably in the range of 0° to 15° with respect to the perpendicular line. More preferably, it is 5° to 12°.
[0042] The feed angle φ of the welding wire of the first electrode 3 and the second electrode 4 to each bottom groove is the same as the inclination of the power feed tips 3a and 4a, particularly the tip of the power feed tip, so the feed angle φ of the welding wire can be controlled by the inclination of the tip of the power feed tip. Note that the feed angle φ is defined as + in the direction facing the groove face. The perpendicular line here refers to the perpendicular line to the bottom groove.
[0043] [Distance d between the side end of the welding wire tip and the bottom groove surface: 0.1mm~3.0mm] As shown in FIG. 2(a), the distance d between the side end of the welding wire tip of the first electrode 3 and the second electrode 4 and the bottom of the groove surface 2 is preferably in the range of 0.1 mm to 3.0 mm. If the distance d between the side end of the tip of the welding wire 3b and 4b at the bottom groove and the bottom groove surface 2 is less than 0.1 mm, an arc is generated between the upper part of the wire and the groove surface 2, and the bottom groove surface 2 cannot be melted efficiently. On the other hand, if it exceeds 3.0 mm, the arc is separated from the groove surface 2, and the groove surface 2 cannot be melted efficiently. For this reason, the distance d between the side end of the welding wire tip and the bottom groove surface is preferably 0.1 mm to 3.0 mm. More preferably, it is 0.5 mm to 2.0 mm, and even more preferably, it is 0.5 mm to 1.0 mm. Note that the "side end of the tip of the welding wire" refers to the side end on the side close to the groove surface 2 of the bottom of the steel plate to be melted by each electrode.
[0044] [Curve radius of the welding wire fed to the power supply tip: 150mm~500mm] In the present invention, in order to control the feed angle φ of the welding wires 3b and 4b fed from the power feed tips 3a and 4a at the tips of the welding torches of the first electrode 3 and the second electrode 4, a power feed tip with a bent tip is used. At this time, the welding wire passes through the power feed tip with a bent tip, and in order to pass through it more smoothly, it is preferable to bend the welding wire in advance using a so-called three-point roller or the like. At this time, if the curvature radius of the welding wire is less than 150 mm, the wire feed resistance increases, the welding wire cannot be fed stably, and it becomes difficult to maintain the arc. On the other hand, if the curvature radius of the welding wire exceeds 500 mm, there is no effect in reducing the wire feed resistance when the power feed tip tip is bent, so the welding wire cannot be fed stably, and it becomes difficult to maintain the arc. From the above, it is preferable that the curvature radius of the welding wires 3b and 4b fed to the power feed tips 3a and 4a of the first electrode 3 and the second electrode 4 is 150 mm to 500 mm. More preferably, it is 175 mm to 475 mm. EXAMPLES
[0045] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0046] A test was conducted in which grooves were prepared by gas cutting, multi-layer welding was performed on steel plates (base materials) with individual groove shapes, and the groove shapes of each layer from the second layer onward were measured (Joints No. 1 to 12). Table 1 shows the groove shapes and the welding conditions for each layer from the second layer onward, from the first electrode to the third electrode.
[0047] The weld metal layer was cut at each welded layer, and the cross section of the weld was corroded with nital, after which the occurrence of hot cracking was confirmed for each layer. The results are also shown in Table 1.
[0048] Here, the conditions other than the welding conditions listed in Table 1 are as follows. The steel type (grade) of the steel plate used was 490 MPa grade steel to 590 MPa grade steel, and the plate thickness t of the steel plate was 30 mm to 100 mm. The steel type (grade) of the welding wire used was YGW18, and the diameter of the welding wire was 1.2 mm.
[0049] The 1st-2nd electrode distance a was 14 mm, the 2nd-3rd electrode distance b was 16 mm, and the 1st-2nd electrode arrangement angle α was 55°.
[0050] The welding speed is 60 cm / min, and the welding heat input is 28 kJ / cm to 41 kJ / cm.
[0051] The REM content of the welding wire used in the negative wire electrode was 0.025% by mass to 0.030% by mass.
[0052] The feed angle φ of the welding wire was 8°, the distance d between the tip end of the welding wire and the groove surface was 0.5 mm, and the curvature radius of the welding wire was 300 mm.
[0053] [Table 1]
[0054] In all of the examples of the present invention, no hot cracking was observed even when narrow-gap multi-layer welding was performed with three-electrode welding. On the other hand, in the comparative examples outside the scope of the present invention, hot cracking occurred and a sound narrow-gap gas-shielded arc welded joint was not obtained. [Explanation of symbols]
[0055] 1 Steel plate (base material) 2 Bevel surface 3 1st electrode 4 Second electrode 5 Third electrode 6 Backing material 3a, 4a, 5a power supply chip 3b, 4b, 5b welding wire 7. Melting Ground 8 Welding seam t plate thickness, θ groove angle C High temperature cracking M Weld metal M1 first layer, M2 second layer, M i-1 The layer before the i-th layer, M i i layer G0 Bottom groove gap, G1 Width of the weld bead on the 1st layer, G i-1 Width of weld bead of layer i-1, G i Width of weld bead of layer i
Claims
1. Plate thickness t: Steel plate of 22 mm or more, groove angle θ: 25° or less, bottom groove gap G 0 A narrow gap gas shielded arc welding method applied to the second layer or later in narrow gap multi-layer welding having a gap of 7 mm to 18 mm, Multi-layer welding is performed using three electrodes. Current value I of the first electrode and the second electrode 1 and I 2 is in the range of 260A to 360A, Current value I of the third electrode of the i-th layer 3 i A narrow gap gas shielded arc welding method in which [A] is in a range that satisfies the following formula (1). I 3 i ≦30×G i-1 -10 ・・・ (1) Here, I 3 i : Current value [A] of the third electrode of the i-th layer, G i-1 i: Width [mm] of the weld bead formed by welding the layer before the i-th layer (i-1th layer), where i is a natural number of 2 or more.
2. One of the first electrode and the second electrode is a wire negative (positive polarity), and the other is a wire positive (reverse polarity), a distance a between the tip of a welding wire supplied from a power feed tip at the tip of each welding torch of the first electrode and the second electrode is set in a range of 5 mm to 16 mm; The angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to a direction perpendicular to the welding line is set to 60° or less, The diameter of the welding wire of all of the electrodes is in the range of 1.0 mm to 1.6 mm; 2. The narrow gap gas-shielded arc welding method according to claim 1, wherein a distance b between tips of the welding wires supplied from the power feed tips at the tips of the welding torches of the second electrode and the third electrode is in the range of 10 mm to 100 mm.
3. The narrow gap gas-shielded arc welding method according to claim 1 , wherein the third electrode is disposed at a center of the groove rearward of the first electrode and the second electrode.
4. The narrow gap gas-shielded arc welding method according to claim 2 , wherein the third electrode is disposed at a center of the groove rearward of the first electrode and the second electrode.
5. Shielding gas containing 20% by volume or more of CO 2 The narrow gap gas-shielded arc welding method according to any one of claims 1 to 4, wherein a mixed gas containing a gas is used.
6. The narrow gap gas-shielded arc welding method according to any one of claims 1 to 4, wherein at least one of the welding wires used for the positive electrode contains 0.005% by mass to 0.060% by mass of REM (rare earth element).
7. The narrow gap gas-shielded arc welding method according to claim 5, wherein at least one of the welding wires used for the positive electrode contains 0.005% by mass to 0.060% by mass of REM (rare earth element).
Citation Information
Patent Citations
Gas shield arc welding of two muliti layer cladded electrodes
JP1999129072A
Tandem welding apparatus, and tandem first pass welding method
JP2011031250A
Narrow groove gas-shield arc-welding method
JP2015223605A
Preparation of cake
JP1986037053A