Soft-bottom carpet made from recycled yarn and its manufacturing method

The soft-sole carpet made from recycled yarn addresses energy and pollution issues in carpet manufacturing by using a structured recycled fiber layer and adhesive bonding, achieving flexibility, comfort, and heat insulation.

JP7561476B2Active Publication Date: 2024-10-04SUZHOU TUNTEX FIBER & CARPET CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022527754
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-20
Filing Date
2020-03-26
Publication Date
2024-10-04
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing carpet manufacturing methods consume large amounts of energy, generate secondary pollution, and produce waste due to the use of PVC and asphalt, while also lacking flexibility and comfort.

Method used

A soft-sole carpet is manufactured using recycled yarn, comprising a carpet fiber layer and a recycled fiber layer bonded with adhesives, with a latex layer in between, and a nonwoven fabric layer below, utilizing a method that classifies and processes defective fibers to maintain uniformity and stability.

Benefits of technology

The method reduces energy consumption and waste, provides a flexible, comfortable, and elastic carpet with excellent physical properties and heat insulation, while utilizing defective fibers effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561476000009
    Figure 0007561476000009
  • Figure 0007561476000010
    Figure 0007561476000010
  • Figure 0007561476000011
    Figure 0007561476000011
Patent Text Reader

Abstract

The present invention is a soft-bottom carpet made using recycled yarn, which comprises, from top to bottom, a carpet fiber layer and a recycled fiber layer. The carpet fiber layer comprises carpet fibers and a first long-fiber nonwoven fabric, with the carpet fibers tufted into the first long-fiber nonwoven fabric. The recycled fiber layer comprises recycled fibers and a second long-fiber nonwoven fabric, with the recycled fibers tufted into the second long-fiber nonwoven fabric. The carpet fiber layer and the recycled fiber layer are fixed together. The present invention has advantages such as a soft material, high comfort, excellent elasticity, stable physical properties, and excellent insulation.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of carpet manufacturing, and more particularly to a soft-bottom carpet manufactured using recycled yarn and a manufacturing method thereof. [Background technology]

[0002] Currently, most domestic carpets are made by applying PVC or asphalt to the carpet surface after tufting, and then adding a glass fiber layer in the middle to improve the dimensional stability of the carpet, or attaching a nonwoven material after tufting the carpet surface. However, when PVC material is used in carpets, it usually has a hard texture and is not comfortable, so major manufacturers are trying to find new materials to replace PVC as carpet materials. Nonwoven materials are relatively more flexible than PVC materials, but they have physical properties such as dimensional instability and warping, which often cause quality defects during use. Therefore, we are working on creating a material that combines the stability of PVC / asphalt and the comfort of soft soles, and incorporates the scientific concepts of green recycling and environmental protection.

[0003] In the production and processing of fibers, some defective products may be generated due to color variation, abnormal physical properties, and color change transition. These defective products cannot be used in normal carpet production, so they are usually discarded or cut and recycled. Cutting and recycling means that after cutting the fibers, they are melted at high temperature, then granulated, and melted again at high temperature to produce other products as needed. However, this recycling method requires the use of equipment for cutting, melting, granulation, molding, etc., and these high-power equipment requires the consumption of large amounts of energy, and high-frequency work requires a large amount of human resources. Moreover, in the process of cutting the fibers, a large amount of hair fluff and dust is generated, which causes damage to the workers' bodies, and the secondary pollution and large amount of energy consumption caused by this will have an irreversible adverse effect on the environment. Summary of the Invention [Problem to be solved by the invention]

[0004] The technical problem that the present invention aims to solve is to provide a carpet made using recycled yarn that reduces energy consumption and secondary pollution during the yarn recycling process, while also having advantages such as a flexible material, high comfort, excellent elasticity, stable physical properties, and excellent insulation properties.

[0005] Another technical problem to be solved by the present invention is to provide a method for producing a carpet made using the above-mentioned regenerated yarn. [Means for solving the problem]

[0006] This is a soft bottom carpet made using recycled yarn, and is provided, from top to bottom, with a carpet fiber layer and a recycled fiber layer. The carpet fiber layer includes carpet fibers and a first long-fiber nonwoven fabric, and the carpet fibers are tufted into the first long-fiber nonwoven fabric. The recycled fiber layer includes recycled fibers and a second long-fiber nonwoven fabric, and the recycled fibers are tufted into the second long-fiber nonwoven fabric. The carpet fiber layer and the recycled fiber layer have tufted pile surfaces that include various loop piles, cut piles, and mixed styles of loop pile and cut pile.

[0007] The carpet fiber layer and the recycled fiber layer are bonded together.

[0008] The material of the carpet fiber is PP, PET, PTT, nylon, PO or wool, preferably nylon or PP.

[0009] The first long fiber nonwoven fabric and the second long fiber nonwoven fabric have a fiber density of 70 to 150 g / m 2 , preferably 90 to 100 g / m 2 It is.

[0010] The carpet fiber layer and the recycled fiber layer are bonded together with an adhesive.

[0011] The adhesive material is PVC, asphalt, PO, PU, ​​PE, or EVA, preferably PO.

[0012] A latex layer is provided between the carpet fiber layer and the recycled fiber layer.

[0013] The material of the latex layer is EVA, water-based PU, acrylic, or SBR, preferably SBR.

[0014] A nonwoven fabric layer is provided under the recycled fiber layer.

[0015] The regenerated fiber layer and the nonwoven fabric layer are bonded together with an adhesive.

[0016] The nonwoven fabric has a gram weight of 50 to 1200 g / m 2 , preferably 50 to 300 g / m 2 It is.

[0017] The nonwoven fabric layer has a heat shrinkage rate of less than 2%.

[0018] The number of piles on the pile surface of the regenerated fiber layer is 100,000 / m 2 The following is the result.

[0019] The manufacturing method of the soft-bottom carpet made with the regenerated yarn includes the following steps: (1) a carpet fiber tufting step of tufting carpet fibers into a first long fiber nonwoven fabric to obtain a carpet fiber layer, the carpet fiber being made of PP, PET, PTT, nylon, PO or wool; (2) Water-based latex SBR, antibacterial agent, calcium carbonate, and foaming agent are uniformly mixed in a mass ratio of 62-100:0-1:0-35:0-2, preferably 65-70:0-1:28-35:0-1, and air-foamed at a foaming ratio of 1.2-10 times, preferably 1.5-3 times, using a foaming machine. The mixture is then uniformly applied to the back surface of the carpet fiber layer in an amount of 50-800 g / m. 2 , preferably 80 to 350 g / m 2and a latex precoat-drying step to obtain a latex layer with a dry adhesive amount of 10 ... (3) Classifying the recycled fibers, combining the recycled fibers into thick recycled fibers of 850D to 4000D, and tufting the thick recycled fibers into a second long fiber nonwoven fabric to obtain a recycled fiber layer, and the pile density of the pile surface in the recycled fiber layer is specifically 100,000 fibers / m 2 ~450000 pieces / m 2 and a pile height is specifically 2.5 mm to 12 mm, preferably 3.5 mm to 6.5 mm. A tufting step of the regenerated fiber to obtain a regenerated fiber layer. (4) PO and calcium carbonate are charged in a mass ratio of 20-45:55-80, preferably 20-30:70-80, followed by heating and melting, uniformly stirring, cooling and granulating to obtain PO-calcium carbonate adhesive chips, which are charged into a tile carpet laminating machine, heated and melted at 130-220°C, and then evenly applied to the pile surface of the regenerated fiber layer by an extruder, and scraped up to a height of 0.5 mm to 1.0 mm, preferably 0.5 mm to 0.8 mm, using a doctor knife or doctor roller, etc., to adjust the amount of PO and calcium carbonate adhesive used to 150-2000 g / m2. 2 , preferably 500 to 800 g / m 2 A step of forming a regenerated fiber tufted soft bottom layer by combining the regenerated fiber tufted layer and the nonwoven fabric layer, pressing them with a roller, and cooling them at 5 to 30 ° C. to form a regenerated fiber tufted soft bottom layer; (5) PO and calcium carbonate are heated and melted in a mass ratio of 25-50:50-75, preferably 25-35:65-75, and then cooled and granulated to obtain PO-calcium carbonate adhesive chips, which are then fed into a tile carpet laminating machine, heated and melted at 130-220°C, and then coated evenly on the tufted back surface of the recycled fiber tufted soft bottom layer by an extruder, and the excess is scraped off with a doctor knife or doctor roller, etc., and the PO-calcium carbonate adhesive is bonded to the latex surface of the carpet fiber tufted layer, with the amount of PO-calcium carbonate adhesive used being 500 g / m per square meter. 2 ~2500g / m 2The method includes a step of bonding the carpet fiber layer and the recycled fiber layer together, controlling the thickness to 0.8mm to 1.5mm, pressing the layers with a roller after bonding, and cooling them in a cooling box at 5 to 30°C. In step (2), the drying conditions are a drying temperature of 140 to 200° C. and a drying time of 2 to 8 minutes.

[0020] The regenerated yarns need to be recycled and produced according to the material of the yarn fibers. Regenerated fibers of the same material need to be further classified according to the fiber thickness (denier number D), and fibers with the same or similar denier numbers can be grouped together, while fibers with different or large differences in denier numbers need to be managed separately. Depending on the fiber thickness required for tufting, thin fibers can be combined to match or approach the thickness of the tufted fibers, and then tufted into the second long fiber nonwoven fabric. The thermal shrinkage of the fibers used in the regenerated fiber layers of the same roll should be approximately the same, and the thermal shrinkage should be maintained within ±3%.

[0021] In the manufacturing process of yarn fibers, defective products are generated due to color variation, physical property deviation, color change transition, etc., and the regenerated fiber of the present invention is a fiber that becomes unusable due to such color variation, physical property deviation, and color change transition. In the conventional technology, the regenerated fiber is directly discarded or cut and recycled, but direct disposal results in waste of raw materials and increases production costs. In the present invention, the regenerated fiber is classified into categories such as PP, nylon, PET, PTT, PO, wool, etc. according to the material, and the defective fiber is classified according to the fiber thickness and heat shrinkage rate. Regenerated fibers of the same material must also be classified according to the fiber thickness (denier number D), and fibers with the same or similar denier number can be grouped together, and fibers with different denier numbers or large differences in denier number must be managed separately. Depending on the fiber thickness required for tufting, thin fibers can be made to match or approach the thickness of the tufted fiber by doubling, and tufted into a second long fiber nonwoven fabric. For example, using nylon regenerated fiber, two 1100D threads are twisted together to make a 2200D thread, and three 680D threads are twisted together to make a 2040D thread. The thermal shrinkage of the fibers used in the regenerated fiber layers of the same roll must be nearly the same, and the thermal shrinkage must be maintained within ±3%.

[0022] The purpose of this classification is to ensure that the fiber raw materials, thickness, height and density are uniform and consistent throughout the entire production process.To ensure the smoothness of the recycled fiber layer during use, the pile height must be strictly controlled during the carpet tufting process, and the height must be within ±2mm, so as to ensure the consistency of comfort and softness throughout the entire batch of products. Effect of the Invention

[0023] Based on the concept of eco-friendliness and environmental protection, the present invention reduces the amount of PVC and asphalt used in the conventional carpet manufacturing process as much as possible, and even eliminates the use of these raw materials, making it possible to produce a greener, more environmentally friendly, safer and more comfortable carpet.

[0024] The present invention has the advantages of being flexible, highly comfortable, excellent elasticity, stable physical properties, excellent heat insulation, etc. In addition, the present invention can not only prevent the disposal of the company's own defective fibers, but also use the defective products produced by other manufacturers, and can utilize the existing equipment in the industry and directly use the defective products in carpets without increasing other equipment, thereby achieving maximum energy conservation and emission reduction in earnest.

[0025] The present invention reduces the serious impact of conventional nonwoven fabric manufacturing techniques on the horizontal and vertical directions of thermal expansion and cold shrinkage environments by tufting recycled fibers into a long-fiber nonwoven fabric to form a three-dimensional fiber structure. When used as a carpet material, this three-dimensional structure has good stability, improves softness and elastic recovery, and further improves the stability of the entire carpet. [Brief description of the drawings]

[0026] [Figure 1] FIG. 2 is a structural schematic diagram of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of the manufacturing process of the present invention. [Diagram 3] FIG. 2 is a schematic diagram of the manufacturing process of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The technical solution of the present invention will be further described below with reference to the drawings.

[0028] In FIG. 1, 1 is carpet fiber, 2 is a first long-fiber nonwoven fabric, 3 is a first resin adhesive layer, 4 is a second long-fiber nonwoven fabric, 5 is recycled fiber, 6 is a second resin adhesive layer, 7 is a latex layer, and 8 is a nonwoven fabric.

[0029] This is a soft bottom carpet made using recycled yarn, and is provided, from top to bottom, with a carpet fiber layer and a recycled fiber layer. The carpet fiber layer includes carpet fibers and a first long-fiber nonwoven fabric, and the carpet fibers are tufted into the first long-fiber nonwoven fabric. The recycled fiber layer includes recycled fibers and a second long-fiber nonwoven fabric, and the recycled fibers are tufted into the second long-fiber nonwoven fabric. After tufting, the carpet fiber layer and the recycled fiber layer have pile surfaces that include various loop piles, cut piles, and mixed styles of loop pile and cut pile.

[0030] The carpet fiber layer and the recycled fiber layer are bonded together.

[0031] The material of the carpet fiber is PP, PET, PTT, nylon, PO or wool.

[0032] The gram weight of the first long fiber nonwoven fabric and the second long fiber nonwoven fabric is 70 to 150 g / m 2 The first long fiber nonwoven fabric and the second long fiber nonwoven fabric are made of polyester fiber, and have a thickness of 1.2 mm or less, a strength of 10 kgf or more, and a thermal shrinkage rate of less than 0.9%. The long fiber nonwoven fabric is a high-quality nonwoven fabric material characterized by its ability to always maintain stable lateral dimensions and high strength.

[0033] The carpet fiber layer and the recycled fiber layer are bonded together with an adhesive.

[0034] The adhesive material is PVC, asphalt, PO, PU, ​​PE, or EVA. The adhesive is used to bond the carpet fiber layer and the recycled fiber layer, and may be used to bond the recycled fiber layer and the nonwoven fabric layer. As the adhesive, a PO material is preferred, and PO and calcium carbonate are mixed in a mass ratio of 25-50:50-75.

[0035] The compounding ratio may be changed or other auxiliary agents may be added as necessary, but first, PO and calcium carbonate are added in a ratio of 25-50:50-75, then heated and melted, the PO is dissolved, and then the mixture is stirred uniformly with calcium carbonate to disperse the calcium carbonate well, and then cooled and granulated. Then, the mixture is put into a tile carpet laminating machine. The raw material is heated and melted at 130-220°C, then put into the inlet of the tile carpet laminating machine, extruded and coated, and applied evenly to the tufted back surface of the recycled fiber tufted soft sole using a doctor knife or doctor roller, and the excess part is removed and bonded to the latex surface of the carpet fiber layer. Depending on the actual needs of the production, the amount used is 500-2500g / m 2 The thickness is controlled to 0.8mm~1.5mm according to the actual manufacturing needs. After coating, it is put into a cooling box at 5~30℃ to cool steadily and ensure that the product is flat during cooling. After cooling, the finished product is cut and manufactured.

[0036] Preferably, a latex layer is provided between the carpet fiber layer and the recycled fiber layer, and the material of the latex layer is EVA, water-based PU, acrylic, or SBR, preferably SBR. The addition of the latex layer improves the elasticity and flexibility of the carpet. The coating amount of EVA, water-based PU, acrylic, or SBR is 50 g / m2 (Dry). 2 ~800g / m 2 The application method is foaming and adhesion.

[0037] Preferably, the formulation of the latex layer is SBR, antibacterial agent, calcium carbonate, and foaming agent in a mass ratio of 62-100:0-1:0-35:0-2, and among these, the antibacterial agent, calcium carbonate, and foaming agent are components that are used as needed.

[0038] Method for producing the latex layer material SBR, antibacterial agent, calcium carbonate, and foaming agent are added to a mixing tank in a specified mixing ratio, and after uniform mixing, the mixture is foamed using a foaming machine and applied uniformly to the backside of the carpet fiber layer, with the excess being scraped off. It functions as a fiber reinforcement material to avoid poor appearance due to falling off. The application amount is 50g / m2 ~800g / m 2 After application, the carpet is dried in an oven at 140-200℃ for 2-8 minutes at a speed of 5m / min, and when the latex is completely dry, the carpet is rolled up.

[0039] Under the regenerated fiber layer, a heat shrinkage rate of less than 2% and a gram weight range of 50 to 1200 g / m 2 The nonwoven fabric layer is a non-essential structure and may be added for aesthetic reasons or to further improve the stability of the carpet. The material of the nonwoven fabric layer may be polyester fiber or nylon, and has a heat shrinkage rate of less than 2%, is not prone to pilling, is free of delamination, and has a gram weight of 50 to 1200 g / m 2 It is.

[0040] Example 1: A method for producing a soft-bottom carpet made with regenerated yarn includes the following steps:

[0041] (1) Carpet fiber tufting A carpet tufting machine is used to tuft nylon fibers into the first long fiber nonwoven fabric to form a carpet fiber layer, which is then wound into a roll. In this carpet fiber layer, one side having pile is the carpet pile side, and the other side is the tufted back side to be latex precoated. (2) Latex pre-coating and drying Use environmentally friendly water-based latex SBR, and the compounding ratio is SBR: antibacterial agent: calcium carbonate: foaming agent = 62-100: 0-1: 0-35: 0-2, preferably 65-70: 0-1: 28-35: 0-1, in which the contents of the antibacterial agent and the foaming agent may be 0. The above raw materials are charged into a mixing tank at the compounding ratio and uniformly mixed, and then air foaming is performed using a foaming machine at a foaming ratio of 1.2-10 times, preferably 1.5-3.0 times, and the mixture is uniformly applied to the tufted back surface of the carpet fiber layer, and excess latex is scraped off using a doctor knife, doctor roller, etc. The application amount is 50-800g / m 2 , preferably 80 to 350 g / m 2After coating, the adhesive is dried in an oven at 140 to 200°C for 2 to 8 minutes at a speed of 5 m / min. After drying the latex, the adhesive is rolled up. (3) Tufting of recycled fibers As the regenerated fiber, thick nylon fiber with a density of about 850D to 4000D after doubling is used, and fibers of a similar thickness are directly tufted onto the second long fiber nonwoven fabric using a carpet tufting machine to produce a regenerated fiber layer, which is then rolled up. The pile density of the pile surface is specifically 100,000 threads / m 2 ~450000 pieces / m 2 Specifically, the pile height is 2.5 mm to 12 mm. The recycled fiber layer may have a different adhesion surface direction as required, i.e., the back surface of the recycled fiber layer may be bonded to the nonwoven fabric layer, and the pile surface of the recycled fiber layer may be bonded to the latex surface of the carpet fiber layer. (4) PO adhesive layer (the second resin adhesive layer is an optional structure) PO and calcium carbonate are added in a ratio of 20-45:55-80 (preferably 20-30:70-80), then heated and melted (at a temperature of 130-220°C), the PO is dissolved, and then uniformly stirred with calcium carbonate to disperse the calcium carbonate well, followed by cooling (at a temperature of 5-30°C) and granulation (particle size of 4-40 mesh or less), thereby ensuring a uniform molten state. The raw material is heated and melted at 130-220°C, then fed into the inlet 11 of a tile carpet laminating machine, extruded and coated, and evenly coated on the pile surface of the regenerated fiber layer using a doctor knife, doctor roller, or the like 10, and scraped up to an appropriate height of 0.5 mm-1.0 mm (preferably 0.5 mm-0.8 mm), with the amount of use being 150-2000 g / m per square meter. 2 (Preferably 500 to 800 g / m 2 ) to combine the recycled fiber layer and the nonwoven fabric layer. Press with a roller and steadily cool at 5-30°C, keeping the product flat during cooling, to form a recycled fiber tufted soft bottom layer, and store in a roll. (5)PO adhesive layer PO and calcium carbonate are added in a ratio of 25-50:50-75, then heated and melted (at a temperature of 130-220°C). After dissolving the PO, it is stirred uniformly with calcium carbonate to disperse the calcium carbonate well, and then cooled (at a temperature of 5-30°C) to granulate to a particle size of 4-40 mesh or less. The raw material is heated and melted at 130-220°C, then fed into the inlet 11 of the tile carpet laminating machine, extruded and coated, and evenly applied to the tufted back surface of the recycled fiber tufted soft bottom layer using a doctor knife, doctor roller, etc. 10, and the excess is removed to adhere to the latex surface of the carpet fiber layer. The usage amount is 500g / m2 2 ~2500g / m 2 (Preferably 600 to 1200 g / m 2 ) and the thickness is controlled at a height of 0.8mm~1.5mm. After gluing, it is pressed by a roller and put into a cooling box at 5~30℃ to cool steadily, and the product is kept flat during cooling. According to actual needs, the finished soft-bottom carpet is cut to a certain size. In the manufacturing method of the soft bottom carpet made using the regenerated yarn, the detection data is as follows:

[0042] Example 2: Elastic recovery rate of caster chair test For a finished tile carpet measuring 500mm x 500mm, the total thickness of the sample was measured using a thickness gauge, and valid data was recorded. The measured carpet was placed on the bottom plate of the caster chair tester and fixed, the legs of a simulated caster chair with a load of 90kg were placed on the carpet, and the rotation speed was set to 2000 rpm and the device was operated. After the rotation was completed, the sample carpet was removed and left to stand horizontally for 24 hours. After the above steps were completed, the total thickness of the sample was measured again using the thickness gauge, and valid data was obtained. The valid data was compared to calculate the elastic recovery rate.

[0043] Referring to the method of Example 1 of the present invention, a recycled yarn soft-bottom carpet and a recycled yarn soft-bottom carpet without non-essential structures were manufactured.

[0044] Conclusion: The higher the percentage, the higher the elastic recovery and the better the elasticity. [Table 1] [Table 2]

[0045] 2 Elastic recovery by hexapod drum test - supplementary data on excellent elasticity The total thickness of the finished carpet tiles was measured using a thickness gauge and valid data was recorded. After cutting, the samples were attached to the inner wall of a drum and placed in a hexapod drum testing machine, which was set to 12,000 RPM and operated. After the rotation was complete, the carpet samples were removed and left to stand horizontally for 24 hours. After the above steps were completed, the total thickness of the samples was measured again using a thickness gauge and valid data was obtained. The valid data was compared to calculate the elastic recovery rate.

[0046] Conclusion: The higher the percentage, the higher the elastic recovery and the better the elasticity. [Table 3] [Table 4]

[0047] 3 Hardness test - supplementary data on flexible material and high comfort For the finished tile carpet measuring 500mm x 500mm, 25 sampling points were uniformly defined, and the data of each sampling point was measured and recorded using a hardness tester in a specific order, and finally, valid measurement data was obtained as the average value of the 25 sampling points.

[0048] Conclusion: The lower the number, the more flexible and soft it is. [Table 5] [Table 6]

[0049] 4. Insulation effect of carpets – supplementary data on their excellent insulation effect The finished carpet tiles were cut to the exact size of the iron plate and covered with the iron plate of the equipment. The temperature of the equipment was set to 80°C and maintained until the end of the test. After the finished carpet tiles were placed on the iron plate of the equipment at 80°C, the initial temperature of the center of the carpet surface was immediately measured and valid data was recorded, and then the time was measured and one thermal conductivity temperature test of the carpet surface was performed every 6 minutes and valid data was recorded.

[0050] Conclusion: A low surface temperature results in poor thermal conductivity and good insulation. [Table 7] [Table 8]

Claims

[Claim 1] A method for manufacturing a soft-bottom carpet using recycled yarn, comprising the steps of: A carpet fiber tufting step (1) of tufting carpet fibers made of nylon fibers into a first long fiber nonwoven fabric to obtain a carpet fiber layer; a latex precoating and drying step (2) in which aqueous latex SBR, antibacterial agent, calcium carbonate, and foaming agent are uniformly mixed in a mass ratio of (62-100):(0-1):(0-35):(0-2), and air foamed using a foaming machine at a foaming ratio of 1.2 to 10 times, and the mixture is uniformly applied to the back surface of the carpet fiber layer in an amount of 50 to 800 g / m 2 , and then dried at a drying temperature of 140 to 200° C. for a drying time of 2 to 8 minutes to obtain a latex layer; (3) a tufting step of the regenerated fibers, which comprises doubling the regenerated fibers made of nylon fibers to form thick regenerated fibers of 850D to 4000D, and tufting the thick regenerated fibers into a second long fiber nonwoven fabric to obtain a regenerated fiber layer having a pile density of 100,000 fibers / m 2 to 450,000 fibers / m 2 on the pile surface and a pile height of 2.5 mm to 12 mm; PO and calcium carbonate are added in a mass ratio of (20-45):(55-80), then heated and melted, uniformly stirred, cooled and granulated to obtain PO-calcium carbonate adhesive chips, which are then added to a tile carpet laminating machine and heated and melted at 130-220°C, then coated on the pile surface of the recycled fiber layer by an extruder, scraped up to a height of 0.5mm-1.0mm using a doctor knife or doctor roller, etc., so that the amount of PO-calcium carbonate adhesive used is 150-2000g / m2 per square meter, the recycled fiber layer and the nonwoven fabric layer are bonded, pressed with a roller, and cooled at 5-30°C to form a recycled fiber tufted soft bottom layer; PO and calcium carbonate are mixed in a mass ratio of (25-50):(50-75), heated and melted, cooled and granulated to obtain PO-calcium carbonate adhesive chips, which are then fed into a tile carpet laminating machine, heated and melted at 130-220°C, and evenly applied to the tufted back surface of the recycled fiber tufted soft bottom layer by an extruder, and excess parts are scraped off using a doctor knife or a doctor roller, and the PO-calcium carbonate adhesive is bonded to the latex surface of the carpet fiber layer, and the amount of PO-calcium carbonate adhesive used is controlled to 500g / m2-2500g / m2 per square meter, and the thickness is controlled to 0.8mm-1.5mm, and after bonding, the mixture is pressed with a roller, and cooled in a cooling box at 5-30°C.

Citation Information

Patent Citations

  • Sheet material, block-like sheet material, method for manufacturing sheet materials and method for separating and recovering fiber formed and packing layers from tile carpet

    JP2005282348A

  • Fiber layer material or block or long sheet material and method of utilizing the material

    JP2006116298A

  • Regeneration reuse system of tile installed carpet in use and regenerated tile carpet

    JP2007159949A

  • Automobile mat excellent in sliding nature prevention

    JP2010046421A

  • Method for processing lining of tufted carpet and tufted carpet made from method for processing lining

    JP2010162275A