Etching method and etching apparatus
The etching method using HF and NH3 gases with controlled ratios and temperatures effectively addresses the challenge of etching a three-layer stacked film, ensuring high selectivity and efficiency in semiconductor manufacturing.
Patent Information
- Application Number
- JP2020188278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-11
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-11-11
AI Technical Summary
Existing methods struggle to efficiently etch a three-layer stacked film consisting of a first silicon oxide film, a silicon nitride film, and a second silicon oxide film simultaneously with high selectivity.
An etching method using a combination of HF and NH3 gases, with controlled gas ratios and temperatures, to etch the three-layer stacked film collectively, optimizing the process to minimize loading and ensure high selectivity.
Enables simultaneous and selective etching of the three-layer stacked film, enhancing throughput and minimizing damage to underlying structures like Si films, while maintaining high selectivity and efficiency.
Smart Images

Figure 0007561579000001 
Figure 0007561579000002 
Figure 0007561579000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an etching method and an etching apparatus. [Background technology]
[0002] Recently, a method called Chemical Oxide Removal (COR) has been known in the manufacturing process of semiconductor devices, which performs chemical etching without generating plasma in a chamber. A known COR technique uses hydrogen fluoride (HF) gas, which is a fluorine-containing gas, and ammonia (NH) gas, which is a basic gas, on the silicon oxide film (SiO2 film) present on the surface of a semiconductor wafer, which is a substrate (see, for example, Patent Documents 1 and 2). In this technique, HF gas and NH3 gas react with the silicon oxide film to generate ammonium silicofluoride ((NH4)2SiF6; AFS), which is then sublimated by heating, thereby etching the silicon oxide film. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-39185 A [Patent Document 2] JP 2008-160000 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides an etching method and an etching apparatus capable of simultaneously removing a three-layer laminate film consisting of a first silicon oxide film, a silicon nitride film, and a second silicon oxide film. [Means for solving the problem]
[0005] An etching method according to one embodiment of the present disclosure includes the steps of: placing a substrate having a three-layer film formed by stacking a first silicon oxide-based film, a silicon nitride-based film, and a second silicon oxide-based film in a chamber; and using an HF-NH3-based gas to etch the three-layer film all at once in the chamber while adjusting the gas ratio for each film. Effect of the Invention
[0006] According to the present disclosure, there is provided an etching method and an etching apparatus capable of simultaneously removing a three-layer laminate film consisting of a first silicon oxide film, a silicon nitride film, and a second silicon oxide film. [Brief description of the drawings]
[0007] [Figure 1] 1 is a cross-sectional view showing an example of an etching apparatus used to carry out an etching method according to an embodiment. [Diagram 2] 1 is a flowchart illustrating an etching method according to an embodiment. [Diagram 3] 1 is a cross-sectional view showing a schematic example of a structure of a substrate to which an etching method according to an embodiment is applied; [Figure 4] 4 is a cross-sectional view showing a schematic state in which the ONO laminated film is etched in the substrate of FIG. 3. FIG. [Diagram 5] 4A to 4C are diagrams illustrating in detail an etching process of step ST2 in the etching method according to the embodiment. [Figure 6] FIG. 13 is a diagram showing the relationship between HF / (HF+NH3) and the selectivity of SiO2 to SiN when a SiO2 film and a SiN film are etched by changing the ratio of NH3 gas and HF gas. [Figure 7] FIG. 13 is a graph showing the relationship between the temperature of the mounting table and the amount of etching of each film when the ALD-SiN film and the Th-SiO2 film are etched while the temperature of the mounting table is changed from 90 to 120° C., and showing the selectivity of the ALD-SiN film to the Th-SiO2 film. [Figure 8]FIG. 1 is a diagram showing a mechanism by which Si is etched when an ONO laminate film is etched. [Figure 9] FIG. 13 is a diagram showing the relationship between the amount of a Th-SiO2 film etched and the amount of a-Si film etched when the Th-SiO2 film is etched with HF gas and NH3 gas at each temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment will be described with reference to the drawings.
[0009] <Etching equipment> FIG. 1 is a cross-sectional view showing an example of an etching apparatus used to carry out an etching method according to an embodiment.
[0010] As shown in FIG. 1, the etching apparatus 1 includes a chamber 10 having a sealed structure, and inside the chamber 10, a mounting table 12 is provided on which a substrate W is placed in a substantially horizontal state.
[0011] The etching apparatus 1 also includes a gas supply mechanism 13 that supplies a process gas to the chamber 10, and an exhaust mechanism 14 that exhausts the inside of the chamber 10.
[0012] The chamber 10 is composed of a chamber body 21 and a lid 22. The chamber body 21 has a substantially cylindrical side wall 21a and a bottom 21b, and the top is open, which is closed by the lid 22 having a recess therein. The side wall 21a and the lid 22 are sealed by a seal member (not shown), ensuring airtightness inside the chamber 10.
[0013] A shower head 26, which is a gas introduction member, is fitted inside the lid 22 so as to face the mounting table 12. The shower head 26 has a cylindrical main body 31 and a shower plate 32 provided at the bottom of the main body 31. An intermediate plate 33 is provided in parallel to the shower plate 32 in the space formed by the main body 31 and the shower plate 32, and a first space 34a is formed between the upper wall 31a of the main body 31 and the intermediate plate 33, and a second space 34b is formed between the intermediate plate 33 and the shower plate 32.
[0014] A first gas supply pipe 61 of the gas supply mechanism 13 is inserted into the first space 34a, and a plurality of gas passages 35 connected to the first space 34a extend from the intermediate plate 33 through a spacer 36 provided in the second space 34b to the upper surface of the shower plate 32. The gas passages 35 are connected to a plurality of first gas discharge holes 37 formed in the shower plate 32. Meanwhile, a second gas supply pipe 63 of the gas supply mechanism is inserted into the second space 34b, and a plurality of second gas discharge holes 38 formed in the shower plate 32 are connected to the second space 34b.
[0015] Then, the gas supplied from the first gas supply pipe 61 to the first space 34a is discharged into the chamber 10 through the gas passage 35 and the first gas discharge hole 37. Also, the gas supplied from the second gas supply pipe 63 to the second space 34b is discharged from the second gas discharge hole 38. That is, this is a post-mix type in which the gas supplied from the first gas supply pipe 61 and the gas supplied from the second gas supply pipe 63 are mixed after being discharged from the shower head 26.
[0016] Alternatively, the shower head may be of a premix type in which the gas supplied from the first gas supply pipe 61 and the gas supplied from the second gas supply pipe 63 are mixed in the shower head.
[0017] A loading / unloading port 41 for loading and unloading the substrate W is provided on the side wall portion 21a of the chamber main body 21. This loading / unloading port 41 can be opened and closed by a gate valve 42, allowing the substrate W to be transported between other adjacent modules.
[0018] The mounting table 12 has a generally circular shape in a plan view, and is fixed to the bottom 21b of the chamber 10. A temperature regulator 45 that regulates the temperature of the mounting table 12 is provided inside the mounting table 12. The temperature regulator 45 can be composed of, for example, a temperature regulation medium flow path through which a temperature regulation medium (e.g., water) that regulates the temperature circulates, or a resistance heater. The temperature regulator 45 regulates the temperature of the mounting table 12 to a desired temperature, thereby controlling the temperature of the substrate W placed on the mounting table 12.
[0019] The gas supply mechanism 13 includes an HF gas supply source 51, an Ar gas supply source 52, an NH3 gas supply source 53, and an N2 gas supply source .
[0020] The HF gas supply source 51 supplies HF gas, and the NH3 gas supply source 53 supplies NH3 gas. The Ar gas supply source 52 and the N2 gas supply source 54 supply N2 gas and Ar gas as inert gases that function as a dilution gas, a purge gas, and a carrier gas. However, both may be Ar gas or N2 gas. Also, the inert gas is not limited to Ar gas and N2 gas, and other rare gases such as He gas can be used.
[0021] These gas supply sources 51-54 are connected to one end of first to fourth gas supply pipes 61-64, respectively. The first gas supply pipe 61 connected to the HF gas supply source 51 has the other end inserted into the first space 34a of the shower head 26 as described above. The second gas supply pipe 62 connected to the Ar gas supply source 52 has the other end connected to the first gas supply pipe 61. The third gas supply pipe 63 connected to the NH3 gas supply source 53 has the other end inserted into the second space 34b of the shower head 26 as described above. The fourth gas supply pipe 64 connected to the N2 gas supply source 54 has the other end connected to the third gas supply pipe 63.
[0022] The HF gas and NH3 gas reach the first space 34a and the second space 34b of the showerhead 26 together with the inert gases Ar gas and N2 gas, respectively, and are discharged into the chamber 10 from the gas discharge holes 37 and the gas discharge holes 38.
[0023] A flow rate control unit 65 that opens and closes the flow paths and controls the flow rates is provided in the first to fourth gas supply pipes 61 to 64. The flow rate control unit 65 is composed of a flow rate control device such as an on-off valve and a mass flow controller (MFC) or a flow control system (FCS).
[0024] The exhaust mechanism 14 has an exhaust pipe 72 connected to an exhaust port 71 formed in the bottom 21b of the chamber 10, and further has an automatic pressure control valve (APC) 73 for controlling the pressure inside the chamber 10 and a vacuum pump 74 for evacuating the inside of the chamber 10, both of which are provided on the exhaust pipe 72.
[0025] Two capacitance manometers 76a, 76b for high pressure and low pressure are provided on the side wall of the chamber 10 to control the pressure inside the chamber 10. A temperature sensor (not shown) for detecting the temperature of the substrate W is provided near the substrate W placed on the mounting table 12.
[0026] The chamber 10, the shower head 26, and the mounting table 12 that constitute the etching apparatus 1 are made of a metal material such as aluminum. A coating such as an oxide coating may be formed on the surfaces of these materials.
[0027] The etching apparatus 1 further includes a control unit 80. The control unit 80 is a computer. The etching apparatus 1 is made up of a main controller equipped with a CPU, an input device, an output device, a display device, and a storage device (storage medium). The main controller controls the operation of each component of the etching apparatus 1. The main controller controls each component based on a control program stored in a storage medium (hard disk, optical disk, semiconductor memory, etc.) built into the storage device. A processing recipe is stored in the storage medium as a control program, and processing of the etching apparatus 1 is carried out based on the processing recipe.
[0028] <Etching method> Next, an etching method according to an embodiment of the present invention will be described, which is performed in the etching apparatus 1 configured as above. The following etching method is performed under the control of the control unit 80.
[0029] FIG. 2 is a flow chart illustrating an etching method according to one embodiment. First, a substrate W having a three-layer laminated film formed by laminating a first silicon oxide film, a silicon nitride film, and a second silicon oxide film in that order is placed in a chamber 10 (step ST1).
[0030] Next, in the chamber 10, the three-layer stacked film is etched at once using HF-NH3-based gas while adjusting the gas ratio for each film (step ST2).
[0031] At this time, the etching of the first silicon oxide film, the silicon nitride film, and the second silicon oxide film is performed by controlling the gas ratio so that each film is appropriately etched with a good selectivity in order to minimize loading. Also, the etching of each film is performed by appropriately controlling the temperature of the mounting table 12 and the pressure in the chamber 10.
[0032] When etching silicon oxide films and silicon nitride films with HF-NH3-based gas, ammonium silicofluoride (AFS) is generated as a reaction product. For this reason, in order to collectively etch each film constituting the three-layer laminated film in the chamber 10, it is preferable to use cycle etching in which the operation of supplying HF-NH3-based gas and the operation of purging the chamber 10 are repeated in the etching of each film. This allows the generation of AFS when HF-NH3-based gas is supplied and the sublimation of AFS by purging to be repeated, thereby progressing the etching. The number of repetitions is appropriately set according to the film thickness of each film.
[0033] This will be explained in more detail below. In step ST1, the structure of the substrate W is not limited as long as it has a three-layer laminated film, but an example of the structure can be, for example, one as shown in FIG. 3. In the example of FIG. 3, the substrate W has a Si film 101 formed on a base (not shown), and an ONO laminated film 102, which is a three-layer laminated film to be etched, formed thereon. The ONO laminated film 102 is configured by laminating a second silicon oxide film 113, a silicon nitride film 112, and a first silicon oxide film 111 in this order from the bottom. The thicknesses of the first silicon oxide film 111, the silicon nitride film 112, and the second silicon oxide film 113 are preferably in the range of 6 to 12 nm. A Si film 103 and a SiN film 104 are formed on the ONO laminated film 102, and a recess (trench or hole) 105 is formed in the Si film 103 and the SiN film 104. The Si films 101 and 103 may be poly-Si films or amorphous Si films (a-Si films).
[0034] By performing collective etching of the first silicon oxide-based film 111, the silicon nitride-based film 112, and the second silicon oxide-based film 113 on the substrate W of FIG. 3 in step ST2, the underlying Si film 101 is exposed as shown in FIG. 4.
[0035] The first silicon oxide film 111 and the second silicon oxide film 113 are mainly composed of Si and O, and may contain additives. They may be made of the same material, but are preferably made of different materials. Examples of the first silicon oxide film include a thermal oxide film (Th-SiO2 film) and a TEOS film (CVD-SiO2 film). The TEOS film is a film formed by a CVD method using tetraethoxysilane (TEOS) as a Si precursor. The TEOS film may be a PTEOS film formed by a plasma CVD method. Examples of the second silicon oxide film 113 include a SiO2 film formed by ALD (ALD-SiO2 film) and a SiON film. These are films with lower density than the thermal oxide film and TEOS film used as the first silicon oxide film 111. By making the second silicon oxide film 113 a film having a lower density than the first silicon oxide film in this manner, the second silicon oxide film 113 can be etched selectively with respect to the first silicon oxide film 111 .
[0036] The silicon nitride film 112 may contain additives and is mainly composed of Si and N. The silicon nitride film 112 is, for example, a SiN film formed by a CVD method or an ALD method (CVD-SiN film, ALD-SiN film).
[0037] 5, in step ST2, a stage of etching the first silicon oxide-based film 111 (ST2-1), a stage of etching the silicon nitride-based film 112 (ST2-2), and a stage of etching the second silicon oxide-based film 113 (ST2-3) are performed. In order to perform desired etching in these stages, the gas ratio of the HF-NH3-based gas is adjusted in the stages ST2-1 and ST2-3 for etching the silicon oxide-based film, and in the stage ST2-2 for etching the silicon nitride-based film.
[0038] FIG. 6 is a diagram showing the relationship between the ratio of HF gas to HF gas and NH3 gas (HF gas ratio; HF / (HF+NH3)×100(%)) and the selectivity of SiO2 to SiN (SiO2 / SiN) when etching an SiO2 film (Th-SiO2 film) and an SiN film with different ratios of NH3 gas and HF gas. As shown in this figure, the etching of the SiO2 film proceeds easily in the range where the NH3 gas is rich, and a high selectivity of 100 or more can be obtained with respect to the silicon nitride film when the HF gas ratio is 20% or less. However, when the HF gas ratio is less than 3%, the reaction does not proceed easily. On the other hand, the etching of the SiN film proceeds easily in the range where the HF gas is rich, and a high selectivity can be obtained with a HF gas ratio of about 99% or more. Specifically, it can be seen that the HF gas ratio is 100% and the SiO2 / SiN is 0.01 or less, that is, the selectivity of SiN to SiO2 is 100 or more.
[0039] Therefore, in the stages ST2-1 and ST2-3 for etching the silicon oxide film, the HF gas ratio is preferably 3 to 20%, more preferably 3 to 9%. In this range, a sufficient etching amount can be obtained in addition to the selectivity.
[0040] On the other hand, in ST2-2, which is the stage of etching the silicon nitride film, the HF gas ratio is preferably 99% or more, and more preferably 100%.
[0041] In the etching process of step ST2, when performing ST2-3, which is a stage of etching the second silicon oxide film 113, it is preferable to selectively etch the second silicon oxide film 113 with respect to the first silicon oxide film 111. When the first silicon oxide film 111 is a Th-SiO2 film or a CVD-SiO2 film and the second silicon oxide film 113 is an ALD-SiO2 film or a SiON film, the second silicon oxide film 113 can be selectively etched as follows. That is, by reducing the ratio of HF gas when etching the second silicon oxide film 113 compared to the etching of the first silicon oxide film 111, the second silicon oxide film 113 can be selectively etched with respect to the first silicon oxide film 111.
[0042] The gas flow rates when etching each film with the above-mentioned preferable gas ratios are preferably in the following ranges. Etching step of the first silicon oxide film 111 (ST2-1) HF gas: 50 to 100 sccm NH3 gas: 450~550sccm N2 gas + Ar gas: 300 to 600 sccm Etching step of silicon nitride film 112 (ST2-2) HF gas: 800 to 1000 sccm NH3 gas: 0 to 10 sccm N2 gas + Ar gas: 300 to 600 sccm Etching step of the second silicon oxide film 113 (ST2-3) HF gas: 30 to 50 sccm (less than when etching the first silicon oxide film) NH3 gas: 450~550sccm N2 gas + Ar gas: 300 to 600 sccm
[0043] Regarding the pressure in step ST2, it is preferable to set the pressure to a relatively low level in the stages (ST2-1 and ST2-3) of etching the first and second silicon oxide films 111, 113. This allows the first and second silicon oxide films 111, 113 to be etched selectively with respect to the silicon nitride film 112. On the other hand, it is preferable to set the pressure to a relatively high level in the stage (ST2-2) of etching the silicon nitride film 112. This allows the silicon nitride film 112 to be etched selectively with respect to the first and second silicon oxide films 111, 113.
[0044] More preferably, the pressure is 5 Torr (667 Pa) or less in the steps of etching the first and second silicon oxide films 111, 113 (ST2-1 and ST2-3), and 5 to 100 Torr (667 to 13,332 Pa) in the step of etching the silicon nitride film 112 (ST2-2).
[0045] The substrate temperature (temperature of the mounting table) in the step (ST2-2) of etching the silicon nitride film 112 is preferably 80 to 100° C., and more preferably 90 to 100° C. By setting the temperature within this range, the silicon nitride film 112 can be etched at a realistic etching amount and with a high selectivity to the first and second silicon oxide films 111, 113.
[0046] Fig. 7 shows the relationship between the temperature of the mounting stage and the etching amount of each film, and the selectivity of the ALD-SiN film to the Th-SiO2 film when an ALD-SiN film and a Th-SiO2 film are etched with 100% HF gas at pressures of 20 Torr and 50 Torr and the temperature of the mounting stage is changed from 90 to 120°C. As shown in this figure, at 90 to 100°C, it is possible to etch the SiN film with a realistic etching amount and with a high selectivity to the SiO2 film. At 105°C, the selectivity is high but the etching amount is small.
[0047] In addition, in the substrate W having the structure of FIG. 3, a high selectivity to the Si films 101 and 103 is required in the etching of each film of the ONO laminated film 102, but if the temperature is low, Si will be etched. The model is as follows. FIG. 8 is a diagram showing a model in which Si is etched when the ONO laminated film is etched. For example, when the first and second silicon oxide-based films 111 and 113 are etched, as shown in FIG. 8, H2O is generated in the process of generating AFS by performing etching with HF gas and NH3 gas. If the temperature is low, H2O remains, and reacts with NH3, which is the introduced gas, and Si will be alkaline etched. In order to suppress this reaction, it is preferable to remove H2O by increasing the substrate temperature. FIG. 9 is a diagram showing the relationship between the etching amount of the Th-SiO2 film and the etching amount of the a-Si film when the Th-SiO2 film is etched with HF gas and NH3 gas at each temperature. As shown in this figure, the selectivity of the Th-SiO2 film to the a-Si film tends to be low at 85°C, but a relatively high selectivity is obtained at 90°C, and the amount of a-Si etched decreases as the temperature increases. Therefore, in order to selectively etch each film to Si in step ST2, the mounting table temperature (substrate temperature) is preferably 90°C or higher. As mentioned above, the amount of SiN film etched is small at 105°C, so 90 to 100°C is preferable.
[0048] Considering the above results of the selectivity of the SiN film to the SiO2 film and the selectivity of the SiO2 film to the Si film, the substrate temperature (temperature of the mounting table) during etching of the ONO stacked film 102 in step ST2 is preferably 80 to 100° C., more preferably 90 to 100° C. Within this range, the temperature may be changed in the stages (ST2-1 to ST2-3) where each film is etched, but it is preferable to keep them at substantially the same temperature.
[0049] In the stages (ST2-1 to ST2-3) of etching each film in step ST2, as described above, it is preferable to perform cycle etching in which an operation of supplying an HF-NH3-based gas to generate a reaction product and an operation of purging the chamber 10 to sublimate the reaction product are repeatedly performed. After etching of the ONO laminated film 102 is completed, it is preferable to carry out the substrate W from the chamber 10 and perform a heat treatment for removing residues by a heating device.
[0050] The time for one operation of supplying HF-NH3-based gas during cycle etching of each film is preferably in the range of 20 to 60 seconds. Also, the time for one purge operation is preferably 3 minutes or more from the viewpoint of sufficiently removing AFS, and more preferably in the range of 3 to 5 minutes. However, when a heat treatment is performed to remove residues after etching of the ONO laminated film 102 is completed, the purge time in the final stage (ST2-3) of etching the second silicon oxide-based film 113 may be short, and is preferably in the range of 30 to 60 seconds.
[0051] The purging operation may involve simply drawing a vacuum inside the chamber 10, or may involve supplying a purge gas while drawing a vacuum. As the purge gas, Ar gas and / or N2 gas supplied from the Ar gas supply source 52 and / or N2 gas supply source 54 may be used. In order to effectively exhaust the AFS, it is preferable to only perform the vacuum drawing.
[0052] During the purging operation, the temperature of the mounting table 12 is set to a temperature at which sublimation of the AFS generated on the substrate W can proceed. If the temperature of the mounting table 12 is in the above-mentioned temperature range of 80 to 100° C., the AFS, which is a reaction product, can be sufficiently removed by the purging operation in the cycle etching.
[0053] In the substrate W having the structure shown in FIG. 3, selectivity to the SiN film 104 is also required when etching the ONO laminated film 102. The SiN film 104 is the same type of film as the silicon nitride-based film 112 of the ONO laminated film 102, but the loss of the SiN film 104 can be reduced by lengthening the purging time when cycle etching the silicon nitride-based film 112 to reduce AFS and H2O as much as possible. This makes it possible to ensure selectivity to the SiN film 104 when etching the silicon nitride-based film 112. The purging time in this case is preferably in the range of 3 to 5 minutes.
[0054] After etching of each film is completed, the chamber 10 is purged. As the purge gas, Ar gas and / or N2 gas supplied from the Ar gas supply source 52 and / or the N2 gas supply source 54 can be used. After etching of the second silicon oxide-based film 113 is completed, the chamber is purged in this manner, and then the substrate W is carried out from the chamber 10.
[0055] As shown in the above-mentioned Patent Document 1, gas etching of SiO2 film with HF gas and NH3 gas has been known for some time. Meanwhile, ONO laminated film as the subject of this embodiment is often used in the structure of a semiconductor device, and etching of the ONO laminated film is required. When etching the ONO laminated film, in order to minimize loading, it is necessary to etch the SiO2 film and the SiN film with high selectivity, and conventionally, gas etching of the SiO2 film and wet etching of the SiN film have been used in combination.
[0056] In contrast, in this embodiment, the gas ratios of the first silicon oxide film, silicon nitride film, and second silicon oxide film constituting the ONO laminate film are optimized, and a cycle etch is applied, making it possible to etch the ONO laminate film in one step by gas etching. This allows the ONO laminate to be etched with a higher throughput using a simpler process than before.
[0057] Furthermore, when a Si film is present adjacent to the ONO laminated film, it is required to etch the ONO laminated film with a high selectivity to the Si film. In particular, as shown in FIG. 3, the Si film 101 underlying the ONO laminated film 102 often becomes the functional part (channel, etc.) of a transistor, and is required to be etched as little as possible when the ONO laminated film 102 is etched. In contrast, in this embodiment, as described above, the ONO laminated film can be etched with a high selectivity to the Si film.
[0058] <Other applications> Although the embodiments have been described above, the embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims.
[0059] For example, the devices in the above-described embodiments are merely illustrative, and devices of various configurations can be applied. In addition, although a semiconductor wafer is exemplified as the substrate, other substrates such as an FPD (flat panel display) substrate and a ceramic substrate may also be used. [Explanation of symbols]
[0060] 1. Etching equipment 10. Chamber 12;Placement table 13. Gas supply mechanism 14; Exhaust mechanism 26; Shower head 45;Temperature controller 51;HF gas source 53;NH3 gas source 80; Control section 101, 103;Si film 102;ONO laminated film 104;SiN film 105; Recess 111: First silicon oxide film 112;Silicon nitride film 113: Second silicon oxide film W; Substrate
Claims
1. Providing a substrate having a three-layer laminated film formed by laminating a first silicon oxide film, a silicon nitride film, and a second silicon oxide film in a chamber; In the chamber, HF-NH 3 a step of simultaneously etching the three-layered film using a base gas while adjusting the gas ratio for each film; The etching method according to claim 1,
2. The first silicon oxide film, the silicon nitride film, and the second silicon oxide film are etched using a HF-NH 3 2. The etching method according to claim 1, wherein the etching is performed by cycle etching in which an operation of supplying a system gas to generate a reaction product and an operation of purging the inside of the chamber to sublimate the reaction product are repeatedly performed.
3. 3. The etching method according to claim 2, wherein the purging operation for said first silicon oxide film, said silicon nitride film, and said second silicon oxide film is performed for a period of 3 to 5 minutes.
4. The method further includes a step of removing the substrate from the chamber after the etching step, and a step of heating the removed substrate to remove residues, 3. The etching method according to claim 2, wherein the purging operation time for the first silicon oxide film and the silicon nitride film is 3 to 5 minutes, and the purging operation time for the second silicon oxide film is 30 to 60 seconds.
5. 3. The etching method according to claim 2, wherein the substrate has a SiN film in a portion other than the three-layer laminated film, and the purging operation is performed for a period of 3 to 5 minutes when etching the silicon nitride film.
6. When etching the first silicon oxide film and the second silicon oxide film, the HF-NH 3 The system gases are HF gas and NH 3 Gas is HF / (HF+NH 3 ) is 3 to 20%, and when etching the silicon nitride film, the HF-NH 3 The system gases are HF gas and NH 3 Gas is HF / (HF+NH 3 6. The etching method according to claim 1, wherein the gases are supplied at a gas ratio such that the ratio of the nitrogen gas to the oxygen gas is 99% or more.
7. 7. The etching method according to claim 1, wherein a pressure in the chamber is set to 667 Pa or less when etching the first silicon oxide film and the second silicon oxide film, and a pressure in the chamber is set to a range of 667 to 13,332 Pa when etching the silicon nitride film.
8. 8. The etching method according to claim 1, wherein the temperature of the substrate when etching the silicon nitride film is 80 to 100.degree.
9. 9. The etching method according to claim 8, wherein the temperature of the substrate when etching the three-layer laminated film is 80 to 100.degree.
10. 10. The etching method according to claim 9, wherein the substrate has Si adjacent to the three-layered film, and the temperature of the substrate is in the range of 90 to 100° C. when etching the three-layered film.
11. Etching of the three-layer stacked film starts from the first silicon oxide film and ends at the second silicon oxide film; 11. The etching method according to claim 1, wherein the first silicon oxide-based film is a thermal oxide film or a TEOS film, and the second silicon oxide-based film is a silicon oxide film formed by ALD or a SiON film.
12. 12. The etching method according to claim 11, wherein a flow rate of HF gas during etching of the second silicon oxide film is set to be smaller than that during etching of the first silicon oxide film.
13. a chamber for accommodating a substrate having a three-layer laminated film formed by laminating a first silicon oxide-based film, a silicon nitride-based film, and a second silicon oxide-based film; a mounting table on which the substrate is placed within the chamber; a gas supply unit for supplying a basic gas and a fluorine-containing gas into the chamber; an exhaust unit that exhausts the inside of the chamber; a temperature control unit for controlling a temperature of the substrate on the mounting table; A control unit; Equipped with The control unit applies HF-NH 3 and controlling the gas supply unit, the exhaust unit, and the temperature adjustment unit so that the three-layer stacked film is etched at the same time while adjusting the gas ratio for each film by using a system gas.
14. The control unit is configured to determine whether the etching of each of the first silicon oxide film, the silicon nitride film, and the second silicon oxide film is performed using HF-NH 3 14. The etching apparatus according to claim 13, wherein the operation of supplying the system gas to generate a reaction product and the operation of purging the chamber to sublimate the reaction product are repeatedly performed.
15. When etching the first silicon oxide film and the second silicon oxide film, the control unit 3 The system gases are HF gas and NH 3 Gas is HF / (HF+NH 3 ) is 3 to 20%, and when etching the silicon nitride film, the HF-NH 3 The system gases are HF gas and NH 3 Gas is HF / (HF+NH 3 15. The etching apparatus according to claim 13, wherein the gases are supplied at a gas ratio such that the ratio of the oxygen to the nitrogen is 99% or more.
16. 16. The etching apparatus according to claim 13, wherein the control unit controls the pressure in the chamber to 667 Pa or less when etching the first silicon oxide-based film and the second silicon oxide-based film, and controls the pressure in the chamber to a range of 667 to 13,332 Pa when etching the silicon nitride-based film.
17. 17. The etching apparatus according to claim 13, wherein the control unit controls the temperature of the substrate to 80 to 100.degree. C. when etching the three-layer laminated film.
18. Etching of the three-layer stacked film starts from the first silicon oxide film and ends at the second silicon oxide film, the first silicon oxide film is a thermal oxide film or a TEOS film, and the second silicon oxide film is a silicon oxide film formed by ALD or a SiON film, 18. The etching apparatus according to claim 13, wherein the control unit controls a HF gas flow rate during etching of the second silicon oxide film so as to be lower than a flow rate during etching of the first silicon oxide film.
Citation Information
Patent Citations
Work processing apparatus, work processing method therefor, pressure control method, work carrying method, and carrying apparatus
JP2005039185A
Gas processing apparatus, gas processing method, and storage medium
JP2008160000A
Etching apparatus and etching method
JP2014060220A
Substrate processing method and substrate processing apparatus
JP2016154209A
Etching method