Resin composition

The resin composition, with a polysilane-based first polymer and UV-absorbing second polymer, addresses the limitations of conventional PVA films by enhancing UV absorption and heat resistance, enabling high-speed and precise UV laser processing.

JP7561599B2Active Publication Date: 2024-10-04FUJI COPIAN
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020210787
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-10-04
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Conventional resist films made of PVA have poor heat resistance and low UV laser absorption, limiting processing speed and precision, and adding ultraviolet absorbers leads to precipitation and insufficient UV laser absorption improvement.

Method used

A resin composition comprising a first polymer with a polysilane skeleton and a second polymer with ultraviolet absorbing monomer units, balanced to enhance UV absorption and heat resistance, allowing high-speed and precise UV laser processing.

Benefits of technology

The resin composition enables high-speed and high-precision UV laser processing with improved heat and plasma resistance, preventing ultraviolet absorber bleeding and maintaining film integrity during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561599000001
    Figure 0007561599000001
  • Figure 0007561599000002
    Figure 0007561599000002
  • Figure 0007561599000003
    Figure 0007561599000003
Patent Text Reader

Abstract

To achieve an ultraviolet laser processing resist which can be processed highly accurately at a high speed.SOLUTION: A resin composition for an ultraviolet laser processing resist contains a first polymer having a polysilane skeleton and a second polymer having no polysilane skeleton. The first polymer has: a first block having a polysilane skeleton; and a second block which is a copolymer of vinyl monomers and contains an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having ultraviolet absorbing action. The second polymer is a copolymer of (meth)acrylate monomers and has a first monomer unit derived from a first monomer having ultraviolet absorbing action and a second monomer unit derived from a second monomer having no ultraviolet absorbing action. The content of the second polymer is 3 pts.mass or more and 50 pts.mass or less based on 100 pts.mass of the first polymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a resin composition, and in particular to a resin composition for use as an ultraviolet laser processing resist. [Background technology]

[0002] Dicing is performed to divide a semiconductor wafer into individual devices. Dicing is generally performed by scribing or sawing. In recent years, plasma dicing, which etches a predetermined portion of a wafer using plasma, has been attracting attention.

[0003] In plasma dicing, a mask made of a resist film is formed on the wafer, and the parts of the wafer exposed through the mask are then plasma etched to separate them into individual devices. The mask must be able to accurately form the pattern for etching, and also be able to protect the elements on the wafer from the plasma.

[0004] The mask can be formed by patterning a photoresist film using standard lithography operations. However, this method has a problem with the cost of mask formation. It has also been considered to form a mask by directly patterning a resist film made of polyvinyl alcohol (PVA) using an ultraviolet (UV) laser instead of a photoresist film (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-165963 A Summary of the Invention [Problem to be solved by the invention]

[0006] Conventional resist films made of PVA and the like have poor heat resistance and low UV laser absorption, which means that processing speeds cannot be increased and high-precision processing is difficult. Adding UV absorbers to resist films has also been considered, but increasing the amount added causes precipitation of the UV absorbers, making it difficult to sufficiently improve UV laser absorption. Furthermore, adding UV absorbers does not solve the problem of low heat resistance of resist films.

[0007] Furthermore, to protect the elements on the wafer from plasma, the resist film needs to be sufficiently thick. However, in the case of conventional resist films made of PVA, increasing the thickness of the film further reduces processability, making it difficult to make the film sufficiently thick.

[0008] An object of the present disclosure is to realize an ultraviolet laser processing resist that can be processed at high speed and with high precision. [Means for solving the problem]

[0009] One embodiment of the resin composition for ultraviolet laser processing resist of the present disclosure contains a first polymer and a second polymer, the first polymer having a first block having a polysilane skeleton and a second block which is a copolymer of a vinyl monomer and contains an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having ultraviolet absorbing activity, the second polymer being a copolymer of an acrylate monomer or a methacrylate monomer and having a first monomer unit derived from the first monomer having ultraviolet absorbing activity and a second monomer unit derived from a second monomer not having ultraviolet absorbing activity, and the second polymer is 3 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the first polymer.

[0010] In one embodiment of the resin composition for ultraviolet laser processing resist, the ultraviolet absorbing monomer and the first monomer have an ultraviolet absorbing group, and the ultraviolet absorbing group in the ultraviolet absorbing monomer and the ultraviolet absorbing group in the first monomer are the same and can be any one of a benzotriazole skeleton, a benzophenone skeleton, and a triazine skeleton.

[0011] In one embodiment of the resin composition for ultraviolet laser processing resist, the ratio of the first monomer unit in the second polymer can be 40 mass % or more and 80 mass % or less.

[0012] In one embodiment of the resin composition for ultraviolet laser processing resist, the proportion of the ultraviolet absorbing monomer units in the first polymer can be 3 mass% or more and 70 mass% or less, and the proportion of the polysilane skeleton in the first polymer can be 30 mass% or more and 97 mass% or less.

[0013] In one embodiment of the resin composition for ultraviolet laser processing resist, the ultraviolet transmittance at a wavelength of 355 nm can be 2% or less.

[0014] One embodiment of the resist material of the present disclosure contains the resin composition of the present disclosure and a solvent. Effect of the Invention

[0015] According to the resin composition of the present disclosure, it is possible to realize an ultraviolet laser processing resist that can be processed at high speed and with high precision. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The resist agent of this embodiment contains a resin composition (resist polymer) and a solvent. The resist agent of this embodiment can be directly patterned by an ultraviolet (UV) laser, and can be used, for example, to form a mask for plasma dicing. The resist polymer contained in the resist agent of this embodiment contains a first polymer and a second polymer.

[0017] The first polymer is a copolymer including a first block having a polysilane skeleton and a second block made of a polymer of a vinyl monomer.

[0018] The first block is made of polysilane, has a main chain formed by silicon-silicon bonds, and has an organic substituent on the side chain. The main chain formed by silicon-silicon bonds may be linear or branched, or may have a ring structure. The organic substituent on the side chain is not particularly limited, and can be preferably an alkyl group, an aryl group, an aralkyl group, or the like. The alkyl group may be linear or branched, or may have a ring structure. It may also be an organic substituent containing a heteroatom. The molecular weight of the polysilane, which is the first block, is not particularly limited, but from the viewpoint of handleability as a resist agent, the number average molecular weight (Mn) is preferably 500 or more, more preferably 800 or more, and preferably 3000 or less, more preferably 2500 or less. The weight average molecular weight (Mw) is preferably 800 or more, more preferably 1000 or more, and preferably 4000 or less, more preferably 3000 or less.

[0019] The second block is made of a polymer of a vinyl monomer, and at least a part of the monomer units constituting the second block is an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having an ultraviolet absorbing group. Therefore, the second block has an ultraviolet absorbing effect. The ultraviolet absorbing group is not particularly limited, but can be, for example, a benzotriazole skeleton, a benzophenone skeleton, or a triazine skeleton. The ultraviolet absorbing monomer may have a vinyl group and an ultraviolet absorbing group, but from the viewpoint of polymerization and the like, an acrylic monomer that is an acrylic acid ester derivative (acrylate) or a methacrylic acid ester derivative (methacrylate) is preferable. Specifically, as the ultraviolet absorbing monomer, 3-(2H-benzotriazol-2-yl)-4-hydroxyphenethyl=methacrylate, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate, or 2-[4-(4,6-diphenyl)-[1,3,5]triazin-2-yl]-3-hydroxy-phenoxy}-ethylprop-2-enoate, etc. can be used. In the following, acrylate or methacrylate will be referred to as (meth)acrylate.

[0020] The first polymer, which includes a first block having a polysilane skeleton and a second block having an ultraviolet absorbing function, can be prepared by mixing and reacting polysilane with an ultraviolet absorbing monomer. Radicals can be generated in the polysilane by irradiation with ultraviolet light, and therefore the ultraviolet absorbing monomer can be copolymerized with the polysilane.

[0021] The proportion of the first block having a polysilane skeleton in the entire first polymer is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 60% by mass or more from the viewpoint of heat resistance, and is preferably 97% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less from the viewpoint of exerting an ultraviolet absorbing effect.

[0022] The proportion of the monomer units derived from the ultraviolet absorbing monomer in the entire first polymer is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of exerting an ultraviolet absorbing effect, and is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less, from the viewpoint of heat resistance.

[0023] The first polymer may contain a monomer unit derived from an ultraviolet non-absorbing monomer that does not have an ultraviolet absorbing group such as a benzotriazole skeleton and does not exhibit ultraviolet absorbing properties. The ultraviolet non-absorbing monomer is not particularly limited, but may be an acrylic monomer such as a (meth)acrylic acid ester or a (meth)acrylamide derivative. By adding a (meth)acrylic acid alkyl ester having an alkyl group with 4 or more carbon atoms, the resist film can be made flexible to improve adhesion to the wafer, and the processability can be further improved. In addition, by adding a hydrocarbon monomer that has a higher plasma etching resistance than polysilane, the plasma resistance of the resist film can be improved.

[0024] The non-UV absorbing monomer can be copolymerized with the polysilane together with the UV absorbing monomer to form a structural unit of the second block, or may be included in the first polymer as a structural unit of a block different from the second block.

[0025] The proportion of monomer units derived from non-UV absorbing monomers in the entire first polymer is preferably 15 mass % or less, and more preferably 10 mass % or less.

[0026] The second polymer is a polymer of a vinyl monomer having compatibility with the first polymer and having ultraviolet absorbing properties. In this embodiment, the second polymer is a copolymer containing a first monomer unit derived from a first monomer having ultraviolet absorbing properties and a second monomer unit derived from a second monomer having no ultraviolet absorbing properties. From the viewpoint of compatibility with the first polymer, the first monomer and the second monomer are preferably acrylic monomers that are (meth)acrylates.

[0027] From the viewpoint of compatibility with the first polymer, the first monomer preferably has the same ultraviolet absorbing group as the ultraviolet absorbing monomer used in the polymerization of the first polymer. The first monomer may be the same monomer as the ultraviolet absorbing monomer.

[0028] The second monomer is preferably a (meth)acrylate monomer that copolymerizes with the first monomer that does not have an ultraviolet absorbing group. Specifically, methyl methacrylate or the like can be used as the second monomer. The second monomer is not limited to one type, and two or more types of monomers may be mixed.

[0029] The first monomer and the second monomer may be alternately copolymerized, randomly copolymerized, or block copolymerized.

[0030] The proportion of the first monomer unit in the second polymer can be within a range that can impart ultraviolet absorbency to the second polymer, but is preferably 40% by mass or more, more preferably 50% by mass or more, and preferably 80% by mass or less, more preferably 70% by mass or less.

[0031] The weight average molecular weight (Mw) of the second polymer is not particularly limited, but from the viewpoint of compatibility with the first polymer, it is preferably 20,000 or more, more preferably 30,000 or more, and preferably 80,000 or less, more preferably 60,000 or less.

[0032] The ratio of each block and each monomer unit in the first polymer and the second polymer is based on the amount charged when the polymers are polymerized, but can also be determined by compositional analysis of the polymers.

[0033] In the resist polymer of this embodiment, the ratio of the second polymer to 100 parts by mass of the first polymer is, from the viewpoint of improving the processing speed and processing accuracy, preferably 3 parts by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, and preferably 50 parts by mass or less, more preferably 45 parts by mass or less.

[0034] The resist polymer of this embodiment has excellent ultraviolet absorption properties because it contains a first polymer having an ultraviolet absorbing function and a second polymer having an ultraviolet absorbing function. In addition, since the compatibility between the first polymer and the second polymer is high, bleeding of the ultraviolet absorber, which occurs when a low molecular weight ultraviolet absorber is added, does not occur. Furthermore, since the first polymer contains a first block having a polysilane skeleton, it has excellent heat resistance and plasma resistance. Therefore, the resist film using the resist polymer of this embodiment can be patterned at high speed and high precision using a UV laser. The resist film using the resist polymer of this embodiment can be laser processed at a processing speed faster than 600 mm / s, and can be processed well even at 700 mm / s or 800 mm / s, and shows sufficient processability up to about 1000 mm / s. It is also possible to laser process at a processing speed of 600 mm / s or less.

[0035] The resist agent of the present embodiment can be prepared by dissolving the first polymer and the second polymer in a solvent, or by mixing a solution in which the first polymer is dissolved with a solution in which the second polymer is dissolved.

[0036] The solvent is not particularly limited as long as it can dissolve the resist polymer, and may be, for example, toluene, tetrahydrofuran, methyl ethyl ketone, propylene glycol monomethyl ether acetate, cyclohexanone, etc. The solvent may be a mixed solvent in which two or more types of solvents are mixed.

[0037] The proportion of the resist polymer in the entire resist agent can be adjusted depending on the thickness of the resist film to be formed, etc., but is preferably 10 mass % or more, more preferably 25 mass % or more, and preferably 70 mass % or less, more preferably 60 mass % or less.

[0038] The resist agent may not contain any components other than the resist polymer and the solvent, but may contain other components. Examples of other components include additive components such as leveling agents, light stabilizers, and antioxidants, and polymer components such as acrylic resins, polyester resins, and epoxy resins. The ratio of other components is 10 parts by mass or less, more preferably 5 parts by mass or less, per 100 parts by mass of the resist polymer. In addition, the resist agent may contain residues such as unpolymerized polysilane and vinyl polymer when the first polymer and the second polymer are polymerized.

[0039] The resist agent of this embodiment can be coated on the surface of a wafer by a method such as spin coating to form a resist film. The formed resist film can be patterned by removing street portions by irradiation with a UV laser. The patterned resist film can be used as a mask to irradiate the wafer with plasma and etch the wafer, thereby performing dicing of the wafer. The thickness of the resist film formed on the surface of the wafer is not particularly limited, but is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more from the viewpoint of resist properties, and is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less from the viewpoint of laser processability.

[0040] The wavelength of the UV laser light used for patterning the resist agent of this embodiment is not particularly limited, but may be about 200 nm to 400 nm, and preferably 355 nm. The frequency of the laser light is also not particularly limited, but may be, for example, about 1 kHz to 300 kHz, and a high frequency is preferable from the viewpoint of high speed processing.

[0041] The resist agent of the present embodiment can be used not only in plasma dicing of wafers, but also as a resist agent capable of laser patterning, and as a protective film in processes requiring heat resistance. EXAMPLES

[0042] The resin composition of the present disclosure will be described in more detail below using examples. The following examples are illustrative and are not intended to limit the present invention.

[0043] <Formation of resist film> The prepared resist agent was applied to the surface of a silicon wafer (φ8 inch, thickness 700 μm) using a spin coater, and the solvent was dried to form a resist film. The rotation speed of the spin coater was 200 rpm, and the thickness of the resist film was 30 μm.

[0044] <Evaluation of liquid stability over time> The prepared resin solution was placed in a transparent, sealed container and allowed to stand at room temperature for 7 days, after which the appearance of the resin solution and the presence or absence of precipitate were visually observed and the liquid stability over time was evaluated according to the following evaluation criteria.

[0045] (Evaluation Criteria) A: The solution is free of turbidity and precipitate.

[0046] B: Slight cloudiness but no sediment.

[0047] C: Separation or precipitation is observed.

[0048] <Evaluation of heat resistance> 5 g of the produced resin solution was placed in an aluminum cup and dried in an oven at 100°C for 180 minutes to evaporate the solvent. The non-volatile components remaining in the aluminum cup were measured for 10% weight loss temperature using a thermogravimetric differential thermal analyzer (TG-DTA). The measurement conditions were a temperature rise rate of 20°C / min and heating from 30°C to 600°C in a nitrogen atmosphere. The measurement results were evaluated for heat resistance according to the following evaluation criteria.

[0049] (Evaluation Criteria) A: The 10% weight loss temperature is 250℃ or higher.

[0050] B: The 10% weight loss temperature is 200°C or higher and less than 250°C.

[0051] C: 10% weight loss temperature is less than 200°C.

[0052] <Evaluation of coating surface quality> The surface condition of the formed resist film was visually observed and the coating surface quality was evaluated according to the following evaluation criteria.

[0053] (Evaluation Criteria) A: The coating is uniform and free of irregularities.

[0054] B: Slight unevenness (citrus peel) is observed.

[0055] C: The coating has defects such as cracks and graininess.

[0056] <Evaluation of laser processability> The surface of the formed resist film was patterned using a UV laser processing device (AL300P, manufactured by Tokyo Seimitsu) to create a checkerboard pattern with a line width of 15 μm, line length of 15 mm, and a pitch of 1 mm. The processing conditions were laser wavelength: 355 nm, pulse width: <15 ns, and frequency: 50 kHz. The processing speed was 600 mm / sec or 800 mm / sec. The laser-processed portion was observed at a magnification of 200 times using a microscope, and the laser processability was evaluated according to the following evaluation criteria.

[0057] (Evaluation Criteria) A: There is no peeling of the coating film at the laser processing end, and there is no resist residue.

[0058] B: A trace amount of resist residue remains at the laser processing end.

[0059] C: A part of the resist film remains in the laser irradiation part, or defects such as peeling and cracking of the coating film are observed at the laser processing end.

[0060] <Evaluation of resist property> After evaluating the laser processability, plasma etching treatment was performed from the resist film side using a plasma etching apparatus. The processing conditions at this time were: plasma source: ICP plasma power 2200 W, process gas: SF6 gas, gas pressure: 2 Pa, processing time: 7 minutes. The surface of the resist film after the plasma etching treatment was magnified 200 times with a microscope and the resist property was evaluated according to the following evaluation criteria.

[0061] (Evaluation criteria) A: No erosion of the resist film due to plasma etching is observed.

[0062] B: Erosion due to plasma etching is observed, but there is no exposure of the silicon wafer.

[0063] C: The resist film disappears and exposure of the silicon wafer is observed.

[0064] <Measurement of UV transmittance> The manufactured resin solution was applied to the surface of a polyethylene terephthalate (PET) film with a thickness of 50 μm using a spin coater to form a resin film. The film thickness after drying of the resin film was 10 μm. The transmittance of ultraviolet light with a wavelength of 355 nm for the PET film on which the resin film was formed was measured using a spectrophotometer. Subtracting the transmittance of the PET film before forming the resin film from the obtained transmittance as a blank, the transmittance of the resin film was obtained.

[0065] (Example 1) The first polymer was a copolymer of polysilane and a methacrylate-based ultraviolet absorbing monomer having a benzotriazole skeleton. The polysilane used had a number average molecular weight (Mn) of 900 and a weight average molecular weight (Mw) of 1100 (Oxol SI-20-10, manufactured by Osaka Gas Chemicals). The ultraviolet absorbing monomer was (3-(2H-benzotriazol-2-yl)-4-hydroxyphenethyl methacrylate (RUVA-93, manufactured by Otsuka Chemicals). 44.2 g of polysilane and 15.8 g of the ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to obtain a solution of the first polymer. The copolymerization was performed under a nitrogen gas flow with a liquid temperature of 60°C to 70°C, and a high-pressure mercury lamp (UV intensity: 170 mW / cm 2 ) and irradiated with ultraviolet light for 60 minutes.

[0066] When the polymer was separated from the solution of the first polymer by gel permeation chromatography (GPC) and analyzed by infrared spectroscopy (IR), a spectrum was obtained that was a composite of the spectrum of the polysilane and the spectrum of the ultraviolet absorbing monomer. 1 The peak of the acrylic polymer chain was confirmed at a chemical shift of 0.5 ppm to 4.5 ppm by HNMR spectroscopy. From these results, it was determined that the obtained first polymer was a copolymer of polysilane and an ultraviolet absorbing monomer. The Mw of the obtained first polymer was 3900.

[0067] The second polymer was a copolymer (Banaresin UVA-7075, manufactured by Shin-Nakamura Chemical Co., Ltd.) obtained by polymerizing a methacrylate monomer having a benzotriazole skeleton as the first monomer and methyl methacrylate as the second monomer. The ratio of the first monomer to the second polymer was 70% by mass, and the weight average molecular weight (Mw) was 30,000 to 50,000. Toluene was added to a solution containing 3.16 g of the second polymer to adjust the amount of solvent to 23.1 g, to prepare a solution of the second polymer.

[0068] A resist agent was prepared by mixing a solution of the first polymer and a solution of the second polymer. The ratio of the second polymer to 100 parts by mass of the first polymer in the resist agent was 5.3 parts by mass. The ratio of the solid content of the first polymer and the second polymer combined in the resist agent was 50% by mass. The obtained resist agent was evaluated for liquid stability over time, coating surface quality, laser processability, resist properties, heat resistance, and UV transmittance. The liquid stability over time was A, the coating surface quality of the resist film was A, the laser processability was A when the processing speed was 600 mm / s and B when it was 800 mm / s, the resist properties were A, the heat resistance was A, and the UV transmittance was 0%.

[0069] Example 2 The second polymer solution was prepared in the same manner as in Example 1, except that the second polymer was 6.68 g and the solvent was 26.6 g.

[0070] The ratio of the second polymer to 100 parts by mass of the first polymer was 11.1 parts by mass, and the solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0071] Example 3 The second polymer solution was prepared in the same manner as in Example 1, except that the second polymer was 15.0 g and the solvent was 35.0 g.

[0072] The ratio of the second polymer to 100 parts by mass of the first polymer was 25.0 parts by mass, and the solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0073] Example 4 The second polymer solution was prepared in the same manner as in Example 1, except that the second polymer was 25.7 g and the solvent was 45.7 g.

[0074] The ratio of the second polymer to 100 parts by mass of the first polymer was 42.8 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was B, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0075] Example 5 The same procedure as in Example 1 was carried out except that the second polymer was a resin (Banaresin UVA-8050, manufactured by Shin-Nakamura Chemical Co., Ltd.) having a weight average molecular weight (Mw) of 40,000 to 60,000, in which the ratio of the first monomer to the second polymer was 50 mass%, and the solution of the second polymer was made of 6.68 g of the second polymer and 26.6 g of the solvent.

[0076] The ratio of the second polymer to 100 parts by mass of the first polymer was 11.1 parts by mass, and the solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0077] Example 6 The same procedure as in Example 2 was carried out except that 57.0 g of polysilane and 3.0 g of an ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to obtain a solution of a first polymer.

[0078] The ratio of the second polymer to 100 parts by mass of the first polymer was 11.1 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A when the processing speed was 600 mm / s and B when it was 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0079] Example 7 The same procedure as in Example 2 was carried out except that 18.0 g of polysilane and 42.0 g of an ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to obtain a solution of a first polymer.

[0080] The ratio of the second polymer to 100 parts by mass of the first polymer was 11.1 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was B, and the UV transmittance was 0%.

[0081] Example 8 The procedure was the same as in Example 2, except that the polysilane used was a polysilane having an Mn of 1100 and an Mw of 1800 (Ogsol SI-10-20, manufactured by Osaka Gas Chemicals).

[0082] The ratio of the second polymer to 100 parts by mass of the first polymer was 11.1 parts by mass, and the solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0083] The conditions and evaluation results of Examples 1 to 8 are shown in Table 1.

[0084] [Table 1]

[0085] (Reference example 1) The first polymer was prepared by dissolving 52.5 g of polysilane and 22.5 g of ultraviolet absorbing monomer in 75 g of toluene and copolymerizing them, and the resist agent was prepared without adding the second polymer. The resist film was evaluated with a thickness of 10 μm.

[0086] The liquid stability over time was A, the coating surface quality was A, the laser processability was A when the processing speed was 600 mm / s and B when it was 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0087] (Reference example 2) The same procedure as in Reference Example 1 was repeated, except that the evaluation was performed with the resist film having a thickness of 30 μm.

[0088] The liquid stability over time was A, the coating surface quality was A, the laser processability was A when the processing speed was 600 mm / s and C when it was 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.

[0089] The conditions and evaluation results of Reference Examples 1 and 2 are shown in Table 2.

[0090] [Table 2]

[0091] Comparative Example 1 The resist agent was prepared by dissolving 75.0 g of polyvinyl alcohol (PVA-205, manufactured by Kuraray) in 75.0 g of distilled water.

[0092] The liquid stability over time was A, the coating surface quality was A, the laser processability was C at a processing speed of 600 mm / s, the resist property was A, the heat resistance was C, and the UV transmittance was 90%. Note that the processability at a processing speed of 800 mm / s was not evaluated.

[0093] Comparative Example 2 The resist agent was prepared by dissolving 75.0 g of polysilane (Ogsol SI-20-10, manufactured by Osaka Gas Chemicals) in 75.0 g of toluene.

[0094] The liquid stability over time was A, the coating surface quality was A, the laser processability was C at a processing speed of 600 mm / s, the resist property was B, the heat resistance was A, and the UV transmittance was 63%. Note that the processability at a processing speed of 800 mm / s was not evaluated.

[0095] Comparative Example 3 The resist agent was prepared by dissolving 52.5 g of polysilane (Oxol SI-20-10, manufactured by Osaka Gas Chemicals) and 22.5 g of a benzotriazole-based ultraviolet absorber (2-(2-hydroxy-5-t-butylphenyl)benzotriazole, Tinuvin PS, manufactured by BASF Japan) in 75.0 g of toluene. The liquid stability over time was rated C, the coating surface quality was rated C, and other items could not be evaluated.

[0096] The conditions and evaluation results of Comparative Examples 1 to 3 are shown in Table 3.

[0097] [Table 3]

[0098] Comparative Example 4 The procedure was the same as in Example 1, except that the solution of the second polymer was prepared by dissolving 3.2 g of an acrylic resin (Dianal BR-113, manufactured by Mitsubishi Chemical) having a number average molecular weight of 30,000 in 23.2 g of toluene. The liquid stability over time was B, the coating surface quality was C, and other items could not be evaluated.

[0099] Comparative Example 5 The procedure was the same as in Comparative Example 4, except that 57.0 g of polysilane and 3.0 g of an ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to prepare a solution of a first polymer. The liquid stability over time was B, the coating surface quality was C, and other items could not be evaluated.

[0100] Comparative Example 6 The procedure was the same as in Comparative Example 4, except that 18.0 g of polysilane and 42.0 g of an ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to prepare a solution of a first polymer. The liquid stability over time was B, the coating surface quality was C, and other items could not be evaluated.

[0101] Comparative Example 7 The procedure was the same as in Example 1, except that the second polymer solution was prepared by adding toluene to a solution containing 3.2 g of a polyester resin (Vylon UR-1400, manufactured by Toyobo Co., Ltd.) having a number average molecular weight of 40,000 to make the amount of solvent 23.2 g. The solution stability over time was rated C, the coating surface quality was rated C, and other items could not be evaluated.

[0102] The conditions and evaluation results of Comparative Examples 4 to 7 are shown in Table 4.

[0103] [Table 4] [Industrial Applicability]

[0104] INDUSTRIAL APPLICABILITY The resin composition of the present disclosure has excellent laser processability and is useful as an ultraviolet laser processing resist, etc.

Claims

1. The composition comprises a first polymer and a second polymer, the first polymer has a first block having a polysilane skeleton and a second block which is a copolymer of a vinyl monomer and contains an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having an ultraviolet absorbing effect; the second polymer is a copolymer of an acrylate monomer or a methacrylate monomer, and has a first monomer unit derived from a first monomer having an ultraviolet absorbing function and a second monomer unit derived from a second monomer having no ultraviolet absorbing function; A resin composition for an ultraviolet laser processing resist, wherein the second polymer is 3 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the first polymer.

2. the ultraviolet absorbing monomer and the first monomer have an ultraviolet absorbing group, 2. The resin composition for ultraviolet laser processing resist according to claim 1, wherein the ultraviolet absorbing group in the ultraviolet absorbing monomer and the ultraviolet absorbing group in the first monomer are the same and have a benzotriazole skeleton, a benzophenone skeleton, or a triazine skeleton.

3. 3. The resin composition for an ultraviolet laser processing resist according to claim 1, wherein a ratio of the first monomer unit in the second polymer is 40 mass % or more and 80 mass % or less.

4. a ratio of the ultraviolet absorbing monomer unit in the first polymer is 3 mass% or more and 70 mass% or less, The resin composition for ultraviolet laser processing resist according to any one of claims 1 to 3, wherein the proportion of the polysilane skeleton in the first polymer is 30 mass% or more and 97 mass% or less.

5. The resin composition for ultraviolet laser processing resist according to any one of claims 1 to 4, which has an ultraviolet transmittance of 2% or less at a wavelength of 355 nm.

6. A resist agent comprising the resin composition according to any one of claims 1 to 5 and a solvent.

Citation Information

Patent Citations

  • Method for forming pattern on substrate by ultraviolet laser beams

    JP1991109553A

  • Positive type resist composition and patterning method

    JP2002196494A

  • Silicon-based positive resist composition, and patterning method

    JP2002226664A

  • Silicon resin composition and process for forming inorganic porous thin film

    JP2003327782A

  • Ultraviolet curable ultraviolet-shielding resin composition

    JP2006307151A