Semiconductor manufacturing components and their manufacturing method

A silicon carbide-containing boron carbide film addresses the corrosion and processing challenges of boron carbide focus rings by enhancing corrosion resistance and facilitating precise shaping for semiconductor manufacturing components.

JP7562482B2Active Publication Date: 2024-10-07COORSTEK GK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021097822
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-28
Filing Date
2021-06-11
Publication Date
2024-10-07
Estimated Expiration
2041-06-11

AI Technical Summary

Technical Problem

Boron carbide focus rings used in plasma processing devices exhibit poor corrosion resistance against oxygen plasma and are difficult to process due to their hardness, leading to high costs and challenges in achieving suitable shapes and surface textures.

Method used

A silicon carbide-containing boron carbide film with a specific weight percentage and porosity range is applied to the surface of a base material, enhancing corrosion resistance against oxygen and Ar plasma, and allowing for easier processing using existing silicon manufacturing techniques.

Benefits of technology

The silicon carbide-containing boron carbide film improves corrosion resistance and reduces plasma exposure, enabling precise shaping of semiconductor manufacturing components like focus rings with reduced damage and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562482000001
    Figure 0007562482000001
  • Figure 0007562482000002
    Figure 0007562482000002
  • Figure 0007562482000003
    Figure 0007562482000003
Patent Text Reader

Abstract

To provide a member for manufacturing a semiconductor formed of boron carbide, in which the processing shape can be obtained easily and the corrosion resistance in the reaction with oxygen plasma in particular is excellent.SOLUTION: A member for manufacturing a semiconductor includes a film, which is formed of silicon carbide and boron carbide contained, on a surface, and the film contains the silicon carbide by 5 wt% or more and 18 wt% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor manufacturing member and a method for manufacturing the same, and more particularly to a semiconductor manufacturing member suitable for a focus ring used in, for example, a plasma processing apparatus, and a method for manufacturing the same. [Background technology]

[0002] In a semiconductor device manufacturing process, a plasma processing apparatus such as a plasma etching apparatus or a plasma CVD apparatus is used to perform processing such as etching on a substrate to be processed. In this case, a focus ring is disposed as a semiconductor manufacturing component so as to surround the periphery of the substrate to be processed in order to make the plasma processing of the substrate uniform. This focus ring is provided on the outside of the substrate to be processed. For example, by placing the substrate to be processed on its inner periphery, a so-called pseudo substrate to be processed (pseudo wafer) is formed around the substrate to be processed, thereby achieving uniform plasma processing of the substrate to be processed (the wafer).

[0003] The focus ring is generally made of silicon and is formed into a ring shape having an outer diameter larger than that of the substrate to be processed. Specifically, the focus ring is manufactured, for example, by cutting a disk-shaped member from a single crystal silicon ingot and then removing a central portion of the disk-shaped member.

[0004] As mentioned above, focus rings have conventionally been manufactured by machining a silicon ingot into a ring shape, but boron carbide (B4C) is expected to become a more durable material in the future. Boron carbide has excellent corrosion resistance because it does not easily react with oxygen-free fluorine-based and chlorine-based corrosive gases or oxygen-free plasma. Even if it reacts with fluorine or chlorine, a reactant with high vapor pressure is generated, so that it is released outside the system as a gas without generating particles.

[0005] Patent Document 1 states that it is desirable for boron carbide to be made of a sintered body with a relative density of 98% or more. This is because if the boron carbide has a low density and a large number of pores, the contact area with corrosive gases and plasma increases accordingly, and wear is accelerated. For this reason, it is preferable for the boron carbide to have a relative density of 98% or more, particularly 99% or more, and furthermore, an open porosity of 0.2 or less. It is considered necessary for the material to be a dense body having a density of less than 50%.

[0006] Furthermore, according to Patent Document 1, as the diameter of silicon wafers increases, the manufacturing equipment and components themselves also become larger, and therefore, in order to maintain the durability of the components, it is desirable for them to have a flexural strength of 300 MPa or more. According to the manufacturing method disclosed in Patent Document 1, for example, boron carbide powder having an average particle size of 20 μm or less is filled into a mold or formed into a desired shape, and hot pressed in a non-oxidizing atmosphere at 2100 to 2300° C. to obtain the boron carbide.

[0007] Patent Document 1 also shows that by adding sintering aids such as C (carbon), SiC, Si3N4, etc., sintering can be performed at lower temperatures in a non-oxidizing atmosphere or in a vacuum, and further that the green body or sintered body can be heat-treated in an inert atmosphere of 1000 atmospheres or more by hot isostatic sintering to further densify it. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 11-102900 Summary of the Invention [Problem to be solved by the invention]

[0009] Incidentally, in recent dry etching techniques, oxygen plasma etching, Ar plasma etching, fluorine-based plasma etching, or the like is used, and further, very high-frequency power is input.

[0010] For example, before performing anisotropic processing on a substrate using dry etching, a resist pattern is generally formed using lithography. Although the resolution of a 193 nm ArF immersion device is 38 nm, multi-patterning technology has exceeded this resolution limit to realize patterns of 10 to 7 nm.

[0011] In addition, a common method for double patterning is the sidewall process, which utilizes the residue on the pattern sidewalls formed after dry etching. Specifically, an amorphous carbon layer, a SiON layer, an anti-reflective film layer, and a resist pattern are formed by ArF immersion exposure on the SiN film on which the line pattern is ultimately to be formed.

[0012] The resist pattern is then shrunk by isotropic etching using oxygen plasma, and the anti-reflective film, SiON film, and amorphous carbon layer are dry etched in that order to form a carbon pattern. When dry etching is performed after an ALD (atomic layer deposition) film is deposited on the carbon pattern, sidewalls remain on the sides of the carbon pattern as etching residues, and when the carbon is removed, only the sidewalls remain. The SiN film is dry etched using these sidewalls as a mask, and when the mask is removed, an extremely fine line pattern is formed.

[0013] In addition, extremely deep holes must be fabricated for DRAM capacitors and 3D NAND memory holes. To form these high aspect ratio microholes, highly accurate anisotropic shapes and high selectivity for masks and underlayers are required. For this purpose, a fluorocarbon gas is used as the etchant gas, and a polymer film is deposited on the side walls of the holes in the mask and SiO2 film as a side wall protection film by CFx radicals, while the CFx + Or Ar + A technique is used in which ions such as these are drawn vertically into the holes in the SiO2 film to perform vertical etching.

[0014] Furthermore, when the hole becomes deep, the reaction products cannot be properly exhausted and may accumulate at the bottom of the hole, causing the etch to stop. In such cases, a method known as "O2 flush" is used to remove the reaction products by oxygen plasma etching.

[0015] In order to increase the etching rate of SiO2 film, it is necessary to increase the amount of ion incidence, increase the total amount of F in the radicals, and provide sufficient ion energy. To achieve this, the power of the high frequency power for plasma generation, the flow rate of the fluorocarbon gas, the power of the high frequency power for ion attraction, etc. are adjusted.

[0016] Thus, in recent dry etching techniques, oxygen plasma etching, Ar plasma etching, fluorine-based plasma etching, or the like is used, and further, very high radio frequency power is input.

[0017] However, when the focus ring (semiconductor manufacturing component) of a plasma processing device is made of boron carbide material, it is difficult to react with fluorine and chlorine-based corrosive gases or plasmas that do not contain oxygen, but when oxygen is contained (oxygen plasma), there is a problem that the corrosion resistance is poor. In addition, boron carbide is a difficult material to process due to its hardness, and it is very difficult and costly to process the shape and surface properties to a state suitable for the substrate to be processed.

[0018] The present invention has been made to solve the above-mentioned problems, and has an object to provide a semiconductor manufacturing component made of boron carbide that can be easily processed into a desired shape and has excellent corrosion resistance, particularly when reacted with oxygen plasma, and a method for manufacturing the same. [Means for solving the problem]

[0019] The present invention has been made to solve the above problems, and provides a semiconductor manufacturing member having a silicon carbide-containing boron carbide film on at least a surface thereof, the silicon carbide content being 5 wt % or more and 18 wt % or less, the remainder being boron carbide. The silicon carbide-containing boron carbide film has a porosity of 3.9% or more and 5.0% or less. Characterized by do. Also It is preferable that the film is formed on the surface of a substrate made of silicon.

[0020] In this way, at least the surface of the semiconductor manufacturing component contains 5 wt% to 18 wt% silicon carbide in boron carbide, improving corrosion resistance against oxygen plasma and Ar plasma. In addition, by reducing the porosity to 5% or less, the surface area exposed to plasma is reduced, and damage can be further reduced. Furthermore, when the substrate of the semiconductor manufacturing component is made of silicon, the substrate can be precisely machined using existing silicon manufacturing technology, and if this is used as the substrate, the shape and surface properties are controlled, so that the shape of a focus ring, for example, can be easily created without much post-processing.

[0021] In addition, the present invention has been made to solve the above problems, and a method for manufacturing a semiconductor manufacturing member includes preparing a raw material containing silicon carbide and boron carbide, spraying the raw material on a substrate, and forming a boron carbide containing 5 wt% to 18 wt% of silicon carbide. The porosity is 3.9% or more and 5.0% or less. It is characterized by forming a thermal sprayed film. The substrate may be removed from the semiconductor manufacturing member to provide only the film.

[0022] In this way, the surface of the semiconductor manufacturing member of the present invention contains 5 wt% to 18 wt% silicon carbide in boron carbide, and therefore the corrosion resistance against oxygen plasma and Ar plasma can be improved. Furthermore, when the substrate of the semiconductor manufacturing member is made of silicon, existing silicon manufacturing technology can be used for the substrate itself, and therefore, precisely machined shapes such as focus rings can be easily produced. Effect of the Invention

[0023] According to the present invention, it is possible to provide a semiconductor manufacturing component made of boron carbide that can be easily processed into a desired shape and has excellent corrosion resistance, particularly when reacted with oxygen plasma, and a method for manufacturing the same. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic configuration of a member for manufacturing a semiconductor device. [Diagram 2] 2(a) and (b) show modified examples of the semiconductor manufacturing member of FIG. [Diagram 3] FIG. 3 is a graph showing the results of the example of the present invention and the comparative example with respect to the amount of Ar sputtering. [Figure 4] FIG. 4 is a graph showing the results of an example of the present invention and a comparative example with respect to oxygen plasma consumption. [Diagram 5] FIG. 5 is a graph showing the results of the embodiment of the present invention and the comparative example with respect to the amount of fluorine plasma consumption. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Hereinafter, an embodiment of the present invention will be described with reference to Fig. 1 and Fig. 2. Note that the present invention is not limited to the embodiment described below. Fig. 1 is a cross-sectional view showing a schematic configuration of a semiconductor manufacturing member, and Fig. 2 shows a modified example of the semiconductor manufacturing member of Fig. 1, so the dimensional relationship between elements, the ratio of elements, etc. differ from the actual ones.

[0026] The illustrated semiconductor manufacturing member 100 is formed of a base material 1 and a silicon carbide-containing boron carbide film 2 formed so as to cover the surface of the base material 1 .

[0027] The base material 1 may be any material having plasma resistance, and is preferably, for example, silicon or alumina. In particular, when silicon is used as the base material 1, when forming, for example, a focus ring as the semiconductor manufacturing member 100, the shape of the base material 100 can be easily processed using existing techniques and devices.

[0028] The silicon carbide-containing boron carbide film 2 is formed to a thickness of, for example, 500 μm. The silicon carbide (SiC) content in this silicon carbide-containing boron carbide film 2 is 5 wt% or more and 18 wt% or less. The silicon carbide content is preferably more than 5 wt%, and more preferably 6 wt% or more and 10 wt% or less. If the silicon carbide content is less than 5 wt %, the corrosion resistance effect against oxygen plasma decreases, which is undesirable. On the other hand, when the silicon carbide content is 5 wt% or more, up to 18 wt%, the corrosion resistance against oxygen plasma improves. When the silicon carbide content exceeds 18 wt%, no further corrosion resistance effect can be expected.

[0029] In addition, for Ar plasma, Ar is eroded by physical corrosion. + Since ion sputtering occurs, corrosion resistance is related to the strength of atomic bonds. Since silicon carbide has smaller atomic bonds than boron carbide, increasing the amount of boron carbide added increases the sputtering rate and decreases the corrosion resistance. When the silicon carbide content is 18wt% or less, the corrosion resistance increases, and when it is further reduced to less than 5wt%, the corrosion resistance remains almost unchanged. Incidentally, the silicon carbide content has almost no effect on fluorine plasma.

[0030] In addition, in the dry etching process in semiconductor manufacturing, the process using a single gas plasma atmosphere is limited, and in most cases, interactions work in a mixed gas plasma atmosphere. Furthermore, considering advanced processes in which very high frequency power is input, it is more preferable that the silicon carbide content be 6 wt% or more and 10 wt% or less to obtain a stable corrosion resistance effect.

[0031] Although the silicon carbide-containing boron carbide film 2 is preferably formed by thermal spraying, it may be formed by a CVD method by adjusting the composition ratio of boron carbide and silicon carbide, or may be formed by a PVD method. While the CVD method can easily form high-purity films, the advantage of thermal spray coating is that it can be easily formed on a variety of substrates.

[0032] In the embodiment shown in FIG. 1, a silicon carbide-containing boron carbide film 2 is formed on the surface of the substrate 1. However, as shown in FIG. 2(a), a thick silicon carbide-containing boron carbide film 2 may be formed on the upper surface of the substrate 1, and as shown in FIG. 2(b), the substrate 1 may be removed to produce a semiconductor manufacturing component 100 consisting only of the silicon carbide-containing boron carbide film 2.

[0033] Furthermore, when the silicon carbide-containing boron carbide coating 2 is formed as a thermal spray coating, the temperature and collision speed of the raw material particles deposited on the substrate 1 during the coating formation process by thermal spraying are important factors that determine the density of the coating and its adhesion to the substrate 1. In the present invention, the temperature and impact speed of the raw material particles are not limited, but a thermal spraying method may be adopted according to the physical properties of the coating material and its application. For example, boron carbide has a high melting point of 2763°C and is oxidized in an oxygen atmosphere, so reduced pressure plasma spraying and electromagnetic acceleration plasma spraying are preferred.

[0034] In addition, silicon carbide has a sublimation temperature of 2545°C to 2730°C, which is lower than the melting point of boron carbide, 2763°C, and usually volatilizes during thermal spraying. Therefore, depending on the thermal spraying method, it may be necessary to adjust the particle size and mixing amount of silicon carbide, and the silicon carbide will have a structure dispersed as particles in the thermal sprayed film.

[0035] As described above, according to the embodiment of the present invention, a silicon carbide-containing boron carbide film 2 is formed on a substrate 1, and the boron carbide contains 5 wt% or more and 18 wt% or less of silicon carbide, more preferably 6 wt% or more and 10 wt% or less of silicon carbide, thereby improving corrosion resistance to oxygen plasma and Ar plasma. Furthermore, when the base material 1 is made of silicon, existing manufacturing techniques can be used, and therefore, it is possible to easily shape components used in semiconductor manufacturing, such as focus rings. EXAMPLES

[0036] The semiconductor manufacturing member and the manufacturing method thereof according to the present invention will be further described with reference to examples.

[0037] Example 1 In Example 1, a silicon carbide-containing boron carbide (B4C) film having a thickness of 500 μm was sprayed onto a silicon substrate to prepare a sample. The silicon carbide (SiC) content in the boron carbide film after spraying was set to 5 wt%. The surface after spraying was mirror-finished. Moreover, the porosity of the silicon carbide-containing boron carbide film, which was observed with an optical microscope and calculated with image editing software, was 3.9%. The sputtering rate of this sample was measured for Ar ions. The measurement conditions were an Ar ion beam capable of generating high energy, a voltage of 3 kV, a beam current of 25 μA, and an irradiation time of 3 hours. After that, the amount of sputtering wear was measured.

[0038] Example 2 In Example 2, the content of silicon carbide in the silicon carbide-containing boron carbide film of the sample was set to 7 wt%. The other conditions were the same as those of Example 1. The porosity of the silicon carbide-containing boron carbide film was 4.1%. The sputtering rate of this sample with respect to Ar ions was measured in the same manner as in Example 1.

[0039] Example 3 In Example 3, the silicon carbide content in the silicon carbide-containing boron carbide film of the sample was set to 18 wt%. The other conditions were the same as in Example 1. The porosity of the silicon carbide-containing boron carbide film was 5.0%. The sputtering rate of this sample with respect to Ar ions was measured in the same manner as in Example 1.

[0040] Comparative Example 1 In Comparative Example 1, the content of silicon carbide in the silicon carbide-containing boron carbide film of the sample was set to 0 wt%. The other conditions were the same as in Example 1. The porosity of the boron carbide film was 3.5%. The sputtering rate of this sample with respect to Ar ions was measured in the same manner as in Example 1.

[0041] Comparative Example 2 In Comparative Example 2, a silicon carbide film (100%) having a thickness of 500 μm was formed on a silicon substrate by a CVD method to prepare a sample. The other conditions were the same as those in Example 1. The porosity of the silicon carbide film was 0%. The sputtering rate of this sample with respect to Ar ions was measured in the same manner as in Example 1.

[0042] Comparative Example 3 In Comparative Example 3, a silicon substrate having no film formed on its surface was used as a sample. The other conditions were the same as in Example 1. The sputtering rate of this sample with respect to Ar ions was measured in the same manner as in Example 1.

[0043] The graph in Fig. 3 shows the results of Examples 1, 2, and 3 and Comparative Examples 1, 2, and 3. In the graph in Fig. 3, the vertical axis represents the etching amount (μm / h). As shown in the graph of FIG. 3, it was found that the amount of etching was suppressed by forming a silicon carbide-containing boron carbide film on the silicon surface (Comparative Example 1, Examples 1, 2, and 3).

[0044] Example 4 The etching rate for oxygen plasma was measured for a sample prepared in the same manner as in Example 1. The etching rate for oxygen plasma was measured by exposing the sample to oxygen plasma for 30 minutes at a reduced pressure of 2.66 Pa, high frequency power of 800 W, O2=50 sccm, and 200°C using an ICP plasma etching device. After that, the amount of wear was measured.

[0045] Example 5 The same experiment as in Example 4 was carried out on a sample prepared in the same manner as in Example 2.

[0046] Example 6 The same experiment as in Example 4 was carried out on a sample prepared in the same manner as in Example 3.

[0047] Comparative Example 4 The experiment of Example 4 was carried out on a sample prepared in the same manner as in Comparative Example 1.

[0048] Comparative Example 5 The experiment of Example 4 was carried out on a sample prepared in the same manner as in Comparative Example 2.

[0049] Comparative Example 6 The experiment of Example 4 was carried out on a sample prepared in the same manner as in Comparative Example 3.

[0050] The graph in Fig. 4 shows the results of Examples 4, 5, and 6 and Comparative Examples 4, 5, and 6. In the graph in Fig. 4, the vertical axis represents the etching amount (μm / h). As shown in the graph of Figure 4, when a boron carbide film is formed on a silicon surface, it was found that the amount of etching was suppressed by setting the silicon carbide content to 5% (Example 4), 7% (Example 5), and 18% (Example 6).

[0051] Example 7 The etching rate for fluorine plasma was measured for a sample prepared in the same manner as in Example 1. The etching rate for fluorine plasma was measured using an ICP plasma etching device, in which the sample was exposed to fluorine plasma for 4 hours at room temperature under a reduced pressure of 2.66 Pa, with a high frequency power of 500 W / bias power of 40 W, and CF4=100 sccm. After that, the amount of wear was measured.

[0052] Example 8 The experiment of Example 7 was carried out on a sample prepared in the same manner as in Example 2.

[0053] Example 9 The experiment of Example 7 was carried out on a sample prepared in the same manner as in Example 3.

[0054] Comparative Example 7 The experiment of Example 7 was carried out on a sample prepared in the same manner as in Comparative Example 1.

[0055] Comparative Example 8 The experiment of Example 7 was carried out on a sample prepared in the same manner as in Comparative Example 2.

[0056] Comparative Example 9 The experiment of Example 7 was carried out on a sample prepared in the same manner as in Comparative Example 3.

[0057] The graph in Fig. 5 shows the results of Examples 7, 8, and 9 and Comparative Examples 7, 8, and 9. In the graph in Fig. 5, the vertical axis represents the etching amount (μm / h). As shown in the graph of FIG. 5, no difference in effectiveness was observed when a boron carbide film, a silicon carbide film, or a boron carbide film with varying silicon carbide content was formed on a silicon surface.

[0058] Example 10 A silicon production member was manufactured in the same manner as in Example 1. However, the thermal spray coating was made thicker to 2.0 mm, and then the silicon substrate was polished and removed. Tests equivalent to those in Examples 1, 4, and 7 were carried out, and the corrosion resistance to various plasmas was equivalent to those in Examples 1, 4, and 7.

[0059] Comparative Example 10 A silicon production member was manufactured in the same manner as in Example 1. However, the thickness of the sprayed film was changed to 100 μm, 200 μm, and 300 μm. As a result, at 100 μm and 200 μm, the sprayed film was slightly non-uniform with a porosity of about 10 to 20%. At 300 μm, the sprayed film was formed almost uniformly, and the porosity was 5% or less.

[0060] From the results of Examples 1 to 10, it was confirmed that the corrosion resistance against Ar plasma and oxygen plasma can be improved by setting the silicon carbide content in the boron carbide film to 5 wt% or more and 18 wt% or less. It was found that the effect is particularly large when the silicon carbide content in the boron carbide film is 6 wt% or more and 10 wt% or less. [Explanation of symbols]

[0061] 1 Base material 2. Silicon carbide-containing boron carbide film 100 Semiconductor manufacturing materials

Claims

1. A semiconductor manufacturing member, comprising: a silicon carbide-containing boron carbide film on at least a surface thereof, the silicon carbide content of which is 5 wt % or more and 18 wt % or less, with the remainder being boron carbide; and the silicon carbide-containing boron carbide film having a porosity of 3.9% or more and 5.0% or less.

2. 2. The member for use in semiconductor manufacturing according to claim 1, wherein the film is formed on a substrate, and the substrate is made of silicon.

3. A method for manufacturing a semiconductor manufacturing member, comprising preparing a raw material containing silicon carbide and boron carbide, spraying the raw material onto a substrate, and forming a sprayed film consisting of boron carbide containing 5 wt% or more and 18 wt% or less of silicon carbide, and having a porosity of 3.9% or more and 5.0% or less.

4. A method for producing a member for use in semiconductor production, comprising removing a base material from the member for use in semiconductor production according to claim 3.

Citation Information

Patent Citations

  • Preparation method of boron carbide-silicon carbide composite coating

    CN103540890A

  • Corrosion resistant member for manufacturing semiconductor

    JP1999102900A

  • Boron carbide based sintered compact and protective member

    JP2008297134A

  • Ring-shaped element for etcher and method for etching substrate using the same

    JP2020027945A