Iron removal from carbon nanotubes and metal catalyst recycling

The method of oxidizing carbon nanotubes with carbon dioxide and carbon monoxide efficiently removes impurities from carbon nanotubes, maintaining their integrity and enabling catalyst recycling, addressing the inefficiencies of existing purification methods.

JP7562688B2Active Publication Date: 2024-10-07NANOCOMP TECHNOLOGIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022550722
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-24
Filing Date
2021-02-23
Publication Date
2024-10-07
Estimated Expiration
2041-02-23

AI Technical Summary

Technical Problem

Existing methods for purifying carbon nanotubes are inefficient and damaging, as they often require high temperatures and pressures, leading to defects and alteration of the nanotubes, while residual metal catalysts and amorphous carbon are difficult to remove without damaging the carbon nanotubes.

Method used

A method involving oxidation with carbon dioxide at elevated temperatures followed by exposure to carbon monoxide gas to remove amorphous carbon and metal catalysts, with the option to recycle the metal catalysts, using a floating catalytic chemical vapor deposition system to maintain low to moderate temperatures and pressures.

Benefits of technology

The method effectively purifies carbon nanotubes by removing impurities while preserving their structure, achieving purity levels below 10% by weight of metal and amorphous carbon, with the potential for recycling the metal catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562688000001
    Figure 0007562688000001
  • Figure 0007562688000002
    Figure 0007562688000002
  • Figure 0007562688000003
    Figure 0007562688000003
Patent Text Reader

Abstract

The present disclosure provides methods for purifying nanostructured materials containing carbon nanotubes, metal impurities, and amorphous carbon impurities. The methods generally involve oxidizing the raw nanostructured material to remove the amorphous carbon, thereby exposing the metal impurities, and subsequently contacting the nanostructured material with carbon monoxide to volatilize the metal impurities, thereby substantially removing them from the nanostructured material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 62 / 980,513, filed February 24, 2020, the entire contents of which are expressly incorporated herein by reference.

[0002] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT This invention was made with Government support under DE-AR0001017 awarded by the DOE, Office of ARPA-E. The Government has certain rights in this invention.

[0003] Field The present disclosure generally relates to methods for purifying carbon nanostructured materials, including carbon nanotubes, by removing impurities formed during their manufacture, such as metal catalysts and particles of amorphous carbon, without substantially damaging or destroying the carbon nanotubes. [Background technology]

[0004] Iron, nickel and cobalt nanoparticles are frequently used as catalysts to promote the initiation and growth of carbon nanotubes. This is true for most carbon nanotube synthesis methods, including forest growth, floating bed, HIPCO, laser ablation, arc and floating catalytic chemical vapor deposition. In many of these methods, including floating catalytic chemical vapor deposition, the metal nanoparticles that successfully create carbon nanotubes remain attached to the nanotubes they create, and the metal nanoparticles that are not successful, typically because they are too large or too small to initiate carbon nanotube growth, are captured as part of the as-created nanotube material. Once carbon nanotubes are formed, these residual metal nanoparticles have no useful contribution to the properties of the carbon nanotubes, and in fact are typically considered parasitic mass in the as-created nanotube material, or worse, are considered chemically or physically undesirable. Similarly, these methods also involve the production of various amounts of carbon material in the as-created nanotube material that is not in the form of nanotubes. In the following, this non-nanotube carbon material will be referred to as "amorphous carbon".

[0005] Removing the residual metal particles and amorphous carbon without damaging the nanotubes can be difficult. Typical methods include vacuum or inert gas bakeout at high temperatures (i.e., above 1600° C.), partial oxidation followed by dissolution of the exposed metal or metal oxide with acids or etchants, and gas phase removal by reaction with halogen-containing gases. Each of these methods can damage the nanotubes by forming defects, removing valuable carbon material, or altering the nanotubes themselves by graphitizing or otherwise.

[0006] Therefore, there is a need for an efficient and safe method for preparing purified carbon nanotubes; in particular, the method should efficiently remove amorphous carbon and metal catalyst impurities at low to moderate temperatures and pressures without damaging or destroying the carbon nanotubes. Summary of the Invention

[0007] Summary of the Invention The present disclosure relates to a method for purifying carbon nanotubes. Known methods for producing carbon nanotubes produce carbon nanotubes that contain impurities including residual metal catalyst particles and small amounts of amorphous carbon sheets that surround the metal catalyst particles and appear on the sides of the carbon nanotubes. The purification method of the present disclosure substantially removes extraneous amorphous carbon and metal-containing residual catalyst particles without damaging or destroying the carbon nanotubes, resulting in carbon nanostructured materials.

[0008] Thus, according to one aspect, the present disclosure relates to a method for purifying carbon nanostructured material, the method comprising the steps of: (a) obtaining a quantity of as-prepared raw carbon nanostructured material, the raw carbon nanostructured material comprising carbon nanotubes and essentially contaminated with metal catalyst particles and other non-nanotube (i.e., amorphous) carbon structures; (b) oxidizing the raw carbon nanostructured material by exposure to carbon dioxide at an elevated temperature, the oxidation removing the non-nanotube carbon structures to form a carbon dioxide treated carbon nanostructured material and carbon monoxide; (c) exposing the carbon dioxide treated carbon nanostructured material to a flowing gas comprising at least the carbon monoxide produced in step (b); (d) increasing the temperature of the carbon dioxide treated carbon nanostructured material and the flowing gas to about 20° C. to about 200° C. to produce a gas stream comprising purified carbon nanostructured material and volatile metal species; and (e) transferring the gas stream away from the purified carbon nanostructured material.

[0009] In a further embodiment, after the gas stream is transferred from the purified carbon nanostructured material, it is passed through a condenser to condense the volatile metal species and separate the carbon monoxide, which may then be recovered and recycled to the process of forming new as-prepared raw carbon nanostructured material, and the carbon monoxide may be recycled into the flowing gas of step (c). [Brief description of the drawings]

[0010] [Figure 1A] FIG. 1 shows a schematic diagram of a floating catalyst chemical vapor deposition system for the production of nanostructures in accordance with an embodiment of the present disclosure. [Figure 1B] FIG. 1B is a schematic diagram of an injector apparatus for use in conjunction with the system shown in FIG. 1A. [Figure 1C] FIG. 1 shows a schematic diagram of a floating catalyst chemical vapor deposition system utilizing a plasma generator for the production of nanostructures in accordance with an embodiment of the present disclosure. [Figure 1D] FIG. 1D is a schematic diagram of a plasma generator suitable for use in connection with the system of FIG. 1C. [Diagram 2] 1 shows a schematic flow diagram of the various steps of the method of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present disclosure generally provides a method for producing highly purified carbon nanostructured materials, which are substantially free of metal catalysts used in the production process and amorphous carbon produced in the production process. In one embodiment, the purified carbon nanostructured materials contain less than about 10% by weight of metals used in the production of the unpurified nanostructured materials. In another embodiment, the purified carbon nanostructured materials contain less than about 8% by weight of such metals, or less than about 7% by weight of such metals, or less than about 6% by weight of such metals, or less than about 5% by weight of such metals, or less than about 2.5% by weight of such metals, or less than about 1% by weight of such metals, or less than about 0.5% by weight of such metals, or even less than about 0.1% by weight of such metals. Furthermore, in one embodiment of the present disclosure, the purified carbon nanostructured materials contain less than about 10% by weight of amorphous carbon. In another embodiment, the purified carbon nanostructure material contains less than about 5% amorphous carbon by weight, or less than about 2% amorphous carbon by weight, or less than about 1% amorphous carbon by weight, or less than about 0.5% amorphous carbon by weight, or even less than about 0.1% amorphous carbon by weight.

[0012] The purified carbon nanostructured material is free of (a) carbon nanotubes, metal impurities, and amorphous carbon; (b) oxidizing the as-prepared raw carbon nanostructured material in a gas atmosphere containing carbon dioxide to form carbon monoxide and carbon dioxide treated carbon nanostructured material; (c) exposing the carbon dioxide treated carbon nanostructured material to a flowing gas containing at least carbon monoxide formed in step (b); (d) increasing the temperature of the carbon dioxide treated carbon nanostructured material and the flowing gas to a maximum temperature of about 20° C. to about 200° C. to produce a gas stream containing purified carbon nanostructured material and volatile metal species; and (e) transferring the gas stream from the purified carbon nanostructured material. The disclosed method is particularly suitable for use in connection with raw carbon nanostructured material produced from a floating catalyst chemical vapor deposition process. However, the method is also readily adaptable for use in connection with raw carbon nanostructured material produced by other metal catalyst processes.

[0013] The following terms shall have the following meanings:

[0014] The term "comprising" and its derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not disclosed herein. In contrast, the term "consisting essentially of," when it appears herein, excludes from the scope of any succeeding recitation any other component, step or procedure, excepting those that are not essential to operability, and the term "consisting of," when used, excludes any component, step or procedure not specifically delineated or listed. The term "or," unless otherwise stated, refers to the listed members individually and in any combination.

[0015] The articles "a" and "an" are used herein to refer to one or to more than one (ie, to at least one) of the grammatical object of the article.

[0016] Phrases such as "in one embodiment," "according to one embodiment," and the like generally mean that the particular feature, structure, or characteristic that follows the phrase is included in at least one aspect of the disclosure, and may be included in more than one aspect of the disclosure. Importantly, such phrases do not necessarily refer to the same aspect.

[0017] When the specification states that a component or feature "may," "can," "could," or "may" be included or have a characteristic, that particular component or feature is not required to be included or have the characteristic.

[0018] It is noted that although reference is made herein to raw nanostructured materials synthesized from carbon, other compounds may be used in connection with the synthesis of nanostructured materials for use in the methods of the present disclosure. For example, it is understood that raw nanostructured materials synthesized from boron may also be produced in a similar system, but using different chemical precursors, and then subjected to the methods of the present disclosure to purify the nanostructured materials.

[0019] Additionally, the present disclosure uses a floating catalyst chemical vapor deposition ("CVD") process to produce raw nanostructured materials. Growth temperatures for the floating catalyst CVD process can be in a relatively low range, for example, from about 400°C to about 1400°C, so that carbon nanotubes, single-walled carbon nanotubes (SWNTs), multi-walled carbon nanotubes (MWNTs), or both, may be grown. Although both SWNTs and MWNTs may be grown, in certain instances, SWNTs may be preferred due to their higher growth rates and tendency to form ropes, which may offer handling, safety, and strength advantages.

[0020] Referring now to FIG. 1A, a carbon nanotube, a metal impurity, and an amorphous carbon 1A, a system 10 is shown that may obtain raw carbon nanostructured material, including carbon nanotubes. The system 10 includes a housing 11 (i.e., a furnace) having opposing ends 111 and 112, and a passageway 113 extending between the ends 111 and 112. A tube 12 (i.e., a reactor) in which the carbon nanostructured material may be produced may be located within the passageway 113 of the housing 11. As shown in FIG. 1A, ends 121 and 122 of the tube 12 may be positioned such that they extend from ends 111 and 112, respectively, of the housing 11. The housing 11 may include a heating element or mechanism (not shown) for generating a temperature in the range of about 1000° C. to about 1500° C. required for the growth of carbon nanotubes within the tube 12. Because the heating element must maintain the temperature environment within the tube 12 within a specific range during the synthesis of the carbon nanostructured material, the system 10 may include a thermocouple on the exterior of the tube 12 for monitoring the temperature environment within the tube 12. Maintenance of a temperature range within the tube 12, for example from about 1100° C. to about 1400° C., may be optimized through the use of an insulating structure 123. The insulating structure 123 may be made, for example, from zirconia ceramic fibers (e.g., zirconia stabilized boron nitride). Other insulating materials may also be used.

[0021] Because the housing 11 and tube 12 must withstand variations in temperature and gas-reactive environments, the housing 11 and tube 12 may be manufactured from a strong, substantially gas-impermeable material that is substantially corrosion-resistant. The housing 11 and tube 12 may be made from quartz or ceramic materials, such as Macor® machinable glass-ceramic, to provide enhanced shock absorption. Of course, other materials may be used as long as the housing 11 and tube 12 are still impermeable to gases and can maintain their non-corrosive properties. Also, although shown with a cylindrical shape, the housing 11 and tube 12 may be provided with any geometric cross-section.

[0022] The system 10 may also include a collection unit 13 in fluid communication with an end 121 of the tube 12 for collecting the nanostructured material generated within the tube 12. At an opposite end 122 of the tube 12, the system 10 may include an injector device 14 (i.e., a sprayer) in fluid communication with the tube 12. The injector 14 may be designed to receive from a reservoir 15 a fluid mixture of components necessary for the growth of the nanostructured material within the tube 12. The injector 14 may also be designed to vaporize or fluidize the mixture (i.e., generate small droplets) prior to directing the mixture into the tube 12 for the generation and growth of the nanostructured material.

[0023] The fluid mixture, in one embodiment, can include, among others, (a) a metal catalyst precursor (from which metal catalyst particles are generated and on which nanostructured material can then be grown), (b) a tuning compound for controlling the particle size distribution of the metal catalyst particles generated from the metal catalyst precursor and thus the diameter of the nanostructured material, and (c) a carbon source for depositing carbon atoms onto the metal catalyst particles to grow the nanostructured material.

[0024] Examples of metal catalyst precursors from which metal catalyst particles may be generated include ferrocene materials such as iron or iron alloys, nickel, cobalt, their oxides, or their alloys (or compounds with other metals or ceramics). Alternatively, metal catalyst particles may be made from metal oxides such as Fe3O4, Fe2O4, or FeO, similar oxides of cobalt or nickel, or combinations thereof.

[0025] Examples of conditioning compounds for use in connection with the fluid mixtures of the present disclosure include thiophene, H2S, other sulfur-containing compounds, or combinations thereof.

[0026] Examples of carbon sources for use in connection with the fluid mixtures of the present disclosure are ethanol, methyl formate, propanol, acetic acid, hexane, methanol, or blends of methanol and ethanol. Other liquid carbon sources may also be used, including, but not limited to, C2H2, CH3, and CH4.

[0027] 1B, a detailed view of the injector 14 is shown. The injector 14 includes a substantially tubular chamber 141 defining a path 142 along which a vaporized fluid mixture may be generated and directed into the reaction tube 12. To vaporize or fluidize the mixture, the injector 14 may include a spray tube 16 designed to provide a Venturi effect to generate small droplets from the fluid mixture introduced from the reservoir 15. It should be appreciated that the vaporization or fluidization of the fluid mixture may occur substantially as the fluid exits through the distal end 161 of the spray tube 16. The generated droplets may range in size from nanoscale to microscale. To direct the vaporized fluid mixture along the spray tube 16 into the reaction tube 12, a certain amount of gas, such as H2, He or any other inert gas, may be used to push the vaporized fluids towards the reaction tube 12.

[0028] Although illustrated as substantially tubular, it should be appreciated that the injector 14 may have any geometric design so long as the injector is capable of accommodating the atomizing tube 16 and providing a path along which the vaporized fluid mixture can be directed into the reaction tube 12.

[0029] Additionally, it should be noted that injector 14 may be designed to allow for the introduction of individual components of a fluid mixture into injector 14 rather than being delivered as part of the fluid mixture. In such an embodiment, each component may be vaporized individually through an atomizing tube similar to tube 16 and introduced into injector 14 where they may be mixed and then directed along injector 14 in a manner similar to that described above.

[0030] Because the injector 14 is located within a portion of the reactor tube 12 and furnace 11, heat generated within the tube 12 and furnace 11 may adversely affect the temperature environment within the injector 14. To shield the injector 14 from the heat within the reactor tube 12 and furnace 11, an insulation package 17 may be provided around the injector 14. In particular, the insulation package 17 may act to maintain a temperature environment along the length of the injector 14.

[0031] Due to the presence of the insulation package 17, the temperature environment within the injector 14 may be reduced to a range that may affect the various reactions required to grow the carbon nanostructured material. As such, the injector 14 may also include a heating zone A located downstream of the atomizing tube 16 to provide a temperature range sufficient to allow for the formation of metal catalyst particles from the metal catalyst precursor. The heating zone A may include a first heater 18 located downstream of the distal end 161 of the atomizing tube 16. The heater 18 may be configured to heat the metal catalyst precursor to a temperature range, e.g., T, required to decompose the metal catalyst precursor into its constituent atoms. p1 and the atoms may be clustered into metal catalyst particles on which nanostructures may then be grown. p1 To maintain the temperature range of T at a level required to decompose the metal catalyst precursor, in one embodiment, the heater 18 is p1 In embodiments where ferrocene is used as a precursor, its constituent atoms (i.e., iron particles) of substantially nanoscale size may be located slightly downstream of T p1 It may be produced when the temperature at can be maintained in the range of about 200°C to about 300°C.

[0032] Heating zone A may further include a second heater 19 disposed downstream of the first heater 18 and within the furnace 11. The heater 19 may be configured to heat the heating zone A to a temperature range, e.g., T p2 In the presence of clusters of metal catalyst particles, these atoms may be provided to interact with the clusters to form metal complexes. The particle size distribution of the metal catalyst particles, and therefore the diameter of the nanostructures produced, can be controlled. In embodiments where thiophene is used as the coordinating compound, sulfur may be released upon decomposition of the thiophene to interact with the clusters of metal catalyst particles. The heater 19, in one embodiment, is p2 The heater 19 may be designed to maintain a temperature range of about 700° C. to about 950° C. at a position slightly downstream of the heater 19 .

[0033] According to one embodiment, T p2 is T p1 Since various parameters may be involved, T p1 From T p2 The distance to the metal catalyst precursor is T p1 From T p2 The flow of the fluid mixture to the target should be such that the amount of decomposition of the conditioning compound is optimized to optimize the particle size distribution of the metal catalyst particles.

[0034] It should be appreciated that in addition to the specific temperature zones created by the first heater 18 and the second heater 19 in the injector 14, the temperature at the distal end 161 of the spray tube 16 may also need to be maintained within a specific range in the injector 14 to avoid either condensation of the vaporized fluid mixture as it exits through the distal end 161 of the spray tube 16 or uneven flow of the fluid mixture. In one embodiment, the temperature at the distal end 161 may need to be maintained between about 100° C. and about 250° C. For example, if the temperature is below the indicated range, condensation of the fluid mixture may occur along the walls of the injector 16. As a result, the fluid mixture introduced from the injector 16 into the reaction tube 12 may be substantially different from that of the mixture introduced from the reservoir 15. For example, if the temperature is above the indicated range, boiling of the fluid mixture may occur at the distal end 161, resulting in sputtering and uneven flow of the fluids into the injector 14.

[0035] The injector 14 may need to maintain a temperature gradient along its length, so that condensation at the distal end 161 of the spray tube 16 is minimized or the required T p1 to allow decomposition of the metal catalyst precursor, or T p2 To maintain the temperature at 0.5° C. to enable decomposition of the conditioning compound, the insulation package 17 can act to maintain a desired temperature gradient along the injector 14 at each strategic location in addition to insulating from heat from the reaction tube 12 and furnace 11.

[0036] In one embodiment, the insulation package 17 may be made from quartz or a similar material, or from a porous ceramic material such as zirconia ceramic fiber (e.g., zirconia stabilized boron nitride). Of course, other insulation materials may also be used.

[0037] With continued reference to FIG. 1B, the system 10 may include at least one inlet through which a carrier gas may be introduced into the reaction tube 12. The introduction of the carrier gas into the tube 12 may aid in moving the fluid mixture along the tube 12 following exit from the injector 14. Additionally, since it may be desirable to minimize turbulence or eddies associated with the fluid mixture as it exits the injector 14, the carrier gas may be allowed to flow along the reaction tube 12 and along the exterior surface of the injector 14. In one aspect, the carrier gas may flow at a velocity substantially similar to the velocity of the fluid mixture as it exits the injector 14, allowing the fluid mixture to maintain a substantially laminar flow. By maintaining a substantially laminar flow, the growth and strength of the nanostructures produced may be optimized. In one aspect, the carrier gas may be H2, He, or any other inert gas.

[0038] To further minimize turbulence or eddies as the fluid mixture exits the injector 14, the insulating package 17 may include a substantially tapered design around the distal end of the injector 14. Alternatively, or in addition, an extension (not shown) may be disposed around the distal end of the injector 14 to minimize turbulence or eddies as the fluid mixture exits the distal end of the injector. The flow of the fluid mixture may be expanded substantially radially away from the center of the ejector 14. The presence of such an extension can slow the flow velocity of the fluid mixture and allow the flow pattern to remain substantially laminar.

[0039] The injector 14 is configured to move the fluid mixture along the injector 14 at a rate of T p1 Decomposition of the metal catalyst precursor at T p2 It should be appreciated that the injector 14 may be designed to decompose the conditioning compound at 200° C. However, as the fluid mixture travels along the injector 14, the carbon source necessary for nanostructure growth may not be decomposed and may remain substantially chemically unchanged.

[0040] 1A-B, the proximity of the substantially higher temperature range within the furnace 11, and thus within the reaction tube 12, can immediately expose the carbon source to the temperature range required to decompose the carbon source upon exiting through the distal end of the injector 14 for subsequent nanostructure growth. In one embodiment, the temperature range at the interface 142 between the distal end of the injector and the furnace 11 can be from about 1000° C. to about 1250° C.

[0041] 1C, a plasma generator 130 may be disposed around the distal end of the injector 14. In this manner, the fluid mixture may pass through a plasma flame 132 of the plasma generator 130 before entering the reaction tube 12. In one embodiment, an air-tight or liquid-tight seal may be provided around the junction between the plasma generator 130 and the injector 14 and between the plasma generator 130 and the reaction tube 12 to prevent gases and particles in the fluid mixture from escaping the system 10. In one embodiment, the plasma generator 130 may be axially or linearly aligned with the tubular chamber 141 of the injector 14 to provide an efficient flow path for the fluid mixture from the injector 14 through the plasma generator 130. In one embodiment, the alignment of the plasma generator 130 and the injector 14 is such as to allow the fluid mixture to pass substantially through the center of the plasma generator 130. In some embodiments, this may result in the fluid mixture passing through a central region of the plasma flame 132 having a more uniform temperature profile than the outer regions of the plasma flame 130. The plasma generator 130 may also be axially or linearly aligned with the reactor tube 12.

[0042] In one embodiment, the plasma generator 130 may provide focused energy in the form of a plasma flame 132 to raise the temperature of the fluid mixture above the temperature range within the injector 14. In one embodiment, the plasma generator 130 may raise the temperature of the fluid mixture to a level sufficient to decompose the carbon source into its constituent atoms for activation of nanostructure growth. In one embodiment, the plasma generator 130 may operate at about 1200° C. to about 1700° C. Because the temperature of the plasma flame 132 is substantially higher than the temperature within the injector 14, the heat generated by the plasma flame 132 may adversely affect the temperature environment within the injector 14. To that end, the plasma generator may include a heat shield 160 (see FIG. 1D) located between the region of the plasma generator 130 where the plasma flame 132 is generated and the injector 14 to preserve the temperature environment along the length of the injector 14. In one embodiment, the heat shield 160 may be made from a porous ceramic material such as zirconia ceramic fibers (e.g., zirconia stabilized boron nitride). Of course, other insulating materials may also be used.

[0043] Because the plasma generator 130 may initiate more rapid decomposition of the carbon source by providing concentrated energy to the fluid mixture, in one embodiment, a shorter reactor tube 12, furnace 11, or both may be used and still produce nanotubes of sufficient length. Of course, to the extent desired, the reactor tube 12, furnace 11, or both may be used without the need for plasma generation. In one embodiment, the use of a plasma generator 130 in the process may enable the production of longer carbon nanotubes.

[0044] It should also be noted that in some embodiments, the injector 14 and plasma generator 130 may be utilized with minimal or no additional heat within the reaction tube 12. It should also be noted that multiple plasma generators may be utilized within the system 10 to provide the desired temperature gradient over the travel distance of the fluid mixture.

[0045] FIG. 1D illustrates an embodiment of a plasma generator 130. In one embodiment, the plasma generator 130 may be a direct current (DC) generator. The plasma generator 130 may include an anode 152 and a cathode 154, which may be cooled by water or another cooling fluid or another material that may act as a heat sink to transfer heat away from the electrodes 152, 154. In one embodiment, the electrodes 152, 154 may be highly diffusive metal electrodes, such as those typically made of copper or silver. A plasma gas may flow around the anode 152 and the cathode 154 and may be ionized by an electric arc 156 initiated between the anode 152 and the cathode 154 to generate the plasma flame 132. Suitable plasma gases may be either reactive or non-reactive and may include, but are not limited to, argon oxygen, nitrogen, helium, hydrogen, or another gas. In one embodiment, the plasma generator 130 may include one or more Helmholtz coils 158 or another device for generating a magnetic field to rotate the arc 156. In such an embodiment, the anode 152 and the cathode 154 may comprise an annular shape to facilitate rotation of the arc 156. Although FIG. 1D illustrates one suitable embodiment of a plasma generator, other designs and types of plasma generators (i.e., radio frequency, alternating current, and other discharge plasma generators) may be implemented.

[0046] In one embodiment, the Helmholtz coils 158 can be used to generate electromagnetic or electrostatic fields for in situ alignment of the nanotubes downstream of the plasma generator 130 in the reactor chamber 12. Additionally or alternatively, the electromagnetic field generated by the plasma generator 130 can act to deflect the carbon nanotubes toward the axis of the reactor tube 12 by generating a torque on the carbon nanotubes, packing the carbon nanotubes toward such axis. In one embodiment, the plasma generator 130 can also be designed to push or focus the cloud of carbon nanotubes into a smaller radial volume as it travels through the reactor tube 12. In one embodiment, the particles on which the carbon nanotubes are grown can be charged by a particle charger such that the particles are responsive to electrostatic forces.

[0047] To the extent that more than one plasma generator 130 is used, the electromagnetic field strength and position of the plasma generators can be optimized to align the carbon nanotubes. Additionally or alternatively, the generators can be linearly aligned with each other, with each successive downstream plasma generator configured to generate a stronger electrostatic field, thereby forcing or condensing the flowing carbon nanotube cloud toward a smaller radial volume and moving the carbon nanotubes into substantial axial alignment with the reaction tube 12. In some embodiments, successive plasma generators can also be used to control the acceleration or deceleration of the flow, allowing the nanotubes to condense radially toward a filamentary shape. Such an approach to condense the carbon nanotube stream can bring the carbon nanotubes closer together, enhancing contact between adjacent nanotubes. Contact between adjacent carbon nanotubes can be further enhanced through non-covalent interactions between the carbon nanotubes, such as London dispersion forces or van der Waals forces.

[0048] During operation, several processes may occur in the region between the spray tube 16 and the main furnace 11 of the system 10. For example, initially, a fluid mixture of metal catalyst precursor, conditioning compound, and carbon source may be introduced from reservoir 15 through the spray tube 16 into the injector 14. An inert gas such as H2 or He may be used to help guide the mixture along the spray tube 16. As the fluid mixture travels along and exits the spray tube 16, the tube 16 may impart a venturi effect to vaporize the fluid mixture (i.e., generate droplets from the fluid mixture). Such range within the injector 14 may be maintained at a temperature level ranging from about 100° C. to about 250° C. to minimize the occurrence of either condensation or boiling as the fluid mixture exits the spray tube 16.

[0049] In one embodiment, additives for the carbon source may be included in the fluid mixture to optimize growth conditions and enhance the strength of the carbon nanotube material made from the carbon nanotubes produced. Examples of additives include C 60 , C 70 , C 72 , C 84 , and C 100 Including, but not limited to:

[0050] The vaporized fluid mixture may then travel along the injector 14 toward the first heater 18, where the temperature increases to T p1 The temperature may be maintained in the range of about 200° C. to about 300° C. at 200° C., and the metal catalyst precursor in the fluid mixture may decompose and release its constituent atoms. In one embodiment, the decomposition temperature of the metal catalyst precursor may depend on the carrier gas (e.g., H2 or He) and may also depend on the presence of other species. The constituent atoms may then cluster into metal catalyst particles of a characteristic size distribution. This size distribution of the metal catalyst particles may generally develop during travel through the injector 14 and into the furnace 11.

[0051] The fluid mixture may then proceed further downstream along the injector 14 to a second heater 19. The second heater 19, in one embodiment, p2 The temperature in the injector 14 may be maintained at a level in the range of about 700° C. to about 950° C. at which the tuning compound may decompose into its constituent atoms. The tuning compound atoms may then react with the clusters of metal catalyst particles to result in a particle size distribution of the clusters of metal catalyst particles. In particular, the tuning compound atoms may act to stop the growth of the metal catalyst particles and / or inhibit evaporation. In one embodiment, the tuning compound atoms may interact with the clusters of metal catalyst particles along with H2 in the injector 14 to affect the particle size distribution of the metal catalyst particles.

[0052] It should be recognized that the carbon source within the fluid mixture may remain chemically unchanged or otherwise decomposed within the injector 14 as the fluid mixture travels along the entire length of the injector 14.

[0053] The conditioned metal catalyst particles that have traveled beyond the second heater 19 may then travel across an interface 142 between the distal end 141 of the injector 14 and the furnace 11 into the main portion of the reactor tube 12. Upon exiting the injector 14, the conditioned metal catalyst particles, along with the carbon source, may maintain a substantially laminar flow in the presence of a carrier gas, such as H2 or He. In the presence of the carrier gas, the conditioned metal catalyst particles may be diluted by the volume of the carrier gas.

[0054] Furthermore, once in the main portion of the reaction tube 12 (wherein the temperature range may be maintained at a level sufficient to decompose the carbon source into its constituent carbon atoms), the presence of the carbon atoms may activate nanostructure growth. In one embodiment, the temperature range may be from about 1000° C. to about 1250° C. Growth generally occurs when the carbon atoms deposit themselves substantially continuously onto the metal catalyst particles to form nanostructures, such as carbon nanotubes.

[0055] In one embodiment, the fluid mixture from the injector 14 may pass through a plasma generator 130 before entering the reactor tube 12 .

[0056] The growth of the nanostructures may terminate when the metal catalyst particles become inactive, or when the concentration of constituent carbon atoms in the vicinity of the metal catalyst particles falls to a relatively low value, or when the temperature decreases as the mixture moves beyond a range within the reaction tube 12 where the temperature range is maintained at a level sufficient for growth.

[0057] Referring now to FIG. 2 , raw carbon nanostructured material 202 produced in system 10 from a fluid mixture 20 (including, among other things, (a) a metal catalyst precursor, (b) a conditioning compound, and (c) a carbon source) as described above and comprising carbon nanotubes, metal impurities, and amorphous carbon is charged to a vessel and oxidized in an oxidation step 210 in a gaseous atmosphere comprising carbon dioxide to remove the amorphous carbon from the nanostructured material 202 and produce carbon monoxide according to the following reaction: C+CO2→CO. The oxidation can be carried out at a temperature of at least about 150° C. to about 500° C. and a pressure ranging from about 0.01 to 100 atmospheres. The oxidation step 210 serves two purposes. The first purpose is to remove amorphous carbon from the nanostructured material 202, thereby exposing metal impurities (i.e., metal catalyst particles), which in one particular embodiment include iron, and the second purpose is to generate carbon monoxide 220, which is used to convert the exposed iron to iron pentacarbonyl.

[0058] The carbon dioxide concentration in the gas atmosphere may range from about 1% to about 100% by volume, or from about 1% to about 30% by volume. An inert gas such as nitrogen or argon may be used to dilute the carbon dioxide concentration. The oxidation time may range from about 0.1 hours to about 20 hours. Shorter times are preferred. Water vapor may also be added to the oxidation gas atmosphere, and the water vapor concentration may range up to the saturation limit of the gas used to introduce the water vapor. The water vapor concentration in the gas atmosphere may range from about 0.5% to about 50% by volume, or from about 0.5% to about 10% by volume, more typically from about 0.5% to about 5% by volume.

[0059] After removal of the amorphous carbon, the carbon dioxide treated carbon nanostructured material 204 is exposed in a high temperature / pressure soak step 212 to a flowing gas containing at least carbon monoxide 220 formed in the oxidation step above.

[0060] Upon exposure to carbon monoxide, metal impurities (iron in the case of the embodiment shown in FIG. 2) found within the carbon dioxide treated carbon nanostructured material 204 are converted to iron pentacarbonyl according to the following reaction: Fe+5CO(gas) → Fe(CO)5 To aid in the rate and completeness of the reaction with the metal, a large excess of carbon monoxide, for example at least 500 mole percent, is preferably used, which is significantly more than the stoichiometric amount required to react with the contaminating metal in the carbon nanostructured material 204. The reaction is generally carried out at a temperature of at least 100°C, or at least 130°C, or even at least 140°C, and also generally at most 200°C, or at most 170°C, or even at most 160°C. An example of a suitable temperature is 150°C. The pressure of the flowing gas is generally at least 5 MPa (50 bar), or at least 10 MPa (100 bar), or even at least 12 MPa (120 bar), and also generally at most 25 MPa (250 bar), or at most 20 MPa (200 bar), or even at most 18 MPa (180 bar). An example of a suitable pressure is 15 MPa (150 bar). If inert gases are present in addition to carbon monoxide, these values ​​are set as carbon monoxide partial pressures.

[0061] The iron pentacarbonyl formed above may be vaporized under the above temperature and pressure and removed as gas stream 222. The carbon nanostructure material 206 may then be harvested in step 214 either batchwise or continuously to produce a purified carbon nanostructure material product 208.

[0062] According to a further embodiment, the pentacarbonyl iron may be recovered in the circulation condenser and recycled to the process of producing new raw carbon nanostructured material, where it is used as a catalyst source. Thus, the gas stream 222 removed from the carbon nanostructured material 206 may be sent to a condenser in step 216, which causes the gas stream 222 to condense and allows separation of the condensate from the water by gravity. Upon separation, the condensed pentacarbonyl iron particles 224 may be returned to the system 10 to produce new raw carbon nanostructured material. The gas stream 222 also generally contains carbon monoxide, which will of course be present when passing the gas stream 222 through the condenser. Although the carbon monoxide dissolves to some extent in the water of the condenser, the water is saturated thereby and the vapor pressure of such gas builds up outside the water, allowing the carbon monoxide to be separated and exit the condenser as gas stream 226, where it may be added to the carbon monoxide fluid gas 220 for step 212.

[0063] Advantages of the disclosed process include, but are not limited to, the possibility of generating sufficient carbon monoxide required to form the carbonyl-forming step in situ during the oxidation step, which may not only reduce the overall carbon emissions of the process, but may also reduce the need for a separate carbon monoxide feedstock.

[0064] While making and using various embodiments of the invention have been described in detail above, it should be appreciated that the invention provides many applicable inventive concepts that can be embodied in a wide variety of specific contexts. The specific embodiments discussed herein are merely illustrative of specific ways to make and use the invention and do not delimit the scope of the invention.

Claims

1. 1. A method for purifying carbon nanostructured material, comprising: (a) obtaining a quantity of raw carbon nanostructured material, said raw carbon nanostructured material being contaminated with metal catalyst particles and amorphous carbon structures; (b) oxidizing the raw carbon nanostructured material by exposure to carbon dioxide at a temperature between about 150° C. and about 500° C., the oxidation removing the amorphous carbon structures to form carbon dioxide treated carbon nanostructured material and carbon monoxide; (c) exposing the carbon dioxide treated carbon nanostructured material to a flowing gas containing at least carbon monoxide produced in step (b) and increasing the temperature of the carbon dioxide treated carbon nanostructured material and the flowing gas to about 20° C. to about 200° C. to produce a gas stream containing purified carbon nanostructured material and volatile metal species; (e) transferring said gas stream from said purified carbon nanostructure material; A method comprising:

2. The method of claim 1 , wherein the amount of raw carbon nanostructured material is obtained from a floating catalyst chemical vapor deposition process.

3. The method of claim 1, wherein the metal catalyst particles comprise iron.

4. The method of claim 1, wherein the oxidation in step (b) is carried out at a pressure in the range of about 0.01 to 100 atmospheres.

5. The method of claim 1, wherein the temperature of the carbon dioxide treated carbon nanostructured material and the flowing gas is increased to at least 150°C.

6. The method of claim 1, wherein the pressure of the flowing gas in step (c) is at least 50 bar.

7. The method of claim 2, wherein the volatile metal species comprises iron pentacarbonyl.

8. 8. The method of claim 7, further comprising: (f) passing the gas stream through a condenser to condense the iron pentacarbonyl.

9. The method of claim 8, wherein the condensed iron pentacarbonyl is recycled to the floating catalytic chemical vapor deposition process to produce a new quantity of raw carbon nanostructured material.

10. The method of claim 8, wherein passing the gas stream through the condenser produces a stream of carbon monoxide exiting the condenser.

11. The method of claim 10, wherein the carbon monoxide stream is added to the flowing gas of step (c).

12. The method of claim 1, wherein the purified carbon nanostructured material contains less than about 10% by weight of metals.

13. The method of claim 1, wherein the purified carbon nanostructured material contains less than about 10% by weight amorphous carbon.

14. The method of claim 1, wherein the carbon nanostructure material comprises single-walled carbon nanotubes, multi-walled carbon nanotubes, or both.

Citation Information

Patent Citations

  • JP1971000151Y1

  • Method and apparatus for producing carbon nanotubes

    JP2003535794A

  • Method of treating carbon nano-structure using fluidizing system

    JP2005001980A

  • Method for purifying nanocarbon

    JP2006182572A

  • Single-walled, multi-walled, functionalized and doped carbon nanotubes, and composites thereof

    JP2007527844A