Process tools for dry photoresist removal
Dry etching of metal-containing EUV resists under atmospheric conditions addresses the limitations of conventional EUV photoresists, improving etch resistance and resolution for precise pattern formation in semiconductor manufacturing.
Patent Information
- Application Number
- JP2022559416
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-13
- Filing Date
- 2021-11-09
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2041-11-09
AI Technical Summary
Current photolithography processes face challenges in achieving small feature sizes due to the wavelength limitations of UV light, particularly in EUV lithography, where conventional organic chemically amplified resists suffer from low absorption and pattern collapse issues, necessitating improved EUV photoresist materials with enhanced properties.
The use of dry etching techniques under atmospheric conditions to remove metal-containing EUV resists, employing etching gases in a controlled or ambient atmosphere to address the limitations of conventional EUV photoresists, including the use of plasma-free thermal processes and controlled atmospheres to enhance etch resistance and resolution.
Dry etching under atmospheric conditions improves etch resistance and resolution, reducing line collapse and increasing throughput by eliminating vacuum requirements, thus enhancing the capability to form precise patterns in semiconductor substrates.
Smart Images

Figure 0007562696000001 
Figure 0007562696000002 
Figure 0007562696000003
Abstract
Description
[Technical field]
[0001] [Incorporated by reference] A PCT application form is being filed contemporaneously herewith as a part of this application. Each application to which this application claims benefit or priority identified in the contemporaneously filed PCT application form is hereby incorporated by reference in its entirety for all purposes. [Background technology]
[0002] The fabrication of semiconductor devices, such as integrated circuits, is a multi-step process that involves photolithography. Typically, this process involves depositing material on a wafer and patterning the material by lithographic techniques to form the structural features of the semiconductor device (e.g., transistors and circuits). A typical photolithography process known in the art includes the following steps: preparing a substrate, applying a photoresist, such as by spin coating, exposing the photoresist to light in a desired pattern such that the exposed areas of the photoresist are generally soluble in a developer, developing by applying a developer and removing either the exposed or unexposed areas of the photoresist, and subsequent processing steps to form features, such as by etching or material deposition, in the areas of the substrate from which the photoresist was removed.
[0003] Advances in semiconductor design have been driven by the need for, and ability to, form ever smaller features on semiconductor substrate materials. This advance in technology is characterized by "Moore's Law," which states that transistor density in high-density integrated circuits doubles every two years. Indeed, advances in chip design and manufacturing have led to modern microprocessors that may contain billions of transistors and other circuit functions on a single chip. Individual features on such chips may be on the order of 22 nanometers (nm) or smaller, and in some cases less than 10 nm.
[0004] One of the challenges in manufacturing devices with such small features is the ability to reliably and reproducibly create photolithography masks with sufficient resolution. Current photolithography processes expose photoresist with ultraviolet (UV) light, typically at 193 nm. An inherent problem arises from the fact that this light has a wavelength that is much larger than the desired size of the features to be formed on the semiconductor substrate. To achieve feature sizes smaller than the wavelength of the light requires the use of complex resolution enhancement techniques such as multiple patterning. Thus, there has been much interest and research effort in developing photolithography techniques using shorter wavelength light, such as extreme ultraviolet (EUV) radiation, which has a wavelength of 10 nm to 15 nm (e.g., 13.5 nm).
[0005] However, EUV photolithography processes can also encounter challenges such as low power and light loss during patterning. Traditional organic chemically amplified resists (CARs), similar to those used in 193 nm UV lithography, have potential drawbacks when used in EUV lithography. In particular, they have low absorption coefficients in the EUV region, and diffusion of photoactivated chemical species can result in blurring or line edge roughness. Furthermore, to provide the etch resistance required to pattern the underlying device layers, small features patterned in traditional CAR materials can be high aspect ratios, risking pattern collapse. Thus, there remains a need for improved EUV photoresist materials with properties such as reduced thickness, greater absorbance, and greater etch resistance.
[0006] The description of the background art provided herein is intended to provide a general background to the present technology. The inventors' work within the scope of this description, and aspects of the description that may not otherwise be admitted as prior art at the time of filing, are not admitted, expressly or implicitly, as prior art to the present technology. Summary of the Invention
[0007] Provided herein is a substrate processing apparatus including a process chamber exposed to atmospheric conditions, the apparatus further including a substrate support pedestal for holding a semiconductor substrate in the process chamber, a heating assembly facing the semiconductor substrate on the substrate support pedestal, the heating assembly including a plurality of heating elements, and an etching gas supply nozzle disposed above the substrate support pedestal, the etching gas supply nozzle being movable such that a supply position of an etching gas is above the semiconductor substrate.
[0008] In some implementations, the semiconductor substrate includes a metal-containing EUV resist, and one or more portions of the metal-containing EUV resist are removable by the etching gas. In some implementations, the process chamber exposed to atmospheric conditions is exposed to an atmospheric pressure between about 50 Torr and about 765 Torr. In some implementations, the process chamber exposed to atmospheric conditions is exposed to a controlled atmosphere, and the exposure to the controlled atmosphere includes exposure to a chamber pressure greater than about 760 Torr and / or exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof. In some implementations, the plurality of heating elements includes a plurality of LEDs, and the plurality of LEDs are arranged in a plurality of independently controllable heating zones. In some implementations, the etching gas supply nozzle is coupled to a movable swing arm configured to position the etching gas supply nozzle from a center to an edge of the semiconductor substrate. In some implementations, the apparatus includes a controller configured with instructions for processing the semiconductor substrate, the instructions including code for providing a metal-containing EUV resist on the semiconductor substrate in the process chamber and supplying the etching gas to the semiconductor substrate through the etching gas supply nozzle to dry etch one or more portions of the metal-containing EUV resist from the semiconductor substrate under atmospheric conditions. In some implementations, the apparatus further includes an exhaust fan configured to remove etching byproducts and other residual gases in the process chamber. In some implementations, the apparatus further includes a gas source coupled to the process chamber for supplying an inert gas and / or a dilution gas to the process chamber. In some implementations, the process chamber is a plasma-free thermal process chamber.
[0009] Also provided herein is a substrate processing apparatus including a process chamber exposed to atmospheric conditions, a bake plate for supporting a semiconductor substrate, the bake plate including a plurality of heating zones, each of the plurality of heating zones including one or more heating elements, and an etching gas distributor disposed above the bake plate and configured to supply an etching gas to the semiconductor substrate.
[0010] In some implementations, the semiconductor substrate includes a metal-containing EUV resist, and one or more portions of the metal-containing EUV resist are removable by the etching gas. In some implementations, the process chamber exposed to atmospheric conditions is exposed to an atmospheric pressure between about 50 Torr and about 765 Torr. In some implementations, the process chamber exposed to atmospheric conditions is exposed to a controlled atmosphere, and the exposure to the controlled atmosphere includes exposure to a chamber pressure greater than about 760 Torr and / or exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or combinations thereof. In some implementations, the bake plate includes a top surface and a plurality of minimum contact area (MCA) supports for supporting the semiconductor substrate above the top surface of the bake plate. In some implementations, the etching gas distributor includes a showerhead having a faceplate facing the semiconductor substrate, the faceplate including a plurality of through holes for supplying the etching gas to the semiconductor substrate. In some implementations, the process chamber is a thermal process chamber that does not use plasma. In some implementations, the apparatus further includes a controller configured with instructions for processing the semiconductor substrate, the instructions including code for providing a metal-containing EUV resist on the semiconductor substrate in the process chamber; and supplying the etching gas to the semiconductor substrate through the etching gas distributor to dry etch one or more portions of the metal-containing EUV resist from the semiconductor substrate under atmospheric conditions.
[0011] Also provided herein is a substrate processing apparatus including a furnace reactor having a substrate support pedestal for holding a plurality of semiconductor substrates, a plurality of heating elements for heating the plurality of semiconductor substrates to an elevated temperature, and one or more etching gas inlets for supplying an etching gas to the furnace reactor, the one or more etching gas inlets configured to supply an etching gas to the plurality of semiconductor substrates.
[0012] In some implementations, the furnace reactor is exposed to atmospheric conditions. In some implementations, the atmospheric conditions include exposure to a controlled atmosphere, and the one or more etching gas inlets are further configured to supply nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof to provide the controlled atmosphere. In some implementations, the apparatus further includes one or more gas outlets for removing etching by-products and other residual gases from the furnace reactor, and a motor for rotating the substrate support. In some implementations, a chamber wall of the furnace reactor includes quartz, a ceramic material, or a low temperature polymer material. In some implementations, each of the plurality of semiconductor substrates includes a metal-containing EUV resist, and one or more portions of the metal-containing EUV resist are removable by the etching gas.
[0013] Also provided herein is a track lithography system, the track lithography system including a cassette loading section including one or more pods for receiving and returning semiconductor substrates, and a processing section including a plurality of processing stations for photoresist processing of the semiconductor substrates. The plurality of processing stations includes a deposition chamber for depositing a metal-containing EUV resist on the semiconductor substrate, a thermal processing chamber, and a substrate cleaning chamber, at least one of the plurality of processing stations being exposed to atmospheric conditions and configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor substrate. The track lithography system further includes an exposure section including a scanner for exposing the semiconductor substrate to EUV radiation, and an interface section for transporting the semiconductor substrate between the processing section and the exposure section.
[0014] In some implementations, the plurality of processing stations further includes a hexamethyldisilazane (HMDS) processing chamber for processing a surface of the semiconductor substrate, the HMDS processing chamber configured to dry remove one or more portions of the metal-containing EUV resist under atmospheric conditions. In some implementations, the at least one of the plurality of processing stations includes a substrate support for holding the semiconductor substrate and a gas distributor for supplying an etching gas to the semiconductor substrate, the one or more portions of the metal-containing EUV resist being removable by the etching gas.
[0015] Also provided herein is a method for dry developing an EUV resist, the method including providing a metal-containing EUV resist on a semiconductor substrate in a process chamber, and dry etching the metal-containing EUV resist by exposure to an etching gas in the process chamber, wherein the dry etching of the metal-containing EUV resist is performed under atmospheric conditions.
[0016] In some implementations, the atmospheric conditions include atmospheric pressures between about 50 Torr and about 765 Torr. In some implementations, the atmospheric conditions include a controlled atmosphere. The controlled atmosphere includes exposing the semiconductor substrate to a chamber pressure greater than about 760 Torr and / or exposing the semiconductor substrate to nitrogen, water vapor, carbon dioxide, argon, helium, or combinations thereof. In some implementations, the method further includes baking the metal-containing EUV resist at an elevated temperature in the same process chamber as dry etching the metal-containing EUV resist. In some implementations, dry etching the metal-containing EUV resist includes dry developing the metal-containing EUV resist by selectively removing portions of the EUV resist by exposure to a dry developing chemical. In some implementations, the method includes performing a bevel edge clean of the semiconductor substrate in the same process chamber as dry developing the metal-containing EUV resist. In some implementations, dry etching the metal-containing EUV resist includes heating the semiconductor substrate to a temperature of about 100° C. or greater. In some implementations, heating the semiconductor substrate includes locally heating an area of the semiconductor substrate. In some implementations, dry etching the metal-containing EUV resist includes positioning a movable discharge nozzle above the semiconductor substrate and preferentially directing the etching gas to one or more areas of the semiconductor substrate. In some implementations, the process chamber includes a substrate support pedestal coupled to a plurality of independently controllable heating zones for locally heating the semiconductor substrate and a movable discharge nozzle positioned above the semiconductor substrate for directing the etching gas to a target area of the semiconductor substrate. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a flow chart of an exemplary method for depositing and developing photoresist according to some embodiments.
[0018] [Figure 2A] 2A-2D are schematic cross-sectional views of various processing stages of dry development, according to some embodiments. [Figure 2B] 2A-2B are schematic cross-sectional views of various processing stages of dry development according to some embodiments. [Figure 2C] 2A-2C are schematic cross-sectional views of various processing stages of dry development according to some embodiments.
[0019] [Figure 3A] FIG. 3A is a schematic diagram of an exemplary process chamber for performing dry etching of photoresist, according to some embodiments. [Figure 3B] FIG. 3B is a schematic diagram of an exemplary process chamber for performing dry etching of photoresist, according to some embodiments.
[0020] [Figure 4] FIG. 4 is a schematic diagram of an exemplary system architecture or track system for photoresist processing, according to some embodiments.
[0021] [Diagram 5] FIG. 5 is a schematic diagram of another exemplary system architecture or track system for photoresist processing, according to some embodiments.
[0022] [Figure 6] FIG. 6 is a schematic diagram of an exemplary batch vertical furnace for dry etching of photoresist, according to some embodiments.
[0023] [Figure 7A] FIG. 7A is a schematic diagram of a wafer cleaning station configured to perform dry etching of photoresist, according to some embodiments. [Figure 7B]FIG. 7B is a schematic diagram of a wafer cleaning station configured to perform dry etching of photoresist, according to some embodiments.
[0024] [Figure 8A] FIG. 8A is a schematic diagram of a wafer cleaning and heating station configured to perform dry etching of photoresist according to some embodiments. [Figure 8B] FIG. 8B is a schematic diagram of a wafer cleaning and heating station configured to perform dry etching of photoresist according to some embodiments.
[0025] [Figure 9] FIG. 9 is a schematic diagram of an exemplary process station for performing dry etching, according to some embodiments.
[0026] [Figure 10] FIG. 10 is a schematic diagram of an exemplary multi-station processing tool suitable for performing the various photoresist processing steps described herein.
[0027] [Figure 11] FIG. 11 is a schematic cross-sectional view of an exemplary inductively coupled plasma apparatus for carrying out some embodiments and processes described herein.
[0028] [Figure 12] FIG. 12 illustrates a semiconductor process cluster tool configuration having a deposition module and a patterning module in conjunction with a transfer module suitable for carrying out the processes described herein.
[0029] [Figure 13] FIG. 13 provides various exemplary tool configurations that can be used to perform methods according to embodiments of the present disclosure. [Figure 14] FIG. 14 provides various exemplary tool configurations that can be used to perform methods according to embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The present disclosure generally relates to the field of semiconductor processing. In a particular embodiment, the present disclosure relates to a method and apparatus for processing EUV photoresist (e.g., photoresist containing EUV-sensitive metal and / or metal oxide) in connection with EUV patterning and developing the EUV-patterned film to form a patterning mask.
[0031] In this specification, reference is made in detail to specific embodiments of the present disclosure. Examples of specific embodiments are shown in the accompanying drawings. Although the present disclosure is described in relation to these specific embodiments, it is understood that it is not intended to limit the present disclosure to such specific embodiments. Rather, it is intended to encompass alternatives, modifications, and equivalents that may be included within the spirit and scope of the present disclosure. In the following description, numerous specific details are given to provide a detailed understanding of the present disclosure, but the present disclosure may be practiced without some or all of these specific details. In other examples, well-known process steps are not described in detail to avoid unnecessarily obscuring the present disclosure.
[0032] [Introduction] Patterning of thin films in semiconductor processing is often a critical step in the manufacture of semiconductors. Patterning involves lithography. In conventional photolithography, such as 193 nm photolithography, a pattern is transferred to a light-sensitive photoresist by irradiating a mask with photons from a photon source, thereby inducing a chemical reaction in the photoresist, which, after development, removes parts of the photoresist to form the pattern.
[0033] Advanced technology nodes (as defined by the International Technology Roadmap for Semiconductors) include 22 nm, 16 nm, and beyond. For example, at the 16 nm node, a typical via or line width in a damascene structure is generally about 30 nm or less. The shrinking features in advanced semiconductor integrated circuits (ICs) and other devices are driving the trend toward higher resolution lithography.
[0034] Extreme ultraviolet (EUV) lithography can extend lithography technology by moving to smaller imaging source wavelengths than are achievable with traditional photolithography methods. EUV sources with wavelengths of approximately 10-20 nm, or 11-14 nm (e.g., 13.5 nm wavelength) are available for state-of-the-art lithography tools (also called scanners). EUV radiation is strongly absorbed by a wide range of solid and fluid materials, including quartz and water vapor.
[0035] EUV lithography uses EUV resists. The EUV resists are patterned to form masks for etching the underlying layers. The EUV resists may be polymeric chemically amplified resists (CARs) that are fabricated by liquid-based spin-on techniques. Alternatives to CARs include directly photopatternable metal oxide-containing films. These metal oxide-containing films are available from Inpria (Corvallis, Oregon), and are described in, for example, U.S. Patent Publication Nos. 2017 / 0102612, 2016 / 021660, and 2016 / 0116839, the disclosures of which relating to photopatternable metal oxide-containing films at least in which are incorporated herein by reference. Such films may be fabricated by spin-on techniques or dry deposited. Metal oxide-containing films can be patterned directly (i.e., without the use of a separate photoresist) by EUV exposure in a vacuum environment, and patterning resolutions of 30 nm or less can be achieved. This is described, for example, in U.S. Pat. No. 9,996,004, entitled "EUV PHOTOPATTERNING OF VAPOR-DEPOSITED METAL OXIDE-CONTAINING HARDMASKS," issued June 12, 2018, and / or International Application No. PCT / US19 / 31618, entitled "METHODS FOR MAKING EUV PATTERNABLE HARD MASKS," filed May 9, 2019, which are incorporated by reference for at least their disclosures regarding the composition, deposition, and patterning of directly photopatternable metal oxide films to form EUV resist masks. In general, patterning involves exposing an EUV resist to EUV radiation to form a photopattern in the resist, followed by development to remove portions of the resist according to the photopattern to form the mask.
[0036] It should also be understood that the present disclosure relates to lithographic patterning techniques and materials exemplified by EUV lithography, but is also applicable to other next-generation lithographic techniques. In addition to EUV, which includes the standard 13.5 nm EUV wavelength currently in use and under development, the most relevant sources of radiation for such lithography are DUV (deep ultraviolet) (generally referring to the use of 248 nm or 193 nm excimer laser sources), X-ray (formally including EUV in the relatively low energy range of the X-ray range), and e-beam (which can cover a wide energy range). Specific methods may depend on the specific materials and applications used for the semiconductor substrate and the final semiconductor device. Thus, the methods described herein are merely exemplary of methods and materials that can be used with the present technology.
[0037] Directly photopatternable EUV resists may consist of or include metal and / or metal oxides mixed with organic components. Metals / metal oxides are very promising in that they can promote EUV photon adsorption, generate secondary electrons, and / or exhibit high etch selectivity relative to the underlying film stack and device layers. So far, these resists have been developed by a wet (solvent) approach, which requires moving the wafer into a track where it is exposed to a developing solvent, dried, and baked. Wet development not only limits productivity, but can also lead to line collapse due to surface tension effects during solvent evaporation between fine features.
[0038] Dry development techniques have been proposed to overcome these challenges by eliminating substrate delamination and interface failure. Dry development can improve performance (e.g., avoid line collapse due to surface tension and delamination in wet development) and increase throughput (e.g., by avoiding wet development tracks). Other advantages include elimination of organic solvent developers, mitigation of adhesion issues, improved dose efficiency due to increased EUV absorption, and no solubility-based limitations. Dry development is also more tunable, providing additional critical dimension (CD) control and scum removal.
[0039] Dry development presents its own challenges, such as the etch selectivity between unexposed and EUV-exposed resist materials, which can lead to higher dose-to-size requirements for effective resist exposure when compared to wet development, and non-optimal selectivity can lead to rounding of photoresist corners due to prolonged exposure under etching gases, which can lead to higher line CD variability in the subsequent transfer etch step.
[0040] [Dry etching of EUV resist] The present disclosure provides dry etching of metal-containing EUV resist under atmospheric conditions. As used herein, "atmospheric conditions" may refer to exposure to non-vacuum conditions. Specifically, atmospheric conditions may comprise a chamber pressure of about 50 Torr to about 760 Torr (i.e., atmospheric pressure), or about 50 Torr to about 765 Torr. The tools and chambers of the present disclosure may operate at an overpressure above atmospheric pressure. The overpressure may be, for example, about 0.1 Torr to about 5 Torr, or about 0.3 Torr to about 1.5 Torr greater than atmospheric pressure. In some embodiments, atmospheric conditions may comprise a controlled atmosphere with a chamber pressure greater than about 760 Torr. Operation at pressures above atmospheric pressure may be useful to avoid leak-in contamination with oxygen or air.
[0041] The atmospheric conditions may include exposure to an ambient gas (e.g., air). The ambient gas may include oxygen, nitrogen, carbon dioxide, water vapor, or a combination thereof. Alternatively, the atmospheric conditions may include exposure to a controlled atmosphere. The exposure to a controlled atmosphere includes exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof. In some embodiments, the controlled atmosphere includes exposure to a gas that is a non-oxidizing gas. Such gases may function as inert or diluent gases that contribute to achieving an overpressure useful for avoiding leak-in contamination by oxygen or air. Dry etching of the metal-containing EUV resist may be performed under atmospheric conditions, although it is understood that the chamber in which the dry etching is performed may or may not include a vacuum system. Rather than exposing the metal-containing EUV resist to a vacuum environment in the dry etching, the metal-containing EUV resist may be exposed to atmospheric conditions. Here, the atmospheric conditions may include exposure to air or to a controlled environment (e.g., a pressure above atmospheric pressure). The dry etching of the present disclosure can be applied to dry development of photopatterned metal-containing EUV resist, bevel edge cleaning of deposited metal-containing EUV resist, or other photoresist processes involving dry etching. Costs can be reduced by eliminating the corresponding steps of wet cleaning / development. Additionally, costs can be reduced by avoiding the vacuum equipment and operation in the corresponding steps of dry cleaning / development.
[0042] An EUV-sensitive metal or metal oxide-containing film (e.g., organotin oxide) is disposed on a semiconductor substrate. Unwanted EUV-sensitive metal or metal oxide-containing film is optionally removed by bevel edge cleaning. The EUV-sensitive metal or metal oxide-containing film is directly patterned by EUV exposure. The pattern is then developed using a developer chemistry to form a resist mask. In some embodiments, the developer chemistry includes a halogen-containing compound. An etching gas may be supplied to the semiconductor substrate under atmospheric conditions to remove the EUV resist during development and / or bevel edge cleaning.
[0043] Dry etching techniques may use either a gentle plasma (low power) or thermal process with flowing etching gas. Dry etching under atmospheric conditions may be performed in a process chamber having a gas distributor for supplying the etching gas and a heating assembly facing the semiconductor substrate and having one or more heating elements. In some embodiments, the gas distributor may include an etching gas supply nozzle disposed above the substrate support. In some embodiments, the etching gas supply nozzle is connected to a movable swing arm for positioning the etching gas supply nozzle over a particular region of the semiconductor substrate. In some embodiments, the heating assembly includes multiple independently controllable heating zones. For example, the heating assembly may be disposed below the semiconductor substrate and may include multiple heating elements such as light emitting diodes (LEDs). Also, the process chamber for performing dry etching of EUV resist under atmospheric conditions may be a wafer cleaning chamber, a bake chamber, or a treatment chamber. Specifically, the process chamber for dry etching the EUV resist may be a wafer spin clean chamber, a bevel edge clean chamber, a post-apply bake chamber, a post-exposure bake chamber, a batch furnace reactor, a buffer module, a development chamber, or a Hexamethyldisilazane (HMDS) processing chamber. Such chambers may be part of a track system or cluster tool for photoresist processing. In this way, the dry etching process (e.g., dry development) may be integrated in the same station, module, or chamber as other processes in the photoresist processing, without transporting to a separate station, module, or chamber. Tool / chamber integration increases throughput and reduces costs.
[0044] FIG. 1 is a flow chart of an exemplary method of depositing and developing photoresist, according to some embodiments. The steps of process 100 may be performed in a different order and / or with different, fewer, or additional steps. Aspects of process 100 may be described with reference to FIGS. 2A-2C. One or more steps of process 100 may be performed using an apparatus or chamber as described in FIGS. 3A, 3B, 4-6, 7A, 7B, 8A, 8B, and 9-14. In some embodiments, the steps of process 100 may be performed, at least in part, according to software stored on one or more non-transitory computer-readable media.
[0045] At block 102 of process 100, a photoresist layer is deposited. This may be a dry deposition process, such as an evaporation process, or a wet process, such as a spin-on deposition process.
[0046] The photoresist may be a metal-containing EUV resist. The EUV sensitive metal or metal oxide-containing film may be deposited on the semiconductor substrate using any suitable technique, including wet (e.g., spin-on) or dry (e.g., CVD) deposition techniques. For example, the process described herein has been demonstrated for organotin oxide-based EUV photoresist compositions, and is applicable to both commercially spin-coatable formulations (e.g., those manufactured by Inpria Corp, Corvallis, Oregon) and formulations applied using dry vacuum deposition techniques, as described further below.
[0047] The semiconductor substrate may comprise any material composition suitable for photolithographic processing, particularly for the manufacture of integrated circuits and other semiconductor devices. In some embodiments, the semiconductor substrate is a silicon wafer. The semiconductor substrate may be a silicon wafer having features (underlying features) formed thereon and an irregular surface topography. As used herein, a "surface" is a surface onto which a film of the present disclosure is deposited or which is exposed to EUV during processing. The underlying features may include areas from which material has been removed (e.g., by etching) or to which material has been added (e.g., by deposition) in processing prior to carrying out the method of the present disclosure. Such pre-processing may include the method of the present disclosure or other processing methods in an iterative process in which two or more layers of features are formed on the substrate.
[0048] EUV-sensitive thin films may be deposited on semiconductor substrates, and such films may act as resists for subsequent EUV lithography and processing. Such EUV-sensitive thin films include materials that undergo changes upon exposure to EUV, such as loss of bulky pendant substituents bonded to metal atoms in low-density M-OH-rich materials, allowing crosslinking to higher-density MOM-bonded metal oxide materials. EUV patterning creates film regions with altered physical or chemical properties compared to unexposed regions. These properties can be exploited in subsequent processing, such as dissolving either the unexposed or exposed regions, or selectively depositing material in either the exposed or unexposed regions. In some embodiments, the unexposed film has a more hydrophobic surface than the exposed film under conditions in which such subsequent processing is performed. For example, material may be removed by exploiting differences in film chemical composition, density, and crosslinking. As described in more detail below, removal may be achieved by dry processing.
[0049] The thin film, in various embodiments, is an organometallic material (e.g., an organotin material including tin oxide), or other metal oxide material / moiety. The organometallic compound may be produced in a gas phase reaction of an organometallic precursor with a counter reactant. In various embodiments, the organometallic compound is formed by mixing a specific combination of an organometallic precursor having a bulky alkyl or fluoroalkyl group and a counter reactant, and polymerizing the mixture in the gas phase to produce a low density EUV sensitive material that is deposited on the semiconductor substrate.
[0050] In various embodiments, the organometallic precursors contain at least one alkyl group on each metal atom that is capable of surviving gas phase reaction, while other ligands or ions coordinated to the metal atom are replaceable with counter reactants. Organometallic precursors include those of formula 1: M a R b L c ...(Formula 1) where M is a metal with a high patterning radiation absorption cross section, R is C n H 2n+1 (preferably n≧2), L is a ligand, ion, or other moiety that reacts with a counter reactant, and a≧1, b≧1, c≧1.
[0051] In various embodiments, M is 1×10 7 cm 2 / mol or more. M may be, for example, selected from the group consisting of tin, hafnium, tellurium, bismuth, indium, antimony, iodine, germanium, and combinations thereof. In some embodiments, M is tin. R may be fluorinated (e.g., a compound of the formula: C n F x H (2n+1)In various embodiments, R has at least one beta hydrogen or beta fluorine. R may be selected from the group consisting of, for example, ethyl, i-propyl, n-propyl, t-butyl, i-butyl, n-butyl, sec-butyl, n-pentyl, i-pentyl, t-pentyl, sec-pentyl, and mixtures thereof. L may be any moiety that is readily displaced with a counter reactant to produce the M-OH moiety, such as a moiety selected from the group consisting of amines (dialkylamino, monoalkylamino, etc.), alkoxy, carboxylate, halogen, and mixtures thereof.
[0052] The organometallic precursor may be any of a variety of possible organometallic precursors. For example, when M is tin, such precursors include t-butyltris(dimethylamino)tin, i-butyltris(dimethylamino)tin, n-butyltris(dimethylamino)tin, sec-butyltris(dimethylamino)tin, i-propyl(tris)dimethylaminotin, n-propyltris(dimethylamino)tin, ethyltris(dimethylamino)tin, and analogous alkyl(tris)(t-butoxy)tin compounds (e.g., t-butyltris(t-butoxy)tin). In some embodiments, the organometallic precursor is partially fluorinated.
[0053] The counter reactant has the ability to replace a reactive moiety, ligand, or ion (e.g., L in formula 1 above) to link at least two metal atoms by a chemical bond. Counter reactants can include water, peroxides (e.g., hydrogen peroxide), di- or polyhydroxy alcohols, fluorinated di- or polyhydroxy alcohols, fluorinated glycols, and other sources of hydroxyl moieties. In various embodiments, the counter reactant reacts with the organometallic precursor by forming oxygen bridges between adjacent metal atoms. Other usable counter reactants include hydrogen sulfide and hydrogen disulfide, which can bridge metal atoms via sulfur bridges.
[0054] The thin film may include optional materials in addition to the organometallic precursor and counter reactant to modify the chemical or physical properties of the film (e.g., modify the film's sensitivity to EUV or increase etch resistance). Such optional materials may be introduced, such as by doping during vapor phase formation, before deposition on the semiconductor substrate, after deposition of the thin film, or both. In some embodiments, a mild remote H2 plasma may be introduced to replace some Sn-L bonds with Sn-H, which can increase the reactivity of the resist under EUV.
[0055] In various embodiments, the EUV patternable film is formed and deposited on the semiconductor substrate using vapor deposition equipment and processes known in the art. In such processes, the polymerized organometallic material is formed in the vapor phase or in situ on the surface of the semiconductor substrate. Suitable processes include, for example, chemical vapor deposition (CVD), atomic layer deposition (ALD), and ALD with CVD elements (such as discontinuous ALD-like processes in which the metal precursor and counter reactant are separated in time or space).
[0056] The methods generally include mixing a vapor flow of an organometallic precursor with a vapor flow of a counter-reactant to form a polymerized organometallic material and depositing the organometallic material on a surface of a semiconductor substrate. In some embodiments, two or more organometallic precursors are included in the vapor flow. In some embodiments, two or more counter-reactants are included in the vapor flow. As will be appreciated by one of ordinary skill in the art, the mixing and deposition aspects of the process may be simultaneous in a substantially continuous process.
[0057] In an exemplary continuous CVD process, two or more gas streams of organometallic precursor and counter reactant sources are introduced into a deposition chamber of a CVD apparatus through separate inlets, where the gas streams mix and react in the gas phase to form an aggregated polymeric material (e.g., by forming metal-oxygen-metal bonds). The gas streams may be introduced, for example, using separate inlets or a dual plenum showerhead. The apparatus is configured to mix the organometallic precursor and counter reactant flows in the chamber, thus allowing the organometallic precursor and counter reactant to react to form a polymerized organometallic material. Without limiting the mechanism, function, or utility of the present technology, it is believed that the products of such gas phase reactions have a high molecular weight due to the metal atoms being crosslinked by the counter reactant, and are precipitated or otherwise deposited on the semiconductor substrate. In various embodiments, the steric hindrance of the bulky alkyl groups prevents the formation of densely packed networks, forming a smooth amorphous low density film.
[0058] CVD processes are typically carried out at low pressures, such as between 10 milliTorr and 10 Torr. In some embodiments, the process is carried out at between 0.5 Torr and 2 Torr. In some embodiments, the temperature of the semiconductor substrate is equal to or lower than the temperature of the reactant stream. For example, the temperature of the substrate may be between 0° C. and 250° C., or between ambient temperature (e.g., 23° C.) and 150° C. In various processes, deposition of the polymerized organometallic material onto the substrate occurs at a rate that is inversely proportional to the surface temperature.
[0059] In some embodiments, the EUV patternable film is formed and deposited on the semiconductor substrate using wet deposition equipment and processes known in the art, for example, the organometallic material is formed by spin coating on the surface of the semiconductor substrate.
[0060] The thickness of the EUV patternable film formed on the surface of the semiconductor substrate may vary depending on the surface characteristics, materials used, and processing conditions. In various embodiments, the film thickness may range from 0.5 nm to 100 nm, and need only be thick enough to absorb most of the EUV light under the conditions of EUV patterning. The EUV patternable film may be capable of 30% or more absorption, which results in significantly fewer EUV photons being available toward the bottom of the EUV patternable film. High EUV absorption results in more crosslinking and densification near the top of the EUV exposed film than the bottom of the EUV exposed film. Insufficient crosslinking may lead to resist lifting and collapse in wet development, but not in dry development. Fully dry lithography schemes use resist films with low transparency to facilitate more efficient utilization of EUV photons. It is understood that while efficient utilization of EUV photons can be achieved with EUV patternable films having high overall absorption, in some cases the EUV patternable film may be less than about 30%. By comparison, most other resist films have a maximum overall absorption of less than 30% (e.g., 10% or less, or 5% or less) so that the resist material at the bottom of the resist film is fully exposed. In some embodiments, the film thickness is 10 nm to 40 nm, or 10 nm to 20 nm. Without limiting the mechanism, function, or utility of the present disclosure, it is believed that the process of the present disclosure is applicable to a wide variety of substrates because, unlike wet spin-coating processes in the art, there are few constraints on the surface adhesion properties of the substrate. Furthermore, as discussed above, the deposited film can closely conform to surface features, which is advantageous in forming a mask on a substrate, such as a substrate having underlying features, without "filling" or otherwise planarizing these features.
[0061] At block 104, an optional cleaning process is performed to clean the backside and / or bevel edge of the semiconductor substrate. In the backside and / or bevel edge cleaning, the EUV resist film may be non-selectively etched to equally remove films with different oxidation or crosslinking levels on the backside and bevel edge of the substrate. When the EUV patternable film is applied by wet or dry deposition processes, resist material may be unintentionally deposited on the bevel edge and / or backside of the substrate. This unintentional deposition may result in unwanted particles that may later migrate to the top side of the semiconductor substrate and become particle defects. Furthermore, this bevel edge and backside deposition may cause problems in downstream processing, such as contamination of the patterning (scanner) and development tools. Traditionally, this bevel edge and backside deposition is removed by wet cleaning techniques. For spin-coated photoresist materials, this process is called Edge Bead Removal (EBR) and is performed by directing a solvent flow from above and below the bevel edge while the substrate is spinning. The same process is applicable to soluble organotin oxide based resists deposited by evaporation techniques, however, in some embodiments, cleaning of the bevel edge and backside may be performed by dry cleaning techniques.
[0062] The bevel edge and / or backside cleaning of the substrate may be a dry cleaning process. In some embodiments, the dry cleaning process includes vapor and / or plasma with one or more of the following gases: HBr, HCl, BCl3, SOCl2, Cl2, BBr3, H2, O2, PCl3, CH4, methanol, ammonia, formic acid, NF3, HF. In some embodiments, the dry cleaning process may use the same chemistry as the dry developing process described herein. For example, the bevel edge and / or backside cleaning may use a halogen-containing developing chemistry. For the bevel edge and / or backside cleaning process, the vapor and / or plasma must be restricted to certain areas of the substrate so that there is no film degradation on the front side of the substrate and only the backside and bevel are removed.
[0063] Process conditions may be optimized for bevel edge and / or backside cleaning. In some embodiments, higher temperatures, higher pressures, and / or higher reactant flow rates may increase the etch rate. Suitable process conditions for bevel edge and backside dry cleaning may be as follows: reactant flow rates of 100-10,000 sccm (e.g., 500 sccm HCl, HBr, HI, or H2 and Cl2 or Br2, BCl3 or H2, or other halogen-containing compounds), temperature of 20° C.-140° C. (e.g., 80° C.), pressure of 20-1000 mTorr (e.g., 100 mTorr), or pressure of 50-765 Torr (e.g., 760 Torr), high frequency (e.g., 13.56 MHz) plasma power of 0-500 W, and time of about 10-20 seconds (depending on the photoresist film composition and properties). The bevel and / or backside cleaning may be performed using a Coronus® tool manufactured by Lam Research Corporation (Fremont, Calif.).
[0064] Alternatively, the dry cleaning step may be extended to complete photoresist removal, or photoresist "rework." "Rework" refers to the removal of applied EUV photoresist to prepare the semiconductor substrate for reapplication of photoresist, such as when the original photoresist is damaged or otherwise defective. Photoresist rework must be performed without damaging the underlying semiconductor substrate, and therefore oxygen-based etches must be avoided. Alternately, variations of halide-containing chemistries as described herein may be used. It is understood that the photoresist rework step may be applied at any stage during process 100. Thus, the photoresist rework step may be applied after photoresist deposition, after bevel edge and / or backside cleaning, after PAB processing, after EUV exposure, after PEB processing, after development, or after hard bake. In some embodiments, the photoresist rework may be performed to non-selectively remove exposed and unexposed areas of the photoresist, but selective to the underlying layers.
[0065] In some embodiments, the photoresist rework process includes steam and / or plasma having one or more of the following gases: HBr, HCl, HI, BCl3, Cl2, BBr3, H2, PCl3, CH4, methanol, ammonia, formic acid, NF3, HF.
[0066] Process conditions may be optimized for photoresist rework. In some embodiments, higher temperatures, higher pressures, and / or higher reactant flow rates may increase the etch rate. Suitable process conditions for photoresist rework may be as follows: reactant flow rates of 100-500 sccm (e.g., 500 sccm HCl, HBr, HI, BCl3 or H2 and Cl2 or Br2), temperature of 20° C.-140° C. (e.g., 80° C.), pressure of 20-1000 mTorr (e.g., 300 mTorr), or pressure of 50-765 Torr (e.g., 760 Torr), plasma power of 0-800 W (e.g., 500 W) at high frequency (e.g., 13.56 MHz), 0-200 V.b (the harder the underlying substrate material, the higher the bias may be used), and a time of about 20 seconds to 3 minutes (depending on the photoresist film composition and properties) sufficient to completely remove the EUV photoresist. It should be understood that these conditions are suitable for some processing reactors (e.g., Kiyo etch tools manufactured by Lam Research Corporation, Fremont, Calif.), but a wider range of processing conditions may be used depending on the capabilities of the processing reactor.
[0067] In some embodiments, the bevel edge cleaning may be performed using an etching gas under atmospheric conditions. Rather than requiring a vacuum device to create a vacuum environment within the process chamber, the bevel edge cleaning process chamber may be exposed to atmospheric conditions. In some embodiments, the bevel edge cleaning process chamber may expose the metal-containing EUV resist to a non-vacuum pressure, where the non-vacuum pressure is from about 50 Torr to about 765 Torr, from about 100 Torr to about 765 Torr, or from about 300 Torr to about 765 Torr. In some embodiments, the bevel edge cleaning process chamber may expose the metal-containing EUV resist to a pressure greater than atmospheric pressure, where the chamber pressure is greater than about 760 Torr. In some embodiments, the bevel edge cleaning process chamber may expose the metal-containing EUV resist to air or an ambient gas. The ambient gas may include oxygen, nitrogen, carbon dioxide, water vapor, or a combination thereof. In some embodiments, the bevel edge cleaning process chamber may expose the metal-containing EUV resist to a controlled atmosphere. Here, the controlled atmosphere includes exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or combinations thereof.
[0068] The process chamber may include one or more heaters for temperature control. The one or more heaters may be coupled to a heating assembly facing the semiconductor substrate in the process chamber for temperature control of the substrate. For example, the heating assembly may be located below the substrate support or between the substrate support and the semiconductor substrate. In some embodiments, the substrate temperature may be controlled using a radiative heating assembly, such as an IR lamp or one or more LEDs. During the bevel edge cleaning of the EUV resist, the semiconductor substrate may be subjected to an elevated temperature. Adjustments to the temperature may be made, and the temperature may affect various aspects of the etching, such as the etch rate. In some embodiments, the bevel edge cleaning includes heating the semiconductor substrate to a temperature of about 50° C. or more, about 100° C. or more, about 120° C. or more, or between about 100° C. and about 230° C.
[0069] In some embodiments, the bevel edge and / or backside cleaning process chamber may be a non-plasma thermal process chamber. The non-plasma thermal process chamber may not be capable of generating direct or remote plasma. In some other embodiments, the bevel edge and / or backside cleaning process chamber may be coupled to a direct or remote plasma source. The plasma source may be useful for generating plasma for bevel and / or backside cleaning or subsequent desorption, descumming, and smoothing steps.
[0070] In some embodiments, the bevel edge cleaning in the process chamber may be performed in a bake chamber, such as a bake chamber for performing the PAB process at block 106 or a bake chamber for performing the PEB process at block 110. In some embodiments, the bevel edge cleaning in the process chamber may be performed in a development chamber for performing development at block 112. In some embodiments, the bevel edge cleaning in the process chamber may be performed in a wafer cleaning chamber, such as a spin clean chamber. In some embodiments, the bevel edge cleaning in the process chamber may be performed in a processing chamber, such as an HMDS processing chamber. In some embodiments, the bevel edge cleaning in the process chamber may be performed in a batch furnace reactor. In some embodiments, the bevel edge cleaning in the process chamber may be performed in a single wafer or mini batch buffer module.
[0071] At block 106 of process 100, an optional post-application bake (PAB) is performed after deposition of the EUV patternable film and before EUV exposure. The PAB process may increase the EUV sensitivity of the EUV patternable film through a combination of thermal treatment, chemical exposure, and moisture, thereby reducing the EUV dose required to develop the pattern in the EUV patternable film. The PAB process temperature may be adjusted and optimized to increase the sensitivity of the EUV patternable film. For example, the process temperature may be about 90° C. to about 200° C., or about 150° C. to about 190° C. In some embodiments, the PAB process may be performed at atmospheric pressure to vacuum pressure and for a process time of about 1 minute to 15 minutes (e.g., about 2 minutes). In some embodiments, the PAB process is performed at atmospheric pressure and a temperature of about 100° C. to about 230° C.
[0072] At block 108 of the process 100, the metal-containing EUV resist film is exposed to EUV radiation for pattern development. In general, the EUV exposure changes the chemical composition and cross-linking within the metal-containing EUV resist film, creating contrast in etch selectivity that can be utilized for subsequent development.
[0073] The metal-containing EUV resist film may then be patterned by exposing a region of the film to EUV light (usually under a relatively high vacuum). EUV apparatus and imaging methods useful herein include methods known in the art. In particular, as described above, EUV patterning results in exposed regions of the film with altered physical or chemical properties compared to unexposed regions. For example, in exposed regions, cleavage of metal-carbon bonds may occur, such as by β-hydride elimination, leaving reactive and accessible metal hydride functional groups. The functional groups can be converted to hydroxides and crosslinked metal oxide moieties via metal-oxygen bridges in a subsequent post-exposure bake (PEB) step. This process can be used to create chemical contrast for development as a negative resist. In general, the higher the number of β-Hs in the alkyl group, the more sensitive the film. This can also be explained as the more branched the Sn-C bond is, the weaker it becomes. After exposure, the metal-containing EUV resist film may be baked. This can further crosslink the metal oxide film. The difference in properties between the exposed and unexposed regions may be exploited in subsequent processing to dissolve the unexposed regions, deposit material in the exposed regions, etc. For example, the pattern can be developed using a dry process to form a metal oxide-containing mask.
[0074] In particular, in various embodiments, hydrocarbyl-terminated tin oxides present at the surface are converted to hydrogen-terminated tin oxides in the exposed regions of the imaging layer, especially when the exposure is performed in a vacuum with EUV. However, when the exposed imaging layer is removed from the vacuum into air or the controlled introduction of oxygen, ozone, H2O2, or water, the surface Sn-H can be oxidized to Sn-OH. The difference in properties between the exposed and unexposed regions can be exploited in subsequent processing, for example by reacting the irradiated regions, the unirradiated regions, or both, with one or more reagents to selectively add or remove material from the imaging layer.
[0075] Without limiting the mechanism, function, or utility of the present technology, for example, 10 mJ / cm 2 ~100mJ / cm 2 EUV exposure at a dose of 100 nm can result in the cleavage of Sn-C bonds, which results in the loss of alkyl substituents and the relaxation of steric hindrance, allowing the collapse of low-density films. Furthermore, the reactive metal-H bonds generated in the β-hydride elimination reaction can react with adjacent active groups, such as hydroxyl groups, in the film, resulting in further cross-linking and densification, and creating a chemical contrast between exposed and unexposed regions.
[0076] The metal-containing EUV resist film is exposed to EUV light to obtain a photopatterned metal-containing EUV resist, which includes EUV exposed and unexposed regions.
[0077] To further enhance the contrast of the etch selectivity of the photopatterned metal-containing EUV resist, an optional post-exposure bake (PEB) is performed at block 110 of the process 100. The photopatterned metal-containing EUV resist may be thermally treated in the presence of various chemical species to promote crosslinking of the EUV exposed regions, or may simply be baked on a hotplate in ambient air at, for example, 100° C.-250° C. for 1-5 minutes (e.g., 190° C. for 2 minutes).
[0078] In various embodiments, the bake method includes careful control of the bake environment, introduction of reactive gases, and / or careful control of the rate of increase of the bake temperature. Examples of useful reactive gases include air, H2O, H2O2 vapor, CO2, CO, O2, O3, CH4, CH3OH, N2, H2, NH3, N2O, NO, alcohol, acetylacetone, formic acid, Ar, He, or mixtures thereof. The PEB process is designed to (1) promote complete evaporation of organic fragments generated during EUV exposure, (2) oxidize Sn-H, Sn-Sn, or Sn radical species generated by EUV exposure to metal hydroxides, and (3) promote cross-linking between adjacent Sn-OH groups to form a more tightly cross-linked SnO2-like network. The bake temperature is carefully selected to achieve optimal EUV lithography performance. Too low a PEB temperature will result in insufficient cross-linking, which will result in poor chemical contrast during development at a given dose. Also, too high a PEB temperature can result in adverse effects such as severe oxidation and film shrinkage in unexposed areas (in this example, areas removed by development of the pattern film to form the mask) and undesirable interdiffusion at the interface between the photopatterned metal-containing EUV resist and the underlayer. Both of these can contribute to loss of chemical contrast and increased defect density due to insoluble scum. The PEB treatment temperature can be about 100°C to about 300°C, about 170°C to about 290°C, or about 200°C to about 240°C. In some embodiments, the PEB treatment can be performed at atmospheric pressure to vacuum and for a treatment time of about 1 minute to 15 minutes (e.g., about 2 minutes). In some embodiments, the PEB heat treatment can be repeated to further increase the etch selectivity.
[0079] At block 112 of process 100, the photopatterned metal-containing EUV resist is developed to form a resist mask. In various embodiments, either the exposed areas are removed (positive tone) or the unexposed areas are removed (negative tone). In some embodiments, the development may include selectively depositing a metal on either the exposed or unexposed areas of the photopatterned metal-containing EUV resist followed by an etching step. In various embodiments, these processes may be dry or wet processes. In some embodiments, the development may be performed with a halogen-containing gas flow without igniting a plasma. Alternatively, the development may be performed with a halogen-containing gas flow activated in a remote plasma source or activated by exposure to remote UV radiation. The developing photoresist may include an element selected from the group consisting of tin, hafnium, tellurium, bismuth, indium, antimony, iodine, and germanium. The element may have a high patterning radiation absorption cross-section. In some embodiments, the element may have a high EUV absorption cross-section. In some embodiments, metal-containing EUV resists may have an overall absorption of greater than 30%, allowing for more efficient utilization of EUV photons in fully dry lithography processes and enabling the development of thicker, less EUV transparent resists.
[0080] An example of a development process involves exposing an organotin oxide-containing EUV-sensitive photoresist film (e.g., 10-30 nm (e.g., 20 nm) thick) to EUV radiation, post-exposure baking, and developing. The photoresist film may be deposited based on a gas-phase reaction of an organotin precursor, such as isopropyl(tris)(dimethylamino)tin, with water vapor, or may be a spin-on film containing tin clusters in an organic matrix.
[0081] 2A-2C are schematic cross-sectional views of various process stages of dry development according to some embodiments. The examples shown in FIGS. 2A-2C illustrate negative tone dry development. As shown in FIG. 2A, wafer 200 includes substrate 202 and substrate layer 204 to be etched. In some embodiments, substrate layer 204 includes an ashable hard mask such as spin-on carbon (SoC) or other materials (e.g., silicon, silicon oxide, silicon nitride, silicon carbide, etc.). In some embodiments, substrate layer 204 may be a layer stack disposed on substrate 202. Wafer 200 further includes photo-patterned metal-containing EUV resist film 206. For example, photo-patterned metal-containing EUV resist film 206 may be an organic metal-containing layer disposed on substrate layer 204 to be etched. Photo-patterned metal-containing EUV resist film 206 may have a thickness of about 5 nm to about 50 nm, or about 10 nm to about 30 nm. The photo-patterned metal-containing EUV resist film 206 may be provided in a process chamber after photo-patterning in an EUV scanner and / or after PEB processing as described above. The photo-patterned metal-containing EUV resist film 206 includes non-EUV exposed regions 206a and EUV exposed regions 206b. As shown in FIG. 2B, the non-EUV exposed regions 206a of the photo-patterned metal-containing EUV resist film 206 can be removed in a dry development process by exposing it to a flow of dry development chemicals without igniting a plasma. The dry development chemicals may include halogen-containing chemicals. After development by removal of the non-EUV exposed regions 206a, a resist mask 208 is formed. The substrate layer 204 to be etched can then be etched using the resist mask 208, resulting in the structure shown in FIG. 2C.
[0082] 1, the photopatterned metal-containing EUV resist is developed by exposure to a dry development chemistry at block 112, where the dry development chemistry is a halogen-containing chemistry. In some embodiments, the dry development of the EUV resist is combined with other dry processing steps, such as dry deposition (e.g., CVD) of a metal-containing EUV resist film.
[0083] In some embodiments, photoresist processing of a semiconductor substrate may combine all dry steps including deposition film formation, backside and / or bevel edge dry clean, PAB processing, EUV lithography patterning, PEB processing, and dry development. Each of the steps in blocks 102-114 of process 100 may be dry processing steps. Such processing steps may avoid material and production costs associated with wet processing steps such as wet development. Dry processing allows for increased tunability as well as additional critical dimension (CD) control and scum removal. Wet development is limited by solubility and cluster size, whereas dry development is not. Wet development is more prone to pattern collapse and delamination issues that can be avoided with dry development.
[0084] In some embodiments, the dry development process can be performed using either a gentle plasma (high pressure, low power) or a thermal process while flowing dry development chemicals. For example, dry development can be performed with a thermal process using dry development chemicals. In some embodiments, dry development can rapidly remove unexposed material and leave a pattern in the exposed film that can be transferred to an underlying layer by a plasma-based etching process, such as a conventional etching process.
[0085] In a thermal development process, the substrate is exposed to a development chemical (e.g., Lewis acid) in a process chamber (e.g., oven). Instead of requiring a vacuum device to create a vacuum environment in the process chamber, the process chamber may be exposed to atmospheric conditions. That is, the thermal development process chamber may expose the photo-patterned metal-containing EUV resist to a non-vacuum pressure. Here, the non-vacuum pressure is about 50 Torr to about 765 Torr, about 100 Torr to about 765 Torr, or about 300 Torr to about 765 Torr. In some embodiments, the thermal development process chamber may expose the metal-containing EUV resist to a pressure above atmospheric pressure. Here, the chamber pressure is greater than about 760 Torr. In some embodiments, the thermal development process chamber may expose the photo-patterned metal-containing EUV resist to air or an ambient gas. The ambient gas may include oxygen, nitrogen, carbon dioxide, water vapor, or a combination thereof. In some embodiments, the thermal development process chamber may expose the photo-patterned metal-containing EUV resist to a controlled atmosphere. Here, the controlled atmosphere includes exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or combinations thereof.
[0086] The thermal development process chamber may include one or more heating elements for temperature control. The one or more heating elements may be coupled to a heating assembly facing the semiconductor substrate in the process chamber for substrate temperature control. In some embodiments, the one or more heating elements may be one or more LEDs. The LEDs may be arranged in multiple independently controllable heating zones. During dry development of the EUV resist, the semiconductor substrate may be subjected to an elevated temperature. Adjustments to the temperature may be made, and may affect various aspects of development, such as etch selectivity. In some embodiments, dry development includes heating the semiconductor substrate to a temperature of about 50° C. or higher, about 100° C. or higher, about 120° C. or higher, or between about 100° C. and about 230° C.
[0087] The thermal development process chamber may include an etching gas supply nozzle or an etching gas distributor disposed above the substrate support. The etching gas flow rate may be adjusted, and the gas flow rate may affect the etching selectivity between exposed and unexposed regions during development. In some embodiments, the gas flow rate is 0.5 SLM to about 30 SLM, about 1 SLM to about 20 SLM, or about 2 SLM to about 15 SLM. The gas flow rate includes the total flow rate of the gases flowing, including the etching gas and the carrier gas (nitrogen, argon, etc.). The flow rate of the etching gas may be a small portion of the total flow rate. Here, the flow rate of the etching gas may be about 0.01 SLM to about 1 SLM. In the thermal development process, the exposure time may be adjusted. The exposure time may depend, among other things, on the desired amount of resist removal, the development chemistry, the amount of crosslinking in the resist, and the composition and properties of the resist. In some embodiments, the exposure time may be about 1 second to about 50 minutes, about 3 seconds to about 20 minutes, or about 10 seconds to about 6 minutes.
[0088] The etch selectivity during dry development is adjustable by controlling process conditions such as temperature, pressure, gas flow, gas composition, and plasma power, among other adjustable process conditions. The etch selectivity may be adjusted in a single step or multiple steps to achieve the desired patterning characteristics. In some embodiments, the etch selectivity during dry development is adjusted over one or more steps to affect the EUV resist profile. More specifically, the amount of taper or re-entrant angle in the EUV resist profile can be controlled by applying developer chemistries with different etch selectivity over one or more steps. Also, scum removal, photoresist work, hardening, smoothing, and cleaning steps can be adjusted according to the adjustable etch selectivity.
[0089] In some embodiments, the dry development process chamber may be a plasma-free thermal process chamber. The plasma-free thermal process chamber may be one that is not capable of generating direct or remote plasma. In some other embodiments, the dry development process chamber may be coupled to a direct or remote plasma source. The plasma source may be one that is useful for generating plasma for dry development or subsequent desorption, descumming, and smoothing steps.
[0090] In some embodiments, the dry development in the process chamber may occur in a bake chamber, such as a bake chamber for performing the PAB process at block 106 or a bake chamber for performing the PEB process at block 110. In some embodiments, the dry development in the process chamber may occur in a wafer cleaning chamber, such as a bevel edge cleaning chamber for performing the bevel edge cleaning at block 104. In some embodiments, the dry development in the process chamber may occur in a wafer cleaning chamber, such as a spin clean chamber. In some embodiments, the dry development in the process chamber may occur in a processing chamber, such as an HMDS processing chamber. In some embodiments, the dry development in the process chamber may occur in a batch furnace reactor. In some embodiments, the dry development in the process chamber may occur in a single wafer or mini batch buffer module.
[0091] At block 114 of the process 100, the semiconductor substrate is optionally hard baked. During the hard bake process, the semiconductor substrate is subjected to an elevated temperature. For example, the semiconductor substrate may be subjected to an elevated temperature of about 50° C. or greater, about 100° C. to about 300° C., or about 170° C. to about 290° C. The hard bake process may remove residual solvent or etching gases from the dry developer.
[0092] 3A and 3B are schematic diagrams of an exemplary process chamber for performing dry etching of photoresist, according to some embodiments. In FIG. 3A and FIG. 3B, the process chamber 300 is in communication with the atmosphere. The process chamber 300 includes a platen or substrate support 310 on which a semiconductor substrate 320 is supported. In some embodiments, the substrate support 310 may be coupled to one or more heaters (not shown) configured to control a substrate temperature of the semiconductor substrate 320. In some embodiments, the substrate support 310 may be configured to spin the semiconductor substrate 320 such that the semiconductor substrate 320 rotates. In some embodiments, the substrate support 310 may be a bake plate used in PAB or PEB processing. Surprisingly, dry etching (e.g., dry development) of EUV resist can be performed under atmospheric pressure in an open air environment or under a controlled atmosphere above atmospheric pressure without subjecting the process chamber 300 to a vacuum. In some embodiments, the process chamber for performing dry etching may be a non-plasma-based thermal process chamber. In other words, a non-plasma based thermal process chamber may be one that is not capable of generating a direct or remote plasma. In some other embodiments, the process chamber for performing dry etching may be a plasma based process chamber.
[0093] In FIG. 3A, the apparatus includes a process chamber 300. The process chamber 300 is exposed to atmospheric conditions. In some embodiments, the process chamber 300 is a bake chamber. In some embodiments, the apparatus includes a bake plate 310 for supporting a semiconductor substrate 320 in the process chamber 300. In some embodiments, the bake plate 310 includes an upper surface and a plurality of minimum contact area (MCA) supports (not shown) for supporting the semiconductor substrate above the upper surface of the bake plate 310. The bake plate 310 may include a plurality of heating zones (not shown), each of which includes one or more heating elements. The apparatus further includes an etching gas distributor 330 disposed above the bake plate 310. The etching gas distributor 330 may be a showerhead having a faceplate facing the semiconductor substrate 320. Here, the faceplate includes a plurality of through holes for supplying an etching gas to the semiconductor substrate 320. The showerhead may function to introduce etching gases during dry development, dry bevel edge cleaning, or other dry photoresist processes. In some embodiments, the showerhead may deliver etching gases to the entire semiconductor substrate 320 or locally to specific regions of the semiconductor substrate 320. The process chamber 300 is not necessarily under vacuum, but an exhaust fan or pump may be coupled to the process chamber 300 to remove etching by-products and other residual gases.
[0094] In FIG. 3B, the apparatus includes a process chamber 300. The process chamber 300 is exposed to atmospheric conditions. It is understood that the process chamber 300 is not necessarily connected to a vacuum pump or other vacuum equipment. However, the process chamber 300 may be coupled to an exhaust fan or pump to remove etch by-products and other residual gases. In some embodiments, the process chamber 300 is a wafer spin clean chamber. In some embodiments, the apparatus includes a substrate support 310 for holding a semiconductor substrate 320 in the process chamber 300. The substrate support 310 may be configured to rotate the semiconductor substrate 320. The apparatus further includes a heating assembly (not shown) facing the semiconductor substrate 320 in the process chamber 300. The heating assembly includes multiple heating elements. The multiple heating elements may include multiple LEDs. The multiple LEDs may be arranged in multiple heating zones that are independently controllable. The apparatus further includes an etching gas supply nozzle 340 disposed above the substrate support 310. The etching gas supply nozzle 340 is movable such that a supply position of the etching gas is located above the semiconductor substrate 320. In some embodiments, the etching gas supply nozzle 340 is coupled to a movable swing arm for locally positioning the etching gas supply nozzle 340 over a particular region of the semiconductor substrate 320. For example, the movable swing arm may position the etching gas supply nozzle 340 radially from the center to the edge of the semiconductor substrate 320. In some embodiments, the etching gas supply nozzle 340 is positioned at an angle or perpendicular to the surface of the semiconductor substrate 320.
[0095] Process chambers for dry development of photoresist or bevel edge cleaning may be implemented within a track lithography system. Many steps associated with photolithography are typically performed within a multi-chamber system or cluster tool that has the ability to sequentially process semiconductor substrates in a controlled manner. Cluster tools for depositing and developing photoresist materials are sometimes referred to as track lithography tools. Track lithography tools typically include a mainframe that houses multiple dedicated process chambers for performing various elements of photolithography. Some of the process chambers may be wet process chambers and some may be dry process chambers. Some of the process chambers may be exposed to an open air environment and some may be in a vacuum environment. Process chambers for dry removal may be exposed to an open air environment or to a controlled atmosphere above atmospheric pressure within the track lithography tool. Track lithography tools often include a pod / cassette loading device for receiving and returning semiconductor substrates to a clean room. Track lithography tools also often include a transfer robot for transferring semiconductor substrates between the various chambers / stations.
[0096] FIG. 4 is a schematic diagram of an exemplary system architecture or track system for photoresist processing, according to some embodiments. The track system 400 includes a cassette loading section 410, a processing section 420, an interface section 430, and an exposure section 440. A semiconductor wafer W may be received in a cassette 402 and returned to a cassette 404. The processing section 420 may have multiple process chambers or stations 421-426. A transfer robot 455 may be configured to move along a central passage 450 to transfer the semiconductor wafer between the chambers. In the present disclosure, at least one of the multiple process chambers or stations 421-426 is exposed to atmospheric conditions and configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor wafer W.
[0097] The exposure unit 440 is connected to the processing unit 420 via the interface unit 430. The exposure unit 440 may include a scanner for exposing a photosensitive material on the semiconductor wafer W to electromagnetic radiation (eg, EUV radiation).
[0098] The processing section 420 may include one or more deposition chambers 421 for depositing a photoresist material on the semiconductor wafer W. One of the deposition chambers 421 may be configured to deposit a resist coating, such as an anti-reflective coating, and another of the deposition chambers 421 may be configured to deposit a photoresist material. The processing section 420 may further include a wafer cleaning chamber 422. For example, the wafer cleaning chamber 422 may clean the semiconductor wafer W with a pure water jet. The processing section 420 may further include a processing chamber 423. For example, the processing chamber 423 may include an adhesion processing chamber for applying HMDS to the surface of the semiconductor wafer W. In some embodiments, the processing section 420 further includes one or more bake chambers 424. For example, each bake chamber 424 may have one or more bake plates for heating the semiconductor wafer W. The bake chamber 424 may perform a PAB process or a PEB process in the photoresist process. In some embodiments, the processing section 420 further includes a scrub station 425 for scrubbing the semiconductor wafer W with a rotating brush. In some embodiments, the processing section 420 optionally includes a development chamber 426 for developing the photoresist with a development chemistry.
[0099] In the present disclosure, it is understood that the process chamber for dry removal may be any of the process chambers 421-426 in the track lithography system 400. Thus, rather than a dedicated station for dry removal, a process chamber in the track lithography system 400 may be modified to perform dry removal or may be integrated to perform dry removal along with baking, cleaning, scrubbing, treating, depositing, or other photoresist processing functions. As an example, the deposition chamber 421 for depositing metal-containing EUV may be configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor wafer W. As another example, the bake chamber 424 may be configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor wafer W. As yet another example, the wafer cleaning chamber 422 may be configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor wafer W. As yet another example, the HMDS processing chamber for processing a surface of the semiconductor wafer W may be configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor wafer W. Alternatively, the development chamber 426 may be modified to perform baking, cleaning, scrubbing, treating, depositing, or other photoresist processing functions along with dry removal, which may be performed under atmospheric conditions.
[0100] 5 is a schematic diagram of another exemplary system architecture or track system for photoresist processing, according to some embodiments. The track lithography system 500 includes a front-end module 510 (also referred to as a factory interface), a central module 520, and a rear module 530 (also referred to as a scanner interface). The front-end module 510 includes one or more pods or Front Opening Unified Pods (FOUPs) 512. The FOUPs 512 are configured to receive one or more semiconductor wafers W to be processed in the track lithography system 500.
[0101] The front-end module 510 includes a first processing rack 514 and a second processing rack 516 along with a front-end robot 518. The central module 520 includes a first processing rack 524 and a second processing rack 526 along with a central robot 528. The rear module 530 includes a first processing rack 534 and a second processing rack 536 along with a back-end robot 538. In some embodiments, the processing racks 534 and 536 of the rear module 530 may be configured to exchange semiconductor wafers W using a stepper or scanner 540. The scanner 540 exposes photoresist material deposited on the semiconductor wafer to some form of electromagnetic radiation (e.g., EUV radiation).
[0102] Each of the processing racks 514, 516, 524, 526, 534, 536 may include multiple processing modules in a vertically stacked arrangement. That is, each of the processing racks 514, 516, 524, 526, 534, 536 may include multiple stacked coating modules, thermal or bake modules, cleaning modules, developing modules, or other modules adapted to perform photoresist processing steps. As an example, the coating modules may deposit an anti-reflective coating or photoresist layer, the thermal and bake modules may perform a bake / chill step, and the developing modules may perform a developing step. The processing racks in the track lithography system 500 may be modified to perform dry stripping or may be integrated to perform dry stripping together with coating, thermal or bake steps, cleaning, or other photoresist processing functions. The processing racks may be exposed to atmospheric conditions to perform dry stripping.
[0103] In some embodiments, the track lithography system 500 further includes a controller 550 in communication with the scanner 540 and configured to monitor and control aspects of the processes occurring in the front end module 510, the central module 520, and the rear module 530. Aspects of the controller 550 are described in further detail below.
[0104] A dry etch process (e.g., dry develop) under atmospheric conditions may be performed in a thermal process chamber, such as a bake plate or oven. In some embodiments, the thermal process chamber may additionally perform a PAB or PEB process in the photoresist processing. In some embodiments, the method of depositing and developing photoresist includes baking the metal-containing EUV resist at an elevated temperature in the same process chamber as the dry developing the metal-containing EUV resist. In some embodiments, the method of depositing and developing photoresist includes baking the metal-containing EUV resist at an elevated temperature in the same process chamber as the bevel edge cleaning the metal-containing EUV resist from the semiconductor substrate.
[0105] The PAB or PEB thermal treatment raises the substrate temperature to an elevated temperature, such as about 100°C to about 170°C or about 120°C to about 150°C. In some embodiments, the substrate temperature may be controlled using a radiative heat source, such as an IR lamp or one or more LEDs. The radiative heat source may be located below the substrate. Alternatively, the radiative heat source may be located above the substrate. The substrate temperature may be actively controlled by a pyrometer in a feedback control loop established with the radiative heat source. The atmosphere during the PAB or PEB thermal treatment may be controlled by flowing an inert gas, such as N2, Ar, He, Xe, or Ne. Here, the inert gas may be mixed with O2 and / or H2O. In some embodiments, the pressure during the PAB or PEB thermal treatment may be controlled to a pressure below atmospheric pressure. In some embodiments, the pressure during the PAB or PEB treatment may be controlled to a pressure above atmospheric pressure.
[0106] In some embodiments, the thermal processing chamber includes a substrate support constructed of a highly conductive metal, such as aluminum, that can be used to spread heat from a source to heat the semiconductor substrate. In some embodiments, the thermal processing chamber includes a bake plate having one or more resistive heating elements embedded therein or in thermal communication with one or more resistive heating elements. The bake plate may include multiple heating zones to control various zone temperatures. In some embodiments, one or more proximity pins or MCA supports may be configured to adjust the height of the semiconductor substrate above the top surface of the bake plate to control the substrate temperature. In some embodiments, a faceplate may be disposed above the bake plate. Control of the substrate temperature may be further achieved by the temperature of the faceplate.
[0107] Dry etching processes (e.g., dry development) under atmospheric conditions may be performed in a batch furnace reactor. A batch furnace reactor may be a vertical oven for processing multiple substrates at once and may operate over a large pressure range. For example, such a vertical oven may operate at pressures from about 50 Torr to about 765 Torr, or even above about 760 Torr. Operating at pressures above atmospheric pressure may be useful to avoid leak-in contamination with oxygen or air.
[0108] FIG. 6 is a schematic diagram of an exemplary batch vertical furnace for performing dry etching of photoresist, according to some embodiments. The batch vertical furnace 600 may be a vertical oven for batch processing of substrates 606. The batch vertical furnace 600 may include a substrate support 620 for holding a plurality of substrates 606. As shown in FIG. 6, the plurality of substrates 606 may be supported and stacked on top of each other. Each substrate 606 may be supported by the substrate support 620 and held by gravity. This allows batch processing of tens or hundreds of wafers 606 in a single pass through the batch vertical furnace 600. The batch vertical furnace 600 includes a plurality of heating elements 610 for subjecting the plurality of substrates 606 to an elevated temperature. As shown in FIG. 6, the plurality of heating elements 610 may surround the chamber wall 602 of the batch vertical furnace 600. However, it is understood that the plurality of heating elements 610 may be integrated into the substrate support 620. In some embodiments, the substrate support 620 may be a number of plates for holding each of the plurality of substrates 606. In some embodiments, the substrate support 620 may support each of the plurality of substrates 606 at their edges, such as a slotted support frame.
[0109] The batch vertical furnace 600 further includes one or more etching gas inlets 630 for supplying an etching gas to a furnace reactor enclosed by the chamber walls 602 of the batch vertical furnace 600. The one or more etching gas inlets 630 may supply a precursor gas for a deposition step or a purge gas for a purge step in addition to or instead of the etching gas. The one or more etching gas inlets 630 may supply a gas flow 632 side-to-side or parallel across the substrate surfaces of the plurality of substrates 606. This promotes uniformity of the gas flow across the plurality of substrates 606. Each of the plurality of substrates 606 may include a metal-containing EUV resist. The etching gas may react with the metal-containing EUV resist to remove one or more portions of the metal-containing EUV resist from the plurality of substrates. This may be done in a bevel edge cleaning process, dry development, or other photoresist processing step.
[0110] In some embodiments, the batch vertical furnace 600 further includes a motor 650 configured to rotate the substrate support 620. In this manner, the substrates 606 may be rotated while being subjected to an elevated temperature and / or exposed to an etching gas. This reduces the possibility of differences due to the position of the gas inlet and / or gas outlet. In some embodiments, the batch vertical furnace 600 further includes one or more gas outlets 640. The one or more gas outlets 640 may be configured to remove etching by-products and residual gases from the batch vertical furnace 600. In some embodiments, the one or more gas outlets 640 may be coupled to a vacuum pump or an exhaust fan.
[0111] In some embodiments, the chamber walls 602 of the batch vertical furnace 600 include a material that is resistant to etching gases, particularly etching gases that include halogen-based compounds such as HBr, HCl, or BCl3. For example, the material of the chamber walls 602 may include quartz, a ceramic material, or a low-temperature polymer material, rather than an aluminum-based material that is more susceptible to corrosion. In some embodiments, the low-temperature polymer material may be polytetrafluoroethylene (PTFE). The batch vertical furnace 600 may be useful in dry development or other photoresist processes that do not require low temperatures, tight control of the stoichiometry of the etching reactants, or uniformity of gas flow across multiple substrate surfaces.
[0112] Dry etching processes under atmospheric conditions (e.g., dry development) may be performed in single-wafer or mini-batch buffer modules. Such buffer modules may provide a controlled atmosphere. The controlled atmosphere may be used in heating or cooling steps. The controlled atmosphere may include exposure to air or ambient gases. Alternatively, the controlled atmosphere may include exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or combinations thereof. In some embodiments, the controlled atmosphere may be operated at atmospheric pressure or above atmospheric pressure.
[0113] The buffer module may hold one or more substrates, where the substrates may include a metal-containing EUV resist. The single-wafer or mini-batch buffer module may include one or more etch gas inlets for supplying etch gas to the one or more substrates. The etch gas may remove one or more portions of the metal-containing EUV resist. In some embodiments, the buffer module may be used within a FOUP or storage case for 300 mm wafers. The buffer module may be directly applied to a slow and / or high temperature degassing step to remove etch by-products, such as volatile tin-containing by-products.
[0114] Dry etching processes (e.g., dry development) under atmospheric conditions may be performed in a wafer cleaning chamber. The wafer cleaning chamber may include one or more discharge nozzles for delivering gas or liquid to the semiconductor substrate. In some embodiments, the wafer cleaning chamber may have a substrate support or chuck configured for rotation such that processing fluids are transferred outward from the edge of the rotating substrate. In some embodiments, the substrate support or chuck may include or be coupled to one or more heating elements for heating the semiconductor substrate. Heating the semiconductor substrate may generally facilitate evaporation of the rinsing liquid. In some embodiments, the wafer cleaning station may be configured to perform bevel edge cleaning of the semiconductor substrate. In some embodiments, the wafer cleaning station may be a thermal process station or chamber that does not use plasma. In some other embodiments, the wafer cleaning station may be configured to generate direct or remote plasma for performing desorption, descumming, and smoothing steps.
[0115] In some embodiments, the method of depositing and developing photoresist includes performing bevel edge cleaning of the semiconductor substrate in the same process chamber as performing dry developing the metal-containing EUV resist. In some embodiments, the method of depositing and developing photoresist includes dry developing the metal-containing EUV resist in the same process chamber as performing bevel edge cleaning of the semiconductor substrate.
[0116] 7A and 7B are schematic diagrams of a wafer cleaning station configured to perform dry etching of photoresist, according to some embodiments. In some embodiments, the wafer cleaning station 700 may be a spin-rinse dry cleaning station. The wafer cleaning station 700 includes a substrate support pedestal 710, a liquid nozzle 714, and a gas nozzle 716. The liquid nozzle 714 may be attached to a liquid supply arm or a movable swing arm 704 such that the liquid nozzle 714 is attached to a distal end of the liquid supply swing arm 704. The gas nozzle 716 may be attached to a gas supply arm or a movable swing arm 706 such that the gas nozzle 716 is attached to a distal end of the gas supply swing arm 706. As shown in FIGS. 7A and 7B, both nozzles 714, 716 are positioned such that liquid or gas is delivered toward the center of the semiconductor substrate 702. A processing fluid may be ejected from the liquid nozzle 714 onto the semiconductor substrate 702. In some embodiments, the processing fluid may be ejected as a water jet. During the cleaning process, the semiconductor substrate 702 may be rotating and the liquid nozzle 714 may supply the processing fluid to the semiconductor substrate 702 such that centrifugal force acting on the processing fluid causes the processing fluid to fly out of the edge of the semiconductor substrate 702. The liquid nozzle 714 may be rotated toward the edge of the semiconductor substrate 702. The gas nozzle 716 may assist in drying the surface of the semiconductor substrate 702. The gas nozzle 716 may be rotated to rotate about a rotatable axis away from the center of the semiconductor substrate 702. In other words, the gas nozzle 716 may move radially outward toward the edge of the semiconductor substrate 702. The gas nozzle 716 may be configured to perform other modes of movement such as translation or rotation. The positioning of the liquid nozzle 714 and / or the gas nozzle 716 may be controlled via a controller and a feedback loop.
[0117] The wafer cleaning station 700 may be modified or integrated to perform dry development and / or dry bevel edge cleaning under atmospheric conditions. In particular, the gas nozzle 716 and gas delivery arm 706 may function to deliver etching gas for photoresist development or photoresist bevel edge cleaning. The gas delivery arm 706 is movable to precisely position the gas nozzle 616 over a particular localized area of the semiconductor substrate 602. The localized gas delivery over the semiconductor substrate 702 may enable increased uniformity in the photoresist dry development or bevel edge cleaning.
[0118] 8A and 8B are schematic diagrams of a wafer cleaning and heating station configured to perform dry etching of photoresist, according to some embodiments. The wafer cleaning and heating station 800 may be configured to perform localized heating of the semiconductor substrate 802 and to provide a fluid (e.g., gas or liquid) to the semiconductor substrate 802. A rotating chuck 810 may be designed to hold and rotate the semiconductor substrate 802. In some embodiments, the semiconductor substrate 802 is held by a series of gripping pins 816. The gripping pins 816 may pass through openings in a plate 825. The plate 825 may be made of quartz or sapphire. The plate 825 may be fixed to the rotating chuck 810. When the semiconductor substrate 802 is placed on the rotating chuck 810, the semiconductor substrate 802 is held above the plate 825 such that the bottom surface of the semiconductor substrate 802 is parallel to the plate 825 and is spaced apart from the plate 825 by a small gap. In some embodiments, the wafer cleaning and heating station 800 further includes an exhaust fan (not shown) for removing etch by-products and other residual gases from the wafer cleaning and heating station 800. In some embodiments, the wafer cleaning and heating station 800 further includes a gas source (not shown) for supplying an inert or diluent gas into the wafer cleaning and heating station 800. The gas source may increase the pressure above atmospheric pressure and / or supply useful gases other than air to the semiconductor substrate 802.
[0119] A movable swing arm 830 is provided adjacent to the rotating chuck 810. The movable swing arm 830 is mounted for pivotal movement about its drive motor 834. The movable swing arm 830 is supplied with a dispensing fluid. The dispensing fluid is dispensed downward through a dispensing nozzle 832 of the movable swing arm 830. The movable swing arm 830 is movable between a standby position shown by a solid line and a center position shown by a dashed line. Thus, the dispensing nozzle 832 can scan over the entire radius of the semiconductor substrate 802 and dispense the dispensing fluid over the entire top surface of the semiconductor substrate 802 as it is rotated by the rotating chuck 810. In some embodiments of the present disclosure, the dispensing fluid includes an etching gas for dry development of a metal-containing EUV resist or bevel edge cleaning of a metal-containing EUV resist. In some embodiments of the present disclosure, the wafer cleaning and heating station 800 may be exposed to an open air environment. For example, the pressure in the wafer cleaning and heating station 800 may be about 50 Torr to about 765 Torr. In some embodiments of the present disclosure, the wafer cleaning and heating station 800 may be under a controlled atmosphere. For example, the controlled atmosphere may include exposure to atmospheric pressure or pressures above atmospheric pressure. The controlled atmosphere may include exposure to an inert or diluent gas, such as nitrogen, water vapor, carbon dioxide, argon, helium, or combinations thereof.
[0120] Below the plate 825 is a heating assembly 850. The heating assembly 850 is attached to a fixed post 820 and does not rotate. The heating assembly 850 may include multiple heating elements 852 for multiple independently controllable heating zones. In some embodiments, the multiple heating elements 852 include multiple LEDs, such as blue LEDs. Thus, the heating assembly 850 may be a radiant heating assembly. The multiple heating elements 852 may be connected to a controller 854. The controller 854 may control the on / off and power of the multiple heating elements 852. In some embodiments, the controller 854 further communicates with a drive motor 834 for positioning the movable swing arm 830.
[0121] As shown in FIG. 8A, the heating elements 852 may be LEDs arranged in multiple concentric circles. For example, the LEDs may be arranged in 20 concentric circles, each circle being a multiple of 16. Such an arrangement therefore allows each concentric circle to be individually controlled as a separate heating zone. The semiconductor substrate 802 may be considered to be divided into N (1, 2, 3, 4, ... N) zones corresponding to the number of independently controllable heating zones in the heating assembly 850. This arrangement allows for rapid localized heating of the semiconductor substrate 802.
[0122] Control of the power supply to the independently controllable heating zones in the heating assembly 850 may correspond to the radial position of the discharge nozzle 832. Thus, the controller 854 may control the power supply to the heating element 852 of the associated heating zone based on the radial position of the discharge nozzle 832.
[0123] In some embodiments, the discharge nozzle 852 may be positioned over an area of the semiconductor substrate 802 to perform dry development of the metal-containing EUV resist. Additionally, the heating assembly 850 may provide localized heating of an area of the semiconductor substrate 802 to facilitate dry development of the metal-containing EUV resist. In some embodiments, the dry development of the metal-containing EUV resist in the wafer cleaning and heating station 800 may be performed under atmospheric conditions.
[0124] In some embodiments, the discharge nozzle 852 may be positioned over a bevel edge region of the semiconductor substrate 802 to perform bevel edge cleaning of the semiconductor substrate 802. Specifically, the bevel edge cleaning exposes the bevel edge of the semiconductor substrate 802 to an etching gas for metal-containing EUV resist removal. The metal-containing EUV resist can be removed using etching gas at various temperatures, with higher temperatures increasing the etch rate. In some embodiments, the heating assembly 850 may provide localized heating at the bevel edge of the semiconductor substrate 802 to facilitate removal of the metal-containing EUV resist. In some embodiments, the bevel edge cleaning of the metal-containing EUV resist in the wafer cleaning and heating station 800 may be performed under atmospheric conditions.
[0125] The apparatus of the present disclosure is configured to perform dry etching of EUV resist. Dry etching may be performed under atmospheric conditions or in a process chamber with or without a vacuum. In some embodiments, the process chamber is a thermal process chamber without the use of plasma. The apparatus may be configured to perform other processing steps such as deposition, bevel and backside cleaning, post-apply bake, EUV scan, post-exposure bake, photoresist work, descumming, smoothing, curing, and other steps. In some embodiments, the apparatus is configured to perform a full dry step. In some embodiments, the apparatus is configured to perform a full wet step. In some embodiments, the apparatus is configured to perform a combination of wet and dry steps.
[0126] 9 is a schematic diagram of an exemplary process station for performing dry etching, according to some embodiments. Multiple process stations 900 may be included within a common process tool environment. For example, FIG. 10 illustrates an embodiment of a multi-station processing tool 1000, such as a VECTOR® processing tool manufactured by Lam Research Corporation (Fremont, Calif.). In some embodiments, one or more hardware parameters in the process station 1000, including those described in more detail below, may be programmatically adjusted by one or more computer controllers 1050.
[0127] The process stations may be configured as modules within a cluster tool. Figure 9 illustrates a semiconductor processing cluster tool structure having deposition and patterning modules suitable for implementing the embodiments described herein. Such a cluster processing tool structure may include resist deposition, resist treatment, resist bevel edge clean, resist bake, resist exposure (EUV scanner), resist dry develop, and etch modules, as described above with reference to Figures 4 and 5 and further below with reference to Figure 10.
[0128] In some embodiments, some of the processing functions may be performed sequentially in the same module, for example dry develop and bake, or dry develop and bevel edge clean may be performed in the same module.
[0129] Returning to Figure 9, the process station 900 is in fluid communication with a reactant delivery system 901 for delivering process gases to a distribution showerhead 906. The reactant delivery system 901 optionally includes a mixing vessel 904 for blending and / or conditioning process gases for delivery to the showerhead 906. Introduction of process gases to the mixing vessel 904 may be controlled by one or more mixing vessel inlet valves 920. If plasma exposure is used, a plasma may also be delivered to the showerhead 906 or may be generated within the process station 900. As discussed above, in at least some embodiments, thermal exposure without the use of plasma is preferred.
[0130] 9 includes an optional vaporization point 903 for vaporizing a liquid reactant provided to the mixing vessel 904. In some embodiments, a Liquid Flow Controller (LFC) may be provided upstream of the vaporization point 903 for controlling the mass flow rate of the liquid that is vaporized and provided to the process station 900. For example, the LFC may include a thermal mass flow meter (MFM) located downstream of the LFC. A plunger valve of the LFC may be adjusted in response to a feedback control signal provided by a Proportional-Integral-Derivative (PID) controller in electrical communication with the MFM.
[0131] The showerhead 906 distributes process gases toward the substrate 912. In the embodiment shown in Figure 9, the substrate 912 is located below the showerhead 906 and rests on a pedestal 908. The showerhead 906 may have any suitable shape and may have any suitable number of ports in any suitable arrangement for distributing process gases to the substrate 912.
[0132] In some embodiments, the pedestal 908 may be raised or lowered to expose the substrate 912 to the space between the substrate 912 and the showerhead 906. It will be appreciated that in some embodiments, the height of the pedestal may be programmatically adjusted by a suitable computer controller 950.
[0133] In some embodiments, the pedestal 908 may be temperature controlled via heater 910. In some embodiments, the pedestal 908 may be heated to a temperature greater than 50° C. to 300° C. or greater, for example, between 50° C. and 230° C. (such as between about 100° C. and 200° C.) during non-plasma thermal exposure of the EUV resist to dry developing or dry cleaning chemistries.
[0134] Additionally, in some embodiments, pressure control of the process station 900 may optionally be performed using a butterfly valve 918. As shown in the embodiment of FIG. 9, the butterfly valve 918 throttles the vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, the process station 900 may be in an open air environment without a vacuum system. The process station 900 may perform photoresist processing steps such as dry develop, bake, and / or dry bevel edge clean.
[0135] In some embodiments, the position of the showerhead 906 may be adjusted relative to the pedestal 908 to vary the space between the substrate 912 and the showerhead 906. Further, it is recognized that the vertical position of the pedestal 908 and / or the showerhead 906 may be varied by any suitable mechanism within the scope of the present disclosure. In some embodiments, the pedestal 908 may include a rotation axis for rotating the orientation of the substrate 912. It is recognized that in some embodiments, one or more of these adjustments may be performed programmatically by one or more suitable computer controllers 950.
[0136] For example, where plasma may be used in a gentle plasma dry development embodiment and / or an etching step performed in the same chamber, the showerhead 906 and pedestal 908 are in electrical communication with a radio frequency (RF) power source 914 and matching network 916 for powering the plasma. In some embodiments, the plasma energy may be controlled by controlling one or more of the process station pressure, gas concentration, RF source power, RF source frequency, and plasma power pulse timing. For example, the RF power source 914 and matching network 916 may be operated at any suitable power to generate a plasma having a desired radical species composition. A suitable power is, for example, up to about 500 W.
[0137] In some implementations, instructions for the controller 950 may be provided by Input / Output Control (IOC) sequence instructions. As an example, instructions for setting conditions for a process phase may be included in a corresponding recipe phase in a process recipe. In some cases, recipe phases of a process may be arranged sequentially, in which case all instructions for a process phase are executed simultaneously with that process phase. In some implementations, instructions for setting one or more reactor parameters may be included in a recipe phase. For example, a recipe phase may include instructions for setting a flow rate of an etching gas, such as a halogen-containing compound, and a time delay instruction for that recipe phase. In some embodiments, the controller 950 may include any of the features described below with respect to the system controller 1050 of FIG. 10.
[0138] As mentioned above, one or more process stations may be included in a multi-station processing tool. FIG. 10 is a schematic diagram of an exemplary multi-station processing tool 1000 suitable for performing various photoresist processing steps described herein. FIG. 10 illustrates an embodiment of the multi-station processing tool 1000 with an input load lock 1002 and an output load lock 1004. Either or both of the input load lock 1002 and the output load lock 1004 may optionally include a remote plasma source. The robot 1006 is configured to move a wafer from a cassette loaded through a pod 1008 under atmospheric pressure through an atmospheric port 1010 to the input load lock 1002. The robot 1006 places the wafer on a pedestal 1012 in the input load lock 1002, the atmospheric port 1010 is closed, and the load lock is evacuated. If the input load lock 1002 includes a remote plasma source, the wafer may be subjected to a remote plasma treatment in the load lock to treat the substrate surface prior to introduction into the processing chamber 1014. Additionally, the substrate may be heated in the input load lock 1002, for example to remove moisture and adsorbed gases. The chamber transfer port 1016 to the processing chamber 1014 is then opened and another robot (not shown) moves the substrate into the reactor and places it on a pedestal in the illustrated first station of the reactor for processing. It will be appreciated that although the embodiment shown in FIG. 10 includes a load lock, in some embodiments the substrate may enter the process station directly.
[0139] The illustrated processing chamber 1014 includes four process stations. In the embodiment shown in FIG. 10, the process stations are numbered 1-4. Each station includes a heated pedestal (indicated at 1018 in station 1) and a gas line inlet. It is recognized that in some embodiments, each process station may have a different or multiple purpose. For example, in some embodiments, the process stations may be switchable between a dry development mode and an etch process mode. Additionally or alternatively, in some embodiments, the processing chamber 1014 may include one or more corresponding pairs of dry development and etch process stations. Although the illustrated processing chamber 1014 includes four stations, it is understood that a processing chamber according to the present disclosure may have any suitable number of stations. For example, in some embodiments, the processing chamber may have five or more stations, while in other embodiments, the processing chamber may have three or fewer stations.
[0140] FIG. 10 illustrates one embodiment of a substrate handling system 1090 for transporting substrates within the processing chamber 1014. In some embodiments, the substrate handling system 1090 may transport substrates between various process stations and / or between the process stations and load locks. It is recognized that any suitable substrate handling system may be employed. Non-limiting examples include a substrate carousel and a substrate handling robot. FIG. 10 also illustrates an embodiment of a system controller 1050 for controlling process conditions and hardware states of the process tool 1000. The system controller 1050 may include one or more memory devices 1056, one or more mass storage devices 1054, and one or more processors 1052. The processor 1052 may include a CPU or computer, analog and / or digital input / output connections, stepper motor control boards, etc.
[0141] In some embodiments, the system controller 1050 controls all operations of the process tool 1000. The system controller 1050 executes system control software 1058. The system control software 1058 is stored in the mass storage device 1054, loaded into the memory device 1056, and executed on the processor 1052. Alternatively, the control logic may be hard-coded into the controller 1050. For this purpose, application specific integrated circuits, programmable logic devices (e.g., field programmable gate arrays (FPGAs)), and the like may be used. In the following description, where "software" or "code" is used, either may be substituted with functionally equivalent hard-coded logic. The system control software 1058 may include instructions for controlling the timing, mixture of gases, gas flow rates, chamber and / or station pressure, chamber and / or station temperature, wafer temperature, target power levels, RF power levels, substrate pedestal, chuck and / or susceptor position, and other parameters of a particular process performed by the process tool 1000. The system control software 1058 may be configured in any suitable manner. For example, various process tool component subroutines or control objects may be written to control the operation of the process tool components used to perform processes with the various process tools. The system control software 1058 may be coded in any suitable computer readable programming language.
[0142] In some embodiments, the system control software 1058 may include input / output control (IOC) sequence instructions for controlling the various parameters described above. In some embodiments, other computer software and / or programs stored in the mass storage device 1054 and / or memory device 1056 associated with the system controller 1050 may be used. Examples of such programs or portions of programs include a substrate positioning program, a process gas control program, a pressure control program, a heater control program, and a plasma control program.
[0143] The substrate positioning program may include program code for process tool components used to load the substrate onto the pedestal 1018 as well as control the spacing between the substrate and other parts of the process tool 1000 .
[0144] The process gas control program may include code for controlling various gas compositions (e.g., halogen-containing compounds) and flow rates, and may optionally include code for flowing gases to one or more process stations to stabilize the pressure in the process stations prior to deposition. The pressure control program may include code for controlling the pressure in the process stations, for example, by adjusting throttle valves in the exhaust systems of the process stations, gas flows to the process stations, etc.
[0145] The heater control program may include code for controlling the current to a heating unit used to heat the substrate, or the heater control program may control the supply of a heat transfer gas (such as helium) to the substrate.
[0146] The plasma control program may include code for setting RF power levels applied to process electrodes in one or more process stations according to embodiments herein.
[0147] The pressure control program may include code for maintaining pressure within a reaction chamber according to embodiments herein.
[0148] In some embodiments, a user interface may be provided associated with the system controller 1050. The user interface may include a display screen, a graphical software representation of equipment and / or process conditions, and user input devices such as a pointing device, keyboard, touch screen, microphone, etc.
[0149] In some embodiments, the parameters adjusted by the system controller 1050 may relate to process conditions. Non-limiting examples include process gas composition and flow rates, temperature, pressure, plasma conditions (such as RF bias power levels), etc. These parameters may be provided to the user as a recipe. The recipe may be entered using a user interface.
[0150] Signals for monitoring the process may be provided from various process tool sensors via analog and / or digital input connections of the system controller 1050. Signals for controlling the process may be output on analog and digital output connections of the process tool 1000. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (such as manometers), thermocouples, etc. Data from these sensors may be used in conjunction with appropriately programmed feedback and control algorithms to maintain process conditions.
[0151] The system controller 1050 may provide program instructions for carrying out the deposition processes described above. The program instructions may control various process parameters such as DC power levels, RF bias power levels, pressure, temperature, etc. These instructions may control parameters for operating the deposition, bake, bevel edge clean, exposure, development, etching, and other photoresist processing steps according to various embodiments described herein.
[0152] The system controller 1050 typically includes one or more memory devices and one or more processors configured to execute instructions to cause the device to perform methods according to embodiments of the present disclosure. Machine-readable media containing instructions for controlling process steps according to embodiments of the present disclosure may be coupled to the system controller 1050.
[0153] In some implementations, the system controller 1050 is part of a system, which may be part of the examples described above. Such systems may include semiconductor processing equipment including one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (such as a wafer pedestal and gas flow systems). These systems may be integrated with electronics to control the operation of the system before, during, and after processing of a semiconductor wafer or substrate. The electronics may be referred to as a "controller" and may control various components or subparts of one or more systems. The system controller 1050 may be programmed to control any of the processes disclosed herein depending on the processing conditions and / or type of system. The processes may include supply of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow settings, fluid supply settings, position and motion settings, wafer loading and unloading from the tool, and wafer loading and unloading from other transport tools and / or load locks connected or associated with the particular system.
[0154] The system controller 1050 may be broadly defined as electronic equipment having various integrated circuits, logic, memory, and / or software to receive instructions, send instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips as firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions may be instructions communicated to the system controller 1050 as various individual settings (or program files), the instructions defining operational parameters for performing a particular process on or for a semiconductor wafer or for a system. In some embodiments, the operational parameters may be part of a recipe defined by a process engineer to accomplish one or more processing steps in the manufacture of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or wafer dies.
[0155] In some embodiments, the system controller 1050 is configured with instructions for processing a semiconductor substrate. The instructions include code for performing the steps of providing a metal-containing EUV resist on a semiconductor substrate in a process chamber and supplying an etching gas to the semiconductor substrate via an etching gas distributor or an etching gas supply nozzle to dry etch one or more portions of the metal-containing EUV resist from the semiconductor substrate under atmospheric conditions. In some embodiments, dry etching one or more portions of the metal-containing EUV resist under atmospheric conditions includes dry developing the metal-containing EUV resist by selectively removing unexposed portions of the metal-containing EUV resist relative to exposed portions of the metal-containing EUV resist. In some embodiments, dry etching one or more portions of the metal-containing EUV resist under atmospheric conditions includes dry cleaning the metal-containing EUV resist from a bevel edge of the semiconductor substrate.
[0156] In some implementations, the system controller 1050 may be part of or coupled to a computer, where the computer is integral to the system, coupled to the system, or otherwise networked to the system, or a combination thereof. For example, the system controller 1050 may reside on the "cloud" or may reside in all or part of a fab host computer system. This allows remote access of wafer processing. The computer may enable remote access to the system to monitor the progress of a manufacturing process, examine past manufacturing process history, or examine trends or performance indicators from multiple manufacturing processes, change parameters of a current process, set up a process process following a current process, or start a new process. In some examples, a process recipe can be provided to the system from a remote computer (e.g., a server) over a network, where the network may include a local network or the Internet. The remote computer may include a user interface that allows for input or programming of parameters and / or settings. These parameters and / or settings are then communicated from the remote computer to the system. In some examples, the system controller 1050 receives instructions as data. This data specifies parameters for each process step performed in one or more operations, with the understanding that these parameters may be specific to the type of process to be performed and the type of tool with which the system controller 1050 is configured to interface or control. Thus, as described above, the system controller 1050 may be distributed, such as by comprising one or more individual controllers, which are networked together and operate toward a common goal, such as the processes and controls described herein.One example of a distributed controller for such purposes includes one or more integrated circuits mounted in the chamber that communicate with one or more remotely located integrated circuits (e.g., at the platform level or as part of a remote computer) that cooperate to control the process in the chamber.
[0157] Non-limiting examples of systems include a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an atomic layer deposition (ALD) chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry develop chamber or module, and any other semiconductor processing system that may be associated with or used in the manufacturing and / or production of semiconductor wafers.
[0158] As described above, depending on one or more process steps being performed by the tool, the system controller 1050 may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, nearby tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport to and from wafer containers to tool locations and / or load ports within a semiconductor manufacturing factory.
[0159] Next, an Inductively Coupled Plasma (ICP) reactor is described. An ICP reactor may be suitable for some embodiments of the etch process suitable for implementing some embodiments. Although an ICP reactor is described herein, it should be understood that in some embodiments, a capacitively coupled plasma reactor may also be used.
[0160] 11 is a schematic cross-sectional view of an exemplary inductively coupled plasma apparatus for carrying out some embodiments and steps described herein. The apparatus may be used for various photoresist processing steps such as dry development and / or bevel edge cleaning. An example of the apparatus is a Kiyo® reactor manufactured by Lam Research Corp. (Fremont, Calif.). Other embodiments may be carried out using other tools or tool types capable of performing dry development and / or bevel edge cleaning.
[0161] The inductively coupled plasma device 1100 includes an overall process chamber 1124 defined by a chamber wall 1101 and a window 1111. The chamber wall 1101 may be made of stainless steel or aluminum. The window 1111 may be made of quartz or other dielectric material. An optional internal plasma grid 1150 divides the overall process chamber into an upper sub-chamber 1102 and a lower sub-chamber 1103. In most embodiments, the plasma grid 1150 may be removed, thereby utilizing the chamber space of the sub-chambers 1102, 1103. A chuck 1117 is disposed near the interior bottom surface of the lower sub-chamber 1103. The chuck 1117 is configured to receive and hold a semiconductor wafer 1119 on which etching and deposition processes are performed. The chuck 1117 may be an electrostatic chuck that supports the wafer 1119 when placed thereon. In some of the present embodiments, an edge ring (not shown) surrounds the chuck 1117. The top surface of the edge ring is approximately coplanar with the top surface of the wafer 1119 when placed on the chuck 1117. The chuck 1117 further includes an electrostatic electrode for chucking and dechucking the wafer 1119. For this purpose, a filter and DC clamp power supply (not shown) may be provided. Other control systems may also be provided for lifting the wafer 1119 from the chuck 1117. The chuck 1117 can be charged by an RF power supply 1123. The RF power supply 1123 is connected to a matching circuit 1121 via a connection 1127. The matching circuit 1121 is connected to the chuck 1117 via a connection 1125. In this manner, the RF power supply 1123 is connected to the chuck 1117. In various embodiments, the bias power of the electrostatic chuck may be set to about 50V or may be set to a different bias power depending on the process being performed according to an embodiment of the present disclosure. For example, the bias power may be about 20Vb to about 100V, or about 30V to about 150V.
[0162] The element for plasma generation includes a coil 1133 disposed above the window 1111. In some embodiments, a coil is not used in the embodiments of the present disclosure. The coil 1133 is made of a conductive material and includes at least one complete turn. The example coil 1133 shown in FIG. 11 includes three turns. A cross section of the coil 1133 is symbolized, with the "X" coils rotating into the page and the "●" coils rotating toward the page. The element for plasma generation further includes an RF power source 1141 configured to provide RF power to the coil 1133. The RF power source 1141 is typically connected to a matching circuit 1139 via a connection 1145. The matching circuit 1139 is connected to the coil 1133 via a connection 1143. In this manner, the RF power source 1141 is connected to the coil 1133. An optional Faraday shield 1149a is disposed between the coil 1133 and the window 1111. The Faraday shield 1149a may be maintained in a spaced relationship with respect to the coil 1133. In some embodiments, the Faraday shield 1149a is disposed directly above the window 1111. In some embodiments, the Faraday shield 1149b is disposed between the window 1111 and the chuck 1117. In some embodiments, the Faraday shield 1149b is not maintained in a spaced relationship with respect to the coil 1133. For example, the Faraday shield 1149b may be disposed directly below the window 1111 with no gap therebetween. The coil 1133, the Faraday shield 1149a, and the window 1111 are configured to be approximately parallel to one another. The Faraday shield 1149a may prevent metals or other species from depositing on the window 1111 of the process chamber 1124.
[0163] Process gases may flow into the process chamber through one or more main gas inlets 1160 located in the upper subchamber 1102 and / or through one or more side gas inlets 1170. Similarly, similar gas inlets, not shown, may be used to supply process gases to the capacitively coupled plasma processing chamber. A vacuum pump (e.g., a one or two stage mechanical dry pump and / or turbomolecular pump 1140) may be used to draw process gases from the process chamber 1124 and maintain pressure therein. For example, the vacuum pump may be used to evacuate the lower subchamber 1103 during an ALD purge step. The vacuum pump may be fluidly connected to the process chamber 1124 using a valve-controlled conduit to selectively control application of a vacuum environment by the vacuum pump. This may be accomplished by a closed-loop controlled flow control device, such as a throttle valve (not shown) or a pendulum valve (not shown), during plasma process processing. Similarly, a vacuum pump and a valve-controlled fluid connection may be used for the capacitively coupled plasma processing chamber.
[0164] During operation of the apparatus 1100, one or more process gases may be provided through the gas inlets 1160 and / or 1170. In certain embodiments, the process gas may be provided only through the main gas inlet 1160 or only through the side gas inlet 1170. In some cases, the illustrated gas inlets may be replaced with more complex gas inlets (e.g., one or more showerheads). The Faraday shield 1149a and / or optional grid 1150 may include internal channels and holes that allow the delivery of process gases to the process chamber 1124. Either or both of the Faraday shield 1149a and optional grid 1150 may function as a showerhead to deliver process gases. In some embodiments, a liquid vaporization supply system may be located upstream of the process chamber 1124. In this case, once the liquid reactant or precursor is vaporized, the vaporized reactant or precursor is introduced into the process chamber 1124 through the gas inlets 1160 and / or 1170.
[0165] Radio frequency power is supplied to the coil 1133 from an RF power supply 1141, causing an RF current to flow through the coil 1133. The RF current flowing through the coil 1133 generates an electromagnetic field around the coil 1133. This electromagnetic field generates an induced current in the upper subchamber 1102. Physical and chemical interactions of the various ions and radicals generated with the wafer 1119 etch features in the wafer 1119 and selectively deposit layers on the wafer 1119.
[0166] When a plasma grid 1150 is used to provide both the upper subchamber 1102 and the lower subchamber 1103, induced currents act on the gas in the upper subchamber 1102 to generate an electron-ion plasma in the upper subchamber 1102. The optional internal plasma grid 650 limits the number of hot electrons in the lower subchamber 1103. In some embodiments, the apparatus 1100 is designed and operated such that the plasma in the lower subchamber 1103 is an ion-ion plasma.
[0167] Both the upper electron-ion plasma and the lower ion-ion plasma may contain positive and negative ions, but the ion-ion plasma has a greater proportion of negative ions than positive ions. Volatile etch and / or deposition by-products may be removed from the lower sub-chamber 1103 via port 1122. The chuck 1117 disclosed herein may operate at elevated temperatures ranging from about 10° C. to about 250° C. The temperature depends on the process step and the specific recipe.
[0168] The tool 1100 may be coupled to equipment (not shown) when installed in a clean room or manufacturing facility. The equipment includes plumbing equipment to provide process gases, vacuum, temperature control, and environmental particle control. These equipment are coupled to the tool 1100 when the tool 1100 is installed in the target manufacturing facility. Additionally, the tool 1100 may be coupled to a transfer chamber that robotically transfers semiconductor wafers into and out of the tool 1100 using conventional automation.
[0169] In some embodiments, a system controller 1130 (which may include one or more physical or logical controllers) controls some or all of the operation of the process chamber 1124. The system controller 1130 may include one or more memory devices and one or more processors. In some embodiments, the apparatus 1100 includes a switching system for controlling flow rates and times when performing embodiments of the present disclosure. In some embodiments, the apparatus 1100 may have a switching time of up to about 600 ms, or up to about 750 ms. The switching time may depend on the flow chemistry, the selected recipe, the reactor configuration, and other factors.
[0170] In some implementations, the system controller 1130 is part of a system, which may be part of the examples described above. Such systems may include semiconductor processing equipment including one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (such as a wafer pedestal and gas flow systems). These systems may be integrated with electronics to control the operation of the system before, during, and after processing of a semiconductor wafer or substrate. Electronics may be integrated into the system controller 1130 to control various components or subparts of one or more systems. The system controller 1130 may be programmed to control any of the processes disclosed herein depending on the processing parameters and / or type of system. These processes include supply of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow settings, fluid supply settings, position and motion settings, wafer loading and unloading from the tool, and wafer loading and unloading from other transfer tools and / or load locks connected or associated with the particular system.
[0171] Broadly, the system controller 1130 may be defined as an electronic device having various integrated circuits, logic, memory, and / or software to receive instructions, send instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits may include chips as firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions may be instructions communicated to the controller as various individual settings (or program files) that define the operating parameters for performing a particular process on or for a semiconductor wafer or for a system. In some embodiments, the operating parameters may be part of a recipe defined by a process engineer to accomplish one or more processing steps in the manufacture and removal of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or wafer dies.
[0172] In some implementations, the system controller 1130 may be part of or coupled to a computer, where the computer is integral to the system, coupled to the system, or otherwise networked to the system, or a combination thereof. For example, the controller may reside on the "cloud" or in all or part of a fab host computer system. This allows remote access of wafer processing. The computer may enable remote access to the system to monitor the progress of a manufacturing process, examine past manufacturing process history, or examine trends or performance indicators from multiple manufacturing processes, change parameters of a current process, set up a process step following a current process, or start a new process. In some examples, a process recipe may be provided to the system from a remote computer (e.g., a server) over a network, where the network may include a local network or the Internet. The remote computer may include a user interface that allows for entry or programming of parameters and / or settings. These parameters and / or settings are then communicated from the remote computer to the system. In some examples, the system controller 630 receives instructions as data, where the data specifies parameters for each process step to be performed in one or more operations. It should be understood that these parameters may be specific to the type of process being performed and the type of tool the controller is configured to cooperate with or control. Thus, as described above, the system controller 630 may be distributed, such as by having one or more individual controllers that are networked together and operate toward a common purpose, such as the process and control described herein. One example of a distributed controller for such purposes includes one or more integrated circuits mounted in the chamber that communicate with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer).These integrated circuits work together to control the process in the chamber.
[0173] Non-limiting examples of systems include a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etch chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an ALD chamber or module, an ALE chamber or module, an ion implantation chamber or module, a track chamber or module, an EUV lithography chamber (scanner) or module, a dry develop chamber or module, and any other semiconductor processing system related to or usable in the manufacturing and / or production of semiconductor wafers.
[0174] As described above, depending on one or more process steps being performed by the tool, the controller may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, nearby tools, tools located throughout the factory, a main computer, another controller, or tools used in material transport to and from wafer containers to tool locations and / or load ports within a semiconductor manufacturing factory.
[0175] EUVL patterning may be performed using any suitable tool (often referred to as a scanner), such as, for example, a TWINSCAN NXE:3300B® platform manufactured by ASML (Veldhoven, The Netherlands). The EUVL patterning tool may be a stand-alone apparatus into which substrates are loaded and unloaded for deposition and etching as described herein. Alternatively, as described below, the EUVL patterning tool may be a module on a larger multi-component tool. FIG. 12 illustrates a semiconductor process cluster tool architecture having a deposition module and a patterning module in conjunction with a transfer module suitable for carrying out the processes described herein. The processes may be carried out without the use of a vacuum-integrated apparatus, although such an apparatus may be advantageous in some implementations.
[0176] 12 illustrates a semiconductor process cluster tool architecture having deposition and patterning modules in conjunction with a transfer module suitable for carrying out the processes described herein. The arrangement of transfer modules for "transporting" wafers between multiple storage facilities and processing modules may be referred to as a "cluster tool architecture" system. The deposition and patterning modules are vacuum integrated according to the requirements of the particular process. Other modules, such as for etching, may also be included in the cluster.
[0177] A Vacuum Transport Module (VTM) 1238 interfaces with four processing modules 1220a-d. The processing modules 1220a-d may be individually optimized to perform various manufacturing processes. By way of example, the processing modules 1220a-d may be implemented to perform deposition, evaporation, ELD, dry development, etching, stripping, and / or other semiconductor processes. For example, module 1220a may be an ALD reactor operable to perform non-plasma thermal atomic layer deposition as described herein, such as a Vector tool manufactured by Lam Research Corporation (Fremont, Calif.), and module 1220b may be a PECVD tool, such as a Lam Vector® tool. It should be understood that the figures are not necessarily to scale.
[0178] Airlocks 1242 and / or 1246 (also known as load locks or transfer modules) interface with the VTM 1238 and the patterning module 1240. For example, as mentioned above, a suitable patterning module may be a TWINSCAN NXE:3300B® platform manufactured by ASML (Veldhoven, The Netherlands). This tool architecture allows workpieces such as semiconductor substrates or wafers to be transferred under vacuum so that they do not react prior to exposure. Considering the strong optical absorption of incident photons by ambient gases (H2O, O2, etc.), EUVL also requires significantly lower pressures, facilitating the integration of the deposition module with the lithography tool.
[0179] As mentioned above, this integrated structure is only one possible embodiment of a tool for carrying out the processes described herein. The processes may be carried out using a conventional stand-alone EUVL scanner and deposition reactor (such as a Lam Vector tool). The deposition reactor here may be stand-alone or may be integrated as a module into a cluster structure with other tools such as etching and stripping (e.g., a Lam Kiyo or Gamma tool) (e.g., the structure described with reference to FIG. 12, except that there is no integrated patterning module).
[0180] Airlock 1242 may be an "out" load lock. "Out" refers to removing substrates from VTM 1238 to feed deposition module 1220a to patterning module 1240. And airlock 1246 may be an "in" load lock. "In" refers to returning substrates from patterning module 1240 to VTM 1238. In load lock 1246 may also provide an interface to the outside of the tool for accessing and unloading substrates. Each process module has a facet that interfaces the module with VTM 1238. For example, deposition process module 1220a has facet 1236. Inside each facet, a sensor (e.g., sensors 1-18 as shown) detects the passage of wafer 1226 as it moves between the respective stations. Patterning module 1240 and airlocks 1242, 1246 may similarly include additional facets and sensors (not shown).
[0181] The main VTM robot 1222 transfers the wafers 1226 between modules including airlocks 1242, 1246. In one embodiment, the robot 1222 includes one arm, and in another embodiment, the robot 1222 includes two arms, each arm including an end effector 1224 that picks up a wafer such as wafer 1226 for transfer. A front-end robot 1244 is used to transfer the wafers 1226 from the exit airlock 1242 to the patterning module 1240 and from the patterning module 1240 to the entry airlock 1246. The front-end robot 1244 may also transfer the wafers 1226 between the entry loadlock and the exterior of the tool for access to and removal of the substrate. The entry airlock module 1246 has the ability to match the environment between atmospheric pressure and vacuum, allowing the wafers 1226 to be moved between the two pressure environments without damage.
[0182] It should be noted that EUVL tools typically operate at a higher vacuum than deposition tools. In this case, it may be desirable to increase the vacuum environment of the substrate during transfer from the deposition tool to the EUVL tool so that the substrate can be degassed before entering the patterning tool. The exit airlock 1242 may achieve this function by holding the transferred wafer at a low pressure below the pressure in the patterning module 1240 for a period of time to evacuate any off-gassing. This ensures that the optics of the patterning tool 1240 are not contaminated by off-gassing from the substrate. A suitable pressure for the exit airlock to degas is 1E-8 Torr or less.
[0183] 13 and 14 show alternative processing tool architecture configurations. Such architectures may be implemented, for example, at least in part, in EOS or Sense.i products from Lam Research Corporation (Fremont, Calif.) that may be used in some embodiments. Resist processing tracks such as those shown in FIGS. 13 and 14 may be used to perform wet development of dry deposited EUV photoresist. Various embodiments described herein may be performed using cluster architectures such as those shown in FIGS. 13 and 14.
[0184] [Conclusion] A process and apparatus are disclosed for dry etching metal and / or metal oxide photoresists to form patterning masks, for example in EUV patterning.
[0185] It is understood that the examples and embodiments described herein are merely for illustrative purposes, and various modifications or variations may be suggested to those skilled in the art in light of them. For the sake of clarity, various details have been omitted, but various design modifications may be made. Therefore, the above examples are merely illustrative and should not be considered as limiting the present disclosure. The present disclosure is not limited to the details described herein, and may be modified within the scope of the present disclosure. The present disclosure may be realized, for example, in the following forms. [Form 1] 1. An apparatus comprising: a process chamber exposed to atmospheric conditions; a substrate support for holding a semiconductor substrate within the process chamber; a heating assembly facing the semiconductor substrate on the substrate support pedestal, the heating assembly including a plurality of heating elements; an etching gas supply nozzle disposed above the substrate support table, the etching gas supply nozzle being movable so that a supply position of the etching gas is located above the semiconductor substrate; 13. An apparatus comprising: [Form 2] 2. The apparatus according to claim 1, the semiconductor substrate comprises a metal-containing EUV resist; one or more portions of the metal-containing EUV resist are removable by the etching gas; Device. [Form 3] 2. The apparatus according to claim 1, The process chamber exposed to atmospheric conditions is exposed to an atmospheric pressure of about 50 Torr to about 765 Torr. Device. [Form 4] 2. The apparatus according to claim 1, the process chamber exposed to atmospheric conditions is exposed to a controlled atmosphere; The exposure to a controlled atmosphere includes exposure to a chamber pressure of greater than about 760 Torr and / or exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof. Device. [Form 5] 2. The apparatus according to claim 1, the plurality of heating elements includes a plurality of LEDs; The LEDs are arranged in a number of independently controllable heating zones. Device. [Form 6] 2. The apparatus according to claim 1, the etching gas supply nozzle is coupled to a movable swing arm configured to position the etching gas supply nozzle from a center to an edge of the semiconductor substrate; Device. [Form 7] 2. The apparatus according to claim 1, the substrate support is configured to rotate the semiconductor substrate; Device. [Form 8] 2. The apparatus according to claim 1, a controller configured with instructions for processing the semiconductor substrate; The instruction: providing a metal-containing EUV resist on the semiconductor substrate in the process chamber; supplying the etching gas to the semiconductor substrate through the etching gas supply nozzle to dry etch one or more portions of the metal-containing EUV resist from the semiconductor substrate under atmospheric conditions; Including the code to Device. [Form 9] The apparatus according to claim 8, dry etching the one or more portions of the metal-containing EUV resist under atmospheric conditions comprises dry developing the metal-containing EUV resist by selectively removing unexposed portions of the metal-containing EUV resist relative to exposed portions of the metal-containing EUV resist. Device. [Form 10] The apparatus according to claim 8, dry etching the one or more portions of the metal-containing EUV resist under atmospheric conditions includes dry cleaning the metal-containing EUV resist from a bevel edge of the semiconductor substrate. Device. [Form 11] The device according to any one of aspects 1 to 10, and further comprising an exhaust fan configured to remove etch by-products and other residual gases within the process chamber. Device. [Form 12] The device according to any one of aspects 1 to 10, a gas source coupled to the process chamber for supplying an inert gas and / or a diluent gas to the process chamber; Device. [Form 13] The device according to any one of aspects 1 to 10, The process chamber is a plasma-free thermal process chamber. Device. [Form 14] 1. An apparatus comprising: a process chamber exposed to atmospheric conditions; a bake plate for supporting a semiconductor substrate, the bake plate including a plurality of heating zones, each of the plurality of heating zones including one or more heating elements; an etching gas distributor disposed above the bake plate and configured to supply an etching gas to the semiconductor substrate; 13. An apparatus comprising: [Form 15] 15. The apparatus of claim 14, the semiconductor substrate comprises a metal-containing EUV resist; one or more portions of the metal-containing EUV resist are removable by the etching gas; Device. [Form 16] 15. The apparatus of claim 14, The process chamber exposed to atmospheric conditions is exposed to an atmospheric pressure of about 50 Torr to about 765 Torr. Device. [Form 17] 15. The apparatus of claim 14, the process chamber exposed to atmospheric conditions is exposed to a controlled atmosphere; The exposure to a controlled atmosphere includes exposure to a chamber pressure of greater than about 760 Torr and / or exposure to nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof. Device. [Form 18] 15. The apparatus of claim 14, the bake plate includes an upper surface and a plurality of minimum contact area (MCA) supports for supporting the semiconductor substrate above the upper surface of the bake plate. Device. [Form 19] The device according to any one of aspects 14 to 18, the etching gas distributor includes a showerhead having a faceplate facing the semiconductor substrate; the face plate includes a plurality of through holes for supplying the etching gas to the semiconductor substrate; Device. [Form 20] The device according to any one of aspects 14 to 18, The process chamber is a plasma-free thermal process chamber. Device. [Form 21] The device according to any one of aspects 14 to 18, and a controller configured with instructions for processing the semiconductor substrate, the instructions comprising: providing a metal-containing EUV resist on the semiconductor substrate in the process chamber; supplying the etching gas to the semiconductor substrate through the etching gas distributor to dry etch one or more portions of the metal-containing EUV resist from the semiconductor substrate under atmospheric conditions; Including the code to do Device. [Form 22] 1. An apparatus comprising: a furnace reactor having a substrate support pedestal for holding a plurality of semiconductor substrates; a plurality of heating elements for heating the plurality of semiconductor substrates to an elevated temperature; one or more etching gas inlets for supplying an etching gas to the furnace reactor, the one or more etching gas inlets configured to supply an etching gas to the plurality of semiconductor substrates; 13. An apparatus comprising: [Form 23] 23. The apparatus of claim 22, The furnace reactor is exposed to atmospheric conditions. Device. [Form 24] 24. The apparatus of claim 23, Atmospheric conditions include exposure to a controlled atmosphere; the one or more etching gas inlets are further configured to supply nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof to provide the controlled atmosphere. Device. [Form 25] 23. The apparatus of claim 22, one or more gas outlets for removing etch by-products and other residual gases from said furnace reactor; a motor for rotating the substrate support; The apparatus further comprising: [Form 26] The device according to any one of aspects 22 to 25, the furnace reactor chamber walls comprise quartz, a ceramic material, or a low temperature polymer material; Device. [Form 27] The device according to any one of aspects 22 to 25, each of the plurality of semiconductor substrates includes a metal-containing EUV resist; one or more portions of the metal-containing EUV resist are removable by the etching gas; Device. [Form 28] 1. A track lithography system comprising: a cassette mount including one or more pods for receiving and returning semiconductor substrates; A processing section including a plurality of processing stations for performing photoresist processing of the semiconductor substrate, the plurality of processing stations including: a deposition chamber for depositing a metal-containing EUV resist on the semiconductor substrate; a thermal process chamber; a processing section including a substrate cleaning chamber, at least one of the plurality of processing stations being exposed to atmospheric conditions and configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor substrate; an exposure section including a scanner for exposing the semiconductor substrate to EUV radiation; an interface unit for transporting the semiconductor substrate between the processing unit and the exposure unit; A track lithography system comprising: [Form 29] 29. The track lithography system of claim 28, The plurality of processing stations include: further comprising a hexamethyldisilazane (HMDS) processing chamber for processing a surface of the semiconductor substrate; the HMDS processing chamber is configured to dry remove one or more portions of the metal-containing EUV resist under atmospheric conditions; Track lithography system. [Form 30] 29. The track lithography system of claim 28, the at least one of the plurality of processing stations includes a substrate support for holding the semiconductor substrate and a gas distributor for supplying an etching gas to the semiconductor substrate; one or more portions of the metal-containing EUV resist are removable by the etching gas; Track lithography system.
Claims
1. 1. A track lithography system comprising: a cassette mount including one or more pods for receiving and returning semiconductor substrates; A processing section including a plurality of processing stations for performing photoresist processing of the semiconductor substrate, the plurality of processing stations including: a deposition chamber for depositing a metal-containing EUV resist on the semiconductor substrate; a processing section including a dry development chamber, wherein either or both of the deposition chamber and the dry development chamber are exposed to atmospheric conditions, and the dry development chamber is configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor substrate by exposure to a dry development chemistry; an interface for transporting the semiconductor substrate between the processing section and a scanner, the scanner being configured to expose the semiconductor substrate to EUV radiation; A track lithography system comprising:
2. 2. The track lithography system of claim 1, a chamber wall of the dry development chamber comprising a polymer material; Track lithography system.
3. 2. The track lithography system of claim 1, the dry development chamber includes an etching gas supply nozzle disposed above a substrate support, the etching gas supply nozzle being movable so that a supply position of the etching gas is located above the semiconductor substrate; Track lithography system.
4. 2. The track lithography system of claim 1, the dry development chamber is exposed to atmospheric pressure between 50 Torr and 765 Torr; Track lithography system.
5. 2. The track lithography system of claim 1, the dry development chamber is configured to expose the semiconductor substrate to a post-apply bake (PAB) process or a post-exposure bake (PEB) process; Track lithography system.
6. 6. A track lithography system according to claim 5, comprising: The PAB or PEB process exposes the semiconductor substrate to oxygen. Track lithography system.
7. 2. The track lithography system of claim 1, the plurality of processing stations further comprising a bake chamber configured to expose the semiconductor substrate to a PAB or PEB process; Track lithography system.
8. 2. The track lithography system of claim 1, the plurality of processing stations further comprising a post-development treatment chamber configured to treat the metal-containing EUV resist on the semiconductor substrate after dry development; Track lithography system.
9. 2. The track lithography system of claim 1, the plurality of processing stations further including a bevel and backside cleaning chamber configured to remove one or more portions of the metal-containing EUV resist from the semiconductor substrate by exposure to a cleaning chemistry; Track lithography system.
10. 10. The track lithography system of claim 9, the bevel and backside cleaning chamber is configured to perform edge bead removal by directing the cleaning chemistry from above and below a bevel edge while rotating the semiconductor substrate. Track lithography system.
11. 10. The track lithography system of claim 9, The cleaning chemical is methane (CH 4 ), Track lithography system.
12. 2. The track lithography system of claim 1, the dry development chamber is configured to heat the semiconductor substrate to a temperature of 50° C. or greater during dry development; Track lithography system.
13. 2. The track lithography system of claim 1, the dry development chemistry comprises a halogen-containing gas; Track lithography system.
14. 2. The track lithography system of claim 1, the deposition chamber for depositing the metal-containing EUV resist is a wet deposition chamber configured to deposit the metal-containing EUV resist by spin coating; Track lithography system.
15. 15. The track lithography system of claim 14, the wet deposition chamber is configured to perform edge bead removal by directing solvent flows from above and below a bevel edge while rotating the semiconductor substrate; Track lithography system.
16. 2. The track lithography system of claim 1, the dry development chamber is configured to expose the semiconductor substrate to a plasma during dry development. Track lithography system.
17. 1. A track lithography system comprising: a cassette mount including one or more pods for receiving and returning semiconductor substrates; A processing section including a plurality of processing stations for performing photoresist processing of the semiconductor substrate, the plurality of processing stations including: a deposition chamber for depositing a metal-containing EUV resist on the semiconductor substrate; a processing section including: a dry development chamber configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor substrate by exposure to an etching gas, the chamber walls of the dry development chamber including a polymer material; an interface for transporting the semiconductor substrate between the processing section and a scanner, the scanner being configured to expose the semiconductor substrate to EUV radiation; Including, the dry development chamber is exposed to atmospheric pressure between 50 Torr and 765 Torr; Track lithography system.
18. A track lithography system comprising: a cassette mount including one or more pods for receiving and returning semiconductor substrates; A processing section including a plurality of processing stations for performing photoresist processing of the semiconductor substrate, the plurality of processing stations including: a deposition chamber for depositing a metal-containing EUV resist on the semiconductor substrate; a processing section including: a dry development chamber configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor substrate by exposure to an etching gas, the chamber walls of the dry development chamber including a polymer material; an interface for transporting the semiconductor substrate between the processing section and a scanner, the scanner being configured to expose the semiconductor substrate to EUV radiation; Including, The dry development chamber is exposed to a controlled atmosphere of greater than 760 Torr. Track lithography system.
19. 19. A track lithography system according to claim 17 or claim 18, comprising: the dry development chamber includes a bake plate for supporting the semiconductor substrate and heating the semiconductor substrate to an elevated temperature; the dry development chamber further comprising an etching gas distributor disposed above the bake plate and configured to deliver the etching gas to the semiconductor substrate. Track lithography system.
20. 19. A track lithography system according to claim 17 or claim 18, comprising: The processing section is configured to adjust a vacuum environment of the semiconductor substrate between each of the plurality of processing stations. Track lithography system.
21. 1. A track lithography system comprising: a cassette mount including one or more pods for receiving and returning semiconductor substrates; A processing section including a plurality of processing stations for performing photoresist processing of the semiconductor substrate, the plurality of processing stations including: a wet deposition chamber for wet depositing a metal-containing EUV resist on the semiconductor substrate; a dry development chamber configured to dry remove one or more portions of the metal-containing EUV resist from the semiconductor substrate by exposure to a dry development chemistry; a processing section including an auxiliary processing chamber configured to perform one or more of PAB processing, PEB processing, post-develop processing, photoresist rework, hexamethyldisilazane (HMDS) processing, and bevel and backside cleaning of the semiconductor substrate, wherein either or both of the dry development chamber and the auxiliary processing chamber are exposed to atmospheric conditions; an interface for transporting the semiconductor substrate between the processing section and a scanner, the scanner being configured to expose the semiconductor substrate to EUV radiation; A track lithography system comprising:
22. 22. The track lithography system of claim 21, at least one of the plurality of processing stations includes a substrate support for holding the semiconductor substrate and a gas distributor for supplying an etching gas to the semiconductor substrate, the one or more portions of the metal-containing EUV resist being removable by the etching gas; Track lithography system.
23. 23. The track lithography system of claim 22, the gas distributor is further configured to supply nitrogen, water vapor, carbon dioxide, argon, helium, or a combination thereof to the at least one of the plurality of processing stations to provide a controlled atmosphere. Track lithography system.
24. 22. The track lithography system of claim 21, The processing section is configured to adjust a vacuum environment of the semiconductor substrate between each of the plurality of processing stations. Track lithography system.
25. 22. The track lithography system of claim 21, Either or both of the dry development chamber and the auxiliary processing chamber are exposed to atmospheric pressure between 50 Torr and 765 Torr. Track lithography system.
26. 22. The track lithography system of claim 21, Either or both of the dry development chamber and the auxiliary processing chamber are exposed to a controlled atmosphere. Track lithography system.
27. 22. The track lithography system of claim 21, either or both of the dry development chamber and the auxiliary processing chamber have chamber walls comprising a polymeric material; Track lithography system.
28. An apparatus comprising: a process chamber for dry development, the process chamber being exposed to atmospheric conditions and the chamber walls of the process chamber comprising a polymeric material; a substrate support for holding a semiconductor substrate in the process chamber, the semiconductor substrate comprising a metal-containing EUV resist; a heating assembly facing the semiconductor substrate on the substrate support pedestal, the heating assembly including a plurality of light emitting diodes (LEDs) and a plurality of heating zones, each of the plurality of heating zones being independently controllable; an etching gas supply nozzle disposed above the substrate support table, the etching gas supply nozzle being movable so that a supply position of the etching gas is located above the semiconductor substrate; 13. An apparatus comprising:
29. 29. The apparatus of claim 28, a controller configured with instructions for processing the semiconductor substrate, the instructions comprising: providing the metal-containing EUV resist on the semiconductor substrate in the process chamber; and supplying the etching gas through the etching gas supply nozzle to the semiconductor substrate to dry etch one or more portions of the metal-containing EUV resist from the semiconductor substrate. Device.
30. 1. An apparatus for performing dry development, comprising: a batch type vertical furnace reactor having a substrate support for holding a plurality of semiconductor substrates; a plurality of heating elements for heating the plurality of semiconductor substrates to an elevated temperature; one or more etching gas inlets for supplying an etching gas to the furnace reactor, the one or more etching gas inlets configured to supply an etching gas to the plurality of semiconductor substrates; Including, The apparatus, wherein the furnace reactor is exposed to atmospheric conditions.
31. 31. The apparatus of claim 30, The apparatus, wherein the furnace reactor chamber wall comprises a polymeric material.
Citation Information
Patent Citations
Far ultraviolet ray emitting dry developing method
JP1986234035A
Ashing apparatus
JP2002118096A
Film stripper
JP2005260015A
Pattern forming method and device production method
JP2010067979A
Interface device
JP2010123732A