Method for producing barium titanate based dielectric particles
By reacting barium and titanium halides with oxalic acid in an aqueous solution and introducing water vapor during calcination, the method addresses halogen impurity issues and enhances crystallinity, producing fine barium titanate particles for electronic components.
Patent Information
- Application Number
- JP2022004316
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-01-14
AI Technical Summary
Conventional methods for synthesizing barium titanate powder, such as the oxalate method, incorporate halogen impurities which can deteriorate electrical characteristics and promote corrosion, and high-temperature firing leads to coarse particles and broad particle size distribution.
A method involving the reaction of barium halide and titanium halide with oxalic acid in an aqueous solution, followed by calcination in a furnace with the introduction of water vapor during the calcination step to remove halogen impurities and enhance crystallinity.
Produces fine barium titanate particles with reduced halogen impurities and high crystallinity, suitable for use in electronic components like multilayer ceramic capacitors and piezoelectric elements.
Smart Images

Figure 0007563396000004 
Figure 0007563396000001 
Figure 0007563396000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing barium titanate-based dielectric particles. [Background technology]
[0002] Barium titanate (BaTiO3) is a type of perovskite-type complex oxide, and belongs to the tetragonal crystal system at room temperature. Barium titanate has a tetragonal crystal structure, and the barium ions (Ba 2+ ) and titanium ions (Ti 4+ ) is displaced in the c-axis direction, causing dielectric polarization, resulting in a high dielectric constant. Therefore, barium titanate powder is useful as a dielectric material for capacitors, especially multilayer ceramic capacitors. Barium titanate also has excellent piezoelectric properties, and when appropriate acceptor and donor components are added, it exhibits a unique temperature dependence of electrical resistance. For this reason, it is used not only in capacitors, but also in piezoelectric elements and PTC thermistors.
[0003] However, there is a demand for multilayer ceramic capacitors to be smaller and have larger capacitance. In order to meet this demand, it is effective to reduce the thickness of the dielectric layers constituting the multilayer ceramic capacitor and to increase the dielectric constant of the dielectric layers. Therefore, the barium titanate powder used as the raw material is required to be fine and have excellent crystallinity. In addition, the barium titanate powder is required to have few impurities, i.e., to have high purity.
[0004] Conventionally, methods such as the solid-state reaction method, the oxalate method, the hydrothermal synthesis method, and the alkoxide method have been used to synthesize barium titanate powder. The solid-state reaction method involves mixing and calcining (firing) a barium compound such as barium carbonate (BaCO3) with a titanium compound such as titanium oxide (TiO2), and has the advantage of being inexpensive to manufacture. However, high-temperature firing is necessary to obtain high crystallinity, and high-temperature firing can cause the particles to become coarse. It is possible to crush the powder after firing, but this can cause the particle size distribution to become broad. In addition, the solid-state reaction method also has the problem of a large amount of impurities derived from the manufacturing process.
[0005] Although the hydrothermal synthesis method and the alkoxide method have the advantage of being able to synthesize fine, high-purity barium titanate, they have the problem of high raw material and production costs. In particular, the raw materials used in the alkoxide method are very expensive, which makes productivity difficult.
[0006] In contrast, oxalates have the advantage that the raw materials are inexpensive, a relatively fine powder can be obtained, and the composition is stable. In the oxalate method, for example, barium chloride (BaCl2·2H2O) and titanium chloride (TiCl4) are reacted with oxalic acid (H2C2O4·2H2O) to obtain barium titanyl oxalate (BaTiO(C2O4)2·4H2O), which is then fired and pyrolyzed to synthesize barium titanate (BaTiO3). The raw materials barium chloride and titanium chloride are inexpensive. In addition, the pyrolysis of barium titanyl oxalate produces barium titanate with a stoichiometric composition, which gives the method excellent composition stability.
[0007] Patent Documents disclosing the synthesis of barium titanate powder by the oxalate method include Patent Documents 1 and 2. Patent Document 1 discloses a production method in which barium titanyl oxalate is heated to 300 to 600°C in an oxygen-containing gas atmosphere, and then heated to 600 to 1100°C in an oxygen-free reduced pressure atmosphere. Patent Document 2 discloses a production method for barium titanate microparticles in which a composite metal complex containing barium and titanium is allowed to remain in a reaction environment of subcritical water or supercritical water. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2010-70391 A [Patent Document 2] JP 2010-83708 A Summary of the Invention [Problem to be solved by the invention]
[0009] Thus, although the synthesis of barium titanate powder by the oxalate method has been proposed in the past, there is room for improvement in the conventional technology. That is, in the oxalate method, raw materials containing halogens such as chlorine are used. When the raw materials are reacted to obtain barium titanyl oxalate, the halogens are taken into the barium titanyl oxalate, and may remain as impurities in the barium titanate powder after firing. If the barium titanate powder contains a large amount of halogen impurities, it may deteriorate the electrical characteristics of the capacitor and promote the corrosion of other parts.
[0010] It is possible to remove halogen impurities by repeatedly washing barium titanyl oxalate or the barium titanate powder obtained by firing it, but in that case, the elution of barium may progress, causing a deviation in composition. It is also possible to volatilize halogen impurities by firing at high temperatures, but in that case, there is a risk that the particles of the barium titanate powder may become coarse. In addition, although the oxalate method can obtain barium titanate powder with relatively high crystallinity, there is still room for improvement.
[0011] In view of these problems, the present inventors have conducted research and have found that by introducing water vapor during calcination when synthesizing barium titanate-based dielectric particles by the oxalate method, it is possible to obtain particles that are fine, have a small amount of halogen impurities, and have high crystallinity.
[0012] The present invention was completed based on such findings, and an object of the present invention is to provide a method for producing barium titanate-based dielectric particles which are fine, have a small amount of halogen impurities, and have high crystallinity. [Means for solving the problem]
[0013] The present invention encompasses the following embodiments. In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."
[0014] According to one aspect of the present invention, there is provided a method for producing barium titanate (BaTiO3)-based dielectric particles, which includes a reaction step of contacting barium halide, titanium halide, and oxalic acid in an aqueous solution to obtain barium titanyl oxalate, and a calcination step of calcining the barium titanyl oxalate in a furnace, the method including supplying water vapor into the furnace in the calcination step. Effect of the Invention
[0015] According to the present invention, there is provided a method for producing barium titanate-based dielectric particles which are fine, have a small amount of halogen impurities, and have high crystallinity. [Brief description of the drawings]
[0016] [Figure 1] 1 is a graph showing the relationship between the specific surface area and the crystallinity (c-axis / a-axis ratio) of barium titanate powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.
[0018] This embodiment relates to a method for producing a barium titanate (BaTiO3)-based dielectric particle (hereinafter, sometimes simply referred to as "dielectric particle"). Here, the barium titanate-based dielectric particle is a particle containing a barium titanate (BaTiO3)-based compound as a main component. The dielectric particle may contain components other than the BaTiO3-based compound. For example, it may contain components containing elements such as rare earth elements (Re), magnesium (Mg), silicon (Si), manganese (Mn), nickel (Ni), iron (Fe), cobalt (Co), copper (Cu), chromium (Cr), and vanadium (V). However, in order to make the most of the excellent properties based on BaTiO3, the higher the content of the BaTiO3-based compound, the more preferable it is. The content of the BaTiO3-based compound is preferably 50 mass% or more, 70 mass% or more, or 90 mass% or more. The dielectric particle may have a composition containing a BaTiO3-based compound, with the balance being inevitable impurities.
[0019] BaTiO3-based compounds are composite oxides having a perovskite structure with a composition represented by the general formula: ABO3. BaTiO3-based compounds contain barium (Ba) as an A-site element and titanium (Ti) as a B-site element. BaTiO3-based compounds include not only BaTiO3 but also BaTiO3 in which a part of Ba contained in BaTiO3 is replaced with other A-site elements such as Sr and / or Ca, or Ti in which a part of Ti is replaced with other B-site elements such as Zr and / or Hf. This allows the temperature characteristic of the dielectric constant to be flattened. However, in order to obtain a high dielectric constant, the higher the Ba and Ti contents, the more preferable. The proportion of Ba in the A-site elements is preferably 70% or more in molar ratio, more preferably 80% or more, and even more preferably 90% or more. The proportion of Ti in the B-site elements is preferably 70% or more in molar ratio, more preferably 80% or more, and even more preferably 90% or more. The A-site elements do not need to contain any components other than Ba and inevitable impurity elements, and the B-site elements do not need to contain any components other than Ti and inevitable impurity elements.
[0020] Next, the manufacturing method of this embodiment will be described. The manufacturing method of this embodiment includes a reaction step of contacting barium halide, titanium halide, and oxalic acid in an aqueous solution to obtain barium titanyl oxalate, and a calcination step of calcining the barium titanyl oxalate in a furnace. In addition, water vapor is supplied into the furnace in the calcination step. Each step will be described below.
[0021] <Reaction process> In the reaction step, barium halide, titanium halide, and oxalic acid are contacted in an aqueous solution to obtain barium titanyl oxalate via the oxalate process.
[0022] The barium halide and the titanium halide are respectively the Ba source and the Ti source of the BaTiO3-based compound. As the barium halide, barium chloride is preferred, but barium bromide or barium iodide may be used. As the titanium halide, titanium chloride is preferred, but titanium bromide or titanium iodide may be used. Oxalic acid is a raw material used in the synthesis of barium titanyl oxalate, which is an intermediate product, by reacting with the barium halide and the titanium halide. Instead of oxalic acid, oxalates such as sodium and potassium can be used. However, if alkali metal impurities such as sodium and potassium remain, the dielectric particles may grow during calcination, making it difficult to obtain fine dielectric particles. In addition, if alkali metal impurities remain, the insulating properties of the dielectric particles may deteriorate. Therefore, it is preferable to use oxalic acid from the viewpoint of preventing the remaining of metal impurities. In addition, an aqueous solution is preferred as the aqueous solution. However, it is also possible to use an aqueous solution containing a small amount of an organic solvent, for example, 10% by volume or less, such as ethanol or ethylene glycol.
[0023] When the objective is to produce dielectric particles in which a portion of Ba is replaced by other elements such as Sr or Ca, and / or when the objective is to produce dielectric particles in which a portion of Ti is replaced by other elements such as Zr or Hf, a halide of another element, for example a halide such as a strontium halide or a zirconium halide, may be added to the raw materials together with the barium halide and titanium halide.
[0024] There is no particular restriction on the ratio of each raw material. However, it is preferable to mix the raw materials so that the stoichiometric composition that obtains the perovskite structure, that is, the molar ratio of the A-site element (Ba, etc.) and the B-site element (Ti, etc.) of the perovskite compound is approximately equal. For example, when synthesizing BaTiO3, the barium halide and titanium halide are mixed so that the Ba / Ti ratio is within the range of 0.99 to 1.01, particularly 0.995 to 1.005. This allows a BaTiO3-based compound with excellent crystallinity to be obtained without any excess of any element. Preferably, approximately equimolar amounts of barium chloride and titanium tetrachloride, and an excess molar amount of oxalic acid are mixed.
[0025] As a method of contacting the raw materials in an aqueous solution, it is preferable to prepare an aqueous solution of each raw material in advance and mix the aqueous solutions. This allows the raw materials to be mixed homogeneously at the molecular level, and as a result, the intermediate product barium oxalate can be obtained in a more homogeneous state. The aqueous solution may contain only one type of raw material, or may contain a mixture of multiple types of raw materials. Specifically, a barium halide aqueous solution, a titanium halide aqueous solution, and an oxalic acid aqueous solution are prepared and these aqueous solutions are mixed simultaneously. Alternatively, a mixed aqueous solution of barium halide and titanium halide may be prepared, and an oxalic acid aqueous solution may be added to this mixed aqueous solution. Furthermore, a barium halide aqueous solution may be added to a mixed aqueous solution of titanium halide and oxalic acid. However, if barium halide and oxalic acid are mixed in advance, barium oxalate (BaC2O4 or its hydrate) may be generated, which may inhibit the generation of barium titanyl oxalate. Therefore, it is preferable to add titanium halide prior to mixing barium halide and oxalic acid.
[0026] When preparing the raw material aqueous solution, it is preferable to dissolve each raw material in water, particularly purified water, to prepare an aqueous solution having a concentration of, for example, about 0.1 mol / L to saturated state, particularly about 0.5 to 5 mol / L. When preparing an aqueous solution of barium halide or oxalic acid, it may be heated to 50°C or higher, for example, about 60 to 90°C, if desired. These aqueous solutions may also dissolve two or more of the above raw materials.
[0027] When mixing the prepared aqueous raw material solutions, it is preferable to heat one of the solutions, particularly the solution not containing titanium halide, to about 50 to 90°C, particularly about 60 to 80°C. By heating, the reaction can proceed more quickly and uniformly. Here, it is preferable to continue stirring for about 30 minutes to 2 hours while heating after mixing. The precipitate formed by this operation matures, making it easier to separate by subsequent filtration or the like, and reducing the amount of residual halogen impurities. It is also preferable to perform the mixing operation by dropping one solution into the other solution. In particular, when mixing a solution of barium halide and titanium halide with an oxalic acid solution, one solution is dropped into the other solution to gradually precipitate, for example, over a period of about 30 minutes to 6 hours, to obtain a more homogeneous precipitate that is easy to filter.
[0028] The raw materials barium halide, titanium halide, and oxalic acid are contacted in an aqueous solution to cause a reaction, and barium titanyl oxalate (BaTiO(C2O4)2 or its hydrate) is produced in the solution. The produced barium titanyl oxalate is recovered by solid-liquid separation. The solid-liquid separation may be performed by a known method such as filtration and / or centrifugation. Prior to the separation, it is preferable to allow the barium titanyl oxalate and the solution to cool. It is also preferable to wash the separated barium titanyl oxalate with water. The separated barium titanyl oxalate may be further subjected to drying or pulverization. There is no particular limitation on the drying conditions, and the drying may be performed, for example, at 100 to 150°C, particularly 105 to 110°C, for about 30 minutes to 3 hours. The drying may be performed under reduced pressure. The pulverization method is not particularly limited, and may be performed by a general-purpose dry or wet method until the average particle size measured by, for example, laser diffraction scattering method is about 200 μm or less, particularly about 10 to 100 μm.
[0029] <Pre-firing process> In the calcination step, the obtained barium titanyl oxalate is calcined (fired) in a furnace. The calcination causes dehydration and thermal decomposition of the barium titanyl oxalate, and produces BaTiO3-based compounds while releasing by-products such as moisture, carbon monoxide, and carbon dioxide.
[0030] The calcination is preferably performed at a temperature of 600°C or higher, more preferably 720°C or higher, for example, 720 to 1300°C, further 800 to 1200°C, and particularly 850 to 1050°C. At 600°C or higher, particularly 720°C or higher, the reaction of generating BaTiO3-based compounds proceeds smoothly, and dielectric particles with excellent crystallinity can be obtained. At 1300°C or lower, particularly 1200°C or lower, grain growth of BaTiO3-based compounds is suppressed, so that fine dielectric particles can be obtained. The calcination may be performed at the above-mentioned temperature for 1 to 30 hours, particularly 4 to 15 hours. As the calcination furnace, a known furnace such as a tunnel furnace, a batch furnace, a rotary kiln, a roller hearth kiln, or a pusher may be used.
[0031] The atmosphere during calcination is not particularly limited as long as the desired dielectric particles can be obtained. However, in order to prevent the reduction of the obtained dielectric particles, it is preferable to use an oxygen-containing atmosphere, particularly an air atmosphere. If the dielectric particles are reduced, they become semiconductors, making it difficult to obtain the desired dielectric properties, particularly insulating properties.
[0032] In the manufacturing method of this embodiment, water vapor is supplied into the furnace in the calcination process. This makes it possible to obtain fine dielectric particles with a low amount of halogen impurities and excellent crystallinity. Although the details of the mechanism are not clear, it is speculated as follows. That is, during calcination, a dehydration reaction of barium titanyl oxalate occurs at a low temperature, and as the temperature rises, oxalic acid is thermally decomposed. With the thermal decomposition of oxalic acid, by-products such as carbon monoxide and carbon dioxide are released, and the production of barium titanate progresses. It is thought that the supply of water vapor in the calcination process promotes the discharge of reaction by-products and the synthesis of barium titanate. Specifically, it is thought that water molecules in the water vapor are temporarily coordinated or bonded to the atoms of barium and titanium. As a result of the reaction sites of barium and titanium atoms being blocked by water molecules, it is expected that the halogen components remaining in the surroundings are discharged outside the furnace in the form of, for example, hydrogen halide without recombining with these atoms. In addition, it is believed that the discharge of oxalic acid decomposition products that are produced as by-products during calcination is also promoted, so that crystallization proceeds in a cleaner state, resulting in improved crystallinity of the dielectric particles.
[0033] There is no particular limitation on the method of supplying water vapor. For example, atmospheric gas may be supplied into the calciner and water vapor (moisture) may be mixed into the gas. An oxygen-containing gas such as air may be used as the atmospheric gas. Alternatively, calcium hydroxide, magnesium sulfate heptahydrate, or the like may be placed in the calciner and the moisture generated from them at a predetermined temperature may be used.
[0034] As long as the desired dielectric particles are obtained, the timing of supplying water vapor is not limited. However, it is preferable to supply water vapor in the calcination step from the time when the temperature in the furnace reaches at least 720°C or higher until the end of calcination. As shown in the examples described later, supplying water vapor at the time when the calcination temperature reaches 720°C or higher improves the crystallinity of the obtained dielectric particles, further reduces impurities such as halogens, and also relatively increases the specific surface area. It is presumed that this is related to the fact that the reaction of producing barium titanate becomes active in the temperature range of 720°C or higher.
[0035] The amount of water vapor to be supplied is not limited as long as the desired dielectric particles are obtained. However, it is preferable to supply water vapor so that the water vapor concentration in the furnace is 0.3% by volume or more. For example, an atmospheric gas with a water vapor concentration of 0.3% by volume or more, more preferably 3% by volume or more, and even more preferably 10 to 50% by volume may be supplied into the furnace. With such a concentration, it is possible to more significantly reduce impurities such as halogens and improve the crystallinity of the dielectric particles, and it is also possible to more accurately and easily supply water vapor.
[0036] It is preferable to supply steam at a rate of about 0.7 to 60 g per minute per kg of barium titanyl oxalate, i.e., at a rate of about 0.7 to 60 g / kg min. It is recommended that the steam supply rate be more preferably about 7 to 50 g / kg min, even more preferably about 10 to 40 g / kg min, and particularly preferably about 20 to 35 g / kg min.
[0037] By calcination, barium titanate-based dielectric particles can be obtained. The obtained particles can be used as dielectric particles as they are. In addition, post-treatment such as pulverization or heat treatment can be performed as necessary. There is no particular limitation on the pulverization method, and the particles can be pulverized to a desired particle size, for example, several tens of μm, 1 to 10 μm, or 1 μm or less, by a dry or wet pulverization method. Furthermore, a heat treatment step can be performed. When heat treatment is performed, it is preferable to perform the heat treatment at a temperature equal to or lower than the calcination temperature in order to suppress grain growth of the dielectric particles.
[0038] In this manner, the barium titanate-based dielectric particles of the present embodiment can be obtained. The dielectric particles are fine, contain a small amount of halogen impurities such as chlorine, and have excellent crystallinity. For example, but not limited to, a specific surface area (SSA) of 5.0 m 2 / g or more, especially 6.0m 2 / g or more. For example, the amount of halogen, particularly the amount of chlorine, is 1000 mass ppm or less, particularly 800 mass ppm or less. Furthermore, the c / a value can be within the range of 1.005 to 1.011, particularly 1.008 to 1.010. Here, the c / a value is the ratio of the c-axis length to the a-axis length, which is the lattice constant of the perovskite crystal structure. If the composition of the dielectric particles is the same, it can be said that the larger the c / a value, the higher the degree of tetragonal crystallization, that is, the more excellent the crystallinity.
[0039] Preferably, the dielectric particles have a specific surface area S (m 2 / g), and the residual halogen amount C (ppm by mass) in the dielectric particles are expressed by the formula: S ≥ 4.0, and C<260×S-1150 Meet the following.
[0040] The dielectric particles of the present embodiment are fine, have a small amount of halogen impurities, and have excellent crystallinity, and therefore have excellent properties including dielectric properties, and are therefore suitable as materials for electronic components such as multilayer ceramic capacitors, piezoelectric elements, and PTC thermistors, particularly small electronic components. EXAMPLES
[0041] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0042] [Example 1] (Preparation of Barium Titanyl Oxalate) A first liquid was prepared by dissolving 600g (2.46 mol) of barium chloride dihydrate and 450g (2.37 mol) of titanium tetrachloride in 4L of purified water, and a second liquid was prepared by dissolving 600g (4.76 mol) of oxalic acid dihydrate in 2L of purified water at 70°C. While stirring the first liquid, the second liquid kept at about 70°C was dropped therein over 2.5 hours. After the dropwise addition, the mixture was stirred at 70-80°C for another hour and allowed to cool overnight. The precipitate was then filtered, washed three times with purified water, and dried at 105°C for two hours. The obtained barium titanyl oxalate was subjected to X-ray fluorescence analysis, and the Ba / Ti molar ratio was 1.00.
[0043] (Pre-firing) 144g of the barium titanyl oxalate obtained above was placed in a batch-type sintering furnace, and while supplying air at a flow rate of 45L / min, the temperature was raised to 900°C at 9.5°C / min. Here, once the temperature of the sintering furnace reached 200°C, water was mixed in at a rate of 5g / min and air heated to 350°C was supplied (water vapor concentration in the supplied air: approximately 30% by volume, water vapor supply amount relative to barium titanyl oxalate: 35g / kg min). After holding at 900°C for 1 hour, the mixing of water (water vapor supply) was stopped, the mixture was allowed to cool, and a barium titanate sample was collected.
[0044] (Physical property evaluation) The chlorine content, specific surface area, and c / a value of the obtained barium titanate sample were measured by the following methods. The test results are shown in Table 1 and FIG. Chlorine content: Measured by combustion ion chromatography. -Specific surface area: The BET specific surface area was measured by the flow method. ·c / a value: Measured by X-ray diffraction method.
[0045] [Examples 2 to 3, Comparative Examples 1 to 3] The same operation as in Example 1 was carried out, except that the holding temperature (calcination temperature) in the firing furnace was 950° C. (Example 2) and 1000° C. (Example 3). The same operations as in Examples 1 to 3 were carried out except that water vapor was not supplied (Comparative Examples 1 to 3). The test results are shown in Table 1 and FIG.
[0046] [Table 1]
[0047] It was shown that the amount of chlorine contained (amount of residual halogen) was reduced and dielectric particles with a relatively large specific surface area were obtained by supplying water vapor in the calcination process. All of the samples of Examples 1 to 3 satisfied the relationship of the above formula. The c / a value was also an appropriate value within the range of 1.008 to 1.010. It is noted that the c / a value appears to be smaller as a result of supplying water vapor. However, when plotted against the specific surface area as in FIG. 1, it can be seen that dielectric particles with the same specific surface area show a larger c / a value than samples produced without supplying water vapor. It was shown that the manufacturing method of this embodiment reduces the amount of impurities and also provides dielectric particles with good crystallinity (tetragonal crystallinity) and a relatively large specific surface area.
[0048] [Examples 4 to 7] The same operation as in Example 1 was carried out, except that the period during which steam was supplied to the calciner was limited to the period within the temperature range shown in Table 2. The test results are shown in Table 2.
[0049] [Table 2]
[0050] [Example 8] The same operation as in Example 3 was carried out, except that the period during which steam was supplied to the calciner was limited to the period within the temperature range shown in Table 3. The test results are shown in Table 3.
[0051] [Table 3]
[0052] According to the manufacturing method of this embodiment, by supplying water vapor in the calcination process, the chlorine content of the obtained dielectric particles is reduced, the c / a value is within the appropriate range, and the specific surface area is increased. It has become clear that such effects are particularly remarkable in Examples 1, 7, and 8, in which water vapor is introduced during the period from when the temperature reaches 720°C or higher until the calcination process is completed.
[0053] As described above, the manufacturing method of this embodiment provided BaTiO3-based dielectric particles having a reduced amount of halogens, good crystallinity (tetragonal), a relatively large specific surface area, and a Ba / Ti atomic ratio close to 1.
Claims
1. contacting a barium halide, a titanium halide, and oxalic acid in an aqueous solution to obtain barium titanyl oxalate; and A calcination step of calcining the barium titanyl oxalate in a furnace. Barium titanate (BaTiO 3 )-based dielectric particles, A method in which, in the calcination step, the temperature inside the furnace is raised to 900°C or higher, and water vapor is supplied into the furnace during the period from when the temperature inside the furnace reaches 720°C or higher until the calcination step is completed.
2. 2. The method according to claim 1, wherein an atmospheric gas having a water vapor concentration of 0.3 vol % or more is supplied into the furnace during a period from when the temperature inside the furnace reaches 720° C. or higher in the calcination step until the calcination step is completed.
3. The method according to claim 1 or 2, wherein the water vapor is supplied in an amount of 0.7 to 60 g per minute per kg of the barium titanyl oxalate.
4. The specific surface area S (m 2 / g), and the residual halogen amount C (ppm by mass) in the dielectric particles is expressed by the formula: S≧4.0, and C<260×S-1150 The method according to any one of claims 1 to 3, wherein
Citation Information
Patent Citations
Method for manufacturing barium titanate
JP2000344519A
Method for manufacturing perovskite-type barium titanate powder
JP2004123431A
Method for producing perovskite-type barium titanate powder
JP2009209002A
Method for producing barium titanate particle
JP2010070391A
Method for producing barium titanate fine particle and method for manufacturing electronic component