Ceramic dielectric material, ceramic capacitor and preparation method thereof
By doping rare earth elements and base metal oxides into barium titanate-based ceramic materials, and using sintering aids and anti-reducing agents, the dielectric constant and reliability of barium titanate-based ceramic materials in miniaturized, large-capacity MLCC capacitors is solved. The high dielectric constant, stable capacitance and temperature characteristics and high reliability of ceramic capacitors are achieved, achieving the effect of X5R standard.
Patent Information
- Application Number
- CN202310577979.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-22
AI Technical Summary
Existing barium titanate-based ceramic materials are difficult to take into account high dielectric constant, stable capacitance and temperature characteristics and high reliability in miniaturized and large-capacity MLCC capacitors. Especially in the production process of ultra-thin-layer devices, increasing the grain size will be This leads to a decrease in reliability and reduces the grain size and makes it difficult to form a stable core-shell structure, which is difficult to achieve the X5R specification.
Through formulation improvement, barium titanate is used as the main material, doped with rare earth element oxides and base metal oxides, and added sintering aids and anti-reducing agents to prepare high dielectric constant, stable capacity and temperature characteristics and high reliability Ceramic dielectric materials are prepared by specific sintering and oxidation treatment methods.
It realizes the stability of the ceramic capacitor's capacitance change rate between +15% and -15% at -55℃~85℃, and reaches the X5R standard. It has a simple preparation process, no toxic substances, high density of products, and grains. Small, few defects, suitable for actual production applications.
Smart Images

Figure CN118993724A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of materials, and in particular relates to a ceramic dielectric material, a ceramic capacitor and a preparation method thereof. Background Art
[0002] With the rapid development of the world's electronics industry, multi-layer ceramic capacitors (MLCC) as the basic components of the electronics industry are also developing at an astonishing speed. Barium titanate (BaTiO3) is often used as the base material of multi-layer ceramic capacitors because of its high dielectric constant at the Curie temperature.
[0003] In recent years, the miniaturization of mobile electronic devices has led MLCC to gradually develop in the direction of miniaturization and large capacity. This has put forward higher requirements on the various properties of barium titanate-based ceramic materials. The following formula is the MLCC capacitance calculation method:
[0004]
[0005] Where C is the capacitance, N is the number of dielectric layers, ε0 is the vacuum dielectric constant, ε r is the dielectric constant of the material, S is the electrode area, and d is the thickness of the dielectric layer. Since the size of MLCCs of specific specifications is fixed, the capacitance is generally not increased by changing the electrode area. Therefore, if a large-capacity barium titanate-based MLCC is to be obtained, it is generally achieved from the following aspects: 1. Increasing the dielectric constant of barium titanate-based ceramic materials, generally by changing the doping system or increasing the grain size; 2. Increasing the number of stacking layers, that is, the number of dielectric layers N, is equivalent to reducing the thickness of the dielectric layer d. Due to the limitations of the size of MLCCs of specific specifications, and at the same time, each dielectric layer requires a thickness of at least five grains to ensure the stability of the base material, so in the process of manufacturing ultra-thin layer MLCC devices, increasing the grain size and reducing the thickness of the dielectric layer are contradictory. In addition, increasing the grain size when the thickness of the dielectric layer is constant will lead to a decrease in the number of grain boundaries, which may lead to a decrease in reliability, but reducing the grain size will make it difficult to form a stable core-shell structure and it is difficult to reach the specifications of X5R. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art by improving the formula, to provide a ceramic dielectric material with high dielectric constant, stable capacitance-temperature characteristics and high reliability, and to prepare high-performance ceramic capacitors using the above material.
[0007] An object of the present invention is to provide a ceramic dielectric material.
[0008] The ceramic dielectric material comprises the following components in molar percentage: 92.0-97.0 mol% of barium titanate, 1.0-2.5 mol% of sintering aid, 0.5-1.0 mol% of anti-reducing agent, 0.5-1.5 mol% of alkaline earth metal compound, 0.5-3.0 mol% of rare earth element oxide, and 1.0 mol%-2.0 mol% of base metal oxide; the above components are mixed, wet-ground, and dried to obtain the ceramic dielectric material.
[0009] Further, the ceramic dielectric material includes the following components in molar percentage: 94.0-96.0 mol% of barium titanate, 1.2-2.0 mol% of sintering aid, 0.8-1.0 mol% of anti-reduction agent, 0.5-1.0 mol% of alkaline earth metal compound, 1.5-2.5 mol% of rare earth element oxide, and 1.2 mol%-2.0 mol% of base metal oxide.
[0010] Further, the sintering aid material is selected from one or more of SiO2, B2O3, Bi2O3 and BaSiO3;
[0011] The anti-reducing agent is selected from one or more of V2O5, MnO and Cr2O3;
[0012] The alkaline earth metal compound is selected from one or more of alkaline earth metal oxides, alkaline earth metal hydroxides and alkaline earth metal salts, the alkaline earth metal salts include alkaline earth metal halides, alkaline earth metal nitrates and alkaline earth metal carbonates, preferably, the alkaline earth metals are Mg and Ca;
[0013] The rare earth oxide is selected from one or more of Y2O3, Sm2O3, Nd2O3, Eu2O3, Dy2O3, La2O3, Ho2O3, Yb2O3, Er2O3 and Tm2O3;
[0014] The base metal oxide is selected from one or more of Al2O3, In2O3, Nb2O3, ZrO2 and SnO2;
[0015] The particle size of the barium titanate is 200-250nm.
[0016] Further, including
[0017] 0.3-1.2mol% Dy2O3, 0.2-1.0mol% Y2O3, 0.2-0.7mol% Ho2O3.
[0018] Further, the sintering aid includes BaSiO3;
[0019] The rare earth oxides include La2O3 and Nd2O3;
[0020] The sintering aid includes BaSiO3;
[0021] The anti-reducing agent includes MnO;
[0022] The alkaline earth metal compound includes MgO;
[0023] Base metal compounds include In2O3.
[0024] An object of the present invention is to provide a method for preparing a ceramic capacitor.
[0025] The preparation method of the ceramic capacitor comprises the following steps:
[0026] The ceramic dielectric material as described in any one of the above items is mixed into a paste slurry;
[0027] The paste slurry is evenly coated on a film, cast into a 1.2-1.5 μm film, and then electrode printed, laminated, pressed, and cut to form a green body;
[0028] The green body is sintered at 1150-1250° C. for 2-4 hours in a reducing atmosphere, cooled to 950-1100° C. and further oxidized for 2-4 hours, and after the oxidation is completed, cooled to room temperature to obtain a porcelain body;
[0029] Copper electrodes are sintered at both ends of the porcelain body, and then nickel and tin layers are plated in sequence to obtain a ceramic capacitor.
[0030] An object of the present invention is to provide a ceramic capacitor.
[0031] The ceramic capacitor is manufactured according to the above-mentioned method for manufacturing the ceramic capacitor.
[0032] Furthermore, the ceramic capacitor has a multi-dielectric layer structure, the number of dielectric layers is 80-100, and the thickness of the dielectric layer is 1.0-1.5 μm.
[0033] Furthermore, the dielectric constant of the ceramic capacitor at 25° C. is 2500-3500, the resistivity is 150-250 MΩ·m, the capacitance is 15-21 μF, and the capacitance change rate is between +15% and -15% at a temperature of -55° C.-85° C.
[0034] Compared with the prior art, the outstanding effects of the present invention are:
[0035] First: The ceramic dielectric material provided by the present invention uses barium titanate as the main material, and is doped in the form of oxides of acceptor-doped rare earth elements (Dy, Y and Ho) and donor-doped rare earth elements (La, Sm and Nd), and sintering aids, anti-reducing agents, alkaline earth metal compounds and base metal oxides (In2O3) are added. The prepared ceramic dielectric material has the characteristics of stable capacitance-temperature characteristics, high dielectric constant and high reliability;
[0036] Second: The ceramic capacitor provided by the present invention has a capacitance change rate between +15% and -15% at a temperature of (-55)-85°C, that is, it can meet the X5R standard;
[0037] Third: The preparation method of the ceramic dielectric material and ceramic capacitor provided by the present invention is simple, easy to operate, and does not contain toxic or harmful substances. The prepared ceramic capacitor has high density, small grains, and few defects, and is suitable for actual production applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 : The preparation method of the ceramic capacitor provided by the present invention.
[0039] Figure 2 : Scanning electron microscope image of the MLCC sample of Example 1 of the present invention.
[0040] Figure 3 : Scanning electron microscope image of the MLCC sample of Example 2 of the present invention.
[0041] Figure 4 : Scanning electron microscope image of the MLCC sample of comparative example 1 of the present invention.
[0042] Figure 5 : Grain size distribution diagram of the MLCC sample of Example 1 of the present invention.
[0043] Figure 6 : Grain size distribution diagram of the MLCC sample of Example 2 of the present invention.
[0044] Figure 7 : Grain size distribution diagram of the MLCC sample of comparative example 1 of the present invention.
[0045] Figure 8 : Capacitance and temperature relationship diagram of MLCC samples of Example 1, Example 2 and Comparative Example 1 of the present invention.
[0046] Fig. 9 : Resistance failure evaluation of MLCC samples in Example 1, Example 2 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0047] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings, but they should not be construed as limiting the applicable scope of the present invention.
[0048] The invention provides a ceramic dielectric material, comprising the following components in molar percentage: 92.0-97.0 mol% of barium titanate, 1.0-2.5 mol% of a sintering aid, 0.5-1.0 mol% of an anti-reducing agent, 0.5-1.5 mol% of an alkaline earth metal compound, 0.5-3.0 mol% of a rare earth element oxide, and 1.0 mol%-2.0 mol% of a base metal oxide; the above components are mixed, wet-ground, and dried to obtain the ceramic dielectric material.
[0049] The ceramic dielectric material provided by the present invention selects rare earth element oxides and base metal oxides as main dopants, modifies barium titanate, and adds sintering aids, anti-reducing agents, and alkaline earth metal compounds to modify the material properties, thereby preparing a ceramic dielectric material with high dielectric, high stable temperature characteristics and high reliability.
[0050] As a preferred embodiment of the ceramic dielectric material of the present invention, the ceramic dielectric material includes the following components in molar percentage: 94.0-96.0 mol% of barium titanate, 1.2-2.0 mol% of sintering aid, 0.8-1.0 mol% of anti-reducing agent, 0.5-1.0 mol% of alkaline earth metal compound, 1.5-2.5 mol% of rare earth element oxide, and 1.2 mol%-2.0 mol% of base metal oxide.
[0051] As a preferred embodiment of the ceramic dielectric material of the present invention, the sintering aid material is selected from one or more of SiO2, B2O3, Bi2O3 and BaSiO3; the anti-reducing agent is selected from one or more of V2O5, MnO and Cr2O3; the alkaline earth metal compound is selected from one or more of alkaline earth metal oxides, alkaline earth metal hydroxides and alkaline earth metal salts, the alkaline earth metal salts include alkaline earth metal halides, alkaline earth metal nitrates and alkaline earth metal carbonates, preferably, the alkaline earth metals are Mg and Ca; the rare earth oxide is selected from one or more of Y2O3, Sm2O3, Nd2O3, Eu2O3, Dy2O3, La2O3, Ho2O3, Yb2O3, Er2O3 and Tm2O3; the base metal oxide is selected from one or more of Al2O3, In2O3, Nb2O3, ZrO2 and SnO2.
[0052] The rare earth element oxides selected by the present invention are divided into two categories, one is acceptor-doped rare earth elements, and the other is donor-doped rare earth oxides. Acceptor-doped rare earth elements include Y, Dy, and Ho. These three elements are mainly doped in the B position and belong to acceptor doping; the oxide form of Y, Dy, and Ho as doping elements of the main material barium titanate can reduce the Curie temperature, and the added rare earth element oxides will affect the formation of barium titanate grains, forming a "core-shell" structure, thereby reducing the peak value at the Curie temperature, and can also significantly reduce the capacitance-temperature change rate. However, the problem caused by acceptor doping is that the acceptor defects formed by doping will form defect dipoles with the oxygen vacancies generated by charge compensation. This composite defect will have a clamping effect on the ferroelectric domain, limiting the flipping of the ferroelectric domain and causing the dielectric constant of the material to decrease. In order to solve the above problems, we adopt the method of introducing donor doping elements. Here we choose rare earth elements doped at the A site, such as Sm, La and Nd. The introduction of donor doping in the barium titanate system can "soften" the ferroelectric domain and promote the reversal of the ferroelectric domain, thereby achieving the purpose of improving the dielectric constant of the system.
[0053] As a preferred embodiment of the ceramic dielectric material of the present invention, based on the total molar amount of the ceramic dielectric material, the Dy2O3 accounts for 0.3-1.2 mol%, the Y2O3 accounts for 0.2-1.0 mol%, and the Ho2O3 accounts for 0.2-0.7 mol%.
[0054] In the preferred embodiment of the ceramic dielectric material of the present invention, the donor rare earth oxide includes La2O3 and Nd2O3. The ion radii of the donor doping elements La and Nd at the A site are 0.136nm and 0.127nm respectively, and the ion size similar to that of barium ions can ensure that the element is doped into the A site to replace Ba. 3+ Replace Ba 2+ ) has the opposite effect on ferroelectrics as acceptor doping. 3+ and Nd 3+ Doping increases the mobility of the domain walls, "softens" the ferroelectric domains and makes them easier to flip, thereby increasing the overall dielectric constant. This is mainly due to La 3+ and Nd 3+ Charge compensation caused by doping will form Ba or Ti vacancies (V Ba or V Ti ), which is caused by the relaxation of internal stress caused by these two vacancies and the transfer of electrons between ionized Ba and Ti vacancies.
[0055] As a preferred embodiment of the ceramic dielectric material described in the present invention, the sintering aid includes BaSiO3. The present invention uses BaSiO3 as a sintering aid. While supplementing the Ba source, it can reduce the sintering temperature to prevent abnormal growth of grains and save energy. The sintering aid plays a role in promoting the formation of the liquid phase during the sintering process. An appropriate sintering aid can allow the liquid phase to fully wrap each grain, physically isolate the grains, and make it impossible for the grains to grow through Oswald ripening, and promote the mass transfer process of BaTiO3 to improve the density of the product; at the same time, the liquid phase on the surface of the inner electrode can hinder the diffusion of metal elements into the dielectric layer, reduce the width of the mixed alloy layer of BT and Ni, and make the surface of the Ni electrode smoother and flatter. The electrode is more continuous after sintering, which enhances the reliability of subsequent products and increases the excellence of the present invention in the application field of MLCC.
[0056] It is a preferred embodiment of the ceramic dielectric material of the present invention, wherein the anti-reduction agent comprises MnO. When the ceramic dielectric material is used for subsequent ceramic capacitor preparation, Ti 4+ When sintered in a reducing atmosphere, it is reduced to Ti 3 + At the same time, oxygen vacancies are generated to compensate for the charge. Oxygen vacancies are prone to directional migration under the action of an external electric field. When oxygen vacancies are enriched at the cathode, the potential barrier at the electrode interface is reduced, resulting in a decrease in the overall reliability of the sample. The addition of MnO allows Mn, which can undergo valence changes, to replace the Ti position in barium titanate (BT), thereby inhibiting the generation of oxygen vacancies and improving the material's anti-puncture performance.
[0057] As a preferred embodiment of the ceramic dielectric material of the present invention, the alkaline earth metal compound includes MgO. The addition of MgO can refine the grains, thereby increasing the unit grain boundary density inside the sample. Grain boundaries serve as a barrier to limit the migration of oxygen vacancies. Increasing the concentration of grain boundaries can improve the material's anti-puncture performance and improve the reliability of the sample.
[0058] As a preferred embodiment of the ceramic dielectric material of the present invention, the base metal compound includes In2O3. 3 + In polycrystalline BaTiO3, it exists as a charge-compensating Ba vacancy occupying the octahedral interstitial and grain boundary. 3+ The defect combination of In ions and Ba vacancies provides a substantial barrier to grain boundary migration during sintering, further inhibiting grain growth during sintering. 3+ The enrichment at the grain boundary will induce induced charges to form a space charge layer. The space charge layer at the grain boundary will increase the activation barrier on both sides of the grain boundary and inhibit the migration of oxygen vacancies between grains, thereby improving the reliability of the sample.
[0059] As a preferred embodiment of the ceramic dielectric material of the present invention, the particle size of the barium titanate is 200-250nm. As the main material of the ceramic dielectric material, the selection of particle size of barium titanate is particularly critical to the performance. In order to control the thickness of the dielectric layer in the ceramic capacitor, the average particle size should be <300nm, but too small a particle size is not easy to form a stable "core-shell" structure, so in the raw material stage, the particle size of barium titanate is preferably 200-250nm, so as to control the grain size of the obtained ceramic dielectric material to be around 250nm, and further make the thickness of the dielectric layer of the prepared ceramic capacitor below 1.5μm.
[0060] As a preferred embodiment of the ceramic dielectric material of the present invention, the ceramic dielectric material includes the following components in molar percentage: barium titanate 92.0-96.0 mol%, sintering aid 1.2-2.0 mol%, anti-reduction agent 0.8-1.0 mol%, alkaline earth metal compound 0.5-1.0 mol%, Dy2O3 0.4-0.8 mol%, Y2O3 0.4-0.8 mol%, Ho2O3 0.3-0.6 mol%, La2O3 0.4-0.8 mol%, Nd2O3 0.4-0.8 mol% and In2O3 0.5-1.0 mol%. When the molar percentage content of the components is within the above range, the prepared ceramic dielectric material is a powder without a second phase and with good dispersibility, and the sintered ceramic material has a suitable grain size and core-shell ratio, so that ceramic capacitors can be further prepared using it as a raw material. The obtained ceramic capacitors have the characteristics of stable capacitance-temperature characteristics, high dielectric constant and high reliability, and can meet the X5R standard, that is, when the temperature is (-55)-85°C, the capacitance change rate is between +15% and -15%.
[0061] In addition, the present invention also provides a method for preparing the ceramic capacitor, comprising the following steps: making a ceramic dielectric material into a slurry and then casting it into a 1.2-1.5μm film, then printing, laminating, pressing and cutting the electrode to form a green body; then sintering the green body at 1150-1250℃ for 2-4h in a reducing atmosphere, then cooling to 950-1100℃ and continuing oxidation for 2-4h, and after the oxidation is completed, cooling to room temperature; subsequently sintering at both ends of the porcelain body to form copper electrodes, and plating nickel layers and tin layers in sequence to obtain a ceramic capacitor. When the above method is used to prepare a ceramic capacitor, the grain size can be well controlled, and the prepared ceramic capacitor has a good density. As a preferred embodiment of the preparation method of the present invention, the reducing atmosphere includes the following components in volume percentage: 1% H2 and 99% N2. As a preferred embodiment of the preparation method of the present invention, the sintering temperature for sintering to form the copper electrode is 800-950℃.
[0062] The present invention also provides a ceramic capacitor, which is manufactured by the above-mentioned method for manufacturing the ceramic capacitor.
[0063] As a preferred embodiment of the ceramic capacitor of the present invention, the particle size of the ceramic grains in the ceramic capacitor is 200-250nm. As a preferred embodiment of the ceramic capacitor of the present invention, the ceramic capacitor is a multi-dielectric layer structure, the number of the dielectric layers is 80-100, and the thickness of the dielectric layer is 1.0-1.5μm. As a preferred embodiment of the ceramic capacitor of the present invention, the dielectric constant of the ceramic capacitor at 25°C is 2500-3500, the resistivity is 150-250MΩ·m, the capacitance is 15-21μF, and the capacitance change rate is between +15% and -15% when the temperature is -55°C to 85°C.
[0064] Example 1
[0065] A ceramic capacitor of this embodiment, wherein the raw materials of the ceramic dielectric material include the following components in molar percentage: BaTiO3 95mol%, BaSiO3 1.5mol%, MgO 0.8mol%, MnO 1mol%, Dy2O3 0.6mol%, Y2O30.6mol%, Ho2O3 0.5mol%, La2O30.4mol%, Nd2O30.4mol%, In2O30.2mol%; the particle size of BaTiO3 is 250nm;
[0066] See instructions Figure 1 , the specific preparation method of ceramic capacitors is as follows:
[0067] (1) Preparation of ceramic dielectric material: Weigh the components according to the above molar percentages, mix them, use zirconium oxide balls as ball milling media, place them in a ball mill, add ethanol solvent and perform wet ball milling for 24 hours. After the ball milling is completed, dry them to obtain a ceramic dielectric material;
[0068] (2) Preparation of green body: The ceramic dielectric material of step (1) is made into slurry, cast into a 1.5 μm membrane, and then formed into a green body through electrode printing, lamination, pressing, and cutting; wherein nickel paste is used as the inner electrode during electrode printing, and the number of layers during lamination is 80-100;
[0069] (3) Preparation of porcelain body: The green body of step (2) was sintered at 1200° C. for 2 h in a reducing atmosphere (1% H2+9% N2), then the temperature was lowered to 950° C. for reoxidation treatment for 2 h, and then the temperature was lowered to 25° C. to complete the sintering, thereby forming a porcelain body;
[0070] (4) Preparation of ceramic capacitors: Copper paste is applied to both ends of the ceramic body in step (3) by copper dipping, and then sintered at 900°C to form copper electrodes firmly bonded to the ceramic body. A nickel layer and a tin layer are then electroplated on the surface of the copper electrode in sequence to obtain a ceramic capacitor.
[0071] Example 2
[0072] A ceramic capacitor of this embodiment, wherein the raw materials of the ceramic dielectric material include the following components in molar percentage: BaTiO3 95mol%, BaSiO3 1.5mol%, MgO 0.8mol%, MnO 1mol%, Dy2O3 0.4mol%, Y2O30.4mol%, Ho2O3 0.5mol%, La2O30.6mol%, Nd2O30.6mol%, In2O30.2mol%; the particle size of BaTiO3 is 250nm; the preparation method is the same as that of Example 1.
[0073] Comparative Example 1
[0074] A ceramic capacitor in this comparative example, wherein the raw materials of the ceramic dielectric material include the following components in molar percentage: BaTiO3 95mol%, BaSiO3 1.5mol%, MgO 0.8mol%, MnO 1mol%, Dy2O3 0.6mol%, Y2O30.6mol%, Ho2O3 0.5mol%, La2O30.4mol%, Nd2O30.4mol%; the particle size of BaTiO3 is 250nm; the preparation method is the same as that in Example 1.
[0075] The ceramic capacitors prepared in Examples 1, 2 and Comparative Example 1 were subjected to the following tests:
[0076] ①Morphology and structure:
[0077] 1) Test instrument: grinding and polishing machine (Tegramin-25; Struers; Denmark) Test method: The device is embedded in epoxy resin, and the vertical surface of the electrode is ground and polished for observation.
[0078] 2) Test instrument: 3D laser confocal microscope (VK-X1100; KEYENCE; Japan) Test method: Observe the polished surface.
[0079] 3) Testing instrument: SEM (Nova NanoSEM 450; FEI; USA). Testing method: Directly observe the microscopic morphology of the polished surface, perform EDS analysis on specific areas; perform acid etching on the polished surface, and observe the grain morphology after gold spraying.
[0080] ②Electrical characteristics:
[0081] 1) Test instrument: Broadband dielectric tester (Alpha-A; Novocontrol GmbH; Germany). Test method: According to the driving field of 0.5V, the capacitance and loss at different frequencies (1.2Hz, 12Hz, 120Hz, 1.2kHz, 12kHz, 120kHz) at the temperature between -100℃ and 200℃ were measured at intervals of 2℃.
[0082] 2) Test instrument: dielectric parameter tester (E4980A; Agilent; USA) Test method: At room temperature of 25°C, the driving field was adjusted to 0.50V and the frequency was 120Hz to measure its basic electrical properties.
[0083] ③Reliability:
[0084] 1) Test instrument: semiconductor tester (708B; Keithley; USA) Test method: set the DC voltage from the rated voltage, test time 120s, and measure the insulation resistance of the device.
[0085] 2) Test instrument: High resistance meter (4980E; Keithley; USA) Test method: At 200°C, measure the leakage current of the device starting from 1 to 3 times the rated voltage intensity until the current increases by a cliff.
[0086] Table 1: Performance test data of ceramic capacitors prepared in Examples 1-2 and Comparative Example 1
[0087]
[0088] Compared with Comparative Example 1, In2O3 base metal oxides are introduced into Examples 1 and 2. On the one hand, the composition fluctuation inside the sample is more obvious, thereby obtaining higher capacitance-temperature characteristics; on the other hand, due to In 3+ The preferential enrichment of grain boundaries makes it easier to form space charge layers on both sides of the grain boundaries, making it more difficult for carriers to transition through the grain boundaries, thereby reducing the probability of sample breakdown during actual use and improving the reliability of the sample in extreme environments.
Claims
1. A ceramic dielectric material, characterized in that: The invention comprises the following components in molar percentage: 92.0-97.0 mol % of barium titanate, 1.0-2.5 mol % of sintering aid, 0.5-1.0 mol % of anti-reducing agent, 0.5-1.5 mol % of alkaline earth metal compound, 0.5-3.0 mol % of rare earth element oxide, and 1.0 mol %-2.0 mol % of base metal oxide; The above components are mixed, wet-milled and dried to obtain the ceramic dielectric material.
2. The ceramic dielectric material according to claim 1, characterized in that The invention comprises the following components in molar percentage: 94.0-96.0 mol% of barium titanate, 1.2-2.0 mol% of sintering aid, 0.8-1.0 mol% of anti-reducing agent, 0.5-1.0 mol% of alkaline earth metal compound, 1.5-2.5 mol% of rare earth element oxide and 1.2 mol%-2.0 mol% of base metal oxide.
3. The ceramic dielectric material according to claim 1, characterized in that The sintering aid material is selected from one or more of SiO2, B2O3, Bi2O3 and BaSiO3; The anti-reducing agent is selected from one or more of V2O5, MnO and Cr2O3; The alkaline earth metal compound is selected from one or more of alkaline earth metal oxides, alkaline earth metal hydroxides and alkaline earth metal salts, the alkaline earth metal salts include alkaline earth metal halides, alkaline earth metal nitrates and alkaline earth metal carbonates, preferably, the alkaline earth metals are Mg and Ca; The rare earth oxide is selected from one or more of Y2O3, Sm2O3, Nd2O3, Eu2O3, Dy2O3, La2O3, Ho2O3, Yb2O3, Er2O3 and Tm2O3; The base metal oxide is selected from one or more of Al2O3, In2O3, Nb2O3, ZrO2 and SnO2; The particle size of the barium titanate is 200-250nm.
4. The ceramic dielectric material according to claim 3, characterized in that include 0.3-1.2mol% Dy2O3, 0.2-1.0mol% Y2O3, 0.2-0.7mol% Ho2O3.
5. The ceramic dielectric material according to claim 3, characterized in that The rare earth oxides include La2O3 and Nd2O3; The sintering aid includes BaSiO3; The anti-reducing agent includes MnO; The alkaline earth metal compound includes MgO; Base metal compounds include In2O3.
6. The ceramic dielectric material according to claim 3, characterized in that The invention comprises the following components in mole percentage: barium titanate 92.0-96.0 mol%, sintering aid 1.2-2.0 mol%, anti-reduction agent 0.8-1.0 mol%, alkaline earth metal compound 0.5-1.0 mol%, Dy2O3 0.4-0.8 mol%, Y2O3 0.4-0.8 mol%, Ho2O3 0.3-0.6 mol%, La2O3 0.4-0.8 mol%, Nd2O3 0.4-0.8 mol% and In2O3 0.5-1.0 mol%.
7. A method for preparing a ceramic capacitor, characterized in that: The steps include: The ceramic dielectric material according to any one of claims 1 to 6 is mixed into a paste slurry; The paste slurry is evenly coated on the film, cast into a 1.2-1.5 μm film, and then formed into a green body through electrode printing, lamination, pressing and cutting; The green body is sintered at 1150-1250° C. for 2-4 hours in a reducing atmosphere, cooled to 950-1100° C. and further oxidized for 2-4 hours, and after the oxidation is completed, cooled to room temperature to obtain a porcelain body; Copper electrodes are sintered at both ends of the porcelain body, and then nickel and tin layers are plated in sequence to obtain a ceramic capacitor.
8. A ceramic capacitor, characterized in that: The ceramic capacitor is manufactured according to the method for preparing the ceramic capacitor according to claim 7.
9. The ceramic capacitor according to claim 8, characterized in that The ceramic capacitor has a multi-dielectric layer structure, the number of dielectric layers is 80-100, and the thickness of the dielectric layers is 1.0-1.5 μm.
10. The ceramic capacitor according to claim 9, characterized in that The dielectric constant of the ceramic capacitor at 25° C. is 2500-3500, the resistivity is 150-250 MΩ·m, the capacitance is 15-21 μF, and the capacitance change rate is between +15% and -15% when the temperature is -55° C.-85° C.
Citation Information
Patent Citations
Dielectric ceramic composition and electronic device
CN103449812A
Co-doped barium titanate ceramic dielectric material as well as preparation method and application thereof
CN114014649A
Medium-high voltage ceramic capacitor dielectric material and application thereof
CN114605144A
Co-doped barium titanate ceramic dielectric material, preparation method and application thereof
CN114823137A
Co-doped barium titanate ceramic dielectric material as well as preparation and application thereof
CN114956806A
Cited By
Preparation method of high-capacity X7R type barium titanate-based dielectric ceramic powder
CN120247551A
High-dielectric low-loss ceramic composition as well as preparation method and application thereof
CN121181346A
High-temperature-stability high-dielectric-constant ceramic composition and preparation method thereof
CN121850646A