Co-doped barium titanate ceramic dielectric material and application thereof
By adding doped materials such as SiO2, MgO, MnO and Ho2O3 to BaTiO3 ceramics, a co-doped barium titanate ceramic dielectric material with high dielectric constant and high capacitance and temperature coefficient was prepared, and the change of pure BaTiO3 dielectric constant with temperature was solved. The major problem is to achieve stability and suitable multi-layer ceramic capacitors in high or wide temperature ranges.
Patent Information
- Application Number
- CN202410960267.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-29
AI Technical Summary
The dielectric constant of pure BaTiO3 ceramic dielectric materials varies greatly with temperature, limiting their application in high temperature or wide temperature ranges.
Co-doped barium titanate ceramic dielectric material, mainly composed of BaTiO3 as the main material, SiO2, MgO, MnO and Ho2O3 as doped materials, was prepared by wet ball milling and reducing atmosphere sintering to form a high dielectric constant and multi-layer ceramic capacitors with high capacitance and temperature coefficient.
It realizes the stability of the dielectric constant in a high temperature or wide temperature range, meets the requirements of X7R temperature characteristics, has a capacitance change rate between +40% and -25%, and is dense in materials and has few defects. It is suitable for multi-layer ceramic capacitors.
Smart Images

Figure CN119038986A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic dielectrics, and in particular to a co-doped barium titanate ceramic dielectric material and application thereof. Background Art
[0002] Multilayer ceramic capacitors (MLCC) are widely used in communication infrastructure equipment circuits such as communication equipment, automotive electronics, industrial machinery, and medical equipment. MLCC can be used as power bypass capacitors such as liquid crystal modules (liquid crystal drive voltage circuits), high power supply voltage LSI / IC / OP amplifiers, or as smoothing capacitors such as DC-DC converters (input and output), switching power supplies (secondary side), etc.
[0003] In recent years, the miniaturization of mobile electronic devices has led to the gradual development of MLCC in the direction of miniaturization and large capacity. BaTiO3-based ceramics are widely used in electronic components due to their excellent dielectric properties, especially as dielectric materials for multilayer ceramic capacitors. However, the dielectric constant of pure BaTiO3 ceramics varies greatly with temperature, which limits its application at high temperatures or in a wide temperature range. Summary of the invention
[0004] In view of the above technical problems, the present invention provides a co-doped barium titanate ceramic dielectric material with high dielectric constant, high temperature coefficient and high stability and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides a co-doped barium titanate ceramic dielectric material, wherein the co-doped barium titanate has BaTiO3 as the main material, the addition amount of which is 95-96 mol%; and SiO2, MgO, MnO and Ho2O3 as doping materials, the total addition amount of which is 4-5 mol%.
[0007] As a preferred embodiment, the particle size of the main material BaTiO3 is 150-200 nm.
[0008] Preferably, the added amount of SiO2 is 1 to 3 mol%.
[0009] Preferably, the added amount of MgO is 1 to 3 mol%.
[0010] Preferably, the added amount of MnO is 0.1-0.5 mol%.
[0011] As a preferred embodiment, the addition amount of Ho2O3 is 1-1.4 mol% based on the co-doped barium titanate ceramic dielectric material; for example, 1 mol%, 1.1 mol%, 1.2 mol%, 1.3 mol%, 1.4 mol% or any value therebetween.
[0012] In the technical solution of the present invention, the preparation method of the co-doped barium titanate ceramic dielectric material is a conventional method. In some specific embodiments, it specifically includes the following steps: wet ball milling the main material and the doping material, and obtaining the co-doped barium titanate ceramic dielectric material after drying.
[0013] The second aspect of the present invention provides the use of the above co-doped barium titanate ceramic dielectric material in electronic packaging;
[0014] Preferably, use in semiconductor packaging;
[0015] Preferably, the invention is used in the preparation of multilayer ceramic capacitors.
[0016] A third aspect of the present invention provides a multilayer ceramic capacitor made of the above co-doped barium titanate ceramic dielectric material.
[0017] The fourth aspect of the present invention provides a method for preparing the above-mentioned multilayer ceramic capacitor, comprising the following steps: sintering the above-mentioned co-doped barium titanate ceramic dielectric material in a reducing atmosphere; cooling and reoxidizing; wherein the sintering temperature is 1220-1280°C, and the cooling and reoxidation temperature is 950-1100°C.
[0018] In the technical solution of the present invention, the grain size of the ceramic dielectric of the multilayer ceramic capacitor is 250-330 nm.
[0019] In certain specific embodiments, the grain size of the ceramic dielectric of the multilayer ceramic capacitor is 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm, or any value therebetween.
[0020] In the technical solution of the present invention, Ho doping can promote BaTiO3 to form ceramic dielectric grains with a "core-shell" structure. In this structure, the "core" part is undoped BaTiO3 ceramic, maintaining its original tetragonal ferroelectric phase structure; while the "shell" part is a pseudo-cubic paraelectric phase structure formed by Ho element doping, and other elements such as Mg and Mn will also be doped into the shell to enhance the stability of the shell structure.
[0021] In the technical solution of the present invention, the Ho element shell concentration of the ceramic dielectric grains of the multilayer ceramic capacitor is 0.15% to 0.33%; the Ho element shell concentration is defined as the peak value of the Ho element concentration of the ceramic dielectric grains in EDS, which increases with the increase of Ho doping concentration.
[0022] In the technical solution of the present invention, the Ho element shell thickness of the ceramic dielectric grains of the multilayer ceramic capacitor is 50-100 nm; the Ho element shell is defined as the thickness of the layer enriched with the Ho element in the ceramic dielectric grains.
[0023] In the technical solution of the present invention, the dielectric constant of the multilayer ceramic capacitor is 2500-3000 at 25°C.
[0024] In the technical solution of the present invention, the capacitance change rate of the multilayer ceramic capacitor is between +40% and -25% at -55°C to 125°C.
[0025] In some specific embodiments, at 25° C., the dielectric constant of the multilayer ceramic capacitor is 2500, 2600, 2700, 2800, 2900, 3000 or any value therebetween.
[0026] The above technical solution has the following advantages or beneficial effects:
[0027] The present invention uses BaTiO3 as the main material and optimizes the ratio of doping materials to prepare a barium titanate ceramic dielectric material with high dielectric constant, high temperature coefficient and high stability. Among them, SiO2 is added as a sintering aid to reduce and widen the sintering temperature to prevent the grain growth of ceramic particles during the sintering process; MgO is added to refine the grains and promote the mass transfer process of BaTiO3 to improve the density of the ceramic; MnO is added to promote the formation of the core-shell structure, and Ho2O3 is added to form a "core-shell" structure to stabilize the effect of temperature on capacitance. By sintering in a reducing atmosphere, the stability of the ceramic dielectric properties is improved and its Curie peak is reduced.
[0028] On this basis, the present invention also prepares a multilayer ceramic capacitor MLCC by sintering the co-doped barium titanate ceramic dielectric material in a reducing atmosphere, and the dielectric constant thereof is between 2500 and 3000, and can meet the X7R temperature characteristic requirements, that is, the capacitance change rate is between +40% and -25% at a temperature of -55°C to 125°C. The co-doped barium titanate ceramic dielectric material and capacitor provided by the present invention have a simple preparation process, do not contain toxic substances, have good matching with base metal internal electrodes such as nickel, have a dense ceramic body, small grains, few defects, and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1The scanning electron microscope image and grain size distribution diagram of the MLCC sample in Example 1 of the present invention.
[0030] Figure 2 The scanning electron microscope image and grain size distribution diagram of the MLCC sample in Example 2 of the present invention.
[0031] Figure 3 The scanning electron microscope image and grain size distribution diagram of the MLCC sample in Example 3 of the present invention.
[0032] Figure 4 This is the Ho element concentration distribution diagram of the MLCC sample in Example 1 of the present invention.
[0033] Figure 5 This is the Ho element concentration distribution diagram of the MLCC sample in Example 2 of the present invention.
[0034] Figure 6 This is the Ho element concentration distribution diagram of the MLCC sample in Example 3 of the present invention.
[0035] Figure 7 Schematic diagram showing the comparison between the dielectric constant and temperature of the MLCC sample in Example 1 of the present invention.
[0036] Figure 8 Schematic diagram comparing the dielectric constant and temperature of the MLCC sample in Example 2 of the present invention.
[0037] Fig. 9 Schematic diagram showing the comparison between the dielectric constant and temperature of the MLCC sample in Example 3 of the present invention.
[0038] Fig.10 The dielectric temperature spectrum (TCC) diagram of the MLCC samples in Examples 1-3 of the present invention.
[0039] Fig.11 1 is the relationship between the dielectric constant and the AC electric field of the MLCC samples in Examples 1-3 of the present invention.
[0040] Fig.12 It is the shell conductivity activation energy of the MLCC sample in Example 1 of the present invention.
[0041] Fig.13 It is the shell conductivity activation energy of the MLCC sample in Example 2 of the present invention.
[0042] Fig.14 It is the shell conductivity activation energy of the MLCC sample in Example 2 of the present invention. DETAILED DESCRIPTION
[0043] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0044] The purpose of the present invention is to design a ceramic dielectric material with high dielectric constant and high temperature coefficient, which uses BaTiO3 as the main material and SiO2, MgO, MnO and Ho2O3 as doping materials, wherein the addition amount of the main material BaTiO3 is 95-96 mol%, and the total addition amount of the doping material is 4-5 mol%.
[0045] Among them, the particle size of the main material BaTiO3 is 150-200nm.
[0046] The present invention adopts the commonly used BaTiO3 main material, which can reduce the complexity of the process and save costs. According to experience, the grain size of BaTiO3 nanoparticles increases by 20% to 35% after sintering to form a multilayer ceramic capacitor (MLCC), so the particle size of the main BaTiO3 is controlled to be 150-200nm, so as to obtain the final ceramic grain size of 250-330nm.
[0047] The present invention adopts amphoteric doping and selects the rare earth element Ho as the doping element of the barium titanate material. As the Ho doping concentration increases, the TCC curve of the ceramic gradually flattens and the dielectric peak is significantly depressed. In addition, the Ho element also affects the formation of barium titanate ceramic grains, forming a "core-shell" structure and improving the reliability of the material.
[0048] Furthermore, in a preferred embodiment of the present invention, in the doping material, the added amount of SiO2 is 1-3 mol%, the added amount of MgO is 1-3 mol%, the added amount of MnO is 0.1-0.5 mol%, and the added amount of Ho2O3 is 1-1.4 mol%.
[0049] As a rare earth element, the doping of Ho can promote the formation of a "core-shell" structure in BaTiO3-based ceramics. In this structure, the "core" is undoped BaTiO3 ceramics, which maintains its original tetragonal ferroelectric phase structure; while the "shell" is a pseudo-cubic paraelectric phase structure formed by Ho doping, as a layer of solid solution wrapped outside the "core". The doping concentration of Ho will affect the quality and characteristics of the "core-shell" structure. When the Ho doping concentration is appropriate, a complete "core-shell" structure can be formed, in which the thickness and concentration of the "shell" layer increase with the increase of Ho doping concentration. However, when the Ho doping concentration is too high, it may exceed its solubility limit in BaTiO3, leading to the formation of a second phase, such as pyrochlore-type holmium metatitanate (Ho2Ti2O7), which may destroy the "core-shell" structure.
[0050] Furthermore, the preparation method of the co-doped barium titanate ceramic dielectric material of the present invention comprises the following steps: mixing the main material and the doping material according to a proportion, using zirconium oxide balls as ball milling media, performing wet ball milling for 20 hours, and drying to obtain the co-doped barium titanate ceramic dielectric material.
[0051] Furthermore, in a preferred embodiment of the present invention, the co-doped barium titanate ceramic dielectric material is sintered at 1220° C. to 1280° C. in a reducing atmosphere for 2 to 4 hours to produce a multi-layer ceramic capacitor.
[0052] Furthermore, in a preferred embodiment of the present invention, the grain size of the ceramic dielectric of the multilayer ceramic capacitor is 250-330 nm.
[0053] Furthermore, in a preferred embodiment of the present invention, the dielectric constant of the prepared multilayer ceramic capacitor is between 2500 and 3000 at 25°C.
[0054] Furthermore, in a preferred embodiment of the present invention, the capacitance change rate of the prepared multilayer ceramic capacitor is between -25% and +40% at a temperature between -55°C and 125°C, meeting the X7R requirement of the Electronic Industries Association (EIA).
[0055] In the following embodiments, the preparation process of co-doped barium titanate ceramic dielectric material and MLCC is as follows:
[0056] (1) High-purity BaTiO3 powder with a particle size of 200 nm was selected and mixed with various doping materials in proportion, and zirconium oxide balls were used as ball milling media. The powder was placed in a ball mill and wet-milled for 24 hours. After the ball milling was completed, the powder was dried to obtain a ceramic dielectric material powder.
[0057] (2) Preparation of MLCC samples: Take the ceramic dielectric material powder obtained by the above method, make it into a slurry, cast it into a 1.2μm diaphragm, and then form a green body with a certain shape and size through electrode printing, lamination, pressing, and cutting. Among them, nickel paste is used as the internal electrode, and the number of layers is 600. The green sheet is sintered for 2 to 4 hours at 1220℃~1280℃ in a reducing atmosphere (1% H2+99% N2), then reduced to 950℃~1100℃ for reoxidation treatment, and then reduced to 25℃ to complete sintering to form a monolithic structure porcelain body. Subsequently, copper paste is applied to both ends of the porcelain body by copper dipping, and then sintered to form a copper electrode firmly bonded to the porcelain body, and then a nickel layer is electroplated on the surface of the copper electrode, and a tin layer is electroplated for the second time to obtain an MLCC sample.
[0058] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0059] Example 1
[0060] In this embodiment, the particle size of the main material BaTiO3 powder is 200nm, the sintering temperature in the reducing atmosphere is 1220°C, the time is 2h, and the temperature is lowered to 950°C for re-oxidation treatment for 2h.
[0061] Table 1 Formula table of Example 1
[0062]
[0063]
[0064] Table 2 Performance test results of Example 1
[0065]
[0066] Example 2
[0067] In this embodiment, the particle size of the main material BaTiO3 powder is 200nm, the sintering temperature in the reducing atmosphere is 1220°C, the time is 2h, and the temperature is lowered to 950°C for re-oxidation treatment for 2h.
[0068] Table 3 Formula table of Example 2
[0069]
[0070] Table 4 Performance test results of Example 2
[0071]
[0072] Example 3
[0073] In this embodiment, the particle size of the main material BaTiO3 powder is 200nm, the sintering temperature in the reducing atmosphere is 1220°C, the time is 2h, and the temperature is lowered to 950°C for re-oxidation treatment for 2h.
[0074] Table 5: Formula of Example 3
[0075]
[0076] Table 6 Performance test results of Example 3
[0077]
[0078] As shown in Tables 2, 4 and 6, the barium titanate ceramic dielectric material prepared by the above process can form an adjustable system ceramic dielectric material with a dielectric constant between 2300 and 3000 at 25°C within a temperature range of 1220°C to 1280°C by adjusting the ratio of the main body and the modified additive.
[0079] Figures 1 to 3 The scanning electron microscope images and grain size distribution diagrams of the MLCC sample ceramic grains prepared in Examples 1 to 3. It can be seen from the figure that the samples prepared in Examples 1 to 3 of the present invention have good density, no obvious holes, and regular distribution of ceramic grain sizes, with average grain sizes of 339nm, 312nm, and 288nm, respectively.
[0080] Figures 4 to 6 The EDS line scan Ho concentration distribution diagrams of the MLCC samples prepared in Examples 1 to 3 are shown. As can be seen from the figure, the Ho element of the sample prepared in Example 3 of the present invention is concentrated in the shell layer, the concentration reaches 0.33%, and the shell layer thickness reaches 100nm.
[0081] Figures 8-9 The dielectric constant-temperature relationship curves of the MLCC samples prepared in Examples 1 to 3 and the raw material high-purity BaTiO3 powder are shown in the figure. It can be seen from the figure that the sample prepared in the embodiment of the present invention improves the dielectric constant of the raw material high-purity BaTiO3 powder and stabilizes the influence of the drastic change of the dielectric constant caused by temperature.
[0082] Fig.10 : is the TCC curve of the prepared MLCC sample. It can be seen from the figure that the samples prepared in the embodiments of the present invention show high stability, especially embodiment 3.
[0083] Fig.11 The dielectric constant change of the prepared MLCC sample measured under AC bias environment. It can be seen from the figure that the example sample also has high stability under bias environment.
[0084] In order to expand the application field, the present invention also tests the complex impedance spectrum test of the samples prepared in Examples 1 to 3, and the calculation results of the shell activation energy are shown in Figures 12-14 As can be seen from the figure, with the increase of doping concentration, the conductivity activation energy of the shell gradually increases, indicating that oxygen vacancies are more difficult to generate.
[0085] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent transformation made by using the contents of the present invention description and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A co-doped barium titanate ceramic dielectric material, characterized in that: The co-doped barium titanate ceramic dielectric material uses BaTiO3 as the main material, and the addition amount of the main material is 95-96 mol%; uses SiO2, MgO, MnO and Ho2O3 as doping materials, and the total addition amount of the doping materials is 4-5 mol%.
2. The co-doped barium titanate ceramic dielectric material according to claim 1, characterized in that: The particle size of the main material BaTiO3 is 150-200nm.
3. The co-doped barium titanate ceramic dielectric material according to claim 1, characterized in that: Based on the co-doped barium titanate ceramic dielectric material, the added amount of SiO2 is 1 to 3 mol%; Preferably, the addition amount of MgO is 1 to 3 mol%; Preferably, the added amount of MnO is 0.1-0.5 mol%.
4. The co-doped barium titanate ceramic dielectric material according to claim 1, characterized in that: Based on the co-doped barium titanate ceramic dielectric material, the added amount of Ho2O3 is 1 to 1.4 mol%.
5. Use of the co-doped barium titanate ceramic dielectric material according to any one of claims 1 to 4 in electronic packaging; Preferably, use in semiconductor packaging; Preferably, the invention is used in the preparation of multilayer ceramic capacitors.
6. A multilayer ceramic capacitor made of the co-doped barium titanate ceramic dielectric material according to any one of claims 1 to 4.
7. The method for preparing a multilayer ceramic capacitor according to claim 6, characterized in that: The following steps are involved: The co-doped barium titanate ceramic dielectric material is sintered in a reducing atmosphere; cooled and then oxidized; wherein the sintering temperature is 1220-1280°C, and the cooling and then oxidized temperature is 950-1100°C.
8. The preparation method according to claim 7, characterized in that: The grain size of the ceramic dielectric of the multilayer ceramic capacitor is 250-330 nm.
9. The preparation method according to claim 8, characterized in that: The crystal grains of the ceramic medium are of a "core-shell" structure, and the shell concentration of the Ho element in the "core-shell" structure is 0.15% to 0.33%.
10. The preparation method according to claim 9, characterized in that: The thickness of the Ho element shell in the "core-shell" structure is 50 to 100 nm.
Citation Information
Patent Citations
Chemical coating prepared base metal internal electrode multi-layer ceramic chip capacitor dielectric material
CN101183610A
Dielectric ceramic and multilayer ceramic capacitor
WO2009145001A1
Cited By
BaTiO3-based high dielectric ceramic with positive temperature coefficient at low temperature