Composite thermoformed tableware and its manufacturing method
A composite thermoforming process for tableware using layered materials with adhesives or self-adhesive properties and an oil-repellent coating addresses the complexity and cost of pulp molding, producing durable and eco-friendly tableware with enhanced strength and functionality.
Patent Information
- Application Number
- JP2023507408
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-14
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-10-14
Smart Images

Figure 0007564604000015 
Figure 0007564604000016 
Figure 0007564604000017
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of tableware, and more particularly to a composite thermoformed tableware and method of making same. [Background technology]
[0002] Pulp molded tableware is a popular tableware in the market in recent years, and has advantages and characteristics to replace some plastic tableware. It is an environmentally friendly material that is widely used in food packaging. However, the production process of pulp molded tableware is complicated, and generally, raw materials need to be crushed to form a pulp slurry solution with a certain concentration, water is sucked by a vacuum system to form a wet blank, and the wet blank is dried by a high-temperature hot press to form a dry product. Pulp molded tableware has high production costs and needs to combine many processes, such as vacuum pulp suction and high-pressure dry molding. And the thickness and strength of pulp molded tableware have an important impact on the use performance of pulp molded tableware. If the thickness and strength cannot meet the requirements, the pulp molded tableware will be easily crumbled and difficult to put food in when used.
[0003] Plastic tableware is a material commonly used in the catering industry and can come into direct contact with food. With the continuous increase in environmental awareness, people are aware that most of the plastic tableware used on the market, such as PP, PET, PE, etc., are not biodegradable, and the production costs of most plastic tableware are high. At present, there are also tableware made of degradable plastics, such as PLA tableware, which has industrial degradability, but its price is high and its market usage rate is relatively low. Summary of the Invention [Problem to be solved by the invention]
[0004] SUMMARY OF THE PRESENT DISCLOSURE ... The first object of the present invention is to provide a method for manufacturing a composite thermoformed tableware which has a simple manufacturing process, low cost, and easy control over thickness and strength.
[0005] A second object of the present invention is to provide a composite thermoformed tableware manufactured by the above manufacturing method. [Means for solving the problem]
[0006] In order to achieve the above-mentioned first objective, the manufacturing method of composite thermoformed tableware of the present invention includes sequentially carrying out a preheating step, a compounding step and a thermoforming step, wherein the preheating step includes heating multiple layers of molding material at a temperature of 35°C to 150°C, the molding material including one or at least two of paper, plastic and inorganic layers, the compounding step includes stacking the preheated molding material to form a composite material, and the thermoforming step includes hot pressing the composite material at a temperature of 80°C to 150°C and a pressure of 0.05MPa to 0.5MPa to form a three-dimensional body.
[0007] As can be seen from the above solution, the tableware is formed into a composite structure by thermoforming multiple layers of the same or different materials, and the obtained tableware has a higher thickness and higher strength; in the pre-heating step, the heating makes the self-adhesive material viscous, which can bond with other molding materials; or the heating reduces the moisture of the composite obtained, which improves the liquid absorption of the composite, and the adhesive can easily bond the composite; the manufacturing method directly obtains the product by thermoforming after pre-heating, and the surface of the product is smooth and wrinkle-free; and the operation process is simple, does not require complicated steps, and better controls the production cost.
[0008] As a further solution, the molding material has self-adhesive properties, and the molding material is in a semi-molten state in the preheating step, and adheres to other molding materials in the semi-molten state in the combining step.
[0009] As can be seen, the pre-heating step causes the self-adhesive molding material to become viscous, allowing it to more easily and quickly bond and laminate with other molding materials to form a composite structure.
[0010] As a further solution, in the preheating step, an adhesive is applied between two adjacent molding materials, the adhesive comprising 20%-50% homopolyacrylate and 50%-80% silica pigment by weight, or the adhesive comprising 50%-95% PVA and 5%-50% starch by weight, and the amount of adhesive used is 3 g / m 2 ~15g / m 2 It is.
[0011] As can be seen, the non-stick molding material is bonded with an adhesive to form a composite structure, ensuring the thickness of the product while also ensuring the adhesive strength of the composite material and avoiding delamination in the final tableware product.
[0012] In a further solution, after the thermoforming step, an oil-repellent layer is applied to the inner and outer surfaces of the three-dimensional body, the oil-repellent layer comprising, in mass %, 1%-50% starch, 50%-98% polyacrylate emulsion and 1%-3% alkyl ketene dimer emulsion, and the application amount of the oil-repellent layer is 0.1 g / m 2 ~2g / m 2 It is.
[0013] As can be seen, by adding an oil-repellent layer, the tableware has good water and oil repellency, which can avoid the tableware leaking when heating the tableware containing food. In addition, the oil-repellent layer does not contain fluorine and does not contain PFAS components, which better meets food safety requirements and is environmentally friendly.
[0014] As a further solution, the manufacturing method includes a drying step, which is performed between the preheating step and the thermoforming step, and the drying step dries the composite material, and the drying temperature is 100℃-200℃.
[0015] As can be seen, by performing the drying step before the thermoforming step, the moisture content of the composite can be better controlled and the liquid absorption of the composite can be improved, so that the composite can absorb the adhesive more uniformly, ensure the interlayer adhesive strength of the composite, and improve the body forming rate.
[0016] As a further solution, the composite thickness of the three-dimensional body is 100μm~10mm, the bending strength of the three-dimensional body is 0.9kgf~2.0kgf, and the interlayer bonding strength of the three-dimensional body is 120J / m 2 Greater than.
[0017] As can be seen, tableware with this thickness and strength can ensure that the daily use performance of the tableware meets the requirements of consumers and provides a better usage experience.
[0018] As a further solution, the manufacturing method is carried out by a composite machine, the composite machine includes a conveying mechanism, a preheating area, a composite area and a thermoforming area, the conveying mechanism includes at least two unwinding devices, the preheating area includes at least two heating rollers, the composite area includes a plurality of press rollers, the thermoforming area includes a molding device, the molding material is conveyed to the preheating area by the unwinding device, the heating rollers heat the molding material, the press rollers combine the multiple layers of the molding material, and the molding device thermoforms the combined molding material.
[0019] As can be seen, the composite machine can realize the automatic production of tableware, further making the tableware manufacturing process easier and effectively improving production efficiency.
[0020] In order to achieve the second object of the present invention, a composite thermoformed tableware according to the present invention is manufactured by the manufacturing method described above, wherein the tableware comprises at least two layers of molding material, the molding material being laminated to form a composite structure, and the molding material comprises one or at least two of paper, plastic and inorganic material.
[0021] As a further solution, an adhesive is provided between two adjacent layers of molding material, the adhesive comprising 20% to 50% by weight of homopolyacrylate and 50% to 80% by weight of silica pigment, or the adhesive comprising 50% to 95% by weight of PVA and 5% to 50% by weight of starch, and the amount of adhesive used is 3 g / m 2 ~15g / m 2The oil-repellent layer is applied to the inner and outer surfaces of the tableware, and the oil-repellent layer contains, by mass%, 1% to 50% starch, 50% to 98% polyacrylate emulsion, and 1% to 3% alkyl ketene dimer emulsion, and the application amount of the oil-repellent layer is 0.1 g / m 2 ~2g / m 2 It is.
[0022] In a further solution, the food container includes a handle and a body portion, the handle and the body portion being integrally molded and connected, and an internal arc being formed at a corner between the handle and the body portion. As can be seen, the formation of an inner arc at the corner between the handle and the body portion prevents cracks from forming in the molded product at the location of the inner arc. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a schematic diagram of a composite structure of a first embodiment of an environmentally friendly composite thermoformed tableware according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a composite structure of a second embodiment of the environmentally friendly composite thermoformed tableware according to the present invention. [Diagram 3] FIG. 3 is a schematic diagram of a composite structure of a third embodiment of the environmentally friendly composite thermoformed tableware according to the present invention. [Figure 4] FIG. 4 is a schematic diagram of a composite structure of a fourth embodiment of the environmentally friendly composite thermoformed tableware according to the present invention. [Diagram 5] FIG. 5 is a front view of the eco-friendly composite thermoformed tableware according to the present invention in the form of a spoon. [Figure 6] FIG. 6 is a front view of the eco-friendly composite thermoformed tableware according to the present invention in the form of a fork. [Figure 7] FIG. 7 is a front view of the eco-friendly composite thermoformed tableware of the present invention in the form of a knife. [Figure 8] FIG. 8 is a flow chart of an embodiment of a method for manufacturing an environmentally friendly composite thermoformed tableware according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will now be further described with reference to the drawings and examples.
[0025] The composite thermoformed tableware comprises at least two layers of molding material, which are laminated to form a composite structure, and the molding material comprises one or at least two of paper, plastic and inorganic material. In the manufacturing process, if the molding material has self-adhesive properties, the molding material is preheated to make the molding material viscous, which makes it easy to bond with other molding materials to form a composite structure. If the molding material does not have self-adhesive properties, an adhesive is provided between two adjacent layers of molding material, and the adhesive comprises 20%-50% homopolyacrylate and 50%-80% silica pigment by mass, or the adhesive comprises 50%-95% PVA and 5%-50% starch by mass, and the amount of adhesive used is 3g / m2. 2 ~15g / m 2 An oil-repellent layer is applied to the inside and outside surfaces of the tableware, and the oil-repellent layer contains, by mass%, 1% to 50% starch, 50% to 98% polyacrylate emulsion, and 1% to 3% alkyl ketene dimer emulsion AKD, and the coating amount of the oil-repellent layer is 0.1 g / m 2 ~2g / m 2 It is.
[0026] 1, the tableware 1 of the first embodiment includes a first molding material 11, a second molding material 12, and a third molding material 13, the first molding material 11, the second molding material 12, and the third molding material 13 are vertically laminated layer by layer, the molding material of the second molding material 12 located in the middle layer has self-adhesive properties, and the molding materials of the adjacent layers are directly adhered. An oil-repellent layer 14 is applied to the inner and outer surfaces of the tableware, respectively.
[0027] 2, the tableware of the second embodiment includes a first molding material 21, a second molding material 22 and a third molding material 23, the first molding material 21, the second molding material 22 and the third molding material 23 are vertically laminated layer by layer, the second molding material 22 located in the middle layer has self-adhesive properties, and the molding materials of the adjacent layers are directly adhered. There is no oil-repellent layer on the inner and outer surfaces of the tableware.
[0028] 3, the tableware of the third embodiment includes a first molding material 31, a second molding material 31, and a third molding material 31, and the first molding material 31, the second molding material 32, and the third molding material 33 are vertically laminated layer by layer. None of the molding materials of each layer has self-adhesive properties, and there is an adhesive layer 34 between the molding materials of the adjacent layers. An oil-repellent layer 35 is applied to the inner and outer surfaces of the tableware, respectively.
[0029] 4, the tableware of the fourth embodiment includes a first molding material 41, a second molding material 42, and a third molding material 43, which are vertically laminated layer by layer. None of the molding materials of each layer has self-adhesive properties, and there is an adhesive layer 44 between the molding materials of adjacent layers. No oil-repellent layer is applied to the inner and outer surfaces of the tableware.
[0030] The tableware structures of the above first to fourth embodiments can be used for different types of tableware, and can be used in direct contact with dry food, wet food, and oily food. In the manufacturing process of the tableware, it is possible to select whether or not to apply an oil-repellent layer to the three-dimensional body based on the final performance of the tableware. If the tableware is not required to have a water- and oil-repellent effect, there is no need to apply an oil-repellent layer to the three-dimensional body, and if the tableware is required to have a water- and oil-repellent effect, an oil-repellent layer is applied to the three-dimensional body.
[0031] Referring to FIG. 5, the tableware may be a spoon, including a handle 51 and a body 52, the handle 51 and the body 52 are integrally molded and connected, and a corner 53 is formed between the handle 51 and the body 52, the corner 53 is an inner arc, and the inner arc is concave toward the tableware. The inner arc having a certain radius of curvature is formed between the handle 51 and the body 52, so as to avoid the formation of cracks at the position of the inner arc of the product after molding. Referring to FIG. 5, when the tableware is a spoon, the body 52 is a concave support block with a substantially elliptical shape, which can hold a small amount of liquid and solid. Referring to FIG. 6, when the tableware is a fork, the body 52 is fork-shaped, and the corner 53 between the handle 51 and the body 52 forms an inner arc. Referring to FIG. 7, when the tableware is a knife, the body 52 is formed with a plurality of sawtooths 54, and the corner 53 between the handle 51 and the body 52 forms an inner arc. In addition to spoons, forks and knives, the tableware may also be bowls, plates, flat plates, etc.
[0032] The molding material is selected from one or at least two of paper, plastic, and inorganic material, and plastic includes normal plastic and bioplastic, therefore, the molding material can be selected from one or at least two of paper, normal plastic, bioplastic, and inorganic material. The main material of paper is plant fiber, and paper, bioplastic, and inorganic material are degradable and environmentally friendly. Preferably, when one of the molding materials is normal plastic, the other one of the molding materials is a degradable material.
[0033] The specific index characteristics of the paper are shown in Table 1.
[0034] JPEG0007564604000001.jpg62170
[0035] In Table 1, the number of layers of paper is 1-5 layers, so that in the tableware, one layer of molding material made of paper has its own structure formed by laminating 1-5 layers of paper, which further ensures the thickness and strength of the tableware. The molding material for manufacturing tableware can be purchased as a finished product on the market, and since the finished product has 1-5 layers of paper, the molding material itself laminated in multiple layers can be purchased and then composited and laminated again, which improves the strength of the tableware and makes the manufacturing process easier.
[0036] The paper may comprise one or two of a first plant fiber and a second plant fiber, the first plant fiber being one of wood pulp, bagasse pulp and wheat straw pulp, and the second plant fiber being one of reed pulp, bamboo pulp and palm pulp.
[0037] The specific index characteristics of bioplastics are shown in Table 2.
[0038] JPEG0007564604000002.jpg48170
[0039] The bioplastic of each layer can be selected from one of PLA, PBAT, PBS or PBSA, and the bioplastic has biodegradability, making the resulting tableware more environmentally friendly.
[0040] The specific index characteristics of common plastics are shown in Table 3.
[0041] JPEG0007564604000003.jpg48170
[0042] The specific index characteristics of inorganic materials are shown in Table 4.
[0043] JPEG0007564604000004.jpg43170
[0044] The inorganic material is consolidated into a plate during the manufacturing process of the dishware, making it easier for the inorganic material to adhere to other molding materials.
[0045] If one of the molding materials of the tableware has self-adhesive properties, adjacent layers can be bonded without using adhesives. Self-adhesive molding materials include PLA, PBAT, PE, PP, PET, PVDC, PBS, etc.
[0046] When the molding material of each layer does not have self-adhesiveness, an adhesive is provided between two adjacent layers of molding material, and the adhesive plays the role of adhesion and bonds the two adjacent layers of molding material. The adhesive contains, by mass%, 20% to 50% homopolyacrylate and 50% to 80% silica pigment, and the amount of adhesive used is 3 g / m 2 ~15g / m 2 Preferably, the adhesive contains 30% homopolyacrylate and 70% silica pigment, and the adhesive loading is 8 g / m 2 In another embodiment, the adhesive comprises, by weight, 50% to 95% PVA and 5% to 50% starch.
[0047] Specific index characteristics of the adhesive are shown in Table 5.
[0048] JPEG0007564604000005.jpg23170
[0049] The oil-repellent layer contains, by mass%, 1% to 50% starch, 50% to 98% polyacrylate emulsion, and 1% to 3% alkyl ketene dimer emulsion, and the coating amount of the oil-repellent layer is 0.1 g / m 2 ~2g / m 2 Preferably, the oil repellent layer contains 20% to 50% starch, 48% to 78% polyacrylate emulsion and 2% alkyl ketene dimer emulsion, and the coating amount of the oil repellent layer is 1 g / m 2 The oil-repellent layer may be provided simultaneously on the inner and outer surfaces of the tableware.
[0050] The specific index characteristics of starch in the oil repellent layer are shown in Table 6.
[0051] JPEG0007564604000006.jpg18170
[0052] The specific index characteristics of the polyacrylate emulsion in the oil repellent layer are shown in Table 7.
[0053] JPEG0007564604000007.jpg50170
[0054] The specific index characteristics of alkyl ketene dimer emulsion (AKD) in the oil repellent layer are shown in Table 8.
[0055] JPEG0007564604000008.jpg54170
[0056] Referring to FIG. 8, the manufacturing method of the composite thermoformed tableware of the present invention includes a preheating step, an adhesive application step, a compounding step, a finishing step, a drying step, a die-cutting step, a thermoforming step, and an oil-repellent layer application step in sequence. The composite thermoformed tableware of the present invention is compounded by a compounding machine, and the compounding machine is provided with a conveying mechanism, a preheating area, an adhesive application area, a compounding area, a finishing area, a drying area, a die-cutting area, and a thermoforming area corresponding to each step. The conveying mechanism includes at least two rewinding devices, and the reel-shaped molding material is conveyed by rolling of the rewinding device. The adhesive application area includes a plurality of application rollers, and adhesive is applied to the application roller. The compounding area includes one or more press rollers, and the multiple layers of molding material pass between the press rollers. The finishing area includes a plurality of polishing devices. The drying area includes a plurality of drying devices. The die-cutting area includes a die-cutting device, and the die-cutting device is used for cutting the composite material. The thermoforming area includes a molding device, and the molding device hot-presses the composite material of a certain size.
[0057] Specifically, the preheating step is to convey the molding materials of the multiple layers to the preheating area by the multiple unwinding devices, and one layer of the molding material corresponds to one unwinding device. In the preheating area, the surface of each layer of the molding material is heated by the heating roller at a temperature of 35°C to 150°C, and heated to a set temperature of 100°C to 200°C, the heating temperature can be adjusted according to the material quality of the molding material, and preferably heated to a set temperature of 150°C, and the heating method can be hot oil heat exchange or steam heat exchange.
[0058] If the molding material has self-adhesiveness, there is no need to carry out the adhesive application step, and after the preheating step, the surface of the molding material is in a semi-molten state, and the compounding step is carried out directly on the molding material.
[0059] If the molding material does not have self-adhesiveness, it is necessary to carry out an adhesive application step on the molding material before the compounding step. The adhesive application step is specifically performed by applying an adhesive to the outer surface of a first application roller, bringing the adhesive surface of the composite material into contact with the outer surface of the first application roller, applying the adhesive to the adhesive surface of the composite material, and bonding the adhesive surface and other molding materials by the adhesive.
[0060] Specifically, the compounding step is to bond the multiple layers of molding material under the pressure of the press roller when the multiple layers of molding material pass through the press roller to form a composite material. In the compounding step, the number of layers of molding material may be 2 to 10 layers, the conveying speed of the press roller is 30 m / min to 150 m / min, and the pressing pressure of the press roller is 10 psi to 200 psi. The thickness of the composite material is 100 μm to 10 mm, and the interlayer bonding strength of the composite material is greater than 120 J / m2. The adhesive contains 20% to 50% homopolyacrylate and 50% to 80% silica pigment, and the amount of adhesive used is 3 g / m2. 2 ~15g / m 2 Or the adhesive comprises 50%-95% PVA and 5%-50% starch.
[0061] The finishing step specifically involves performing a sanding or printing action on the composite by a finishing tool while the composite is in the finishing area.
[0062] The drying step is specifically to dry the composite material in a drying area, the drying temperature is 100°C to 200°C, and the heating method is hot oil heat exchange or steam heat exchange.
[0063] Specifically, the die-cutting step involves cutting the composite material with a die-cutting device to form a number of small pieces having a certain size.
[0064] Specifically, the thermoforming step is performed by cutting the composite material to a required size in the die-cutting step, and then the composite material enters the thermoforming area, where a molding device of a predetermined shape, such as a mold of a specific shape, is used to perform hot press molding to form a three-dimensional body. In the thermoforming step, the hot press speed is 60pcs / min, the hot press temperature is 80°C to 150°C, the hot press pressure is 0.05MPa to 0.5MPa, the hot press time is 0.5s to 2s, and the heating method is electric heating. Preferably, the hot press temperature is 100°C, the hot press pressure is 0.15MPa, and the hot press time is 1.5s.
[0065] A body having a three-dimensional shape is obtained through a thermoforming step. Depending on the final function of the tableware, an oil-repellent layer can be applied to the tableware to give the tableware a water- and oil-repellent effect, and the application of the oil-repellent layer is not necessary. Specifically, the oil-repellent layer application step involves immersing the body having a three-dimensional shape in a container containing an oil-repellent agent to form a coating layer on the inner and outer surfaces of the body. The oil-repellent layer contains, by mass, 20% to 50% starch, 48% to 78% polyacrylate emulsion, and 2% alkyl ketene dimer emulsion, and the coating amount of the oil-repellent layer is 1 g / m2. 2 After the application of the oil repellent layer is completed, the tableware to which the oil repellent has been applied is dried at a drying temperature of 100°C to 180°C for a drying time of 5s to 10s.
[0066] Referring to FIG. 8, after the preheating and compounding steps are completed, the composite can be directly subjected to die-cutting and thermoforming steps.
[0067] The performance of the composite thermoformed tableware of the present invention is demonstrated by detecting its water resistance, oil and grease resistance, bending resistance and interlayer bonding strength.
[0068] The water resistance test involves testing the time that tableware can withstand immersion in water at 85°C. The specific test method is to immerse the tableware in water at 85°C, remove it at regular intervals, and observe the penetration status of the tableware. If penetration occurs, the immersion time is considered to be the time that the tableware can withstand immersion.
[0069] The oil and grease resistance test involves testing the time that tableware can withstand immersion in 85°C oil.The specific test method is to immerse the tableware in 85°C oil, remove it at regular intervals, and observe the state of penetration into the tableware.If penetration occurs, that immersion time is considered to be the time that the tableware can withstand immersion.
[0070] The bending resistance test kgf is used to indicate the maximum pressure that the tableware can withstand, and the higher the value, the better the product's ability to withstand bending and breaking. For the bending resistance test before immersion in water, a load is continuously applied to the tableware, and the weight of the load on the tableware when the tableware bends is the maximum pressure the tableware can withstand. For the bending resistance test after immersion in water, the maximum pressure value that the tableware can withstand after immersion in water for 10 minutes is tested.
[0071] The interlayer bond strength of a product is used to indicate the adhesive strength between adjacent layers of tableware, and the higher the value, the stronger the adhesive strength between adjacent layers of the product and the higher the resistance to delamination. The test method for the interlayer bond strength of a product can be in accordance with the test method set forth in the US paper industry international standard TAPPI T569.
[0072] The present invention will now be further described with reference to specific examples, so that the present invention may be better understood.
[0073] The present invention provides 16 examples and 5 comparative examples, the manufacturing methods of the 16 examples are basically the same, and the differences are shown in the following tables. The selection of molding material for each layer of Examples 1 to 10, and the ratio of adhesive and oil-repellent layer components are shown in Table 9, the selection of molding material for each layer of Examples 11 to 13, and the ratio of adhesive and oil-repellent layer components are shown in Table 10, the selection of molding material for each layer of Examples 14 to 16, and the ratio of adhesive and oil-repellent layer components are shown in Table 11, and the material selection of Comparative Examples 1 to 5 are shown in Table 12. The number of adhesive layers in the above tables is not equal to the number of adhesive layers, because some molding materials have self-adhesive properties and do not require adhesive between the molding materials having self-adhesive properties and other molding materials, for example, the adhesive g / m 2 As shown in the example where is 0.
[0074] JPEG0007564604000009.jpg67170
[0075] JPEG0007564604000010.jpg86170
[0076] JPEG0007564604000011.jpg74170
[0077] JPEG0007564604000012.jpg19170
[0078] The tableware of Examples 1 to 16 and Comparative Examples 1 to 5 were tested.
[0079] Table 13 shows the performance test results of the tableware of Examples 1 to 16 and the tableware of Comparative Examples 1 to 5.
[0080] JPEG0007564604000013.jpg147170
[0081] As can be seen from Tables 9 to 13, the tableware of Example 4 and Example 5 are compared, and the number of layers of the tableware of Example 4 and Example 5 is different, that is, 3 layers in Example 4 and 4 layers in Example 5. The tableware of Example 10 and Example 13 are compared, and the number of layers of the tableware of Example 10 and Example 13 is different, that is, 3 layers in Example 10 and 4 layers in Example 13. The tableware of Example 15 and Example 16 are compared, and the number of layers of the tableware of Example 15 and Example 16 is different, that is, 3 layers in Example 15 and 4 layers in Example 16. The water resistance and oil resistance of the tableware having a four-layer molding material are basically the same as the water resistance and oil resistance of the tableware having a three-layer molding material, and the bending resistance of the tableware having a four-layer molding material is better than the bending resistance of the tableware having a three-layer molding material, but the interlayer bonding strength of the tableware having a three-layer molding material is better than the interlayer bonding strength of the tableware having a four-layer molding material. Therefore, the interlayer strength of the tableware having a three-layer molding material is better, and it is preferable that the tableware has a three-layer molding material.
[0082] Comparing Example 10 and Example 13, the amount of adhesive used is different in the two examples. By increasing the amount of adhesive applied, the interlayer bonding strength of the product can be increased, and at the same time, the water resistance and oil resistance of the product can be improved. The adhesive amount of 8g / m 2 The coating amount is based on the stable parameters that the coating production equipment can provide.
[0083] The tableware of Examples 6 to 9 do not have an oil-repellent layer, and when the tableware of Examples 6 to 9 are compared with the tableware of Example 4, the bending resistance of the tableware without an oil-repellent layer is clearly lower than the bending resistance of the tableware with an oil-repellent layer, which explains why the oil-repellent layer can reduce leakage from the tableware.
[0084] As a result of comparing Example 1 with Example 3, Example 2 with Example 4, and Example 14 with Example 15, it was found that by increasing the proportion of starch used in the oil repellent layer, the bending resistance of the product can be increased, but if the proportion is increased too much, the water resistance of the product decreases. An appropriate amount of use can achieve both of these performance properties.
[0085] A comparison of Examples 1-16 with Comparative Example 1 shows that the tableware of Examples 1-16 have high rigidity and flex resistance and interlayer bonding strength, and are superior to ordinary single-ply paperboard tableware on the market. A comparison of Examples 1-16 with Comparative Examples 2-4 shows that the rigidity and flex resistance of the tableware of Examples 1-16 before immersion in water is equivalent to that of conventional plastic tableware, and the performance of some Examples is superior to that of conventional plastic tableware, indicating that the tableware of the Examples can be used as disposable tableware to replace conventional plastic tableware. A comparison of Examples 1-16 with Comparative Example 5 shows that the decrease rate of rigidity and flex resistance of the tableware of Examples 1-16 before and after immersion in water is lower than that of conventional paper molded tableware, and the strength stability is better.
[0086] Furthermore, the tableware of Example 4 was compared with the tableware of Comparative Examples 1 to 5, and the improvement in performance is shown in Table 14.
[0087] JPEG0007564604000014.jpg101170
[0088] As can be seen from Table 14, the composite thermoformed tableware of Example 4 has significantly improved performance in each performance area compared to conventional tableware, and has good biodegradability and can be composted at home.
[0089] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention, and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for producing a composite thermoformed tableware, comprising: The manufacturing method includes sequentially performing a preheating step, a compounding step, and a thermoforming step; The preheating step includes heating a plurality of layers of molding material at a temperature of 35° C. to 150° C., the molding material including one or at least two of a paper, a plastic, and an inorganic layer; The compounding step forms a composite material by stacking the preheated molding material, the thermoforming step includes hot pressing the composite at a temperature of 80° C. to 150° C. and a pressure of 0.05 MPa to 0.5 MPa to form a three-dimensional shaped body; In the preheating step, an adhesive is applied between two adjacent molding materials, the adhesive comprising 20% to 50% homopolyacrylate and 50% to 80% silica pigment by mass, or the adhesive comprising 50% to 95% PVA and 5% to 50% starch by mass, and the amount of the adhesive is 3 g / m 2 ~15g / m 2 is A method for producing a composite thermoformed tableware.
2. 2. The method for manufacturing a composite thermoformed tableware according to claim 1, wherein the molding material has self-adhesiveness, and the molding material is in a semi-molten state during the preheating step and adheres to other molding materials.
3. After the thermoforming step, an oil repellent layer is applied to the inner and outer surfaces of the three-dimensional body, the oil repellent layer comprising, by weight, 1% to 50% starch, 50% to 98% polyacrylate emulsion, and 1% to 3% alkyl ketene dimer emulsion, and the application amount of the oil repellent layer is 0.1 g / m 2 ~2g / m 2 2. The method for producing the composite thermoformed tableware according to claim 1,
4. The manufacturing method of the composite thermoformed tableware as claimed in claim 1, characterized in that the manufacturing method includes a drying step, which is performed between the compounding step and the thermoforming step, and the drying step dries the composite material, and the drying temperature is 100°C to 200°C.
5. The three-dimensional body has a composite thickness of 100 μm to 10 mm, a bending strength of the three-dimensional body is 0.9 kgf to 2.0 kgf, and an interlayer bonding strength of the three-dimensional body is 120 J / m 2 The method for producing the composite thermoformed food container according to claim 1, characterized in that the diameter of the composite thermoformed food container is greater than 1 mm.
6. A method for manufacturing a composite thermoformed tableware described in any one of claims 1 to 5, characterized in that the manufacturing method is performed by a composite machine, the composite machine including a conveying mechanism, a preheating area, a combining area and a thermoforming area, the conveying mechanism including at least two rewinding devices, the preheating area including at least two heating rollers, the combining area including a plurality of press rollers, the thermoforming area including a molding device, the molding material being conveyed to the preheating area by the rewinding device, the heating rollers heating the molding material, the press rollers combining multiple layers of the molding material, and the molding device thermoforming the combined molding material.
7. An invention of a method for producing a composite thermoformed tableware, characterized in that the tableware is produced by the manufacturing method described in any one of claims 1 to 6.
8. the adhesive comprises, by weight, 20% to 50% homopolyacrylate and 50% to 80% silica pigment, or the adhesive comprises, by weight, 50% to 95% PVA and 5% to 50% starch; An oil-repellent layer is applied to the inner and outer surfaces of the tableware, the oil-repellent layer containing, by mass %, 1% to 50% starch, 50% to 98% polyacrylate emulsion, and 1% to 3% alkyl ketene dimer emulsion, and the application amount of the oil-repellent layer is 0.1 g / m 2 ~2g / m 2 8. The method of producing the composite thermoformed food container of claim 7,
9. The invention of the method for producing a composite thermoformed tableware as claimed in claim 7 or 8, characterized in that the tableware includes a handle and a body portion, the handle and the body portion being integrally molded and connected, and an internal arc is formed at the corner between the handle and the body portion.
Citation Information
Patent Citations
Double-color thin-wall plastic tableware and processing method thereof
CN105029984A
JP1972029461U
The spool - amine
JP1985195585U
Sheet laminated structure and its molding