Highly selective silicon oxide / silicon nitride etching with selective boron nitride or aluminum nitride deposition

By forming protective boron or aluminum nitride layers on silicon nitride using boron or aluminum-containing gases and plasma-enhanced etching, the method achieves high selectivity in removing silicon oxide without significant nitride loss, addressing the etch selectivity challenge in semiconductor manufacturing.

JP7564605B2Active Publication Date: 2024-10-09TOKYO ELECTRON LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021575312
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-20
Filing Date
2020-06-16
Publication Date
2024-10-09
Estimated Expiration
2040-06-16

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing is achieving high etch selectivity when removing silicon oxide relative to silicon nitride using plasmas containing fluorocarbon or hydrofluorocarbon gases, particularly for devices like self-aligned contacts where silicon nitride loss tolerance is minimal.

Method used

A method involving the use of boron or aluminum-containing gases to form protective boron or aluminum nitride layers on silicon nitride, followed by plasma-enhanced etching to selectively remove silicon oxide while protecting the nitride layer, utilizing etching gases like fluorocarbon and hydrofluorocarbon gases.

Benefits of technology

Enables high selectivity in etching silicon oxide relative to silicon nitride, ensuring minimal nitride loss and effective film removal, suitable for advanced semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564605000001
    Figure 0007564605000001
  • Figure 0007564605000002
    Figure 0007564605000002
  • Figure 0007564605000003
    Figure 0007564605000003
Patent Text Reader

Abstract

A method for selectively etching silicon oxide relative to silicon nitride includes exposing a substrate to a first gas that forms a first layer on the silicon oxide film and a second layer on the silicon nitride film, the first gas containing boron, aluminum, or both boron and aluminum, and exposing the substrate to a nitrogen-containing gas that reacts with the first layer to form a first nitride layer on the silicon oxide film and with the second layer to form a second nitride layer on the silicon nitride film, the second nitride layer having a thickness greater than the first nitride layer. The method further includes exposing the substrate to an etching gas that etches the first nitride layer and the silicon oxide film, the second nitride layer protecting the silicon nitride film from etching by the etching gas.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is related to and claims priority to U.S. Provisional Patent Application No. 62 / 864,378, filed June 20, 2019, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the field of semiconductor manufacturing and semiconductor devices, and more specifically to a method for selectively etching silicon oxide relative to silicon nitride. [Background technology]

[0003] The need to remove some materials with dry etching that is selective to other materials poses significant challenges in the development of advanced semiconductor technologies. Selective etching of silicon oxide to silicon nitride has many applications in semiconductor manufacturing, and preferential passivation (mainly carbon-based) has been widely considered to achieve high etch selectivity when using plasmas containing fluorocarbon (FC) or hydrofluorocarbon (HFC) gases. The need for high etch selectivity is particularly important for devices such as self-aligned contacts (SACs), which have a tight tolerance to silicon nitride loss. Summary of the Invention [Means for solving the problem]

[0004] A method for selective etching of silicon oxide relative to silicon nitride is disclosed in some embodiments. According to one embodiment, the method includes the steps of: providing a substrate including a silicon oxide film and a silicon nitride film; a1) exposing the substrate to a first gas that forms a first layer on the silicon oxide film and a second layer on the silicon nitride film, the first gas including boron, aluminum, or both; and a2) exposing the substrate to a nitrogen-containing gas that reacts with the first layer to form a first nitride layer on the silicon oxide film and reacts with the second layer to form a second nitride layer on the silicon nitride film, the thickness of the second nitride layer being greater than the thickness of the first nitride layer. The method further comprises a3) exposing the substrate to an etching gas that etches the first nitride layer and the silicon oxide film, the second nitride layer protecting the silicon nitride film from being etched by the etching gas. According to one embodiment, the method further comprises a0) exposing the substrate to an etching gas that terminates the silicon oxide film with -OH surface species and the silicon nitride film with -NH x The method further includes exposing the substrate to an H2-containing gas to terminate the surface species.

[0005] According to one embodiment, the method includes the steps of: providing a substrate including a silicon oxide film and a silicon nitride film; a1) exposing the substrate to BCl3 gas to form a first BCl3 layer on the silicon oxide film and a second BCl3 layer on the silicon nitride film; a2) exposing the substrate to NH3 gas to react with the first BCl3 layer to form a first boron nitride layer on the silicon oxide film and react with the second BCl3 layer to form a second boron nitride layer on the silicon nitride film, the thickness of the second boron nitride layer being greater than the thickness of the first boron nitride layer. The method further includes a3) exposing the substrate to plasma-excited CF4 gas to etch the first boron nitride layer and the silicon oxide film, the second boron nitride layer protecting the silicon nitride film from being etched by the etching gas. According to one embodiment, the method includes the steps of: a0) terminating a substrate with a silicon oxide film with -OH surface species and a silicon nitride film with -NH xThe method further includes exposing the substrate to an H2-containing gas to terminate the surface species. [Brief description of the drawings]

[0006] [Figure 1] 1 is a schematic process flow diagram for selective etching of silicon oxide films relative to silicon nitride films in accordance with one embodiment of the present invention. [Figures 2A-2D] 1 illustrates, in cross-sectional views, a method for selective etching of a silicon oxide film relative to a silicon nitride film, according to one embodiment of the present invention. [Diagram 3] 1 is a schematic process flow diagram for selective etching of silicon oxide films relative to silicon nitride films in accordance with one embodiment of the present invention. [Figure 4A-4E] 1 illustrates, in cross-sectional views, a method for selective etching of a silicon oxide film relative to a silicon nitride film, according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] FIG. 1 is a schematic process flow diagram of selective etching of silicon oxide films relative to silicon nitride films in accordance with one embodiment of the present invention, and FIGS. 2A-2D show, in cross-sectional views, a schematic of a method of selective etching of silicon oxide films relative to silicon nitride films in accordance with one embodiment of the present invention.

[0008] 1 and 2, a processing method according to a process flow schematic 10 includes providing at 12 a substrate 2 including a SiO2 film 200 and a Si3N4 film 220. In the example shown in FIG. 2A, the SiO2 film 200 and the Si3N4 film 220 are in the same horizontal plane, however, an embodiment of the present invention can also be applied to films that are not in the same horizontal plane, but are vertically offset. Si3N4 is the most thermodynamically stable of the silicon nitrides and is therefore the most commercially important of the silicon nitrides. However, an embodiment of the present invention can be applied to other silicon nitrides that contain Si and N as the main components, and silicon nitrides can be found in a wide range of Si and N compositions (Si x N y ). Similarly, SiO2 is the most thermodynamically stable of the silicon oxides and is therefore the most commercially important of the silicon oxides. However, an embodiment of the present invention can be applied to other silicon oxides that contain Si and O as the major components, and silicon oxides can have a wide range of Si and O compositions (Si x O y ).

[0009] The method further includes exposing the substrate 2 to a first gas 201 at 14. The first gas 201 may include boron, aluminum, or both boron and aluminum. The first gas 201 may include boron hydride, boron halide, organoaluminum compound, aluminum hydride, aluminum chloride, or combinations thereof. According to an embodiment, the first gas 201 may be selected from the group consisting of BH3, BCl3, BF3, Al(CH3)3, AlH3, AlCl3, and combinations thereof. The exposure may be performed with or without plasma excitation of the first gas 201. The exposure of the first gas 201 forms a first layer 202 (e.g., BCl3) on the SiO2 film 200 and a second layer 222 (e.g., BCl3) on the Si3N4 film 220. 2B, the first layer 202 is thinner than the second layer 222, and the former may be incomplete with voids exposing the underlying SiO2 film 200. This preferential adsorption of the first gas 201 in the Si3N4 film 220 is due to the higher adsorption energy of the first gas 201 in the Si3N4 film 220 than in the SiO2 film 200, an effect that is strongly supported in the absence of plasma excitation or when using remote plasma excitation of the first gas 201.

[0010] The method further includes exposing the substrate 2 to a nitrogen-containing gas 203 at 16. According to one embodiment, the nitrogen-containing gas 203 can be selected from the group consisting of nitrogen hydride, nitrogen halide, N2, and combinations thereof. The nitrogen hydride can include, for example, NH3, N2H4, or combinations thereof. The nitrogen halide can include, for example, NCl3. In one example, the nitrogen-containing gas 203 can be selected from the group consisting of NH3, N2H4, NCl3, N2, and combinations thereof.

[0011] The exposure may be performed with or without plasma excitation of the nitrogen-containing gas 203. The nitrogen-containing gas 203 reacts with the first layer 202 and the second layer 222 to form a first nitride layer 204 and a second nitride layer 224, respectively. The first nitride layer 204 and the second nitride layer 224 may include boron nitride, aluminum nitride, or both. As shown generally in FIG. 2C, the first nitride layer 204 may be incomplete with voids exposing the underlying SiO2 film 200. However, this is not required, and the first nitride layer may be continuous. The second nitride layer 224 has a thickness greater than the first nitride layer 204 and is at least substantially continuous in the underlying Si3N4 film 220.

[0012] In one example, the first gas 201 includes BCl3 and the nitrogen-containing gas includes NH3. The elementary reactions that form boron nitride (BN) and the volatile HCl by-product are: BCl3+NH3→BN+3HCl It can be expressed as:

[0013] The formation of boron nitride is thermodynamically favorable, and boron nitride provides strong etch protection against a variety of commonly used etch gases.

[0014] According to one embodiment, the exposure steps 14 and 16 may be performed alternately and sequentially. According to another embodiment, the exposure steps 14 and 16 may at least partially overlap in time. As indicated by process arrow 18, the exposure steps 14 and 16 may be repeated at least once until the thickness of the second nitride layer 224 is sufficient to act as an etch stop layer while the thickness of the first nitride layer 204 is not sufficient to protect the SiO2 film 200 in the subsequent etching process.

[0015] The method further includes exposing the substrate 2 to an etching gas 205 at 20, which is shown in schematic form in FIG. 2D. In general, the etching gas 205 can be selected from any gas that etches silicon oxide, boron nitride, and aluminum nitride. The etching gas 205 can be plasma excited and can include a fluorocarbon gas, a hydrofluorocarbon gas, a hydrochlorocarbon gas, a hydrochlorofluorocarbon gas, or a combination thereof. In some examples, the etching gas 205 can include CF4, CF2Cl2, CH2F2, CH4, CH3F, CHF3, C4H6, C2H4, C3H6, CH2Cl2, CH3Cl, CHCl2, CH2ClF, CHCl2F, or a combination thereof. The etching gas 205 can optionally further include Ar, He, or a combination thereof. Exposure to the etching gas 205 etches the first nitride layer 204 and the SiO2 film 200. The second nitride layer 224 is partially etched, but the Si3N4 film 220 is not etched as long as the second nitride layer 224 provides adequate protection against the etching gas 205. In one example, exposure to the etching gas 205 can be stopped before the second nitride layer 224 ceases to adequately protect the Si3N4 film 220 from etching.

[0016] Plasma excitation of the etching gas 205 can be performed in conventional commercial plasma processing systems, including inductively coupled plasma (ICP) systems, capacitively coupled plasma (CCP) systems, microwave plasma systems, remote plasma systems that generate plasma-excited species upstream from the substrate, electron cyclotron resonance (ECR) systems, and other systems.

[0017] As indicated by process arrow 22, exposure steps 14, 16, and 20 can be repeated at least once to redeposit the first nitride layer 204 and the second nitride layer 224 and further etch the SiO2 film 202. According to an embodiment shown diagrammatically in FIG. 2D, exposure to the etching gas 205 completely removes the first nitride layer 204 from the substrate 2 and etches the SiO2 film 202. According to another embodiment, exposure to the etching gas 205 can only partially remove the first nitride layer 204 and etch the SiO2 film 202 before exposure steps 14 and 16 are repeated. Once the SiO2 film 202 is properly etched, the second nitride layer 224 can be removed using a dry or wet etching process using a strong oxidizing agent.

[0018] Figure 3 is a process flow diagram of selective etching of silicon oxide films relative to silicon nitride films according to one embodiment of the present invention, and Figures 4A-4E show, in cross-sectional views, a schematic of a method of selective etching of silicon oxide films relative to silicon nitride films according to one embodiment of the present invention. The processing method in process flow diagram 30 is similar to process flow diagram 10 of Figure 1, but the former further includes a pre-treatment step of exposing the substrate to an H2-containing gas that enhances preferential formation of a first layer on the silicon nitride film relative to the silicon oxide film, thereby promoting the subsequent formation of a nitride layer on the silicon nitride film.

[0019] The process flow diagram 30 includes providing a substrate 4, at 32, comprising a SiO2 film 400 and a Si3N4 film 420, as shown generally in Figure 4A. The method then includes exposing the substrate 4 to a H2-containing gas 401, as shown generally in Figure 4B. Upon exposure to the H2-containing gas 401, the SiO2 film 400 terminates at -OH surfaces 402 and -NH x At surface 422 the Si3N4 film 420 terminates.

[0020] The method further includes exposing the substrate 4 to a first gas 403 at 36. Exposure to the first gas 403 forms a first layer 404 (e.g., BCl3) on the SiO2 film 400 and a second layer 424 (e.g., BCl3) on the Si3N4 film 420. This is shown diagrammatically in FIG. 4C.

[0021] The method further includes exposing the substrate 4 to a nitrogen-containing gas 405 at 38. The nitrogen-containing gas 405 reacts with the first layer 404 and the second layer 424 to form a first nitride layer 406 and a second nitride layer 426, respectively. According to one embodiment, the exposure steps 34, 36, and 38 can be performed alternately and sequentially. According to another embodiment, the exposure steps 34, 36, and 38 can at least partially overlap in time. As indicated by the process arrow 40, while the thickness of the first nitride layer 406 is not sufficient to protect the SiO2 film 400 in a subsequent etching process, the exposure steps 34, 36, and 38, or the exposure steps 36 and 38, can be repeated at least once until the thickness of the second nitride layer 426 is sufficient to act as an etch stop layer.

[0022] The method further includes exposing the substrate 4 to an etching gas 407 at 42, which is shown diagrammatically in FIG. 4E. Exposure to the etching gas 407 etches the first nitride layer 406 and the SiO2 film 400. The second nitride layer 426 is partially etched, but the Si3N4 film 420 is not etched as long as the second nitride layer 426 provides adequate protection against the etching gas 407. In one example, exposure to the etching gas 407 can be stopped before the second nitride layer 426 ceases to adequately protect the Si3N4 film 420 from etching.

[0023] As indicated by process arrow 44, exposure steps 34, 36, 38, and 42 can be repeated at least once to redeposit the first nitride layer 406 and the second nitride layer 426 and further etch the SiO2 film 402. According to an embodiment shown diagrammatically in FIG. 2E, exposure to the etching gas 407 completely removes the first nitride layer 406 from the substrate 4 and etches the SiO2 film 402. According to another embodiment, exposure to the etching gas 407 can only partially remove the first nitride layer 406 and etch the SiO2 film 402 before exposure steps 36, 38, and 42 or exposure steps 34, 36, 38, and 42 are repeated.

[0024] Several embodiments have been described for selective etching of silicon oxide relative to silicon nitride. The above description of the embodiments of the present invention has been presented for purposes of illustration and description. This description is not intended to be exhaustive or to limit the invention to the precise form disclosed. This description and the following claims include terms that are used for descriptive purposes only and should not be construed as limiting. Those skilled in the relevant art will appreciate that many modifications and variations are possible in light of the above teachings. Those skilled in the art will recognize various equivalent combinations and substitutions of the various components shown in the figures. It is therefore intended that the scope of the present invention be limited not by this detailed description, but rather by the claims appended hereto.

Claims

1. 1. A method for processing a substrate, comprising: Providing a substrate comprising a silicon oxide film and a silicon nitride film; a1) exposing the substrate to a first gas that forms a first layer on the silicon oxide film and a second layer on the silicon nitride film, the first gas comprising boron, aluminum, or both boron and aluminum; a2) exposing the substrate to a nitrogen-containing gas that reacts with the first layer to form a first nitride layer on the silicon oxide film and reacts with the second layer to form a second nitride layer on the silicon nitride film, the second nitride layer having a thickness greater than a thickness of the first nitride layer, and the step (a2) being performed after the step (a1); a3) adding an etching gas for etching the first nitride layer and the silicon oxide film, exposing the substrate, wherein the second nitride layer protects the silicon nitride film from etching by the etching gas; A method comprising:

2. The method of claim 1 , further comprising repeating steps a1) and a2) at least once before performing step a3).

3. 10. The method of claim 1, further comprising repeating steps a1), a2), and a3) at least once to further etch the silicon oxide film.

4. a0) terminating the silicon oxide film with —OH surface species and terminating the silicon nitride film with —NH x H terminating on surface species 2 The method of claim 1 further comprising exposing the substrate to a containing gas.

5. 5. The method of claim 4, further comprising repeating a0), a1), a2), and a3) at least one time to further etch the silicon oxide film.

6. 5. The method of claim 4, further comprising repeating a1), a2), and a3) at least one time to further etch the silicon oxide film.

7. 10. The method of claim 1, wherein the first gas comprises a boron hydride, a boron halide, an organoaluminum compound, an aluminum hydride, an aluminum chloride, or a combination thereof.

8. The first gas is BH 3 , BCl 3 , B.F. 3 , Al(CH 3 ) 3 , AlH 3 , AlCl 3 and combinations thereof.

9. The nitrogen-containing gas may be nitrogen hydride, nitrogen halide, N 2 and combinations thereof.

10. The nitrogen-containing gas is NH 3 , N 2 H 4 , NCl 3 , N 2 and combinations thereof.

11. 10. The method of claim 1, wherein the etching gas comprises a fluorocarbon gas, a hydrofluorocarbon gas, a hydrochlorocarbon gas, a hydrochlorofluorocarbon gas, or a combination thereof.

12. The etching gas is CF 4 , C.F. 2 C 2 , C.H. 2 F 2 , C.H. 4 , C.H. 3 F, C.H.F. 3 , C 4 H 6 , C 2 H 4 , C 3 H 6 , C.H. 2 C 2 , C.H. 3 Cl, CH 2 ClF, CHCl 2 F, and combinations thereof.

13. Providing a substrate comprising a silicon oxide film and a silicon nitride film; a1) A first BCl 3 A layer is formed on the silicon nitride film, and a second BCl 3 BCl forming layer 3 exposing the substrate to a gas; a2) the first BCl 3 layer to form a first boron nitride layer on the silicon oxide film, and the second BCl 3 layer to form a second boron nitride layer on the silicon nitride film. 3 exposing the substrate to a gas, wherein a thickness of the second boron nitride layer is greater than a thickness of the first boron nitride layer, and step (a2) is performed after step (a1); a3) Plasma-enhanced CF etching the first boron nitride layer and the silicon oxide film. 4 exposing the substrate to a gas, the second boron nitride layer being formed from the plasma excited CF 4 protecting the silicon nitride film from etching by a gas; A method for processing a substrate, comprising:

14. The method of claim 13, further comprising repeating steps a1) and a2) at least once before performing step a3).

15. 14. The method of claim 13, further comprising repeating a1), a2), and a3) at least one time to further etch the silicon oxide film.

16. a0) terminating the silicon oxide film with —OH surface species and terminating the silicon nitride film with —NH x H terminating on surface species 2 The method of claim 13 further comprising exposing the substrate to a containing gas.

17. 17. The method of claim 16, further comprising repeating a0), a1), a2), and a3) at least one time to further etch the silicon oxide film.

18. 17. The method of claim 16, further comprising repeating a1), a2), and a3) at least one time to further etch the silicon oxide film.

19. Providing a substrate comprising a silicon oxide film and a silicon nitride film; a1) exposing the substrate to a boron-containing gas that forms a first boron-containing layer on the silicon oxide film and a second boron-containing layer on the silicon nitride film; a2) exposing the substrate to a nitrogen-containing gas that reacts with the first boron-containing layer to form a first boron nitride layer on the silicon oxide film and reacts with the second boron-containing layer to form a second boron nitride layer on the silicon nitride film, the second boron nitride layer having a thickness greater than a thickness of the first boron nitride layer, and step (a2) being performed after step (a1); a3) exposing the substrate to an etching gas that etches the first boron nitride layer and the silicon oxide film, the second boron nitride layer protecting the silicon nitride film from etching by the etching gas; A method for processing a substrate, comprising:

20. The boron-containing gas is BH 3 , BCl 3 , B.F. 3 and combinations thereof, wherein the nitrogen-containing gas is selected from the group consisting of NH 3 , N 2 H 4 , NCl 3 , N 2 and combinations thereof, and the etching gas is selected from the group consisting of CF 4 , C.F. 2 C 2 , C.H. 2 F 2 , C.H. 4 , C.H. 3 F, C.H.F. 3 , C 4 H 6 , C 2 H 4 , C 3 H 6 , C.H. 2 C 2 , C.H. 3 Cl, CH 3 Cl, CH 2 ClF, CHCl 2 20. The method of claim 19, wherein the compound is selected from the group consisting of: F, and combinations thereof.

21. The method of claim 19, further comprising the step of: a0) exposing the substrate to an H 2 containing gas that terminates the silicon oxide film with --OH surface species and the silicon nitride film with --NH x surface species.

Citation Information

Patent Citations

  • Method of etching boron nitride

    JP1994236859A

  • Method of manufacturing dual damascene wiring

    JP2006041519A

  • Electronic device and manufacturing method of the same

    JP2012212877A

  • Formation method of boron nitride film and method of manufacturing semiconductor device

    JP2017084894A

  • Deposition device

    JP2017212246A