Bound stopper and manufacturing method thereof

The polyurethane foam bound stopper, produced using a specific composition and method, addresses mechanical strength and ride comfort issues by dispersing loads and enhancing durability, resulting in improved vehicle performance.

JP7564672B2Active Publication Date: 2024-10-09BASF INOAC POLYURETHANE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020164872
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-10-09
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Conventional bound stoppers for vehicle shock absorbers face challenges in achieving high mechanical strength, durability against fatigue, and improving ride comfort due to difficulties in controlling the reaction parameters during polyurethane foam production, leading to poor performance under repeated loads and discomfort from road unevenness.

Method used

A bound stopper made of polyurethane foam composed of a polyurethane foam composition containing a polyol component, polyrotaxane with a cyclic molecule having an active hydrogen group, and diphenylmethane diisocyanate, which is produced through a method involving mixing in a molten state and reacting with diphenylmethane diisocyanate to form a urethane prepolymer with isocyanate groups, followed by foaming to create a bound stopper.

Benefits of technology

The solution enhances mechanical strength, durability, and ride comfort by dispersing external loads effectively, preventing crosslinking destruction and providing an air spring effect, thus improving the overall performance of the vehicle's shock absorber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564672000001
    Figure 0007564672000001
  • Figure 0007564672000002
    Figure 0007564672000002
  • Figure 0007564672000003
    Figure 0007564672000003
Patent Text Reader

Abstract

To provide a bound stopper having large mechanical strength and excellent ride quality, and further capable of being manufactured easily.SOLUTION: In a polyurethane foam-based bound stopper 10, a polyurethane foam may be obtained from a composition for a polyurethane foam containing at least an isocyanate component and a foaming agent, and the isocyanate component is composed of a urethane prepolymer having, at its terminal, an isocyanate group obtained by blending diphenylmethane diisocyanate after mixing a polyol component and polyrotaxane containing an annular molecule having an active hydrogen group in its constituent in a molten state.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bound stopper that is attached to a piston rod of a shock absorber for a vehicle and a method for manufacturing the same. [Background technology]

[0002] As shown in Figure 7, a shock absorber 70 for a vehicle has a bound stopper 75 attached to a piston rod 72 of a cylinder. Reference numeral 71 denotes a cylinder body, and reference numeral 73 denotes a spring. The bound stopper 75 is made of an elastic foam molded into a bellows shape, and when the shock absorber 70 expands or contracts due to impact or vibration from the road surface and the cylinder body 71 collides with the bound stopper 75, the bound stopper 75 is compressed and deformed to absorb the impact.

[0003] The bound stopper 75 is subjected to repeated collisions with the cylinder body and the resulting compressive deformation, and therefore is required to have high mechanical strength and durability against fatigue failure and settling when subjected to repeated heavy loads.

[0004] Conventionally, as a bound stopper that aims to reduce costs while providing durability and resistance to settling under high loads and large deformations, a polyurethane foam has been proposed that is made by injecting a urethane raw material containing a polyester polyol as the polyol component and diphenylmethane diisocyanate as the isocyanate component into a mold and heating it to 70°C or higher for primary vulcanization, and then removing the molded body from the mold and heating it for secondary vulcanization, whereby the density (Da) and foam cell diameter (Ra) of the skin layer and the density (Db) and foam cell diameter (Rb) of the core satisfy specific formulas and relationships (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2015-183832 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the primary and secondary vulcanization processes must be performed so that the density (Da) and foam cell diameter (Ra) of the skin layer and the density (Db) and foam cell diameter (Rb) of the core layer satisfy specific formulas and relationships, making it difficult to control the reaction.

[0007] Furthermore, comfort (good ride quality) is required in vehicles, but with conventional bound stoppers, there is a feeling of being pushed up due to unevenness in the road surface when the vehicle is traveling, and improvement in ride quality cannot be achieved.

[0008] SUMMARY OF THE PRESENT INVETION The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a bound stopper which has high mechanical strength, can improve the ride comfort, and is easy to manufacture, and a manufacturing method thereof. [Means for solving the problem]

[0009] The invention of claim 1 relates to a polyurethane foam bound stopper to be attached to a piston rod of a vehicle shock absorber, the bound stopper comprising a polyurethane foam obtained from a polyurethane foam composition containing at least an isocyanate component and a blowing agent, the isocyanate component comprising a urethane prepolymer having an isocyanate group at a terminal thereof obtained from a polyol component, a polyrotaxane containing a cyclic molecule having an active hydrogen group as a constituent, and diphenylmethane diisocyanate.

[0010] The invention of claim 2 is characterized in that in the urethane prepolymer having an isocyanate group at its terminal, the blending amount of the polyrotaxane is 0.1 to 6.5 parts by weight per 100 parts by weight of the polyol component.

[0011] The invention of claim 3 is the same as that of claim 1 or 2, wherein the density of the polyurethane foam is 0.2 to 0.7 g / cm 3 It is characterized in that:

[0012] The invention of claim 4 relates to a method for manufacturing a bound stopper made of polyurethane foam to be attached to a piston rod of a shock absorber for a vehicle, characterized in that a polyol component and a polyrotaxane containing, in a molten state, cyclic molecules having active hydrogen groups as constituents are mixed, and then diphenylmethane diisocyanate is added to prepare a urethane prepolymer having an isocyanate group at its terminal, and a polyurethane foam composition containing at least the urethane prepolymer having an isocyanate group at its terminal and a foaming agent is injected into a mold and foamed to form a bound stopper made of the polyurethane foam. Effect of the Invention

[0013] The bound stopper of the present invention is composed of a polyurethane foam obtained from a polyurethane foam composition containing at least a urethane prepolymer having an isocyanate group at its terminal and a foaming agent. The urethane prepolymer having an isocyanate group at its terminal is obtained by mixing a polyol component and a polyrotaxane containing a cyclic molecule having an active hydrogen group in a molten state, and then adding diphenylmethane diisocyanate.

[0014] As shown in the schematic diagram of FIG. 2, in the polyrotaxane 20, an axial molecule 23 is inserted in a skewer-like manner into the opening of a cyclic molecule 21, and the axial molecule 23 has blocking groups 25 at both ends. The blocking groups 25 prevent the cyclic molecule 21 from detaching from the axial molecule 23. According to the present invention, when preparing a urethane polymer having an isocyanate group at its terminal, a hydroxyl group of a polyol component and an active hydrogen group in the cyclic molecule 21 of the polyrotaxane 20 react with diphenylmethane diisocyanate to form a urethane bond. Thereafter, a polyurethane foam is formed by a foaming reaction between a urethane prepolymer having at least an isocyanate group at its terminal and a foaming agent, and a bound stopper made of the polyurethane foam is obtained.

[0015] In the polyrotaxane 20, the cyclic molecules 21 can move relatively freely along the axial molecules 23, and in the polyurethane foam constituting the bound stopper, the urethane bonds (crosslinking points) formed in the cyclic molecules 21 of the polyrotaxane 20 can also move along the axial molecules 23 (pulley effect). Even if the polyurethane foam is repeatedly subjected to a large load from the outside, the load can be dispersed by the pulley effect, so that the crosslinking points can be prevented from being destroyed. In addition, when the cyclic molecules 21 approach each other on the axial molecules 23, an air spring effect is generated in which the cyclic molecules 21 try to keep the distance constant, and the air spring effect gives the polyurethane foam excellent restorability. Due to these actions, the polyurethane foam of the present invention can increase mechanical strength, reduce dynamic energy applied from the outside, improve durability against destruction and sagging, and improve ride comfort.

[0016] In addition, according to the present invention, when preparing a urethane prepolymer having an isocyanate group at its end, polyrotaxane is added to a polyol component in a molten state, and the polyol component and polyrotaxane are mixed in a molten state, so that the polyrotaxane can be uniformly dispersed in the polyol component. The polyol component and polyrotaxane are preferably mixed at a temperature equal to or higher than the melting point of the polyrotaxane. On the other hand, in a one-shot method in which a polyol component, a foaming agent, an isocyanate component, and the like are mixed at once and injected into a mold, the polyrotaxane, which is a solid at room temperature, needs to be melted at a temperature equal to or higher than the melting point, or dissolved or dispersed in a dispersion medium, but it becomes difficult to uniformly disperse the polyrotaxane due to differences in temperature, viscosity, and the like of each component. Furthermore, it is difficult to reliably react all the active hydrogen groups of the polyrotaxane, which is an ultra-high molecular weight compound, with the isocyanate component, so that the pulley effect and air spring effect of the polyrotaxane cannot be sufficiently obtained, and it is difficult to obtain a polyurethane foam that is excellent in mechanical strength and durability and provides a good ride comfort.

[0017] Furthermore, in the present invention, a dispersion medium such as a surfactant is not required to disperse the polyrotaxane in the polyurethane foam, and it is possible to prevent a decrease in mechanical strength and durability against breakage, settling, etc., which is caused by the dispersion medium of the polyurethane foam. When a compound having no active hydrogen groups in the molecule is used as the dispersion medium, a decrease in mechanical strength and bleeding, etc. occur, and when a compound (mono-ol) having one active hydrogen group in the molecule is used, a decrease in mechanical strength due to a decrease in crosslink density, etc. may occur.

[0018] In addition, diphenylmethane diisocyanate used in the present invention is less expensive than 1,5-naphthalene diisocyanate (NDI), and compared to NDI, it is produced in larger quantities worldwide and can be procured globally. [Brief description of the drawings]

[0019] [Figure 1] FIG. 2 is a cross-sectional view of a bound stopper according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing a structure of a polyrotaxane containing, as a constituent, a cyclic molecule having an active hydrogen group. [Diagram 3] 1A and 1B are cross-sectional views of a mold used in manufacturing the bound stopper of the present invention and a cross-sectional view of the mold during foaming. [Figure 4] 4 is a cross-sectional view of a mold during demolding in the manufacture of the bound stopper of the present invention. FIG. [Diagram 5] 1 is a table showing the compositions and physical properties of Examples 1 to 9. [Figure 6] 1 is a table showing the compositions and physical properties of Examples 10 to 16 and Comparative Examples 1 and 2. [Figure 7] FIG. 4 is a cross-sectional view showing a state in which the bound stopper is attached. BEST MODE FOR CARRYING OUT THEINVENTION

[0020] The bound stopper 10 according to one embodiment of the present invention shown in FIG. 1 is attached to a piston rod 72 of a shock absorber of a vehicle, similar to the bound stopper 75 shown in FIG.

[0021] The bound stopper 10 is made of a cylindrical polyurethane foam with a side outer peripheral surface 10a molded into a bellows shape, and has a through hole 11 formed in the center to allow the piston rod of the shock absorber to pass through. The bound stopper 10 is formed so that the upper part 10b has a larger outer diameter than the lower part 10c. The length and diameter of the bound stopper 10 are determined according to the shock absorber.

[0022] The density of the polyurethane foam constituting the bound stopper 10 (in accordance with JIS K7222:2005) is 0.2 to 0.7 g / cm 3 The density is preferably 0.2 g / cm 3 If the density is less than 0.7 g / cm3, the physical properties of the polyurethane foam will be deteriorated. 3 If it exceeds this value, the foaming pressure during foam molding of the polyurethane foam becomes too high, making molding difficult.

[0023] The tensile strength (in accordance with JIS K6251:2017) of the polyurethane foam constituting the bound stopper 10 is preferably 3.5 MPa or more.

[0024] The polyurethane foam constituting the bound stopper 10 is obtained from a polyurethane foam composition. The polyurethane foam composition contains at least an isocyanate component and a foaming agent.

[0025] The isocyanate component is composed of a urethane prepolymer having an isocyanate group at its terminal, obtained by mixing a polyol component and a polyrotaxane containing, in a molten state, cyclic molecules having active hydrogen groups as constituents, and then blending diphenylmethane diisocyanate therein.

[0026] As the polyol component, a polyester polyol is used, and a polyester polyol having an average carbon number between ester bonds of 3 to 8 is preferred. The polyester polyol having an average carbon number between ester bonds of 3 to 8 is a condensation polyester polyol or a ring-opening polyester polyol. The polyol component is polytetramethylene ether glycol (PTMG) [HO-(CH2CH2CH2CH2O) n -H] can also be used.

[0027] The condensation polyester polyol is preferably one obtained by polycondensing a diol having 2 to 6 carbon atoms between hydroxyl groups and a dicarboxylic acid having 4 to 10 carbon atoms between carboxyl groups.

[0028] Examples of diols having 2 to 6 carbon atoms between hydroxyl groups include ethylene glycol [HO-CH2CH2-OH], 1,4-butanediol [HO-(CH2)4-OH], and 1,6-hexanediol [HO-(CH2)6-OH]. Dicarboxylic acids with 4 to 10 carbon atoms between the carboxyl groups include adipic acid [HOOC-(CH2)4-COOH], suberic acid [HOOC-(CH2)6-COOH], sebacic acid [HOOC-(CH2)8-COOH], and dodecanedioic acid [HOOC-(CH2 10 The number of carbon atoms between the carboxyl groups does not include the number of carbon atoms constituting the carboxyl groups.

[0029] As the ring-opening polyester polyol, polycaprolactone diol (PCL) obtained by ring-opening polymerization of ε-caprolactone is preferable.

[0030] The weight average molecular weight (Mw) of the polyol for the urethane prepolymer having an isocyanate group at its terminal is 800 to 5000, more preferably 1000 to 3000, and the hydroxyl value is 20 to 200 mgKOH / g, more preferably 35 to 180 mgKOH / g.

[0031] The polyrotaxane containing a cyclic molecule having an active hydrogen group in its constituents is as shown in the schematic diagram of FIG. 2, and has a structure in which an axial molecule 23 is inserted in a skewer-like manner into the opening of a cyclic molecule 21 having an active hydrogen group, and the cyclic molecule 21 is prevented from being released by blocking groups 25 at both ends of the axial molecule 23. Examples of the active hydrogen group of the cyclic molecule 21 include a hydroxyl group and an amino group, and a hydroxyl group is particularly preferable. The polyrotaxane containing a cyclic molecule having an active hydrogen group in its constituents preferably has a hydroxyl value of 60 to 100 mgKOH / g, a molecular weight of the axial molecule of 10,000 to 40,000, and a total molecular weight of 150,000 to 800,000. The amount of the polyrotaxane containing a cyclic molecule having an active hydrogen group in its constituents is preferably 0.1 to 6.5 parts by weight, more preferably 0.5 to 6 parts by weight, based on 100 parts by weight of the polyol component. If it is less than 0.1 part by weight, the effect of improving physical properties cannot be obtained. If it exceeds 6.5 parts by weight, the viscosity of the urethane prepolymer becomes too high, making molding difficult.

[0032] Diphenylmethane diisocyanate (MDI) includes 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, and polymeric MDI (crude MDI). 4,4'-diphenylmethane diisocyanate is also called monomeric MDI or pure MDI. Polymeric MDI (crude MDI) is a mixture of monomeric MDI and high molecular weight polyisocyanate. Among them, 4,4'-diphenylmethane diisocyanate is preferred. The diphenylmethane diisocyanate used in the present invention is less expensive than 1,5-naphthalene diisocyanate (NDI), and compared to NDI, it is produced in larger quantities worldwide and can be procured globally.

[0033] The NCO% of the urethane prepolymer having an isocyanate group at its end is preferably 2 to 7%, more preferably 3 to 6%. If the NCO% is less than 2%, sufficient strength is not obtained and durability is also deteriorated. On the other hand, if the NCO% is more than 7%, the flexibility is lost and the prepolymer becomes hard, brittle, and durability is also deteriorated.

[0034] The blowing agent contained in the polyurethane foam composition may be water, a fluorocarbon substitute, or a hydrocarbon such as pentane, either alone or in combination. In the case of water, carbon dioxide gas is generated during the reaction of the isocyanate component, and the foaming is caused by the carbon dioxide gas. The amount of water used as the blowing agent is preferably 0.2 to 5 parts by weight per 100 parts by weight of the urethane prepolymer having an isocyanate group at its terminal.

[0035] The polyurethane foam composition may contain additives such as a catalyst, a foam stabilizer, a hydrolysis stabilizer, a crosslinking agent, a flame retardant, a colorant, a stabilizer, and a filler.

[0036] The catalyst may be a known urethanization catalyst or a retardation catalyst (temperature-sensitive catalyst). Examples of the urethanization catalyst include amine catalysts such as triethylamine, triethylenediamine, diethanolamine, dimethylaminomorpholine, N-ethylmorpholine, and tetramethylguanidine, tin catalysts such as stannous octoate and dibutyltin dilaurate, and metal catalysts such as phenylmercury propionate and lead octenate (also called organometallic catalysts). The retardation catalyst is an amine salt in which the active group of the urethanization catalyst is blocked with an acid such as formic acid or octylic acid, and examples of the retardation catalyst include phenol salts of diazabicycloalkenes, octylic acid salts of diazabicycloalkenes, and tertiary amine salts.

[0037] The foam stabilizer may be any foam stabilizer that is used for polyurethane foam, and examples of such foam stabilizers include silicone foam stabilizers, fluorine-containing compound foam stabilizers, and known surfactants. If the foam stabilizer is added during the preparation of the urethane prepolymer having an isocyanate group at its end, it will be uniformly dispersed in the urethane prepolymer, improving the foam stabilizing ability and allowing the production of a polyurethane foam with fine and uniform cells.

[0038] Examples of the hydrolysis stabilizer include carbodiimide compounds. In particular, when a polyester polyol is used as the polyol component, the hydrolysis resistance of the polyurethane foam can be improved by adding a hydrolysis stabilizer. Since a carbodiimide group is reactive with an active hydrogen group, it is preferable to add the carbodiimide group together with a blowing agent during the production of the polyurethane foam.

[0039] Examples of the crosslinking agent include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, glycerin, trimethylolpropane, etc. The crosslinking agent is preferably blended when preparing a urethane prepolymer having an isocyanate group at its end, and by mixing the crosslinking agent in a molten state together with a polyol component and a polyrotaxane, the crosslinking agent can be uniformly dispersed in the urethane prepolymer.

[0040] Examples of the flame retardant include halogenated compounds such as polyvinyl chloride, chloroprene rubber, and chlorinated polyethylene, condensed phosphoric acid compounds such as phosphoric acid esters and halogenated phosphoric acid esters, organic compounds such as melamine resins and urea resins, and inorganic compounds such as antimony oxide and aluminum hydroxide. If the flame retardant is added during the preparation of a urethane prepolymer having an isocyanate group at its terminal, it can be uniformly dispersed in the urethane prepolymer.

[0041] Examples of the colorant include pigments, dyes, etc. If the colorant is added during the preparation of the urethane prepolymer having an isocyanate group at its end, it can be uniformly dispersed in the urethane prepolymer.

[0042] Examples of the stabilizer include an antioxidant, an ultraviolet absorber, a light stabilizer, etc. If the stabilizer is added during the preparation of the urethane prepolymer having an isocyanate group at its end, it can be uniformly dispersed in the urethane prepolymer.

[0043] The isocyanate index (INDEX) is preferably 90 to 120. If the isocyanate index is less than 90, the degree of crosslinking is small, and the polyurethane foam does not obtain sufficient mechanical strength, and the polyurethane foam is more likely to collapse when subjected to repeated load, while if the isocyanate index is more than 120, the degree of crosslinking is large, and the polyurethane foam becomes hard and has low elasticity. A more preferred isocyanate index is 95 to 115. The isocyanate index is an index used in the field of polyurethane foams, and is a numerical value that represents the equivalent ratio of isocyanate groups to active hydrogen groups in a polyurethane foam composition as a percentage [NCO group equivalent / active hydrogen group equivalent×100].

[0044] The method for producing the bound stopper will be described below. The production of the bound stopper comprises a urethane prepolymer preparation step, a polyurethane foam composition injection / foaming step into a mold, and a demolding step.

[0045] In the urethane prepolymer preparation process, a polyrotaxane containing a cyclic molecule having an active hydrogen group as a constituent is added to a polyol component that has been heated to a predetermined temperature and brought to a molten state, and after mixing in the molten state for a predetermined time, isocyanate is added to react the active hydrogen groups of the polyol component and the cyclic molecules of the polyrotaxane with the isocyanate to produce a urethane prepolymer having an isocyanate group at its terminal.

[0046] To heat the polyol component and the polyrotaxane to a molten state, it is preferable to heat them at 60 to 120° C., depending on the melting point of the polyol component used. Even if the polyol component and the polyrotaxane are solid at room temperature, the polyol component and the polyrotaxane can be uniformly dispersed because they are mixed in a molten state.

[0047] In order to add an isocyanate and react the active hydrogen groups of the polyol component and the cyclic molecules of the polyrotaxane with the isocyanate, it is preferable to heat the mixture at 100 to 180°C.

[0048] In the step of injecting and foaming the polyurethane foam composition into a mold, the polyurethane foam composition, which contains at least a urethane prepolymer having an isocyanate group at its terminal, the foaming agent, and appropriate additives, is injected into a mold and foamed to form a bound stopper made of the polyurethane foam.

[0049] 3(3-A) shows one embodiment of a bound stopper mold 30. The mold 30 comprises a lower mold 31, a middle mold 33, and an upper mold . The lower die 31 is made up of a first lower die 31a and a second lower die 31b which can be separated into left and right halves, and has die surfaces 311a, 311b which form the side outer peripheral surface 10a of the bound stopper 10. The middle die 33 is substantially rod-shaped and has a die surface 33a on its outer periphery that forms the through hole 11 of the bound stopper 10, and is disposed between the first lower die 31a and the second lower die 31b. The lower die 31 and the middle die 33 are combined to form a cavity 34 between the die surface 311a of the first lower die 31a and the die surface 311b of the second lower die 31b and the die surface 33a of the middle die 33.

[0050] After the polyurethane foam composition is injected into the cavity 34, as shown in Fig. 3 (3-B), an upper mold 35 is placed over the cavity 34 to close the mold, and the polyurethane foam composition 40 is reacted and foamed. The mold is left in the closed state for a predetermined time to cure (primary cure), and the bound stopper 10 made of polyurethane foam is formed. The primary cure is preferably performed at 60 to 120°C for 10 to 120 minutes.

[0051] In the demolding process, as shown in FIG. 4, the upper mold 35 is removed, the first lower mold 31a and the second lower mold 31b are opened, and the middle mold 33 is separated. The middle mold 33 separated from the first lower mold 31a and the second lower mold 31b is in a state of being fitted into the through hole 11 of the bound stopper 10 made of the polyurethane foam. Thereafter, the bound stopper 10 is wiped off from the middle mold 33 by utilizing its elasticity, and the bound stopper 10 is obtained. It is preferable that the bound stopper 10 is subjected to a secondary cure after demolding. The secondary cure is preferably performed at 90 to 180° C. for 8 to 24 hours. EXAMPLES

[0052] <Preparation of urethane prepolymer having isocyanate groups at its terminals> Polyester polyols PO-1 to PO-7 and isocyanate were used to prepare urethane prepolymers having an isocyanate group at the end, which were used in the examples and comparative examples shown in FIGS. The polyester polyols PO-1 to PO-7 and the isocyanates have the following contents.

[0053] Polyester polyol PO-1 The polyester polyol PO-1 is a condensation polyester polyol having an average of 3 carbon atoms between ester bonds, composed of adipic acid (AA) having 4 carbon atoms between the carboxylic acid groups and ethylene glycol (EG) having 2 carbon atoms between the hydroxyl groups, and has Mw; 2000, functionality; 2, hydroxyl value; 56 mg KOH / g, product name; Polylite OD-X-102, manufactured by DIC Corporation.

[0054] Polyester polyol PO-2 The polyester polyol PO-2 is a condensation polyester polyol having an average of 4 carbon atoms between ester bonds, consisting of adipic acid (AA) having 4 carbon atoms between the carboxylic acids and 1,4-butanediol (BG) having 4 carbon atoms between the hydroxyl groups, and has Mw; 2000, functionality; 2, hydroxyl value; 56 mg KOH / g, product name; Polylite OD-X-668, manufactured by DIC Corporation.

[0055] Polyester polyol PO-3 Polyester polyol PO-3 is a condensation polyester polyol having an average of 5 carbon atoms between ester bonds, composed of adipic acid (AA) having 4 carbon atoms between the carboxylic acids and 1,6-hexanediol (HD) having 6 carbon atoms between the hydroxyl groups, and has Mw; 2000, functionality; 2, hydroxyl value; 56 mg KOH / g, product name; HS2H-201AP, manufactured by Toyokuni Oil Mills.

[0056] Polyester polyol PO-4 Polyester polyol PO-4 is a condensation polyester polyol having an average of 7 carbon atoms between ester bonds, composed of sebacic acid (SA) with 8 carbon atoms between the carboxylic acids and 1,6-hexanediol (HD) with 6 carbon atoms between the hydroxyl groups, and has Mw; 2000, functionality; 2, hydroxyl value; 56 mg KOH / g, product name; HS2H-201AP, manufactured by Toyokuni Oil Mills.

[0057] Polyester polyol PO-5 Polyester polyol PO-5 is a condensation polyester polyol with an average of 8 carbon atoms between ester bonds, consisting of dodecanedioic acid (DDA) with 10 carbon atoms between the carboxylic acids and 1,6-hexanediol (HD) with 6 carbon atoms between the hydroxyl groups, and has Mw; 3700, functionality; 2, hydroxyl value; 30 mg KOH / g, product name: Polylite OD-X-2555, manufactured by Toyokuni Oil Mills.

[0058] Polyester polyol PO-6 The polyester polyol PO-6 is a polycaprolactone diol (PCL) having an average carbon number of 5 between ester bonds obtained by ring-opening polymerization of ε-caprolactone, and has Mw of 2000, functionality of 2, hydroxyl value of 56 mg KOH / g, product name: Plaxel 220, manufactured by Daicel Corporation.

[0059] Polyester polyol PO-7 The polyester polyol PO-7 is polytetramethylene ether glycol (PTMG), having an average carbon number between ester bonds of 4, Mw of 2000, functionality of 2, hydroxyl value of 56 mgKOH / g, product name: PTMG2000, manufactured by Mitsubishi Chemical Corporation.

[0060] Polyrotaxane: Polyrotaxane containing cyclic molecules with hydroxyl groups as its constituents, molecular weight: 180,000, hydroxyl value: 85 mg KOH / g, product name: Super Polymer SH1300P (melting point: approx. 40°C), manufactured by Advanced Materials Corporation

[0061] Isocyanates In Examples 1 to 16 and Comparative Example 2, the isocyanate was 4,4'-diphenylmethane diisocyanate (monomeric MDI), NCO %: 33.6%, product name: Cosmonate MT, manufactured by Tosoh Corporation. In Comparative Example 1, the isocyanate is 1,5-naphthalene diisocyanate (NDI).

[0062] The above-mentioned polyol, polyrotaxane, and isocyanate were mixed in the ratios of each of the examples and comparative examples shown in Figures 5 and 6 to prepare urethane prepolymers having isocyanate groups at their ends as follows. Examples 1 to 16 and Comparative Example 1 contain polyrotaxane in the urethane prepolymer having isocyanate groups at their ends, and Comparative Example 2 does not contain polyrotaxane.

[0063] A 20L metal reaction vessel is charged with a specified amount of polyol (preliminarily heated to about 100°C to make it molten) according to the examples and comparative examples, and then heated to 130°C. In this state, a specified amount of polyrotaxane (solid state) according to the examples is charged into the reaction vessel, and mixed for 10 minutes while maintaining the temperature at 130°C to melt the polyrotaxane and disperse it uniformly in the polyol. With the reaction vessel maintained at 130°C, a specified amount of isocyanate according to the examples is charged and mixed for another 20 minutes. Thereafter, the reaction vessel is left at room temperature and slowly cooled to produce a urethane prepolymer having an isocyanate group at its end. The urethane prepolymer having an isocyanate group at its end in Comparative Example 1 was produced only from polyol and isocyanate.

[0064] <Preparation of test pieces> Using the prepared urethane polymer having an isocyanate group at its end and the following foaming liquid, test pieces of Examples 1 to 16 and Comparative Examples 1 to 3 were prepared by the methods described below. Foaming liquid: water / castor oil = 50 / 50, product name: Advado SV, manufactured by Rhein Chemie Japan

[0065] A polyurethane foam composition was prepared by blending a urethane polymer having an isocyanate group at its end, the temperature of which was adjusted to 80°C, and a foaming liquid, the temperature of which was adjusted to 40°C, in the ratios shown in Figs. 5 and 6 for Examples 1 to 16 and Comparative Examples 1 to 2. The polyurethane foam composition was mixed and then poured in a specified amount into a test piece mold, the temperature of which was adjusted to 80°C. The test piece mold had a cavity of 200 x 110 x 30 mm. The pouring amount for each Example and Comparative Example is shown in Figs. 5 and 6. The polyurethane foam was foamed in the mold, cured at 80°C for 30 minutes (primary curing), and then demolded. The polyurethane foam after demolding was further cured at 100°C for 12 hours (secondary curing) to obtain test pieces for Examples 1 to 16 and Comparative Examples 1 to 2.

[0066] <Product creation> The products (bound stoppers) of Examples 1 to 16 and Comparative Examples 1 to 3 were obtained in the same manner as in the production of the test pieces, except that the production mold (cavity volume 152 ml) shown in Figures 3 and 4 was used and the injection amounts were set to those of each Example and Comparative Example shown in Figures 5 and 6.

[0067] The density and tensile strength of the test pieces of each Example and Comparative Example were measured, and the ride comfort of the finished product was also measured. The measurement results are shown in Figs. 5 and 6.

[0068] The density was measured in accordance with JIS K7222:2005 using a test piece (200×110×30 mm) as a measurement sample (with skin layers on all top, bottom and side surfaces).

[0069] Tensile strength was measured in accordance with JIS K6251:2017 by slicing a measurement sample of No. 2 dumbbell size and thickness of 2 mm (no skin layer on the top, bottom or sides) from the test piece. Tensile strength was judged as "x" when it was less than 3.5 MPa, "good" when it was between 3.5 MPa and 4 MPa, and "excellent" when it was 4 MPa or more.

[0070] The ride comfort was evaluated by inserting the product (bound stopper 10) into the shaft, measuring (A) the load (N) at 1% compression (displacement) and (B) the load (N) at 5% compression (displacement) using an autograph (Shimadzu Corporation), and calculating the slope of the load change from the displacement of the bound stopper (the difference between the 5% compression and the 1% compression) and the load change using the following formula. The displacement of the bound stopper was 4 mm. Load change slope = (BA) / displacement

[0071] The smaller the gradient of the load change, the smaller the feeling of being pushed up by unevenness of the road surface while the vehicle is traveling, and the better the ride comfort. The gradient of the load change was judged as "x" when it was 10.0 or more, "good" when it was 8.5 to less than 10.0, and "excellent" when it was less than 8.5.

[0072] In addition, if either the tensile strength judgment or the ride comfort judgment was marked with an "X", the overall judgment was marked with an "X", if both judgments were marked with an "O" or if both judgments were marked with an "O" and an "◎", the overall judgment was marked with an "O", and if both judgments were marked with an "◎", the overall judgment was marked with an "◎".

[0073] In Example 1, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-1 (AA / EG) having an average carbon number of 3 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was mixed with 3.0 g of foaming liquid. The amounts of the mixture injected into a test piece mold and a product mold were 323 g and 75 g, respectively, to produce a test piece and a product. Example 1 has a density of 0.49 g / cm 3 The tensile strength was 3.5 MPa, the tensile strength was judged as "good", the slope of the load change was 8.2, and the ride comfort was judged as "excellent", resulting in an overall judgement of "good".

[0074] In Example 2, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-2 (AA / BG) having an average carbon number of 4 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 5.0%, and 3.0 g of foaming liquid. 330 g and 76 g were injected into a test piece mold and a product mold to produce a test piece and a product. Example 2 has a density of 0.50 g / cm 3 The tensile strength was 3.8 MPa, the tensile strength was judged as "good", the load change slope was 8.0, and the ride comfort was judged as "excellent", resulting in an overall judgement of "good".

[0075] In Example 3, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-3 (AA / HD) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 5.0%, and 3.0 g of foaming liquid. 317 g and 73 g were injected into a test piece mold and a product mold to produce a test piece and a product. Example 3 has a density of 0.48 g / cm 3 The tensile strength was 4.2 MPa, the tensile strength was judged as "◎", the load change slope was 7.5, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0076] In Example 4, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-4 (SA / HD) having an average carbon number of 7 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was made from this urethane prepolymer. The amounts of the composition injected into the test piece mold and the product mold were 343 g and 79 g, respectively, to produce a test piece and a product. Example 4 has a density of 0.52 g / cm 3 The tensile strength was 4.8 MPa, the tensile strength was judged as "◎", the load change slope was 7.2, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0077] In Example 5, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-5 (DDA / HD) having an average carbon number of 8 between ester bonds, 30 g of polyrotaxane, and 266 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 337 g and 78 g, respectively, to produce a test piece and a product. Example 5 has a density of 0.51 g / cm 3 The tensile strength was 4.9 MPa, the tensile strength was judged as "◎", the load change slope was 7.0, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0078] In Example 6, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at a terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 323 g and 75 g, respectively, to prepare a test piece and a product. Example 6 has a density of 0.49 g / cm 3 The tensile strength was 4.4 MPa, the tensile strength was judged as "◎", the load change slope was 7.6, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0079] In Example 7, a polyurethane foam composition with an isocyanate index of 103 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 245 g of 4,4'-diphenylmethane diisocyanate, and 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 3.0%, and 1.9 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to prepare a test piece and a product. Example 7 has a density of 0.50 g / cm 3 The tensile strength was 4.0 MPa, the tensile strength was judged as "◎", the load change slope was 7.3, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0080] In Example 8, a polyurethane foam composition with an isocyanate index of 104 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 288 g of 4,4'-diphenylmethane diisocyanate, 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 4.0%, and 2.5 g of foaming liquid. 337 g and 78 g were injected into a test piece mold and a product mold, respectively, to produce a test piece and a product. Example 8 has a density of 0.51 g / cm 3 The tensile strength was 4.2 MPa, the tensile strength was judged as "◎", the load change slope was 7.4, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0081] In Example 9, a polyurethane foam composition with an isocyanate index of 103 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 383 g of 4,4'-diphenylmethane diisocyanate, and 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 6.0%, and the prepolymer was injected in amounts of 323 g and 75 g into a test piece mold and a product mold to produce a test piece and a product. Example 9 has a density of 0.49 g / cm 3 The tensile strength was 4.7 MPa, the tensile strength was judged as "◎", the load change slope was 7.8, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0082] In Example 10, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 191 g and 45 g, respectively, to produce a test piece and a product. Example 10 has a density of 0.29 g / cm 3 The tensile strength was 4.0 MPa, the tensile strength was judged as "◎", the load change slope was 7.0, and the ride comfort was judged as "◎", and the overall judgement was "◎".

[0083] In Example 11, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 271 g and 62 g, respectively, to produce a test piece and a product. Example 11 has a density of 0.41 g / cm 3 The tensile strength was 4.2 MPa, the tensile strength was judged as "◎", the load change slope was 7.5, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0084] In Example 12, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 30 g of polyrotaxane, and 334 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 409 g and 94 g, respectively, to produce a test piece and a product. Example 12 has a density of 0.62 g / cm 3 The tensile strength was 4.5 MPa, the tensile strength was judged as "◎", the load change slope was 8.0, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0085] In Example 13, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 5 g of polyrotaxane, and 324 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at a terminal and NCO% (theoretical value) of 5.0%, and 3.0 g of foaming liquid. The amounts of the composition injected into the test piece mold and the product mold were 323 g and 75 g, respectively, to prepare a test piece and a product. Example 13 has a density of 0.49 g / cm 3 The tensile strength was 4.0 MPa, the tensile strength was judged as "◎", the load change slope was 8.0, and the ride comfort was judged as "◎", and the overall judgement was "◎".

[0086] In Example 14, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 10 g of polyrotaxane, and 326 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 330 g and 76 g, respectively, to produce a test piece and a product. Example 14 has a density of 0.50 g / cm 3 The tensile strength was 4.1 MPa, the tensile strength was judged as "◎", the slope of the load change was 7.9, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0087] In Example 15, a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds, 50 g of polyrotaxane, and 342 g of 4,4'-diphenylmethane diisocyanate, as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, and the prepolymer was made from the above-mentioned mixture, and 3.0 g of foaming liquid was poured into a test piece mold and a product mold in amounts of 337 g and 78 g, respectively, to produce a test piece and a product. Example 15 has a density of 0.51 g / cm 3 The tensile strength was 4.7 MPa, the tensile strength was judged as "◎", the load change slope was 7.4, and the ride comfort was judged as "◎", resulting in an overall judgement of "◎".

[0088] In Example 16, a polyurethane foam composition with an isocyanate index of 102 was prepared from 1000 g of polyester polyol PO-7 made of polytetramethylene ether glycol (PTMG), 30 g of polyrotaxane, and 100 g of a urethane prepolymer having an isocyanate group at a terminal and an NCO% (theoretical value) of 5.0%, which was made from 334 g of 4,4'-diphenylmethane diisocyanate, and 2.1 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to prepare a test piece and a product. Example 16 has a density of 0.51 g / cm 3 The tensile strength was 5.0 MPa, the tensile strength was judged as "◎", the slope of the load change was 9.6, and the ride comfort was judged as "◯", resulting in an overall judgement of "◯".

[0089] In Comparative Example 1, 1,5-naphthalene diisocyanate (NDI) was used as the isocyanate, and a polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-1 (AA / EG) having an average carbon number between ester bonds of 3, 30 g of polyrotaxane, and 273 g of 1,5-naphthalene diisocyanate (NDI), as well as 100 g of a urethane prepolymer having an isocyanate group at its terminal and NCO% (theoretical value) of 5.0%, and 3.0 g of foaming liquid. 330 g and 76 g were injected into the test piece mold and the product mold to produce a test piece and a product. Comparative Example 1 has a density of 0.50 g / cm 3 The tensile strength was 4.3 MPa, the tensile strength was judged as "◎", the slope of the load change was 11.3, and the ride comfort was judged as "×", resulting in an overall judgement of "×".

[0090] Comparative Example 2 is an example that does not contain polyrotaxane. A polyurethane foam composition with an isocyanate index of 108 was prepared from 1000 g of polyester polyol PO-6 (PCL) having an average carbon number of 5 between ester bonds and 334 g of 4,4'-diphenylmethane diisocyanate, 100 g of a urethane prepolymer having an isocyanate group at a terminal and NCO% (theoretical value) of 5.0%, and 3.0 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 323 g and 75 g, respectively, to produce a test piece and a product. Comparative Example 2 has a density of 0.49 g / cm 3 The tensile strength was 4.0 MPa, the tensile strength was judged as "◎", the load change slope was 10.1, and the ride comfort was judged as "×", resulting in an overall judgement of "×".

[0091] Thus, each Example has high mechanical strength (tensile strength) and good ride comfort. In contrast, Comparative Example 1, which used 1,5-naphthalene diisocyanate (NDI) as the isocyanate, and Comparative Example 2, which did not contain polyrotaxane, are inferior in ride comfort to Examples 1 to 16. The present invention is not limited to the embodiments, and can be modified without departing from the spirit of the invention. [Explanation of symbols]

[0092] 10 Bound Stopper 20 Polyrotaxane containing cyclic molecules with active hydrogen groups as its constituents 30 Mold 31 Lower mold 33 medium size 35 Upper mold

Claims

1. A polyurethane foam bound stopper is attached to a piston rod of a shock absorber for a vehicle. The polyurethane foam is obtained from a polyurethane foam composition including at least an isocyanate component and a blowing agent. the isocyanate component is composed of a urethane prepolymer having an isocyanate group at a terminal thereof, the urethane prepolymer being obtained from a polyol component, a polyrotaxane containing a cyclic molecule having an active hydrogen group as a constituent, and diphenylmethane diisocyanate; The urethane prepolymer having an isocyanate group at its end has a polyrotaxane content of 0.1 parts by weight or more per 100 parts by weight of the polyol component, The bound stopper is characterized in that the density of the polyurethane foam is 0.2 g / cm 3 or more.

2. 2. The bound stopper according to claim 1, wherein the urethane prepolymer having an isocyanate group at its terminal has a polyrotaxane content of 0.1 to 6.5 parts by weight per 100 parts by weight of the polyol component.

3. The density of the polyurethane foam is 0.2 to 0.7 g / cm 3 3. The bound stopper according to claim 1, wherein:

4. A method for manufacturing a bound stopper made of polyurethane foam to be attached to a piston rod of a shock absorber for a vehicle, comprising the steps of: A polyol component and a polyrotaxane containing, as a constituent, a cyclic molecule having an active hydrogen group are mixed in a molten state, and then diphenylmethane diisocyanate is added to the mixture to prepare a urethane prepolymer having an isocyanate group at its terminal. A polyurethane foam composition including at least a urethane prepolymer having an isocyanate group at a terminal thereof and a foaming agent is injected into a mold and foamed to form a bound stopper made of the polyurethane foam; The urethane prepolymer having an isocyanate group at its end has a polyrotaxane content of 0.1 parts by weight or more per 100 parts by weight of the polyol component, The method for producing a bound stopper, wherein the density of the polyurethane foam constituting the bound stopper is 0.2 g / cm 3 or more.

Citation Information

Patent Citations

  • Urethane-based bumper spring and manufacturing method thereof

    JP2015183832A

  • Bound stopper and manufacturing method thereof