ABSORBENT ARTICLES HAVING CONFORMING FEATURES - Patent application
By integrating conformable features through hydroentangling and mesoscale processes, the absorbent articles enhance fluid dynamics and comfort, addressing the trade-offs in conventional designs and reducing leakage.
Patent Information
- Application Number
- JP2023019873
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-11-06
- Filing Date
- 2023-02-13
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2038-11-06
AI Technical Summary
Absorbent articles face a trade-off between providing a comfortable fit and effective fluid dynamics, with conventional topsheets either prioritizing quick fluid acquisition at the cost of rewetting performance or improving rewetting at the expense of acquisition time, and often compromising structural integrity leading to wearer discomfort and leakage.
The absorbent articles incorporate multiple layers with integrated conformable features, utilizing hydroentangling and mesoscale processes to create intimate contact between layers, enhancing fluid transfer rates and mechanical compatibility without relying on adhesives, which maintain structural integrity and adapt to complex body contours.
The solution achieves improved fluid handling, comfort, and reduced leakage by ensuring close contact between layers, allowing for rapid fluid acquisition and rewetting while maintaining resilience and conformability to body shape.
Smart Images

Figure 0007565395000008 
Figure 0007565395000009 
Figure 0007565395000010
Abstract
Description
[Technical field]
[0001] The present invention relates to absorbent articles having conforming features and methods of forming conforming features in absorbent articles. [Background technology]
[0002] Absorbent articles, such as diapers, training pants, feminine pads, adult incontinence pads, etc., are widely used among consumers. Generally, such absorbent articles include a topsheet and a backsheet with an absorbent core disposed therebetween. Some may include additional layers between the topsheet and the absorbent core or between the backsheet and the absorbent core to provide additional fluid management properties.
[0003] In general, absorbent articles are expected to absorb liquid insults and transfer the liquid from the insult point on the topsheet to the absorbent core. Also, once the liquid insult is absorbed, the absorbent article is expected to limit the amount of liquid that will drain from the absorbent core and rewet the topsheet. To capture the liquid insult within a reasonable time, the absorbent core or an additional layer between the topsheet and the core must be in liquid contact with the topsheet and adequately wick the liquid insult away from the topsheet.
[0004] However, the variables that affect acquisition speed can be opposite to rewet performance. For example, some conventional topsheets require a trade-off between capillarity, permeability and rewet properties. Therefore, good liquid acquisition can be achieved by making the topsheet hydrophilic so that fluid passes through quickly, but then the topsheet typically suffers from poor rewet performance. The reverse is also true. A hydrophobic topsheet may provide better rewet performance, but the hydrophobicity of the topsheet is likely to result in longer fluid acquisition times.
[0005] In addition, absorbent articles are expected to provide a comfortable feel to the user in addition to fluid acquisition and rewet performance. This can be a real challenge, especially in the context of feminine hygiene articles or adult female incontinence articles. Although some articles may be manufactured that provide a high degree of conformity to the complex female anatomy, such conformity can reduce the structural integrity of the absorbent article. The reduced structural integrity of the article can result in bunching during use and inhibit the article from returning to its original shape. Unfortunately, bunching of the article can result in discomfort for the wearer and leakage during use. Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, it would be beneficial to have an improved absorbent article that addresses the tradeoffs of providing comfortable fit and elasticity, as well as good fluid dynamics, and it would be beneficial to provide a method for making such an article without sacrificing the leakage performance of the absorbent article. [Means for solving the problem]
[0007] The present disclosure relates to absorbent articles having improved fluid transport rates between layers and unexpectedly improved mechanical and comfortable conformance to the body, and methods of making same.
[0008] Disposable absorbent articles of the present disclosure include multiple layers that are assembled together to form a completed article. For example, disposable absorbent articles of the present disclosure include a topsheet, a backsheet, and an absorbent core disposed between the topsheet and the backsheet. A fluid management layer, such as a secondary topsheet or acquisition layer, may be disposed between the topsheet and the absorbent core. Additional layers may be positioned between the absorbent core and the backsheet and / or between the absorbent core and the topsheet.
[0009] The disposable absorbent article may further include a first region having a longitudinal centerline and a lateral centerline, a second region, and a target region disposed between the first region and the second region. Each of the first region, the second region, and the target region extend laterally across the disposable absorbent article. The disposable absorbent article may further include a topsheet, a backsheet, an absorbent core disposed between the topsheet and the backsheet, a fluid management layer disposed between the topsheet and the absorbent core, a target zone disposed within the target region, the target zone including a first plurality of conforming features at least in the absorbent core or in a combination of the absorbent core and at least one of the topsheet or the fluid management layer, and a long fiber network included in at least one of the absorbent core, the topsheet, the fluid management layer, or in a combination of the absorbent core and at least one of the fluid management layer or the topsheet. [Brief description of the drawings]
[0010] [Figure 1A] FIG. 1 is a cross-sectional view showing a laminate of two materials joined by conventional lamination techniques. [Figure 1B] FIG. 1 is a cross-sectional view showing a laminate of two materials joined by conventional lamination techniques. [Figure 2A] FIG. 1 is a cross-sectional view of a topsheet and a secondary topsheet according to the present disclosure. [Figure 2B] 1 is a graph showing fluid management data between laminates of conventional processing and materials of the present disclosure. [Figure 2C] FIG. 2 is a cross-sectional view of a topsheet and an absorbent core according to the present disclosure. [Figure 3A] FIG. 1 is a schematic diagram illustrating the process of creating interweb / intraweb coherence of the present disclosure. [Figure 3B] FIG. 1 is a schematic diagram illustrating the process of creating interweb / intraweb coherence of the present disclosure. [Figure 3C] FIG. 1 is a schematic diagram illustrating the process of creating interweb / intraweb coherence of the present disclosure. [Figure 3D]FIG. 1 is a schematic diagram illustrating the process of creating interweb / intraweb coherence of the present disclosure. [Figure 3E] FIG. 1 is a schematic diagram illustrating the process of creating interweb / intraweb coherence of the present disclosure. [Figure 3F] FIG. 1 is a schematic diagram illustrating the process of creating interweb / intraweb coherence of the present disclosure. [Figure 4] FIG. 1 is a schematic diagram of a topsheet and acquisition / distribution laminate web with a separate acquisition / distribution web portion depicted on top of the topsheet web. [Diagram 5] FIG. 2 is a schematic diagram of a topsheet and acquisition laminate web including protrusions. [Figure 6A] FIG. 2 is a diagram of a pair of rolls capable of forming protrusions in a laminate web of the present disclosure. [Figure 6B] 6B is a photograph showing an exemplary roll pattern that may be utilized with the apparatus shown in FIG. 6A. [Figure 7A] FIG. 13 is an illustration of another pair of rolls capable of forming protrusions in a web of the present disclosure. [Figure 7B] FIG. 13 is an illustration of another pair of rolls capable of forming protrusions in a web of the present disclosure. [Figure 7C] FIG. 13 is an illustration of another pair of rolls capable of forming protrusions in a web of the present disclosure. [Figure 7D] FIG. 13 is an illustration of another pair of rolls capable of forming protrusions in a web of the present disclosure. [Figure 8A] FIG. 13 is an illustration of another pair of rolls or other elements capable of forming both holes and protrusions in the topsheet and acquisition / distribution laminate web. [Figure 8B] FIG. 13 is an illustration of another pair of rolls or other elements capable of forming both holes and protrusions in the topsheet and acquisition / distribution laminate web. [Figure 8C] FIG. 13 is an illustration of another pair of rolls or other elements capable of forming both holes and protrusions in the topsheet and acquisition / distribution laminate web. [Figure 8D]FIG. 13 is an illustration of another pair of rolls or other elements capable of forming both holes and protrusions in the topsheet and acquisition / distribution laminate web. [Figure 9A] FIG. 13 is an illustration of another pair of rolls capable of forming holes in the web of the present disclosure. [Figure 9B] FIG. 13 is an illustration of another pair of rolls capable of forming holes in the web of the present disclosure. [Figure 10] FIG. 2 is a diagram of an apparatus capable of forming holes and protrusions in zones in a web of the present disclosure. [Figure 11A] 1 is a schematic diagram of an absorbent article including a treatment area of the article. [Figure 11B] 1 is a schematic diagram of an absorbent article including a treatment area of the article. [Figure 11C] 1 is a schematic longitudinal cross-sectional view showing an additional embodiment of an absorbent article according to the present disclosure. [Figure 11D] 1 is a schematic longitudinal cross-sectional view showing an additional embodiment of an absorbent article according to the present disclosure. [Figure 11E] 1 is a schematic longitudinal cross-sectional view showing an additional embodiment of an absorbent article according to the present disclosure. [Figure 12A] 1 is a photograph showing a top view of a web constructed according to the present disclosure. [Figure 12B] 12B is a photograph showing a cross section of the web of FIG. 12A. [Figure 13A] 1 is a photograph showing a top view of another web constructed in accordance with the present disclosure. [Figure 13B] 13B is a photograph showing a cross section of the web of FIG. 13A. [Figure 13C] 13B is a photograph showing a cross section of the web of FIG. 13A. [Figure 14] 1 is a schematic cross-sectional view of a web of the present disclosure showing exaggerated features for ease of visualization. [Figure 15A] 1 is a photograph showing a plan view of a web constructed from a material lacking a long fiber network of the present disclosure. [Figure 15B] 15B is a photograph showing a cross section of the web of FIG. 15A. [Figure 15C]15B is a photograph showing a cross section of the web of FIG. 15A. [Figure 16] 1 is a schematic cross-sectional view of a web of the present disclosure showing exaggerated features for ease of visualization. [Figure 17A] 1 is a photograph showing a top view of an absorbent article constructed in accordance with the present disclosure. [Figure 17B] 1 is a schematic diagram showing another possible pattern arrangement for the web of the present disclosure. [Figure 18] 1 is a schematic of a partial exemplary process for making an absorbent article. [Figure 19] FIG. 1 is a top view of a feminine hygiene article, i.e., a sanitary napkin, constructed in accordance with the present disclosure. [Figure 20] FIG. 1 is a top view of an absorbent article with some layers partially removed in accordance with the present disclosure. [Figure 21] 1 is a photograph showing tooling for creating matching features as described herein. [Figure 22] 1 is a photograph of a nonwoven web including a hole pattern as described herein. [Figure 23] FIG. 1 is a schematic diagram of the apparatus for the NMR mouse assay described herein. [Figure 24] FIG. 24 is a schematic diagram of a test specimen setup for the apparatus of FIG. 23. [Diagram 25] FIG. 1 is a schematic diagram showing an apparatus for the bunch compression testing method described herein. [Figure 26A] This relates to the test method of FIG. [Figure 26B] This relates to the test method of FIG. [Figure 27A] This relates to the test method of FIG. [Figure 27B] This relates to the test method of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] As used herein, "disposable absorbent article" or "absorbent article" is intended to refer to articles such as diapers, training pants, diaper pants, refastenable pants, adult incontinence pads, adult incontinence pants, feminine hygiene pads, tampons, pessary devices, cleaning pads, etc., each of which is intended to be discarded after use.
[0012] As used herein, "hydrophilic" and "hydrophobic" have their well-established meanings in the art with respect to the contact angle of water on a material surface. Thus, a material having a water contact angle of more than about 90 degrees is considered hydrophobic, and a material having a liquid contact angle of less than about 90 degrees is considered hydrophilic. A composition that is hydrophobic will increase the contact angle of water on the surface of the material, while a composition that is hydrophilic will decrease the contact angle of water on the surface of the material. Notwithstanding the above, reference to relative hydrophobicity or hydrophilicity between a material and a composition, between two materials, and / or between two compositions does not mean that the material or composition is hydrophobic or hydrophilic. For example, the composition may be more hydrophobic than the material. In this case, neither the composition nor the material may be hydrophobic. However, the composition exhibits a contact angle that is greater than that of the material. As another example, the composition may be more hydrophilic than the material. In this case, neither the composition nor the material may be hydrophilic. However, the composition exhibits a contact angle that is less than that of the material.
[0013] The term "filament" refers to any type of continuous synthetic fiber produced by a spinning process, a meltblown process, a melt fibrillation or film fibrillation process, or an electrospinning production process, or any other suitable process for manufacturing filaments. The term "continuous" in the context of filaments can be distinguished from staple filaments, where the staple filaments are cut to a specific targeted length. In contrast, "continuous filaments" are not cut to a predetermined length, but instead can break at random lengths, but are usually much longer than staple filaments.
[0014] As used herein, "machine direction" refers to the direction in which a web runs through an absorbent article conversion process. For simplicity, it may be referred to as "MD."
[0015] As used herein, "cross machine direction" refers to the direction perpendicular to the MD, which for simplicity may be referred to as "CD."
[0016] The absorbent articles of the present disclosure can provide improved fluid handling, fit, and recovery. It has been discovered that by utilizing a repeating pattern of bending manner at the mesoscale versus the traditional microscale and / or macroscale, which is bendable and moldable based on each user's unique anatomical shape and the way the user deforms the absorbent system while wearing it, an absorbent structure can be created that can have improved contact between the absorbent product and the user.
[0017] The inventors have surprisingly found that forming a tight fit between layers of an absorbent article can achieve improved fluid dynamics along with improved mechanical fit. The inventors have also found that if not implemented correctly, such tight fit between layers can cause leakage problems in the corresponding absorbent article. In addition, depending on the scale of integration, the inventors have surprisingly found that some integration processes can provide the additional benefit of compatibility with the complex contours of the user's body in addition to the fluid dynamics benefit.
[0018] Cross-sectional views of a non-coherent conventionally processed topsheet and secondary topsheet combination are shown in Figures 1A and 1B. In Figure 1A, a topsheet melt-bonded to a secondary topsheet is shown in cross section. Although the layers are joined together, they are not coherent. For example, an opening 7 is shown between the topsheet and the secondary topsheet. In addition, the melt-bonded regions 9 arguably unite the components of the topsheet and the secondary topsheet, but they destroy the morphology of the components, forming instead a film-like region that does not allow liquid to pass through. Thus, the melt-bonded topsheet and secondary topsheet lack the coherence described herein.
[0019] In Figure IB, a cross-sectional view of a topsheet and a secondary topsheet joined by an adhesive is shown. Like the topsheet and secondary topsheet configuration of Figure 1A, the configuration shown in Figure IB also includes an opening 7 between the topsheet and the secondary topsheet. Thus, like the melt-bonded configuration, the adhesive configuration does not provide the intimate contact between the topsheet and the secondary topsheet that is desired and described herein.
[0020] Another conventional method of promoting contact between layers involves the use of a vacuum. During formation, the substrate, e.g., a nonwoven fabric, can be exposed to a vacuum conveyor. Additional material, e.g., fibers, can be deposited on the substrate. At the interface between the substrate and the fibers, the vacuum can cause some degree of material integration, but this is believed to be a surface phenomenon rather than the intimate contact created by integration disclosed herein.
[0021] Furthermore, while embossing arguably creates adhesion between adjacent layers, embossing tends to create areas of densification due to compression. Also, as previously mentioned, densification of areas can create localized stiffness, which can lead to compatibility issues and can adversely affect consumer comfort during use. Thus, the desired adhesion between adjacent layers herein does not include embossing.
[0022] In contrast to the conventional configurations shown in Figures 1A and 1B, Figure 2A shows a cross-sectional view of a topsheet and a secondary topsheet of the present disclosure. Figure 2A shows a cross-sectional view of a secondary topsheet and a hydroentangled topsheet. As shown, the components of the topsheet and the components of the secondary topsheet are integrated in the Z direction. This integration in the Z direction can create a tight fit between the topsheet and the secondary topsheet across the entire cross section between the topsheet and the secondary topsheet, and there is no or a reduced number of openings between the topsheet and the secondary topsheet.
[0023] As used herein, "cohesion" refers to the integration of layers of an absorbent article. This integration brings the constituent materials of the layers into contact such that the constituent materials of the lower layer are more easily accessible through the upper layer. For example, the integration of the constituent materials between the layers allows the constituent materials of the lower layer to be more easily accessible through the upper layer. Also, as previously described, the cohesion between the layers allows for more efficient fluid transfer from the upper layer to the lower layer, rather than preventing fluid transfer as described for embossing and bonding. For example, filaments and / or fibers of one layer are believed to penetrate into the adjacent layer. This filament and / or fiber penetration is believed to provide a bridge across the interface between one layer and another layer. Furthermore, this bridge is believed to facilitate fluid transfer from one layer to another layer. Unlike the conventional processes described above, the cohesion created by the process described herein can create integration of material layers not only at the surface, but at a depth of millimeters in the adjacent layers. In addition, by creating cohesion between adjacent layers as described herein, the resulting absorbent article does not have to rely on adhesives to hold the layers together. Adhesives tend to increase stiffness, which can adversely affect conformability and, in some cases, can inhibit fluid transfer. Finally, the intimacy described herein differs from the surface interaction (two-dimensional) created by vacuum forming in that the intimacy via the processes described in this disclosure can provide three-dimensional access to the underlying layer, e.g., the material of the absorbent core.
[0024] Data showing the fluid acquisition rate of hydroentangled topsheet / secondary topsheet combinations is shown in FIG. 2B. As shown in FIG. 2B, the hydroentangled topsheet and secondary topsheet coupled with the absorbent core are represented by curve 201, and the conventionally treated topsheet, secondary topsheet, and absorbent core are represented by curve 200. As shown, the samples with hydroentangled topsheet and secondary topsheet show faster fluid acquisition, as shown by the slope of curve 201 relative to curve 200. In addition, over time, the samples with hydroentangled topsheet and secondary topsheet move fluid from the surface of the topsheet more quickly than the conventionally treated topsheet, secondary topsheet, and absorbent core combination. The data shown in FIG. 2B was obtained by NMR-Mouse technology, for example, Profile NMR-MOUSE model PM25 with High-Precision Lift available from Magritek Inc. (San Diego, CA). The NMR-Mouse method measured the amount of liquid in the top 200 micrometers of the topsheet, secondary topsheet, and absorbent core samples shown in Figure 2B.
[0025] FIG. 2C is a cross-sectional view of a topsheet in close contact with an absorbent core in the Z direction. There are no obvious openings between the topsheet and the absorbent core, much like the topsheet and secondary topsheet. The topsheet and absorbent core have undergone mesoscale processing as described herein. As shown, there are multiple peaks and depressions. Due to the close contact between the topsheet and the absorbent core, such a configuration of the topsheet / absorbent core laminate is believed to improve fluid acquisition and rewet.
[0026] The disposable absorbent article of the present disclosure includes at least one cohesive region, where the topsheet, the secondary topsheet, the absorbent core, an additional layer between the topsheet and the backsheet, or any combination thereof, includes a cohesive portion. Forming cohesion between layers requires an operation of mechanically treating the constituent materials of adjacent layers. For example, the constituent materials of adjacent layers may be treated by hydroentanglement, as described above in connection with Figures 2A and 2B, or may undergo a mesoscale process, as mentioned in connection with Figure 2C. These processes can create cohesion between adjacent layers of the absorbent article. Further processes for creating cohesion between layers in the absorbent article are disclosed herein. Also, a combination of processes may be utilized. For example, some layers may be hydroentangled / needlepunched, while other layers may be integrated through another process that is not hydroentangled / needlepunched. Alternatively, a hydroentangled / needlepunched layer may be combined with another layer through a process different from hydroentangled / needlepunched. Alternatively, some layers may be integrated via mesoscale processes without being hydroentangled / needlepunched.
[0027] It should be noted that in addition to hydroentangling, some processes that are taught to be used for lofting materials such as nonwovens may also provide some degree of inter-layer cohesion. These processes generally utilize hot air jets to move the fibers of the material. This process is described in detail in U.S. Patent No. 8,720,021, which is incorporated herein by reference. When hydroentangling or needle punching is mentioned, hot air jets may also be used.
[0028] Furthermore, although nonwoven (fibrous) materials are shown in Figures 2A and 2C, adhesion can be established with a wide variety of materials as described herein. For example, films may be utilized in conjunction with nonwoven (fibrous) materials as described herein. Surprisingly, it has also been found that the use of forming means that integrates the topsheet, secondary topsheet, and absorbent core improves the softness of the pad (measured by bunch compression) by providing a fibrous network. This is different from conventional systems that become more rigid when welding, adhesives, embossing, or improving capillarity by densification.
[0029] For purposes of simplicity and clarity of the following disclosure, the topsheet is generally soft feeling to the wearer of the absorbent article. Further, the topsheet should be configured to readily accept a liquid insult so as to maintain a dry feeling to the wearer. Topsheets are described in more detail below.
[0030] A fluid management layer, or simply "FM" layer, is generally placed directly beneath the topsheet and should be configured to rapidly acquire liquid insults to the topsheet and distribute the liquid insults to the absorbent core. The FM layer may have some ability to absorb and retain liquid insults, but may be primarily designed to rapidly drain the topsheet and transfer liquid to the absorbent core. The FM layer is also described further herein.
[0031] The absorbent core is the main storage element of a disposable absorbent article. The absorbent core receives and stores the liquid insult to the topsheet. The absorbent core may generally be located under the FM layer or under the topsheet. In addition, the absorbent core tends to have more associated volume than other components of the absorbent article and therefore also tends to dominate the mechanical properties of the absorbent article. For example, mechanical properties such as flexibility, conformability, and moldability, i.e., the shape that the product assumes while being worn, may be primarily influenced by the properties of the absorbent core. The absorbent core is described in more detail below.
[0032] process The process of the present disclosure can provide absorbent articles with cohesive regions between components of the absorbent article, which can reduce the likelihood of leakage along with improved acquisition rates. Also, as discussed herein, the process of the present disclosure can provide absorbent articles with improved acquisition rates and the ability to conform to much more complex surfaces than their conventional counterparts.
[0033] The tight contact between the topsheet and the FM layer, the FM layer and the absorbent core, the topsheet and the absorbent core, or the topsheet, the FM layer, and the absorbent core can be achieved by mechanical manipulation of at least two of the topsheet, the FM layer, and the absorbent core. However, as mentioned above, the FM layer and the absorbent core are generally configured to rapidly receive and / or store liquid insults from the topsheet. Thus, both the FM layer and the absorbent core are typically more absorbent than the topsheet. Without pre-treating the FM layer and / or the absorbent core, there is a risk that the FM layer and / or the absorbent core will be coextensive with the topsheet, which may cause liquid insults to leak from the FM layer and / or the absorbent core in the final product. Also, trimming the FM layer and / or the absorbent core after joining with the topsheet, although reasonable, proves difficult at best for high speed manufacturing.
[0034] The inventors have discovered a process that significantly reduces the risk of leakage due to the feature of the FM layer and / or absorbent core being coextensive with the topsheet. The FM layer and / or absorbent core can be pretreated to reduce its size, e.g., width, such that the periphery of the FM layer and / or absorbent core is positioned inside the periphery of the topsheet. This process is described in more detail below.
[0035] 3A and 4, a topsheet web 10 (shown as a roll) may be provided as a carrier to a cutting and placing operation 30. An FM web 20 (shown as a roll) may similarly be provided to the cutting and placing operation 30. The cutting and placing operation 30 may cut the FM web 20 into a plurality of separate portions 20A.
[0036] The topsheet web 10 may be made as part of the absorbent article processing process or may be obtained from a manufacturer of suitable topsheet materials. Similarly, the FM layer may be made as part of the absorbent article processing process or may be obtained from a manufacturer of fluid management materials. The absorbent core web may be similarly made as part of the absorbent article processing line or may be obtained from a manufacturer of suitable absorbent core materials.
[0037] 3A and 4, the separate portion 20A has opposing longitudinal sides 24 and lateral ends 26 connecting the opposing longitudinal sides 24. The topsheet web 10 includes longitudinal sides 14 that are outboard of the longitudinal sides 24 of the separate portion 20A. The lateral sides of the topsheet web 10 can be defined during subsequent processing. If it is desired that the separate portion 20A not be longitudinally coextensive with the topsheet web 10, then the lateral sides of the topsheet web 10 after cutting should be outboard of the lateral ends 26 of the separate portion 20A. Furthermore, it is important to ensure that the longitudinal sides 24 are inboard of the longitudinal sides 14 of the topsheet web 10. In some forms, the longitudinal side 24 can be disposed 2 mm long inward, more than 3 mm long inward, more than 4 mm long inward, 5 mm long inward, or about 6 mm long inward, specifically all values within these ranges and any ranges created thereby. The distance between the longitudinal side 14 and the longitudinal side 24 can be beneficial when the seal of the final product is made. A larger distance can ensure a robust seal between the topsheet and the backsheet and / or another layer in the final absorbent product.
[0038] It should be noted that in general, the affinity layer may be advantageously trimmed and not necessarily be part of the edge seal of the article, as this may lead to leakage. For example, the topsheet may include multiple layers of nonwoven material. The layer facing the wearer may be hydrophobic and the underlayer may be hydrophilic. In such a configuration, the underlayer may be cut so that the longitudinal edge of the underlayer is inside the edge of the hydrophobic layer. In addition, the longitudinal edge of the underlayer may be spaced inside the wings extending laterally outward. In such a configuration, the hydrophobic layer may extend into the wings, while the hydrophilic layer may terminate inside the wings and / or inside the edge seal of the absorbent article.
[0039] The separate portions of the FM web 20A are placed on the topsheet web 10, thereby forming a topsheet and FM layer laminate web 35, hereafter "TFM laminate web." As shown, the TFM laminate web 35 may be subjected to a first unit operation 40. The first unit operation 40 may mechanically manipulate the TFM laminate web 35 to create a bond between the topsheet web 10 and the separate portions of the FM web 20A, thereby forming a final web 58. Various mechanical operations that may create a bond between the topsheet and the FM layer are described below. Suitable mechanical operations are described in more detail below.
[0040] 3A and 4, the cut and place operation 30 can cut the FM web 20 into any suitable shape. For example, the separate portion of the FM web 20A can be dog-bone shaped (two bulbous ends with a narrow middle portion connecting the bulbous ends). As another example, the separate portion 20A can be tapered at the first end and / or the second end to facilitate folding of the article. In yet another embodiment, the separate portion 20A can include a shape that conveys a particular orientation of the article in which the separate portion is placed. For example, a front end of the separate portion 20A can be narrower than an opposite rear end of the separate portion 20A. As another example, the front end may include multiple corrugations having a small radius, while the rear end has a large radius. Each of these configurations may convey to the wearer the proper orientation of the article in which the separate portions 20A are placed. If no FM layer is provided, the FM web 20 of Figures 3A and 4 may be replaced by an absorbent core web. Alternatively, the FM layer and absorbent core web may be provided to a cutting and placing operation 30 and then processed as described herein.
[0041] The form of the final web 58 can vary widely depending on the unit operations involved and the manner in which the corresponding web is processed. Figures 3B-3F disclose additional processing options resulting in different final webs 58. Now referring to Figures 3B and 4, the TFM laminate web 35 can be subjected to two or more unit operations. For example, after passing through the first unit operation 40, the TFM laminate web 35 can become an intermediate web 48. The intermediate web 48 can then be subjected to a second unit operation 50. Similar to the first unit operation 40, the second unit operation 50 can provide further intimacy between the topsheet web 10 and the separate portions of the FM web 20A. After passing through the second unit operation 50, the intermediate web 48 becomes the final web 58.
[0042] The TFM laminate web 35 may be subjected to one or more unit operations in addition to the needlepunch or spunlace (hydroentanglement) operation. Further details regarding some exemplary unit operations are provided below. The order of operations in these processes may be interchanged unless otherwise specified. For example, the TFM laminate web 35 may be subjected to needlepunch and / or hydroentanglement before being subjected to a separate unit operation as described herein, or vice versa. If no FM layer is provided, the FM web 20 of Figures 3B and 4 may be replaced by an absorbent core web. Alternatively, the FM layer and absorbent core web may be provided to a cutting and placing operation 30 and then processed as described herein.
[0043] 3C and 4, the topsheet web 10 (shown as a roll) may pass through a first unit operation 40 before being fed to the cutting and placing operation 30. The first unit operation 40 can mechanically manipulate the topsheet web 10 as described herein. After mechanical manipulation by the first unit operation 40, the topsheet web 10 becomes the intermediate topsheet web 11.
[0044] Downstream of the first unit operation 40, the intermediate topsheet web 11 and the FM web 20 may be provided to a cutting and placing operation 30. As previously described, the cutting and placing operation 30 may cut the FM web 20 into separate portions 20A. These separate portions may then be placed onto the intermediate topsheet 11, thereby forming an intermediate topsheet and FM layer laminate, or "iTFM laminate" 148. The iTFM laminate 148 may then be provided to a second unit operation 50, which provides intimate contact between the intermediate topsheet 11 and the separate portions 20A of the FM web 20. After processing by the second unit operation 50, the iTFM laminate 148 becomes the final web 58. The second unit operation 50 may include a hydroentanglement or needle punching operation to consolidate the layers of the iTFM laminate 148, thereby forming the final web 58. Additional unit operations may be provided in the above process to provide further mechanical manipulation of the iTFM laminate 148.
[0045] It should be noted that the topsheet web 10 and the FM web 20 may be interchanged in the process. For example, the FM web 20 may be provided to the first unit operation 40 and then to the cutting and placing operation 30. An unmanipulated topsheet may be provided to the cutting and placing operation 30 together with the improved FM web 20. The remainder of the process may be as described herein. Additionally, the topsheet web 10 may pass through the first unit operation 40 and the FM web 20 may pass through a separate unit operation. The intermediate topsheet 11 and the improved FM web 20 may then be provided to the cutting and placing operation 30. The remainder of the process may be as described herein. If no FM layer is provided, the FM web 20 in Figures 3C and 4 may be replaced by an absorbent core web. Or, the FM layer and the absorbent core web may be replaced by the FM layer 20 and then processed as described herein.
[0046] 3D and 4, the topsheet web 10 and the FM web 20 may be provided to a cutting and placing operation 30 as previously described with respect to FIG. 3A. The resulting TFM laminate 35 may then be exposed to a first unit operation 40. The first unit operation 40 may combine the topsheet and the FM separate portions 20A, thereby creating an intermediate web 48. Downstream of the first unit operation 40, the intermediate web 48 may be provided to a second cutting and placing operation 31. Together with the intermediate web 48, the absorbent core web 18 may be provided to the second cutting and placing operation 31. The second cutting and placing operation 31 may create a plurality of separate absorbent cores from the absorbent core web 18. As with the separate FM portions, the separate absorbent cores may not be coextensive with the topsheet. For example, the longitudinally extending side edges of the separate absorbent cores should be located laterally inward of the longitudinally extending edges 14 of the topsheet web 10. The separate absorbent cores can be larger than the separate FM portions 20A, smaller than the separate FM portions 20A, or the same size as the separate FM portions 20A.
[0047] A plurality of separate absorbent cores and intermediate webs 48 may be combined in a second cutting and placing operation 31, thereby creating an intermediate laminate and absorbent core web laminate 37, hereafter "TFMAC laminate." The TFMAC laminate 37 may then be further processed by a second unit operation 50, thereby producing a final web 58. After the addition of the separate absorbent cores, no further manipulation of the TFMAC laminate 37 may occur. In that case, the TFMAC laminate 37 may be the final web 58.
[0048] The first unit operation may include a hydroentanglement / needlepunch process that combines the topsheet layer and the FM layer of the TFM laminate 35. The second unit operation 50 may include a mechanical manipulation process as described herein that combines the layers of the TFMAC laminate 37.
[0049] Additionally, the topsheet web 10 and / or the FM web 20 may be subjected to separate unit operations before being provided to the cutting and placing operation 30. In conjunction with or independent of these, the absorbent core web 18 may be provided to a unit operation before being provided to the second cutting and placing operation 31.
[0050] 3E and 4, the topsheet web 10 may be provided to a first unit operation 40 that mechanically manipulates the topsheet web 10, thereby forming an intermediate topsheet web 11. The absorbent core web 18 and the FM web 20 may be provided to a second unit operation 50 that mechanically manipulates the absorbent core web 18 and the FM web 20, thereby forming an absorbent core and FM web laminate, hereafter "FMAC", laminate web 49. The intermediate topsheet web 11 and the FMAC laminate web 49 may then be provided to a cutting and placing operation 30. The cutting and placing operation 30 may cut separate portions from the FMAC laminate web 49. The cutting and placing operation 30 may combine the intermediate topsheet 11 web and the separate portions of the FMAC laminate web 49 to create an iTFMAC laminate 137. The iTFMAC laminate web 137 may then be provided to a third unit operation that consolidates the layers of the iTFMAC laminate web 137.
[0051] 3F and 4, as shown, the topsheet web 10 can be provided to the cutting and placing operation 30 in an unmanipulated state, i.e., without the first unit operation 40. After the cutting and slipping operation 30, a separate portion of the FMAC laminate web 49 is combined with the topsheet to create the TFMAC laminate 37. In some forms, the TFMAC laminate web 37 may not undergo further operations other than the processing required to create an absorbent article from the TFMAC laminate web 37. In that case, the TFMAC laminate web 37 may also be the final web 58. Additionally, the FM web 20 and the absorbent core web 18 may be subjected to separate unit operations before being provided to the cutting and placing operation 30.
[0052] 3E and 3F, the absorbent core web 18 may be subjected to a cutting and placing operation and joined to the FM layer web 20 in a plurality of separate absorbent cores. The advantage of providing the absorbent core web 18 to the cutting and placing operation before joining with the FM layer web 20 is that the cutting and placing operation can shape the separate absorbent cores as desired. In contrast, when the FM layer web 20 and the absorbent core web 18 are provided together to the cutting and placing operation, the shapes of the separate FM portions and the separate absorbent cores are likely to be the same. Therefore, to maximize the design flexibility of the absorbent article, it may be advantageous to provide the absorbent core web 18 to the cutting and placing operation and then join the separate absorbent cores to the FM layer web 20.
[0053] The unit operations of the present disclosure can impart a variety of different features / structures to the web that is subjected to the unit operations. Below, we discuss some suitable structures / features for creating tight contact between adjacent absorbent article layers that can be formed through the unit operations. As discussed below, tight contact features include conforming features, but conforming features are a smaller subset of tight contact features, since not all tight contact features include conforming features.
[0054] In the discussion of suitable features / structures, unless otherwise noted, the general term "modified web" shall be utilized in place of intermediate topsheet 11, intermediate web 48, iTFM laminate web 148, TFMAC laminate web 37, iTFMAC laminate web 137, FMAC laminate web 49, and final web 58, or any web that has been mechanically manipulated by a unit operation. Thus, the features / structures described below may apply to the webs described herein. The term "precursor web" shall be utilized to refer to webs that have not been modified (mechanically manipulated) by a unit operation, such as topsheet web 10, FM web 20, absorbent core web 18, combinations thereof, and TFM laminate 35, or those webs that are upstream of one or more unit operations that create a bond between two adjacent webs or portions thereof.
[0055] Unit Operation There are several unit operations that can be utilized to create intimate contact between adjacent layers of an absorbent article, some examples are described in more detail below.
[0056] Spunlace One example of a process for creating cohesion between layers is hydroentanglement, or spunlacing. In a spunlacing unit operation, a precursor web or modified web is subjected to high-velocity water jets that interengage the filaments and / or fibers of the nonwoven web. In addition to providing structural integrity to the resulting laminate, the spunlacing process can create cohesion between nonwoven webs by creating Z-direction integration of the filaments and / or fibers of the nonwoven web. Spunlacing processes are generally known in the art. Any unit operation or operations described herein may include a spunlacing process.
[0057] Needle punch Another example is needle punching. Similar to spunlacing, the needle punching process can create cohesion between layers by creating Z-direction integration of the filaments and / or fibers of a nonwoven web. Needle punching involves mechanical interengagement of the filaments and / or fibers of a spunbonded, carded, or woven web. In the needle punching process, multiple barbed needles repeatedly pass through a precursor web or modified web, pushing the filaments and / or fibers of the web in the positive and / or negative Z direction. Needle punching processes are generally well known in the art. Any unit operation or operations thereof described herein may include a needle punching process.
[0058] Protrusions / recesses Some examples of suitable unit operations for forming intimate contact between layers of an absorbent article include unit operations capable of forming protrusions in a precursor web. With reference to FIG. 5, some unit operations described herein can produce a modified web 335 that includes protrusions 460 in the positive and / or negative Z direction. Protrusions in the negative Z direction can also be referred to as recesses. Generally, the protrusions 460 include a distal end 462 and a sidewall 466 that connects the distal end to a base portion 450. The base portion 450 connects the sidewall 466 to the first surface 60 or the opposing second surface 62 of the modified web 335. Protrusions of the present disclosure may include outer tufts, tunnel tufts, solid tufts, nested tufts, ridges and grooves, and corrugations.
[0059] It should be noted that passing the precursor web between two rolls (with opposing protrusions and grooves) with a relatively narrow gap tends to impart some shear and compression forces to the material. However, this process differs from the embossing process, in which teeth, or male members, press the precursor web against the bottom of the opposing roll, or female element, thereby increasing the density of the material in the compressed areas. Instead, the process described herein displaces the material, and although density changes occur, they are negligible compared to the density changes created by embossing.
[0060] 6A, unit operations 40, 50, and 60 (shown in FIGS. 3A-3F) may include an apparatus 500 for forming tufts in modified web 335. Apparatus 500 includes a pair of intermeshing rolls 502 and 504, each rotating about an axis A, which are parallel and coplanar. Roll 502 includes a plurality of ridges 506 and corresponding grooves 508 that extend uninterruptedly around the entire circumference of roll 502.
[0061] Depth of engagement (DOE) is a measure of the level of intermeshing of the rolls 502 and 504. The DOE should be selected to provide the desired structure. For fluid management purposes, the DOE should be selected to ensure sufficient adhesion to the constituent materials of the layers being manipulated. In addition, the gap between the ridges and grooves is highly dependent on the caliper of the materials being manipulated. For example, if a topsheet, FM layer, and absorbent core layer are being manipulated, the gap between the ridges and grooves may need to be larger than for just the topsheet and FM layer. If the gap is too small, the web may tear.
[0062] Roll 504 is similar to roll 502, but rather than having ridges that extend in an uninterrupted fashion around the entire circumference, roll 504 includes a plurality of circumferentially extending rows of ridges that are modified to result in rows of circumferentially spaced teeth 510 that extend in spaced apart relationship around at least a portion of roll 504. The individual rows of teeth 510 of roll 504 are separated by corresponding grooves 512. During operation, rolls 502 and 504 intermesh such that the ridges 506 of roll 502 extend into the grooves 512 of roll 504 and the teeth 510 of roll 504 extend into the grooves 508 of roll 502. A nip 516 is formed between the counter-rotating, intermeshing rolls 502 and 504. Either or both of rolls 502 and 504 may be heated by means known in the art, such as using hot oil filled rollers or electrically heated rollers.
[0063] Apparatus 500 is shown in a configuration with one patterned roll, e.g., roll 504, and one grooved roll 502 without a pattern. However, it may be preferable to use two patterned rolls similar to roll 504 with the same or different patterns in the same or different corresponding areas of each roll. Such an apparatus can produce a modified web 335 with tufts protruding from both sides of the modified web 335, i.e., tufts extending in the positive Z direction and tufts extending in the negative Z direction. Also, different rolls with different patterned areas can be utilized to create different operational zones with different fluid handling and / or different mechanical properties and performance. Such configurations are described below.
[0064] The modified web 335 of the present disclosure can be made by mechanically deforming a precursor web 100, which may be described as generally planar and two-dimensional, prior to processing by the apparatus shown in FIG. 6A. "Planar" and "two-dimensional" simply mean that the precursor web 100 may begin the process in a generally flat state, whereas the modified web 335, which has a distinct out-of-plane Z-direction three-dimensionality due to the formation of the tufts 570. "Planar" and "two-dimensional" do not imply any flatness, smoothness or dimensionality. The intermeshing rolls 502 and 504 can urge the material of the precursor web 100 in a positive Z-direction or a negative Z-direction, depending on whether the roll 504 engages the second surface 62 or the first surface 60 (shown in FIG. 5).
[0065] 3A-6A, the process described with respect to FIG. 6A can provide a variety of tufts, such as tunnel tufts, solid tufts, and outer tufts. For example, tunnel tufts can be created when a localized area of the precursor web 100's constituent material is forced in the positive Z direction such that the material of the precursor web 100 in the localized area is forced toward the first surface 60 of the modified web 335. The localized area can be disposed immediately above the first surface 60. It should be noted that the webs shown in FIGS. 3A-5 include multiple layers, such as the topsheet web 10 and the separate portion 20A of the FM web 20. Thus, when the precursor web 100's constituent material is forced in the positive Z direction, the tunnel tufts can include, for example, the constituent material of the separate portion 20A of the FM web 20, and the topsheet web 10 can form, for example, the outer tufts.
[0066] In contrast, when a localized area of the constituent material of the precursor web 100 is forced in the negative Z direction, the material of the precursor web 100 in the localized area may be forced toward the second surface 62. The constituent material may be disposed below the second surface 62 of the modified web 335. When the constituent material of the precursor web 100 is forced in the negative Z direction, the tunnel tufts may be formed, for example, by the topsheet web 10 and the outer tufts may be formed, for example, by the separate portions 20A of the FM web 20.
[0067] A photograph of a suitable roll for use with apparatus 500 is shown in Figure 6B. As shown, the roll includes teeth 510 and a plurality of open areas 511. Each of the open areas 511 is separated by a tooth 510 disposed therebetween. The pattern of teeth 510 and open areas 511 corresponds to the recesses and nodes of Figures 12A-12C, 13A-13C, and 15A-15C, respectively.
[0068] In addition to or independent of the tufts described above, the modified web 335 may include solid tufts. Solid tufts may occur when the precursor web 100 includes crimped filaments. When the precursor web 100 of the present invention includes crimped filaments, the precursor web 100 has a higher caliper for a given basis weight. This higher caliper in turn can provide consumer benefits of comfort due to cushion-like softness, more rapid absorbency due to higher transmittance, and improved masking. Additional benefits may include reduced red staining, more breathability, and elasticity. The crimped filaments may be utilized in various layers of the absorbent article. For example, the topsheet web 10 may include crimped filaments, the FM web 20 may include crimped filaments, and / or the absorbent core may include crimped filaments.
[0069] The difference between solid tufts and tunnel tufts is that solid tufts are generally filled with filaments. Due to the nature of crimped filaments, mechanical manipulations tend to simply unravel the filaments to some extent. In contrast, non-crimped filaments can be stretched and thinned during mechanical manipulations. This stretching and thinning generally means that the resulting tufts have less fiber in their internal space and therefore look more like tunnels. Methods of making tunnel tufts, outer tufts, and solid tufts are described in further detail in U.S. Patent Nos. 7,172,801, 7,838,099, 7,754,050, 7,682,686, 7,410,683, 7,507,459, 7,553,532, 7,718,243, 7,648,752, 7,732,657, 7,789,994, 8,728,049, and 8,153,226. Solid tufts and corresponding outer tufts are described in further detail in U.S. Patent Application No. 2016 / 0166443.
[0070] 3A-6A, the apparatus 500 for forming tufts in precursor web 100 may be first unit operation 40, second unit operation 50, and / or third unit operation 60. In some configurations, the apparatus 500 may be the only operation, other than cutting and placing operations 30 and 31, that provides intimate contact between layers of precursor web 100. Additionally, configurations are contemplated in which tufts, such as tunnel, outer, and / or solid tufts, are provided on modified web 335 in both the positive Z and negative Z directions.
[0071] Yet another form of protrusion suitable for the modified web 335 of the present disclosure includes nested tufts. 7A-7D show an apparatus 600 suitable for use as a unit operation according to the present disclosure. As shown, precursor web 100 may be subjected to apparatus 600. Apparatus 600 may include forming members 602 and 604, which may be in the form of non-deforming, intermeshing counter-rotating rolls forming a nip 606 therebetween. Precursor web 100 may be fed into nip 606 between rolls 602 and 604. The gap between rolls 602 and 604 is described herein as a nip, although, as discussed in more detail below, in some cases it may be desirable to avoid compression of precursor web 100 as much as possible.
[0072] A first forming member (e.g., "male roll") 602 has a surface with a plurality of first forming elements, including separate, spaced apart male forming elements 612. These male forming elements are spaced apart in the machine direction and the cross machine direction. The term "separate" does not include continuous or non-separate forming elements, such as, for example, ridges and grooves on a corrugating roll (or "ring roll"). Such corrugating rolls have ridges that may be spaced apart in one of the machine direction and the cross machine direction, but not in both directions.
[0073] 7B, the male molding element 612 has a base 616 that is joined (in this case integrally formed) to the first molding member 602, a top surface 618 spaced from the base, and sidewalls (or "sides") 620 that extend between the male molding element's base 616 and top surface 618. The molding element 612 also has a planar perimeter and a height H1 (the latter measured from the base 616 to the top 618).
[0074] 7A-7D, the second molding member (e.g., "female roll") 604 has a surface 624 with a plurality of cavities or recesses 614. The recesses 614 are aligned and configured to receive the male molding elements 612 therein. The male molding elements 612 thus mate with the recesses 614 such that the single male molding element 612 fits within the perimeter of the single recess 614 as well as at least partially within the recess 614 in the Z direction. The recesses 614 have a planar perimeter 626 that is greater than the planar perimeter of the male elements 612. As a result, when the rolls 602 and 604 are interlocked, the recesses 614 on the female roll 604 can fully contain the male molding elements 612. As shown in FIG. 7C, the recesses 614 have a depth D1 that may be greater than the height H1 of the male molding elements 612 in some forms. The recess 614 has a planar configuration, sidewalls 628, a top edge or rim 634 around the top of the recess where the sidewalls 628 meet the surface 624 of the second molding member 604, and a bottom edge 630 around the bottom 632 of the recess where the sidewalls 628 meet the bottom 632 of the recess.
[0075] As mentioned above, the recesses 614 may be deeper than the height H1 of the molding elements 612 so that, as much as possible, the precursor web 100 is not pinched (or compressed) between the male molding elements and the recesses.
[0076] Depth of engagement (DOE) is a measure of the level of interlocking of forming members. As shown in Figure 7C, the DOE is measured from the apex 618 of the male element 612 to the (outermost) surface 624 of the female forming member 614 (e.g., a roll with recesses). The DOE must be high enough to create nested tufts when combined with a stretch nonwoven material.
[0077] 7C, there is a gap C between the side 620 of the molding element 612 and the side (or sidewall) 628 of the recess 614. The gap and DOE have a relationship in that if the gap is larger, a deeper DOE can be used. The gap C between the male roll and the female roll can be the same around the circumference of the molding element 612, or it can vary. For example, the molding member can be designed such that the gap between the side of the molding element 612 and the adjacent sidewall 628 of the recess 614 is narrower than the gap between the sidewall at the end of the male element 612 and the adjacent sidewall of the recess 614. In other cases, the molding member can be designed such that the gap between the sidewall 620 of the male element 612 and the adjacent sidewall 628 of the recess 614 is wider than the gap between the sidewall at the end of the male element 612 and the adjacent sidewall of the recess. In still other cases, the gap between a sidewall on one side of the male element 612 and the adjacent sidewall of the recess 614 may be wider than the gap between a sidewall on the opposite side of the same male element 612 and the adjacent sidewall of the recess. For example, there may be different gaps at each end of the molding element 612 and / or there may be different gaps on each side of the male element 612.
[0078] Some of the aforementioned forming element 612 configurations alone or in conjunction with the second forming element 604 and / or recess 614 configurations may provide additional benefits. This may be by more firmly securing the precursor web 335 on the male elements 612, which may result in more uniform and controlled strain in the precursor web 335. The apparatus 600 is further described in U.S. Patent Application Publication No. 2016 / 0074252.
[0079] As shown in Figure 7D, the precursor web 100 may be subjected to a nip 606 between a first roll 602 and a second roll 604. As the precursor web 100 passes through the nip 606, a forming member 612 engages the second surface 62 (shown in Figure 5) of the precursor web 100 and urges the constituent material of the precursor web 100 into the recesses 614. This process forms a modified web 335 having a flat first surface and a plurality of integrally formed nested tufts extending outwardly from the first surface 60 (shown in Figure 5) of the modified web 335 (of course, if the second surface 62 of the modified web 335 were placed in contact with the second forming member 604, the nested tufts would extend outwardly from the second surface 62 of the modified web 335 and openings would be formed in the first surface 60 of the modified web 335).
[0080] 3A-4 and 7A, an apparatus 600 for forming nested tufts in a modified web 335 may be the first unit operation 40, the second unit operation 50, or the third unit operation 60. The apparatus 600 may be the only operation, other than the cutting and placing operations 30 and 31, that provides intimate contact between the topsheet web 10, the separate portions 20A of the FM layer web 20, and / or the separate portions of the absorbent core web 18. The processes and apparatus for making the nested tufts described herein are further described in U.S. Patent Application Publication Nos. 2016 / 0074256 and 2016 / 0074252 A1.
[0081] Other suitable protrusions that may be included in the modified web 335 of the present disclosure include ridges and grooves or corrugations. With reference to FIGS. 8A-8D, an apparatus 2200 may be utilized to create corrugations in a precursor web. The apparatus 2200 includes a pair of counter-rotating intermeshing rolls 2202, 2204 that form a single nip N therebetween. As shown in FIGS. 8A and 8B, the first roll 2202 includes a plurality of grooves 2210 and ridges 2220, as well as a plurality of staggered, spaced apart teeth 2230 that extend outwardly from the upper surfaces 2222 of the ridges 2220. The configuration of the roll 2202 is such that the upper surfaces 2222 of the ridges 2220 are directionally disposed between the distal ends 2234 of the teeth 2230 and the lower surfaces 2212 of the grooves 2210, relative to the axis A of the roll.
[0082] As shown, the second roll 2204 includes a plurality of grooves 2240 and ridges 2250. The grooves 2240 have a lower surface 2242 and the ridges 2250 have an upper surface 2252, where the distance between the upper surface 2252 of the ridges 2250 and the lower surface 2242 of the grooves 2240 is substantially the same around the circumference of the roll. The teeth 2230 and ridges 2220 of the first roll 2202 extend toward the axis A of the second roll 2204 and engage to a depth beyond the upper surfaces 2252 of at least some of the ridges 2250 on the second roll 2204.
[0083] Teeth suitable for this process may contribute to the perforation of the web. The teeth on the roll may have any suitable configuration. A given tooth may have the same plan view length and width dimensions (such as a tooth with a circular or square plan view). Alternatively, a tooth may have a length greater than its width (such as a tooth with a rectangular plan view), in which case the tooth may have any suitable aspect ratio of its length to its width. Suitable configurations of teeth include, but are not limited to, teeth with triangular, quadrangular or rectangular sides, cylindrical, pyramidal sides, teeth with plan configurations including circular, elliptical, hourglass, star, polygonal, and the like, and combinations thereof. Polygonal shapes include, but are not limited to, rectangular, triangular, pentagonal, hexagonal, or trapezoidal. The sidewalls of the teeth may taper at a constant angle from the base to the tip, or the angle may vary. The teeth may taper to a point at the tip of the tooth, such as the tooth shown in FIG. 8A. The teeth can have tips that form rounded, flat, or pointed points. In some forms, the distal ends of the teeth may form a pointed apex with at least one vertical wall of the tooth (e.g., vertical walls at the leading and trailing ends of the tooth) such that the tooth apertures or pierces the web. In some forms, each tooth may form two holes, one at the leading end and one at the trailing end of each tooth.
[0084] Apparatus 2200 can deform a precursor web to produce alternating regions of greater and lesser thickness and greater and lesser basis weight, with the greater thickness and greater basis weight areas located at the tops of the ridges and bottoms of the grooves, and the lesser thickness and lesser basis weight areas located on the intermediate sidewalls. In the case of nonwovens, the basis weight is also reduced in the stretched regions, producing a modified web with alternating regions of greater and lesser basis weight, with the greater basis weight areas located at the tops of the ridges and bottoms of the grooves, and the lesser basis weight areas located on the intermediate sidewalls.
[0085] 3A-4 and 8A, an apparatus 2200 for forming ridges and grooves in a precursor web may be the first unit operation 40, the second unit operation 50, or the third unit operation 60. The apparatus 2200 may be the only operation, other than the cutting and placing operations 30 and 31, that provides intimate contact between the topsheet web 10, the separate portions 20A of the FM layer web 20, and / or the separate portions of the absorbent core web 18.
[0086] Any suitable process for forming the ridges and grooves may be utilized. Some additional processes for creating ridges and grooves in a web are described in U.S. Patent Nos. 6,458,447, 7,270,861, 8,502,013, 7,954,213, 7,625,363, 8,450,557, 7,741,235, U.S. Patent Application Publication Nos. 2003 / 018741, 2009 / 0240222, 2012 / 0045620, 20120141742, 20120196091, 20120321839, 2013 / 0022784, 2014 / 0022786, 2014 / 0022788, 2014 / 0022789, 2014 / 0022791, 2014 / 0022792, 2014 / 0022794, 2014 / 0022796, 2014 / 0022798, 2014 / 002279 ... This is described in detail in International Publication Nos. 2013 / 0017370, 2013 / 013732, 2013 / 0165883, 2013 / 0158497, 2013 / 0280481, 2013 / 0184665, 2013 / 0178815, 2013 / 0236700, WO 2008 / 156075, 2010 / 055699, 2011 / 125893, 2012 / 137553, 2013 / 018846, 2013 / 047890, and 2013 / 157365.
[0087] As mentioned above, the protrusions may be oriented in the positive Z direction or the negative Z direction. In the positive Z direction, the protrusions may have some shape associated with them, assuming there is no construction material surrounding the protrusions. However, when oriented in the negative Z direction, these protrusions / recesses may not have much to them and may simply include side walls and bottoms. The compressive forces of the surrounding construction material may force these recesses to have a very similar shape when oriented in the negative Z direction.
[0088] It should be noted that spunlace and needlepunch operations are typically utilized primarily to create integrity within the web. However, as discussed above, both spunlace and needlepunch processes can also provide some degree of intimacy between adjacent layers. These processes operate on a microscale. In other words, they transfer small amounts of component material at multiple locations on the web.
[0089] In contrast, without being bound by theory, it is believed that the process for forming conformal features can provide additional benefits over needle punching and spunlacing. Rather than operating at the microscale, the process for conformal features operates at the mesoscale. These mesoscale processes involve the movement of larger amounts of component material. For example, needle punching may involve the movement of 1-10 fibers, whereas mesoscale mechanical processes may involve more than 10 up to 100 fibers or more. In contrast, the features of the mesoscale processes described herein may have lengths ranging from about 3 mm to 11 mm, by way of example. There are patterns that can utilize longer teeth and patterns that can utilize shorter ones. However, a length of about 1 mm is probably the minimum that can be expected for a mesoprocess.
[0090] Thus, spunlace and / or needle punch processes may be utilized, but mesoscale mechanical processes may also be provided to the precursor web to achieve additional benefits, such as conformability and / or resilience. Also, recall that mesoscale processes are different from embossing. Embossing provides a densified bottom surface where the building material is compressed, whereas any densification in the bottom surface created by mesoscale processes is relatively small. In addition, conforming features created by mesoscale processes are generally visible to the naked eye from a suitable distance, e.g., 30 cm, without the use of a microscope, assuming the observer has corrective or unaided visual acuity of 1.0 (20 / 20) or better. Depending on the layer subjected to the mesoscale process, the topsheet and / or secondary topsheet may need to be removed from the article to see the conforming features. In contrast, microscale processes may require the use of a microscope to determine their presence. Some suitable examples of conforming features include protrusions, ridges, grooves, recesses, tufts, and the like.
[0091] Additional Processes hole Suitable unit operations that provide some benefit in fluid management include holes. However, for purposes of this disclosure, holes are not considered to be conforming features. With reference to FIGS. 3A-3F and 9A-9B, the first unit operation 40 or the second unit operation may include an aperture process. For example, the unit operations described herein may include a thinning roller configuration 108 and an incremental stretching system 132. The precursor web 100 may be thinned in multiple distinct densified thinned regions by passing through a nip 106 of a thinning roller (or strong bond) configuration 108 formed by rollers 110 and 112, thereby forming a thinned precursor web 100'. The thinned precursor web 100 after passing through the nip 106 has a pattern of strong bonds or densified thinned regions. At least some or all of these strong bonds are used to form holes in the web of the present disclosure, and thus the pattern of strong bonds can generally correlate with the pattern of holes formed in the web of the present disclosure.
[0092] 9A, the attenuating roller configuration 108 may include a patterned calender roller 110 and a smooth anvil roller 112. One or both of the patterned calender roller 110 and the smooth anvil roller 112 may be heated, and the pressure between these two rollers may be adjusted to provide the desired temperature (if applicable) and pressure to simultaneously attenuate and melt stabilize (i.e., strongly bond) the precursor material web 100 at the multiple locations 202. After the precursor web 100 passes through the attenuating roller configuration 108, the attenuated precursor web 100 may be stretched in the CD or approximately the CD by a transverse tensile force to at least partially or completely break the multiple attenuated melt stabilized locations 202, as described in more detail below.
[0093] The patterned calender roller 110 is configured with a cylindrical surface 114 and a plurality of protrusions or pattern elements 116 extending outwardly from the cylindrical surface 114. The pattern elements 116 are illustrated as a simplified example of the patterned calender roller 110, however, more detailed patterned calender rollers are contemplated and described below. The protrusions 116 may be arranged in a predetermined pattern, with each protrusion 116 configured and arranged to generate thinned melt-stabilized sites in the thinned precursor material 102 to achieve the predetermined pattern of thinned melt-stabilized sites 202. The protrusions 116 may correspond one-to-one to the pattern of melt-stabilized sites in the thinned precursor material 102. As shown in FIG. 9A, the patterned calender roll 110 can have a repeating pattern of protrusions 116 that extend around the entire circumference of the surface 114. Alternatively, the protrusions 116 may extend around a portion or portions of the circumference of the surface 114. Additionally, a single patterned calender roller may have multiple patterns in various zones (i.e., first zone, first pattern, second zone, second pattern, etc.). Protrusions 116 extend radially outward from surface 114 and may have a tip surface 117. Anvil roller 112 may be a smooth-surfaced cylinder made of steel, rubber, or other material. Anvil roller 112 and patterned calender roller 110 may be swapped (i.e., anvil up) to achieve similar results.
[0094] 9A and 9B, from the thinning roller configuration 108, the thinned precursor web 100 passes through a nip 130 formed by an incremental stretching system 132 that employs opposed pressure applicators having three-dimensional surfaces that are at least somewhat complementary. After the thinned precursor web 100' passes through the nip 130, the thinned precursor web 100' becomes a modified web 335.
[0095] The incremental stretching system 132 includes two incremental stretching rollers 134 and 136. The incremental stretching roller 134 may include a plurality of teeth 160 and corresponding grooves 161 disposed around the entire circumference of the roller 134. The incremental stretching roller 136 may include a plurality of teeth 162 and a plurality of corresponding grooves 163. The teeth 160 of the roller 134 may intermesh or engage with the grooves 163 of the roller 136, and the teeth 162 of the roller 136 may intermesh or engage with the grooves 161 of the roller 134. As the thinned precursor web 100' having the thinned melt stabilized points 202 passes through the incremental stretching system 132, a CD tension is applied to the thinned precursor web 100' to stretch (or activate) the thinned precursor web 100' in the CD or approximately in the CD. Additionally, the thinned precursor web 100' may be tensioned in the MD or approximately in the MD. The CD tension on the thinned precursor web 100' is adjusted so that the thinned melt stabilized locations 202 at least partially or completely break to form a plurality of partially formed or formed holes 204 aligned with the thinned melt stabilized locations 202 in the modified web 335. The melt stabilized locations 202 form melt lips that define the perimeters of the holes 204. However, the bonds of the thinned precursor web 100' (in the non-strong bond regions) are strong enough that many do not break during the application of tension, thereby maintaining the thinned precursor web 100' in integrity even as the thinned melt stabilized locations break. However, some bond rupture during tensioning may be desirable.
[0096] The holes 204 may be of any suitable size. For example, the holes 204 may be approximately 0.1 mm 2 ~about 15mm 2 , about 0.3mm 2 ~ approx. 14mm 2 , about 0.4mm 2 ~ approx. 12 mm 2 , approx. 1.0 mm 2 ~about 5mm 2 and specifically, every 0.05 mm within the specified range. 2 and all ranges therein or formed thereby. All effective open area percentages are determined using the Opening Test described herein. Effective open area is further described in U.S. Patent Application Nos. 2016 / 0167334, 2016 / 0278986, and 2016 / 0129661. Smaller pores may be more aesthetically appealing to a user of the absorbent article, but smaller pores may negatively impact fluid acquisition rate.
[0097] The process described in Figures 9A and 9B illustrates one suitable process for forming holes. Some additional processes for perforating a web are described in U.S. Patent Nos. 8,679,391 and 8,158,043, and U.S. Patent Application Publication Nos. 2001 / 0024940 and 2012 / 0282436. Other methods for perforating a web are provided in U.S. Patent Nos. 3,566,726, 4,634,440, and 4,780,352. Additionally, holes may be provided in a pattern in the modified web of the present disclosure. Processes for forming hole patterns and some suitable hole patterns are disclosed in U.S. Patent Application Publication Nos. 2016 / 0167334, 2016 / 0278986, and 2016 / 0129661.
[0098] zone The unit operations described herein and the features provided thereby may be provided in an absorbent article in a zone configuration. A zone is an area that exhibits one of the following: a visual pattern, a topography, an absorption rate or characteristic, a bending parameter, a compressive modulus, a resilience, an elongation parameter, or any combination thereof, that is different from another part of the absorbent article. A visual pattern may include any known geometric shape or pattern that can be seen by the eye and conceived by the human mind. A topography may be any known pattern that can be measured and conceived by the human mind. A zone may be repeated or distinct. A zone may be orthogonal shapes and continuities that provide a visual appearance.
[0099] The use of zones allows for tailoring of fluid handling and mechanical properties of and within the pad. The integrated absorbent structure may have one or more visual patterns that include zones along either the longitudinal or transverse axis of the integrated layer. The integrated layer may have two or more zones that include one or more visual patterns. The two or more zones may be separated by a boundary. The boundary may be a topographical boundary, a mechanical boundary, a visual boundary, a boundary of fluid handling properties, or a combination thereof, when the boundary is not a densified portion of the absorbent core structure. The boundary properties may be different from the two zones adjacent to the boundary. The absorbent structure may have a peripheral boundary that exhibits properties at the border that are different from one or more adjacent zones.
[0100] One specific example of a process by which zones can be provided is shown in Figure 10. As shown, incremental stretching system 832 may include rolls 834 and 836. As shown, precursor web 100 may include multiple melt stabilization stations 722 prior to entering nip 816. Recall that melt stabilization stations 722 may be provided in zones on thinning precursor web 100' (as shown in Figures 9A and 9B). In the case of incremental stretching system 832, melt stabilization stations 722 may be provided in central zone 813.
[0101] Upon stretching in the CD in the portion of apparatus 832 corresponding to region 813, the melt-stabilized locations 722 rupture to form holes. Again, the melt-stabilized locations 722 may be limited to a central region of modified web 335. However, if melt-stabilized locations 722 are provided throughout precursor web 100, holes 2214 will be formed in region 813, while a combination of protrusions and holes may be formed in region 811.
[0102] As shown, the apparatus 832 includes a pair of rolls 834 and 836 each rotating about a parallel axis A. The roll 834 may be configured as described with respect to the roll 502 (shown in FIG. 6A). That is, the roll 834 may include a plurality of circumferentially extending ridges 760 separated by grooves 761. The second intermeshing roll 836 has an essentially matching roll 834 and includes a central region 813 having ridges 762 separated by grooves 763. The intermeshing ridges 760, 762 and grooves 761, 763 of the rolls 834 and 836 incrementally stretch the intermediate web 48 to form the holes 2214. In addition to the region 813, the roll 836 has two regions 811 including ridges having teeth 810 formed therein, the toothed ridges being separated by grooves 812. The ridges 760 of roll 834 interlock with the grooves 812 of roll 836 to form the tufts described herein. Combining both in one apparatus forms both the holes 2212 and the tufts 230 in the precursor web 100.
[0103] The depth of engagement between the toothed ridges and the grooves may vary around the circumference of the roll. In this case, protrusions with different heights and widths may be formed. For example, the depth of engagement in the front region of the absorbent article may be smaller than the depth of engagement in the center of the article. A higher depth of engagement in the center may form protrusions that facilitate liquid acquisition in the absorbent article.
[0104] The modified web 335 of the present disclosure may include various zones. For example, the modified web 335 may include zones that provide improved fit and fluid dynamics, while other zones may provide a soft feel to the user along with increased structural integrity. As discussed above, the zones of the absorbent article may include various layers of the absorbent article as well. Thus, one zone may include a fitting feature, while another zone may include a fitting feature, a combination of fitting and fitting features, a different arrangement of fitting features, etc.
[0105] In one particular example, one or more zones may comprise holes along the protrusions / recesses, e.g., tunnel tufts, solid tufts, nested tufts, or ridges and grooves. In one particular configuration, a first portion of the protrusions (tunnel, solid, or nested) may face in the positive Z direction, while a second portion may face in the negative Z direction. In another particular configuration, a zone may include a combination of tunnel, solid, or nested tufts. In such a configuration, the first portion may face in the positive Z direction and the second portion may face in the negative Z direction. Alternatively, configurations are contemplated in which at least one zone of the modified web 335 includes both holes and protrusions in either the positive and / or negative Z direction.
[0106] Further zone configurations are contemplated. For example, the zones may be positioned individually along the length of the absorbent article. An exemplary absorbent article 1510 is shown in FIG. 11A. Although the absorbent article 1510 is shown in the form of a feminine hygiene pad, the zones described herein may be applied to the absorbent article as desired. The absorbent article 1510 may include zones that extend laterally across the pad. For example, the absorbent article may include a first outer region 1520 disposed at one end of the absorbent article 1510 and an opposing second outer region 1540 disposed at an opposite end of the absorbent article 1510. Between the first outer region 1520 and the second outer region 1540 is a target region 1530. The dashed lines shown in FIG. 11A are imaginary and indicate an exemplary delineation between adjacent regions.
[0107] The target area 1530 may comprise approximately one third of the length of the absorbent article together with the first outer area 1520 and the second outer area 1540, respectively. Each of the aforementioned areas may be treated differently to provide different benefits to the user. For example, the first outer area 1520 may be associated with the front of the pad and may comprise the first zone 1525. The first zone 1525 may comprise protrusions that are smaller in scale compared to the protrusions located outside this area. The smaller scale protrusions may be provided to provide a softer, more cushioned feel to the wearer of the absorbent article 1510. The front of the pad may be associated with the user's pubic region, and thus a softer, more cushioned feel may be beneficial. Additionally, the first zone 1525 may comprise more protrusions than the target zone 1535, or vice versa, or may have the same number. Although the first zone 1525 is shown in the form of a rectangle, any suitable shape may be utilized. For example, the first zone 1525 may be in the form of a heart, moon, star, horseshoe, cloud, flower, etc. In some configurations, multiple separate protrusions may form the aforementioned shapes. It should be noted that while the first zone 1525 is associated with the first outer region 1520, the first zone 1525 may not necessarily be limited to the first outer region 1520. Instead, the first zone 1525 may extend to some extent into the target region 1530 and / or to some extent into the second outer region 1540. The target zone 1535 and the second zone 1545 may be similarly configured, e.g., they may extend to some extent into adjacent regions. Alternatively, the zones may extend the entire length of the absorbent article.
[0108] As another example, the target area 1530 may include a target area zone 1535. The target zone 1535 may correspond to an area of the absorbent article 1510 that is expected to receive a fluid insult from the body. For example, in the case of a feminine hygiene pad, the target zone 1535 may be located in an area of the article that corresponds to the vaginal opening during use. In the case of an adult incontinence product, the target zone 1535 may be located in an area of the article that corresponds to the urethral opening.
[0109] Since the target zone 1535 may receive a liquid insult from the body, the target zone 1535 may be engineered to allow the liquid insult to be quickly acquired and distributed to the absorbent core of the article. Thus, the target zone 1535 may be provided with holes as described herein to allow for rapid fluid acquisition. In some forms, the target zone 1535 may be provided with larger protrusions than the first zone 1525 to facilitate liquid acquisition. In some forms, the target zone 1535 may be provided with larger protrusions than those provided with holes in the first zone 1525. In some forms, the target zone 1535 may be provided with protrusions with holes of similar dimensions to the protrusions in the first zone 1525.
[0110] Similar to the first zone 1525, the target zone 1535 is shown in the shape of a rectangle, although any suitable shape may be used. For example, the target zone 1535 may be in the shape of a heart, a star, a horseshoe, a cloud, a flower, etc. Configurations are contemplated in which the holes present in the target zone 1535 are arranged in a pattern. Suitable patterns and methods of making the holes in the pattern are described above. Similarly, configurations are contemplated in which the separate protrusions in the target zone 1535 are arranged in a pattern as indicated by the shape of the target zone 1535.
[0111] The target area 1530 and the target zone 1535 of the absorbent article can play an important role in the functionality of the absorbent article. For example, the target area 1530 and the target zone 1535 should provide a stable but conformable center of the absorbent article close to the source of liquid insult. In some specific configurations, the topsheet, the FM layer, and the absorbent core are mechanically manipulated to form a tight fit between them. In such configurations, protrusions facing the negative Z direction can be beneficial to improve acquisition rate and improve absorbency.
[0112] Also, as another example, the second outer region 1540 may include a second zone 1545. The second zone 1545 may correspond to a region of the article that corresponds to the gluteal sulcus of the wearer. In such a configuration, it may be beneficial to specially treat the second zone 1545 to allow the second zone 1545 to conform to the gluteal sulcus, thereby allowing a better fit of the article to the wearer. The second zone 1545 may be provided with protrusions that increase the flexibility of the second zone 1545, allowing the article 1510 to bend more easily than one without the protrusions. The second zone 1545 may include conforming features as described herein that increase the flexibility / conformity within the second zone 1545. In one particular example, the second zone 1545 may include protrusions that face in the positive Z direction, which may provide assistance for wiping fluids from the body.
[0113] Typically, the stiffest part of an absorbent article is the absorbent core, which is located between the topsheet and the backsheet. Some conventional methods utilized to increase the flexibility of the core are to remove (cut out) the core material where additional flexibility is needed. However, this may increase costs since the absorbent core material is typically discarded after removal. In contrast, for the present disclosure, the absorbent core in the second zone 1545 may include conforming features that increase the flexibility of the absorbent core in the second zone 1545. In some forms, in addition to the absorbent core, the topsheet and / or the FM layer may include conforming features to increase the flexibility of the second zone 1545. Although the second zone 1545 is shown as a triangle, similar to the previously described regions, the second zone 1545 may include any suitable shape. Some examples include a heart shape, a rainbow shape, a star shape, a cloud shape, an animal shape, and the like. In some forms, the conforming features, and the like, may be arranged in a pattern of the previously described shapes.
[0114] Configurations of the present disclosure are contemplated in which the first zone 1525, the second zone 1545, and the target zone 1535 are similarly treated to include conforming features. Such configurations can eliminate some of the need for alignment, since all zones include features of the same size. Configurations are contemplated in which the first zone 1525, the second zone 1545, and the target zone 1535 are similarly treated, but include various layers within their corresponding zones. For example, in some configurations, the first zone 1525 and the second zone 1545 may include mechanical manipulation, e.g., conforming features, of the combination of the FM layer and the absorbent core, e.g., the first layer. However, the target zone 1535 may include mechanical manipulation, e.g., conforming features, of the combination of the topsheet, the FM layer, and the absorbent core, e.g., the second layer. Such a configuration may allow the absorbent article to be designed such that the first zone 1525 and the second zone 1545 focus on comfort and fit of the absorbent article, while the target zone 1535 focuses on reducing fluid acquisition and rewet. Or the zones may include different clinging and / or conforming features. For example, the first zone and / or the second zone may include a first plurality of clinging and / or conforming features, and the target zone may include a second plurality of clinging and / or conforming features, the first plurality differing from the second plurality in at least one of the shape, density (number per square cm), depth, length, shape, and / or spacing (from nearest edge of feature to nearest edge of adjacent feature) between adjacent clinging and / or conforming features.
[0115] As previously mentioned, the shapes of the various zones within the region may be configured as desired. For example, the zones may extend the entire width of the article in the X direction. Regardless of the shapes of the zones within the region shown in Figures 11A and 11B, a first distance 1570 of unmodified or differently modified material may be disposed between the first zone 1525 and the target zone 1535.
[0116] The determination of differently modified and / or unmodified materials may be determined by visual inspection of the materials similar to the identification of conforming features described above. That is, unmodified materials have not been subjected to meso-processing as described herein. For clarity, unmodified materials between adjacent zones may have been subjected to micro-processing such as hydroentanglement and needle punching. Additionally, the differently modified materials may have been subjected to meso-scale processing as described herein, but the differently modified materials may have different conforming features than adjacent zones.
[0117] Similarly, a second distance 1575 of unmodified or differently modified material may be disposed between the target zone 1535 and the second zone 1545. In some configurations, the first distance 1570 may be greater than the second distance 1575. The region of unmodified or differently modified material may help maintain the structure of the absorbent article 1510. This may ensure that the article 1510 maintains some structural integrity that promotes conformability by the article within the desired zone and provides compression resistance. In some configurations, the first distance 1570 may be about 5 mm to about 10 mm or more. In some configurations, the second distance 1575 may be about 5 mm to about 10 mm or more as well. For example, the first distance and / or the second distance may be about 5 mm to about 30 mm, about 7 mm to about 20 mm, or about 9 mm to about 15 mm. The first distance and the second distance represent the shortest straight line distance between the first zone and the target zone or between the target zone and the second zone.
[0118] The zones described herein may be provided in the absorbent article 1510 in any suitable manner. For example, the article 1510 may include a modified web as described herein and may be configured in zones as described above with respect to Figures 11A and 11B. For example, the modified web may include a first zone 1525, a second zone 1545, and a target zone 1535. Additional zone configurations are contemplated.
[0119] In addition to the zone configuration, there are many possible combinations that can be achieved for the zones on the absorbent article based on the process description above. Some of the possible combinations are described below with associated benefits. For example, configurations are contemplated in which the zones are provided uniformly throughout multiple layers, throughout only individual layers, or throughout various combinations of layers. Specifically, at least one of the first zone 1525 or the second zone 1545 may include a clinging feature and / or conforming feature applied to at least two of the topsheet, the FM layer, or the absorbent core. The target zone 1535 may include a clinging feature and / or conforming feature applied to at least two of the topsheet, the FM layer, or the absorbent core, and the combination of layers of the target zone 1535 is different from the first zone 1525. Or these combinations may be the same in these zones. Further configurations are contemplated, including additional material layers disposed between the topsheet and the backsheet. The additional material layers can be treated in one or more zones as described herein.
[0120] 3A, 3B, 3D, 11A, and 11B, in some examples, prior to any unit operation, the topsheet web 10 and the FM layer web 20 can be joined in a cutting and placing operation 30, thereby forming a TFM laminate 35. In such configurations, any operation provided to the TFM laminate 35 is provided to both the topsheet and the FM layer. In such configurations, the first unit operation 40 can provide features to the TFM laminate corresponding to the first zone 1525, the target zone 1535, and / or the second zone 1545. Also, as previously described, these features can help create a tight fit between the topsheet and the FM layer. For any of the zones not provided with features, these zones can remain unmodified.
[0121] In contrast, in Figure 3C, the topsheet web 10 may be mechanically manipulated in a first unit operation 40 before being joined to the FM layer web 20 in the cutting and placing operation 30. The first unit operation 40 may provide features in the topsheet web 10 corresponding to the first zone 1525 and the target zone 1535. In conjunction with or independently of the foregoing, the first unit operation may similarly provide matching features corresponding to the second zone 1545. With respect to any of the zones not provided with features, these zones may remain unmodified.
[0122] The FM layer web 20 may be subjected to a first unit operation 40 before being joined to the topsheet web 10 in the cutting and placing operation 30. In such a configuration, the first unit operation 40 may provide features to the FM layer web 20 corresponding to the first zone 1525, the target zone 1535, and / or the second zone 1545. In such a configuration, the topsheet web 10 may be provided unmodified to the cutting and placing operation 30. With respect to any of the zones not provided with features, these zones may remain unmodified.
[0123] In some forms, the topsheet web 10 and the FM layer web 20 may be subjected to separate unit operations before being joined in the cut and slip operation 30. The separate unit operations can impart features to the topsheet web 10 and / or the FM layer web 20 corresponding to the first zone 1525, the target zone 1535 and / or the second zone 1545, or any combination thereof.
[0124] 3D, 11A, and 11B, in some configurations, the absorbent core may be provided to a cutting and placing operation 31 along with an intermediate laminate 48. The resulting TFMAC laminate 37 may then be provided to a second unit operation 50. The second unit operation 50 may impart features to the TFMAC laminate 37 corresponding to the first zone 1525, the target zone 1535, and / or the second zone 1545. Also, as previously described, the features provided to the TFMAC laminate 37 may create intimate contact between the topsheet, the FM layer, and the AC layer. For any of the zones not provided with features, these zones may remain unmodified.
[0125] 3E, 11A, and 11B, in some configurations, the FM layer web 20 and the absorbent core web 18 may be provided to a second unit operation 50 that imparts features to the FMAC laminate web 49. In such configurations, the features provided to the FMAC laminate web 49 are provided to both the absorbent core web 18 and the FM layer web 20. In some configurations, the second unit operation 50 can impart features described herein corresponding to the first zone 1525, the target zone 1535, and / or the second zone 1545. As previously mentioned, since the absorbent core is typically the stiffest portion of the absorbent article, in some particular configurations, the second unit operation 50 can impart conforming features, such as those corresponding to the second zone 1545, to the FMAC laminate web 49.
[0126] Configurations are also contemplated in which the absorbent core web 18 and the FM layer web 20 are subjected to separate unit operations. In such configurations, features may be imparted to the FM layer corresponding to the first zone 1525, the target zone 1535, and / or the second zone 1545. Similarly, features may be provided to the absorbent core web 18 corresponding to the first zone 1525, the target zone 1535, and / or the second zone 1545. In some particular configurations, the absorbent core web may include conforming features only in the second zone 1545. Or, the absorbent core web may include conforming features corresponding to a different zone than the FM layer web 20.
[0127] 3E, 3F, 9A, and 9B, the topsheet web 10, in some configurations, may be subjected to the first unit operation 40 or may be provided unmodified to the cut and place operation 30. In configurations in which the topsheet web 10 may be subjected to the first unit operation 40, features imparted to the topsheet web 10 may correspond to the first zone 1525, the target zone 1535, and / or the second zone 1545.
[0128] The zone can be further improved by creating a non-boundary material. For example, a configuration is envisioned in which the length of the absorbent core web is shorter than the length of the FM layer. Such a configuration can reduce the amount of absorbent core web utilized in the absorbent article. This can save material costs. An example of a non-boundary configuration is shown in FIG. 11C. As shown, in some configurations, the FM layer 20 and the absorbent core layer 18 can be sandwiched between the topsheet web 10 and the backsheet web 1716. As previously mentioned, the FM layer 20 may have a shorter length than the topsheet 10 and the backsheet 1716. However, in some configurations, the absorbent core 18 can have a shorter length than the FM layer 20. For example, as shown, the absorbent core 18 may be disposed within the target area 1530 and may extend a small length into the first area 1520 and the second area 1540, e.g., less than 50% of the length of the first area and / or the second area. In some configurations, the absorbent core 18 may be disposed only within the target area 1530. In such configurations, the absence of absorbent core 18 adjacent the ends of the absorbent article 1510 may allow for greater flexibility of the ends of the article 1510. Such configurations may be achieved via the cutting and placing operations described herein.
[0129] Additionally, in such configurations, additional layers of material can be added to reduce the possibility of leakage. For example, as shown in FIG. 11D, an auxiliary absorbent layer 19 can be added between the absorbent core 18 and the backsheet 1716. As shown, the auxiliary absorbent layer 19 can be located primarily in the second zone 1540 and overlap the absorbent core 18 in the target area 1530.
[0130] In one particular example, as shown in FIG. 11E, the absorbent article 1510 may include protrusions 1571 and 1572, each disposed adjacent a longitudinal side edge of the absorbent article 1510. The protrusions 1571 and 1572 may be disposed only in the target area 1530. Alternatively, in some forms, the protrusions 1571 and 1572 may be disposed along the entire length of each longitudinal side edge. In some forms, the protrusions 1571 and 1572 may include tufts as described herein, such as tunnel tufts, outer tufts, solid tufts, nested tufts, ridges and grooves, or may include corrugations as described herein. In these forms, when the protrusions 1571 and 1572 include tufts, a plurality of tufts may be disposed longitudinally adjacent the length of the longitudinal side edge of the absorbent article 1510. For those configurations that include corrugations, multiple ridges and grooves may similarly be disposed longitudinally along the longitudinal side edge of the absorbent article 1510, or in some configurations, a single ridge and groove may be disposed longitudinally along the length of the longitudinal side edge.
[0131] Configurations incorporating protrusions 1571 and 1572 can provide additional leak protection by acting as a barrier. Additional configurations are contemplated. For example, an absorbent article of the present disclosure may include multiple rows of protrusions laterally spaced apart from one another. Such configurations can provide a barrier against leakage and can also provide a softness benefit to the user. In some configurations, protrusions 1571 and 1572 may be formed in the topsheet of the absorbent article. In other configurations, protrusions 1571 and 1572 may be formed in the topsheet and absorbent core or the topsheet and FM layer. In these configurations, protrusions 1571 and 1572 may be absorbent to some extent.
[0132] Configurations are contemplated in which the first region, target region, and / or second region include two or more zones. For example, for the configuration shown in FIG. 11E, the target region may include an outer zone in which protrusions 1571 and 1572 are disposed. The outer zone may be disposed outside the target zone. For those configurations in which the first region and / or second region include protrusions, the protrusions may be disposed in outer zones that are outside the first zone and / or second zone, respectively.
[0133] In addition to the mechanical manipulations and formation of zones described above, aspects of the present disclosure are contemplated in which zones can be created or reinforced by chemical heterogeneity in addition to the intimate contact by mechanical manipulations described herein. For example, if protrusions are provided in the absorbent article, the distal ends of the protrusions may be provided with the composition. Or the land areas between adjacent protrusions may be provided with the composition. In one particular example, if the protrusions are oriented in a positive Z direction, the distal ends of the protrusions may be provided with a hydrophobic composition. In another particular example, if the protrusions are oriented in a negative Z direction, the distal ends of the protrusions may be provided with a hydrophilic composition. Suitable compositions and methods for applying the compositions to the web are detailed in U.S. Patent Application Publication Nos. 2017 / 0225449(A1), 2017 / 0120260(A1), and 2017 / 0258650(A1).
[0134] Compliant modified web The inventors have surprisingly found that coherence, while beneficial for fluid management, may not be sufficient for product conformance by itself. For example, needle punched and spunlaced webs, while providing good fluid handling properties by providing coherence between adjacent layers, are unable to provide the level of conformance required by themselves. Rather, the mesoscale processes described herein may be utilized at appropriate intervals to form conforming features within modified webs as described herein.
[0135] In addition to good fluid management, the absorbent articles of the present disclosure can provide good conformity to the wearer's body. However, while good fluid management can result from the close fit that can be produced by microscale and mesoscale processes, good conformity can only be achieved by the mesoscale processes described herein, or a combination of microscale and mesoscale processes.
[0136] Traditional fibrous absorbent core materials, such as thick (or high density cellulose fluff) or absorbent airlaid materials, are primarily composed of short (~2.5 mm) cellulose fibers that form an inherently weak mechanical structure. These traditional structures struggle to maintain their integrity and shape during significant physical exertion in dry conditions. In wet conditions, the integrity and product retained shape is further deteriorated as the wet cellulose fibers plasticize, become soft, pliable, and disintegrate. Historically, two approaches have been taken to improve the mechanical performance of cellulosics: densification (a typical fluff core has a density of 0.04 g / cm when undensified); 3 to approximately 0.2 g / cm when densified 3 in the range of 0.08-0.15 g / cm), and in the case of airlaid, in addition to densification, thermally bondable bicomponent fibers (typically less than 6 mm in length) or latex-based binders (airlaid is typically 0.08-0.15 g / cm 3 (It is.)
[0137] The problem with densification of cellulosic short fiber absorbent core systems is that they tend to make the absorbent core system significantly stiffer. Unfortunately, densification can have a negative effect on both comfort and the ability of the stiffened absorbent system to directly conform to the body shape. The delicate zone area is characterized by significant topographical changes on a relatively short (sub-centimeter) length scale. This complex shape can be difficult to conform due to densification. That is, when absorbent systems are densified, their bending modulus (ease of bending) and bending stiffness increase dramatically, making it very difficult to closely conform to the labia (labia majora and protruding labia minora) surface. Also, as described, these short fiber cellulosic fiber structures collapse significantly from dry to wet state.
[0138] The conformability of an absorbent article during use is generally governed by the stiffest layer in the absorbent article. To create an absorbent article that can provide good conformity to the wearer's body, the stiffest layer of the absorbent article should be mechanically manipulated as described herein to create a more conforming structure. In some forms, this may include mechanically manipulating the topsheet, any FM layer, and absorbent core, either throughout the absorbent article or in zones, as described herein. As previously mentioned, such manipulation of these layers may occur throughout the absorbent article or in zones, as described herein. Also, the benefit of improved conformity can be realized along with the benefit of tightness, and therefore good fluid management.
[0139] In Figures 12A-12B and 13A-13C, patterns of posts, nodes, and recesses are shown. The nodes are interconnected to one another via posts that are spaced apart from one another via recesses. The nodes are essentially unmodified material of the modified web, while the material associated with the posts and recesses is mechanically strained. There may be at least one post connecting adjacent nodes, or there may be multiple posts between adjacent nodes. For example, the number of posts may be from about 2 to about 10, or more than 10 posts may be utilized.
[0140] 12A-12B show plan and cross-sectional views, respectively, of a topsheet integrated with an absorbent core utilizing the tufting process described herein. The tufts were oriented in the negative Z direction. As shown, the topsheet 1217 and absorbent core 1219 composite 1200 includes a plurality of nodes 1211 and a plurality of struts 1213 between adjacent nodes, which not only provides good fluid management, but also provides good conformability to the body. Between adjacent struts 1213 are recesses 1215 extending in the negative Z direction. The recesses 1215 may be formed when the described features (see, e.g., FIG. 6B for protrusions herein) impinge on the topsheet and absorbent core web. As shown, the fibers of the topsheet 1217 are disposed within the recesses 1215 along with the fibers of the absorbent core 1219.
[0141] The sample in Figures 12A-12B included a 28 gsm calendar bonded, bicomponent, spunbond fibrous topsheet 1217. Coformed with an absorbent core 1219 was 30% continuous, e.g., about 5 to about 10 micrometers, or longer, polypropylene fibers longer than staple fibers. The tufts that formed the recesses 1215 were as described for the tufts. The DOE of the tufts was 1.9 mm.
[0142] 13A-13C show plan and cross-sectional views, respectively, of a topsheet 1317 integrated with an absorbent core 1319. The tufts were oriented in the negative Z direction. As shown, the composite web 1300 of the topsheet 1317 and absorbent core 1319 includes nodes 1311 and struts 1313. Between adjacent struts 1313 are recesses 1315 extending in the negative Z direction. The recesses 1315 may be formed when a feature, as described with respect to protrusions herein, impinges on the topsheet and absorbent core web. As shown, the fibers of the topsheet 1317 are disposed within the recesses 1315 along with the fibers of the absorbent core 1319. The sample in FIG. 13A-13C included a 28 gsm calendar bonded, bicomponent, spunbond fibrous topsheet 1317. The absorbent core 1219 was a hydroentangled nonwoven having a fiber length of 38 mm. The shaping that created the recesses 1215 was as described for the tunnel tufts. The DOE of the shaping was 1.9 mm.
[0143] It is noteworthy that for both samples in Figures 12A-12B and Figures 13A-13C, the topsheet migrates into and between adjacent struts. As previously mentioned, the same microscale processes, e.g., needle punching or spunlacing, move only a small amount of the topsheet fibers within each recess. In contrast, the mesoscale process described herein moves a much larger amount of the topsheet's constituent material into the absorbent core, allowing the resulting features to provide conformability benefits to the absorbent article. Furthermore, the mesoscale process allows the topsheet and absorbent core to be intimately attached to one another to provide good fluid management properties.
[0144] FIG. 14 shows a schematic enlarged cross-sectional view of a topsheet and absorbent core composite 1400. As shown, the recess 1415 (exaggerated for ease of visualization) does not extend through the entire thickness of the composite, but rather rearranges the topsheet and / or absorbent core components. In other words, the recess has a bottom 1421. As shown, the recess bottom 1421 may be located between the first and second surfaces of the composite 1400. Alternatively, at least one recess bottom 1421 may be located under the second layer of the composite 1400. For example, when the teeth of the rolls described in FIG. 6A or 6B engage with the topsheet and / or absorbent core components, some of the components may extend and thin, and some may even break. In the case of a nonwoven material, the fibers of the nonwoven may become thinner and some fibers may break. Similarly, in the absorbent core, some of the components may break or become unattached to the absorbent core components. Thus, in a sense, the recesses 1415 form thinned areas between adjacent posts 1413. By reducing the amount of material, the thinned areas can allow the posts 1413 to move, bend, and / or rotate somewhat independently of one another. However, the base 1421 connects adjacent posts 1413 together such that the absorbent core still retains some structural importance.
[0145] In addition to connecting adjacent struts 1413, the base 1421 also forms a bridge between adjacent struts 1413. This bridge can function as a fluid transport pathway that can help utilize more material in the absorbent core as opposed to when the bridge is not present.
[0146] In addition, it is believed that by forcing the topsheet and absorbent core materials in the negative Z direction, the topsheet and absorbent core materials intermix to some extent along the sidewalls of the recesses and the bottom of the recesses. Thus, the recesses can provide a fluid management effect by faster fluid acquisition. In contrast, embossing can provide some intermixing of materials between the topsheet and the absorbent core, but densification of the areas formed by embossing does not increase the rate of fluid acquisition in the densified areas.
[0147] Each of the recesses 1415 has a length that extends generally parallel to its long axis. As shown in Figures 12A-12C and 13A-13C, the length of the recesses may vary. As shown, the long axis may be oriented generally parallel to the longitudinal axis of the absorbent article. However, the recesses 1415 may have a long axis that is generally parallel to the transverse axis of the absorbent article. The recesses 1415 may have a long axis that is at an angle to the longitudinal axis of the absorbent article. For example, a first portion of the recesses 1415 may have a long axis that is generally parallel to the longitudinal axis and a second portion of the recesses 1415 may have a long axis that is generally parallel to the transverse axis. A third portion of the recesses 1415 may have a long axis that is generally at an angle to the longitudinal axis. The third portion of the recesses 1415 may include recesses having long axes that are at various angles to the longitudinal axis. As examples, some of the recesses 1415 may have major axes that form a first angle with respect to MD, some of the recesses 1415 may have major axes that form a second angle with respect to MD, some of the recesses' major axes may form a third angle, some of the recesses' major axes may form a fourth angle, etc.
[0148] The spacing between adjacent recesses generally perpendicular to the major axis of the recesses can be any suitable distance and depends on the spacing of the forming elements on the associated roll. Because there may be mechanical limitations on the rolls with respect to spacing, such limitations may affect the spacing between adjacent recesses. In addition, the caliper of the integrated layers may also relate to the spacing between the recesses. For example, a thicker caliper material may require a higher spacing between adjacent teeth. Depending on the integrated material, closer spacing between the teeth may cause the layers to chip / tear. In some particular forms, the recesses may be spaced apart by more than about 1 mm in the CD and more than about 2 mm in the MD.
[0149] In some configurations, the bottom portion 1421 may be bonded by heated teeth or other suitable mechanism. The bonded bottom portion 1421 can provide additional stability to the web and ensure a tighter attachment of the topsheet to the absorbent core. Suitable processes are described in further detail in U.S. Patent No. 7,682,686.
[0150] Although the composites described with respect to Figures 12A-12B and 13A-13C include a topsheet and an absorbent core, a topsheet and FM layer composite may be formed, or the composite may include an FM layer and an absorbent core, or the composite may include a topsheet, an FM layer, and an absorbent core.
[0151] As previously mentioned, some cellulosic materials may tear, break, and / or shred to some degree when exposed to the mesoscale processes described herein. An example of what happens to some materials when subjected to the mesoscale processes described herein is shown in Figures 15A-15C. As shown, from the plan view of Figure 15A, the topsheet and absorbent core composite 1500 does not appear all that different from the composites 1200 and 1300 (shown in Figures 12A-12B and 13A-13C, respectively). The composite 1500 includes a node 1511 and a plurality of struts 1513A and 1513B. Each strut forms a sidewall portion of a recess 1515 on opposite sides of the other. However, as shown in Figures 15B and 15C, the recesses 1515 extend throughout the composite 1500 and act like slits between adjacent struts. From a mechanical standpoint, the recesses 1515 may allow the struts 1513A and 1513B to move relative to each other without binding to the adjacent struts. This may initially allow for high compliance. However, as shown, without the connection between adjacent struts described with respect to FIG. 14 (present in FIGS. 12A-12B and 13A-13C), the struts 1513 may be too flexible in the degree of movement available. For example, as shown, a portion of the first strut 1513A is disposed under a portion of the second strut 1513B. As such, any movement of the absorbent core requires sufficient energy to overcome the sliding of the struts 1513A and 1513B relative to each other. Also, rather than being stored as potential energy within the core, the energy of movement is dissipated in overcoming the relative movement of one strut relative to the other, as well as friction losses. Due to the lost energy, once deformed, the struts 1513A and 1513B may not have the energy necessary to recover to their undeformed state in the absence of the connection regions described in Figure 14. Thus, the composite 1500 lacks sufficient integrity to withstand the mechanical stresses generated while the article is worn and will eventually collapse into a bunched state. This can also cause discomfort to the wearer, so too much fit can lead to comfort issues while wearing, as can not fitting well enough.
[0152] In contrast, materials selected in accordance with the present disclosure can reduce friction losses of a portion of one strut disposed under another. Referring now to FIG. 15C, adjacent struts overlap significantly. When materials are selected in accordance with the present disclosure, the overlap distance 1503 may be less than about 0.75 mm, less than about 0.5 mm, or less than about 0.2 mm, or about 0 mm. The overlap distance test is described in further detail herein.
[0153] The materials utilized for the samples of Figures 15A-15C were a 28 gsm bicomponent 80 percent polypropylene and 20 percent polyethylene spunbond topsheet and an airlaid absorbent core containing 180 gsm 4.9 percent, 3 mm long, 1.7 dtex bicomponent fibers, 14.7 percent AGM particles, and approximately 80 percent short cellulosic fibers.
[0154] As previously mentioned, conventional fibrous absorbent core materials include short cellulose fibers. It is believed that if the fiber length is, for example, short, it is not possible to form a substantial fiber network that can withstand the mesoscale processes described herein. It is believed that mechanical manipulation of these short fibers causes these short fiber materials to deform and stretch (e.g., as they flow around teeth) to an extent that such processing typically results in tearing of the material. Tearing of the material weakens the structure's ability to recover its shape when deformed while being worn by a user performing daily activities. For example, as shown in Figures 15A-15C, if the fibers are too short, slits and tears can occur.
[0155] As mentioned above, the layer of the absorbent article that provides the highest stiffness to provide good conformity is likely to be a good candidate for the formation of conforming features described herein. Thus, as an example, the FM layer disposed between the topsheet and the absorbent core may not need to be designed to withstand the mesoscale processes described herein. In such a configuration, if the absorbent core is the stiffest part of the absorbent article, the breakage of the constituent material of the FM layer may not adversely affect the integrity of the absorbent article. The reverse is also applicable. If the absorbent article includes an FM layer that is stiffer than the corresponding part of its absorbent core, the FM layer may be designed to withstand the mesoscale processes described herein. However, the absorbent core in such a configuration may not need to be designed to withstand such processes. Alternatively, in some cases, it may be beneficial to design the system to withstand the mesoscale processes described herein.
[0156] Therefore, material selection can affect the degree of conformity of the modified web of the present disclosure. The inventors have surprisingly found that by supporting long fiber networks, for example longer than 6 mm, conformity features can be formed in absorbent articles that provide hydrodynamic benefits along with desired mechanical properties. These long fiber networks may be realized in the absorbent core, FM layer, and / or topsheet, or any combination thereof. However, it should be noted that a sufficient amount of long fibers / filaments should be utilized to create the long fiber network. Suitable materials for achieving the thinned areas between the struts are described in more detail below.
[0157] As previously discussed, the DOE between the features affects the level at which one layer engages with another. For example, as shown in FIG. 16 for a small DOE, the bottom 1621B of the recess may be located closer to the wearer-facing surface of the absorbent core. In contrast, for a large DOE, the bottom 1621A of the recess may be located more distally than the bottom 1621B. Configurations are envisioned in which various depths of engagement are utilized. In such cases, recesses with large DOEs may be deeper than recesses with less large DOEs.
[0158] Without being bound by theory, it is believed that the long fiber network can reduce the possibility of crushing of the absorbent core or the layer that governs the flexibility of the absorbent article. It is believed that the fibers in the absorbent core, FM layer, and / or topsheet should be greater than about 6 mm. It is further believed that the longer thermoplastic fibers can span the recesses and support the bottom of the recesses connecting adjacent struts. It is also believed that during mechanical manipulation, shorter fibers, such as cellulose, tend to separate from each other because they do not have sufficient length to bond within the fiber network of the absorbent system. It is noted that longer fibers may be required when the engagement depth of the filigree referred to herein is higher. Conversely, shorter fibers may be utilized with a lower engagement depth, but it is believed that a lower engagement depth, for example, less than 5 mm, may adversely affect the conformity of the absorbent article. In some forms, a fiber length longer than the filigree length, such as the length of the teeth 510 (shown in FIG. 6A), may be sufficient to create a long fiber network that can withstand mesoscale processes. Therefore, the depth of the recesses may be less than the average length of the thermoplastic fibers in the absorbent system, for example the FM layer and / or the absorbent core.
[0159] It is believed that the long fiber network allows the component materials of the layer to flow more easily around the features utilized in the mesoscale process. Allowing the component materials to flow in this manner allows the component materials to remain intact after processing without significant fiber breakage. It is further believed that the extensible materials and / or crimped fibers can help the long fiber network maintain its structural integrity.
[0160] In addition to fiber length, it is believed that the way the fibers are joined together can also affect the fiber network. For example, it is believed that the density of bond sites (bond sites per square centimeter) via calendar bonding can affect the long fiber network. For example, if the bond density is high, the spacing of adjacent bond sites can effectively shorten the long fibers. In contrast, it is believed that air-through bonding can beneficially affect the long fiber network because these types of bonds are believed to be more easily broken during processing. As another example, ultrasonic and / or thermal bonding of the fibers of these layers can be used to build a fiber network that can support the long fiber network. Further examples include spunlacing and needle punching. Bonding spacing, spunlacing, and / or needle punching can allow the long fiber network to flex / move and then recover. Proper bonding spacing will ensure that the effective fiber length is about 6 mm or greater. Some specific examples of sufficient fiber networks are listed in Tables 1-4.
[0161] In the absorbent articles of the present disclosure, the main layer, i.e., the layer that most impacts the flexibility of the article (generally the thickest material), can benefit from including a long fiber network. The "long" filaments or fibers of the long fiber network may comprise 15% to 50% by weight of the filaments and / or fibers in the fibrous structure, 17% to 40% of the fibers in the fibrous structure, or 20% to 30% of the fibers in the fibrous structure, specifically all values within these ranges and any ranges created thereby. For example, long fibers, i.e., longer than 6 mm, may be present in the absorbent core. It is believed that the basis weight of the long fibers should be at least 15 percent of the basis weight of the absorbent core in order for the absorbent core to survive the mesoscale processes described herein. However, if the absorbent core does not contain the required long fiber percentage, layers of materials adjacent to the absorbent core, such as the fluid management layer and / or topsheet, may contribute to the long fiber network. However, it is believed that if the absorbent core lacks the required long fiber percentage, a percentage greater than 15 percent may be required from adjacent layers. For example, assuming the fluid management layer and absorbent core are provided with matching features, if the absorbent core does not contain at least 25 percent long fibers, the long fibers in the fluid management layer should also be evaluated. In such instances, the cumulative basis weight of the long fibers should be evaluated against the cumulative basis weight of the fluid management layer and absorbent core to determine the appropriate percentage of long fibers.
[0162] The filaments and / or fibers of the long fiber network can be interconnected or bonded with other filaments and / or fibers, such as thermoplastic fibers. The filaments and / or fibers of the long fiber network should have an average length that is greater than the average strut height and / or greater than the average recess depth in the absorbent mesh. The average length of the fibers of the long fiber network can be from about 6 mm to about 100 mm. Alternatively, the long fiber network can include continuous filaments, such as meltblown, spunmelt, spunbond, etc. Additionally, the long fiber network can include continuous filaments as well as fibers.
[0163] The filaments and / or fibers used to form the long fiber network may be bundles of filaments and / or fibers. For example, 10-100 fibers may be in the form of a bundle such that at least 5% of the filaments and / or fibers are bonded together. Bundling the filaments and / or fibers together allows the filaments and / or fibers to form a fiber network while maintaining the desired permeability.
[0164] An exemplary absorbent article 1700 made in accordance with the present disclosure is shown in Figure 17A. The article shown has been modified to provide good fluid acquisition in a target area 1530. As shown, a target zone 1535 having a figure eight shape can include a tight fit between the FM layer and the absorbent core in the target zone 1535. Additionally, in some forms, the target zone 1535 can include holes that extend through the topsheet or through the topsheet and the FM layer.
[0165] In addition, the absorbent article 1700 may also include conforming features in the target region 1530, allowing the absorbent article 1700 to conform to the outer labia structure of the wearer. Similarly, the first region 1520 and the second region 1540 may include conforming features that allow those portions of the absorbent article 1700 to conform to the complex surface of the user. However, the patterns utilized in the first region 1520 and the second region 1530 may provide more structural integrity to the absorbent article, while the pattern in the target zone 1535 may provide more conformance to the body. Similarly, outside of the target zone 1535, the target region 1530 may include the pattern of the first region 1520 and / or the second region 1540, or may include a pattern that provides more structural integrity than the target zone 1535.
[0166] As shown, the first region 1520 and the second region 1540 may be generally diamond-shaped and include matching features with a repeating pattern. Within each of the diamond shapes are multiple recesses of various lengths. As shown, the recesses are generally oriented generally parallel to the long axis of the absorbent article 1700. However, the recesses may be oriented at an angle thereto, or generally parallel to the lateral axis of the absorbent article. Alternatively, some of the diamonds in the pattern may include recesses that face in one direction, while other diamonds in the pattern may include recesses that face in another direction. This is true regardless of the shape of the units in the pattern, e.g., diamonds, circles, etc. Further suitable shapes are disclosed below.
[0167] Also, as shown, a portion of the target area 1530 may include conforming features generally oriented in a column direction and alternating row direction, with the columns generally parallel to the long axis of the absorbent article 1700. The recesses may be longer than the diamond recesses or at least some of the recesses in the diamond pattern.
[0168] Additional patterns that may be utilized in webs of the present disclosure are provided with respect to Figure 17B. As shown, the nodes may be any suitable shape, such as oval, hexagonal, diamond, semicircular, heart, donut, rainbow, etc. Additional shapes include moon, clover, balloon, star, or combinations thereof. As shown, multiple struts extend between each node.
[0169] Absorbent articles After the topsheet, FM layer, absorbent core, or any combination thereof, are provided with cling and / or conforming features, the modified web can be further converted to produce an absorbent article. As shown in Figure 18, the final web 1058 (including the final webs described herein) can then be processed as described with respect to Figure 18 to create a plurality of absorbent articles 1039.
[0170] For example, for those configurations where an absorbent core was not previously provided, an absorbent core web 1718A (shown as a roll) may be provided to a cutting and placing operation 1030, which cuts the absorbent core web 1718A and creates a plurality of separate absorbent cores therefrom. The plurality of separate absorbent cores may be placed on a plurality of separate FM portions 20A (shown in FIG. 4), thereby forming a TFMAC laminate web 37. A backsheet 1716A (shown as a roll) may then be placed on the TFMAC laminate web 37, thereby forming an absorbent article laminate web 1073. A joining operation 1031 may be utilized to join the backsheet with the TFMAC laminate web 37. The absorbent article laminate web 1073 may then be subjected to a cutting operation 1032, which cuts the absorbent article laminate web 1037 into a plurality of separate absorbent articles 1039. Cutting operations, as well as cutting and placing operations, are known in the art of manufacturing disposable absorbent articles.
[0171] The topsheet of a disposable absorbent article is the surface of the article that faces the wearer. The absorbent articles of the present disclosure may include any known or other effective topsheet that is conformable, soft-feeling, non-irritating, etc. against the wearer's skin. Suitable topsheet materials include water-permeable materials that are oriented toward and in contact with the wearer's body, allowing rapid penetration of bodily exudates, and do not allow fluids to flow back through the topsheet to the wearer's skin.
[0172] Suitable topsheets may be manufactured from a wide range of materials, such as, for example, porous foams, reticulated foams, perforated plastic films, woven materials, nonwoven materials, woven or nonwoven materials of natural fibers (e.g., wood or cotton fibers), synthetic fibers or filaments (e.g., polyester fibers, or polypropylene fibers, or bicomponent PE / PP fibers, or mixtures thereof), or combinations of natural and synthetic fibers. Additional fibers or filaments include meltblown, nano, spunbond, carded, etc. The topsheet may have one or more layers, such as spunbond-meltblown-spunbond materials. Any portion of the topsheet may be coated with a skin care composition, antimicrobial agents, surfactants, and / or other beneficial agents. The topsheet may be hydrophilic or hydrophobic, or may have hydrophilic and / or hydrophobic portions. If the topsheet is hydrophobic, there will typically be holes so that bodily exudates can pass through the topsheet.
[0173] If it is desired that the topsheet be mechanically manipulated, for example to form conforming features, the topsheet may comprise an extensible material or a material that includes crimped fibers / filaments. If a non-extensible material is utilized to form conforming features, the topsheet may break or tear. Further details of nonwoven webs with extensible fibers / filaments are provided in U.S. Patent Application Publication No. 2014 / 0170367. Also, details of nonwoven webs with crimped fibers are provided in U.S. Patent Application Publication No. 2016 / 0166443.
[0174] Furthermore, in some configurations, the concept of adhesion can be applied to the topsheet. For example, the topsheet may include a film substrate and a nonwoven substrate. In such configurations, the nonwoven substrate may be a carrier material onto which the film substrate can be extruded. Since the extruded film is in a semi-molten state, the resulting composite material is believed to provide adhesion and performance benefits over a film and nonwoven laminate of the same constituent materials. The film / nonwoven composite may then be processed as described herein, for example, the addition of holes to provide fluid acquisition capabilities and the provision of conforming features may be performed on such film / nonwoven composite. Such film / nonwoven composites and their processing are described in detail in U.S. Patent Application Publication No. 2009 / 0026651, International Application Nos. PCT / CN2017 / 089550, PCT / CN2017 / 089553, and PCT / CN2017 / 089554.
[0175] In some configurations, the topsheet may comprise a composite of nonwoven materials. For example, a first nonwoven substrate may be formed by a first spin beam, and a second nonwoven substrate may be formed by a second spin beam. In some configurations, the second spin beam may form filaments on the filaments of the first spin beam. It is believed that making a composite nonwoven in this manner can create intimate contact between the substrates of the topsheet, as opposed to making a composite nonwoven by laminating a first web to a second web. Such nonwoven webs and processes for making such webs are described in U.S. Patent Application Publication No. 2017 / 0258651 A1.
[0176] In some embodiments, the FM layer and absorbent core may comprise any suitable material. For example, if the FM layer is not the stiffest layer of the absorbent article, the FM layer may comprise any suitable material capable of rapidly absorbing liquid insult from the topsheet and subsequently transferring the liquid insult to the absorbent core. Similarly, if the absorbent core is not the stiffest layer of the absorbent article, the absorbent core may comprise any suitable material capable of absorbing and retaining liquid insult from the FM layer (if present) or the topsheet. Where conventional materials are available, there are many commercially available variations for the FM layer and absorbent core.
[0177] However, if the FM layer or absorbent core is the stiffest layer of the absorbent article, the material of the FM layer or absorbent core should be carefully selected. Note that in some forms, the FM layer and absorbent core can be designed to withstand the mesoscale processes described herein, including, for example, long fiber networks.
[0178] Any of the absorbent system, the FM layer and / or the absorbent core can be webs such as, for example, nonwovens, fibrous structures, thermoplastic long filament and / or fiber reinforced airlaid webs, high loft nonwovens, needle punched webs, hydroentangled webs, fiber tow webs, woven webs, knit webs, flocked webs, spunbond webs, layered spunbond / meltblown webs, carded fiber webs, coform webs of cellulose fibers and meltblown or spunmelt fibers, coform webs of staple fibers and meltblown or spunmelt fibers, and layered combinations thereof, such as layered webs.
[0179] The constituent filaments and / or fibers of the absorbent system may be composed of polymers such as polyethylene, polypropylene, polyester, and blends thereof. The filaments may be spunbond. The filaments may be meltblown. The filaments and / or fibers may comprise cellulose, rayon, cotton, or other natural materials or blends of polymers and natural materials. The filaments and / or fibers may also comprise superabsorbent materials such as polyacrylates, or any combination of suitable materials. The filaments and / or fibers may be monocomponent, bicomponent, and / or bicomponent, non-round in shape (e.g., capillary channel fibers), and may have a major cross-sectional dimension (e.g., diameter of a circular fiber) in the range of 0.1 to 500 micrometers. The constituent filaments and / or fibers of the absorbent system may also be a mixture of different fiber types, differing in characteristics such as chemistry (e.g., polyethylene and polypropylene), (mono- and bi-)component, dtex (micro dtex and >20 dtex), shape (i.e., capillary and circular), etc. The constituent filaments and / or fibers may range from about 0.1 dtex to about 100 dtex.
[0180] Suitable thermoplastic filaments and / or fibers can be made of a single polymer (monocomponent fibers) or can be made of more than one type of polymer (e.g., bicomponent fibers). The polymer that comprises the sheath often melts at a different, typically lower, temperature than the polymer that makes up the core. As a result, these bicomponent filaments and / or fibers provide thermal bonding due to the melting of the sheath polymer while retaining the desirable strength properties of the core polymer.
[0181] Bicomponent filaments and / or fibers suitable for use in the present invention may include sheath / core fibers having polymer combinations such as polyethylene / polypropylene, polyethylvinylacetate / polypropylene, polyethylene / polyester, polypropylene / polyester, copolyester / polyester, etc. Particularly suitable bicomponent thermoplastic filaments and / or fibers for use herein are those having a polypropylene or polyester core and a lower melting temperature copolyester, polyethylvinylacetate, or polyethylene sheath (e.g., DANAKLON.RTM, CELBOND.RTM, or CHISSO.RTM. bicomponent fibers). These bicomponent filaments and / or fibers may be concentric or eccentric. As used herein, the terms "concentric" and "eccentric" refer to whether the sheath has a uniform or non-uniform thickness throughout the cross-sectional area of the bicomponent fiber. Eccentric bicomponent filaments and / or fibers may be desirable to provide higher compressive strength at a thinner fiber thickness. Bicomponent filaments and / or fibers suitable for use herein can be either uncrimped (i.e., uncurled) or crimped (i.e., curved). Bicomponent fibers can be crimped by typical textile means, such as stuffing box or gear crimping, to achieve a predominantly two-dimensional or "planar" crimp.
[0182] The length of the bicomponent fibers may vary depending on the particular properties desired for the fibers and the web forming process. Ideally, in air-formed webs such as long fiber reinforced airlaid webs, these thermoplastic fibers have a length of about 6 mm to about 15 mm, preferably greater than about 6 mm to about 12 mm. The properties of these thermoplastic fibers can also be adjusted by varying the diameter (caliper) of the fiber. The diameter of these thermoplastic fibers is typically defined in terms of denier (grams per 9000 meters) or decitex (grams per 10,000 meters). When used in airlaid manufacturing machines, such as DanWeb machines, suitable thermoplastic bicomponent fibers may have a decitex ranging from about 1.0 to about 16 decitex, preferably from about 1.4 to about 10 decitex, and most preferably from about 1.7 to about 7 decitex.
[0183] Without being bound by theory, it is believed that the FM layer and / or absorbent core with good long fiber network can withstand mesoscale process. Also, as mentioned above, the topsheet can contribute to the long fiber network to some extent. It is believed that fibers with a length of 6 mm or more can be used to help provide good long fiber network. For example, co-forming utilizes continuous filaments much longer than 6 mm. Furthermore, it is believed that thermoplastic bonded filaments and / or fibers are more advantageous to use than latex bonded.
[0184] With respect to the form of the absorbent system including the FM layer and the absorbent core, the FM layer and / or the absorbent core may be constructed as described herein. In one particular example, the absorbent core may include a substrate including a superabsorbent polymer material. For example, a tissue web may include absorbent gelling material granules or fibers disposed on the tissue web.
[0185] The backsheet is generally the portion of the absorbent article disposed adjacent to the garment-facing surface of the absorbent core. The backsheet may be joined to a portion of the topsheet, the absorbent core, and / or any other layer of the absorbent article by any attachment method known to those skilled in the art. The backsheet prevents or at least inhibits body exudates absorbed and contained in the absorbent core from soiling articles such as bedsheets, undergarments, and / or clothing. The backsheet is typically liquid impermeable or at least substantially impermeable. The backsheet may be or include a thin plastic film, such as a thermoplastic film having a thickness of about 0.012 mm to about 0.051 mm, for example. Other suitable backsheet materials may include breathable materials that allow vapors to escape from the absorbent article while still preventing or at least inhibiting body exudates from passing through the backsheet.
[0186] Exemplary absorbent articles of the present invention include diapers and / or feminine pads. Referring to FIG. 19, an absorbent article 1710 that can utilize the precursor webs described herein may be a sanitary napkin, feminine hygiene pad. As shown, the sanitary napkin 1710 may include a liquid permeable topsheet 1714, a liquid impermeable or substantially liquid impermeable backsheet 1716, and an absorbent core 1718 disposed intermediate the topsheet 1714 and the backsheet 1716. The sanitary napkin 1710 may include wings 1720 that extend outwardly with respect to a longitudinal axis 1780 of the sanitary napkin 1710. The sanitary napkin 1710 may also have a lateral axis 1790. The wings 1720 may be joined to the topsheet 1714, the backsheet 1716, and / or the absorbent core 1718. The sanitary napkin 1710 may also include a leading edge 1722, a trailing edge 1724 longitudinally opposite the leading edge 1722, a first side edge 1726, and a second side edge 1728 laterally opposite the first side edge 1726. The longitudinal axis 1780 may extend from a midpoint of the leading edge 1722 to a midpoint of the trailing edge 1724. The lateral axis 1790 may extend from a midpoint of the first side edge 1726 to a midpoint of the second side edge 1728. The sanitary napkin 1710 may also include additional features commonly found in sanitary napkins as is known in the art. In some forms of the invention, the wings may include extensibility zones as described in U.S. Pat. No. 5,972,806.
[0187] The absorbent article 1710 may further comprise an FM layer disposed between the topsheet 1714 and the absorbent core 1718. The FM layer can be configured as described herein. Similarly, the absorbent core can be configured as described herein.
[0188] One suitable material for the backsheet can be a liquid impermeable thermoplastic film having a thickness of about 0.012 mm (0.50 mil) to about 0.051 mm (2.0 mil), for example comprising polyethylene or polypropylene. Typically, the backsheet has a weight of about 5 g / m 2 ~Approx. 35g / m2 It should be noted, however, that other flexible, liquid impermeable materials may be used as the backsheet. "Flexible" in this specification refers to a material that is conformable and will easily adapt to the overall shape and contours of the wearer's body.
[0189] The backsheet may be generally disposed adjacent to the outer surface of the absorbent core and may be joined thereto by any suitable attachment means known in the art. For example, the backsheet may be secured to the absorbent core by a uniform continuous layer of adhesive, a patterned layer of adhesive, or an array of discrete lines, spirals, or dots of adhesive. Exemplary, but non-limiting, adhesives include those manufactured by HB Fuller Company (St. Paul, Minn., USA) and commercially available as HL-1358J. One example of a suitable attachment means, including an open pattern network of filaments of binder, is disclosed in U.S. Patent No. 4,573,986, entitled "Disposable Waste-Containment Garment," issued March 4, 1986 to Minetola et al. Another suitable attachment means, including several lines of binder filaments wound in a helical pattern, is exemplified in the apparatus and methods shown in U.S. Patent No. 3,911,173, issued October 7, 1975 to Sprague, Jr., U.S. Patent No. 4,785,996, issued November 22, 1978 to Ziecker et al., and U.S. Patent No. 4,842,666, issued June 27, 1989 to Werenicz. Alternatively, the attachment means may include thermal bonding, heat fusion, pressure bonding, ultrasonic bonding, dynamic mechanical bonding, or any other suitable attachment means or combinations of these attachment means. The backsheet may be further secured to the topsheet by any of the attachment means / methods described above.
[0190] Yet another example of a disposable absorbent article that can utilize the precursor web of the present invention is a diaper, such as a non-refastenable pant, a refastenable pant, and / or a refastenable diaper. The diaper can have a structure similar to that of a sanitary napkin. Exemplary diapers are described below.
[0191] 20, a plan view of an exemplary absorbent article, diaper 1900, laid flat and in an uncontracted state (i.e., with elastic induced contraction removed), with a portion of the structure cut away to more clearly show the structure of the diaper 1900 and its wearer-facing surface facing the viewer. This diaper is shown for illustrative purposes only, as the present disclosure may be used to manufacture a wide variety of diapers and other absorbent articles.
[0192] The absorbent article may include a liquid permeable topsheet 1924, a liquid impermeable backsheet 1925, an absorbent core 1928 disposed at least partially between the topsheet 1924 and the backsheet 1925, and barrier leg cuffs 1934. The absorbent article may also include a distribution layer 1954 and an acquisition layer 1952, both of which are described in more detail below. In various configurations, the acquisition layer 1952 may alternatively distribute body exudates, and the distribution layer 1954 may alternatively acquire body exudates, or either layer may be capable of distribution and / or acquisition of body exudates. The absorbent article may also include elastic gasket cuffs 1932, which typically join the chassis of the absorbent article through the topsheet and / or backsheet and are substantially planar to the chassis of the diaper.
[0193] The figures also show typical components of a taped diaper, such as a fastening system comprising tie tabs 1942 or other mechanical fasteners attached towards the rear edge of the absorbent article 1900 and cooperating with a landing zone at the front of the absorbent article 1900. The absorbent article may further comprise other typical elements not shown, such as, for example, a rear elastic waist feature, and a front elastic waist feature.
[0194] The absorbent article 1900 may have a front waist edge 1910, a back waist edge 1912 longitudinally opposite the front waist edge 1910, a first side edge 1903, and a second side edge 1904 laterally opposite the first side edge 1903. The front waist edge 1910 is the edge of the absorbent article 1900 that is intended to lie toward the front of the user when worn, and the back waist edge 1912 is the opposite edge. When a wearer wears the absorbent article 1900, the front waist edge 1910 and the back waist edge together form a waist hole. The absorbent article 1900 may have a longitudinal axis 1980 that extends from the lateral midpoint of the front waist edge 1910 to the lateral midpoint of the back waist edge 1912 of the absorbent article 1900, dividing the absorbent article 1900 into two halves that are substantially symmetrical about the longitudinal axis 1980, when the article is laid flat and viewed from the wearer-facing surface as illustrated in Figure 20. The absorbent article may also have a lateral axis 1990 that extends from the longitudinal midpoint of the first side edge 1903 to the longitudinal midpoint of the second side edge 1904. The length L of the absorbent article 1900 may be measured along the longitudinal axis 1980 from the front waist edge 1910 to the back waist edge 1912. The crotch width of the absorbent article 1900 may be measured along a transverse axis 1990 from a first side edge 1903 to a second side edge 1904. The absorbent article 1900 may include a front waist region 1905, a back waist region 1906, and a crotch region 1907. The front waist region, the back waist region, and the crotch region each define one-third of the longitudinal length of the absorbent article. Additionally, front and back portions may also be defined on either side of the transverse axis 1990.
[0195] The backsheet 1925 may be joined to the topsheet 1924, the absorbent core 1928, and / or any other elements of the absorbent article 1900 by any attachment method known to one of ordinary skill in the art. Suitable attachment methods are described above with respect to methods for joining the topsheet 1924 to other elements of the absorbent article 1900.
[0196] The absorbent article 1900 may include a pair of barrier leg cuffs 1934. Each barrier leg cuff may be formed by a piece of material that extends upwardly from the inner surface of the absorbent article and is bonded to the absorbent article to improve containment of liquids and other body exudates near the junction of the wearer's torso and legs. The barrier leg cuffs 1934 are bounded by a proximal edge 1964 that is bonded directly or indirectly to the topsheet 1924 and / or backsheet 1925, and a free end edge 1966 that is intended to contact and form a seal with the wearer's skin. The barrier leg cuffs 1934 extend at least partially between the front waist edge 1910 and the back waist edge 1912 of the absorbent article on either side of the longitudinal axis 1980, and are present at least in the crotch region 1907. The barrier leg cuff 1934 may be joined to the chassis of the absorbent article at a proximal edge 1964 by a bond 1965, which may be made by a combination of glue bonding, melt bonding, or other suitable bonding processes. The bond 1965 at the proximal edge 64 may be continuous or intermittent. The bond 1965 closest to the raised section of the leg cuff 1934 defines the proximal edge 1964 of the raised section of the leg cuff 1934.
[0197] The barrier leg cuffs 1934 may be integral with the topsheet 1924 or backsheet 1925 or may be a separate material joined to the chassis of the absorbent article. The barrier leg cuff 1934 material may extend throughout the entire length of the diaper but may be "tack bonded" to the topsheet 1924 toward the front waist edge 1910 and back waist edge 1912 of the article such that the barrier leg cuff material remains flush with the topsheet 1924 in these sections.
[0198] Each barrier leg cuff 1934 may include one, two, three or more elastic strands or strips of film 1935 adjacent its free end edge 1966, which may provide a more effective seal.
[0199] In addition to the barrier leg cuffs 1934, the absorbent article may include gasket cuffs 1932 that are joined to the chassis of the absorbent article, particularly the topsheet 1924 and / or backsheet 1925, and are positioned outward relative to the barrier leg cuffs 1934. The gasket cuffs 1932 may provide a more effective seal around the wearer's thighs. Each gasket leg cuff may include one or more elastic strings 1933 or elastic elements between the topsheet 1924 and the backsheet 1925 in the leg hole areas in the chassis of the absorbent article. All or a portion of the barrier legs and / or gasket cuffs may be treated with a lotion or skin care composition. The barrier leg cuffs may be made in a number of different configurations, including those described in U.S. Patent Application Publication No. 2012 / 0277713.
[0200] In one form, the absorbent article may include front ears 1946 and back ears 1940 . The ears can be an integral part of the chassis, such as formed from the topsheet 1924 and / or backsheet 1925 as side panels. Alternatively, as shown in FIG. 19, the ears (1946, 1940) can be separate elements attached by glue bonding, heat embossing, and / or crimping. The back ears 1940 can be stretchable to easily attach the tabs 1942 to the landing area 1944 and keep the taped diaper in place around the waist of the wearer. The back ears 1940 can also be elastic or stretchable to provide a more comfortable, wraparound fit by allowing the sides of the absorbent article to stretch, thereby initially fitting the absorbent article to the wearer in a conforming manner, and then maintaining this fit throughout the entire wear period, even long after the absorbent article has been filled with exudates.
[0201] Data for various samples are listed in the tables below. Sample descriptions are provided after all data tables. In Table 1, data is provided on the mechanical properties of modified (samples 6a-8c) and unmodified samples (no conforming features-samples 1-5). The samples listed in Table 1 are absorbent core samples only. Additionally, the mechanical property values listed in Table 1 are for the 3-point bending test described herein and the bunch compression test described herein. The 3-point bend test measures basic bending properties and stiffness related to a material or product's ability to conform to complex anatomical features. A lower number indicates a more conformable material. In contrast, the bunch compression test is a measure of a material's ability to recover its original shape or form after compression, especially when measured when wet. For this data, a high value indicates the material's ability to recover to its initial shape even when wet. A high number can indicate the conformability of a material even after being invaded by a liquid.
[0202] [Table 1]
[0203] Table 2 includes data for the three-point bending test and bunch compression test disclosed herein. The samples in Table 2 include an absorbent core and a fluid management layer that includes the conforming features described herein. The data shows that while some samples exhibit high conformability during initial use, e.g., low flexural modulus, low flexural stiffness, their in-use condition does not show the same effect. For example, these same samples may show very low recovery energy, which suggests that these products may collapse during use and actually lead to leakage problems. However, without additional consideration regarding potential problems in use, one may be fooled by "fool's gold" and rely solely on the initial conformity of the product.
[0204] [Table 2]
[0205] The data in Table 2 shows that the addition of a fluid management layer increases the values for recovery energy and percent recovery. It is also noted that the addition of a fluid management layer increases the values of flexural modulus and flexural stiffness. However, the increase in flexural modulus and flexural stiffness compared to recovery energy and percent recovery is not one to one.
[0206] Table 3 includes data on the integration of the topsheet, fluid management layer, and absorbent core for the three-point bending and bunch compression tests disclosed herein. In each sample, the topsheet, fluid management layer, and absorbent core include conforming features that integrate all three layers. Additionally, there are several samples of currently available products that were similarly tested.
[0207] [Table 3]
[0208] The ratio 1 is between bending stiffness and recovery energy. In samples 12a-14d, the samples show that in most cases, the embossed only samples have high stiffness to provide acceptable recovery energy. Meanwhile, for the samples with conforming features, acceptable recovery energy is achieved at a lower stiffness level. In addition, the ratio of "stiffness / recovery energy" is reduced by almost 50% or more for the samples with conforming features. Therefore, it is believed that the samples with these conforming features can recover from bunching and maintain the pad shape more comfortably and conformably without relying on synthesis to do so. It is believed that a wet recovery energy of less than 0.4 mJ may cause the absorbent article to have conformability and possible performance issues during use since it cannot recover its shape when wet.
[0209] The stiffness to wet energy recovery ratio of less than 17 can be achieved as shown by the data, regardless of the type of absorbent system. Specifically, when the absorbent core comprises a co-formed absorbent core with continuous filaments (Sample 2), a stiffness to wet energy recovery ratio of less than 4, more preferably less than 3, was achieved. In airlaid type absorbent cores, such as Samples 3 and 4, much lower stiffness to wet energy recovery ratios were achieved. For example, for Sample 3, by utilizing the conforming features described herein, the stiffness to wet energy recovery ratio was less than 17, more preferably less than 15, and most preferably less than 10. For Sample 4, by utilizing the conforming features described herein, the stiffness to wet energy recovery ratio was less than 13, more preferably less than 10, and most preferably less than 8.
[0210] The ratio 2 is between bending stiffness and caliper. As the data shows, there is a significant reduction in stiffness of products with conforming features compared to those that are embossed. Many of the samples with conforming features show a 50% reduction in stiffness over the embossed samples, even when the samples have a higher caliper, theoretically increasing stiffness.
[0211] As demonstrated by the data, stiffness to caliper ratios of 4 or less can be achieved. Specifically, when the absorbent core comprises a coformed absorbent core with continuous filaments (Sample 2), stiffness to caliper ratios of 4 or less, more preferably less than 2, were achieved. Much lower stiffness to caliper ratios were achieved for airlaid type absorbent cores, such as Samples 3 and 4. For example, for Sample 3, by utilizing the conforming features described herein, the stiffness to caliper ratio was less than 5, more preferably less than 4. For Sample 4, by utilizing the conforming features described herein, the stiffness to caliper ratio was less than 15, more preferably less than 10, and most preferably less than 5.
[0212] In addition, the data shows the fact that the bending stiffness and bending modulus can be influenced based on the fitting features provided in the article to allow for a customizable fit to the unique anatomy of the user. In addition, the data shows that the arrangement of zones within the absorbent article can similarly affect the bending stiffness and bending modulus to provide the most comfortable fit to the body. The same is true for the recovery energy and recovery rate.
[0213] In terms of bending stiffness, absorbent articles including the conforming features described herein exhibited lower bending stiffness than their conventional counterparts. For example, for products including the absorbent core of Sample 2, the bending stiffness was less than 12, more preferably less than 8, and most preferably less than 5. For Sample 3, the bending stiffness was less than 15, more preferably less than 12. For Sample 4, the bending stiffness was less than 40, more preferably less than 20, and most preferably less than 15.
[0214] The data on the fluid dynamics of the samples listed in Table 3 are listed in Table 4 below. The data are from the NMR mouse method, the free fluid acquisition test, and the blot test described herein. The NMR test measures the ability of the product to wick fluid away from the area closest to the body. A low value in this test suggests that the user may experience a dry feel. In addition, a low value in the NMR test suggests that the article can regenerate void volume for the next insult. The free fluid acquisition test measures the rate of absorption of a fluid insult into the topsheet. A lower number suggests that the article can quickly absorb a liquid insult. The blot test measures the amount of residual fluid remaining on the body as well as how much of the product area can stain.
[0215] [Table 4]
[0216] Ratio 3 is between blot residue vs. caliper. In Samples 12a-14d, the samples including conforming features provide at least a 50% reduction in residual fluid compared to embossing alone. Thus, not only do we achieve less fluid on the skin analog, but we can achieve this in a thinner, more conforming, and more comfortable absorbent article.
[0217] Blot to caliper ratios of less than 11 can be achieved regardless of the type of absorbent system as shown by the data. Specifically, when the absorbent core comprises a co-formed absorbent core with continuous filaments (Sample 2), blot to caliper ratios of less than 12, more preferably less than 11, and most preferably less than 8 were achieved. Much lower blot to caliper ratios were achieved with airlaid type absorbent cores, such as Samples 3 and 4. For example, for sample 3, by utilizing the matching features described herein, the blot to caliper ratio was less than 19, more preferably less than 15, and most preferably less than 10. For sample 4, by utilizing the matching features described herein, the blot to caliper ratio was less than 20, more preferably less than 15, and most preferably less than 10.
[0218] In addition, the data shows the fact that residual fluid (NMR), free fluid acquisition time, blot residual amount, and blot stain size can be improved from that shown by conventional layer attachment methods or embossing based on the conforming features provided on the article.For example, the NMR data for the absorbent core of sample 4 was much lower than that measured for the absorbent article that does not include the conforming features of the present disclosure, less than 200 μL, more preferably less than 100 μL, and most preferably less than 50 μL.Similarly, for the absorbent core of sample 3, the NMR data showed a decrease by providing conforming features, i.e., less than 20 μL, more preferably less than 17 μL.For the product including the absorbent core of sample 2, it showed NMR data of less than about 7 μL, while also having a free fluid acquisition time of less than 100 seconds.
[0219] With respect to blot testing, the data also show that products including the Compliant Features consistently had lower values than their conventional counterparts. For example, for those products utilizing the absorbent core of Sample 2, the blot residue values were less than 30 mg, more preferably less than 20 mg, and most preferably less than 18 mg. For each of Samples 3 and 4, the blot residue values were less than 50 mg, more preferably less than 40 mg, and most preferably less than 30 mg.
[0220] In addition, the data shows that the placement of the zones within the absorbent article can affect bending stiffness and bending modulus as well as recovery energy and recovery rate.
[0221] sample: Sample 1: A co-formed absorbent core having a total basis weight of 224 gsm. The co-formed absorbent core contained 121.8 gsm cellulose fibers, 52.2 gsm 3.0 micrometer continuous polypropylene fibers, and 50 gsm superabsorbent polymer (AGM). These materials were homogeneously blended.
[0222] Sample 2: A co-formed absorbent core having a total basis weight of 186 gsm. The co-formed absorbent core contained 105 gsm cellulose, 45 gsm 3.0 micrometer continuous polypropylene fibers, with 36 gsm AGM. These materials were homogeneously blended.
[0223] Sample 3: 150 gsm airlaid absorbent on a carded nonwoven material. The material contained 4 mm polyethylene / polyethylene terephthalate fibers, cellulose fibers, and a latex binder material. This material did not contain any superabsorbent polymer.
[0224] Sample 4: Monolithic airlaid absorbent core with a basis weight of 160 gsm. The absorbent core comprises cellulose fibers and superabsorbent polymer with a low percentage of binding fibers. Available from Gladfelter GmbH, Falkenhagen Germany. Fibrous superabsorbent polymers may also be utilized.
[0225] Sample 5: Carded spunlace (38-40 mm fiber length) material having a basis weight of 140 gsm containing 21.8 percent viscose rayon, 35.4 percent bicomponent fibers (polyethylene terephthalate and copolyethylene terephthalate), and 42.9 percent polyethylene terephthalate monocomponent fibers.
[0226] For samples 6a-14d, many were provided with matching features oriented in the negative Z direction according to the following patterns: Diamond - shown in first zone 1520 and second zone 1540 of FIG. 17A. The diamond pattern features teeth of different lengths. The engagement depth of the features was 2.54 mm and the spacing between the teeth was 2.03 mm. Center - shown in a portion of target area 1530 of FIG. 17A (in the area seen as a figure eight). The teeth in the center pattern were staggered. The engagement depth of the features was 2.54 mm and the spacing between the teeth was 2.03 mm. ALT - this pattern was formed by teeth 7000 shown in FIG. 21. Teeth were provided in a column direction and alternating row direction as shown. The engagement depth was 2.54 mm and the spacing between the teeth was 2.54 mm.
[0227] Samples 6a, 6b, and 6c: Sample 2 material was provided with matching features including a diamond pattern in 6a, a center pattern in 6b, and an ALT pattern in 6c.
[0228] Samples 7a, 7b, and 7c: Sample 3 material was provided with matching features including a diamond pattern in 7a, a center pattern in 7b, and an ALT pattern in 7c.
[0229] Samples 8a, 8b, and 8c: Sample 4 material was provided with matching features including a diamond pattern in 8a, a center pattern in 8b, and an ALT pattern in 8c.
[0230] Samples 9a, 9b, and 9c: A 24 gsm hydrophilic carded nonwoven and Sample 2 material were provided with matching features including a diamond pattern in 9a, a center pattern in 9b, and an ALT pattern in 9c. The 24 gsm nonwoven was utilized as a fluid management layer in these samples and was placed directly above the absorbent core.
[0231] Samples 10a, 10b, and 10c: Laminate materials including the material of Sample 3 and 35 gsm AGM and tissue layers were provided with matching features including a diamond pattern in 10a, a center pattern in 10b, and an ALT pattern in 10c.
[0232] Samples 11a, 11b, and 11c: 110 gsm carded spunlace (38-40 mm fiber length) material comprising 35.9 percent viscose, 34.1 percent polyethylene terephthalate, and 30 percent polyethylene terephthalate / copolyethylene terephthalate bicomponent fibers with matching features including a diamond pattern in 11a, a center pattern in 11b, and an ALT pattern in 11c, and Sample 4 material were provided.
[0233] Each of Samples 12a-14d included a hydrophobic 24 gsm carded through-air bonded nonwoven having bicomponent fibers having polyethylene and polyethylene terephthalate, and a bottom layer of a 25 gsm spunbond web including bicomponent fibers having polyethylene and polypropylene components, the bottom layer being surfactant treated at 0.45% by weight. The top and bottom layers were perforated via the strong bonding process described in Figures 9A and 9B and contained the hole pattern shown in Figure 22. This material is collectively referred to as the topsheet in the remaining sample descriptions.
[0234] In addition, some of the samples, namely 12a, 13a, and 14a, were provided with embossing, which, as previously mentioned, is not considered a conforming feature in this disclosure. To facilitate review of this data, the terms "embossed," "DIA" (for diamond), "CEN" (for center), or "ALT" are utilized in the tables for samples 12a-14d.
[0235] Samples 12a, 12b, 12c, and 12d: Topsheets and materials described in Samples 9a, 9b, and 9c were provided, including an embossed pattern in 12a, a diamond pattern in 12b, a center pattern in 12c, and an ALT pattern in 12d.
[0236] Samples 13a, 13b, 13c, and 13d: Topsheets and materials described in Samples 10a, 10b, and 10c were provided, including an embossed pattern in 13a, a diamond pattern in 13b, a center pattern in 13c, and an ALT pattern in 13d.
[0237] Samples 14a, 14b, 14c, and 14d: Topsheets and materials described in Samples 11a, 11b, and 11c were provided, including an embossed pattern in 14a, a diamond pattern in 14b, a center pattern in 14c, and an ALT pattern in 14d.
[0238] Conventional sample 1 - Always Ultra Thin size 1 available on the Western market.
[0239] Conventional sample 2 - SCA Bodyform size 1 available on the Western European market.
[0240] Test Method Target demographic For any of the following methods in which not all of the constituent layers of an article are tested, the layers of interest may be separated from the layers not being tested, if necessary, using cryospray.
[0241] AMF (Artificial Menstrual Fluid) Artificial menstrual fluid (AMF) is composed of a mixture of defibrinated sheep blood, phosphate buffered saline, and mucus components. AMF is prepared to have a viscosity of 7.15-8.65 centistokes at 23 °C.
[0242] The viscosity of the AMF is performed using a low viscosity rotational viscometer (a suitable instrument is a Cannon LV-2020 Rotary Viscometer with a UL adapter (Cannon Instrument Co., State College, US) or equivalent). The appropriate size spindle for the viscosity range is selected and the instrument is operated and calibrated according to the manufacturer. Measurements are taken at 23° C.±1° C. and 60 rpm. Results are reported to the nearest 0.01 centistokes.
[0243] Reagents required for AMF preparation include defibrinated sheep blood with a hematocrit of 38% or greater (drawn under sterile conditions, available from Cleveland Scientific, Inc., Bath, Ohio, or equivalent), gastric mucin (crude form, available from Sterilized American Laboratories, Inc., Omaha, Neb., or equivalent) with a target viscosity of 3-4 centistokes when prepared as a 2% aqueous solution, 10% v / v lactic acid in water, 10% w / v potassium hydroxide in water, sodium phosphate dibasic anhydrous (reagent grade), sodium chloride (reagent grade), sodium phosphate monobasic monohydrate (reagent grade), and distilled water (each available from VWR International or an equivalent source).
[0244] The phosphate buffered saline solution consists of two individually prepared solutions (Solution A and Solution B). To prepare 1 L of solution A, add 1.38 ± 0.005 g of sodium phosphate monobasic monohydrate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the vessel volume. Mix thoroughly. To prepare 1 L of solution B, add 1.42 ± 0.005 g of sodium phosphate dibasic anhydrous and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the vessel volume. Mix thoroughly. To prepare phosphate buffered saline, add 450 ± 10 mL of solution B to a 1000 mL beaker and stir at low speed on a stir plate. Insert a calibrated pH probe (accurate to 0.1) into the beaker of Solution B and add, with stirring, enough Solution A to bring the pH to 7.2±0.1.
[0245] The mucus component is a mixture of phosphate buffered saline solution, aqueous potassium hydroxide solution, gastric mucin, and aqueous lactic acid solution. The amount of gastric mucin added to the mucus component directly affects the final viscosity of the prepared AMF. To determine the amount of gastric mucin required to obtain an AMF within the target viscosity range (7.15-8.65 centistokes at 23°C), three batches of AMF with various amounts of gastric mucin in the mucus component are prepared, then a least squares linear fit through the three points is performed and the exact amount required is interpolated from the concentration vs. viscosity curve. A good range for gastric mucin is usually 38-50 grams.
[0246] To prepare approximately 500 mL of mucus component, add 460±10 mL of previously prepared phosphate buffered saline solution and 7.5±0.5 mL of 10% w / v potassium hydroxide solution in water to a 1000 mL sturdy glass beaker. Place the beaker on a stirring hot plate and bring the temperature to 45°C±5°C while stirring. Weigh out a predetermined amount of gastric mucus (±0.50 g) and slowly sprinkle it into the previously prepared liquid at 45°C without clumping. Cover the beaker and continue mixing. Over the course of 15 minutes, bring the temperature of the mixture to above 50°C but below 80°C. Continue heating with gentle stirring while maintaining this temperature range for 2.5 hours. After 2.5 hours, remove the beaker from the hot plate and allow it to cool to below 40°C. Then add 1.8±0.2 mL of 10% v / v lactic acid solution in water and mix thoroughly. Autoclave the mucus component mixture at 121°C for 15 minutes and allow to cool for 5 minutes. Remove the mucus component mixture from the autoclave and stir until the temperature reaches 23°C ± 1°C.
[0247] Allow the temperature of the sheep blood and mucus components to be 23 °C ± 1 °C. Using a 500 mL graduated cylinder, measure the volume of the entire batch of previously prepared mucus components and add that volume to a 1,200 mL beaker. Add an equal volume of sheep blood to the beaker and mix thoroughly. Using the viscosity method previously described, verify that the viscosity of the AMF is between 7.15 - 8.65 centistokes. If not, discard the batch and make another batch, adjusting the mucus components as needed.
[0248] Certified AMF should be refrigerated at 4°C unless intended for immediate use. AMF may be stored in an airtight container at 4°C for up to 48 hours after preparation. Prior to testing, AMF should be at 23°C ± 1°C. After testing is complete, any unused portion is discarded.
[0249] Blot test The blot test measures the amount of AMF transferred from the blotter to the article (as residual AMF left on the blotter) and measures the size of the stain as measured on the surface of the article. The blot was repeated on the same specimen a total of five times, and the cumulative blot dimensions and individual amounts remaining on the blotter were recorded after each blot. The blotter sheet (Apollo Plain Paper Copier Transparency Film, available under the ACCO brand, Ronkonkoma, NY, or equivalent) was used as the blotting surface. The surface energy of the blotting sheet, as determined by ASTM D7490-13, is approximately 50 mJ / m 2 For testing, the blotter sheet is cut to dimensions of 76 mm long by 63 mm wide. A 76 mm long by 63 mm wide by 3 mm thick nylon plate is combined with a weight to have a total mass that provides a confining pressure of 0.69 KPa on the test specimen. The AMF described herein is used as the test fluid.
[0250] A cutting die (76 mm long x 63 mm wide) is used to cut a test specimen from the longitudinal and lateral midpoints of the article. The release paper is removed and lightly dusted with talc to reduce tack. The mass of one blotter sheet is measured and recorded to the nearest 0.0001 g. The sheet is placed on the bench top. 1.00 mL of AMF is pipetted onto the center of the blotter sheet. Align the specimen with the edge of the sheet and place the specimen on the blotter sheet with the side facing the body down. Place a nylon plate and weight on top of the specimen and wait for 15 minutes. The plate and weight are then removed and the specimen is removed. Place the body side of the specimen face up on the bench. The mass of the blotter sheet and the residual AMF is measured and recorded to the nearest 0.0001 g. Subtract the original mass of the blotter sheet from the total mass and report to the nearest 0.0001 g as the residual AMF. Using a calibrated ruler, measure the bounding box (rectangle) surrounding the stain as observed from the top of the specimen and record its length in the CD and its length in the MD. Calculate and record the stain area as observed from the top (CD x MD) and measure to within 1 mm 2The specimen is turned over and the bounding box (rectangle) surrounding the stain observed from the bottom of the specimen is measured and recorded as its length in the CD and its length in the MD. The stain area observed from the bottom (CD x MD) is calculated and recorded to within 1 mm 2 Record in units.
[0251] The specimen is loaded in a similar manner using the same blotter sheet and specimen four more times, using 1.00 mL aliquots for each cycle. For each cycle, the amount of AMF remaining on the blotter sheet and the stained area as viewed from both the top and bottom of the specimen are reported.
[0252] Bunch Compression The bunch compression properties of the samples are measured with a constant rate of extension tensile tester (a suitable instrument is MTS Alliance using Testworks 4.0 Software, or equivalent, available from MTS Systems Corp., Eden Prairie, Minn.) using a load cell that measures forces within 10% to 90% of the cell limits. All tests are performed in a room conditioned at 23°C ± 3°C and 50% ± 2% relative humidity. Tests can be performed under wet or dry conditions.
[0253] 25-27B, the bottom stationary fixture 3000 includes two matching specimen clamps 3001, each 100 mm wide, attached to a unique moveable platform 3002a, 3002b. The clamps have a 110 mm long "knife edge" 3009 that grips a 1 mm thick hard rubber surface 3008. When closed, the clamps are flush with the inside of their respective platforms. The clamps are aligned to hold the loose specimen horizontally and perpendicular to the tensile axis of the tensile tester. The platform is mounted on rails 3003, which allow it to be moved horizontally from side to side and locked into place. The rails have an adapter 3004 that fits the tensile tester, which allows the platform to be fixed horizontally and perpendicular to the tensile axis of the tensile tester. The top fixture 2000 is a cylindrical plunger 2001 with an overall length of 70 mm and a diameter of 25.0 mm. The contact surface 2002 is flat and has no curvature. The plunger 2001 has an adapter 2003 that fits onto a load cell, which can fix the plunger perpendicular to the tensile axis of the tensile tester.
[0254] Condition the specimens at 23°C ± 3°C and 50% ± 2% relative humidity for at least 2 hours prior to testing. If testing the entire article, remove the release paper from the panty fastening adhesive on the garment-facing side of the article. Lightly coat the adhesive with talc powder to reduce any sticky feeling. Cut off any cuffs with scissors so that they do not affect the topsheet of the product. Place the article body-facing surface up on the bench. Identify the intersection of the longitudinal and transverse centerlines on the article. Using a rectangular cutting die, cut the specimen 100 mm long and 80 mm wide, centered on the intersection of the centerlines. If testing only the absorbent portion of the article, place the absorbent portion on the bench in the same orientation as it will be incorporated into the article (i.e., identify the body-facing surface and the transverse and longitudinal axes). Using a rectangular cutting die, cut the specimen 100 mm long and 80 mm wide, centered on the intersection of the centerlines.
[0255] Specimens may be analyzed both wet and dry. No further preparation is required for dry samples. For wet specimens, add 7.00 mL ± 0.01 mL of 10% w / v saline solution (100.0 g NaCl diluted in 1 L deionized water). The dose is applied using a graduated Eppendorf pipette while spreading the fluid over the entire body-facing surface of the specimen within approximately 3 seconds. Wet specimens are tested 15.0 minutes ± 0.1 minutes after dose application.
[0256] The tensile tester is programmed to zero the load cell and then lower the upper fixture at 2.00 mm / sec until the plunger contact surface touches the sample and the load cell reads 0.02 N. The crosshead is zeroed. The system is programmed to lower the crosshead 15.00 mm at a rate of 2.00 mm / sec and immediately raise the crosshead 15.00 mm at a rate of 2.00 mm / sec. This cycle is repeated for a total of 5 cycles with no delay between cycles. Data during all compression / decompression cycles is collected at 100 Hz.
[0257] The left platform 3002a is positioned 2.5 mm from the side of the upper plunger (distance 3005). The left platform is fixed in position. This platform 3002a remains stationary throughout the experiment. The right platform 3002b is aligned 50.0 mm from the stationary clamp (distance 3006). The upper probe 2001 is raised so that it does not interfere with the loading of the specimen. Both clamps are opened. The specimen is fixed in the clamps along its longitudinal edge (i.e. the 100 mm long edge). The specimen is laterally centered and both edges are clamped securely. The right platform 3002b is moved a distance of 20.0 mm towards the fixed platform 3002a. When the movable platform is positioned, the specimen is bent upwards. The probe 2001 is manually lowered until its lower surface is approximately 1 cm from the top surface of the bent specimen.
[0258] The test is started and data of displacement (mm) vs. force (N) is collected for all five cycles. A graph of force (N) vs. displacement (mm) is generated for every cycle individually. A representative curve is shown in FIG. 27A. From the curve, the maximum compression force for each cycle is recorded to the nearest 0.01 N. The % recovery between the first and second cycle is calculated as (TD-E2) / (TD-E1)×100, where TD is the total deflection and E2 is the extension in the two compression curves above 0.02 N. It is recorded to the nearest 0.01%. In a similar manner, the % recovery between the first and other cycles is calculated as (TD-E i ) / (TD-E1) * Calculate the energy loss for cycle 1 as the area under the compression curve (i.e., area A+B) and record to the nearest 0.1 mJ. Calculate the energy loss for cycle 1 as the area between the compression curve and the decompression curve (i.e., area A) and record to the nearest 0.1 mJ. Calculate the recovery energy for cycle 1 as the area under the decompression curve (i.e., area B) and record to the nearest 0.1 mJ. Similarly, calculate the compression energy (mJ), energy loss (mJ), and recovery energy (mJ) for each of the other cycles and record to the nearest 0.1 mJ.
[0259] A total of five replicates were analyzed for each sample and the arithmetic mean for each parameter is reported. All results are reported specifically for dry or wet, including the test fluid (0.9% or 10%).
[0260] Caliper Caliper measurements at 0.69 KPa can be performed on the entire product or on specific layers of interest, which are isolated using cryospray if necessary. Prior to testing, the samples are conditioned for 2 hours at 23°C ± 3°C and 50% ± 2% relative humidity. Unless otherwise specified, caliper measurements are taken at the center of a visually identifiable zone.
[0261] The caliper of the specimen is measured using a calibrated digital linear caliper (e.g., Ono Sokki GS-503 or equivalent) with a 24.2 mm diameter foot and an anvil large enough to allow the specimen to lie flat. The foot applies a confining pressure of 0.69 kPa against the specimen. Zero the caliper foot against the anvil. Raise the foot and insert the specimen flat against the anvil with the side facing the body facing up, with the site of interest centered on the foot. Lower the foot onto the specimen at approximately 5 mm / sec. Read the caliper (mm) 5.0 seconds after the foot is on the specimen and record to the nearest 0.01 mm.
[0262] Long fiber basis weight Long fiber basis weight determines the basis weight of fibers longer than 6.0 mm found in the topsheet, secondary topsheet, and core of the article. Nonwovens such as spunlace, spunbond, or film laminates used as topsheets or fluid management layers are treated as long fiber.
[0263] A cutting die is used to cut a 25.4 mm x 25.4 mm specimen through the article at the longitudinal and transverse centers of the article. The edges of the specimen are cut parallel and perpendicular to the longitudinal and transverse axes of the article. The backsheet is then removed from the cut specimen and the mass of the remaining specimen is measured and recorded to the nearest 0.0001 g. The basis weight of the specimen is calculated and recorded to the nearest 0.01 gsm. The topsheet, secondary topsheet, and core are separated into individual specimens to be tested. The mass of each layer is measured to the nearest 0.0001 g and recorded as TS1, STS1, and C1, respectively. Each layer is inspected to determine whether it contains cellulose fibers.
[0264] The layer containing cellulose fibers is analyzed as follows: Prepare Schweizer stock reagent by dissolving copper(II) hydroxide in ammonium hydroxide (%50 v / v) in a ratio of 1:4 w / w. Immerse the test specimen in an amount of reagent in excess of 30 g for each gram of cellulose in the specimen. Place the mixture on an orbital shaker and allow to digest for 16 hours. The polymer fibers are then recovered from the mixture and placed in 50 mL of water. The washing process is repeated until the blue reagent is removed from the fibers. Transfer the fibers to a tared Petri dish and use a stereomicroscope to determine if the fibers are longer than 6.0 mm in length. Dry the fibers longer than 6.0 mm and measure and record their mass to the nearest 0.001 g.
[0265] Calculate the basis weight of layers that do not contain cellulose fibers and record to the nearest 0.01 gsm. For layers that contain cellulose, calculate the basis weight of fibers longer than 6.0 mm and record to the nearest 0.001 gsm. Add the basis weights of each layer to determine the total basis weight of fibers longer than 6.0 mm and report to the nearest 0.01 gsm.
[0266] 3-point bending The flexural properties of the samples are measured with a constant rate of extension tensile tester (a suitable instrument is an MTS Insight HSEL using Testworks 4.0 Software, available from MTS Systems Corp., Eden Prairie, Minn.) using a load cell that measures forces within 2% to 90% of the cell limits. All testing is performed in a conditioned room at 23° C.±3° C. and 50%±2% relative humidity.
[0267] The bottom fixture consists of two polished stainless steel bars, 3.175 mm in diameter and 60 mm in length, each mounted on its own vertical fork. The two bars are mounted horizontally, parallel to each other with their front and rear sides aligned, and the top radii of the bars are vertically aligned. The fixture also allows the two bars to move horizontally away from each other on a track, so that the distance between them can be determined while maintaining the orientation of the bars. The top movable fixture consists of a third bar, 3.175 mm in diameter and 60 mm in length, polished stainless steel, mounted on the vertical fork. When in position, the bars of the top fixture are parallel to and aligned front to back with the bars of the bottom fixture. Both fixtures include integral adapters suitable for fitting and fixing in place at their respective positions on the tensile tester, so that the bars are perpendicular to the movement of the tensile tester cross beam.
[0268] Set the distance between the bars of the lower fixture to 25mm ± 0.05mm (centre of bar to centre of bar) and centre the upper bar to the midpoint between the lower bars. Set the gauge (bottom of upper bar to top of lower bar) to 1.0cm.
[0269] Condition the specimens for 2 hours at 23°C ± 3°C and 50% ± 2% relative humidity prior to testing. The overwrap is removed and the release paper is removed from the pad. The exposed adhesive surface on the backsheet and wings, if present, is powdered with talc to remove adhesion. Excess talc is removed from the surface. The pad is laid flat, top sheet facing up on the lab bench, and the longitudinal centerline of the product is marked. The longitudinal centerline of the wings is then used to mark transverse lines throughout the product. If wings are not present, mark the midpoint of the core with a transverse line. Remove rectangular specimens from the front (Zone A), middle (Zone B), and rear (Zone C). Each specimen is centered along the longitudinal axis of the specimen and is 50.8 mm long by 30 mm wide, spanning the entire thickness of the product. Specimens in Zone A are centered 45.4 mm from the leading edge of the product. Zone B is centered between the transverse marks on the specimen. Zone C is centered 45.4 mm from the rear of the product. For each test, measure the caliper at the center as noted and record to the nearest 0.01 mm.
[0270] For compression testing, program the tensile testing machine to lower the crosshead 25 mm at a rate of 1.0 mm / sec and collect force (N) and displacement (m) data at 50 Hz before returning the crosshead to the gauge. The specimen is mounted so that it straddles the two lower bars and is centered under the upper bar. CD bending refers to bending along the longitudinal axis of the pad (longitudinal direction parallel to the bars) and MD bending refers to bending along the transverse axis of the pad (transverse direction parallel to the bars). Zero the crosshead and load cell. Start the experiment and collect data.
[0271] A graph of force (N) versus displacement (mm) is made. The maximum peak force is read from the graph and divided by the width of the specimen (m). The peak force / width is recorded to the nearest 0.1 N / m. From the curve, the slope is calculated as the maximum slope of a linear segment fitted to the curve, where the length of the segment incorporates 20% of the curve, then divided by the width of the specimen and reported to the nearest 0.1 N / mm. From the slope, the following is calculated: Elastic modulus (N / mm2 ) = gradient * [twenty five 3 / (4 * Sample Width * Caliper 3 )] Moment of inertia (mm 4 )=(sample width * Caliper 3 ) / 12 Bending stiffness (N * mm 2 ) = Elastic modulus * Moment of inertia In this case, the units of the caliper and the sample width are mm.
[0272] The measurements were repeated in the same manner for 10 MD and 10 CD specimens, and the elastic modulus was adjusted to 0.01 N / m for each of the 10 values. 2 The unit of bending stiffness is 0.01N. * mm 2 Report the averages separately in units of
[0273] NMR MOUSE The NMR-MOUSE (Mobile Universal Surface Explorer) is a portable open NMR sensor with a permanent magnet geometry that generates a very uniform gradient perpendicular to the scanner surface. With reference to Figs. 23 and 24, a frame 1007 with a horizontal plane 1006 supports the specimen and remains stationary during testing. The flat active volume of the specimen is excited and detected by a surface rf coil 1012 positioned above the magnet 1010 at a position that defines the maximum penetration depth into the specimen. By repositioning the active slice across the specimen with a high precision lift 1008, the scanner can generate a one-dimensional profile of the specimen's structure with high spatial resolution.
[0274] An exemplary instrument is the Profile NMR-MOUSE model PM25 with High-Precision Lift available from Magritek Inc. (San Diego, Calif.). The requirements for the NMR-MOUSE are a z-resolution of 100 μm, a measurement frequency of 13.5 MHz, a maximum measurement depth of 25 mm, a static gradient of 8 T / m, and an active volume (xy dimensions) of 40×40 mm. 2 Before enabling the instrument, perform phase alignment, check the resonant frequency, and check the external noise level according to the manufacturer's instructions. Inject the test fluid into the test specimen using a syringe pump capable of delivering in the range of 1 mL / min to 5 mL / min ± 0.01 mL / min. All measurements are performed in a room controlled at 23°C ± 0.5°C and 50% ± 2% relative humidity.
[0275] The test solutions are Paper Industry Fluid (PIF) prepared as follows: 15 g carboxymethylcellulose, 10 g NaCl, 4 g NaHCO3, 80 g glycerol (all available from SigmaAldrich) in 1000 g distilled water. 2 mM / L diethylenetriaminepentaacetate gadolinium(III) dihydrogen salt (available from SigmaAldrich) is added to each. After addition, the solutions are agitated for 1 hour at 160 rpm using a shaker. The solutions are then checked to ensure that no visible undissolved crystals remain. The solutions are prepared 10 hours prior to use.
[0276] Condition the test product for 2 hours at 23°C ± 0.5°C and 50% ± 2% relative humidity prior to testing. Identify the intersection of the lateral and longitudinal centerlines of the product. Cut a 40.0 mm x 40.0 mm test specimen from the product, centered on the intersection and with the cut edges parallel and perpendicular to the longitudinal axis of the product. Attach the garment-facing side of the test specimen 1003 onto a 50 mm x 50 mm x 0.30 mm glass slide 1001 using 40.0 mm x 40.0 mm double-sided tape 1002 (the tape should be suitable for providing an NMR amplitude signal). Prepare the top cap 1004 by adhering two 50 mm x 50 mm x 0.30 mm glass slides 1001 using 40 mm x 40 mm double-sided tape 1002. The cap is then placed over the test specimen. The two tape layers are used as functional markers to define the dimensions of the instrumented test specimen.
[0277] First, collect a 1-D drying distribution profile of the specimen. Place the prepared specimen on the instrument aligned above the coil. Program the NMR-MOUSE for a Carr-Purcell-Meiboom-Gill (CPMG) pulse sequence consisting of a 90x pulse followed by a 180y refocused pulse using the following conditions: Repeat time = 500ms Number of scans = 8 Number of echoes = 8 Resolution=100μm Step size = -100μm
[0278] Collect NMR amplitude data (arbitrary units, au) versus depth (µm) as the precision lift step through the entire depth of the specimen.
[0279] The second measurement is an experiment of the velocity of the test fluid moving through the active NMR volume as it is slowly added onto the specimen. A calibrated dispenser pipette is used for a "drip" and then a "bulk" addition. The NMR-MOUSE is programmed for the CPMG pulse sequence using the following conditions: Measurement depth = 5mm Repeat time = 200ms 90° amplitude = -7dB 180° amplitude = 0dB Pulse length = 5 μs Echo time = 90 μs Number of echoes = 128 Echo shift = 1 μs Pre-trigger experiment = 50 Post-trigger experiment = 2000 Rx Gain = 31dB Acquisition time = 8μs Number of scans = 1
[0280] The Rx phase is determined during phasing as described by the vendor. In our experiments, a value of 230° was typical. The pulse length depends on the measurement depth, which here is 5 mm. If necessary, the depth can be adjusted using the spacer 1011.
[0281] Use the precision lift to adjust the height of the specimen so that the desired target area is aligned with the active volume of the instrument. The target area can be selected based on the SEM cross section. Program the syringe pump to deliver 1.00 mL / min ± 0.01 mL for 1.00 min for PIF test fluid or 5.00 mL / min ± 0.01 mL for 1.00 min for 0.9% saline test fluid. Start the measurement and collect NMR amplitudes (au) for 50 runs to obtain a signal baseline before flowing any fluid. Place the outlet tubing of the syringe pump over the center of the specimen and move it while applying the liquid to the entire sample surface, but do not touch the sample border. Start the system and continue collecting NMR amplitude data while simultaneously beginning to flow 1 mL of fluid over 60 seconds. 300 seconds after starting, add 0.50 mL of test fluid to the center of the specimen via a calibrated Eppendorf pipette at approximately 0.5 mL / sec. After the second "bump" dose is added, the generated NMR amplitude versus time graph can be used to similarly determine the % change in signal amplitude versus time, e.g., the time required for the amplitude signal to drop by 20%, 30%, 50%, 75% or 100% from the peak after the "bump" dose. The drop in signal amplitude occurs as fluid is absorbed and dispersed beyond the preset NMR viewing range.
[0282] The third measurement is a 1-D wetting profile. Immediately after the rate measurement is completed, the cap is replaced on the specimen. The wetting profile is run under the same experimental conditions as the preceding drying profile described above.
[0283] Calibration of the NMR amplitude to the velocity signal can be performed by filling glass vials (external diameter 8 mm, defined internal diameter with a height of at least 50 mm) with the appropriate fluid. Set the instrument conditions as described for the velocity experiment. A calibration curve is constructed by increasing the number of vials on the instrument (vials should be equally placed over a measurement area of 40 mm x 40 mm) and perform velocity measurements. The volume is calculated as the total cross-sectional area of the vials present x z-resolution, where the resolution (mm) is calculated as 1 / acquisition time (s) ÷ gradient strength of the instrument (Hz / mm). Calibration of the NMR amplitude to the distribution profile is performed as an internal calibration based on the dry and wet profiles. In this procedure, the areas under the wet and dry profiles are calculated and, after subtracting them, the total area (excluding markers) is obtained. This total area correlates with the amount of liquid applied (here 1.5 mL). The amount of liquid (µL) per 100 µm step can then be calculated. From the 1-D wetting distribution profile, the volume of the top 0.5 mm of the sample is calculated and reported in microliters (to the nearest 0.1 microliter).
[0284] free fluid capture Artificial menstrual fluid (AMF) prepared as described herein is applied onto the surface of the article. All measurements are performed at constant temperature (23° C.±2° C.) and relative humidity (50%±2%).
[0285] Prior to testing, absorbent article samples are conditioned for 2 hours at 23°C ± 2°C and 50% ± 2% relative humidity. Lay the sample article flat with the top sheet of the product facing up. Position the tip of a mechanical pipette approximately 1 cm above the center (longitudinal and lateral midpoint) of the absorbent core of the article and precisely pipette 1.00 mL ± 0.05 mL of AMF onto the surface. Dispense the fluid without splashing within 2 seconds. As soon as the fluid comes into contact with the test sample, start a timer with 0.01 second accuracy. After the fluid is acquired (no pooling of fluid remaining on the surface), stop the timer and record the acquisition time to the nearest 0.01 second. Wait 2 minutes. Similarly, apply a second and third AMF to the test sample and record the acquisition time to the nearest 0.01 second.
[0286] This entire procedure is repeated on five substantially similar replicate articles, and the reported value is the average of five individual recorded measurements of free fluid acquisition time (1st, 2nd and 3rd) to the nearest 0.01 seconds.
[0287] Overlap distance test A scanning electron microscope (SEM) is used to obtain an image of a cross section of an absorbent article in which recesses have been purposefully created, from which the amount of overlap of the fiber masses immediately adjacent the recesses is measured. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and specimens are conditioned in this environment for at least 2 hours prior to testing.
[0288] If necessary, a test specimen is obtained by excising the layer of interest from the absorbent article. When excising the individual layer (or layers), care is taken not to impart any contamination or distortion to the test area during the process. The test area includes the area where the recess is intentionally created. A razor blade (e.g., VWR Single Edge Industrial, 0.009 inch thick surgical carbon steel, available from VWR Scientific, Radnor, PA, USA, or equivalent) is used to excise the test specimen. The razor blade is used to cut along the transverse axis of the recess at its longitudinal midpoint so that the cross section of the recess can be imaged. The test specimen is then attached to a mount using double-sided Cu tape, cross-section side up, and sputter-coated with AU.
[0289] Secondary electron (SE) images of the cross-section of the specimen are obtained using an SEM (e.g., FEI Quanta 450, available from FEI Company, Hillsboro, OR, USA, or equivalent) operated in high vacuum mode, using an accelerating voltage of 3-5 kV and a working distance of approximately 12-18 mm. This method assumes that the analyst is skilled in operating the SEM and can obtain images of sufficient contrast for analysis. The instrument is calibrated according to the manufacturer's specifications prior to use to ensure an accurate distance scale.
[0290] The specimen is observed at a magnification that allows clear visualization of the entire depth of the recess along with the fiber clumps on each side of the recess, and an image is acquired. The image is then analyzed to determine the overlap of the fiber clumps. Referring again to FIG. 15C, first, a centerline 1507 running parallel to the z-direction (thickness) of the specimen is drawn and intersects with the center of the recess (e.g., where the fiber clumps meet). A base line 1509 running parallel to the xy-directions of the specimen at the base of the recess is drawn on the image. Following the contour of the fiber clump along the edge closest to the recess, determine where the fiber clump edge reaches the base line and marks it as "OD" (line 1505). The distance 1503 between the centerline and the location "OD" is measured to the nearest 0.01 mm and recorded as the overlap distance. The same method was repeated a total of five times. The arithmetic mean of the overlap distance is calculated and reported to the nearest 0.01 mm.
[0291] Surface Energy / Contact Angle Method Contact angles on substrates are determined using ASTM D7490-13, modified according to the specifications described herein, using a goniometer fitted with a 1 mL gas-tight syringe with a No. 27 rounded tip stainless steel needle and suitable image analysis software (a suitable instrument is an FTA200 from First Ten Angstroms, Portsmouth, VA or equivalent). Two test fluids are used: Type II reagent water (distilled water) according to ASTM specification D1193-99 and 99+% pure diiodomethane (both available from Sigma Aldrich, St. Louis, MO). The contact angles from these two test fluids can further be used to calculate the surface energy based on the Owens-Wendt-Kaeble equation. All tests shall be performed at about 23° C.±2° C. and a relative humidity of about 50%±2%.
[0292] Place the goniometer on a vibration isolation table and level the stage according to the manufacturer's instructions. The video imaging device should have an acquisition rate capable of capturing at least 10-20 images from the time the droplet strikes the specimen surface until it can no longer be resolved from the specimen surface. A typical imaging rate is 900 images / sec. Depending on the hydrophobicity / hydrophilicity of the specimen, the droplet may or may not wet the surface of the nonwoven specimen quickly. If acquisition is slow, images should be taken until 2% of the droplet volume is absorbed within the specimen. If acquisition is too fast, the first resolved image should be used if the second image shows a volume loss of more than 2%.
[0293] The specimen is placed on the stage of the goniometer and the hypodermic needle is adjusted to the distance from the surface recommended in the manufacturer's instructions (typically 3 mm). If necessary, the position of the specimen is adjusted to place the specimen at the desired site under the tip of the needle. The video device is focused so that a clear image of the droplet on the surface of the specimen can be captured. Image acquisition is started. A 5 μL ± 0.1 μL droplet is placed on the specimen. If there is visible deformation of the droplet shape due to movement, repeat at a different but equivalent desired location. From images where there is a 2% drop volume reduction, take two angle measurements at the droplet (one for each droplet edge). If the contact angles at the two edges differ by more than 4°, the value is to be excluded and the test is repeated at an equivalent location on the specimen. Five additional equivalent locations on the specimen are identified and a total of six measurements (12 angles) are repeated. The arithmetic mean for this side of the specimen is calculated and reported to the nearest 0.01°. In a similar manner, the contact angles on the opposite surface of the specimen for six drops (12 angles) are measured and reported separately to the nearest 0.01°.
[0294] To calculate the surface energy, the contact angles for both water and diiodomethane are to be tested as described above. The values for each test fluid are then substituted into two separate equations (one for each fluid) of the Owens-Wendt-Kaelble equation. This results in two equations and two unknowns. The unknowns are then resolved into the dispersive and polar components of the surface tension.
[0295] Owens-Wendt-Kaelble equation:
[0296]
number
[0297] [Table 5]
[0298] Since the polar component is zero, when a dispersive solvent, such as diiodomethane, is used, the Owens-Wendt-Kaelble equation simplifies to:
[0299]
number
[0300] Using the values from the table for diiodomethane and the measured value of θ, the equation can be rewritten as d s ) where the values from the table for water and θ (measured) and the calculated value (γ d s) to rewrite the Owens-Wendt-Kaelble equation into the polar component of the surface energy (γ p s ) can be solved. γ d s +γ p s The sum of these is the total solid surface tension and is reported to the nearest 0.1 dyn / cm.
[0301] Dimensions and values disclosed herein should not be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise indicated, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm."
[0302] All documents cited in this application, including all cross-referenced or related patents or patent applications, and any patent applications or patents to which this application claims priority or benefit, are incorporated by reference in their entirety herein, unless expressly stated to the contrary, exclusion or limitation. The citation of any document shall not be deemed to be prior art to any invention disclosed or claimed herein, or that it alone, or in combination with any other reference(s), teaches, suggests or discloses any such invention. Furthermore, in the event that any meaning or definition of a term in this document conflicts with a meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall control.
[0303] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.
Claims
1. A disposable absorbent article (1510, 1700) having a longitudinal centerline and a lateral centerline, a first region (1520) disposed at one end of the absorbent article, a second region (1540) disposed at an opposite end of the absorbent article, and a target region (1530) disposed between the first region and the second region, each of the first region, the second region, and the target region extending laterally across the disposable absorbent article, the absorbent article including zones which are areas exhibiting any one of a visual pattern, topography, absorption rate or characteristics, bending parameters, compression modulus, resilience, stretch parameters, or combinations thereof, different from another portion of the absorbent article, the disposable absorbent article further comprising: A top sheet (1217, 1317, 1714, 1924), Back seat (1716, 1925) and an absorbent core (1219, 1319, 1718, 1928) disposed between the topsheet and the backsheet; a fluid management layer disposed between the topsheet and the absorbent core; a target zone (1535) disposed within at least the target area, the target zone including a first plurality of conforming features (1215, 1315, 1415, 1615) in a combination of the absorbent core and at least one of the topsheet or the fluid management layer; a long fiber network included in at least one of the absorbent core, the topsheet, the fluid management layer, or a combination of the absorbent core and at least one of the fluid management layer or the topsheet; the long fiber network comprises fibers longer than 6 mm; the plurality of conforming features are not formed by embossing; A disposable absorbent article, wherein the absorbent core is intermixed with at least one of the topsheet and the fluid management layer in the conformation feature.
2. the matching feature is a recess formed between adjacent posts; The disposable absorbent article of claim 1 , wherein the fibers forming the long fiber network span the recess and support a bottom of the recess.
3. The disposable absorbent article of claim 1 or 2, wherein the absorbent core has a volume greater than any of the topsheet, the backsheet, and the fluid management layer.
4. The disposable absorbent article of any one of claims 1 to 3, further comprising a second plurality of conforming features, said second plurality of conforming features differing from said first plurality of conforming features in at least one of the following: shape, depth, length, distance between adjacent features, density of features per square centimeter, or orientation of the features.
5. The disposable absorbent article of claim 4 , wherein the second plurality of conforming features are included in the zones, the first zone and / or the second zone.
6. The disposable absorbent article of claim 5, wherein the absorbent article comprises the first zone and the second zone, the first zone and the second zone being positioned laterally and / or longitudinally outboard of the target zone within the target area.
7. The disposable absorbent article of any one of claims 1 to 6, wherein the absorbent core comprises a plurality of cellulosic fibers, and the absorbent core comprises the long fiber network.
8. The disposable absorbent article of any one of claims 1 to 7, wherein the absorbent core is an airlaid absorbent core comprising a plurality of cellulose fibers and a plurality of bonding fibers, the bonding fibers constituting at least 15% by weight of the absorbent core.
9. The disposable absorbent article of claim 8 , wherein said bondable fibers are of staple length.
10. The disposable absorbent article of claim 8 , wherein said bonded fibers are continuous.
11. The disposable absorbent article of any one of claims 1 to 6, wherein the long fiber network is comprised in combination of the absorbent core and the fluid management layer.
12. 12. The disposable absorbent article of claim 11, wherein said absorbent core comprises a first basis weight and said fluid management layer comprises a second basis weight, said second basis weight being at least 25 percent of said first basis weight.
13. The disposable absorbent article of claim 12, wherein said fluid management layer comprises staple filaments.
14. The disposable absorbent article of any one of claims 11 to 13, wherein said fluid management layer is hydroentangled or needlepunched.
15. 15. The disposable absorbent article of any one of claims 11 to 14, wherein the fluid management layer comprises cellulosic fibers and a plurality of bonding fibers, the absorbent core comprises a first basis weight, the bonding fibers comprise a second basis weight, and the second basis weight is at least 25 percent of the first basis weight.
16. The disposable absorbent article of any one of claims 1 to 6, wherein the long fiber network is comprised in a combination of the absorbent core and the topsheet.
17. The disposable absorbent article of any one of claims 1 to 6, wherein the long fiber network is comprised in combination of the absorbent core, the fluid management layer, and the topsheet.
18. The disposable absorbent article of claim 6 , wherein each of said first zone and said second zone extends from said first region to said second region.
19. 20. The disposable absorbent article of claim 18, wherein said target zone extends from said first region to said second region.
20. The disposable absorbent article according to any one of claims 18 to 19, wherein each of the first zone and the second zone is disposed longitudinally outboard of the target zone.
21. The disposable absorbent article of claim 6, wherein the target zone has a lower flexural modulus and / or flexural stiffness than the first zone and / or the second zone when measured by a three-point bending test disclosed in the specification filed together with the present claims.
22. 7. The disposable absorbent article of claim 6, wherein the absorbent article has a blot-to-caliper ratio of less than 11 and / or a stiffness-to-caliper ratio of 4 or less when measured by the blot test, caliper test, and three-point bend test disclosed in the specification filed with the present claims.
23. The disposable absorbent article of any one of the preceding claims, wherein said topsheet comprises a hydrophobic nonwoven having a basis weight of at least 20 gsm.
Citation Information
Patent Citations
Optical fiber cable for induction countermeasures
JP1985029715A
Absorbent article and its production method
JP2003291234A
Absorbent articles equipped with a fluid handling zone
JP2013518701A
Method and apparatus for producing an absorbent structure having an absorbent material (1)
JP2014515972A
Absorbent article
JP2015198798A