Conductive paste and its use

The conductive paste with surface-treated conductive particles, phenol resin, and oxidation inhibitors addresses the issue of surface oxidation, resulting in highly conductive films for improved electronic component performance.

JP7565812B2Active Publication Date: 2024-10-11NORITAKE MACHINE TECHNO CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021012250
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-28
Publication Date
2024-10-11
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

Existing conductive pastes used for forming conductive films in electronic components face challenges in maintaining high conductivity due to surface oxidation of conductive particles, which reduces the effectiveness of the films.

Method used

A conductive paste comprising conductive powder with a surface treatment agent, a phenol resin as the binder, and an oxidation inhibitor such as formic acid or acetic acid is used to suppress surface oxidation and improve conductivity.

Benefits of technology

The conductive paste effectively forms films with enhanced conductivity, enabling higher performance in electronic components by reducing surface oxidation and improving dispersibility of the conductive particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565812000005
    Figure 0007565812000005
  • Figure 0007565812000001
    Figure 0007565812000001
  • Figure 0007565812000002
    Figure 0007565812000002
Patent Text Reader

Abstract

To provide a conductive paste capable of forming a conductive film excellent in conductivity.SOLUTION: The conductive paste herein disclosed includes: a conductive powder; a binder resin; an organic solvent; and an oxidation retardant. A conductive particle having a surface preparation agent attached to its surface is included as the conductive powder. A phenol resin is included as the binder resin. The oxidation retardant is constituted mainly by one or two or more carboxylic acids selected from the group consisting of formic acid, acetic acid, and propionic acid. The oxidation retardant is contained by at least 0.05 wt.% of all.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive paste and its use. [Background technology]

[0002] In electronic elements for electric and electronic devices, a technique of printing a powder made of a conductive material on an insulating substrate to form a wiring pattern is widely adopted. The conductive powder for forming the wiring pattern is generally printed in the form of a conductive paste dispersed in a dispersion medium together with a binder resin. Such a conductive paste is applied to a substrate so as to form a desired shape, and a coating film made of the conductive paste is formed. Then, typically, the substrate and the coating film are subjected to a heat treatment to form a conductive film (i.e., a wiring pattern, etc.) on the substrate.

[0003] A thermosetting resin may be used as the binder resin, as in the techniques described in Patent Documents 1 to 5. In this case, a conductive film can be formed by curing the thermosetting resin contained in the coating film (i.e., the conductive paste). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 4-264302 [Patent Document 2] Patent No. 6089175 [Patent Document 3] Patent No. 5880441 [Patent Document 4] JP 2015-133182 A [Patent Document 5] Patent No. 5439995 Summary of the Invention

[0005] However, when forming a conductive film as described above, if the surface of the conductive particles constituting the conductive powder is oxidized, an oxide film is formed, which may reduce the conductivity of the conductive film. For this reason, Patent Documents 1 to 5 propose various methods for suppressing the surface oxidation of conductive particles. In recent years, there has been an increasing demand for electronic components with higher performance, and this has led to a demand for forming a conductive film with higher conductivity.

[0006] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a conductive paste capable of forming a conductive film having higher conductivity.

[0007] The conductive paste disclosed herein includes a conductive powder, a binder resin, an organic solvent, and an oxidation inhibitor. The conductive powder includes conductive particles having a surface treatment agent attached to the surface. The binder resin includes a phenol resin. The oxidation inhibitor is mainly composed of one or more carboxylic acids selected from the group consisting of formic acid, acetic acid, and propionic acid. The oxidation inhibitor is contained in an amount of at least 0.05% by weight of the total. In the conductive paste having such a configuration, by including the oxidation inhibitor, surface oxidation of the conductive particles constituting the conductive powder can be suppressed, and the conductivity of the conductive film can be improved.

[0008] In a preferred embodiment of the conductive paste disclosed herein, the surface treatment agent is composed of at least one compound selected from the group consisting of carboxylic acids, amines, and benzotriazoles. By using a conductive paste containing conductive particles to which a surface treatment agent of this composition is attached, a conductive film with improved conductivity can be obtained. In addition to the above effects, the dispersibility of the conductive particles can be improved.

[0009] In another preferred embodiment, the conductive powder is mainly composed of silver particles or copper particles, and a conductive film containing silver particles or copper particles having improved conductivity can be obtained.

[0010] In another preferred embodiment, the conductive powder is mainly composed of conductive particles having an aspect ratio of not more than 1.5, which can further improve the conductivity of the conductive film.

[0011] In another preferred embodiment, the conductive paste is used to form a wiring pattern on a substrate. By using the conductive paste, a wiring pattern with improved conductivity can be obtained, and high performance of electronic components can be realized.

[0012] According to the technology disclosed herein, a method for producing a conductive film is provided. The method includes preparing a substrate and the conductive paste, applying the conductive paste to the substrate, and heating the conductive paste applied to the substrate to harden the phenol resin contained in the conductive paste. By using the conductive paste disclosed herein, a conductive film having high conductivity can be formed. [Brief description of the drawings]

[0013] [Figure 1] 1 is a cross-sectional view illustrating a schematic diagram of a wiring board according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Preferred embodiments of the present invention will be described below. Note that matters other than those specifically mentioned in this specification (e.g., the configuration of the conductive paste) that are necessary for carrying out the present invention (e.g., the method of preparing the conductive paste, etc.) can be understood as design matters of a person skilled in the art based on the prior art in the field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the field.

[0015] In the following description, the term "conductive film" refers to an unfired film-like body obtained by applying a conductive paste onto a substrate and performing a heat treatment (i.e., thermal curing of the binder resin) at a temperature below the thermal decomposition temperature of the binder resin contained in the conductive paste (for example, below 300°C). The conductive film also includes wiring (linear body), wiring patterns, and solid patterns. In this specification, the expression "A to B" indicating a numerical range means A or more and B or less, and includes a range above A and below B. In this specification, "mainly composed of A" means that A is contained in at least 90% by weight or more, preferably 95% by weight or more, more preferably 98% by weight or more, and even more preferably 99% by weight or more, or 100% by weight of A.

[0016] <Conductive paste> The conductive paste disclosed herein is configured to form a conductive film by hardening a binder resin (described later) contained in the conductive paste. The conductive paste disclosed herein contains a conductive powder (A), a binder resin (B), an oxidation inhibitor (C), and an organic solvent (D). In this specification, the term "paste" includes a composition, an ink, a slurry, a suspension, and the like. Each component will be described below in order.

[0017] (A) Conductive powder The conductive powder is typically a powdered conductive material and is composed of conductive particles. The conductive powder is a component that imparts electrical conductivity to the resulting conductive film. The conductive particles are typically made of metal. The constituent material may be appropriately selected from various commonly used metallic conductive particle constituent materials, one or more of which may be selected depending on the application. Specific examples of the metal include simple metals such as aluminum (Al), nickel (Ni), copper (Cu), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), osmium (Os), iridium (Ir), platinum (Pt), and gold (Au), as well as alloys containing these metals.

[0018] Examples of the alloy include a silver-palladium (Ag-Pd) alloy, a silver-platinum (Ag-Pt) alloy, a silver-copper (Ag-Cu) alloy, a copper-nickel (Cu-Ni) alloy, a copper-manganese (Cu-Mn) alloy, a copper-tin (Cu-Sn) alloy, a copper-zinc (Cu-Zn) alloy, and a copper-aluminum (Cu-Al) alloy.

[0019] From the viewpoints of handling, cost, and electrical conductivity, it is preferable that the conductive powder is mainly composed of silver particles or copper particles. Here, "silver particles" refers to particles containing silver (Ag), examples of which include particles made of a simple substance of silver (Ag), particles made of an alloy containing silver, and silver-coated particles having a coating layer containing silver on the surface of a core particle. The silver-coated particles include core-shell particles having particles made of a simple substance of silver or an alloy containing silver on the surface. "Copper particles" refers to powders containing copper (Cu), examples of which include particles made of a simple substance of copper (Cu), particles made of an alloy containing copper, and copper-coated particles having a coating layer containing copper on the surface of a core particle. The copper-coated particles include core-shell particles having particles made of a simple substance of copper or an alloy containing copper on the surface.

[0020] Among the above, copper particles have been known to be easily oxidized on the surface, and the conductivity of the conductive film is easily reduced. The effects of the present invention can be particularly preferably achieved when a conductive powder mainly composed of copper particles is used.

[0021] The properties of the conductive particles, such as size and shape, are not particularly limited as long as they fall within the minimum dimension of the cross section of the desired conductive film (typically the thickness and / or width of the conductive film). The average particle diameter of the conductive particles can be approximately several tens of nm to several tens of μm, for example, 1 μm to 10 μm. In this specification, the term "average particle diameter" refers to the particle diameter (D) that corresponds to 50% cumulatively from the fine particle side in the volume-based particle size distribution measured by particle size distribution measurement based on a general laser diffraction / light scattering method. 50 Also called particle size.

[0022] Although not particularly limited, the average aspect ratio of the conductive particles can be about 1 to 100. The average aspect ratio can be obtained by observing the conductive particles with a SEM, randomly selecting a plurality of particles (e.g., 10 to 300 particles) from the obtained observation image, calculating the aspect ratio (ratio of major axis to minor axis) based on the major axis and minor axis of each particle, and obtaining the arithmetic average value.

[0023] The conductive particles may be spherical or non-spherical. "Spherical" refers to a shape that can be roughly regarded as a sphere (ball), including ellipsoids, polygons, and disks. The average aspect ratio of the spherical particles is 1.5 or less, and may be 1.4 or less, 1.3 or less, or 1.2 or less. "Non-spherical" refers to an average aspect ratio exceeding 1.5 (e.g., 1.6 or more, or 1.7 or more), including plate-like, scale-like, flake-like, and amorphous shapes. The upper limit of the aspect ratio is not particularly limited, and may be, for example, 50 or less, 20 or less, 10 or less, 5 or less, 4 or less, 3 or less, 2.5 or less, or 2 or less.

[0024] The conductive powder may be a mixture of spherical particles and non-spherical particles. From the viewpoint of improving the conductivity of the conductive film, it is preferable that the conductive powder contains more spherical particles than non-spherical particles. The content of the spherical particles contained in the conductive powder may be, for example, more than 50% by weight, and may be 60% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more, when the entire conductive powder is taken as 100% by weight.

[0025] The conductive powder includes conductive particles (A1) having a surface treatment agent attached to the surface. The surface treatment agent, when attached to the surface of the conductive particles, can suppress the surface oxidation of the conductive particles and improve the dispersibility of the conductive particles in the dispersion medium. As the surface treatment agent, any surface treatment agent typically used in this type of conductive paste can be used without any particular limitation. Suitable examples thereof include various carboxylic acids, amines, and benzotriazoles. The surface treatment agent is preferably composed of at least one compound selected from the group consisting of carboxylic acids, amines, and benzotriazoles.

[0026] The carboxylic acid may be either a monocarboxylic acid or a dicarboxylic acid. When the carboxylic acid has a hydrocarbon group (for example, a fatty acid), the number of carbon atoms contained in the hydrocarbon group of the carboxylic acid is, for example, 4 or more, and from the viewpoint of suppressing surface oxidation of the conductive particles and improving the dispersibility of the conductive particles in the dispersion medium, it is preferably 10 or more, and may be 15 or more. From the viewpoint of not excessively increasing the viscosity of the conductive paste, the number of carbon atoms may be 30 or less, may be 26 or less, or may be 22 or less, and is preferably 20 or less, for example, may be 18 or less. Alternatively, a polycarboxylic acid may be used as a surface treatment agent. The conductive particles having a carboxylic acid as a surface treatment agent attached to the surface may be a commercially available product, or may be prepared by reacting a carboxylic acid or a carboxylate with a metal powder (i.e., a conductive particle) in a liquid phase. The carboxylic acid or the carboxylate may be one type or two or more types.

[0027] Specific examples of carboxylic acids include saturated aliphatic monocarboxylic acids (saturated fatty acids) such as butanoic acid, pentanoic acid (valeric acid), hexanoic acid (caproic acid), heptanoic acid (enanthic acid), octanoic acid (caprylic acid), nonanoic acid (pelargonic acid), decanoic acid (capric acid), lauric acid, myristic acid, pentadecylic acid, palmitic acid, heptadecanoic acid (margaric acid), stearic acid, isostearic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, and melissic acid; and dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedicarboxylic acid. Examples of the carboxylic acid salt include carboxylic acids such as carboxylic acids or saturated aliphatic dicarboxylic acids, unsaturated aliphatic monocarboxylic acids (unsaturated fatty acids) such as palmitoleic acid, oleic acid, vaccenic acid, linoleic acid, eleostearic acid, linolenic acid, arachidonic acid, and nervonic acid, unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, itaconic acid, mesaconic acid, citraconic acid, dimer acid, trimer acid, and cyclohexanedicarboxylic acid, aromatic carboxylic acids such as benzoic acid, phthalic acid, terephthalic acid, isophthalic acid, orthophthalic acid, phenylbutyric acid, phenoxyacetic acid, ascorbic acid, and naphthalenedicarboxylic acid, and alkyl- and alkenyl-substituted carboxylic acids thereof, and acid anhydrides. Examples of the carboxylic acid salt as the surface treatment agent include alkali metal salts (sodium salt, potassium salt, etc.) and alkaline earth metal salts (magnesium salt, calcium salt, etc.) of the above-mentioned carboxylic acids.

[0028] The amine is preferably an aliphatic amine. The total number of carbon atoms contained in one molecule of the amine is preferably 5 or more, may be 10 or more, or may be 15 or more, from the viewpoint of suppressing the surface oxidation of the conductive particles and improving the dispersibility of the conductive particles in the dispersion medium. From the viewpoint of not excessively increasing the viscosity of the conductive paste, the total number of carbon atoms is, for example, preferably 30 or less, may be 26 or less, or may be 24 or less, or may be 20 or less. Alternatively, a polyamine may be used as the surface treatment agent. The conductive particles having an amine as a surface treatment agent attached to the surface may be a commercially available product, or may be prepared by reacting an amine with a metal powder (i.e., conductive particles) in a liquid phase. The amine may be one type or two or more types.

[0029] Specific examples of amines include primary amines such as pentylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine (laurylamine), tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, stearylamine, oleylamine, nonadecylamine, and eicosylamine; secondary amines such as dibutylamine, dipentylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, and didecylamine; and tertiary amines such as triethylamine, tripropylamine, tributylamine, tripentylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, and tridecylamine.

[0030] As the benzotriazoles, from the viewpoint of suppressing the surface oxidation of the conductive particles and improving the dispersibility of the conductive particles in the dispersion medium, the compounds described below can be preferably used. The conductive particles having the benzotriazoles attached to the surface as the surface treatment agent may be commercially available products, or may be prepared by reacting the benzotriazoles with metal powder (i.e., conductive particles) in a liquid phase. The benzotriazoles may be one type or two or more types.

[0031] Specific examples of benzotriazoles include 1H-benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, and the like.

[0032] Although not particularly limited, the amount of the surface treatment agent applied can be about 0.01 to 3 parts by weight, for example about 0.01 to 1 part by weight, relative to 100 parts by weight of the conductive powder.

[0033] From the viewpoint of better realizing the above-mentioned oxidation suppression effect and the above-mentioned dispersion improvement effect, the content of the conductive particles (A1) can be, for example, 60% by weight or more of the entire conductive powder, and is preferably 70% by weight or more, more preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight or more (for example, 98% by weight or more, or 100% by weight). The conductive powder may contain conductive particles (A2) having no surface treatment agent attached thereto, as long as the effects of the present invention can be realized.

[0034] The content of the conductive powder is not particularly limited, but may be, for example, 40% by weight or more of the entire conductive paste, typically 50% by weight to 95% by weight, for example 60% by weight to 90% by weight, 75% by weight to 85% by weight. By satisfying the above range, the denseness and conductivity of the conductive film can be improved. In addition, the handleability of the conductive paste and the workability during film formation can be improved.

[0035] (B) Binder resin The binder resin is a component having a function of binding the conductive particles together in the conductive film. The binder resin can also realize adhesion between the conductive film and the substrate and impart durability to the conductive film. Since the conductive film produced using the conductive paste disclosed herein is formed by thermal curing of the binder resin, the properties of the binder resin can be maintained in the conductive film. From the viewpoint of facilitating printing using the conductive paste (i.e., forming wiring), the binder resin is preferably dissolved homogeneously in an organic solvent described below at room temperature (25°C). That is, when storing the conductive paste, it is preferable that the binder resin and the organic solvent are a mixture of homogeneous phases, with no residual binder resin being visually confirmed. From the viewpoint of improving solubility in the organic solvent at room temperature, the binder resin is preferably liquid at room temperature.

[0036] The conductive paste disclosed herein contains a phenolic resin (B1) as a binder resin. The inclusion of the phenolic resin can improve the conductivity of the conductive film. Although not particularly limited, it is considered that the inclusion of the phenolic resin suppresses surface oxidation of the conductive particles in the conductive paste or conductive film. As the phenolic resin (B1), any phenolic resin used in this type of conductive paste can be used without any particular limitation. The weight average molecular weight of the phenolic resin (B1) is preferably 300 or more, 500 or more, 1000 or more, or 2000 or more from the viewpoint of the denseness of the conductive film, and is preferably 30000 or less, 20000 or less, 10000 or less, or 5000 or less from the viewpoint of solubility in organic solvents. The weight average molecular weight can be calculated by converting the value measured by gel permeation chromatography (GPC) into styrene. Alternatively, the nominal value of the manufacturer or the like may be referred to.

[0037] From the viewpoint of improving the density of the conductive film and the adhesion to the substrate, and from the viewpoint of suppressing the shrinkage of the conductive film due to thermal curing, it is preferable to use a resol type phenolic resin (resole type phenolic resin) as the phenolic resin (B1). In addition, the phenolic resin (B1) may contain a compound having a phenolic hydroxyl group in the repeating unit. Examples of the phenolic resin containing the compound having the phenolic hydroxyl group include alkylphenol resins and rosin-modified phenolic resins. Alternatively, a phenol-modified xylene resin can be used as the phenolic resin (B1).

[0038] As described above, the conductive paste disclosed herein must contain a phenol resin (B1). However, the conductive paste disclosed herein may contain other binder resins (B2) as long as the effects of the present invention can be achieved. The other binder resins (B2) may be one or more of epoxy resins, urea resins, melamine resins, alkyd resins, unsaturated polyester resins, silicone resins, polyurethane resins, and the like.

[0039] From the viewpoint of improving the conductivity of the conductive film, when the total amount of the binder resin (B) contained in the conductive paste is taken as 100% by weight, the content of the phenol resin (B1) is preferably 70% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more. The closer to the upper limit of 100% by weight, the better, and it can be 95% by weight or more, or 98% by weight or more. When the conductive paste contains another binder resin (B2), the content of the other binder resin (B2) is preferably 30% by weight or less, more preferably 20% by weight or less, and even more preferably 10% by weight or less (for example, 5% by weight or less, or 2% by weight or less) of the total amount of the binder resin (B).

[0040] The content of the binder resin is not particularly limited, but from the viewpoint of buffering external vibration and thermal shock to the conductive film, it is preferably 3% by weight or more of the entire conductive paste, more preferably 5% by weight or more, and even more preferably 7% by weight or more. On the other hand, from the viewpoint of preventing an increase in resistance due to the binder resin present between the conductive powders, the content is preferably 30% by weight or less, preferably 25% by weight or less, and more preferably 20% by weight or less.

[0041] In this type of conductive paste, the conductive particles have been conventionally surface-treated using various surface treatment agents. By carrying out such surface treatment, as described above, a coating containing the surface treatment agent can be formed on at least a part of the surface of the conductive particles. This makes it possible to suppress the formation of an oxide film on the surface of the conductive particles. However, the above-mentioned surface treatment alone may not be sufficient to reduce the once oxidized portion and improve the conductivity of the conductive film. As a result of intensive research by the present inventors, it has been found that the conductivity of the conductive film can be significantly improved by adding a specific type of compound to the conductive paste as an oxidation inhibitor.

[0042] (C) Oxidation inhibitor As described above, the conductive paste disclosed herein contains an oxidation inhibitor. The oxidation inhibitor is a component that has a function of suppressing surface oxidation of conductive particles in the conductive paste, and suitable examples include formic acid, acetic acid, and propionic acid. The oxidation inhibitor may be composed of one of these carboxylic acids, or two or more of them may be blended. When the oxidation inhibitor is composed of a mixture of two or more kinds, the mixing ratio can be appropriately set as necessary.

[0043] The content of the oxidation inhibitor (C) can be, for example, 3% by weight or less, 2% by weight or less, or 1% by weight or less of the entire conductive paste. From the viewpoint of better realizing the effect of improving the conductivity of the conductive film, it is preferably 0.15% by weight or more, may be 0.2% by weight or more, may be 0.4% by weight or more, may be 0.6% by weight or more, can be 0.8% by weight or less, can be 0.6% by weight or less, or can be 0.4% by weight or less.

[0044] (D) Organic solvent The organic solvent is a component that disperses or dissolves the above components (A) to (C) and adjusts the viscosity and thixotropy of the conductive paste, thereby improving the coatability and handleability. The type of organic solvent is not particularly limited, and any conventionally known organic solvent used to prepare this type of conductive paste can be appropriately selected. For example, from the viewpoint of improving the dispersibility of the conductive particles, it is preferable to use an organic solvent that can dissolve the binder resin (B) (especially the phenolic resin (B1)). It is also preferable to use an organic solvent that is easily removed by heat treatment (100°C to 300°C) in the process of preparing the conductive film.

[0045] Examples of organic solvents include, but are not limited to, glycol ether-based solvents such as ethylene glycol monomethyl ether (methyl cellosolve), ethylene glycol monoethyl ether (cellosolve), diethylene glycol monoethyl ether (ethyl carbitol), diethylene glycol monobutyl ether (butyl carbitol), dipropylene glycol methyl ether, and propylene glycol phenyl ether; glycol-based solvents such as ethylene glycol, propylene glycol, and diethylene glycol; ethylene glycol monoethyl ether acetate (cellosolve acetate), diethylene glycol methyl ether acetate, and diethylene glycol phenyl ether; Examples of the solvent include acetate-based solvents such as ethylene glycol monobutyl ether acetate, dipropylene glycol methyl ether acetate, cyclohexyl acetate, propylene glycol 1-monomethyl ether 2-acetate, 3-methoxybutyl acetate, and ethylene glycol monobutyl ether acetate; ketone-based solvents such as isophorone, cyclohexanone, and diacetone alcohol; alcohol-based solvents such as terpineol, dihydroterpineol, dihydroterpineyl propionate, benzyl alcohol, 1-phenoxy-2-propanol, and 3-methyl-3-methoxybutanol; and ester-based solvents. Among these, glycol ether-based solvents such as diethylene glycol monoethyl ether are preferred.

[0046] The content of the organic solvent (D) is not particularly limited, but may be the remainder obtained by subtracting the conductive powder (A), the binder resin (B), and the oxidation inhibitor (C) from the entire conductive paste. That is, the content is, for example, 30% by weight or less of the entire conductive paste, and from the viewpoint of easy removal by heat treatment during production, it is preferable to set it to 20% by weight or less, and it can be set to 15% by weight or less. From the viewpoint of imparting appropriate fluidity to the conductive paste, the content is preferable to set it to 5% by weight or more, and it can be set to 7% by weight or more, or 9% by weight or more.

[0047] (E) Optional Added Ingredients The conductive paste disclosed herein may be composed of only the above components (A) to (D), or may contain various additive components as necessary in addition to the above components (A) to (D) as long as the effects of the present invention can be realized. As the optional additive components, one or more of those known to be usable in general conductive pastes can be appropriately used. As the optional additive components, curing agents, surfactants, leveling agents, thickeners, wetting agents, dispersants, defoamers, antistatic agents, antigelling agents, plasticizers, stabilizers, antioxidants (excluding the above oxidation inhibitor (C)), preservatives, colorants (pigments, dyes), fillers (inorganic fillers, organic fillers), etc. are exemplified. The curing agent is a component that can react with the binder resin (B) to form a crosslinked structure. As the antioxidant, various carboxylic acids used in the following examples can be used in addition to conventionally known antioxidants.

[0048] When the conductive paste disclosed herein contains an optional additive component (E), the content is, for example, 5% by weight or less of the entire conductive paste, preferably 3% by weight or less, and can be 1% by weight or less, although this is not particularly limited.

[0049] The conductive paste disclosed herein can be prepared by weighing out the various materials described above to a predetermined content ratio and mixing them homogeneously. The materials can be mixed by any of various known mixing and stirring devices, such as a roll mill, a magnetic stirrer, a planetary mixer, a disperser, etc.

[0050] <Applications of conductive paste> The conductive paste disclosed herein can form a conductive film with excellent conductivity on any substrate. Therefore, the conductive paste is preferably used, for example, to form a wiring pattern or a conductive circuit on a substrate. It can also be used to bond electronic components or mount electronic components on a substrate.

[0051] <Substrate with conductive film> 1 is a schematic cross-sectional view of a substrate 10 with a conductive film. The substrate 10 with a conductive film includes a substrate 12 and a conductive film 14 formed on the substrate 12. The substrate 10 with a conductive film is, for example, a wiring substrate. The substrate 12 can be, for example, various ceramic substrates, resin substrates (polyimide substrates, polyester substrates such as polyethylene terephthalate, epoxy resin substrates, etc.), glass substrates, etc. A base layer (coat layer) such as a conductive layer, an insulating protective layer, an anti-reflection layer, an optical adjustment layer, or a moisture-proof layer may be formed on a part or all of the surface of the substrate 12.

[0052] The conductive film 14 is composed of an unbaked resin cured product formed by thermal curing of the phenolic resin (B1). The conductive film 14 is formed in a predetermined pattern. In FIG. 1, a plurality of independent conductive films 14 are formed at a predetermined interval on one surface of the substrate 12. The conductive film 14 may be provided on only one side of the substrate 12 as shown in FIG. 1, or may be provided on both sides of the substrate 12. The conductive film 14 may be provided on only a part of the substrate 12, or may be provided over the entire surface of the substrate 12. The conductive film 14 has a reduced volume resistivity and achieves good conductivity. For example, as shown in the following examples, the volume resistivity after drying at 150° C. for 30 minutes can be, for example, 500 μΩ·cm or less, preferably 200 μΩ·cm or less, more preferably 150 μΩ·cm or less, and even more preferably 100 μΩ·cm or less, and 75 μΩ·cm or less.

[0053] The conductive film-coated substrate 10 can be suitably used as a flexible device mounted on portable electronic devices such as mobile phones, smartphones, tablet computers, notebook computers, electronic paper, digital video cameras, etc., such as electronic components of touch panels, liquid crystal displays, organic EL displays, etc. Here, "portable" means having a level of portability that allows an individual (typically an adult) to easily carry it around.

[0054] <Method of manufacturing conductive film> A method for producing a conductive film using the conductive paste disclosed herein (i.e., a method for producing a substrate with a conductive film) includes preparing a substrate and the conductive paste; applying the conductive paste to the substrate to form a coating film made of the conductive paste; and heating the substrate and the coating film to harden the phenolic resin contained in the coating film.

[0055] The method of applying the conductive paste to the substrate (i.e., the method of forming the coating film on the substrate) can be carried out using, for example, screen printing, gravure printing, a bar coater, a doctor blade, a slit coater, a gravure coater, a dip coater, a spray coater, a dispenser, etc. In this case, the thickness of the coating film can be (for example, 0.01 to 10 mm, 0.1 to 1 μm).

[0056] Next, the coating film is heated. The heating temperature is preferably set to a temperature at which the phenolic resin contained in the coating film hardens and at which the organic solvent can be removed without damaging the substrate. The heating temperature is, for example, 300°C or less, preferably set to 250°C or less, more preferably 200°C or less, or can be set to 175°C or less or 150°C or less. The heating time is not particularly limited, but can be about 15 minutes to several hours. As a result, a conductive film is formed on the substrate. The surroundings when the conductive film is formed may be air or an atmosphere with little oxygen, such as a nitrogen atmosphere. From the viewpoint of simplifying the equipment during heat treatment or making it inexpensive, it is preferable to form the conductive film in air. EXAMPLES

[0057] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in the following examples. In the following examples, "%" is by weight unless otherwise specified.

[0058] <1. Thermosetting resin> [Conductive paste] <Example 1> A conductive paste according to Example 1 was prepared by mixing Cu powder A as a conductive powder, a phenolic resin (Resitop PL-5208 (Gun-ei Chemical Industry)) as a binder resin, formic acid as an oxidation inhibitor, and diethylene glycol monoethyl ether as an organic solvent. Here, assuming that the entire conductive paste is 100%, the content of the conductive powder was 80%, the content of the binder resin was 9%, the content of the formic acid was 0.5%, and the content of the organic solvent was 10.5%. As the Cu powder A, Cu particles produced by an atomization method were formed into flakes. The aspect ratio of the flake particles constituting the Cu powder A was 1.8, and the average particle diameter was 3 μm. In addition, stearic acid was attached to the surfaces of the flake copper particles as a surface treatment agent. <Example 2> A conductive paste according to Example 2 was prepared in the same manner as in Example 1, except that Cu powder B was used as the conductive powder. Cu powder B was a wet spherical powder with an aspect ratio of 1.2 and an average particle size of 4 μm. Oleic acid was attached to the surfaces of the copper particles constituting Cu powder B as a surface treatment agent. <Example 3> A conductive paste according to Example 3 was prepared in the same manner as in Example 1, except that no formic acid was added. <Example 4> The conductive paste of Example 4 was prepared in the same manner as in Example 2, except that no formic acid was added. <Example 5> A conductive paste according to Example 5 was prepared in the same manner as in Example 1, except that Cu powder C was used as the conductive powder. Cu powder C was mainly composed of spherical copper particles prepared by an atomization method, and had an aspect ratio of 1.3 and an average particle diameter of 2 μm. No surface treatment agent was attached to the surfaces of the copper particles constituting Cu powder C. <Example 6> A conductive paste according to Example 6 was prepared in the same manner as in Example 1, except that an epoxy resin (JER1007 (Mitsubishi Chemical)) was used as the binder resin.

[0059] [Conductive film] The conductive pastes according to Examples 1 to 6 were applied (coated) to the surface of a glass substrate in a square pattern of 2 cm x 2 cm with a thickness of about 20 μm by a screen printing method to obtain a coating film made of the conductive paste.The substrate and the coating film were then heated at 150°C for 30 minutes to harden the resin, thereby forming a conductive film according to each example on the substrate.

[0060] [Resistivity (volume resistivity)] The surface resistivity of the conductive film formed as described above was measured by the four-probe method using a resistivity meter (model: Loresta GP MCP-T610) manufactured by Mitsubishi Chemical Analytech Co., Ltd. The thickness of the conductive film was also measured using a surface roughness meter (Surfcom manufactured by Tokyo Seimitsu Co., Ltd.). The resistivity (volume resistivity) (μΩ·cm) was calculated by multiplying the surface resistivity by the film thickness. The results are shown in the "Resistivity" column of Table 1. Note that for Examples 5 and 6, the resistivity of the conductive film exceeded the measurement tolerance of the resistivity meter, and the resistivity could not be measured (overflow level). The corresponding column in Table 1 is marked "OL."

[0061] [Table 1]

[0062] As shown in Table 1, when Examples 1 and 2 are compared with Examples 3 and 4, it is confirmed that the inclusion of an oxidation inhibitor (formic acid) significantly reduces the resistivity of the conductive film. Also, when Examples 1 and 6 are compared, it is confirmed that the inclusion of a phenolic resin as the binder resin significantly reduces the resistivity of the conductive film. Furthermore, when Examples 1 to 4 are compared with Example 5, it is confirmed that the inclusion of copper particles having a surface treatment agent attached thereto as the conductive powder significantly reduces the resistivity of the conductive film.

[0063] <2. Examination of the content of oxidation inhibitor> [Conductive paste] <Examples 7-12> Conductive pastes according to Examples 7 to 12 were prepared in the same manner as in Example 2, except that the content of formic acid was set to the content shown in the corresponding column in Table 2. Although not shown in the table, the content of the organic solvent (diethylene glycol monoethyl ether) was set so that the entire conductive paste was 100%.

[0064] [Conductive film] Using the conductive pastes of Examples 7 to 12, conductive films of the respective examples were formed using the same materials and procedures as in Test Example 1 above.

[0065] [Resistivity (volume resistivity)] The resistivity (volume resistivity) (μΩ·cm) of the conductive film formed as described above was calculated using the same materials and procedures as in Test Example 1 above. The results are shown in the "Resistivity" column in Table 2. Note that Table 2 also lists the data for Examples 2 and 4 for reference in comparing the measurement results.

[0066] [Table 2]

[0067] As shown in Table 2, it was confirmed that the resistivity of the conductive film is significantly reduced by setting the content of formic acid in the conductive paste to 0.05% or more. It was also found that a more effective resistivity reduction effect can be obtained when the content of formic acid in the conductive paste is 0.175% or more and 0.75% or less.

[0068] <3. Examination of types of oxidation inhibitors> [Conductive paste] <Examples 13-18> As the oxidation inhibitor to be contained in the conductive paste, acetic acid, propionic acid, stearic acid, lauric acid, malonic acid, and citric acid were prepared. The conductive pastes according to Examples 13 to 18 were produced in the same manner as in Example 2, except that the type of oxidation inhibitor was as shown in the corresponding column in Table 3.

[0069] [Conductive film] Using the conductive pastes of Examples 13 to 18, conductive films of the respective examples were formed using the same materials and procedures as in Test Example 1 above.

[0070] [Resistivity (volume resistivity)] The resistivity (volume resistivity) (μΩ·cm) of the conductive film formed as described above was calculated using the same materials and procedures as in Test Example 1 above. The results are shown in the "Resistivity" column in Table 3. Note that Table 3 also lists the data from Examples 2 and 4 for reference in comparing the measurement results.

[0071] [Table 3]

[0072] As shown in Table 3, it was confirmed that the resistivity of the conductive film was reduced by adding various oxidation inhibitors to the conductive paste in Examples 13 to 18. It was also found that a more effective resistivity reduction effect could be obtained by adding at least one of formic acid, acetic acid, and propionic acid to the conductive paste.

[0073] <4. Consideration of the type of conductive powder> [Conductive paste] <Example 19> A conductive paste according to Example 19 was prepared in the same manner as in Example 1, except that Ag powder was used as the conductive powder. The Ag powder had an aspect ratio of 1.1 and an average particle size of 2 μm. Stearic acid was attached to the surfaces of the silver particles constituting the Ag powder as a surface treatment agent. <Example 20> A conductive paste according to Example 20 was prepared in the same manner as in Example 3, except that the Ag powder used in Example 19 was used as the conductive powder.

[0074] [Conductive film] Using the conductive pastes of Examples 19 and 20, conductive films of the respective examples were formed using the same materials and procedures as in Test Example 1 above.

[0075] [Resistivity (volume resistivity)] The resistivity (volume resistivity) (μΩ·cm) of the conductive film formed as described above was calculated using the same materials and procedures as in Test Example 1. The results are shown in the "Resistivity" column of Table 4.

[0076] [Table 4]

[0077] As shown in Table 4, from the results of Examples 19 and 20, it was confirmed that the effect of the present invention (resistivity reduction effect) could be obtained even when Ag powder was used as the conductive powder.

[0078] From the above, it was found that the resistivity of the conductive film can be reduced by using a conductive paste containing a conductive powder, a binder resin, an organic solvent, and an oxidation inhibitor, in which the conductive powder contains conductive particles having a surface treatment agent adhered to the surface, the binder resin contains a phenolic resin, and the oxidation inhibitor is mainly composed of one or more carboxylic acids selected from the group consisting of formic acid, acetic acid, and propionic acid, and the oxidation inhibitor accounts for at least 0.05% of the total.

[0079] Although the present invention has been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes to the specific examples exemplified above. [Explanation of symbols]

[0080] 10. Substrate with conductive film 12 Substrate 14 Conductive film

Claims

1. A conductive powder; A binder resin; An oxidation inhibitor; An organic solvent; A conductive paste comprising: the conductive powder is mainly composed of conductive particles, which are particles made of simple silver, particles made of an alloy containing silver, particles made of simple copper, or particles made of an alloy containing copper, and a surface treatment agent is attached to the surfaces of the conductive particles; the binder resin is made of a resol type phenolic resin, the oxidation inhibitor is mainly composed of one or more carboxylic acids selected from the group consisting of formic acid, acetic acid, and propionic acid; The oxidation inhibitor is contained in an amount of 0.05% by weight or more and 1% by weight or less of the total weight of the conductive paste.

2. The conductive paste according to claim 1 , wherein the surface treatment agent is composed of at least one compound selected from the group consisting of carboxylic acids, amines, and benzotriazoles.

3. 3. The conductive paste according to claim 1, wherein the conductive powder is mainly composed of conductive particles having an aspect ratio of 1.5 or less.

4. The conductive paste according to any one of claims 1 to 3, which is used for forming a wiring pattern on a substrate.

5. A method for producing a conductive film, comprising the steps of: Providing a substrate and a conductive paste according to any one of claims 1 to 4; applying the conductive paste to the substrate to form a coating film made of the conductive paste; and heating the substrate and the coating film to cure the phenolic resin contained in the coating film; The manufacturing method includes the steps of:

Citation Information

Patent Citations

  • Thickening agent for discharge excrement in container

    JP1979039995A

  • Water heater

    JP1983080441A

  • Noise eliminating device of television signal

    JP1985089175A

  • Copper powder for conductive paste, and conductive paste thereof

    JP1992264302A

  • Conductive paste and its manufacture

    JP2000322933A