Light-transmitting conductive film and transparent conductive film

An amorphous light-transmitting conductive film with krypton and specific resistance of 4×10^-4 Ω·cm or more is developed to address low resistance and warpage issues, enabling low-resistance crystalline films for transparent electrodes in devices.

JP7565936B2Active Publication Date: 2024-10-11NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021550146
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-02
Filing Date
2021-03-18
Publication Date
2024-10-11
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Existing light-transmitting conductive films face challenges in achieving low resistance and are prone to warpage, which is critical for applications in transparent electrodes.

Method used

An amorphous light-transmitting conductive film containing krypton and a specific resistance of 4×10^-4 Ω·cm or more, with a thickness exceeding 40 nm, is developed, which can be converted into a low-resistance crystalline film with suppressed warpage through heat treatment.

Benefits of technology

The film achieves low resistance and reduced warpage, making it suitable for transparent conductive films in devices like touch sensors and image displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565936000002
    Figure 0007565936000002
  • Figure 0007565936000003
    Figure 0007565936000003
  • Figure 0007565936000004
    Figure 0007565936000004
Patent Text Reader

Abstract

A light-transmitting conductive film (20) according to the present invention is amorphous, includes a conductive oxide layer containing krypton, and has a specific resistance of at least 4×10-4 Ω•cm. A transparent conductive film (X) according to the present invention includes: a transparent base material (10); and a light-transmitting conductive film (20) positioned on one surface side of the transparent base material (10) in the thickness direction (D).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a light-transmitting conductive film and a transparent conductive film. [Background technology]

[0002] Transparent electrodes in various devices such as liquid crystal displays, touch panels, and optical sensors are formed from a film (light-transmitting conductive film) that has both light transparency and electrical conductivity. The light-transmitting conductive film may also be used as an antistatic layer provided in a device. The light-transmitting conductive film is formed, for example, by forming a film of a conductive oxide on a transparent substrate by a sputtering method. In the sputtering method, an inert gas such as argon is used as a sputtering gas for colliding with a target (film-forming material supply material) and displacing atoms on the target surface. Technology related to such light-transmitting conductive films is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-334924 Summary of the Invention [Problem to be solved by the invention]

[0004] Light-transmitting conductive films are required to have low resistance. This requirement is particularly strong for light-transmitting conductive films used as transparent electrodes. Light-transmitting conductive films are also required to have low internal stress and to be less prone to warping.

[0005] The present invention provides an amorphous light-transmitting conductive film suitable for obtaining a crystalline light-transmitting conductive film having low resistance and suppressed warping, and a transparent conductive film including the light-transmitting conductive film. [Means for solving the problem]

[0006] The present invention [1] is an amorphous light-transmitting conductive film that contains a conductive oxide containing krypton and has a 4×10 -4 It includes a light-transmitting conductive film having a resistivity of Ω·cm or more.

[0007] In the present invention [2], the resistivity is 20×10 -4 The optically transparent conductive film according to the above item [1] has a resistivity of Ω·cm or less.

[0008] The present invention [3] includes the light-transmitting conductive film according to the above [1] or [2], which has a thickness of more than 40 nm.

[0009] The present invention [4] includes the light-transmitting conductive film according to any one of the above [1] to [3], which is patterned.

[0010] The present invention [5] has a resistivity of 3×10 after heat treatment at 165°C for 1 hour. -4 The optically transparent conductive film according to any one of [1] to [4] above has a resistivity of less than Ω·cm.

[0011] The present invention [6] includes a transparent conductive film comprising a transparent substrate and the light-transmitting conductive film according to any one of [1] to [5] above, which is arranged on one side in a thickness direction of the transparent substrate. Effect of the Invention

[0012] The light-transmitting conductive film of the present invention is amorphous, contains a conductive oxide containing krypton, and has a molecular weight of 4×10 -4 Since the transparent conductive film of the present invention has a resistivity of Ω·cm or more, it is suitable for obtaining a low-resistance crystalline light-transmitting conductive film with suppressed warping. Since the transparent conductive film of the present invention has such a light-transmitting conductive film, it is suitable for obtaining a transparent conductive film with a low-resistance crystalline light-transmitting conductive film and suppressed warping. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of a transparent conductive film of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a modified example of the transparent conductive film of the present invention. [Diagram 3] 3 shows a method for manufacturing the transparent conductive film shown in Fig. 1. Fig. 3A shows a step of preparing a transparent resin film, Fig. 3B shows a step of forming a functional layer on the transparent resin film, and Fig. 3C shows a step of forming a light-transmitting conductive film on the functional layer. [Figure 4] This shows a case where the light-transmitting conductive film in the transparent conductive film shown in FIG. 1 is patterned. [Diagram 5] This represents a case where the amorphous light-transmitting conductive film in the transparent conductive film shown in FIG. 1 is converted into a crystalline light-transmitting conductive film. [Figure 6] 1 is a graph showing the relationship between the amount of oxygen introduced when forming a light-transmitting conductive film by a sputtering method and the resistivity of the formed light-transmitting conductive film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] 1 is a schematic cross-sectional view of a transparent conductive film X, which is one embodiment of the transparent conductive film of the present invention. The transparent conductive film X includes a transparent substrate 10 and a light-transmitting conductive film 20, in this order, toward one side in a thickness direction D. The transparent conductive film X, the transparent substrate 10, and the light-transmitting conductive film 20 each have a shape that spreads in a direction (plane direction) perpendicular to the thickness direction D. The transparent conductive film X and the light-transmitting conductive film 20 included therein are elements included in touch sensors, light control elements, photoelectric conversion elements, heat ray control members, antenna members, electromagnetic wave shielding members, heater members, image display devices, and the like.

[0015] The transparent substrate 10 includes a transparent resin film 11 and a functional layer 12 in this order toward one side in the thickness direction D.

[0016] The transparent resin film 11 is a transparent resin film having flexibility. Examples of the material of the transparent resin film 11 include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyolefin resin include polyethylene, polypropylene, and cycloolefin polymer. Examples of the acrylic resin include polymethacrylate. As the material of the transparent resin film 11, for example, from the viewpoint of transparency and strength, polyester resin is preferably used, and more preferably PET is used.

[0017] The surface of the transparent resin film 11 facing the functional layer 12 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0018] The thickness of the transparent resin film 11 is preferably 1 μm or more, more preferably 10 μm or more, and even more preferably 30 μm or more. The thickness of the transparent resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 75 μm or less. These configurations regarding the thickness of the transparent resin film 11 are suitable for ensuring the handleability of the transparent conductive film X.

[0019] The total light transmittance (JIS K 7375-2008) of the transparent resin film 11 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, an image display device, and the like. The total light transmittance of the transparent resin film 11 is, for example, 100% or less.

[0020] In this embodiment, the functional layer 12 is located on one surface of the transparent resin film 11 in the thickness direction D. In this embodiment, the functional layer 12 is a hard coat layer that makes it difficult for scratches to form on the exposed surface (the upper surface in FIG. 1 ) of the light-transmitting conductive film 20.

[0021] The hard coat layer is a cured product of a curable resin composition. Examples of the resin contained in the curable resin composition include polyester resin, acrylic resin, urethane resin, amide resin, silicone resin, epoxy resin, and melamine resin. Examples of the curable resin composition include an ultraviolet-curable resin composition and a thermosetting resin composition. Since the curable resin composition can be cured without high-temperature heating, and therefore is useful for improving the production efficiency of the transparent conductive film X, an ultraviolet-curable resin composition is preferably used as the curable resin composition. Specific examples of the ultraviolet-curable resin composition include the hard coat layer-forming composition described in JP 2016-179686 A.

[0022] The surface of the functional layer 12 facing the light-transmitting conductive film 20 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0023] The thickness of the functional layer 12 as a hard coat layer is preferably 0.1 μm or more, more preferably 0.5 μm or more. Such a configuration is suitable for achieving sufficient scratch resistance in the light-transmitting conductive film 20. From the viewpoint of ensuring the transparency of the functional layer 12, the thickness of the functional layer 12 as a hard coat layer is preferably 10 μm or less, more preferably 5 μm or less.

[0024] The thickness of the transparent substrate 10 is preferably 1 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and particularly preferably 30 μm or more. The thickness of the transparent substrate 10 is preferably 310 μm or less, more preferably 210 μm or less, even more preferably 110 μm or less, and particularly preferably 80 μm or less. These configurations regarding the thickness of the transparent substrate 10 are suitable for ensuring the handleability of the transparent conductive film X.

[0025] The total light transmittance (JIS K 7375-2008) of the transparent substrate 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, an image display device, and the like. The total light transmittance of the transparent substrate 10 is, for example, 100% or less.

[0026] The thermal shrinkage of the transparent substrate 10 in the direction in which it shrinks most when it is subjected to a heat treatment is, for example, 1% or less, preferably 0.6% or less, and more preferably 0.5% or less, from the viewpoint of suppressing warping of the light-transmitting conductive film 20. The thermal shrinkage is, for example, 0.0% or more. The thermal shrinkage can be obtained by measuring the dimensional change of the transparent substrate 10 after the transparent substrate 10 is subjected to a heat treatment and then left to stand at room temperature for 30 minutes. The heating temperature in the heat treatment is the same as the temperature at which the light-transmitting conductive film 20 is crystallized, for example, 165°C. The heating time in the heat treatment is, for example, 1 hour.

[0027] In this embodiment, the light-transmitting conductive film 20 is located on one surface of the transparent substrate 10 in the thickness direction D. The light-transmitting conductive film 20 is one embodiment of the light-transmitting conductive film of the present invention, and is an amorphous film that has both light transparency and conductivity. The amorphous light-transmitting conductive film 20 is converted into a crystalline light-transmitting conductive film (light-transmitting conductive film 20' described below) by heating, and the specific resistance decreases.

[0028] The light-transmitting conductive film 20 includes a conductive oxide containing at least krypton (Kr) as a rare gas atom, and is preferably made of a conductive oxide containing at least Kr as a rare gas atom. In this embodiment, the rare gas atoms in the light-transmitting conductive film 20 are derived from rare gas atoms used as a sputtering gas in a sputtering method described below for forming the light-transmitting conductive film 20. In this embodiment, the light-transmitting conductive film 20 is a film formed by a sputtering method (sputtered film).

[0029] Examples of the conductive oxide include metal oxides containing at least one metal or metalloid selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W. Specifically, examples of the conductive oxide include indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), indium gallium zinc composite oxide (IGZO), and antimony tin composite oxide (ATO). From the viewpoint of realizing high transparency and good electrical conductivity, the conductive oxide is preferably indium tin composite oxide (ITO) containing both In and Sn. This ITO may contain a metal or metalloid other than In and Sn in an amount less than the respective contents of In and Sn.

[0030] When ITO is used as the conductive oxide, the ratio of the content of tin oxide to the total content of indium oxide (In2O3) and tin oxide (SnO2) in the ITO is preferably 0.1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and particularly preferably 7 mass% or more. The ratio of the number of tin atoms to the number of indium atoms in the ITO used (number of tin atoms / number of indium atoms) is preferably 0.001 or more, more preferably 0.03 or more, even more preferably 0.05 or more, and particularly preferably 0.07 or more. These configurations are suitable for ensuring the durability of the light-transmitting conductive film 20. In addition, the ratio of the content of tin oxide to the total content of indium oxide (In2O3) and tin oxide (SnO2) in the ITO used is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less. The ratio of the number of tin atoms to the number of indium atoms in the ITO used (number of tin atoms / number of indium atoms) is preferably 0.16 or less, more preferably 0.14 or less, and even more preferably 0.13 or less. These configurations are suitable for obtaining a light-transmitting conductive film 20 that is easily crystallized by heating. The ratio of the number of tin atoms to the number of indium atoms in the ITO is determined, for example, by specifying the abundance ratio of indium atoms and tin atoms for the measurement object by X-ray photoelectron spectroscopy. The above-mentioned content ratio of tin oxide in the ITO is determined, for example, from the abundance ratio of indium atoms and tin atoms thus specified. The above-mentioned content ratio of tin oxide in the ITO may be determined from the content ratio of tin oxide (SnO2) in the ITO target used during sputtering film formation.

[0031] The light-transmitting conductive film 20 includes a region in at least a part of the thickness direction D in which the Kr content is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, even more preferably 0.5 atomic % or less, particularly preferably 0.3 atomic % or less, very preferably 0.2 atomic % or less, and particularly preferably less than 0.1 atomic %. The Kr content of the region is, for example, 0.0001 atomic % or more. Preferably, the light-transmitting conductive film 20 satisfies such a Kr content in the entire region in the thickness direction D. Specifically, the Kr content in the light-transmitting conductive film 20 is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, even more preferably 0.5 atomic % or less, particularly preferably 0.3 atomic % or less, very preferably 0.2 atomic % or less, and particularly preferably less than 0.1 atomic % in the entire region in the thickness direction D. These configurations are suitable for achieving good crystal growth and forming large crystal grains when the light-transmitting conductive film 20 is heated for crystallization, and are therefore suitable for obtaining a light-transmitting conductive film 20' with low resistance (the larger the crystal grains in the crystalline light-transmitting conductive film 20', the lower the resistance of the light-transmitting conductive film 20').

[0032] The presence or absence and content of rare gas atoms such as Kr in the light-transmitting conductive film 20 is identified, for example, by Rutherford backscattering spectrometry, which will be described later in the examples. The presence or absence of rare gas atoms such as Kr in the light-transmitting conductive film 20 is identified, for example, by X-ray fluorescence analysis, which will be described later in the examples. In the light-transmitting conductive film to be analyzed, when the content of rare gas atoms is not quantifiable because it is not equal to or greater than the detection limit (lower limit) according to Rutherford backscattering analysis, and the presence of rare gas atoms is identified according to X-ray fluorescence analysis, the light-transmitting conductive film is determined to include a region in which the content of rare gas atoms such as Kr is 0.0001 atomic % or more.

[0033] The light-transmitting conductive film 20 may contain rare gas atoms other than Kr. Examples of rare gas atoms other than Kr include argon (Ar), xenon (Xe), and radon (Rn). From the viewpoint of reducing the manufacturing costs of the light-transmitting conductive film 20 and the transparent conductive film X, Ar is preferably used.

[0034] When the light-transmitting conductive film 20 contains rare gas atoms other than Kr in addition to Kr, the content ratio of rare gas atoms in the light-transmitting conductive film 20 (for example, the total content ratio of Kr and Ar) is preferably 1.2 atomic % or less, more preferably 1.1 atomic % or less, even more preferably 1.0 atomic % or less, even more preferably 0.8 atomic % or less, even more preferably 0.5 atomic % or less, especially preferably 0.4 atomic % or less, very preferably 0.3 atomic % or less, and particularly preferably 0.2 atomic % or less in the entire region in the thickness direction D. Such a configuration is suitable for reducing impurity scattering of carriers because the content of rare gas atoms (impurity atoms) in the light-transmitting conductive film 20 is small, and therefore is suitable for obtaining a light-transmitting conductive film 20' with low resistance.

[0035] The light-transmitting conductive film 20 may contain Kr throughout the entire region in the thickness direction D. The light-transmitting conductive film 20 may contain only Kr as rare gas atoms throughout the entire region in the thickness direction D, or may contain rare gas atoms other than Kr in addition to Kr.

[0036] As illustrated in FIG. 2, the light-transmitting conductive film 20 may contain Kr in a part of the region in the thickness direction D. FIG. 2A shows a case where the light-transmitting conductive film 20 includes a first region 21 and a second region 22 in this order toward one side of the thickness direction D. The first region 21 contains Kr, and the second region 22 does not contain Kr. FIG. 2B shows a case where the light-transmitting conductive film 20 includes a second region 22 and a first region 21 in this order toward one side of the thickness direction D. FIG. 2C shows a case where the light-transmitting conductive film 20 includes a first region 21, a second region 22, and a first region 21 in this order toward one side of the thickness direction D. FIG. 2D shows a case where the light-transmitting conductive film 20 includes a second region 22, a first region 21, and a second region 22 in this order toward one side of the thickness direction D. In Figure 2, the boundary between the first region 21 and the second region 22 is depicted by a virtual line, but in cases where the first region 21 and the second region 22 do not differ significantly in composition other than that of rare gas atoms, which are contained in trace amounts, the boundary between the first region 21 and the second region 22 may not be clearly distinguishable.

[0037] When the light-transmitting conductive film 20 includes the first region 21 and the second region 22, the ratio of the thickness of the first region 21 (the total thickness of the first regions 21 in the case of a plurality of first regions 21) to the total thickness of the first region 21 and the second region 22 is preferably 1% or more, more preferably 20% or more, even more preferably more than 50%, particularly preferably 60% or more, and particularly preferably 64% or more. The ratio is less than 100%. Moreover, the ratio of the thickness of the second region 22 (the total thickness of the second regions 22 in the case of a plurality of second regions 22) to the total thickness of the first region 21 and the second region 22 is preferably 99% or less, more preferably 80% or less, even more preferably less than 50%, particularly preferably 40% or less, and particularly preferably 36% or less. The configuration regarding the ratio of the thickness of each of the first region 21 and the second region 22 is suitable for forming a low-resistance light-transmitting conductive film 20' from the light-transmitting conductive film 20.

[0038] The content of Kr in the first region 21 is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, even more preferably 0.5 atomic % or less, even more preferably 0.3 atomic % or less, even more preferably 0.2 atomic %, and particularly preferably less than 0.1 atomic % in the entire region of the thickness direction D of the first region 21. Such a configuration is suitable for realizing good crystal growth and forming large crystal grains when heating for crystallization of the light-transmitting conductive film 20, and is therefore suitable for obtaining a light-transmitting conductive film 20' with low resistance (the larger the crystal grains in the crystalline light-transmitting conductive film 20', the lower the resistance of the light-transmitting conductive film 20'). The content of Kr in the first region 21 is, for example, 0.0001 atomic % or more in the entire region of the thickness direction D of the first region 21.

[0039] The Kr content in the first region 21 may be non-uniform in the thickness direction D of the first region 21. For example, in the thickness direction D of the first region 21, the Kr content may gradually increase or decrease as it moves away from the transparent substrate 10. Alternatively, in the thickness direction D of the first region 21, a partial region in which the Kr content gradually increases as it moves away from the transparent substrate 10 may be located on the transparent substrate 10 side, and a partial region in which the Kr content gradually decreases as it moves away from the transparent substrate 10 may be located on the opposite side to the transparent substrate 10. Alternatively, in the thickness direction D of the first region 21, a partial region in which the Kr content gradually decreases as it moves away from the transparent substrate 10 may be located on the transparent substrate 10 side, and a partial region in which the Kr content gradually increases as it moves away from the transparent substrate 10 may be located on the opposite side to the transparent substrate 10.

[0040] The thickness of the light-transmitting conductive film 20 is, for example, 10 nm or more. The thickness of the light-transmitting conductive film 20 is preferably more than 40 nm, more preferably 70 nm or more, even more preferably 100 nm or more, and particularly preferably 130 nm or more. Such a configuration is suitable for achieving low resistance of the light-transmitting conductive film 20' obtained by crystallizing the light-transmitting conductive film 20. In addition, the thickness of the light-transmitting conductive film 20 is preferably 1000 nm or less, more preferably 250 nm or less, even more preferably 200 nm or less, particularly preferably 160 nm or less, and most preferably less than 150 nm. Such a configuration is suitable for suppressing warpage in the transparent conductive film X including the light-transmitting conductive film 20' obtained by crystallizing the light-transmitting conductive film 20.

[0041] The surface resistance of the light-transmitting conductive film 20 is, for example, 500 Ω / □ or less, preferably 200 Ω / □ or less, more preferably 100 Ω / □ or less, and even more preferably 80 Ω / □ or less. The surface resistance of the light-transmitting conductive film 20 is, for example, 1 Ω / □ or more. The surface resistance can be measured by a four-terminal method in accordance with JIS K7194.

[0042] The specific resistance of the light-transmitting conductive film 20 is 4×10 -4 Ω cm or more, preferably 4.3×10 -4 Ω cm or more, preferably 4.5×10 -4 Ω cm or more, more preferably 4.8×10 -4 Ω cm or more, and more preferably 5×10 -4 Ω cm or more, preferably 5.2×10 -4 The resistivity of the light-transmitting conductive film 20 is preferably 20×10 -4 Ω·cm or less, preferably 12×10 -4 Ω cm or less, more preferably 11×10 -4 Ω cm or less, particularly preferably 10.5×10 -4 Ω·cm or less, most preferably 8.5×10 -4Ω·cm or less. Such a configuration regarding the resistivity is suitable for forming a low-resistance light-transmitting conductive film 20' from the light-transmitting conductive film 20. The resistivity is calculated by multiplying the surface resistance by the thickness. The resistivity can be controlled, for example, by adjusting the Kr content in the light-transmitting conductive film 20 and adjusting various conditions when the light-transmitting conductive film 20 is formed by sputtering. Such conditions include, for example, the temperature of the base (the transparent substrate 10 in this embodiment) on which the light-transmitting conductive film 20 is formed, the amount of oxygen introduced into the film formation chamber, the air pressure in the film formation chamber, and the horizontal magnetic field strength above the target.

[0043] The resistivity of the light-transmitting conductive film 20 after heat treatment at 165° C. for 1 hour is preferably 3×10 -4 Ω cm or less, preferably 2.8×10 -4 Ω cm or less, more preferably 2.5×10 -4 Ω cm or less, more preferably 2×10 -4 Ω cm or less, particularly preferably 1.8×10 -4 The resistivity of the light-transmitting conductive film 20 after heat treatment at 165° C. for 1 hour is preferably 0.1×10 -4 Ω·cm or more, preferably 0.5×10 -4 Ω cm or more, more preferably 1.0×10 -4 This configuration is suitable for ensuring the low resistance required for the light-transmitting conductive film 20' obtained by crystallizing the light-transmitting conductive film 20 when the light-transmitting conductive film 20' is provided in a touch sensor, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, an image display device, and the like.

[0044] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive film 20 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring transparency in the light-transmitting conductive film 20' obtained by crystallizing the light-transmitting conductive film 20. The total light transmittance of the light-transmitting conductive film 20 is, for example, 100% or less.

[0045] For example, whether the light-transmitting conductive film is amorphous can be determined as follows. First, the light-transmitting conductive film (light-transmitting conductive film 20 on transparent substrate 10 in transparent conductive film X) is immersed in hydrochloric acid with a concentration of 5% by mass at 20° C. for 15 minutes. Next, the light-transmitting conductive film is washed with water and then dried. Next, the resistance between a pair of terminals separated by a distance of 15 mm (inter-terminal resistance) is measured on the exposed flat surface of the light-transmitting conductive film (the surface of light-transmitting conductive film 20 opposite to the transparent substrate 10 in transparent conductive film X). If the inter-terminal resistance exceeds 10 kΩ in this measurement, the light-transmitting conductive film is amorphous.

[0046] The transparent conductive film X is produced, for example, as follows.

[0047] First, as shown in FIG. 3A, a transparent resin film 11 is prepared.

[0048] 3B, a functional layer 12 is formed on one surface of the transparent resin film 11 in the thickness direction D. By forming the functional layer 12 on the transparent resin film 11, a transparent substrate 10 is produced.

[0049] The functional layer 12 as a hard coat layer can be formed by applying a curable resin composition to the transparent resin film 11 to form a coating film, and then curing the coating film. When the curable resin composition contains an ultraviolet-curable resin, the coating film is cured by ultraviolet irradiation. When the curable resin composition contains a thermosetting resin, the coating film is cured by heating.

[0050] The exposed surface of the functional layer 12 formed on the transparent resin film 11 is subjected to a surface modification treatment as necessary. When a plasma treatment is used as the surface modification treatment, for example, argon gas is used as an inert gas. The discharge power in the plasma treatment is, for example, 10 W or more and, for example, 5000 W or less.

[0051] 3C, a light-transmitting conductive film 20 is formed on the transparent substrate 10. Specifically, the light-transmitting conductive film 20 is formed by depositing a material on the functional layer 12 of the transparent substrate 10 by a sputtering method.

[0052] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a film formation process by a roll-to-roll method. When using a sputtering deposition apparatus of the roll-to-roll method in the manufacture of the transparent conductive film X, a material is deposited on the long transparent substrate 10 while the transparent substrate 10 is traveling from a pay-out roll to a take-up roll provided in the apparatus, to form the light-transmitting conductive film 20. In addition, in the sputtering method, a sputtering deposition apparatus having one deposition chamber may be used, or a sputtering deposition apparatus having multiple deposition chambers arranged in order along the traveling path of the transparent substrate 10 may be used (when forming the light-transmitting conductive film 20 including the above-mentioned second region 22, a sputtering deposition apparatus having multiple deposition chambers is used).

[0053] Specifically, in the sputtering method, a sputtering gas (inert gas) is introduced under vacuum conditions into a deposition chamber of a sputter deposition apparatus, while a negative voltage is applied to a target placed on a cathode in the deposition chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed to eject target material from the target surface, and the ejected target material is deposited on the functional layer 12 of the transparent substrate 10.

[0054] The material of the target placed on the cathode in the film formation chamber is the conductive oxide described above for forming the light-transmitting conductive film 20, and preferably ITO. The ratio of the tin oxide content to the total content of tin oxide and indium oxide in ITO is preferably 0.1 mass% or more, more preferably 1 mass% or more, even more preferably 3 mass% or more, still more preferably 5 mass% or more, particularly preferably 7 mass% or more, and is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less.

[0055] The sputtering method is preferably a reactive sputtering method, in which a reactive gas is introduced into the deposition chamber in addition to the sputtering gas.

[0056] In the case of forming a light-transmitting conductive film 20 containing Kr throughout the thickness direction D (first case), the gas introduced into one or more film-forming chambers of the sputtering film-forming apparatus contains Kr as a sputtering gas and oxygen as a reactive gas. The sputtering gas may contain an inert gas other than Kr. Examples of the inert gas other than Kr include rare gas atoms other than Kr. Examples of the rare gas atoms include Ar, Xe, and Rn. When the sputtering gas contains an inert gas other than Kr, the content is preferably 80% by volume or less, more preferably 50% by volume or less.

[0057] When forming the light-transmitting conductive film 20 including the above-mentioned first region 21 and second region 22 (second case), the gas introduced into the film formation chamber for forming the first region 21 contains Kr as a sputtering gas and oxygen as a reactive gas. The sputtering gas may contain an inert gas other than Kr. The type and content of the inert gas other than Kr are the same as those described above for the inert gas other than Kr in the first case.

[0058] In the second case, the gas introduced into the deposition chamber for forming the second region 22 contains an inert gas other than Kr as a sputtering gas and oxygen as a reactive gas. Examples of the inert gas other than Kr include the inert gases mentioned above as the inert gas other than Kr in the first case.

[0059] In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of sputtering gas and oxygen introduced into the film formation chamber is, for example, 0.01 flow % or more and, for example, 15 flow % or less.

[0060] The air pressure in the film formation chamber during film formation by sputtering (sputter film formation) is, for example, 0.02 Pa or more and, for example, 1 Pa or less.

[0061] The temperature of the transparent substrate 10 during sputtering is, for example, 100°C or lower. In order to suppress the thermal expansion of the transparent substrate 10 during sputtering, it is preferable to cool the transparent substrate 10. Suppressing the thermal expansion of the transparent substrate 10 during sputtering helps to obtain a low-resistance light-transmitting conductive film 20' (crystalline light-transmitting conductive film) with suppressed warping. From this viewpoint, the temperature of the transparent substrate 10 during sputtering is preferably 20°C or lower, more preferably 10°C or lower, even more preferably 5°C or lower, particularly preferably 0°C or lower, and is, for example, -50°C or higher, preferably -20°C or higher, more preferably -10°C or higher, and even more preferably -7°C or higher.

[0062] Examples of the power source for applying voltage to the target include a DC power source, an AC power source, an MF power source, and an RF power source. The power source may be a combination of a DC power source and an RF power source. The absolute value of the discharge voltage during sputtering is, for example, 50V or more, and, for example, 500V or less, preferably 400V or less.

[0063] For example, the transparent conductive film X can be produced as described above.

[0064] The light-transmitting conductive film 20 in the transparent conductive film X may be patterned as shown in Fig. 4. The light-transmitting conductive film 20 can be patterned by etching the light-transmitting conductive film 20 through a predetermined etching mask. The patterned light-transmitting conductive film 20 functions as, for example, a wiring pattern.

[0065] Moreover, the light-transmitting conductive film 20 in the transparent conductive film X is converted into a crystalline light-transmitting conductive film 20' (shown in FIG. 5) by heating. Examples of heating means include an infrared heater and an oven (heat medium heating oven, hot air heating oven). The environment during heating may be either a vacuum environment or an air environment. Preferably, heating is performed in the presence of oxygen. From the viewpoint of ensuring a high crystallization rate, the heating temperature is, for example, 100° C. or higher, preferably 120° C. or higher. From the viewpoint of suppressing the influence of heating on the transparent substrate 10, the heating temperature is, for example, 200° C. or lower, preferably 180° C. or lower, more preferably 170° C. or lower, and even more preferably 165° C. or lower. The heating time is, for example, less than 600 minutes, preferably less than 120 minutes, more preferably 90 minutes or lower, and even more preferably 60 minutes or lower, and also, for example, 1 minute or more, preferably 5 minutes or more. The above-mentioned patterning of the light-transmitting conductive film 20 may be carried out before or after the heating for crystallization.

[0066] The surface resistance of the crystalline light-transmitting conductive film 20' is, for example, 200 Ω / □ or less, preferably 100 Ω / □ or less, more preferably 70 Ω / □ or less, even more preferably 50 Ω / □ or less, even more preferably 30 Ω / □ or less, and particularly preferably 20 Ω / □ or less. The surface resistance of the light-transmitting conductive film 20' is, for example, 1 Ω / □ or more. The surface resistance can be measured by a four-terminal method in accordance with JIS K7194.

[0067] The resistivity of the light-transmitting conductive film 20' is preferably 3×10 -4 Ω cm or less, preferably 2.8×10 -4 Ω cm or less, more preferably 2.5×10 -4 Ω cm or less, more preferably 2×10 -4 Ω cm or less, particularly preferably 1.8×10 -4 The resistivity of the light-transmitting conductive film 20' is preferably 0.1×10 -4 Ω·cm or more, preferably 0.5×10 -4 Ω cm or more, more preferably 1.0×10 -4Ω·cm or more.

[0068] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive film 20' is preferably 65% ​​or more, more preferably 80% or more, and further preferably 85% or more. The total light transmittance of the light-transmitting conductive film 20 is, for example, 100% or less.

[0069] As described above, the light-transmitting conductive film 20 of the transparent conductive film X is amorphous, contains a conductive oxide containing krypton, and has a specific resistance of 4×10 -4 Ω cm or more, preferably 4.5×10 -4 Ω cm or more, preferably 4.8×10 -4 Ω cm or more, more preferably 5×10 -4 Ω cm or more, preferably 5.2×10 -4 Ω·cm or more. Such a configuration is suitable for obtaining a low-resistance light-transmitting conductive film 20' (crystalline light-transmitting conductive film) with suppressed warping. Specifically, this is as shown in the examples and comparative examples described later. The transparent conductive film X includes such a light-transmitting conductive film 20, and is therefore suitable for including a low-resistance light-transmitting conductive film 20' (crystalline light-transmitting conductive film) and suppressing warping.

[0070] In the transparent conductive film X, the functional layer 12 may be an adhesion improving layer for realizing high adhesion of the light-transmitting conductive film 20 (light-transmitting conductive film 20′ after crystallization of the light-transmitting conductive film 20; the same applies below) to the transparent substrate 10. The configuration in which the functional layer 12 is an adhesion improving layer is suitable for ensuring adhesion between the transparent substrate 10 and the light-transmitting conductive film 20.

[0071] The functional layer 12 may be an index-matching layer for adjusting the reflectance of the surface (one surface in the thickness direction D) of the transparent substrate 10. The configuration in which the functional layer 12 is an index-matching layer is suitable for making the pattern shape of the light-transmitting conductive film 20 less visible when the light-transmitting conductive film 20 on the transparent substrate 10 is patterned.

[0072] The functional layer 12 may be a peelable functional layer for making it practical to peel the light-transmitting conductive film 20 from the transparent substrate 10. The configuration in which the functional layer 12 is a peelable functional layer is suitable for peeling the light-transmitting conductive film 20 from the transparent substrate 10 and transferring the light-transmitting conductive film 20 to another member.

[0073] The functional layer 12 may be a composite layer in which a plurality of layers are arranged in the thickness direction D. The composite layer preferably includes two or more layers selected from the group consisting of a hard coat layer, an adhesion improving layer, a refractive index adjustment layer, and a release functional layer. Such a configuration is suitable for the functional layer 12 to exhibit the above-mentioned functions of each selected layer in a composite manner. In a preferred embodiment, the functional layer 12 includes an adhesion improving layer, a hard coat layer, and a refractive index adjustment layer on the transparent resin film 11 in this order toward one side of the thickness direction D. In another preferred embodiment, the functional layer 12 includes a release functional layer, a hard coat layer, and a refractive index adjustment layer on the transparent resin film 11 in this order toward one side of the thickness direction D.

[0074] The transparent conductive film X is used in a state where it is fixed to an article and the light-transmitting conductive film 20' is patterned as necessary. The transparent conductive film X is attached to the article, for example, via an adhesive functional layer.

[0075] Examples of the article include an element, a member, and a device. That is, examples of the article with a transparent conductive film include an element with a transparent conductive film, a member with a transparent conductive film, and a device with a transparent conductive film.

[0076] Examples of the element include a light control element and a photoelectric conversion element. Examples of the light control element include a current-driven light control element and an electric field-driven light control element. Examples of the current-driven light control element include an electrochromic (EC) light control element. Examples of the electric field-driven light control element include a PDLC (polymer dispersed liquid crystal) light control element, a PNLC (polymer network liquid crystal) light control element, and a SPD (suspended particle device) light control element. Examples of the photoelectric conversion element include a solar cell. Examples of the solar cell include an organic thin-film solar cell and a dye-sensitized solar cell. Examples of the member include an electromagnetic wave shielding member, a heat ray control member, a heater member, and an antenna member. Examples of the device include a touch sensor device, a lighting device, and an image display device.

[0077] Examples of the above-mentioned fixing functional layer include an adhesive layer and a bonding layer. The material of the fixing functional layer is not particularly limited as long as it has transparency and exhibits a fixing function. The fixing functional layer is preferably formed from a resin. Examples of the resin include acrylic resin, silicone resin, polyester resin, polyurethane resin, polyamide resin, polyvinyl ether resin, vinyl acetate / vinyl chloride copolymer, modified polyolefin resin, epoxy resin, fluororesin, natural rubber, and synthetic rubber. The resin is preferably an acrylic resin because it exhibits adhesive properties such as cohesiveness, adhesiveness, and moderate wettability, is excellent in transparency, and is excellent in weather resistance and heat resistance.

[0078] The adhesion functional layer (resin forming the adhesion functional layer) may contain a corrosion inhibitor to inhibit corrosion of the light-transmitting conductive film 20'. The adhesion functional layer (resin forming the adhesion functional layer) may contain a migration inhibitor (such as a material disclosed in JP 2015-022397 A) to inhibit migration of the light-transmitting conductive film 20'. The adhesion functional layer (resin forming the adhesion functional layer) may contain an ultraviolet absorbing agent to inhibit deterioration of the article when used outdoors. Examples of ultraviolet absorbing agents include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, oxalic acid anilide compounds, cyanoacrylate compounds, and triazine compounds.

[0079] In addition, when the transparent substrate 10 of the transparent conductive film X is fixed to an article via the fixing functional layer, the light-transmitting conductive film 20' (including the light-transmitting conductive film 20' after patterning) is exposed in the transparent conductive film X. In such a case, a cover layer may be disposed on the exposed surface of the light-transmitting conductive film 20'. The cover layer is a layer that covers the light-transmitting conductive film 20', and can improve the reliability of the light-transmitting conductive film 20' and suppress the deterioration of the function of the light-transmitting conductive film 20' due to damage. Such a cover layer is preferably formed from a dielectric material, and more preferably from a composite material of a resin and an inorganic material. Examples of the resin include the resins described above with respect to the fixing functional layer. Examples of the inorganic material include inorganic oxides and fluorides. Examples of the inorganic oxide include silicon oxide, titanium oxide, niobium oxide, aluminum oxide, zirconium dioxide, and calcium oxide. Examples of the fluoride include magnesium fluoride. The cover layer (a mixture of resin and inorganic material) may further contain the above-mentioned corrosion inhibitor, migration inhibitor, and ultraviolet absorbing agent. EXAMPLES

[0080] The present invention will be specifically described below with reference to examples. The present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding thereto described in the above-mentioned "Form for carrying out the invention".

[0081] Example 1 A long PET film with hard coat layers on both sides (product name: KB Film CANIA, thickness 54 μm, manufactured by Kimoto Co., Ltd.) was prepared as a transparent substrate. After heat treatment of this transparent substrate at 165° C. for 1 hour, the thermal shrinkage rate of the transparent substrate in the direction in which it shrinks the most (maximum thermal shrinkage rate, in this example, the thermal shrinkage rate of the substrate in the MD direction) was 0.65%.

[0082] Next, a 150 nm thick amorphous light-transmitting conductive film was formed on the hard coat layer of the transparent substrate by reactive sputtering. In the reactive sputtering, a sputtering film-forming device (DC magnetron sputtering device) capable of performing a film-forming process by roll-to-roll method was used. The sputtering film-forming conditions in this embodiment are as follows.

[0083] The target used was a sintered body of indium oxide and tin oxide (tin oxide concentration was 10% by mass). A DC power supply was used as the power source for applying voltage to the target (horizontal magnetic field strength above the target was 90 mT). The film formation temperature (temperature of the transparent substrate on which the light-transmitting conductive film was laminated) was -5°C. The ultimate vacuum in the film formation chamber of the device was 0.8×10 -4After evacuating the film formation chamber until the pressure reached 0.4 Pa, Kr as a sputtering gas and oxygen as a reactive gas were introduced into the film formation chamber, and the pressure in the film formation chamber was set to 0.4 Pa. The ratio of the amount of oxygen introduced to the total amount of Kr and oxygen introduced into the film formation chamber was about 2.5 flow %, and the amount of oxygen introduced was within region R of the resistivity-oxygen introduction amount curve as shown in FIG. 6, and the resistivity value of the formed film was 6.2×10 -4 The resistivity vs. oxygen introduction amount curve shown in Figure 6 was created by investigating in advance the dependence of the resistivity of the optically transparent conductive film on the amount of oxygen introduced, when the optically transparent conductive film was formed by reactive sputtering under the same conditions as above, except for the amount of oxygen introduced.

[0084] In this manner, a transparent conductive film was produced in Example 1. The light-transmitting conductive film (thickness: 150 nm, amorphous) in the transparent conductive film in Example 1 was composed of a single Kr-containing ITO layer.

[0085] [Examples 2 to 7, 10] In the sputtering deposition, the pressure in the deposition chamber was changed from 0.4 Pa to 0.2 Pa, the thickness of the light-transmitting conductive film was changed from 150 nm to 130 nm, and the resistivity of the film was changed to 6.2×10 -4 6.5×10 instead of Ω cm -4 Ω cm (Example 2), 7.5×10 -4 Ω cm (Example 3), 10.4 × 10 -4 Ω cm (Example 4), 8.8×10 -4 Ω cm (Example 5), 11.6 × 10 -4 Ω cm (Example 6), 5.0×10 -4 Ω cm (Example 7), or 8.2 × 10 -4 Except for adjusting the amount of oxygen introduced to be Ω·cm (Example 10), the transparent conductive films of Examples 2 to 7 and 10 were produced in the same manner as the transparent conductive film of Example 1. The light-transmitting conductive film (thickness 130 nm) of each of the transparent conductive films of Examples 2 to 7 and 10 was composed of a single Kr-containing ITO layer.

[0086] Example 8 The transparent conductive film of Example 8 was produced in the same manner as the transparent conductive film of Example 1, except that in forming the light-transmitting conductive film, a first sputtering deposition for forming a first region (thickness 85 nm) of the light-transmitting conductive film on the transparent substrate and a second sputtering deposition for forming a second region (thickness 45 nm) of the light-transmitting conductive film on the first region were carried out sequentially.

[0087] The conditions for the first sputtering film formation in this example are as follows. A sintered body of indium oxide and tin oxide (tin oxide concentration: 10 mass %) was used as the target. A DC power supply was used as the power supply for applying voltage to the target (horizontal magnetic field strength above the target: 90 mT). The film formation temperature was -5°C. The ultimate vacuum in the first film formation chamber of the device was 0.8×10 -4 After the pressure in the deposition chamber was adjusted to 0.2 Pa, Kr as a sputtering gas and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was adjusted to 0.2 Pa. The amount of oxygen introduced into the deposition chamber was adjusted so that the resistivity of the film to be formed was 6.5×10 -4 The resistivity was adjusted to Ω·cm.

[0088] The conditions for the second sputtering deposition in this embodiment are as follows: The ultimate vacuum in the second deposition chamber of the device is 0.8×10 -4 After the pressure in the deposition chamber was set to 0.4 Pa, Ar as a sputtering gas and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was set to 0.4 Pa. In this embodiment, the other conditions in the second sputter deposition were the same as those in the first sputter deposition.

[0089] In this manner, a transparent conductive film of Example 8 was produced. The light-transmitting conductive film (thickness 130 nm) of the transparent conductive film of Example 8 had a first region (thickness 85 nm) made of a Kr-containing ITO layer and a second region (thickness 45 nm) made of an Ar-containing ITO layer, in this order from the transparent substrate side.

[0090] Example 9 The transparent conductive film of Example 9 was produced in the same manner as the transparent conductive film of Example 1, except that in the formation of the light-transmitting conductive film, a first sputtering film was formed on the transparent substrate to form a second region (thickness 42 nm) of the light-transmitting conductive film, and a second sputtering film was formed on the second region to form a first region (thickness 76 nm) of the light-transmitting conductive film on the second region. The conditions for the first sputtering film formation in this example were the same as the conditions for the second sputtering film formation in Example 8. The conditions for the second sputtering film formation in this example were the same as the conditions for the first sputtering film formation in Example 8.

[0091] In this manner, a transparent conductive film of Example 9 was produced. The light-transmitting conductive film (thickness 118 nm) of the transparent conductive film of Example 9 has, in order from the transparent substrate side, a second region (thickness 42 nm) made of an Ar-containing ITO layer and a first region (thickness 76 nm) made of a Kr-containing ITO layer.

[0092] Example 11 The transparent conductive film of Example 11 was produced in the same manner as the transparent conductive film of Example 1, except for the following in the sputtering film formation: A mixed gas of krypton and argon (Kr 90 volume %, Ar 10 volume %) was used as the sputtering gas. The pressure in the film formation chamber was 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of the mixed gas and oxygen introduced into the film formation chamber was about 2.7 flow %, and the amount of oxygen introduced was such that the resistivity of the formed film was 5.7×10 -4 The resistivity was adjusted to Ω·cm. The thickness of the light-transmitting conductive film formed was 146 nm.

[0093] The light-transmitting conductive film (thickness: 146 nm) of the transparent conductive film of Example 11 is composed of a single ITO layer containing Kr and Ar.

[0094] Comparative Example 1 A light-transmitting conductive film was formed in the same manner as in Example 1, except that the film formation temperature in the sputtering film formation was changed from -5°C to 30°C (the amount of Kr and the amount of oxygen introduced in Comparative Example 1 were the same as those in Example 1). In this way, the transparent conductive film of Comparative Example 1 was produced. The light-transmitting conductive film (thickness 150 nm) of the transparent conductive film of Comparative Example 1 was composed of a single Kr-containing ITO layer.

[0095] Comparative Example 2 A light-transmitting conductive film was formed in the same manner as in Example 2, except that Ar was used instead of Kr as the sputtering gas in the sputtering deposition (the amount of Ar and the amount of oxygen introduced in Comparative Example 2 were the same as the amount of Kr and the amount of oxygen introduced in Example 2). In this way, the transparent conductive film of Comparative Example 2 was produced. The light-transmitting conductive film (thickness 130 nm) of the transparent conductive film of Comparative Example 2 was composed of a single Ar-containing ITO layer.

[0096] <Thickness of the light-transmitting conductive film> The thickness of each of the light-transmitting conductive films in Examples 1 to 11 and Comparative Examples 1 and 2 was measured by FE-TEM observation. Specifically, first, a cross-sectional observation sample of each of the light-transmitting conductive films in Examples 1 to 11 and Comparative Examples 1 and 2 was prepared by FIB microsampling. In the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the thickness of the light-transmitting conductive film in the cross-sectional observation sample was measured by FE-TEM observation. In the FE-TEM observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0097] The thickness of the first region of the light-transmitting conductive film in Example 8 was measured by preparing a sample for cross-sectional observation from an intermediate product before the second region was formed on the first region, and observing the sample with FE-TEM. The thickness of the second region of the light-transmitting conductive film in Example 8 was determined by subtracting the thickness of the first region from the total thickness of the light-transmitting conductive film in Example 8. The proportion of the first region in the thickness direction of the light-transmitting conductive film in Example 8 was 65.4%.

[0098] The thickness of the second region of the light-transmitting conductive film in Example 9 was measured by preparing a sample for cross-sectional observation from an intermediate product before the first region was formed on the second region, and observing the sample with FE-TEM. The thickness of the first region of the light-transmitting conductive film in Example 9 was determined by subtracting the thickness of the second region from the total thickness of the light-transmitting conductive film in Example 9. The proportion of the first region in the thickness direction of the light-transmitting conductive film in Example 9 was 64.4%.

[0099] <Specific resistance> For each of the light-transmitting conductive films in Examples 1 to 11 and Comparative Examples 1 and 2, the initial resistivity before the heat treatment (first resistivity R1) and the resistivity after the heat treatment (second resistivity R2) were examined. In the heat treatment, a hot air oven was used as the heating means, the heating temperature was 165°C, and the heating time was 1 hour. After measuring the surface resistance of the light-transmitting conductive film by the four-terminal method in accordance with JIS K 7194 (1994), the resistivity (Ω·cm) was calculated by multiplying the surface resistance value by the thickness of the light-transmitting conductive film. The results are shown in Table 1.

[0100] <Evaluation of warpage suppression> The degree of warping after heat treatment was examined for each transparent conductive film of Examples 1 to 11 and Comparative Examples 1 and 2. Specifically, first, a sample (short side 50 mm x long side 400 mm) was cut out from the transparent conductive film. Next, the sample was placed on the surface of an iron plate, and both short sides of the sample were fixed to the iron plate surface with heat-resistant tape. Next, the iron plate was heated to heat-treat the sample on the iron plate. In the heat treatment, the heating temperature was 165°C, and the heating time was 1 hour. Next, the heat-resistant tape was peeled off from the iron plate surface and the sample, and the sample was left to stand for 10 minutes in a room temperature (24°C) environment. Next, 175 mm was cut off from both ends of the long side of the sample. As a result, a measurement sample with a size of 50 mm x 50 mm was prepared. Next, the measurement sample was placed on a work table having a horizontal surface (placed so that the light-transmitting conductive film of the measurement sample was located on the opposite side to the horizontal surface). Then, the dimensions of each of the four sides of the measurement sample (specifically, the distance between the two vertices of each side) were measured. Regarding the suppression of warping, the smallest dimension value among the measured dimensions of the four sides was evaluated as "○" when it was 30 mm or more, evaluated as "△" when it was 16 mm or more and less than 30 mm, and evaluated as "×" when it was less than 16 mm. The closer the dimension value is to 50 mm, the more the warping is suppressed. In addition, in the transparent conductive film of Comparative Example 2, the measurement sample took a cylindrical shape during the dimension measurement, and the dimensions of the four sides could not be measured (therefore, it can be practically evaluated as "×"). The evaluation results are shown in Table 1.

[0101] Quantitative analysis of rare gas atoms in optically transparent conductive films The contents of Kr and Ar atoms contained in each of the light-transmitting conductive films in Examples 1 to 11 and Comparative Examples 1 and 2 were analyzed by Rutherford backscattering spectroscopy (RBS). The abundance (atomic %) of Kr atoms and Ar atoms in the light-transmitting conductive film was obtained by calculating the element ratio for the five elements detected, In+Sn (since it is difficult to measure In and Sn separately in RBS, they were evaluated as the sum of the two elements), O, Ar, and Kr. The apparatus used and the measurement conditions are as follows. The analysis results, Kr content (atomic %) and Ar content (atomic %) are shown in Table 1. Regarding the analysis of the Kr content, in Examples 1 to 11 and Comparative Example 1, no reliable measured value equal to or above the detection limit (lower limit) was obtained (the detection limit may vary depending on the thickness of the light-transmitting conductive film used in the measurement). Therefore, in Table 1, the Kr content of the light-transmitting conductive film is expressed as "<specific detection limit for the thickness of the light-transmitting conductive film used in the measurement" to indicate that it is below the detection limit for the thickness of the film (the same applies to the expression of the rare gas atom content).

[0102] <Equipment used> Pelletron 3SDH (manufactured by National Electrostatics Corporation) <Measurement conditions> Incident ions: 4 He ++ Incident energy: 2300keV Incident angle: 0deg Scattering angle: 160deg Specimen current: 6nA Beam diameter: 2mmφ In-plane rotation: None Irradiation dose: 75μC

[0103] <Confirmation of Kr atoms in light-transmitting conductive film> It was confirmed that each of the light-transmitting conductive films in Examples 1 to 11 and Comparative Example 1 contained Kr atoms as follows. First, using a scanning X-ray fluorescence analyzer (product name "ZSX PrimusIV", manufactured by Rigaku Corporation), fluorescent X-ray analysis measurements were repeated five times under the following measurement conditions, and the average value of each scanning angle was calculated to create an X-ray spectrum. Then, it was confirmed that a peak appeared near a scanning angle of 28.2° in the created X-ray spectrum, thereby confirming that the light-transmitting conductive film contained Kr atoms.

[0104] <Measurement conditions> Spectrum;Kr-KA Measurement diameter: 30mm Atmosphere: Vacuum Target: Rh Tube voltage: 50kV Tube current: 60mA Primary filter: Ni40 Scanning angle (deg): 27.0~29.5 Step(deg):0.020 Speed ​​(deg / min): 0.75 Attenuator: 1 / 1 Slit: S2 Spectroscopic crystal: LiF(200) Detector: SC PHA: 100~300

[0105] [Table 1] [Industrial Applicability]

[0106] The light-transmitting conductive film of the present invention can be used as a conductive film for patterning transparent electrodes in various devices such as liquid crystal displays, touch panels, and optical sensors, etc. The transparent conductive film of the present invention can be used as a supply material for such conductive films. [Explanation of symbols]

[0107] X Transparent conductive film D Thickness direction 10 Transparent base material 11 Transparent resin film 12 Functional Layer 20 Light-transparent conductive film

Claims

1. An amorphous light-transmitting conductive film, A conductive oxide containing krypton, 4×10 -4 It has a resistivity of Ω cm or more, A light-transmitting conductive film having a resistivity of less than 3×10 −4 Ω·cm after heat treatment at 165° C. for 1 hour.

2. The resistivity is 20×10 -4 The light-transmitting conductive film according to claim 1 , which has a resistivity of Ω·cm or less.

3. 3. The light-transmitting conductive film according to claim 1 or 2, having a thickness of more than 40 nm.

4. The light-transmitting conductive film according to claim 1 , which is patterned.

5. A transparent substrate; A transparent conductive film comprising: the light-transmitting conductive film according to claim 1 , which is disposed on one surface side in a thickness direction of the transparent substrate.

Citation Information

Patent Citations

  • Manufacture of transparent conductive film

    JP1993334924A

  • Method of manufacturing and reforming film

    JP1996077845A

  • Production of substrate with transparent electrically conductive film, substrate with transparent electrically conductive film and liquid crystal displaying element

    JP2000038654A

  • Method for manufacturing transparent laminate