Silicides and methods for depositing films using the same - Patents.com

Hydridoalkylsilanes in chemical vapor deposition methods create low-k dielectric films with increased carbon content and mechanical strength, addressing weaknesses in existing films and improving device reliability by maintaining low dielectric constants and mechanical integrity.

JP7568714B2Active Publication Date: 2024-10-16VERSUM MATERIALS US LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022509119
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-16
Filing Date
2020-08-14
Publication Date
2024-10-16
Estimated Expiration
2040-08-14

AI Technical Summary

Technical Problem

Existing dielectric films with lower dielectric constants suffer from mechanical weakness, leading to defects such as delamination and increased electromigration, and carbon depletion causes issues like increased dielectric constant, etching, and water adsorption, which affect the integrity and performance of microelectronic devices.

Method used

The use of hydridoalkylsilanes as silicon precursors in chemical vapor deposition methods, allowing for the formation of low-k dielectric films with increased carbon content and improved mechanical strength, achieved through thermal, plasma, or UV energy treatments, which enhance the film's properties without compromising mechanical integrity.

Benefits of technology

The resulting films exhibit a dielectric constant of 2.5-3.2, hardness of 1.0-7.0 GPa, and modulus of elasticity of ~40.0 GPa, providing improved mechanical properties and resistance to plasma damage, while maintaining low dielectric constants, thus enhancing the reliability of microelectronic devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A chemical vapor deposition method for depositing a dielectric film, comprising the steps of: providing a substrate in a reaction chamber; introducing a gaseous reagent into the reaction chamber, the gaseous reagent having a formula R as defined herein. n H 4-n A method comprising: including a silicon precursor comprising a silicon compound having Si; and applying energy to the gaseous reagents in a reaction chamber to induce a reaction of the gaseous reagents to deposit a film on a substrate, wherein the as-deposited film is suitable for its intended use without any optional further curing step applied to the as-deposited film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to U.S. Provisional Application No. 62 / 888,019, filed August 16, 2019, which is incorporated herein by reference in its entirety. [Background technology]

[0002] Described herein are compositions and methods for forming dielectric films using hydridoalkylsilane compounds.More specifically, described herein are compositions and methods for forming films with low dielectric constants ("low k" films or films with a dielectric constant of about 3.2 or less), and the method used to deposit the films is a chemical vapor deposition (CVD) method.The low dielectric films produced by the compositions and methods described herein can be used, for example, as insulating layers in electronic devices.

[0003] The electronics industry utilizes dielectric materials as insulating layers between circuits and components of integrated circuits (ICs) and related electronic devices. To increase the speed and memory storage capacity of microelectronic devices (e.g., computer chips), the dimensions of interconnects are being reduced. As the dimensions of interconnects are reduced, the insulation requirements for the interlayer dielectric (ILD) become much more stringent. Shrinking spacing requires lower dielectric constants to minimize the RC time constant (R is the resistance of the conductive interconnect and C is the capacitance of the insulating dielectric interlayer). Capacitance (C) is inversely proportional to spacing and proportional to the dielectric constant (k) of the interlayer dielectric (ILD). Conventional silica (SiO2) CVD dielectric films made from SiH4 or TEOS (Si(OCH2CH3)4, tetraethyl orthosilicate) and O2 have a dielectric constant k greater than 4.0. There are several approaches that the industry has attempted to produce silica-based CVD films with lower dielectric constants, with doping of insulating silicon oxide films with organic groups being the most successful, resulting in dielectric constants of about 2.7 to about 3.5. Typically, this organosilica glass is produced as a dense film (density ∼1.5 g / cm 3 ) from an organosilicon precursor, such as mesitylene or siloxane, and an oxidizer, such as O2 or N2O. Herein, organosilicon glasses are referred to as OSG. As the carbon content of OSG increases, the mechanical strength of the film, such as the film's hardness (H) and elastic modulus (EM), tends to decrease rapidly as the dielectric constant decreases.

[0004] A difficulty recognized in the industry is that films with lower dielectric constants typically have lower mechanical strength, which leads to additional defects in narrow pitch films, such as delamination, buckling, and increased electromigration, such as observed for conductive lines made from copper embedded in dielectric films with reduced mechanical properties. Such defects may cause premature breakdown of the dielectric, or void formation in the conductive copper lines leading to premature device failure. Furthermore, carbon depletion in the OSG film may cause one or more of the following problems: increase in the dielectric constant of the film, film etching and shape bending during wet clean steps, moisture adsorption in the film due to loss of hydrophobicity, pattern collapse of fine features during wet clean steps after pattern etching, and / or integration problems when depositing subsequent layers, such as, but not limited to, copper diffusion barriers, such as Ta / TaN or advanced Co or MnN barrier layers.

[0005] A possible solution to one or more of these problems is to use OSG films that have increased carbon content but maintain mechanical strength. Unfortunately, increased Si-Me content typically results in reduced mechanical properties, and thus films with more Si-Me negatively impact the mechanical strength that is important for integration.

[0006] One proposed solution is a compound of general formula R x (RO) 3-x Si(CH2) y SiR z (OR) 3-zThe use of ethylene or methylene bridged alkoxysilanes, where x=0-3, y=1 or 2, z=0-3, is believed to avoid the negative impact on mechanical properties since the network connectivity remains the same by replacing the bridging oxygen with a bridging carbon chain. This is due to the idea that replacing the bridging oxygen with a terminal methyl group reduces the mechanical strength by reducing the network connectivity. In this approach, the oxygen atom can be replaced with one or two carbon atoms to increase the atomic weight percent (%) of C without reducing the mechanical strength. However, these crosslinked precursors generally have very high boiling points due to the increased molecular weight from having two silicon groups. The elevated boiling point can negatively impact the manufacturing process by making it difficult to transport the chemical precursor into the reaction chamber as a gas phase reagent without condensing in the vapor delivery line or process pump discharge. Summary of the Invention [Problem to be solved by the invention]

[0007] Thus, there is a need in the art for dielectric precursors that provide films with increased carbon content upon deposition and that do not suffer from the above-mentioned drawbacks. [Means for solving the problem]

[0008] The method and composition described herein meet one or more of the above requirements. The method and composition described herein use hydridoalkylsilane, such as triethylsilane or tri-n-propylsilane, as a silicon precursor that can be used to provide low-k interlayer dielectric when deposited, or can be subsequently treated by thermal, plasma or UV energy source to change the properties of the film, such as to provide chemical crosslinking and improve mechanical strength. In addition, the film deposited using the silicon compound described herein as one or more silicon precursors contains a relatively large amount of carbon. In addition, the one or more silicon compounds described herein have a lower molecular weight (mw) than other prior art silicon precursors, such as crosslinked precursors (e.g. alkoxysilane precursors), which have higher molecular weight (mw) and higher boiling point that inherently have two silicon groups, thereby making the silicon precursor described herein with a boiling point of 250°C or less, more preferably 200°C or less, more accessible to processes, such as mass production processes.

[0009] A single precursor-based dielectric film having the formula Si v O w C x H y F z Described herein are films comprising materials represented by the formula: where v+w+x+y+z=100%, v is 10-35 at%, w is 10-65 at%, x is 5-45 at%, y is 10-50 at%, and z is 0-15 at%, having pores with 0-30% porosity, a dielectric constant of 2.5-3.2, and mechanical properties such as hardness of 1.0-7.0 gigapascals (GPa) and elastic modulus of 4.0-40.0 GPa. In certain embodiments, the films comprise a higher carbon content (10-40%) as measured by X-ray photoelectron spectroscopy (XPS) and exhibit reduced depth of carbon removal when exposed to, for example, O2 or NH3 plasma, as measured by analyzing the carbon content determined by XPS depth profile.

[0010] In one embodiment, a chemical vapor deposition method for producing a dielectric film comprises the steps of: providing a substrate in a reactor; introducing a gaseous agent into the reaction chamber, the gaseous agent comprising at least one oxygen source and a compound represented by the formula R n H 4-n Si, wherein each R is a straight chain, branched chain or cyclic C2-C 10 and a silicon precursor comprising a hydridoalkyl silicon compound independently selected from the group consisting of alkyl, n being 2 to 3; and applying energy to the gaseous reagents in the reaction chamber to induce reaction of the gaseous reagents to deposit a film on the substrate. The as-deposited film can be used with or without further processing, such as thermal annealing, plasma exposure, or UV curing.

[0011] In another aspect, a chemical vapor deposition or plasma enhanced chemical vapor deposition method for producing a low k dielectric film comprises the steps of: providing a substrate in a reaction chamber; introducing a gaseous agent into the reaction chamber, the gaseous agent comprising at least one oxygen source and a compound represented by the formula R n H 4-n Si, wherein each R is a straight chain, branched chain or cyclic C2-C 10 and a hydridoalkyl silicon compound, independently selected from the group consisting of alkyl, n being 2-3; and applying energy to the gaseous agent in the reaction chamber to induce the reaction of the gaseous agent to deposit a film on the substrate.Optionally, the method includes a further step of applying energy to the deposited film, the further energy being selected from the group consisting of thermal annealing, plasma exposure and UV curing, the further energy changing chemical bonds and thereby improving the mechanical properties of the film.The silicon-containing film deposited by the method disclosed herein has a dielectric constant of less than 3.3.In certain embodiments, the silicon precursor further comprises a curing additive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] A chemical vapor deposition method for producing a dielectric film, comprising the steps of: providing a substrate in a reaction chamber; introducing a gaseous agent into the reaction chamber, the gaseous agent being a compound represented by the formula R n H 4-n Si, wherein each R is a straight chain, branched chain or cyclic C2-C 10 Described herein is a method comprising: a silicon precursor comprising a hydridoalkyl silicon compound, independently selected from the group consisting of alkyl, n being 2-3, and at least one oxygen source; and applying energy to the gaseous reagents in a reaction chamber to induce reaction of the gaseous reagents to deposit a film on a substrate. The film can be used as deposited, or can be subsequently treated with additional energy selected from the group consisting of thermal energy (annealing), plasma exposure, and UV curing to modify the chemical properties of the film by improving the mechanical strength of the film and providing a dielectric constant of less than 3.3.

[0013] The hydridoalkylsilane compounds described herein offer unique properties that allow for the incorporation of higher carbon content in the dielectric film with less impact on the mechanical properties of the low-k dielectric film compared to prior art structures forming precursors such as diethoxymethylsilane (DEMS). For example, DEMS provides a mixed complex system in DEMS with two alkoxy groups, one silicon-methyl (Si-Me) and one silicon-hydride that provide a balance of reactive sites, allowing for the formation of a more mechanically robust film while retaining the desired dielectric constant. The use of hydridoalkylsilane compounds offers the advantage of the absence of silicon-methyl groups in the precursor, which tend to reduce mechanical strength, while the carbon in the higher alkyl groups reduces the dielectric constant of the OSG film and confers hydrophobicity. Although there are no methyl groups in the precursor, there are some alkyl groups and some methyl groups in the resulting OSG film that bridge two different silicon atoms, and it is presumed that these groups are formed as a result of fragmentation that occurs in the plasma itself.

[0014] Low-k dielectric films are organosilica glass ("OSG") films or materials. Organosilicates are candidates for low-k materials. Since the type of organosilicon precursor has a strong effect on the structure and composition of the film, it is beneficial to use a precursor that provides the required film properties to ensure that the addition of the required amount of carbon to reach the desired dielectric constant does not produce a film that is mechanically unstable. The methods and compositions described herein provide a means to produce low-k dielectric films that have a desired balance of electrical and mechanical properties, as well as other beneficial film properties such as high carbon content, and provide improved integrated plasma damage resistance.

[0015] In certain embodiments of the methods and compositions described herein, a layer of silicon-containing dielectric material is deposited on at least a portion of a substrate via chemical vapor deposition (CVD) or plasma-enhanced chemical vapor deposition (PECVD), preferably a PECVD process using a reaction chamber.Suitable substrates include, but are not limited to, semiconductor materials, such as gallium arsenide ("GaAs"), silicon, and silicon-containing compositions, such as crystalline silicon, polysilicon, amorphous silicon, epitaxial silicon, silicon dioxide ("SiO2"), silicon glass, silicon nitride, fused silica, glass, quartz, borosilicate glass, and combinations thereof.Other suitable materials include chromium, molybdenum, and other metals commonly used in semiconductor, integrated circuit, flat panel display, and flexible display applications. The substrate may have further layers such as silicon, SiO2, organosilicate glass (OSG), fluorinated silicate glass (FSG), boron carbonitride, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boron nitride, organic-inorganic composites, photoresists, organic polymers, porous organic and inorganic materials and composites, metal oxides such as aluminum oxide and germanium oxide. Additionally, further layers may be germanosilicates, aluminosilicates, copper and aluminum, and diffusion barrier materials such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W, or WN.

[0016] In certain embodiments, the layer of silicon-containing dielectric material is deposited on at least a portion of substrate by introducing into reaction chamber the gaseous agent comprising at least one silicon precursor comprising silicon compound without porogen precursor.In another embodiment, the layer of silicon-containing dielectric material is deposited on at least a portion of substrate by introducing into reaction chamber the gaseous agent comprising at least one silicon precursor comprising hydridoalkylsilane compound with curing additive.

[0017] The methods and compositions described herein comprise a compound of formula Rn H 4-n Si (wherein each R is a straight chain, branched chain or cyclic C2-C 10 wherein n is 2 to 3).

[0018] In the above formula and throughout this specification, the term "alkyl" refers to a straight chain, branched chain, or cyclic functional group having 2 to 10 carbon atoms. Exemplary straight chain alkyl groups include, but are not limited to, ethyl, n-propyl, butyl, pentyl, and hexyl groups. Exemplary branched chain alkyl groups include, but are not limited to, iso-propyl, iso-butyl, sec-butyl, tert-butyl, iso-pentyl, tert-pentyl, iso-hexyl, and neo-hexyl. Exemplary cyclic alkyl groups include, but are not limited to, cyclopentyl, cyclohexyl, or methylcyclopentyl.

[0019] Throughout this specification, the term "oxygen source" refers to a gas that includes oxygen (O2), a mixture of oxygen and helium, a mixture of oxygen and argon, carbon dioxide, carbon monoxide, or a combination thereof.

[0020] Throughout this specification, the term "dielectric film" refers to a Si v O w C x H y F z This refers to a film containing silicon and oxygen atoms and having a composition of (v+w+x+y+z=100%, where v is 10 to 35 at%, w is 10 to 65 at%, x is 5 to 40 at%, y is 10 to 50 at%, and z is 0 to 15 at%).

[0021] formula R n H 4-n Si (wherein each R is a straight chain, branched chain or cyclic C2-C 10Examples of embodiments of the silanes (independently selected from the group consisting of alkyl, and n is 2-3) are the following: triethylsilane, diethylsilane, tri-n-propylsilane, di-n-propylsilane, ethyldi-n-propylsilane, diethyl-n-propylsilane, di-n-propylsilane, di-n-butylsilane, tri-n-butylsilane, tri-iso-propylsilane, diethylcyclopentylsilane, or diethylcyclohexylsilane.

[0022] The hydridoalkylsilanes, and methods and compositions comprising same, described herein are preferably substantially free of one or more impurities, such as, but not limited to, halide ions and water. As used herein, the term "substantially free" means, when referring to a respective impurity, 100 parts per million (ppm) or less, 50 ppm or less, 10 ppm or less, 5 ppm or less, and 1 ppm or less of the respective impurity, such as, but not limited to, chloride or water.

[0023] In some embodiments, the hydridoalkylsilane compounds disclosed herein are substantially free or free of halide ions (or halides), such as chloride, fluoride, bromide and iodide. As used herein, the term "substantially free" means 100 parts per million (ppm) or less, 50 ppm or less, 10 ppm or less, 5 ppm or less, or 1 ppm or less of halide impurities. As used herein, the term "free" means 0 ppm of halide. For example, chloride is known to act as a decomposition catalyst for hydridoalkylsilane compounds, as well as a contaminant that may be detrimental to the performance of manufactured electronic devices. The slow decomposition of hydridoalkylsilane compounds can directly affect the film deposition process, making it difficult for semiconductor manufacturers to meet film specifications. In addition, the shelf life or stability is negatively affected by the faster decomposition rate of silicon compounds, making it difficult to guarantee a shelf life of 1 to 2 years. Thus, accelerated decomposition of hydridoalkylsilane compounds poses safety and performance concerns related to the formation of these flammable and / or pyrophoric gaseous by-products. Preferably, the silicon compound further contains no metal ions, such as Al. 3+ Ion, Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+ As used herein, the term "substantially free" means a material that is substantially free of Al. 3+ Ion, Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+ By "absolute content" is meant less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, and most preferably less than 0.1 ppm.

[0024] The compositions according to the present invention that are substantially free of halides can be achieved by (1) reducing or eliminating chloride sources during chemical synthesis, and / or (2) performing an effective purification process to remove chloride from the crude product, so that the final purified product is substantially free of chloride. The chloride source can be reduced by using halide-free reagents during synthesis, such as reagents that do not contain chlorodisilanes, bromodisilanes or iododisilanes, thereby avoiding the generation of by-products containing halide ions. In addition, the reagents should be substantially free of chloride impurities, so that the resulting crude product is substantially free of chloride impurities. Similarly, the synthesis should not use halide-based solvents, catalysts, or solvents that contain unacceptably high levels of halide contaminants. The crude product can also be treated by various purification methods to render the final product substantially free of halides, such as chloride. Such methods are well described in the prior art and may include purification processes such as, but not limited to, distillation or adsorption. Generally, distillation is used to separate impurities from the desired product by using the difference in boiling points. Adsorption can also be used to affect separation by taking advantage of the different adsorption properties of the components so that the final product is substantially free of halides. Adsorbents, such as commercially available MgO-Al2O3 blends, can be used to remove halides, such as chloride.

[0025] It is believed that the silicon-containing silicon precursors of the prior art, such as DEMS, polymerize after being excited in a reaction chamber to form structures with -O- bonds (e.g. -Si-O-Si- or -Si-OC-) in the polymer backbone, while hydridoalkylsilane compounds, such as triethylsilane molecules, polymerize to form structures in which some of the -O- bridges in the backbone are replaced by -CH2-methylene or -CH2CH2-ethylene bridges. In films deposited using DEMS as a structure-forming precursor, in which carbon is mainly present in the form of terminal Si-Me groups, there is a relationship between the percentage of Si-Me (directly related to the percentage of C) and mechanical strength, and the replacement of a bridging Si-O-Si group by two terminal Si-Me groups reduces the mechanical properties because the network structure is destroyed. Furthermore, it is also believed that during plasma deposition of, for example, triethylsilane, there is the formation of some Si-Me groups by bridging methylene or ethylene groups. Similarly, from the standpoint of mechanical strength, carbon can be incorporated in the form of bridging groups to prevent the network structure from being destroyed by increasing the carbon content in the film. Without intending to be bound by a particular theory, it is believed that this is due to the addition of carbon to the film, which can make the film more recoverable against carbon depletion of the porous OSG film due to processes such as film etching, plasma ashing of the photoresist, and NH3 plasma treatment of the copper surface. Carbon depletion in the OSG film can cause an incomplete increase in the dielectric constant of the film, as well as problems with feature bending during film etching and wet cleaning steps, and / or integration problems when depositing copper diffusion barriers.

[0026] The phrase "gaseous reagent" is sometimes used herein to describe reagents, which is intended to emphasize reagents that are delivered directly to the reactor as a gas, reagents that are delivered as a vaporized liquid, a sublimated solid, and / or reagents that are delivered into the reactor by an inert carrier gas.

[0027] In addition, the reagents can be delivered to the reactor either individually from separate sources or as a mixture. The reagents can be delivered to the reactor system by a number of means, preferably using pressurizable stainless steel vessels equipped with suitable valves and adapted to allow delivery of liquids to the process reactor.

[0028] In addition to the structure-forming species (i.e., the compound of formula I), additional materials can be introduced into the reaction chamber before, during and / or after the deposition reaction. Such materials include, for example, inert gases (e.g., He, Ar, N2, Kr, Xe, etc., which can be used as carrier gases for less volatile precursors and / or promote the hardening of the as-deposited material and provide a more stable final film), and reactive substances, such as oxygen-containing sources, such as O2, O3 and N2O, gaseous or liquid organic substances, CO2 or CO. In one particular embodiment, the reaction mixture introduced into the reaction chamber includes at least one oxidizing agent selected from the group consisting of O2, N2O, NO, NO2, CO2, water, H2O2, ozone, and combinations thereof. In an alternative embodiment, the reaction mixture does not include an oxidizing agent.

[0029] Energy is applied to the gaseous reagents to react the gases and form a film on the substrate. Such energy can be provided by, for example, plasma, pulsed plasma, helicon plasma, high density plasma, inductively coupled plasma, remote plasma, hot filament and heat (i.e. non-filament) and methods. A secondary rf frequency source can be used to modify the plasma characteristics at the substrate surface. Preferably, the film is formed by plasma enhanced chemical vapor deposition ("PECVD").

[0030] The flow rates for each of the gaseous reagents are preferably between 10 and 5000 sccm, more preferably between 30 and 1000 sccm per single 200 mm wafer. The individual amounts are selected to provide the desired amounts of silicon, carbon and oxygen in the film. The actual flow rates required may depend on the wafer size and chamber configuration, and are in no way limited to 200 mm wafers or single wafer chambers.

[0031] In some embodiments, the film is deposited at a deposition rate of about 50 nanometers (nm) / minute.

[0032] The pressure in the reaction chamber during deposition is from about 0.01 to about 600 torr, or from about 1 to about 15 torr.

[0033] The films are preferably deposited to a thickness of 0.002 to 10 microns, although thickness can vary as required. Blanket films deposited on unpatterned surfaces have excellent uniformity with less than 2% thickness variation per standard deviation across the substrate with reasonable edge exclusion, where the outermost edges of the substrate, e.g., 5 mm, are not included in the statistical calculation of uniformity.

[0034] Preferred embodiments of the present invention provide thin film materials having low dielectric constants and improved mechanical properties, thermal stability and chemical resistance (to oxygen, aqueous oxidizing environments, etc.) compared to other porous low-k dielectric films deposited using other structure-forming precursors known in the art. The structure-forming precursors described herein, including one or more hydridoalkylsilane compounds having the formulas above, are preferably formed from organic carbon in the form (-CH x (where x is 1-3)) provides greater incorporation of carbon into the film whereby a particular precursor or network forming chemical is used to deposit the film. In certain embodiments, much of the hydrogen in the film is bonded to carbon.

[0035] The low-k dielectric films deposited by the compositions and methods described herein comprise: (a) about 10 to about 35 at%, more preferably about 20 to about 30 at% silicon; (b) about 10 to about 65 at%, more preferably about 20 to about 45 at% oxygen; (c) about 10 to about 50 at%, more preferably about 15 to about 40 at% hydrogen; (d) about 5 to about 40 at%, more preferably about 10 to about 45 at% carbon. The films may further comprise about 0.1 to about 15 at%, more preferably about 0.5 to about 7.0 at% fluorine to improve one or more of the material's properties. Smaller amounts of other elements may also be present in certain films of the invention. OSG materials are considered low-k materials when their dielectric constant is less than that of the standard material conventionally used in industry - silica glass.

[0036] The total porosity of the film may be 0-15% or more depending on the process conditions and the desired final film properties. Preferably, the films of the present invention have a density less than 2.3 g / ml, or alternatively less than 2.0 g / ml or less than 1.8 g / ml. The total porosity of the OSG film can be influenced by post-deposition treatments including thermal or UV curing, exposure to a plasma source. Although preferred embodiments of the present invention do not include the addition of porogen during deposition of the film, porosity can be induced by post-deposition treatments such as UV curing. For example, UV treatments can result in porosity reaching about 15 to about 20%, preferably about 5 to about 10%.

[0037] The film of the present invention may contain fluorine in the form of inorganic fluorine (eg, Si-F). Preferably, fluorine, if present, is contained in an amount of about 0.5 to about 7 at %.

[0038] The films of the present invention are thermally stable and have good chemical resistance. In particular, the preferred films after annealing have an average weight loss of less than 1.0 wt% / hr isothermal at 425° C. under N2. Furthermore, the films preferably have an average weight loss of less than 1.0 wt% / hr isothermal at 425° C. under air.

[0039] The films are suitable for a variety of uses. They are particularly suitable for deposition on semiconductor substrates, for example for use as insulator layers, interlayer dielectric layers and / or interlayer metal dielectric layers. They can form conformal coatings. The mechanical properties exhibited by these films make them particularly suitable for use in Al-depletion and Cu-damascene or dual-damascene technologies.

[0040] The film is compatible with chemical mechanical planarization (CMP) and anisotropic etching, and can adhere to a variety of materials, such as silicon, SiO2, Si3N4, OSG, FSG, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boron nitride, anti-reflective coatings, photoresists, organic polymers, porous organic and inorganic materials, metals, such as copper and aluminum, diffusion barrier layers, such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W, WN, or W(C)N. Preferably, the film can adhere sufficiently to at least one of the aforementioned materials to pass a conventional pull test, such as the tape pull test of ASTM D3359-95a. A sample is considered to have passed the test if there is no discernible removal of the film.

[0041] Thus, in certain embodiments, the film is an insulator layer, an interlevel dielectric layer, an interlevel metal dielectric layer, a cap layer, a chemical mechanical planarization (CMP) or etch stop layer, a barrier layer, or an adhesion layer in an integrated circuit.

[0042] The present invention is particularly suitable for providing films, and the products of the present invention are often described herein as films, but the present invention is not limited thereto. The products of the present invention can be provided in any form that can be deposited by CVD, such as coatings, assemblies of layers, and other types of articles that are not necessarily flat or thin, some of which are not necessarily used in integrated circuits. Preferably, the substrate is a semiconductor.

[0043] In addition to the OSG products of the present invention, the disclosure includes processes for making the products, methods for using the products, and compounds and compositions useful for preparing the products. For example, a process for fabricating integrated circuits on semiconductor devices is disclosed in U.S. Patent No. 6,583,049, which is incorporated herein by reference.

[0044] The composition of the present invention may be, for example, equipped with a suitable valve and n H 4-n Si (wherein R is a linear, branched or cyclic C2-C 10 The process reactor may further comprise at least one pressurizable vessel (preferably made of stainless steel) suitable for enabling the transport of a silicon precursor having a silane group, such as triethylsilane, having a molar ratio of 1 to 10, and a molar ratio of 1 to 10, such as 1 to 10, to the process reactor.

[0045] The preliminary (or as-deposited) film can be further treated by a curing step, i.e., applying an additional energy source to the film, which may include thermal annealing, chemical treatment, in-situ or remote plasma treatment, photocuring (e.g., UV) and / or microwave. Other in-situ or post-deposition treatments can be used to improve material properties such as hardness, stability (against shrinkage, atmospheric exposure, etching, wet etching, etc.), conformity, uniformity, and adhesion. Thus, the term "post-treatment" as used herein means treating the film with energy (e.g., heat, plasma, photons, electrons, microwaves, etc.) or chemicals to improve material properties.

[0046] The conditions under which post-treatment is carried out may vary widely, for example, post-treatment may be carried out under high pressure or in a vacuum environment.

[0047] UV annealing is the preferred method of curing and is typically carried out under the following conditions:

[0048] The environment may be inert (e.g., nitrogen, CO2, noble gases (He, Ar, Ne, Kr, Xe), etc.), oxidizing (e.g., oxygen, air, oxygen-lean environment, oxygen-enriched environment, ozone, nitrous oxide, etc.), or reducing (dilute or concentrated hydrogen, hydrocarbons (saturated, unsaturated, straight or branched chain, aromatic), ammonia, hydrazine, methylhydrazine, etc.). The pressure is preferably from about 1 Torr to about 1000 Torr, more preferably atmospheric pressure. However, a vacuum environment is also possible for the thermal anneal as well as any other post-processing means. The temperature is preferably 200-500°C, with a temperature ramp rate of 0.1-100°C / min. The total UV anneal time is preferably 0.01 min to 12 h.

[0049] The chemical treatment of the OSG film is carried out under the following conditions:

[0050] Use of chemical processes such as fluorination (HF, SiF4, NF3, F2, COF2, CO2F2, etc.), oxidation (H2O2, O3, etc.), chemical drying, methylation, or other chemical processes to improve the properties of the final material. Chemicals used in such processes may be in solid, liquid, gaseous and / or supercritical fluid states.

[0051] The plasma treatment for possible chemical modification of the OSG film is carried out under the following conditions:

[0052] The environment may be inert (such as nitrogen, CO2, noble gases (He, Ar, Ne, Kr, Xe)), oxidizing (such as oxygen, air, oxygen-lean environments, oxygen-enriched environments, ozone, nitrous oxide, etc.), or reducing (such as dilute or concentrated hydrogen, hydrocarbons (saturated, unsaturated, straight or branched chain, aromatic), ammonia, hydrazine, methylhydrazine, etc.). The plasma power is preferably 0-5000 W. The temperature is preferably from about ambient to about 500° C. The pressure is preferably from 10 mtorr to atmospheric pressure. The total curing time is preferably from 0.01 min to 12 h.

[0053] UV curing for chemical crosslinking of organosilicate films is typically carried out under the following conditions:

[0054] The environment may be inert (e.g., nitrogen, CO2, noble gases (He, Ar, Ne, Kr, Xe), etc.), oxidizing (e.g., oxygen, air, oxygen-lean environments, oxygen-enriched environments, ozone, nitrous oxide, etc.), or reducing (e.g., lean or concentrated hydrocarbons, hydrogen, etc.). The temperature is preferably from about ambient to about 500°C. The power is preferably from 0 to about 5000 W. The wavelength is preferably IR, visible, UV or deep UV (<200 nm wavelength). The total UV cure time is preferably from 0.01 minutes to 12 hours.

[0055] Microwave post-treatment of organosilicate films is typically carried out under the following conditions:

[0056] The environment may be inert (e.g., nitrogen, CO2, noble gases (He, Ar, Ne, Kr, Xe), etc.), oxidizing (e.g., oxygen, air, oxygen-lean environments, oxygen-enriched environments, ozone, nitrous oxide, etc.), or reducing (e.g., lean or concentrated hydrocarbons, hydrogen, etc.). Temperature is preferably from about ambient to about 500°C. Power and wavelength can be varied and adjusted for specific bonds. Total cure time is preferably from 0.01 minutes to 12 hours.

[0057] Electron beam post-treatment to improve film properties is typically performed under the following conditions:

[0058] The environment may be vacuum, inert (e.g., nitrogen, CO2, noble gases (He, Ar, Ne, Kr, Xe), etc.), oxidizing (e.g., oxygen, air, oxygen-lean environments, oxygen-enriched environments, ozone, nitrous oxide, etc.), or reducing (e.g., lean or concentrated hydrocarbons, hydrogen, etc.). Temperature is preferably from ambient to 500°C. Electron density and energy can be varied and adjusted for specific bonds. Total cure time is preferably from 0.001 minutes to 12 hours and may be continuous or pulsed. Further guidance on the general use of electron beams is available in publications such as S. Chattopadhyay et al., Journal of Materials Science, 36 (2001) 4323-4330; G. Kloster et al., Proceedings of IITC, June 3-5, 2002, SF, CA; and U.S. Patent Nos. 6,207,555, 6,204,201, and 6,132,814. The use of electron beam treatment can provide for the removal of porogens, an improvement in the mechanical properties of the film through bond formation processes in the matrix.

[0059] The present invention will be illustrated in more detail with reference to the following examples, but it should be understood that the present invention is not to be regarded as being limited to the following examples. EXAMPLES

[0060] Exemplary films or 200 mm wafer processes were formed from a variety of different chemical precursors and process conditions via a plasma-enhanced CVD (PECVD) process using an Applied Materials Precision-5000 system in a 200 mm DxZ or DxL reaction chamber or vacuum chamber equipped with an Advance Energy 200 RF generator. In general, the PECVD process included the following basic steps: initial setup and stabilization of gas flows, deposition of the film on the silicon wafer substrate, and purging / evacuation of the chamber prior to removal of the substrate. After deposition, some of the films were subjected to UV annealing. UV annealing was performed at one or more pressures of <10 torr and one or more temperatures of <400° C. using a Fusion UV system with a broadband UV bulb with the wafer under helium gas flow. Experiments were performed on p-type Si wafers (resistivity range = 8-12 Ω·cm).

[0061] The thickness and refractive index were measured on an SCI FilmTek 2000 reflectometer. The dielectric constant was determined using the Hg probe technique on medium resistivity p-type wafers (range 8-12 Ω·cm). In Examples 1 and 2, the mechanical properties were determined using an MTS Nano Indenter.

[0062] Example 1: Deposition of OSG films from triethylsilane (3ES) without subsequent UV curing OSG films were deposited on 200 mm Si wafers from 3ES using the following process conditions: Precursors were delivered to the reaction chamber via direct liquid injection (DLI) at a flow rate of 1400 mg / min, and a 700 W plasma was applied for 60 seconds with a helium carrier gas flow of 200 sccm, 60 sccm O2, a 350 mil showerhead to the wafer spacing, a wafer chuck temperature of 390°C, and a chamber pressure of 8 Torr. The resulting film had a refractive index (RI) of 1.49 and a dielectric constant (k) of 3.0, and was 704 nm thick. The hardness of the film was measured to be 2.7 GPa, and Young's modulus was 16.3 GPa. The elemental composition was measured by XPS. The film composition was 32.7% C, 36.6% O, and 30.7% Si.

[0063] Example 2: Deposition of OSG films from triethylsilane (3ES) followed by a 4 minute post-deposition UV cure OSG films were deposited on 200 mm Si wafers from 3ES using the following process conditions: Precursors were delivered to the reaction chamber via direct liquid injection (DLI) at a flow rate of 1400 mg / min, and a 700 W plasma was applied for 60 seconds with a helium carrier gas flow of 200 sccm, 60 sccm O2, a 350 mil showerhead to the wafer spacing, a wafer chuck temperature of 390° C., and a chamber pressure of 8 Torr. After deposition, the wafer was removed by load lock into a UV cure chamber and the film was cured by UV irradiation at 400° C. for 4 minutes. The resulting film had a refractive index (RI) of 1.48 and a dielectric constant (k) of 3.0 and was 646 nm thick. The hardness of the film was measured to be 3.2 GPa and Young's modulus was 18.8 GPa. The elemental composition was measured by XPS and the film composition was 26.8% C, 41.2% O, and 32% Si.

[0064] Example 3: Deposition of OSG films from tri-n-propylsilane (3nPS) without subsequent UV curing OSG films were deposited from 3nPS onto 200 mm Si wafers using the following process conditions: 3nPS precursor was delivered to the reaction chamber via direct liquid injection (DLI) at a flow rate of 1500 mg / min, and a 600 W plasma was applied for 60 seconds with a helium carrier gas flow of 200 sccm, 60 sccm O2, a 350 mil showerhead to the wafer spacing, a wafer chuck temperature of 390°C, and a chamber pressure of 6 Torr. The resulting film had a refractive index (RI) of 1.45 and a dielectric constant of 3.0, and was 528 nm thick. The hardness of the film was measured to be 2.6 GPa, and Young's modulus was 15.6 GPa. The elemental composition was measured by XPS and the film composition was 26.1% C, 43.0% O, and 30.9% Si.

[0065] Example 4: Deposition of OSG films from tri-n-propylsilane (3nPS) followed by a 4 minute post-deposition UV cure OSG films were deposited on 200 mm Si wafers from 3nPS using the following process conditions: Precursors were delivered to the reaction chamber via direct liquid injection (DLI) at a flow rate of 1500 mg / min, and a 600 W plasma was applied for 60 seconds with a helium carrier gas flow of 200 sccm, 60 sccm O2, a 350 mil showerhead to the wafer spacing, a wafer chuck temperature of 390°C, and a chamber pressure of 6 Torr. After deposition, the wafer was transferred by load lock to a UV cure chamber and the film was cured by UV exposure at 400°C for 4 minutes. The resulting film was 495 nm thick with a refractive index (RI) of 1.437 and a dielectric constant of 3.2. The hardness of the film was measured to be 3.7 GPa and Young's modulus was 23.4 GPa. The elemental composition was measured by XPS and the film composition was 18.8% C, 49% O, and 32.2% Si.

[0066] Comparative Example 1: Deposition of OSG films from 1-methyl-1-ethoxy-1-silacyclopentane (MESCAP) without subsequent UV curing OSG films were deposited from 1-methyl-1-ethoxy-1-silacyclopentane in a DxZ chamber for a 200 mm run using the following process conditions: Precursors were delivered to the reaction chamber via direct liquid injection (DLI) at a flow rate of 1500 milligrams per minute (mg / min), and 600 W plasma was applied with a helium carrier gas flow of 200 standard cubic centimeters (sccm), 10 sccm O2, 350 milliinch showerhead / wafer spacing, 400° C. wafer chuck temperature, and 7 Torr chamber pressure. The resulting as-deposited films had a dielectric constant (k) of 3.03, a hardness (H) of 2.69 GPa, and a refractive index (RI) of 1.50.

[0067] Comparative Example 2: Deposition of OSG films from 1-methyl-1-ethoxy-1-silacyclopentane (MESCAP) with subsequent UV curing OSG films were deposited from 1-methyl-1-ethoxy-1-silacyclopentane in a DxZ chamber for a 200 mm run using the following process conditions: Precursors were delivered to the reaction chamber via direct liquid injection (DLI) at a flow rate of 1000 milligrams per minute (mg / min), and 400 W plasma was applied with a helium carrier gas flow of 200 standard cubic centimeters (sccm), 10 sccm O2, 350 milliinch showerhead / wafer spacing, 400° C. wafer chuck temperature, and 7 Torr chamber pressure. The resulting as-deposited film had a dielectric constant (k) of 3.01, a hardness (H) of 2.06 GPa, and a refractive index (RI) of 1.454. After UV curing, k was 3.05, H was 3.58 GPa, and RI was 1.46. This example shows a significant improvement in mechanical strength with a very small increase in k.

[0068] Although illustrated and described above with reference to certain specific embodiments and examples, the present invention is not intended to be limited to the details shown. Rather, various changes in details may be made without departing from the spirit of the present invention, within the scope and range of equivalents of the claims. For example, all ranges broadly described in this document are expressly intended to include within their scope all narrower ranges that are subsumed within that broad range. The present invention can be embodied in the following manner. (Appendix 1) 1. A chemical vapor deposition method for producing a dielectric film, comprising: Providing a substrate in a reaction chamber; introducing a gaseous agent into the reaction chamber, the gaseous agent comprising: R n H 4-n Si, wherein R is a straight chain, branched chain or cyclic C 2 ~C 10 a silicon precursor selected from the group consisting of alkyl, n being 2 to 3; At least one oxygen source; and applying energy to the gaseous reagent in the reaction chamber to induce a reaction of the gaseous reagent, thereby depositing a film on the substrate; wherein the film has a dielectric constant of about 2.5 to 3.3. (Appendix 2) 2. The method of claim 1, wherein the silicon precursor is at least one selected from the group consisting of triethylsilane, diethylsilane, tri-n-propylsilane, di-n-propylsilane, ethyldi-n-propylsilane, diethyl-n-propylsilane, di-n-propylsilane, di-n-butylsilane, tri-n-butylsilane, tri-isopropylsilane, diethylcyclopentylsilane, and diethylcyclohexylsilane. (Appendix 3) 2. The method of claim 1, wherein the deposition method is a plasma-enhanced chemical vapor deposition method. (Appendix 4) The oxygen source is O 2 、N 2 O, NO, NO 2 , CO 2 , water, H 2 O 2 and ozone. (Appendix 5) During the energy application step, He, Ar, N 2 , Kr, Xe, NH 3 、H 2 , CO 2 or CO is combined with the gaseous reagent in the reaction chamber. (Appendix 6) 2. The method of claim 1, further comprising applying additional energy to the deposited film. (Appendix 7) 7. The method of claim 6, wherein the additional energy is at least one selected from the group consisting of heat treatment, ultraviolet light (UV) treatment, electron beam treatment, and gamma irradiation treatment. (Appendix 8) 8. The method of claim 7, wherein the additional energy includes a UV treatment and a heat treatment, and the UV treatment occurs during at least a portion of the heat treatment. (Appendix 9) The film has a composition of Si v O w C x H y F z wherein v+w+x+y+z=100%, v is 10 to 35 at%, w is 10 to 65 at%, x is 5 to 40 at%, y is 10 to 50 at%, and z is 0 to 15 at%. (Appendix 10) A gaseous reagent for producing a dielectric film by a chemical vapor deposition process, comprising: n H 4-n Si, wherein R is a straight chain, branched chain or cyclic C 2 ~C 10 A gaseous reagent comprising a silicon precursor selected from the group consisting of alkyl, n being 2-3, and having 100 ppm or less of halide ions or water. (Appendix 11) 11. The gaseous reagent of claim 10 having 1 ppm or less of halide ions or water.

Claims

1. 1. A chemical vapor deposition method for producing a dielectric film, comprising: providing a substrate in a reaction chamber; introducing a gaseous agent into the reaction chamber, the gaseous agent comprising: R n H 4-n Si, wherein R is a linear, branched or cyclic C 2 ~C 10 a silicon precursor selected from the group consisting of alkyl, n being 2-3; At least one oxygen source; having 100 ppm or less of halide ions or water; and applying energy to the gaseous reagent in the reaction chamber to induce a reaction of the gaseous reagent, thereby depositing a film on the substrate; wherein the film has a dielectric constant of about 2.5 to 3.

3.

2. 2. The method of claim 1, wherein the silicon precursor is at least one selected from the group consisting of triethylsilane, diethylsilane, tri-n-propylsilane, di-n-propylsilane, ethyldi-n-propylsilane, diethyl-n-propylsilane, di-n-propylsilane, di-n-butylsilane, tri-n-butylsilane, tri-iso-propylsilane, diethylcyclopentylsilane, diethylcyclohexylsilane.

3. The method of claim 1 , wherein the deposition method is a plasma enhanced chemical vapor deposition method.

4. The oxygen source is O 2 , N 2 O, NO, NO 2 , CO 2 , water, H 2 O 2 10. The method of claim 1, further comprising at least one selected from the group consisting of:

5. During the energy application step, He, Ar, N 2, Kr, Xe, NH 3 , H 2 , CO 2 2. The method of claim 1, wherein at least one gas selected from the group consisting of CO or H O is combined with the gaseous reagent in the reaction chamber.

6. The method of claim 1 further comprising applying additional energy to the deposited film.

7. 7. The method of claim 6, wherein the additional energy is at least one selected from the group consisting of heat treatment, ultraviolet light (UV) treatment, electron beam treatment, and gamma irradiation treatment.

8. The method of claim 7 , wherein the additional energy comprises a UV treatment and a heat treatment, the UV treatment occurring during at least a portion of the heat treatment.

9. The film has a composition of Si v O w C x H y F z 2. The method of claim 1, comprising: wherein v+w+x+y+z=100%, v is 10-35 at%, w is 10-65 at%, x is 5-40 at%, y is 10-50 at%, and z is 0-15 at%.

10. A gaseous reagent for producing a dielectric film by a chemical vapor deposition process, comprising: n H 4-n Si, wherein R is a linear, branched or cyclic C 2 ~C 10 A gaseous reagent comprising a silicon precursor selected from the group consisting of alkyl, where n is 2-3, and having 100 ppm or less of halide ions or water.

11. 11. The gaseous reagent of claim 10 having less than 1 ppm of halide ions or water.

Citation Information

Patent Citations

  • Mechanical enhancement of high-density porous organic silicate material by UV irradiation

    JP2004274052A

  • Silicon-containing film and formation method thereof

    JP2009194037A