Grain-oriented electrical steel sheet, steel sheet for final annealing, annealing separator, method for manufacturing grain-oriented electrical steel sheet, and method for manufacturing steel sheet for final annealing
By controlling the interface structure and composition of grain-oriented electrical steel sheets with specific elements and an annealing separator, the method addresses adhesion and magnetic flux density issues, resulting in improved performance and reduced iron loss.
Patent Information
- Application Number
- JP2020019188
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-06
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-02-06
AI Technical Summary
Existing methods for producing grain-oriented electrical steel sheets face challenges in maintaining high magnetic flux density and adhesion of the primary coating due to flat interfaces between the base material steel plate and the primary coating, which are prone to peeling under compressive stress, and do not effectively address point defects or iron loss.
The method involves controlling the interface structure between the primary coating and the base steel sheet by adjusting the chemical composition and morphology, including specific ranges for elements like C, Si, Mn, S, Se, Al, N, Ti, and B, and using an annealing separator containing MgO, Ti, and B to form a primary coating with a complex three-dimensional shape, enhancing adhesion and maintaining magnetic properties.
The solution results in a grain-oriented electrical steel sheet with improved adhesion against bending and shearing, reduced iron loss, and maintained magnetic flux density by optimizing the interface structure and composition, thereby enhancing the overall performance of the steel sheet.
Smart Images

Figure 0007568894000006 
Figure 0007568894000007 
Figure 0007568894000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a grain-oriented electrical steel sheet, a steel sheet for finish annealing, an annealing separator, a method for manufacturing a grain-oriented electrical steel sheet, and a method for manufacturing a steel sheet for finish annealing. [Background technology]
[0002] Grain-oriented electrical steel sheets contain about 0.5 to 7% Si by mass and have a crystal orientation of {110} <001> This steel sheet is made of steel with grains assembled in the Goss orientation. The crystal orientation is controlled by using a catastrophic grain growth phenomenon called secondary recrystallization.
[0003] The manufacturing method of grain-oriented electrical steel sheet is as follows: A slab is heated and hot-rolled to produce a hot-rolled steel sheet. The hot-rolled steel sheet is annealed as necessary. The hot-rolled steel sheet is pickled. The pickled hot-rolled steel sheet is cold-rolled at a cold rolling rate of 80% or more to produce a cold-rolled steel sheet. The cold-rolled steel sheet is subjected to decarburization annealing to induce primary recrystallization. The cold-rolled steel sheet after decarburization annealing is subjected to finish annealing to induce secondary recrystallization. Grain-oriented electrical steel sheet is manufactured by the above steps.
[0004] After the above-mentioned decarburization annealing and before the finish annealing, an annealing separator mainly composed of MgO is applied to the surface of the cold-rolled steel sheet. Usually, this is done by applying an aqueous slurry containing the annealing separator component and drying it. The cold-rolled steel sheet to which the annealing separator is applied is wound into a coil, and then the finish annealing is performed. During the finish annealing, MgO in the annealing separator reacts with SiO2 in the internal oxide layer formed on the surface of the cold-rolled steel sheet during the decarburization annealing, and in the final product, a primary coating mainly composed of forsterite (Mg2SiO4) is formed on the surface. After the primary coating is formed, an insulating coating (also called a secondary coating) made of, for example, colloidal silica and phosphate is formed on the primary coating. The primary coating and the insulating coating have a smaller thermal expansion coefficient than the base steel sheet. Therefore, the primary coating, together with the insulating coating, applies tension to the base steel sheet to reduce iron loss. The primary coating also improves the adhesion of the insulating coating to the base steel sheet, and therefore it is preferable for the primary coating to have high adhesion to the base steel sheet.
[0005] On the other hand, in order to reduce the iron loss of grain-oriented electrical steel sheets, it is also effective to increase the magnetic flux density and reduce the hysteresis loss.
[0006] In order to increase the magnetic flux density of grain-oriented electrical steel sheets, it is effective to further concentrate the crystal orientation of the base steel sheet in the Goss orientation. Technologies for increasing the concentration in the Goss orientation are proposed in Patent Documents 1 to 3. In these patent documents, magnetic property improving elements (Cu, Sn, Sb, Bi, Te, Pb, Se, etc.) that strengthen the inhibitor action are contained in the base steel sheet. This increases the concentration in the Goss orientation, and the magnetic flux density can be increased.
[0007] Furthermore, Patent Documents 4 and 5 disclose techniques for improving the adhesion of the primary coating to the steel sheet.
[0008] Patent Document 4 describes a method in which the slab contains 0.001 to 0.1% Ce and the steel sheet surface contains 0.01 to 1000 mg / m 2 A method for producing a grain-oriented electrical steel sheet is disclosed in which a primary coating including a
[0009] Patent Document 5 describes a grain-oriented electrical steel sheet containing 1.8 to 7% Si and having a primary coating on the surface mainly composed of forsterite, in which one or two of Ce, La, Pr, Nd, Sc, and Y are contained in the primary coating in an amount of 0.001 to 1000 mg / m per side. 2 , Sr, Ca, Ba, one or more of which is added in an amount of 0.01 to 100 mg / m per side 2 The present invention discloses a grain-oriented electrical steel sheet comprising:
[0010] Patent Document 5 discloses a method for producing grain-oriented electrical steel sheet having excellent magnetic properties and coating adhesion, which includes a series of steps of applying an annealing separator to the surface of a base steel sheet that has been subjected to decarburization annealing, drying, and performing finish annealing, and is characterized in that the annealing separator contains one or more of oxides, hydroxides, sulfates, and carbonates of Ce, La, Pr, Nd, Sc, and Y having an average particle size of 0.1 to 25 μm in an amount of 0.01 to 14 mass% in total relative to the MgO in metal conversion. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 6-88171 [Patent Document 2] Japanese Patent Application Publication No. 8-269552 [Patent Document 3] JP 2005-290446 A [Patent Document 4] JP 2008-127634 A [Patent Document 5] JP 2012-214902 A Summary of the Invention [Problem to be solved by the invention]
[0012] However, the base steel sheet / primary coating interface is formed so that the interface energy is as low as possible, and the above-mentioned base steel sheet / primary coating interface becomes flat. In particular, when a magnetic property improving element is contained as in the techniques described in Patent Documents 1 to 3, the interface is more likely to become flat. When the interface becomes flat, the interdigitated structure that creates the physical bonding force between the primary coating and the base steel sheet is lost, and the adhesion of the primary coating to the base steel sheet decreases. In particular, the interface becomes more susceptible to peeling due to compressive stress caused by bending, and adhesion decreases significantly.
[0013] Furthermore, although the technology described in Patent Document 4 takes steps to improve coating adhesion, it can provide sufficient adhesion when bending a few tens of millimeters and adhesion to shearing, but the physical bond between the base steel and the coating is insufficient to withstand the compressive stress that occurs when bending a small bending diameter, such as 10 mm, so coating adhesion is insufficient. Furthermore, the technology described in Patent Document 4 does not take measures against the occurrence of point defects. Furthermore, the technology described in Patent Document 4 does not allow sufficient magnetic properties to be maintained.
[0014] Furthermore, the measures taken in Patent Document 5 to improve coating adhesion include making the morphology of the interface between the base steel and the oxide into a complex structure, or increasing the thickness of the coating, thereby increasing the number of non-magnetic layers, but these respectively result in increased iron loss and decreased magnetic flux density, and no measures are taken to address the occurrence of point defects.
[0015] Regarding the adhesion of the coating, various means for improving it have been proposed from various viewpoints, but it cannot be said that an optimal method for manufacturing a steel sheet and a method for forming a primary coating have been presented for controlling the primary coating form to obtain good coating adhesion from the viewpoint of maintaining or improving magnetic flux density and iron loss. Therefore, there is a demand for a primary coating forming technology that reduces the decrease in magnetic flux density for a parent phase with excellent magnetic properties, and for a coated grain-oriented electrical steel sheet.
[0016] An object of the present invention is to provide a grain-oriented electrical steel sheet in which deterioration of magnetic properties is minimal and in which a primary coating exhibits excellent adhesion, a steel sheet for finish annealing, an annealing separator, a method for manufacturing a grain-oriented electrical steel sheet, and a method for manufacturing a steel sheet for finish annealing. [Means for solving the problem]
[0017] In order to solve the above problems, according to one aspect of the present invention, the composition contains, by mass%, C: 0.005% or less, Si: 2.5 to 4.5%, Mn: 0.01 to 0.15%, one or more elements selected from the group consisting of S and Se: 0.005% or less in total, sol. Al: 0.010% or less, and N: 0.0150% or less, with the balance being Fe and impurities. Consists ofA steel sheet having a base material and a primary coating formed on a surface of the base material steel sheet and containing Mg2SiO4 as a main component, wherein the sum of the content of one or more elements selected from the group consisting of S and Se in the base material steel sheet and the content of one or more elements selected from the group consisting of S and Se in the primary coating is 0.005 to 0.050 mass%, the sum of the content of Al in the base material steel sheet and the content of Al in the primary coating is 0.005 to 0.040 mass%, and the content of N in the base material steel sheet is The sum of the N content in the primary coating and the N content in the primary coating is 0.0005 to 0.0200 mass %, and in an unevenness distribution diagram of the primary coating at the interface between the primary coating and the base steel sheet, obtained by projecting the primary coating onto a plane parallel to the surface where the base steel sheet and the primary coating are laminated, a direction from the primary coating toward the base steel sheet is defined as a positive direction, H0 is the center position of the interface between the primary coating and the base steel sheet, and a region where the primary coating is present on the positive side of H0 is defined as an indented oxide layer region. the average value H1 of the distance from H0 to the surface is 0.40 to 2.00 μm, the surface roughness Ra of the primary coating at the interface between the primary coating and the base steel sheet is 0.30 to 4.00 μm, the total content of Ti contained in the base steel sheet and the content of Ti contained in the primary coating is 0.50 to 12.00 mass% when the amount of oxides contained in the primary coating is 100 mass%, and the content of B contained in the base steel sheet is 0.50 to 12.00 mass% when the amount of oxides contained in the primary coating is 100 mass%. the sum of the B content contained in the primary coating and the B content contained in the primary coating is 0.20 to 5.00 mass%, a ratio RB of the B content contained in the base steel sheet to the B content contained in the primary coating and the base steel sheet satisfies RB ≥ 0.25, a ratio RT of the Ti content contained in the base steel sheet to the Ti content contained in the primary coating and the base steel sheet satisfies RT ≤ 0.75, and a ratio RB / RT of RB to RT satisfies RB / RT ≥ 0.80.
[0019] In order to solve the above-mentioned problems, according to another aspect of the present invention, there is provided a steel sheet for finish annealing that is applied to the production of the grain-oriented electrical steel sheet, the steel sheet containing, by mass%, C: 0.005% or less, Si: 2.5 to 4.5%, Mn: 0.01 to 0.15%, one or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, sol. Al: 0.005 to 0.050%, and N: 0.0030 to 0.0300%, with the balance being Fe and impurities. Consists of Provided is a steel sheet for finish annealing, comprising: a steel sheet; and an annealing separator layer adhering to a surface of the steel sheet and containing MgO, Ti, and B as main components, wherein, when the content of Ti contained in the annealing separator relative to the content of MgO is defined as CT, the content of B contained in the annealing separator layer relative to the content of MgO is defined as CB, and the content of B contained in an MgO raw material powder containing B, which is contained in an aqueous slurry that forms the annealing separator layer, is defined as CB', the following relationships are satisfied: CT: 0.50 to 6.00%, CB: 0.10 to 2.00%, CB' / CB: 0.05 to 0.60, and 2.2×CB / CT: 0.05 to 3.00.
[0020] In order to solve the above problems, according to another aspect of the present invention, An annealing separator applied to the production of the grain-oriented electrical steel sheet, Provided is an annealing separator containing MgO, Ti, and B as main components, wherein MgO is contained as a powder containing B, and Ti and B are each contained as particles containing at least Ti or B, and wherein, when the content of Ti relative to the content of MgO, the content of B relative to the content of MgO, and the content of B contained in the powder are defined as CT, CB, and CB', respectively, the annealing separator satisfies CT: 0.50 to 6.00%, CB: 0.10 to 2.00%, CB' / CB: 0.05 to 0.60, and 2.2×CB / CT: 0.05 to 3.00.
[0021] The particles containing at least Ti or B preferably further contain oxygen.
[0022] In order to solve the above-mentioned problems, according to another aspect of the present invention, there is provided a method for producing the grain-oriented electrical steel sheet, comprising the steps of: in mass%, C: 0.100% or less, Si: 2.5 to 4.5%, Mn: 0.01 to 0.15%, one or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, sol. Al: 0.005 to 0.050%, 、N :0.0030~0.0300%, One or more selected from the group consisting of Cu, Sb, and Sn: 0 to 0.30% in total, and one or more selected from the group consisting of Bi, Te, and Pb: 0 to 0.030% in total or less and the balance containing Fe and impurities, to produce a hot-rolled steel sheet; cold rolling the hot-rolled steel sheet at a cold rolling rate of 80% or more to produce a cold-rolled steel sheet; decarburization annealing the cold-rolled steel sheet to produce a decarburization annealed sheet; applying an aqueous slurry to a surface of the decarburization annealed sheet and drying it; and finish annealing the steel sheet after the aqueous slurry has dried, wherein the substance adhering to the surface of the steel sheet after the aqueous slurry has dried is the annealing separator.
[0025] In order to solve the above problems, according to another aspect of the present invention, there is provided a method for producing a steel sheet for finish annealing, comprising the steps of: C: 0.100% or less; Si: 2.5 to 4.5%; Mn: 0.01 to 0.15%; one or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total; sol. Al: 0.005 to 0.050% 、N :0.0030~0.0300%, One or more selected from the group consisting of Cu, Sb, and Sn: 0 to 0.30% in total, and one or more selected from the group consisting of Bi, Te, and Pb: 0 to 0.030% in total or less and the balance containing Fe and impurities, to produce a hot-rolled steel sheet; cold rolling the hot-rolled steel sheet at a cold rolling rate of 80% or more to produce a cold-rolled steel sheet; decarburization annealing the cold-rolled steel sheet to produce a decarburization annealed sheet; and applying an aqueous slurry to a surface of the decarburization annealed sheet and drying it, wherein the layer of a substance adhered to the steel sheet surface after the drying is the annealing separator layer. Effect of the Invention
[0026] The grain-oriented electrical steel sheet according to the present invention has excellent magnetic properties and excellent adhesion of the primary coating to the base steel sheet. The above-mentioned grain-oriented electrical steel sheet can be manufactured by the manufacturing method of the grain-oriented electrical steel sheet according to the present invention. The annealing separator according to the present invention is applied to the above-mentioned manufacturing method, thereby manufacturing the grain-oriented electrical steel sheet of the present invention. The steel sheet for finish annealing according to the present invention is for manufacturing the grain-oriented electrical steel sheet of the present invention. The manufacturing method of the steel sheet for finish annealing according to the present invention can manufacture the above-mentioned steel sheet for finish annealing. [Brief description of the drawings]
[0027] [Figure 1] FIG. 2 is a schematic diagram of a primary coating. [Diagram 2] FIG. 13 is a diagram illustrating a Gaussian filter applied to height information data obtained by a laser microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] A preferred embodiment of the present invention will be described in detail below with reference to the accompanying drawings. Fig. 1 is a schematic diagram of a primary coating of a grain-oriented electrical steel sheet according to this embodiment. Fig. 2 is a diagram explaining a Gaussian filter applied to height information data obtained by a laser microscope.
[0029] In this embodiment, the structure of the interface between the primary coating and the base steel sheet of a grain-oriented electrical steel sheet and the characteristics of the oxide on the surface are controlled and specified. In this embodiment, the primary coating is divided into two regions in the sheet thickness direction based on the shape characteristics shown typically in FIG. 1, and the structure in each region is specified. The primary coating is made of oxides. In the grain-oriented electrical steel sheet according to this embodiment, for example, as shown in FIG. 1, a primary coating 2 is formed on the surface of a base steel sheet 1. The primary coating presence region 10 in which the primary coating 2 exists is divided into a surface oxide layer region 11 and an indented oxide layer region 12 as shown in FIG. 1. The surface oxide layer region 11 is a region in the sheet thickness direction in which a primary coating portion (hereinafter, this may be referred to as "surface oxide") that relatively uniformly covers the surface of the base steel sheet 1 exists. The indented oxide layer region 12 is a region in the sheet thickness direction in which a primary coating portion (hereinafter, this may be referred to as "indented oxide") that is embedded in the base steel sheet exists. The reference depth H0 for dividing the two will be described later.
[0030] In this specification, the structure of the interface between the primary coating and the base steel sheet is defined by the morphological characteristics of the primary coating observed from the base steel sheet side. Details will be described later together with the measurement method. It should be noted that the structure of the interface between the primary coating and the base steel sheet, particularly the shape characteristics, are generally sometimes expressed using the term "root."
[0031] The interface between the primary coating of grain-oriented electrical steel sheet and the base steel sheet has an uneven shape due to inclusion oxides penetrating into the base steel sheet. When the penetration depth of the inclusion oxides into the base steel sheet becomes deeper and the number density increases, the adhesion of the primary coating to the base steel sheet increases due to the so-called anchor effect.
[0032] On the other hand, in the production of grain-oriented electrical steel sheets, if intercalated oxides penetrate too far into the steel sheet that becomes the base steel sheet, they will hinder grain growth during secondary recrystallization and domain wall motion during magnetization, resulting in deterioration of magnetic properties.
[0033] The primary coating also has the effect of applying tension to the steel sheet and reducing iron loss. To increase tension, it is desirable for the surface oxide layer region of the primary coating to be thick and have a high content of Mg2SiO4, which has a small linear expansion coefficient.
[0034] Based on the above, the present inventors have investigated and examined the magnetic properties of grain-oriented electrical steel sheets containing magnetic property improving elements, and the adhesion of primary coatings formed using annealing separators containing Ti compounds and B compounds. As a result, the present inventors have obtained the following findings. In this embodiment, the term "annealing separator" refers to a substance formed on the surface of a decarburized annealed sheet that is subjected to a finish annealing process, which is one of the manufacturing processes for grain-oriented electrical steel sheets, in order to impart an anti-seizure function during finish annealing. The layer of annealing separator formed on the surface of a decarburized annealed sheet is called an "annealing separator layer."
[0035] When a primary coating is formed by adding Ti and B to an annealing separator, the coating may have sufficient adhesion to shear processing, but the coating may become a major factor in degrading the properties of the base steel sheet. When the thickness of the coating is reduced to maintain the magnetic properties, the adhesion may actually deteriorate. The present inventors further investigated the effects of Ti and B in the annealing separator and obtained the following findings.
[0036] When the annealing separator contains Ti, the thickness of the intercalated oxide layer region becomes thicker. This improves the coating adhesion to shear processing. When the annealing separator contains B, the decrease in the thickness of the intercalated oxide phase layer due to the change in oxide morphology during annealing is slowed down, and the number density of the intercalated oxides increases, improving the coating adhesion to shear processing. Furthermore, among the contents of Ti and B, and the B contained in the annealing separator, when the content of B contained in the MgO raw material powder, which is one of the components constituting the annealing separator, and the content of B contained in the annealing separator are set to an appropriate ratio, the coating adhesion to bending processing is improved and the deterioration of magnetic properties is suppressed. At this time, the thickness of the surface oxide layer region of the primary coating becomes uniform, and the interface between the primary coating and the base steel (base steel sheet) has a roughness that suppresses the deterioration of magnetic properties while maintaining a complex form. The improvement in coating adhesion during bending is believed to be due to the fact that the thickness of the surface oxide layer becomes uniform, preventing localized stress concentration in thin areas of the surface oxide layer during bending. The improvement in magnetic properties is believed to be due to the fact that the amount of Mg2SiO4 phase in the surface oxide layer increases, increasing the tension acting on the steel sheet, and preventing the structure from becoming too deeply intricate, preventing the magnetic flux density and core loss properties from deteriorating.
[0037] Since the interface between the base steel sheet and the primary coating has a complex three-dimensional shape having irregularities as described above, an attempt was made to define the structural characteristics of the interface, which has a three-dimensional shape. Although the definition should essentially quantify the "three-dimensional structure", this was difficult because the structure is three-dimensional and complex. For this reason, the inventors attempted to project information on the interface structure onto a plane (projection plane) parallel to the steel sheet surface as described below, and to define the characteristics of the interface on the "projection plane" (characteristics on the projection plane). Then, it was confirmed that the effects of the grain-oriented electrical steel sheet, the steel sheet for finish annealing, the annealing separator, the method for manufacturing the grain-oriented electrical steel sheet, and the method for manufacturing the steel sheet for finish annealing according to the present embodiment can be evaluated and explained by quantitatively defining the "characteristics on the projection plane".
[0038] The grain-oriented electrical steel sheet according to the present embodiment, which is obtained based on these findings, has the following features. That is, when a primary coating mainly composed of Mg2SiO4 is formed using an annealing separator mainly composed of MgO and containing B and Ti, if the primary coating and the interface between the primary coating and the base steel sheet satisfy the characteristics shown in (1) and (2) below, the morphology of the intercalated oxide layer region and the surface oxide layer region will be appropriate, and it will be possible to achieve both adhesion of the primary coating to shear processing and bending processing and iron loss characteristics. (1) Average height H1 from H0 of the indented oxide layer region: 0.40-2.00 μm (2) Surface roughness Ra of primary coating / substrate interface: 0.30~4.00μm
[0039] Furthermore, it is a preferred embodiment that the primary coating contains B and Ti and satisfies the following (3) to (7). (3) The sum of the Ti content in the base steel sheet and the Ti content in the primary coating when the amount of oxide in the primary coating is taken as 100 mass%: 0.50 to 12.00% (4) The sum of the content of B contained in the base steel sheet and the content of B in the primary coating when the amount of oxide in the primary coating is taken as 100% by mass: 0.20 to 5.00% (5) The ratio of B present in the base steel sheet (B content of the steel sheet from which the primary coating has been peeled off / B content of the steel sheet with the primary coating) RB ≧ 0.25 (6) Ti content ratio in the base steel sheet (Ti content in the steel sheet from which the primary coating has been peeled off / Ti content in the steel sheet with the primary coating) RT≦0.75 (7) The ratio of B and Ti in the base steel plate R1:RB / RT≧0.80
[0040] The annealing separator capable of forming the above-mentioned primary coating satisfies the following conditions (10) to (13). (10) CT(%): 0.50~6.00% (11) CB(%): 0.10~2.00% (12) CB' / CB: 0.05-0.60, (13) 2.2×CB / CT:0.05~3.00, CT, CB, and CB' respectively represent the Ti content relative to the MgO content, the B content relative to the MgO content, and the B content contained in the MgO raw material powder, which is one of the components constituting the annealing separator, out of the B contained in the annealing separator.
[0041] The gist of the present invention obtained based on these findings is as follows. The grain-oriented electrical steel sheet according to the present invention comprises a base steel sheet containing, by mass%, C: 0.005% or less, Si: 2.5 to 4.5%, Mn: 0.01 to 0.15%, one or more elements selected from the group consisting of S and Se: 0.005% or less in total, sol.Al: 0.010% or less, and N: 0.0150% or less, with the balance containing Fe and impurities, and a primary coating formed on the surface of the base steel sheet and containing Mg2SiO4 as a main component, and the steel sheet including the base steel sheet and the primary coating contains, by mass%, one or more elements selected from the group consisting of S and Se: 0.005 to 0.050% in total, Al: 0.005 to 0.040%, and N: 0.0005 to 0.050%. In an unevenness distribution diagram of the primary coating at the interface between the primary coating and the base steel sheet, obtained by projecting the primary coating onto a plane parallel to the surface where the base steel sheet and the primary coating are laminated, the direction from the primary coating toward the base steel sheet is defined as a positive direction, H0 is the central position of the interface between the primary coating and the base steel sheet, and a region where the primary coating exists on the positive side of H0 is defined as an indented oxide layer region, the following are satisfied: (1) average distance H1 from H0 to an end face of the indented oxide layer region: 0.40 to 2.00 μm; and (2) surface roughness Ra of the primary coating at the interface between the primary coating and the base steel sheet (primary coating / base steel interface): 0.30 to 4.00 μm.
[0042] Further, a steel sheet for finish annealing for producing the above-mentioned grain-oriented electrical steel sheet comprises a steel sheet containing, by mass%, C: 0.100% or less, Si: 2.5 to 4.5%, Mn: 0.01 to 0.15%, one or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, sol. Al: 0.005 to 0.050%, and N: 0.003 to 0.0300%, with the balance containing Fe and impurities, and an annealing separator layer adhered to a surface of the steel sheet and containing MgO as a main component, wherein the annealing separator layer contains Ti and B, and when the content of MgO in the annealing separator is taken as 100% by mass, the contents of Ti and B in the annealing separator are respectively CT and CB, and the content of B contained as an impurity in MgO of the annealing separator is CB', (1) CT: 0.50-6.00% (2)CB: 0.10~2.00% (3) CB' / CB: 0.05-0.60 (4) 2.2×CB / CT: 0.05~3.00 Satisfy.
[0043] The annealing separator according to the present embodiment is an annealing separator mainly composed of MgO, and contains B and Ti. The raw powder containing B is preferably boric acid or a borate, and the raw powder containing Ti is preferably titanium oxide, titanium nitride, titanate, or the like. The raw powder containing MgO (MgO raw powder) contains B. In this specification, the term "main component" refers to a substance containing 50% by mass or more, preferably 70% by mass or more, and more preferably 90% by mass or more.
[0044] The method for producing a grain-oriented electrical steel sheet according to the present invention includes a step of producing a hot-rolled steel sheet by hot rolling a slab containing, by mass%, 0.100% or less C, 2.5 to 4.5% Si, 0.01 to 0.15% Mn, one or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, 0.005 to 0.050% sol. Al, and 0.0030 to 0.0300% N, with the balance containing Fe and impurities; The method includes a step of producing a cold-rolled steel sheet by cold rolling a rolled steel sheet at a cold rolling rate of 80% or more, a step of producing a decarburization annealed sheet by performing decarburization annealing on the cold-rolled steel sheet, a step of applying an aqueous slurry to a surface of the decarburization annealed sheet and drying it, and a step of performing finish annealing on the steel sheet after the aqueous slurry has been dried, wherein the substance adhered to the steel sheet surface after the drying is the annealing separator according to claim 4 or 5.
[0045] The method for producing the steel sheet for finish annealing includes the steps of: hot rolling a slab containing, by mass%, C: 0.100% or less, Si: 2.5 to 4.5%, Mn: 0.01 to 0.15%, one or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, sol. Al: 0.005 to 0.050%, and N: 0.0030 to 0.0300%, with the balance containing Fe and impurities; cold rolling the hot rolled steel sheet at a cold rolling rate of 80% or more to produce a cold rolled steel sheet; decarburization annealing the cold rolled steel sheet to produce a decarburization annealed sheet; and applying an aqueous slurry to a surface of the decarburization annealed sheet and drying it, wherein the layer of a substance adhered to the steel sheet surface after the drying is the annealing separator layer.
[0046] Although details will be described later, in this embodiment, in order to identify the structure of the interface between the primary coating of the grain-oriented electrical steel sheet and the base steel sheet, the surface of the side of the primary coating that was in close contact with the base steel sheet of the grain-oriented electrical steel sheet, that is, the surface of the primary coating that formed the interface between the primary coating and the base steel sheet, is observed. The observed surface is analyzed with a scanning confocal laser microscope to obtain the unevenness distribution of the interface (information in the depth direction of the interface). Furthermore, the observed surface is analyzed with SEM-EDS (scanning electron microscope-energy dispersive X-ray spectroscopy) to obtain the concentration distribution of various elements from the characteristic X-ray intensity. Since the observations with each of these instruments are performed in a direction perpendicular to the surface of the steel sheet from which it was peeled off, the information obtained is information on the primary coating having a three-dimensional structure projected onto a plane parallel to the steel sheet surface (hereinafter, sometimes simply referred to as a projection plane).
[0047] It should be noted at the outset that the following description of the interface in this specification uses characteristics on the above-mentioned "projected plane." For example, the "area" of the interface structure is the area obtained on the above-mentioned projected plane, and the presence area of an element is specified based on the concentration information of the element obtained on the above-mentioned projected plane.
[0048] However, the inventors have confirmed that the features obtained on these projection planes can adequately define the features of the grain-oriented electrical steel sheet, the steel sheet for finish annealing, the annealing separator, the manufacturing method of the grain-oriented electrical steel sheet, and the manufacturing method of the steel sheet for finish annealing according to this embodiment, and it goes without saying that explaining this embodiment using information on these projection planes does not detract from the significance of the present invention.
[0049] In this specification, unless otherwise specified, the expression "A to B" for numerical values A and B means "A or more and B or less." In such an expression, when a unit is added only to numerical value B, the unit is also applied to numerical value A.
[0050] Hereinafter, the grain-oriented electrical steel sheet, the manufacturing method of the grain-oriented electrical steel sheet, the annealing separator used in the manufacture of the grain-oriented electrical steel sheet, the steel sheet for finish annealing for manufacturing the grain-oriented electrical steel sheet, and the manufacturing method of the steel sheet for finish annealing according to the present embodiment will be described in detail. In this specification, % relating to the content of an element means % by mass unless otherwise specified.
[0051] [Grain-oriented electrical steel sheet] The grain-oriented electrical steel sheet according to this embodiment includes a base steel sheet and a primary coating formed on the surface of the base steel sheet.
[0052] [Base material steel plate] <Chemical composition of base steel plate> First, the chemical composition of the base steel sheet will be described. The chemical composition of the base steel sheet constituting the above-mentioned grain-oriented electrical steel sheet contains the following elements. However, the grain-oriented electrical steel sheet according to this embodiment is characterized in the primary coating, and the base steel sheet does not need to be special as long as it has the chemical composition described below. As will be described in the manufacturing method described later, the base steel sheet is manufactured by cold rolling using a hot-rolled steel sheet having a chemical composition described later, and since some components are lost during finish annealing, the chemical composition of the base steel sheet constituting the grain-oriented electrical steel sheet and the chemical composition of the hot-rolled steel sheet are significantly different.
[0053] C: 0.005% or less Carbon (C) is an element effective for controlling the structure until the completion of the decarburization annealing process in the manufacturing process, but if the C content exceeds 0.005%, the magnetic properties of the finished grain-oriented electrical steel sheet deteriorate. Therefore, the C content is 0.005% or less. The C content is preferably as low as possible. However, even if the C content is reduced to less than 0.0001%, the manufacturing cost increases and the above-mentioned effects do not change significantly. Therefore, the preferred lower limit of the C content is 0.0001%. The upper limit of the C content is preferably 0.004%, and more preferably 0.003%. Moreover, the lower limit of the C content is more preferably 0.0005%.
[0054] Silicon: 2.5 to 4.5% Silicon (Si) increases the electrical resistance of steel and reduces eddy current loss. If the Si content is less than 2.5%, the above effect cannot be sufficiently obtained. On the other hand, if the Si content exceeds 4.5%, the cold workability of the steel decreases. Therefore, the Si content is 2.5 to 4.5%. The preferred lower limit of the Si content is 2.8%, and more preferably 3.0%. The preferred upper limit of the Si content is 4.0%, and more preferably 3.8%.
[0055] Mn: 0.01 to 0.15% Manganese (Mn) combines with S and Se, which will be described later, to form MnS and MnSe during the manufacturing process. These precipitates function as inhibitors (suppressants of normal grain growth) and cause secondary recrystallization in steel. Mn also improves the hot workability of steel. If the Mn content is less than 0.01%, the above effects cannot be sufficiently obtained. On the other hand, if the Mn content exceeds 0.15%, secondary recrystallization does not occur and the magnetic properties of the steel may deteriorate. Therefore, the Mn content is 0.01 to 0.15%. The preferable lower limit of the Mn content is 0.02%, and more preferably 0.03%. The preferable upper limit of the Mn content is 0.13%, and more preferably 0.11%.
[0056] One or more elements selected from the group consisting of S and Se: 0.005% or less in total During the manufacturing process, sulfur (S) and selenium (Se) combine with Mn to form MnS and MnSe, which function as inhibitors. However, if the total content of these elements exceeds 0.005%, the remaining excess amount of inhibitors reduces the magnetic properties. Furthermore, surface defects occur in the grain-oriented electrical steel sheet due to the segregation of S and Se. Therefore, the total content of one or more elements selected from the group consisting of S and Se in the grain-oriented electrical steel sheet is 0.005% or less. The total of the S content and Se content in the grain-oriented electrical steel sheet is preferably as low as possible. However, even if the total of the S content and Se content in the grain-oriented electrical steel sheet is reduced to less than 0.0001%, the manufacturing cost will increase and the above-mentioned effects will not change significantly. Therefore, the preferred lower limit of the total content of one or more elements selected from the group consisting of S and Se in the grain-oriented electrical steel sheet is 0.0001%. The upper limit of the total content of at least one of S and / or Se is preferably 0.0045%, more preferably 0.004%, and the lower limit of the C content is more preferably 0.0002%.
[0057] Sol.Al: 0.010% or less During the manufacturing process of grain-oriented electrical steel sheet, acid-soluble aluminum (sol.Al) combines with N to form AlN and functions as an inhibitor. However, if the sol.Al content in the base steel sheet exceeds 0.010%, the inhibitor remains in excess in the base steel sheet, resulting in a decrease in magnetic properties. Therefore, the sol.Al content is 0.010% or less. A preferred upper limit of the sol.Al content is 0.006%, more preferably 0.004%. The sol.Al content is preferably as low as possible. However, even if the sol.Al content in the base steel sheet is reduced to less than 0.001%, the manufacturing cost will increase and the above-mentioned effects will not change significantly. Therefore, a preferred lower limit of the sol.Al content in the base steel sheet is 0.0005%. The lower limit of the sol.Al content is more preferably 0.001%. In this specification, sol.Al means acid-soluble Al. Therefore, the sol.Al content is the content of acid-soluble Al.
[0058] It should be noted that, as described later, the primary coating of the grain-oriented electrical steel sheet according to this embodiment may contain Al, but this Al is derived from the sol. Al contained in the base steel sheet. For this reason, at first glance, the fact that the sol. Al content of the base steel sheet is zero seems to contradict the presence of Al in the primary coating, but what is concentrated in the primary coating is the sol. Al contained in the steel sheet during production, and in the manufacturing method of the grain-oriented electrical steel sheet according to this embodiment, after the concentration of Al occurs, the sol. Al of the steel sheet is discharged outside the system by a high-temperature heat treatment also called "purification annealing" as part of the finish annealing process. For this reason, there is no contradiction between the absence of sol. Al in the final base steel sheet and the presence of Al derived from the base steel sheet in the final primary coating.
[0059] N: 0.0150% or less Nitrogen (N) combines with Al to form AlN during the manufacturing process of grain-oriented electrical steel sheet, and functions as an inhibitor. However, if the N content in the base steel sheet exceeds 0.0150%, the inhibitor remains in the grain-oriented electrical steel sheet in excess, resulting in a deterioration in magnetic properties. Therefore, the N content is 0.0150% or less. The preferred upper limit of the N content is 0.0080%, and more preferably 0.0060%. The N content is preferably as low as possible. However, even if the total N content in the base steel sheet is reduced to less than 0.0010%, the manufacturing cost will increase and the above-mentioned effects will not change significantly. Therefore, the preferred lower limit of the N content in the base steel sheet is 0.0010%.
[0060] The balance of the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to the present embodiment contains Fe and impurities. Here, the impurities refer to those elements that are mixed in from raw materials such as ore, scrap, or the manufacturing environment when the base steel sheet is industrially manufactured, or the following elements that remain in the steel without being completely purified during purification annealing, and are permissible within a range that does not adversely affect the grain-oriented electrical steel sheet according to the present embodiment.
[0061] Regarding impurities, copper (Cu), tin (Sn), antimony (Sb), bismuth (Bi), tellurium (Te) and lead (Pb) may all be contained as impurities. All of these elements reduce the magnetic properties of grain-oriented electrical steel sheets. Since these elements are impurities, it is preferable that the total content of these elements is as low as possible. As a rough target for the upper limit of the content, the total content of one or more elements selected from the group consisting of Cu, Sn and Sb is 0.30% or less, and the total content of one or more elements selected from the group consisting of Bi, Te and Pb is 0.020% or less. Note that Cu, Sn, Sb, Bi, Te and Pb are not essential in the base steel sheet, so the lower limit of the content is 0%.
[0062] When a coating is formed on the surface of the grain-oriented electrical steel sheet, the chemical composition of the base steel sheet is measured by completely removing the coating by physical polishing, pickling, etc. Measurement is performed by quantitative analysis using known methods such as ICP-MS (inductively coupled plasma mass spectrometry) and NDIR (non-dispersive infrared) gas detection.
[0063] [Primary coating] The characteristics of the primary coating structure are also the most important specification in this embodiment. As described above, due to the limitations of the measurement method, this characteristic is specified on the projected plane by projecting information on the interface between the primary coating and the base steel sheet onto a plane parallel to the steel sheet surface. Since it is considered important to understand this measurement method in order to grasp the characteristics of the primary coating, the measurement method will be described first.
[0064] <Method of measuring primary coating, especially interface structure> A grain-oriented electrical steel sheet with a primary coating formed on the surface of the base steel sheet is electrolyzed at a constant potential in an electrolytic solution so that only the base steel sheet dissolves, and then the primary coating is separated from the base steel sheet to prepare a sample for observation. Note that, in electrolysis for obtaining samples, since the interface is selectively electrolyzed, it is not necessary to electrolyze the entire base steel sheet, and an appropriate amount of electrolysis can be set. The amount of electrolysis is, for example, 1 cm of steel sheet area. 2 80C per cm 2) The primary coating may be separated by adhering the primary coating to the adhesive surface of a commercially available metal tape or the like and then peeling it off to remove the base steel sheet, thereby observing what remains on the tape, or by embedding the coating in paraffin and then removing the paraffin. Hereinafter, this separated coating may be referred to as the "interface observation sample", and the surface of the primary coating to be observed that was in contact with the base steel sheet may be referred to as the "observation surface".
[0065] Next, the interface observation sample is observed with various observation instruments from a direction perpendicular to the original steel sheet surface. Therefore, the data obtained from each instrument is the information held by the interface observation sample expanded onto a projection plane. The following explanation will be given on the premise that the data is on this projection plane.
[0066] An area of 20μm x 15μm or more is analyzed on the observation surface of the interface observation sample using a scanning confocal laser microscope (model number: VK9710, manufactured by Keyence) to obtain data on the interface unevenness on the projection plane. The scanning step is set to 0.1μm or less. The obtained unevenness data of 30,000 or more pieces (200 x 150 pieces) is smoothed once using a 3 x 3 Gaussian filter (Figure 2). Furthermore, automatic quadratic surface correction is performed on the smoothed unevenness data based on the center line in the width direction and the center line in the height direction, and this data is expanded on the projection plane to obtain a final unevenness distribution map of 200 x 150 pieces.
[0067] From the unevenness distribution map thus obtained, the median height H0 within the observation area, the average height H1 of the ingrown oxides, and the surface roughness Ra of the interface between the primary coating and the base steel sheet are determined by the following procedure.
[0068] H0 is the median height of the primary coating surface (interface between the primary coating and the base steel sheet) in the unevenness distribution diagram. Next, the average height H1 in the height region above H0 is determined. This H1 represents the average height of the intruded oxides. Ra is the surface roughness of the primary coating / base steel interface. Ra is determined by performing a surface roughness analysis in accordance with JIS B 0601-2001 over the entire region of the unevenness distribution diagram.
[0069] <Average value H1 of indented oxide height of primary coating and surface roughness Ra of primary coating> An example of a primary coating characteristic of this embodiment will be described below. The primary coating of this embodiment is a non-magnetic coating mainly composed of Mg2SiO4. The primary coating of this embodiment has a characteristic morphology at the interface with the base steel sheet, and can be specified by the height and roughness of intercalated oxides in particular, so these will be described.
[0070] The grain-oriented electrical steel sheet according to the present embodiment is characterized in that H1, which is the average height of the inclusion oxides, is 0.40 to 2.00 μm. If this value is less than 0.40 μm, the effect of improving the coating adhesion during bending cannot be obtained. If H1 exceeds 2.00 μm, the inclusion of the primary coating, which is a non-magnetic layer, into the base steel sheet increases, mainly deteriorating the magnetic flux density. The grain-oriented electrical steel sheet according to the present embodiment is characterized in that the surface roughness Ra of the primary coating / base steel interface is in the range of 0.30 to 4.00 μm. If this value is less than 0.30 μm, the effect of improving the coating adhesion during bending cannot be obtained. If Ra exceeds 4.00 μm, the movement of the magnetic domains is hindered, deteriorating the core loss characteristics.
[0071] <Chemical composition of the primary coating> The primary coating is mainly composed of oxides, and the oxides contain forsterite (Mg2SiO4) as a main component. More specifically, when the mass of the oxides in the primary coating is taken as 100%, the primary coating contains 50 to 98% of Mg2SiO4. The content of Mg2SiO4 is preferably 52 to 98%, and more preferably 54 to 98%. The primary coating may contain S, Se, Al, or N, as described later.
[0072] The remainder of the components contained in the primary coating are mainly oxides such as MgAl2O4 and sulfides such as MnS, which are generally known.
[0073] [Chemical composition of steel sheet with primary coating] In the present invention, the chemical compositions of S, Se, Al, and N of the grain-oriented electrical steel sheet on which the primary coating is formed are specified in addition to the chemical compositions in the base steel sheet described above. These elements fall within the following ranges as a result of the decomposition of MnS, MnSe, or AlN precipitates by finish annealing and concentration in the primary coating, thereby suppressing deterioration such as iron loss. As with the chemical composition of the base steel sheet, the chemical composition of the steel sheet with the primary coating may differ from the composition of the molten steel and the composition of the base steel sheet, since the components of the base steel sheet and the annealing separator layer are concentrated in the primary coating, and there are components lost from the steel sheet surface. It is also important to note that after the primary coating is formed on the grain-oriented electrical steel sheet, an insulating coating may be applied and dried to insulate the layers of the grain-oriented electrical steel sheet when they are stacked, so the chemical composition of the steel sheet with the primary coating must be measured without this insulating coating by the procedure described below. The term "steel sheet with a primary coating" used herein refers to a steel sheet that is composed of a base steel sheet and a primary coating.
[0074] When the total S and Se content of a steel sheet with a primary coating (the sum of the content of one or more elements selected from the group consisting of S and Se in the base steel sheet and the content of one or more elements selected from the group consisting of S and Se in the primary coating), the Al content (the sum of the Al content in the base steel sheet and the Al content in the primary coating), and the N content (the sum of the N content in the base steel sheet and the N content in the primary coating) are within the following ranges while satisfying the above-mentioned ranges of the content of each element in the base steel sheet, deterioration of the magnetic properties is suppressed. One or more elements selected from the group consisting of S and Se: 0.005 to 0.050% Al: 0.005 to 0.040% N: 0.0005~0.0200%
[0075] As mentioned above, the Al, N, S and Se contents of steel sheet with a primary coating are determined by removing the insulating coating that may contain Al, N, S and Se and measuring them. After final annealing, and before applying and drying the insulating coating, the contents can be determined by washing away excess annealing separator adhering to the surface of the steel sheet with water. In addition, since the chemical composition of the steel sheet with a primary coating does not change significantly during the process of applying and drying the insulating coating, it is also possible to immerse the steel sheet after applying and drying the insulating coating in hot alkali to remove only the insulating coating, and then measure the chemical composition by a known method.
[0076] When the mass of the oxide in the primary coating is taken as 100%, the Ti content (total of the Ti content in the base steel sheet and the Ti content in the primary coating) in the steel sheet with the primary coating is preferably 0.50 to 12.00%, and the total B content (total of the B content in the base steel sheet and the B content in the primary coating) in the steel sheet with the primary coating is preferably 0.20 to 5.00%. When the Ti and B contents are within these ranges, the coating adhesion to bending is improved, and excellent magnetic properties can be maintained. When the Ti and B contents in the steel sheet with the primary coating are less than 0.50% and 0.20%, respectively, when the mass of the oxide in the primary coating is taken as 100%, the effects of Ti and B in the annealing separator are not fully exhibited, and the coating adhesion to bending may not be improved. On the other hand, when the mass of the oxide of the primary coating is taken as 100%, if the contents of Ti and B in the steel sheet with the primary coating are more than 12.00% and more than 5.00%, respectively, the thickness of the intercalated oxide layer region becomes too thick, or the roughness of the intercalated oxide phase (the interface between the primary coating and the base steel sheet) becomes too high, which may significantly affect the magnetic properties. When the mass of the oxide of the primary coating is taken as 100%, the content of Ti in the steel sheet with the primary coating is more preferably 0.80 to 11.00%, and even more preferably 1.20 to 10.00%. When the mass of the oxide of the primary coating is taken as 100%, the content of B in the steel sheet with the primary coating is more preferably 0.30 to 4.50%, and even more preferably 0.40 to 4.20%.
[0077] As described above, when the mass of the oxide in the primary coating is taken as 100%, the content of B in the steel sheet with the primary coating is more preferably 0.30 to 4.50%, and further preferably 0.40 to 4.20%. B complicates the morphology of the inlaid oxide layer region and improves the coating adhesion against bending, so that it is contained in the above range in the steel sheet with the primary coating.
[0078] As described above, when the mass of the oxide in the primary coating is taken as 100%, the Ti content in the steel sheet with the primary coating is more preferably 0.80 to 11.00%, and further preferably 1.20 to 10.00%. Ti is contained in the above range in the steel sheet with the primary coating as a result of thickening the intercalated oxide layer region and improving the coating adhesion against shear processing.
[0079] The contents of Ti and B elements in a steel sheet with a primary coating, when the oxides in the primary coating are taken as 100 mass %, are determined as follows. First, the oxide content in the primary coating is calculated. Since the oxides in the primary coating are almost entirely composed of Mg2SiO4 and MgAl2O4, the oxide content in the primary coating may be calculated as the sum of the Mg2SiO4 content and the MgAl2O4 content. In this case, the Mg2SiO4 content and the MgAl2O4 content may be determined by considering that Al is contained as MgAl2O4 and the remaining Mg is contained as Mg2SiO4.
[0080] Here, the Al content as MgAl2O4 is determined as follows: A steel sheet on which a primary coating has been formed is used as a sample, and Al, Ti, and B are quantitatively analyzed by ICP-MS. O is quantitatively analyzed by NDIR gas detection. Also, a steel sheet from which the primary coating has been completely removed by physical polishing, pickling, or other means is used as a sample, and Ti, B, and Al are quantitatively analyzed by ICP-MS. O is quantitatively analyzed by NDIR gas detection. By subtracting the amounts of Al and O in the steel sheet from which the primary coating has been completely removed from the amounts of Al and O in the steel sheet on which a primary coating has been formed, C is obtained as the increase in Al and O concentration concentrated in the primary coating. Al , C O (% by mass) can be calculated.Al The content of MgAl2O4 in the steel sheet with the primary coating, C, is calculated by multiplying the coefficient by SP (% by mass) is calculated as follows: C SP =C Al × (molecular weight of MgAl2O4) / (2 × atomic weight of Al)%
[0081] Next, the content of Mg2SiO4 in the primary coating, C FO The O content C quantitatively analyzed by the above method is calculated as follows. O (mass%), the following calculation is performed to obtain the Mg2SiO4 content C FO Calculate the mass percentage. C FO =(C O -(C SP × 4 × atomic weight of O / molecular weight of MgAl2O4) × (molecular weight of Mg2SiO4 / (4 × atomic weight of O))
[0082] Since most of the O-enriched increment concentrated in the primary coating exists as Mg2SiO4 and MgAl2O4, it can be assumed that O is contained only in Mg2SiO4 and MgAl2O4. In addition, since most of Mg2SiO4 and MgAl2O4 exist in the primary coating, the O content C calculated from the quantitative analysis value is O can be regarded as the O content of the primary coating. Therefore, the O content C calculated from the quantitative analysis value O Using the above calculation, C FO can be regarded as the content of Mg2SiO4 in the primary coating.
[0083] Oxide content in the primary coating C OX (mass%) is C OX =C SP +C FO It is expressed as:
[0084] Here, the contents of Ti and B in the steel sheet with the primary coating of the grain-oriented electrical steel sheet according to this embodiment are the oxide amount C OXThe quantitative values of Ti and B in the steel sheet with the primary coating analyzed by ICP-MS are expressed as 100 / C OX It is calculated by multiplying
[0085] In addition, although details will be described later, in order for the primary coating to achieve the above-mentioned coating form, it is preferable to use an annealing separator containing B and Ti. In this case, B and Ti remain in the primary coating and the base steel after finish annealing.
[0086] <Presence and ratio of B and Ti in base steel plate> The characteristics of the B and Ti contents in the steel sheet with the primary coating of the grain-oriented electrical steel sheet according to this embodiment and the B and Ti contents in the base steel sheet will be described below. In the grain-oriented electrical steel sheet according to this embodiment, the ratio RB (abundance tendency ratio RB) of the content of B contained in the base steel sheet to the total content of B contained in the primary coating and the base steel sheet satisfies RB≧0.25, the ratio RT (abundance tendency ratio RT) of the content of Ti contained in the base steel sheet to the content of Ti contained in the primary coating and the base steel sheet satisfies RT≦0.75, and the ratio R1 of RB to RT satisfies R1≧0.80.
[0087] The presence tendency ratio RT of Ti contained in the base steel plate relative to the content of Ti contained in the primary coating and the base steel plate, the presence tendency ratio RB of B relative to the content of B contained in the primary coating and the base steel plate, and the presence tendency ratio R1 of B and Ti in the base steel plate are determined as follows.
[0088] A steel sheet from which the primary coating has been completely removed by physical polishing, pickling or other such means is used as a sample, and Ti and B are quantitatively analyzed by ICP-MS to obtain the B content CB1 (mass%) and Ti content CT1 (mass%). A steel sheet on which the primary coating has been formed is also used as a sample, and B and Ti are quantitatively analyzed by ICP-MS to obtain the B content CB2 and Ti content CT2. The presence tendency ratios of Ti and B in the base steel sheet are determined as follows, using CT1 and CT2, and CB1 and CB2 determined by the above means. B presence tendency ratio RB: CB1 / CB2 Ti existence tendency ratio RT:CT1 / CT2
[0089] The existence tendency ratio R1 is calculated as follows. R1:RB / RT
[0090] When the base steel sheet contains Ti, fine Ti compounds that deteriorate iron loss are precipitated, so it is desirable that the Ti existence tendency ratio RT is low. However, when a Ti compound is contained in the annealing separator to improve the coating adhesion, Ti may diffuse into the base steel sheet, and fine compounds (mainly TiN) may precipitate, which may deteriorate the iron loss. When a B compound is contained in the annealing separator at the same time as Ti, B diffuses into the parent phase (base steel sheet) instead of Ti, and coarse B-containing precipitates (mainly BN) that have little effect on iron loss are formed. When a B compound is contained in the annealing separator, the diffusion of Ti into the base steel sheet at low temperatures is suppressed. In addition, the impurity B in MgO contained in the annealing separator suppresses the diffusion of Ti into the base steel sheet from low to high temperatures. By effectively suppressing the diffusion of Ti into the base steel sheet at low and high temperatures, the diffusion of Ti into the base steel sheet can be suppressed. As a result, the existence tendency ratio RT of Ti in steel becomes smaller, and the existence tendency ratio RB of B increases. In other words, the abundance tendency ratio R1 is high, and the deterioration of iron loss is suppressed. Therefore, if the grain-oriented electrical steel sheet satisfies RT≦0.75, RB≧0.25, and RB / RT≧0.8, the deterioration of iron loss is small. The grain-oriented electrical steel sheet preferably satisfies RT≦0.66, and more preferably satisfies RT≦0.50. The grain-oriented electrical steel sheet preferably satisfies RB≧0.33, and more preferably satisfies RT≧0.50. The grain-oriented electrical steel sheet preferably satisfies RB / RT≧1.00, and more preferably satisfies RB / RT≧1.20.
[0091] In the grain-oriented electrical steel sheet according to the present embodiment, the primary coating / base steel interface maintains a complex shape while having a degree of roughness that suppresses deterioration of the magnetic properties. This prevents localized stress concentration in the thin surface oxide layer region. As a result, the coating adhesion during bending is improved.
[0092] Moreover, with the grain-oriented electrical steel sheet according to this embodiment, the amount of Mg2SiO4 phase in the surface oxide layer region increases, so that the tension acting on the steel sheet increases. Also, since the non-magnetic Mg2SiO4 does not form an excessively deep and complicated structure, it is possible to maintain the magnetic flux density and core loss characteristics. So far, the grain-oriented electrical steel sheet according to this embodiment has been described.
[0093] [Method of manufacturing grain-oriented electrical steel sheets] Next, an example of a method for manufacturing a grain-oriented electrical steel sheet according to the present embodiment will be described. As an example, the method for manufacturing a grain-oriented electrical steel sheet according to the present embodiment includes a steelmaking process, a hot rolling process, a hot-rolled sheet annealing process, a cold rolling process, a decarburization annealing process, an annealing separator layer forming process, a finish annealing process, an insulating coating forming process, and a magnetic domain control process. Each process will be described below. Note that the processing conditions for each of the following processes do not deviate from the general range and do not need to be special. A characteristic of the method for manufacturing a grain-oriented electrical steel sheet according to the present embodiment is the state of the steel sheet surface containing the annealing separator in the steel sheet before finish annealing, which is used to control the structure of the primary coating.
[0094] <Steelmaking process> In the steelmaking process, molten steel is produced by a conventional method such as the converter process, and a slab having the following chemical composition is produced by carrying out well-known refining and casting processes. Some of the elements in the chemical composition of the slab are removed to a certain extent from the steel components in the finish annealing process described below. In particular, S, Se, Al, N, etc., which function as inhibitors, are largely removed. Therefore, the chemical composition of the slab described here differs from the chemical composition of the final product. The chemical composition of the slab used in the manufacturing method of the grain-oriented electrical steel sheet according to this embodiment is described below.
[0095] C: 0.100% or less If the C content exceeds 0.100%, the time required for decarburization annealing becomes longer. In this case, the manufacturing cost increases and the productivity decreases. Therefore, the C content in the slab is 0.1% or less. If the C content is less than 0.005%, the dispersion state of precipitates such as MnS, MnSe, and AlN and the steel sheet grain structure after decarburization annealing are not uniformly obtained, and the Goss orientation concentration after secondary recrystallization may be deteriorated. Therefore, the C content is preferably 0.005% or more. The preferred upper limit of the C content in the slab is 0.092%, and more preferably 0.085%. The more preferred lower limit of the C content in the slab is 0.020%, and even more preferably 0.030%.
[0096] Silicon: 2.5 to 4.5% As explained in the section on the chemical composition of the finished grain-oriented electrical steel sheet, Si increases the electrical resistance of the steel, but if it is contained in excess, the cold workability decreases. If the Si content in the slab is 2.5 to 4.5%, the Si content of the grain-oriented electrical steel sheet after the finish annealing process will be 2.5 to 4.5%. The Si content is preferably 2.6 to 4.0%, and more preferably 2.8 to 3.8%.
[0097] Mn: 0.01 to 0.15% As explained in the section on the chemical composition of the finished grain-oriented electrical steel sheet, Mn combines with S and Se to form precipitates during the manufacturing process, and functions as an inhibitor. Mn also improves the hot workability of the steel. If the Mn content in the slab is 0.01-0.15%, the Mn content of the grain-oriented electrical steel sheet after the final annealing process will be 0.01-0.15%.
[0098] One or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total During the manufacturing process, sulfur (S) and selenium (Se) combine with Mn to form MnS and MnSe. Both MnS and MnSe function as inhibitors necessary to suppress grain growth during secondary recrystallization. If the total content of one or more elements selected from the group consisting of S and Se is less than 0.005%, the above effect is difficult to obtain. On the other hand, if the total content of one or more elements selected from the group consisting of S and Se exceeds 0.070%, secondary recrystallization does not occur during the manufacturing process, and the magnetic properties of the steel are deteriorated. Therefore, in the slab, the total content of one or more elements selected from the group consisting of S and Se is 0.005 to 0.070%. The preferred lower limit of the total content of one or more elements selected from the group consisting of S and Se is 0.008%, more preferably 0.012%. The preferred upper limit of the total content of one or more elements selected from the group consisting of S and Se is 0.6%, more preferably 0.05%.
[0099] Sol.Al: 0.005~0.050% During the manufacturing process, acid-soluble aluminum (sol.Al) bonds with N to form AlN. AlN functions as an inhibitor. If the sol.Al content in the slab is less than 0.005%, the above effect cannot be obtained. On the other hand, if the sol.Al content in the slab exceeds 0.050%, AlN becomes coarse. In this case, AlN does not function as an inhibitor easily, and secondary recrystallization may not occur. Therefore, the sol.Al content in the slab is 0.005 to 0.050%. The preferred upper limit of the sol.Al content in the slab is 0.040%, more preferably 0.035%. The preferred lower limit of the sol.Al content in the slab is 0.010%, more preferably 0.015%.
[0100] N: 0.0030~0.0300% In the manufacturing process, nitrogen (N) combines with Al to form AlN, which functions as an inhibitor. If the N content in the slab is less than 0.0030%, the above effect cannot be obtained. On the other hand, if the N content in the slab exceeds 0.0300%, AlN becomes coarse. In this case, AlN does not function as an inhibitor easily, and secondary recrystallization may not occur. Therefore, the N content in the slab is 0.0030 to 0.0300%. The preferred upper limit of the N content in the slab is 0.0200%, and more preferably 0.0150%. The preferred lower limit of the N content in the slab is 0.0040%, and more preferably 0.0060%.
[0101] The remainder of the chemical composition of the slab used in the production of the grain-oriented electrical steel sheet according to this embodiment contains Fe and impurities. Here, the term "impurities" refers to substances that are mixed in from raw materials such as ore and scrap, or the production environment, during industrial production of the slab, and are permissible within a range that does not adversely affect the slab of this embodiment.
[0102] Regarding optional elements, the slab according to the present embodiment may further contain one or more selected from the group consisting of Cu, Sn, and Sb in a total amount of 0.60% or less. All of these elements are optional elements. Therefore, the lower limit of the content of Cu, Sn, and Sb is 0%.
[0103] One or more elements selected from the group consisting of Cu, Sn, and Sb: 0 to 0.30% in total Copper (Cu), tin (Sn) and antimony (Sb) are optional elements and may not be contained. When one or more elements selected from the group consisting of Cu, Sn and Sb are contained, Cu, Sn and Sb all increase the magnetic flux density of the grain-oriented electrical steel sheet. If even a small amount of Cu, Sn and Sb is contained, the above effect can be obtained to a certain extent. However, if the total content of Cu, Sn and Sb exceeds 0.30%, the internal oxide layer formed on the cold-rolled steel sheet during decarburization annealing becomes difficult to form. In this case, the formation of the primary coating, which progresses during the finish annealing due to the reaction between MgO in the annealing separator and SiO2 in the internal oxide layer, is delayed. As a result, the adhesion of the primary coating decreases. In addition, Cu, Sn or Sb is likely to remain as an impurity element after purification annealing. As a result, the magnetic properties deteriorate. Therefore, the total content of one or more elements selected from the group consisting of Cu, Sn and Sb is 0 to 0.60%. The preferred lower limit of the total content of one or more elements selected from the group consisting of Cu, Sn, and Sb is 0.005%, more preferably 0.007%. The preferred upper limit of the total content of one or more elements selected from the group consisting of Cu, Sn, and Sb is 0.28%, more preferably 0.25%.
[0104] The slab according to this embodiment may further contain one or more elements selected from the group consisting of Bi, Te, and Pb in a total amount of 0.030% or less. All of these elements are optional elements. Therefore, the lower limit of the content of Bi, Te, and Pb is 0%.
[0105] One or more elements selected from the group consisting of Bi, Te, and Pb: 0 to 0.030% in total Although bismuth (Bi), tellurium (Te) and lead (Pb) are all optional elements, they are noteworthy elements in the present invention from the following viewpoint. These elements increase the magnetic flux density of grain-oriented electrical steel sheets. For this purpose, the preferred lower limit of the total content of one or more elements selected from the group consisting of Bi, Te and Pb is 0.0005%, and more preferably 0.001%.
[0106] On the other hand, if these elements are segregated on the surface during the finish annealing described later, the intercalated oxide layer region does not become thick, and the coating adhesion of the primary coating decreases. For this reason, in the past, in order to ensure coating adhesion, it was necessary to limit the content of the above elements to about 0.005% or less, despite the effect of increasing the magnetic flux density. The effect of the manufacturing method of the grain-oriented electrical steel sheet according to the present embodiment is to improve coating adhesion by changing the structure of the intercalated oxides, and is particularly effective when applying a manufacturing method containing these elements. When applying the manufacturing method of the grain-oriented electrical steel sheet according to the present embodiment, it is possible to ensure good coating adhesion even if these elements are 0.010% or more, or even 0.015% or more. However, if they are contained excessively, the decrease in adhesion cannot be avoided even with the effect of the manufacturing method of the grain-oriented electrical steel sheet according to the present embodiment, so the upper limit is set to 0.030%. The upper limit value of one or more elements selected from the group consisting of Bi, Te and Pb is preferably 0.028%, more preferably 0.022%.
[0107] <Hot rolling process> Next, the slab having the above-mentioned chemical composition is heated to completely dissolve precipitates such as MnS and AlN in the steel sheet. The heating temperature of the slab is, for example, 1280 to 1350° C. The heated slab is hot-rolled to produce a hot-rolled steel sheet.
[0108] The thickness of the hot-rolled steel sheet obtained through the hot rolling process and any hot-rolled sheet annealing is preferably, for example, 1.8 mm or more and 3.5 mm or less. If the thickness of the hot-rolled steel sheet is less than 1.8 mm, the steel sheet temperature after hot rolling becomes low, and the amount of precipitation of AlN in the steel sheet increases, making secondary recrystallization unstable, and the magnetic properties may be deteriorated in a grain-oriented electrical steel sheet with a final thickness of 0.23 mm or less, which is not preferable. If the thickness of the hot-rolled steel sheet exceeds 3.5 mm, the rolling load in the cold rolling process may be large, which is not preferable. By having the thickness of the hot-rolled steel sheet be 1.8 mm or more and 3.5 mm or less, the rolling load in the cold rolling process is suppressed, and the precipitation of AlN is suppressed, causing stable secondary recrystallization, which makes it possible to further improve the magnetic properties.
[0109] <Hot-rolled sheet annealing process and pickling process> The prepared hot-rolled steel sheet may be annealed as necessary (hot-rolled steel sheet annealing). The conditions for hot-rolled steel sheet annealing are, for example, an annealing temperature of 900 to 1000°C and an annealing time of 3 to 5 minutes. In addition, pickling may be performed before cold rolling of the hot-rolled steel sheet. When hot-rolled steel sheet annealing is performed, pickling may be performed before or after the hot-rolled steel sheet annealing. The pickling conditions are not particularly limited, and may be performed by a known method.
[0110] <Cold rolling process> Furthermore, cold rolling is performed to produce a cold-rolled steel sheet that becomes a base steel sheet. Cold rolling may be performed only once or multiple times. The cold rolling temperature is, for example, in the range of the coil temperature (atmospheric temperature) before cold rolling to about 300°C. When cold rolling is performed multiple times, intermediate annealing for the purpose of softening is performed after cold rolling, and then cold rolling is performed. Cold rolling is performed once or multiple times to produce a cold-rolled steel sheet having a product thickness (thickness as a product). The preferable upper limit of the cold rolling rate is 95%.
[0111] The cold rolling rate in one or more cold rolling passes is 80% or more, where the cold rolling rate (%) is defined as follows: Cold rolling rate (%) = (1-(thickness of cold rolled steel sheet after the last cold rolling / thickness of hot rolled steel sheet before the start of the first cold rolling)) x 100
[0112] <Decarburization annealing process> Next, the cold-rolled steel sheet produced by the cold rolling process is subjected to decarburization annealing, and nitriding annealing is performed as necessary. The decarburization annealing is performed in a well-known hydrogen-nitrogen-containing wet atmosphere. The decarburization annealing reduces the C concentration of the steel sheet after decarburization annealing in the grain-oriented electrical steel sheet to 0.005% or less, which is capable of suppressing magnetic aging deterioration. In the decarburization annealing, primary recrystallization is further generated in the steel sheet structure, and the processing strain introduced by the cold rolling process is released. Furthermore, in the decarburization annealing process, an internal oxide layer mainly composed of SiO2 is formed in the surface layer portion of the base steel sheet. The SiO2 formed here reacts with MgO in the aqueous slurry that is applied thereafter during the finish annealing, forming a primary coating whose shape is controlled. The annealing temperature in the decarburization annealing is well-known, and is, for example, 750 to 950°C. The holding time at the annealing temperature is, for example, 1 to 5 minutes.
[0113] In addition, rapid heating during the temperature rise process in the decarburization annealing step is also effective in improving the magnetic properties. This process is also called primary recrystallization annealing, and in the case of rapid heating, it is preferable to carry out it consecutively with the decarburization annealing.
[0114] <Annealing separator layer forming process> In this annealing separator layer forming process, an aqueous slurry containing compounds constituting the annealing separator is prepared, and the annealing separator layer is formed by applying the annealing separator to the decarburized annealed sheet and drying the annealing separator layer. The aqueous slurry (hereinafter, sometimes simply referred to as "slurry") is prepared by, for example, adding compounds constituting the annealing separator to pure water and stirring the mixture. The slurry is applied to the surface of the decarburized annealed sheet by a roll coater or a spray. The steel sheet to which the slurry is applied is inserted into a furnace maintained at 400 to 1000°C and held for 10 to 90 seconds to dry the slurry on the surface. At this time, the furnace conditions are controlled so that the temperature of the steel sheet itself rises only to about 400°C. Therefore, no change in the crystal structure such as recrystallization occurs in the cold-rolled steel sheet. What remains on the steel sheet surface at this point is the annealing separator according to this embodiment, and the layer formed by the annealing separator adhering to the surface of the steel sheet before the final annealing is the annealing separator layer.
[0115] In this embodiment, the annealing separator is specified by the substance attached to the surface of the steel sheet after the decarburization annealing process. The reason why the annealing separator is specified by the substance at the time of attachment to the surface of such an intermediate product (steel sheet after the decarburization annealing process) is to avoid the difficulty in identifying the invention depending on the time point at which the substance attached to the steel sheet surface is defined as the "annealing separator" since various compounds can be mixed in any order in the manufacturing process of the above-mentioned slurry, or different types of substances can be applied separately to function as the intended annealing separator. In other words, by defining the substance formed on the surface of the above-mentioned decarburization annealed sheet to which the finish annealing is performed as the annealing separator, it becomes possible to more easily identify the invention. Note that, basically, the annealing separator finally attached to the surface of the steel sheet before the finish annealing can be considered to be a simple mixture of various compounds used as its raw materials. The above-mentioned annealing separator and annealing separator layer belong to the present invention. This will be described later.
[0116] <Finishing annealing process> After the annealing separator is dried, finish annealing is performed. The steel sheet after drying the annealing separator (steel sheet for finish annealing) comprises, by mass%, a steel sheet containing 0.100% or less C, 2.5 to 4.5% Si, 0.01 to 0.15% Mn, 0.005 to 0.070% in total of one or more elements selected from the group consisting of S and Se, 0.005 to 0.050% sol. Al, and 0.0030 to 0.0300% N, with the balance containing Fe and impurities, and an annealing separator layer formed by the annealing separator described later.
[0117] In the final annealing, the decarburized annealed sheet on which the annealing separator layer is formed is soaked at an annealing temperature of, for example, 1150 to 1250°C. The soaking time is, for example, 15 to 30 hours. The atmosphere in the furnace during the final annealing is a well-known atmosphere, and may be, for example, a dry atmosphere, a wet atmosphere, dry hydrogen gas, or a mixed gas of nitrogen and hydrogen. In the final process of the final annealing step, in particular, some of the elements such as S, Al, and N that function as inhibitors are discharged out of the system. This process is sometimes called "purification (annealing)".
[0118] A primary coating containing Mg2SiO4 as a main component is formed on the surface of the grain-oriented electrical steel sheet manufactured by the above manufacturing process. In this case, by applying an annealing separator described later, the interface structure between the base steel sheet and the primary coating satisfies the requirements of the invention, and the coating adhesion is improved.
[0119] In addition, the decarburization annealing process and the finish annealing process remove each element in the chemical composition of the hot-rolled steel sheet to a certain extent from the steel components. In particular, S, Se, Al, N, etc., which function as inhibitors, are largely removed. Therefore, compared with the chemical composition of the hot-rolled steel sheet, the content of elements such as S, Se, Al, N, etc. in the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet is lower as described above. By carrying out the above manufacturing method using a hot-rolled steel sheet having the above chemical composition, a grain-oriented electrical steel sheet having a base steel sheet having the above chemical composition can be manufactured.
[0120] <Insulating film formation process> In one example of the method for producing the grain-oriented electrical steel sheet according to the present embodiment, an insulating coating forming step may be further performed after the final annealing step. In the insulating coating forming step, an insulating coating agent mainly composed of colloidal silica and phosphate is applied to the surface of the grain-oriented electrical steel sheet after the temperature drop in the final annealing step, and then baking is performed. As a result, an insulating coating, which is a tensile coating, is formed on the primary coating.
[0121] <Magnetic domain refinement process> In the method for producing a grain-oriented electrical steel sheet according to this embodiment, a well-known magnetic domain refinement process may be further carried out after cold rolling, decarburization annealing, finish annealing, or after the insulating coating formation process. In the magnetic domain refinement process, the surface of the grain-oriented electrical steel sheet is irradiated with a laser beam having a magnetic domain refinement effect, or grooves are formed on the surface. In this case, a grain-oriented electrical steel sheet with even better magnetic properties can be produced.
[0122] The method for producing a grain-oriented electrical steel sheet according to the present embodiment has been described above. Next, the annealing separator according to the present embodiment will be described.
[0123] [Annealing separator] The annealing separator according to the present embodiment contains magnesium oxide (MgO) as a main component, and further contains Ti and B. MgO is contained as a powder containing B, and Ti and B are each contained as particles containing at least Ti or B. In addition, when the Ti content, B content, and B content contained in the MgO raw material powder contained in the slurry to become the annealing separator are defined as CT, CB, and CB', respectively, with respect to the MgO content in the annealing separator, (10) CT: 0.50-6.00% (11)CB: 0.10~2.00% (12) CB' / CB: 0.05-0.60 (13) 2.2×CB / CT: 0.05~3.00% Satisfy.
[0124] <mgo> The annealing separator according to the present embodiment contains MgO as a main component. Therefore, MgO is contained in an amount of 50 mass% or more based on the mass of the solid content in the slurry. The content of MgO is preferably 70 mass% or more, and more preferably 90 mass% or more.
[0125] <ti> In the annealing separator according to the present embodiment, when the content of MgO in the annealing separator is 100% by mass and the content of Ti relative to the content of MgO is CT by mass, CT: 0.50~6.00% Meet the following.
[0126] In addition, Ti is preferably contained in the annealing separator as a compound containing oxygen or a compound that is oxidized to a compound containing oxygen during final annealing. The Ti compound is preferably, for example, TiO2 or Ti sulfate that is partially or completely converted to an oxide during the baking treatment (drying treatment) in the annealing separator layer formation step and the final annealing treatment.
[0127] In the final annealing, Ti promotes the reaction between MgO in the annealing separator and SiO2 in the surface layer of the decarburized annealed sheet formed by decarburization annealing, and promotes the formation of Mg2SiO4. If CT is less than 0.5%, the formation of Mg2SiO4 is delayed, and the coating adhesion improvement effect is not sufficiently obtained. On the other hand, if CT exceeds 6.0%, the coating becomes thick and the magnetic flux density decreases significantly. CT is preferably 0.80 to 5.50%, and more preferably 1.00 to 5.00%.
[0128] When the content of MgO in the annealing separator is taken as 100% by mass and the content of B relative to the content of MgO is taken as CB by mass, the following properties are satisfied: CB: 0.10~2.00% Meet the following.
[0129] During final annealing, B enhances the heat resistance of SiO2 and Mg2SiO4 in the surface layer of the base steel sheet formed by decarburization annealing, and maintains the complex morphology of Mg2SiO4. If CB is less than 0.10%, the formation of Mg2SiO4 is delayed and the morphology of the coating cannot be maintained in a complex form through aggregation. On the other hand, if CB exceeds 2.00%, the amount of B compounds formed in the base steel increases, deteriorating the iron loss characteristics.
[0130] In addition, when the MgO raw material powder serving as the annealing separator is taken as 100 mass % and the content of B contained in the MgO raw material powder is taken as CB', CB' and CB are CB' / CB:0.05~0.60 Satisfy the relationship.
[0131] The B in the oxygen-containing additive (MgO raw material powder) has the effect of accelerating the formation of Mg2SiO4 by promoting the reaction with SiO2. In addition, the B in the MgO raw material powder is supplied to the primary coating little by little at high temperatures, which has the effect of maintaining the complex coating morphology. Therefore, if there is an excessive amount of B in the MgO raw material powder, a large amount of B will be supplied to the substrate (steel sheet) at high temperatures. In this case, at low temperatures, Mg is supplied to SiO2 before B, and Mg2SiO4 is formed, so the complex coating morphology of the primary coating cannot be maintained. Furthermore, excessive B is supplied to the primary coating at high temperatures, which causes the morphology of the primary coating to deteriorate (become flat). Conversely, if the supply of B from the B-containing powder other than the MgO raw material powder is excessively large at low temperatures and the supply of B from the MgO raw material powder is small, the supply of B that stabilizes the primary coating cannot be maintained at high temperatures, and the supply of B is insufficient for the complex Mg2SiO4 formed at high temperatures, resulting in the aggregation of Mg2SiO4 and making it impossible to maintain the complex morphology of the primary coating. Therefore, it is necessary to balance the supply amounts of B in the MgO raw material powder and B outside MgO. If CB' / CB is between 0.05 and 0.60, the primary coating morphology is maintained. CB' / CB is preferably 0.08 to 0.55, more preferably 0.10 to 0.45.
[0132] In addition, the CB and CT are 2.2×CB / CT:0.05~3.00 Satisfy the relationship.
[0133] Both Ti and B are elements that form nitrides, but Ti precipitates finer than B, and therefore has a greater adverse effect on magnetic properties. When the B content of the mother steel sheet is higher than the Ti content of the mother steel sheet, coarse boron nitride precipitates instead of fine titanium nitride, or precipitates in combination with titanium, suppressing the effect on magnetic properties. On the other hand, when the amount of boron added is excessively low relative to titanium, boron does not exert its effect of maintaining a complex shape in the coating, and adhesion deteriorates. Therefore, 2.2×CB / CT is between 0.05 and 3.00. 2.2×CB / CT is preferably between 0.12 and 2.20, and more preferably between 0.20 and 1.80.
[0134] It is preferable that B is contained in the annealing separator as a compound containing oxygen or a compound that is oxidized and changed to a compound containing oxygen during final annealing. B is preferably, for example, BO or a boride that is partially or completely changed to an oxide during the baking treatment (drying treatment) and final annealing treatment in the annealing separator layer formation step.
[0135] To calculate the above CT and CB, the content of each element and the content of Mg are quantitatively analyzed by ICP-MS as a sample after the above-mentioned annealing separator layer formation process is completed and before final annealing, by rubbing the dried annealing separator with a brush or the like to remove it from the steel sheet. As for CB', the removed annealing separator or, if necessary, a powder obtained by separating only the MgO powder particles (MgO raw material powder) is quantitatively analyzed as a sample. Separation of only the MgO powder particles can be performed by applying a single or multiple known methods, such as separation by a specific gravity method using a known heavy liquid, classification, or extraction methods according to other chemical species. Quantitative analysis is performed using ICP-MS or EPMA (electron probe microanalyzer). EXAMPLES
[0136] An embodiment of the present invention will be described in detail below with reference to an example. The following example is an example for confirming the effects of the present invention, and is not intended to limit the present invention.
[0137] One aspect of the present invention relates to an annealing separator applied to a steel sheet before final annealing, which plays an important role in the formation of a primary coating, and the primary coating formed by the annealing separator, and the base steel sheet does not need to be special. For this reason, in this embodiment, the base steel sheet was manufactured under constant conditions (hot rolling, cold rolling, annealing conditions, etc.) that do not directly affect the effects of the invention. First, the common points among all the embodiments will be explained, and then the results of examining the effects of the invention by changing the conditions related to the formation of the primary coating in Examples 1 and 2 will be explained.
[0138] [Measurement and evaluation method] <Magnetic properties> A sample of 300mm length in the rolling direction and 60mm width was taken from the grain-oriented electrical steel sheet, and excited at 800A / m to determine the magnetic flux density B8. In addition, after baking an insulating coating mainly composed of colloidal silica and phosphate, the iron loss W17 / 50 was measured when excited at a maximum magnetic flux density of 1.7T and a frequency of 50Hz. If the magnetic flux density B8 is 1.92T or more and W17 / 50 is 0.750W / kg or less, the magnetic properties are considered to be excellent, and the evaluation result is given as "A" in Table 5. In addition, the difference between the magnetic flux density B8' and B8, which was obtained by exciting the steel sheet at 800A / m after the coating was peeled off, was calculated, and ΔB8=B8'-B8 was calculated. If ΔB8 is 0.030T or less, it was determined that the coating has excellent suppression of the decrease in magnetic flux density.
[0139] <Adhesion> A sample measuring 60 mm in length in the rolling direction and 15 mm in width was taken from the grain-oriented electrical steel sheet, and a bending test was performed with a curvature of 10 mm. The bending test was performed using a cylindrical mandrel bending tester, with the sample placed so that the axial direction of the cylinder coincided with the width direction of the sample. The surface of the sample after the bending test was observed, and the total area of the region where the primary coating remained without peeling was calculated. The primary coating remaining rate was calculated using the following formula. Primary coating remaining rate (%) = (total area of area where primary coating remains without peeling / area of sample surface) x 100
[0140] <Point Defect> A sample of 1 m in length in the rolling direction and 1 m in width was taken from the grain-oriented electrical steel sheet, and the occurrence frequency NP of point defects was determined by visual inspection. 2 If the number of point defects in the sample was five or less, it was determined that point defects had been suppressed.
[0141] <Primary coating structure> The primary coating was peeled off from the grain-oriented electrical steel sheet, and the structure and composition of the primary coating were investigated. The peeling method and measurement method were as described above, and the following values were ultimately obtained. (1) Average height H1 from H0 of the intruded oxide layer area (2) Surface roughness Ra of the primary coating / base steel interface (3) Ti content when the oxide in the primary coating is taken as 100 mass% (4) B content when the oxide in the primary coating is taken as 100 mass%
[0142] The analysis of the morphology of the primary coating was carried out by the following method. First, the grain-oriented electrical steel sheet on which the primary coating was formed on the surface was placed in an AA-based (10% acetylacetone) electrolyte with a potentiostat at an electrolysis rate of 80 C / cm so that only the base steel sheet would dissolve. 2 As a result of the above, a sample for observing the interface was obtained in which the surface of the primary coating that had been in close contact with the base steel sheet was exposed.
[0143] Next, an area of 20 μm × 15 μm or more was analyzed with a scanning confocal laser microscope (model number: VK9710, manufactured by Keyence) on the observation surface in the vertical direction from the side that was in contact with the base steel sheet in the primary coating, and unevenness data was obtained. In this case, the scanning step was set to 0.1 μm or less. The obtained unevenness data of 30,000 or more (200 × 150 pieces) was smoothed once using a Gaussian filter of size 3 × 3. Furthermore, automatic quadratic surface correction was performed on the unevenness data after smoothing, based on the center line in the width direction and the center line in the height direction, and this data was developed on a projection plane to obtain a final unevenness distribution map of 200 × 150 pieces.
[0144] From the obtained unevenness distribution map, the median height in the unevenness distribution map was set as H0, and the average height H1 in the height region above H0 was calculated. This H1 is the average height of the intruded oxides.
[0145] In addition, a surface roughness analysis was carried out in accordance with JIS B 0601-2001 over the entire area of the unevenness distribution map to determine the surface roughness Ra of the primary coating / base steel interface.
[0146] The B content and Ti content in the primary coating, relative to 100 mass % of the oxide, were quantitatively analyzed by ICP-MS.
[0147] <Annealing separator> The following values were obtained according to the above-mentioned method from the raw powder of the aqueous slurry and the steel sheet in a state in which the aqueous slurry before final annealing was dried. (5) Ti content CT(%) (6) B content CB (%) (7) B content in MgO CB' (%) (8) The ratio of impurity B in MgO to the amount of B in the annealing separator, CB' / CB: (7) / (6) (9) 2.2×CB / CT
[0148] To analyze the components of the annealing separator, after the annealing separator layer was formed and before final annealing, the dried annealing separator was rubbed off with a brush or the like, and this was used as a sample for quantitative analysis by ICP-MS.
[0149] Furthermore, the ratio of the B content CB1 in the base steel sheet to the B content CB2 contained in the primary coating and base steel sheet of the electrical steel sheet after the finish annealing (abundance tendency ratio RB), and the ratio of the Ti content CT1 in the base steel sheet to the Ti content CT2 contained in the primary coating and base steel sheet (abundance tendency ratio RT) were calculated by the following method. First, the steel sheet from which the primary coating was completely removed by means such as physical polishing or pickling was quantitatively analyzed using ICP-MS to obtain the B content CB1 and Ti content CT1 in the base steel sheet. Next, the steel sheet on which the primary coating was formed was used as a sample and quantitatively analyzed using ICP-MS to obtain the B content CB2 and Ti content CT2 contained in the primary coating and base steel sheet. The B abundance tendency ratio RB and Ti abundance tendency ratio RT were calculated using CT1 and CT2, and CB1 and CB2 obtained by the above means.
[0150] Furthermore, from the results of quantitative analysis of the components in the base steel plate by ICP-MS, the abundance tendency ratio R1, which is the B content relative to the Ti content in the base steel plate, was obtained.
[0151] [Manufacturing of decarburized annealed sheets] Molten steel having the chemical composition shown in Table 1 was produced in a vacuum melting furnace. Using the produced molten steel, slabs (steel numbers 1 to 27) were produced by a continuous casting method.
[0152] [Table 1]
[0153] Next, the slabs of Steel Nos. 1 to 27 were heated at 1350°C and hot rolled to produce hot rolled steel sheets having a thickness of 2.3 mm. In Steel No. 5, the Si content in the steel sheet was too high, so cracks occurred during hot rolling and production was not possible.
[0154] Each hot-rolled steel sheet was subjected to annealing treatment, and then pickled. The hot-rolled steel sheet was annealed at 1100°C for 5 minutes.
[0155] After pickling, each hot-rolled steel sheet was cold-rolled to produce a cold-rolled steel sheet having a thickness of 0.22 mm. The cold rolling rate was 90.4%.
[0156] Each cold-rolled steel sheet was subjected to decarburization annealing, which also served as primary recrystallization annealing. The annealing temperature in the decarburization annealing was 750 to 950° C., and the holding time at the annealing temperature was 2 minutes. In this manner, decarburized annealed sheets corresponding to steel numbers 1 to 4 and 6 to 27 were obtained (steel number 5 is missing because a hot-rolled steel sheet could not be obtained).
[0157] <Example 1> Using decarburized annealed sheets corresponding to steel numbers 1 to 27 (steel number 5 is a missing number) as materials, tests with test numbers A1 to A27 were carried out as follows. The raw materials constituting the annealing separator were 0.075% B and 0.020% MgO powder containing impurities, with 0.20% B2O3 powder, 0.3% BN powder, 1.2% TiO2 powder, 1.3% TiN powder, and 1.5% TiB2 powder added and mixed with pure water to prepare an aqueous slurry, which was applied to the front and back surfaces of each decarburized annealed sheet. In this case, the B content CB was 0.66% and the Ti content CT was 2.64%.
[0158] The decarburized annealed sheet with the aqueous slurry applied to its surface was held in a furnace at 900°C for 10 seconds to dry the aqueous slurry. The sheet was then subjected to finish annealing at 1200°C for 20 hours. Through the above manufacturing process, a grain-oriented electrical steel sheet having a base steel sheet and a primary coating was manufactured.
[0159] In the above manufacturing process, as with general grain-oriented electrical steel sheets, the composition of the base steel sheet differs from that of the raw slab or decarburization annealed sheet due to decarburization annealing and finish annealing (purification annealing). The chemical composition of the base steel sheet of the manufactured grain-oriented electrical steel sheet is shown in Table 2, and the evaluation results are shown in Table 3.
[0160] [Table 2]
[0161] [Table 3]
[0162] In test numbers A3, A4 and A6 to A17, the contents of C, Si, Mn, S, Se, Sol.Al or N were outside the range of appropriate amounts for forming precipitates necessary for secondary recrystallization to occur, and secondary recrystallization did not occur, so the magnetic flux density B8 value was significantly deteriorated and fell outside the range of the present invention.
[0163] In test number A19, the Cu content of the slab was too high, and the deterioration of the coating morphology during heat treatment progressed too quickly, so the additive effect was not sufficient. As a result, H1 was too small, and the coating adhesion was extremely poor, falling outside the scope of the present invention.
[0164] In test number A23, the total content of Cu and Sn in the slab was too high, and the deterioration of the coating morphology during heat treatment progressed too quickly, so the additive effect was not sufficient. As a result, H1 was too small and the coating adhesion was extremely poor, falling outside the scope of the present invention.
[0165] In test number A27, the total content of Bi, Te, and Pb in the slab was too high, and the deterioration of the coating morphology during heat treatment progressed too quickly, so the additives were not effective enough. As a result, H1 and Ra were too small, and the coating adhesion was poor, falling outside the scope of the present invention.
[0166] <Example 2> Using decarburized annealed sheets corresponding to steel numbers 1, 2, and 18 to 27 as materials, tests with test numbers B1 to B28 were carried out as follows. The aqueous slurry to be applied to each decarburized annealed sheet was prepared by mixing MgO, Ti compound and B compound with water so that the content of each element was as shown in Table 4. In this case, the type of compound and the content of each element (CT, CB) were changed. Table 4 shows the component contents of the annealing separator. Note that the MgO content in Table 4 is the content relative to the mass of the annealing separator. The contents of CB' and other impurities are the B content (mass%) in the MgO raw material powder contained in the aqueous slurry. The contents of components other than MgO and CB' indicate the content of each component relative to the MgO content.
[0167] The decarburized annealed sheet with the aqueous slurry applied to its surface was placed in a furnace at 900°C for 10 seconds to dry the aqueous slurry. The sheet was then subjected to finish annealing at 1200°C for 20 hours. By the above manufacturing process, a grain-oriented electrical steel sheet having a base steel sheet and a primary coating was manufactured. The results are shown in Table 5. In Table 5, the column "Oxide content C in the primary coating" indicates the amount of oxide in the primary coating. OX " is the amount of oxide calculated as Mg2SiO4 and MgAl2O4 from the amount of Mg and Al, C FO and C. SP The "B content" is the sum of the B content in the base steel sheet and the B content in the primary coating when the amount of oxides contained in the primary coating is taken as 100% by mass. The "Ti content" is the sum of the Ti content in the base steel sheet and the Ti content in the primary coating when the amount of oxides contained in the primary coating is taken as 100% by mass.
[0168] [Table 4]
[0169] [Table 5]
[0170] If the primary coating remaining rate was 90% or more, it was determined that the adhesion of the primary coating to the base steel sheet was excellent, and the coating adhesion evaluation result in Table 5 was given an "A", while if the primary coating remaining rate was less than 90%, the coating adhesion evaluation result was given a "B". In addition, if the magnetic flux density B8 was 1.92T or more, W17 / 50 was 0.750W / kg or less, and ΔB8 was 0.03T or less, it was determined that the magnetic properties were excellent, and the magnetic properties evaluation result in Table 5 was given an "A".
[0171] It can be seen that the one satisfying the requirements of the present invention has good coating adhesion and suppresses coating defects. It can also be seen that the magnetic flux density B8 is 1.92 or more, W17 / 50 is 0.750 W / kg or less, and ΔB8 is 0.03 T or less.
[0172] With reference to Table 5, in test numbers B17 to B25, the chemical composition was appropriate, and the conditions in the annealing separator (CT, CB, CB' / CB, 2.2×CB / CT) were appropriate. As a result, the average height H1 from H0 of the intercalated oxide layer region was in the range of 0.4 to 2.0 μm, and the surface roughness Ra of the primary coating / base steel interface was in the range of 0.30 to 4.00 μm, which were within the range of the present invention. As a result, in the grain-oriented electrical steel sheets of these test numbers, the magnetic flux density B8 was 1.92 T or more, W17 / 50 was 0.750 W / kg or less, and ΔB8 was 0.03 T or less, and excellent magnetic properties were obtained. Furthermore, the primary coating remaining rate was 90% or more, and the number of point defects was 5 / m 2 The results are as follows. Excellent coating adhesion and suppression of coating defects and deterioration of magnetic properties were demonstrated.
[0173] On the other hand, in test numbers B1 and B2, the total B content CB was too small, the morphology of the primary coating did not develop, and the average height H1 from H0 was less than 0.40. As a result, the primary coating remaining rate and the frequency of point defects were both outside the ranges of the present invention, and the coating adhesion and coating defects were inferior.
[0174] In test numbers B3 and B4, the total B content CB was too high, the morphology of the primary coating was overdeveloped, and the surface roughness Ra of the primary coating / base steel interface exceeded 4.00 μm. As a result, the iron loss W17 / 50 exceeded 0.75, and the magnetic properties were inferior.
[0175] In test numbers B5 and B6, the ratio CB' / CB of the amount of B impurities in MgO to the amount of B in the annealing separator was too small, and the supply of B was insufficient early during the final annealing, and the supply of B increased at high temperatures, resulting in a surface roughness Ra of less than 0.30 μm. As a result, the frequency of point defects was 5 pieces / m 2 The coating defects became noticeable.
[0176] In test numbers B7 and B8, the B abundance ratio CB' / CB was too large, so that B was not supplied in the middle and later stages of the final annealing, and the shape of the coating in the process of being formed could not be maintained, resulting in a surface roughness Ra of less than 0.30 μm. As a result, the frequency of point defects was 5 pieces / m 2 The coating defects became noticeable.
[0177] In test numbers B9 and B10, the Ti content CT relative to the MgO content in the annealing separator was too small, and H1 was less than 0.40, resulting in poor coating adhesion.
[0178] In test numbers B11 and B12, the Ti content CT was too high relative to the MgO content in the annealing separator, and the Ti content in the base steel sheet was too high, forming precipitates and resulting in poor magnetic properties.
[0179] In test numbers B13 and B14, the total content of B in the annealing separator was too small relative to the total content of Ti, and 2.2 × CB / CT was too small. As a result, RT exceeded 0.75, and the iron loss exceeded 0.75 W / kg, resulting in inferior results.
[0180] In test numbers B15 and B16, the total B content of the annealing separator was too high compared to the total Ti content, and 2.2 × CB / CT was too large. As a result, RB was less than 0.25, Ra was less than 0.30, and the coating adhesion was poor.
[0181] The above describes the embodiments of the present invention. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention. < / ti> < / mgo>
Claims
1. In mass percent, C: 0.005% or less, Si: 2.5-4.5%, Mn: 0.01 to 0.15%, One or more elements selected from the group consisting of S and Se: 0.005% or less in total; sol. Al: 0.010% or less, and N: 0.0150% or less, and the remainder being Fe and impurities; formed on the surface of the base steel plate, 2 SiO 4 and a primary coating containing as a main component, a total content of one or more elements selected from the group consisting of S and Se in the base steel sheet and a total content of one or more elements selected from the group consisting of S and Se in the primary coating is 0.005 to 0.050 mass%, the sum of the Al content in the base steel sheet and the Al content in the primary coating is 0.005 to 0.040 mass%, the sum of the N content in the base steel sheet and the N content in the primary coating is N: 0.0005 to 0.0200 mass%, In an unevenness distribution diagram of the primary coating at the interface between the primary coating and the base steel sheet, obtained by projecting the primary coating onto a plane parallel to the plane where the base steel sheet and the primary coating are laminated, the direction from the primary coating toward the base steel sheet is defined as a positive direction, the central position of the interface between the primary coating and the base steel sheet is defined as H0, and a region on the positive side of H0 where the primary coating is present is defined as an inclusion oxide layer region, the average distance H1 from H0 to the end face of the intercalated oxide layer region is 0.40 to 2.00 μm; a surface roughness Ra of the primary coating at the interface between the primary coating and the base steel sheet is 0.30 to 4.00 μm; the total of the Ti content in the base steel sheet and the Ti content in the primary coating is 0.50 to 12.00 mass% when the amount of oxides contained in the primary coating is taken as 100 mass%, the sum of the content of B contained in the base steel sheet and the content of B contained in the primary coating is 0.20 to 5.00 mass%, when the amount of oxides contained in the primary coating is 100 mass%, a ratio RB of the content of B contained in the base steel plate to the content of B contained in the primary coating and the base steel plate satisfies RB ≧ 0.25; a ratio RT of the content of Ti contained in the base steel sheet to the content of Ti contained in the primary coating and the base steel sheet satisfies RT≦0.75; A grain-oriented electrical steel sheet, characterized in that a ratio of RB to RT, RB / RT, satisfies RB / RT≧0.
80.
2. A steel sheet for finish annealing that is applied to the production of the grain-oriented electrical steel sheet according to claim 1, In mass percent, C: 0.005% or less, Si: 2.5-4.5%, Mn: 0.01 to 0.15%, One or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, sol. Al: 0.005 to 0.050%, and N: 0.0030-0.0300%, and the balance being Fe and impurities; and an annealing separator layer containing MgO as a main component and attached to the surface of the steel sheet, The annealing separator layer contains Ti and B, and when the content of Ti contained in the annealing separator layer relative to the content of MgO is defined as CT, the content of B contained in the annealing separator layer relative to the content of MgO is defined as CB, and the content of B contained in the B-containing MgO raw material that forms the annealing separator layer is defined as CB', CT: 0.50-6.00%, CB: 0.10-2.00%, CB' / CB: 0.05-0.60, (2.2×CB) / CT: 0.05-3.00, A steel sheet for finish annealing, characterized in that it satisfies the above.
3. An annealing separator applicable to the production of the grain-oriented electrical steel sheet according to claim 1, An annealing separator containing MgO, Ti, and B as main components, MgO is contained as a powder containing B, Each of Ti and B is contained as a particle containing at least Ti or B, The Ti content relative to the MgO content, the B content relative to the MgO content, and the B content contained in the powder are defined as CT, CB, and CB', respectively. CT: 0.50-6.00%, CB: 0.10 to 2.00%, and CB' / CB: 0.05-0.60, (2.2×CB) / CT: 0.05-3.00, An annealing separator characterized by satisfying the above.
4. The annealing separator according to claim 3, wherein the particles containing at least Ti or B further contain oxygen.
5. A method for producing the grain-oriented electrical steel sheet according to claim 1, In mass percent, C: 0.100% or less, Si: 2.5-4.5%, Mn: 0.01 to 0.15%, One or more elements selected from the group consisting of S and Se: 0.005 to 0.070% in total, sol. Al: 0.005 to 0.050%, N: 0.0030-0.0300%, One or more selected from the group consisting of Cu, Sb, and Sn: 0 to 0.30% in total; and One or more selected from the group consisting of Bi, Te, and Pb: 0 to 0.030% in total and a balance consisting of Fe and impurities, by hot rolling the slab to produce a hot rolled steel sheet; A step of producing a cold-rolled steel sheet by cold rolling the hot-rolled steel sheet at a cold rolling rate of 80% or more; A step of producing a decarburization annealed sheet by performing decarburization annealing on the cold-rolled steel sheet; A step of applying an aqueous slurry to a surface of the decarburized annealed sheet and drying the same; and performing a finish annealing process on the steel sheet after the aqueous slurry has been dried. A substance adhered to the surface of the steel sheet after the aqueous slurry is dried is A method for producing a grain-oriented electrical steel sheet, comprising the annealing separator according to claim 3.
6. The method for producing a steel sheet for finish annealing according to claim 2, In mass percent, C: 0.100% or less, Si: 2.5-4.5%, Mn: 0.01 to 0.15%, One or more elements selected from the group consisting of S and Se: 0.005 to 0.07% in total; sol. Al: 0.005 to 0.05%, N: 0.0030-0.0300%, One or more selected from the group consisting of Cu, Sb, and Sn: 0 to 0.30% in total; and One or more selected from the group consisting of Bi, Te, and Pb: 0 to 0.030% in total and a balance consisting of Fe and impurities, by hot rolling the slab to produce a hot rolled steel sheet; A step of producing a cold-rolled steel sheet by cold rolling the hot-rolled steel sheet at a cold rolling rate of 80% or more; and a step of producing a decarburization annealed sheet by performing decarburization annealing on the cold-rolled steel sheet. A step of applying an aqueous slurry to the surface of the decarburized annealed sheet and drying the same; a layer of a substance adhered to the surface of the steel sheet after drying is the annealing separator layer.
Citation Information
Patent Citations
Grain oriented electrical steel sheet having excellent magnetic characteristic
JP1986124584A
Production of ultrahigh magnetic flux density grain oriented silicon steel sheet
JP1994088171A
Production of grain oriented silicon steel sheet having ultrahigh magnetic flux density
JP1996269552A
Magnesium oxide for separation agent for annealing
JP2004176144A
Method for manufacturing grain-oriented electromagnetic steel sheet superior in magnetic property and in characteristics of coating
JP2005290446A