Surface-treated steel
A surface-treated steel material with a zinc-based plating layer and a P-enriched coating adjacent to the interface addresses paint adhesion and corrosion resistance issues by forming a complex salt with zinc, improving the material's protective properties.
Patent Information
- Application Number
- JP2020197243
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Conventional surface-treated steel materials face issues with poor paint adhesion and corrosion resistance due to the presence of an oxide film that interferes with the chemical conversion treatment, leading to uneven coating or peeling.
A surface-treated steel material with a zinc-based plating layer and a coating containing Si, C, O, P, and F, featuring a concentrated layer where the P concentration is higher than the average, adjacent to the interface with the plating layer, enhancing adhesion and corrosion resistance.
The solution provides improved paint adhesion and corrosion resistance by forming a complex salt with zinc at the interface, preventing air and water permeation, thereby enhancing the material's protective properties.
Smart Images

Figure 0007568916000008 
Figure 0007568916000009 
Figure 0007568916000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel material. [Background technology]
[0002] Conventionally, plated steel sheets (zinc-based plated steel sheets), in which a plating layer mainly made of zinc is formed on the surface of the steel sheet, have been used in a wide range of applications, such as automobiles, building materials, home appliances, etc. Normally, the surface of plated steel sheets is subjected to a chromium-free chemical conversion treatment to impart further corrosion resistance without the need for oil application. The chemical conversion coating formed by this chemical treatment is required to cover the surface uniformly, have excellent adhesion to the plating, and also have excellent corrosion resistance. However, because the surface of zinc-based plated steel sheets is covered with an oxide coating, even if an attempt is made to form a chemical conversion coating, the oxide coating becomes an obstacle and the adhesion of the chemical conversion coating is low, resulting in poor painting and uneven painting due to the reduced adhesion of the chemical conversion coating, or in some cases the chemical conversion coating peels off from the plating layer.
[0003] In response to such problems, for example, Patent Document 1 discloses that a coating having good adhesion to an adhesive and excellent corrosion resistance can be obtained by forming on a zinc-plated steel sheet a coating that contains acrylic resin, zirconium, vanadium, phosphorus, and cobalt, in which the area ratio of the acrylic resin is 80 to 100 area % in a region from the surface to 1 / 5 of the thickness of the film in the cross section of the coating, and the area ratio of the acrylic resin is 5 to 50 area % in a region consisting of a region from the film thickness center to 1 / 10 of the film thickness on the surface side and a region from the film thickness center to 1 / 10 of the film thickness on the plating layer side.
[0004] Patent Document 2 discloses a surface-treated steel sheet comprising a steel sheet and a resin-based chemical conversion coating, the resin-based chemical conversion coating having a matrix resin and colloidal particles of poorly soluble chromate dispersed in the matrix resin at a weight ratio in the range of 50 / 1 to 1 / 1, and the colloidal particles dispersed in the matrix resin have an average particle size of less than 1 μm. Patent Document 2 describes that this surface-treated steel sheet is excellent in chromium elution resistance, SST (240 hr), corrosion resistance of processed parts, and stability of treatment solution.
[0005] Patent Document 3 discloses a chemically treated steel sheet having a Zn-based plating layer containing 0.1 to 22.0 mass % Al, and a chemical conversion coating disposed on the Zn-based plating layer, the chemical conversion coating having a first chemical conversion layer disposed on the surface of the Zn-based plating layer and containing V, Mo, and P, and a second chemical conversion layer disposed on the first chemical conversion layer and containing a Group 4A metal oxoacid salt, the ratio of pentavalent V to total V in the chemical conversion coating being 0.7 or more. Patent Document 3 discloses that this chemically treated steel sheet is a chemically treated steel sheet made from a Zn-based plated steel sheet, can be produced by drying an applied chemical conversion treatment solution at a low temperature in a short time, and has excellent corrosion resistance and blackening resistance.
[0006] Patent Document 4 describes a method for treating a steel material by applying to a surface thereof (1) a silane coupling agent (A) containing one amino group in the molecule and a silane coupling agent (B) containing one glycidyl group in the molecule in a solid content mass ratio [(A) / (B)] of 0.5 to 1.7, which is obtained by applying to the surface of the steel material (2) a silane coupling agent (A) containing one amino group in the molecule and a silane coupling agent (B) containing one glycidyl group in the molecule. 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3(a) an organosilicon compound (W) having an average molecular weight of 1,000 to 10,000 and containing two or more functional groups (a) represented by the formula (a) (each of which independently represents an alkoxy group or a hydroxyl group, at least one of which represents an alkoxy group) and one or more hydrophilic functional groups (b) selected from a hydroxyl group (other than those that may be contained in the functional group (a)) and an amino group; (b); (c); (d); and (e); and (9) a surface-treated steel material is disclosed which forms a composite coating containing the following components of the composite coating: (6) the solid content mass ratio of the organosilicon compound (W) to the fluoro compound (X) [(X) / (W)] is 0.02 to 0.07, (7) the solid content mass ratio of the organosilicon compound (W) to the phosphoric acid (Y) [(Y) / (W)] is 0.03 to 0.12, (8) the solid content mass ratio of the organosilicon compound (W) to the vanadium compound (Z) [(Z) / (W)] is 0.05 to 0.17, and (9) the solid content mass ratio of the fluoro compound (X) to the vanadium compound (Z) [(Z) / (X)] is 1.3 to 6.0. Patent Document 4 discloses that this surface-treated steel material satisfies all of the requirements for corrosion resistance, heat resistance, fingerprint resistance, electrical conductivity, paintability, and resistance to black residue during processing.
[0007] However, in recent years, increasingly more stringent quality requirements have been placed on chemical conversion coatings, which have created a demand for better corrosion resistance, including corrosion resistance after drawing, and paint adhesion. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 6191806 [Patent Document 2] International Publication No. 97 / 00337 [Patent Document 3] Patent No. 6272207 [Patent Document 4] Patent No. 4776458 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide a surface-treated steel material that is excellent in paint adhesion and corrosion resistance. [Means for solving the problem]
[0010] The present inventors have investigated a method for improving corrosion resistance without reducing paint adhesion, and have found that paint adhesion and corrosion resistance can be improved by distributing optimal components in the cross-sectional direction for the components constituting the matrix of a coating (e.g., a chemical conversion coating) formed on the surface of a plating layer.
[0011] The present invention has been made in view of the above findings. The present invention relates to the following. [1] A steel sheet, a zinc-containing plating layer formed on the steel sheet, and a coating formed on the plating layer, the coating containing Si, C, O, P, F, and Zn as constituent elements, the coating having a concentrated layer in a thickness direction in which the P concentration is higher than the average P concentration in the range from the surface of the coating to the interface between the coating and the plating layer, the concentrated layer being adjacent to the interface with the plating layer, and when EDS line analysis is performed on the P concentration from the surface of the coating to the interface between the coating and the plating layer, the concentrated layer shows a maximum P concentration in the concentrated layer. When an EDS line analysis is performed on the concentration of F from the surface of the coating to the interface between the coating and the plating layer, a maximum F concentration is observed in the concentrated layer, and the ratio of the maximum F concentration to the average F concentration in the range from the surface of the coating to the interface between the coating and the plating layer is 1.5 or more and 2.3 or less, and the chemical composition of the plating layer is, in mass %, Al: 4.0% to less than 25.0%, Mg: 0% to less than 12.5%, Sn: 0% to 20%, Bi: 0% to less than 5.0%, In: 0% to less than 2.0%, and Ca: 0% to 3. 0%, Y: 0% to 0.5%, La: 0% to less than 0.5%, Ce: 0% to less than 0.5%, Si: 0% to less than 2.5%, Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25%, Ni: 0% to less than 0.25%, Co: 0% to less than 0.25%, V: 0% to less than 0.25%, Nb: 0% to less than 0.25%, Cu: 0% to less than 0.25%, Mn: 0% to less than 0.25%, Fe: 0% to 5.0%, Sr: 0% to less than 0.5%, Sb: 0% to less than 0.5%, Pb: 0% to less than 0.5%, B: 0% to less than 0.5%, and the balance: Zn and impurities. Surface treated steel. [2] The surface-treated steel material according to [1], wherein the ratio of the maximum value to the average concentration of P is 1.2 or more and 2.0 or less. 。 [ 3 ] The thickness of the concentrated layer is 5 nm or more and 100 nm or less, [1] or [2] The surface-treated steel material described above. [ 4]When EDS line analysis is performed on the concentration of Zn from the surface of the coating to the interface between the coating and the plating layer, Zn is continuously detected, and the concentration of Zn is 1.0 atomic % or more,[1] to [ 3 ] The surface-treated steel material according to any one of the preceding claims. 。 Effect of the Invention
[0012] According to the present invention, it is possible to provide a surface-treated steel material having excellent paint adhesion and corrosion resistance. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a cross-sectional schematic diagram of a surface-treated steel material according to the present embodiment. [Figure 2A] 1 is a HAAD-STEM image of a region including a plating layer and a coating in a cross section of a surface-treated steel material according to an embodiment of the present invention. [Figure 2B] 2B is a BF-STEM image of a region including the plating layer and coating (same field of view as FIG. 2A) of a cross section of the surface-treated steel material according to the present embodiment. [Diagram 3] FIG. 2 is a diagram showing an example of the results of EDS line analysis of Si, C, O, P, F and Zn for a cross section of a surface-treated steel material according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, a surface-treated steel material according to one embodiment of the present invention (a surface-treated steel material according to this embodiment) will be described. As shown in FIG. 1, the surface-treated steel material 1 according to this embodiment has a steel sheet 11, a zinc-containing plating layer 12 formed on the steel sheet 11, and a coating 13 formed on the plating layer 12 and containing Si, C, O, P, F and Zn as constituent elements. Furthermore, the coating 13 has a concentrated layer in the thickness direction where the P concentration is higher than the average P concentration in the coating (from the surface of the coating 13 to the interface between the coating 13 and the plating layer 12). Moreover, this concentrated layer is present on the interface side of the coating 13 between the coating 13 and the plating layer 12 (more specifically, at a position adjacent to the interface between the coating 13 and the plating layer 12). Furthermore, in the surface-treated steel material according to this embodiment, when an EDS line analysis is performed on the P concentration from the surface of the coating 13 to the interface between the coating 13 and the plating layer 12, the P concentration shows a maximum value within the concentrated layer. 1, the plating layer 12 and the coating 13 are formed on only one side of the steel sheet 11, but they may be formed on both sides. In addition, a protective layer 14 may be formed on the coating 13.
[0015] The steel sheet 11, the plating layer 12, and the coating 13 will be described below.
[0016] <Steel plate> The surface-treated steel material 1 according to this embodiment has excellent paint adhesion and corrosion resistance due to the plating layer 12 and the coating 13. Therefore, there are no particular limitations on the steel sheet 11. The steel sheet 11 may be determined depending on the product to which it is applied and the required strength, sheet thickness, etc., and for example, a hot-rolled steel sheet as described in JIS G3193:2008 or a cold-rolled steel sheet as described in JIS G3141:2017 can be used.
[0017] <Plating layer> The plating layer 12 of the surface-treated steel material 1 according to this embodiment is formed on the surface of the steel sheet 11 and is a zinc-based plating layer that contains zinc.
[0018] There are no limitations on the chemical composition of the plating layer 12 as long as it is a zinc-based plating layer. However, the chemical composition may be as follows: Al: 4.0% to less than 25.0%, Mg: 0% to less than 12.5%, Sn: 0% to 20%, Bi: 0% to less than 5.0%, In: 0% to less than 2.0%, Ca: 0% to 3.0%, Y: 0% to 0.5%, La: 0% to less than 0.5%, Ce: 0% to less than 0.5%, Si: 0% to less than 2.5%, Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25%, Ni: 0% to less than 0.25%. The composition is preferably composed of less than 0.25% Co, 0% to less than 0.25% V, 0% to less than 0.25% Nb, 0% to less than 0.25% Cu, 0% to less than 0.25% Mn, 0% to less than 0.25% Fe, 0% to less than 0.5% Sr, 0% to less than 0.5% Sb, 0% to less than 0.5% Pb, 0% to less than 0.5% B, and the balance being Zn and impurities, as this has the effect of improving corrosion resistance more significantly.
[0019] The reasons for the preferred chemical composition of the plating layer 12 will be described below. In the following, the numerical ranges indicated with "to" basically include the numerical values at both ends as the lower and upper limits, but when a numerical value is described as less than or greater than, the numerical value is not included as the lower or upper limit. That is, for example, 0% to 20% indicates 0% or more and 20% or less, and 4.0% to less than 25.0% indicates 4.0% or more and less than 25.0%. Moreover, unless otherwise specified, % regarding the chemical composition of the plating layer is % by mass.
[0020] [Al: 4.0% to less than 25.0%] Al is an element effective for improving the corrosion resistance of a zinc-based plating layer. In order to fully obtain this effect, it is preferable that the Al content be 4.0% or more. On the other hand, if the Al content is 25.0% or more, the corrosion resistance of the cut end surface of the plating layer decreases, so the Al content is preferably less than 25.0%.
[0021] The plating layer 12 may contain Al, with the remainder being Zn and impurities. However, if necessary, it may further contain the following elements. The following elements do not necessarily have to be contained, so the lower limit is 0%.
[0022] [Mg: 0% to less than 12.5%] Mg is an element that has the effect of increasing the corrosion resistance of the plating layer. In order to fully obtain this effect, it is preferable that the Mg content be more than 1.0%. On the other hand, if the Mg content is 12.5% or more, the effect of improving corrosion resistance becomes saturated and the workability of the coating layer may decrease. In addition, problems in manufacturing such as an increase in the amount of dross generated in the coating bath may occur. Therefore, it is preferable that the Mg content is less than 12.5%.
[0023] [Sn:0%~20%] [Bi: 0% to less than 5.0%] [In: 0% to less than 2.0%] These elements contribute to improving corrosion resistance and sacrificial corrosion protection. Therefore, any one or more of them may be contained. To obtain the above effects, the content of each is preferably 0.05% or more. Among these, Sn is preferred because it is a low melting point metal and can be easily incorporated into the plating bath without impairing the properties of the bath. On the other hand, if the Sn content exceeds 20%, the Bi content is 5.0% or more, or the In content is 2.0% or more, the corrosion resistance decreases. Therefore, it is preferable that the Sn content is 20% or less, the Bi content is less than 5.0%, and the In content is less than 2.0%, respectively.
[0024] [Ca: 0%~3.0%] Ca is an element that reduces the amount of dross that is easily formed during operation and contributes to improving the productivity of plating. Therefore, Ca may be contained. To obtain this effect, the Ca content is preferably 0.1% or more. On the other hand, if the Ca content is high, the corrosion resistance of the flat parts of the plating layer itself tends to deteriorate, and the corrosion resistance around the welded parts may also deteriorate. Therefore, the Ca content is preferably 3.0% or less.
[0025] [Y:0%~0.5%] [La: 0% to less than 0.5%] [Ce: 0% to less than 0.5%] Y, La, and Ce are elements that contribute to improving corrosion resistance. To obtain this effect, it is preferable to contain at least one of these elements in an amount of at least 0.05% each. On the other hand, if the contents of these elements are excessive, the viscosity of the coating bath increases, making it difficult to prepare the coating bath itself, and there is a concern that it may not be possible to produce steel products with good coating properties. Therefore, it is preferable to keep the Y content at 0.5% or less, the La content at less than 0.5%, and the Ce content at less than 0.5%.
[0026] [Si: 0% to less than 2.5%] Si is an element that contributes to improving corrosion resistance. In addition, when forming a plating layer on a steel sheet, Si is also an element that has the effect of suppressing the formation of an excessively thick alloy layer between the steel sheet surface and the plating layer, thereby enhancing the adhesion between the steel sheet and the plating layer. To obtain these effects, the Si content is preferably 0.1% or more, and more preferably 0.2% or more. On the other hand, if the Si content is 2.5% or more, excessive Si is precipitated in the plating layer, which not only reduces the corrosion resistance but also reduces the workability of the plating layer. Therefore, it is preferable that the Si content is less than 2.5%. The Si content is more preferably 1.5% or less.
[0027] [Cr: 0% to less than 0.25%] [Ti: 0% to less than 0.25%] [Ni: 0% to less than 0.25%] [Co: 0% to less than 0.25%] [V: 0% to less than 0.25%] [Nb: 0% to less than 0.25%] [Cu: 0% to less than 0.25%] [Mn: 0% to less than 0.25%] These elements contribute to improving corrosion resistance. In order to obtain this effect, it is preferable that the content of one or more of these elements is 0.05% or more. On the other hand, if the content of these elements is excessive, the viscosity of the coating bath increases, making it difficult to prepare the coating bath itself, and there is a concern that it may not be possible to produce steel products with good coating properties. Therefore, it is preferable to set the content of each element to less than 0.25%.
[0028] [Fe:0%~5.0%] Fe is mixed into the plating layer as an impurity when the plating layer is manufactured. It may be contained up to about 5.0%, but within this range, the adverse effect on the effect of the surface-treated steel material according to the present embodiment is small. Therefore, it is preferable to set the Fe content to 5.0% or less.
[0029] [Sr: 0% to less than 0.5%] [Sb: 0% to less than 0.5%] [Pb: 0% to less than 0.5%] When Sr, Sb, and Pb are contained in the plating layer, the appearance of the plating layer changes, spangles are formed, and an improvement in metallic luster is confirmed. To obtain this effect, it is preferable that the content of one or more of Sr, Sb, and Pb is 0.05% or more. On the other hand, if the content of these elements is excessive, the viscosity of the coating bath increases, making it difficult to prepare the coating bath itself, and there is a concern that it may not be possible to produce steel products with good coating properties. Therefore, it is preferable to set the content of each element to less than 0.5%.
[0030] [B: 0% to less than 0.5%] When B is contained in the plating layer, it combines with Zn, Al, Mg, etc. to form various intermetallic compounds. These intermetallic compounds have the effect of improving LME. To obtain this effect, it is preferable to set the B content to 0.05% or more. On the other hand, if the B content is excessive, the melting point of the plating increases significantly, which may lead to deterioration in plating operability and failure to obtain a surface-treated steel product with good plating properties. Therefore, it is preferable to set the B content to less than 0.5%.
[0031] The coating weight of the plating layer 12 is not limited, but is set to 10 g / m 2 On the other hand, the coating weight is preferably 200 g / m or more. 2 If the coating weight exceeds 200g / m, the corrosion resistance will saturate and it will be economically disadvantageous. 2 It is preferable that:
[0032] <Coating> [Contains Si, C, O, P, F, and Zn as constituent elements] The coating 13 of the surface-treated steel material according to this embodiment is obtained by applying a treatment liquid containing a silane coupling agent, a fluoride, a phosphate, or other P compound onto a zinc-containing plating layer under specified conditions, and then drying. Therefore, the coating 13 of the surface-treated steel material according to this embodiment contains Si, C, and O derived from the silane coupling agent, P derived from the P compound, F derived from the fluoride, and Zn dissolved from the plating layer. Furthermore, the coating 13 may contain Zr or V derived from a Zr compound or a V compound, as necessary.
[0033] The coating weight is 0.05 to 2.0 g / m 2 It is preferable that the thickness is 0.2 to 1.0 g / m 2 More preferably, the thickness is 0.3 to 0.6 g / m 2 It is most preferable that the coating weight is 0.05 g / m 2 If it is less than 2.0 g / m, the surface of the steel material cannot be covered and the corrosion resistance is significantly reduced, which is not preferable. 2 If it is larger, the resistance to black scum during processing decreases, which is undesirable.
[0034] [In the thickness direction, there is a concentrated layer where the P concentration is higher than the average P concentration in the range from the surface of the coating to the interface between the coating and the plating layer] [The concentrated layer exists adjacent to the interface with the plating layer] [When EDS line analysis was performed on the P concentration from the surface of the coating to the interface between the coating and the plating layer, the maximum P concentration was observed in the concentrated layer.] As a result of the inventors' investigations, it was found that for the coating formed on the plating layer of surface-treated steel, the paint adhesion and corrosion resistance can be improved by distributing the optimal components constituting the matrix in the thickness direction. More specifically, in the thickness direction, at the interface side of the coating with the plating layer (the position adjacent to the interface with the plating layer), there is a region (enriched layer) where the P concentration is higher than the average P concentration in the range from the surface of the coating to the interface between the coating and the plating layer (i.e., the average P concentration in the entire coating), and when a line analysis of the P concentration from the surface of the coating to the interface between the coating and the plating layer was performed using EDS, it was found that the position where the P concentration was maximum was within the enriched layer (showing the maximum P concentration within the enriched layer), and therefore corrosion resistance was improved. The reason why the corrosion resistance is improved when the above-mentioned concentrated layer is present is believed to be as follows. When a treatment solution containing a fluorine compound and a P compound as an inhibitor is applied to a zinc-containing plating layer under specified conditions and then dried, the P compound migrates to the plating layer side to neutralize the pH fluctuation that occurs with the etching reaction caused by the fluorine compound. The P compound that migrates to the plating layer side forms a complex salt with Zn that has dissolved from the plating layer into the coating near the interface between the coating and the plating layer, resulting in a coating that is less permeable to air and water. This is thought to result in improved corrosion resistance. The presence of the above-mentioned concentrated layer indicates that a complex salt of P and Zn is formed in the coating near the interface with the plating layer, and it is therefore believed that the presence of the above-mentioned concentrated layer improves corrosion resistance. If the concentrated layer does not exist or if the P concentration is high in locations other than near the interface with the plating layer, a complex salt of P and Zn will not be formed sufficiently, the permeation of air and water through the coating will not be sufficiently suppressed, and corrosion resistance will not be sufficiently improved. From the viewpoint of improving corrosion resistance, the ratio of the maximum P concentration to the average P concentration (maximum concentration / average concentration) is preferably 1.2 or more. More preferably, it is 1.3 or more, and even more preferably, it is 1.5 or more. On the other hand, if the (maximum concentration / average concentration) exceeds 2.0, the adhesion between the plating layer and the coating decreases, and the corrosion resistance of the processed part and the paint adhesion decrease, which is not preferable. Although the cause of this is unclear, it is presumed to be due to the excessive generation of a complex salt of P and Zn between the plating layer and the coating. Therefore, it is preferable that the ratio of the maximum P concentration to the average P concentration is 2.0 or less.
[0035] The thickness of the thickened layer is preferably 5 nm or more in order to obtain a sufficient effect, whereas the thickness of the thickened layer is preferably 100 nm or less in terms of the film conformability during processing.
[0036] In the surface-treated steel material according to this embodiment, the treatment liquid contains hydrofluoric acid as an etching component, and after the treatment liquid is applied, the oxide film on the surface of the plating layer is removed, thereby promoting the reaction between the plating layer and the treatment liquid. In addition, the plating layer components are dissolved into the coating by the etching reaction. Zinc (Zn) constituting the plating layer is dissolved into the coating, and zinc is contained in the coating near the plating layer, improving the coating between the plating layer and the chemical conversion layer.
[0037] Furthermore, in the surface-treated steel material according to this embodiment, when a line analysis of the F concentration is performed using EDS from the surface of the coating to the interface between the coating and the plating layer, it is preferable that the maximum F concentration is shown within the above-mentioned concentrated layer (the position where the F concentration is maximum is within the concentrated layer). The concentration of F is caused by the etching components in the treatment solution. The etching components in the treatment solution react with the plating surface, causing F to migrate to the plating surface and concentrate on the plating surface. The presence of a point where the F concentration is at its maximum within the concentrated layer satisfies the concentration threshold required for a complex chloride reaction with Zn, and the formation of a complex salt between F and Zn results in a coating that is difficult for corrosive factors such as water to penetrate. This is thought to result in improved corrosion resistance. It is more preferable that the ratio of the maximum F concentration to the average F concentration in the range from the surface of the coating to the interface between the coating and the plating layer is 1.5 or more. In this case, the corrosion resistance is further improved. More preferably, it is 1.7 or more. On the other hand, if the ratio of the maximum F concentration to the average F concentration exceeds 2.3, the adhesion between the plating layer and the coating decreases, and the corrosion resistance of the processed part and the paint adhesion decrease, which is not preferable. Although the cause of this is not clear, it is presumed to be due to the excessive generation of a complex salt of F and Zn between the plating layer and the coating. Therefore, it is preferable that the ratio of the maximum F concentration to the average F concentration in the range from the surface of the coating to the interface between the coating and the plating layer is 2.3 or less. In this embodiment, if the EDS line analysis reveals an area where the P concentration and F concentration are higher than the average, it is determined that there is a concentrated layer. On the other hand, for the maximum values of the P concentration and F concentration, the point where the concentration is the highest and is 1.1 times or more the average is used. In other words, if there is no point where the concentration is 1.1 times or more the average (all points are less than 1.1 times), it is determined that there is no maximum value.
[0038] Furthermore, in the surface-treated steel material according to this embodiment, when EDS line analysis is performed on the concentration of Zn from the surface of the coating to the interface between the coating and the plating layer, it is preferable that Zn is continuously detected and that the concentration of Zn is 1.0 atomic % or more over the entire target range. The continuous presence of 1.0 atomic % or more of Zn results in a structure in which Zn compounds are chemically bonded from the surface of the coating to the interface between the coating and the plating layer, which allows the coating and the plating layer to be strongly bonded together, improving the adhesion between the coating and the plating layer. Although there is no upper limit for the Zn concentration, the solubility limit is thought to be about 5.5 atomic %.
[0039] In the surface-treated steel material according to this embodiment, whether the coating contains Si, C, O, P, F, or Zn, the position and thickness of the concentrated layer, and the position and maximum value of the concentration of each element are determined by EDS line analysis. Specifically, a test piece having a thickness of 80 to 200 nm is cut out from a Zn-based plated steel sheet on which a coating is formed by a cryo-FIB (Focused Ion Beam) method, and the cross-sectional structure of the cut out test piece is observed by a transmission electron microscope (TEM) at a magnification where the entire coating is included in the observation field. In order to identify the constituent elements of each layer, a line analysis is performed along the thickness direction using TEM-EDS (Energy Dispersive X-ray Spectroscopy) to quantitatively analyze the chemical composition at each location. The method of line analysis is not particularly limited, and may be a continuous point analysis at intervals of several nm, or an element map within an arbitrary region may be measured and the thickness distribution of the elements may be measured as an average in the surface direction. The elements to be quantitatively analyzed are six elements, namely C, O, F, Si, P, and Zn, and the denominator for calculating the concentration of each element is the sum of the concentrations of the six elements. The apparatus used is not particularly limited, but for example, a TEM (field emission transmission electron microscope: JEM-2100F manufactured by JEOL Ltd.) or an EDS (JED-2300T manufactured by JEOL Ltd.) may be used. From the above-mentioned TEM-EDS line analysis results, the concentration distributions of Si, C, O, P, F, and Zn are obtained, the enriched layer is identified, and the thickness of the enriched layer is measured. When the thickness of the concentrated layer determined by TEM is about 5 nm, it is preferable to use a TEM with a spherical aberration correction function from the viewpoint of spatial resolution.
[0040] Fig. 2A is a HAAD-STEM image of a region including the plating layer and coating in the cross section of the surface-treated steel according to this embodiment, and Fig. 2B is a BF-STEM image of the region including the plating layer and coating (same field of view as Fig. 2A) in the cross section of the surface-treated steel according to this embodiment. Fig. 3 is a diagram showing an example of the results of line analysis using EDS for Si, C, O, P, F and Zn in the range shown in Fig. 2B of the cross section of the surface-treated steel according to this embodiment. (Only Zn has a right scale for the vertical axis, and the others have a left scale.) As shown in FIG. 3, in the surface-treated steel material according to this embodiment, a point where the P concentration is maximum exists near the interface of the coating with the plating layer, and within a certain thickness range from the interface with the plating layer, there exists a region (concentrated layer) where the P concentration is higher than the average P concentration in the plating layer. Similarly, the concentration of F is high near the interface with the plating layer.
[0041] Next, a preferred method for producing the surface-treated steel material according to this embodiment will be described. The surface-treated steel material according to this embodiment can obtain its effects as long as it has the above-mentioned characteristics regardless of the manufacturing method, but the manufacturing method described below is preferable because it can be manufactured stably.
[0042] That is, the surface-treated steel material according to this embodiment can be manufactured by a manufacturing method including the following steps. (I) a plating process in which a steel material (steel sheet) is immersed in a plating bath containing Zn to form a plating layer on the surface; (II) applying a surface treatment metal agent to a steel material having a plating layer; (III) A heating process in which the steel material to which the surface treatment metal agent has been applied is heated to form a coating containing Si, C, O, P, F, and Zn. Here, the heating step is (III-1) a holding process in which the steel material to which the surface treatment metal agent has been applied is held at a temperature range of less than 40°C for a predetermined period of time; (III-2) After the holding step, a heating reaction step of holding the mixture at a temperature in the range of 40 to less than 55° C. for a predetermined period of time is included.
[0043] [Plating process] The plating process is not particularly limited, and may be carried out in a conventional manner so as to obtain sufficient plating adhesion. Furthermore, there is no limitation on the method for producing the steel material to be subjected to the plating step. For example, the method may be a method for producing a zinc-plated steel sheet specified in JIS G3302:2019, or a method for producing a plated steel sheet specified in JIS G3323:2019.
[0044] [Coating process] In the painting process, a surface treatment metal agent containing a Si compound, a P compound, and an F compound is applied to the steel material having a plating layer containing Zn. The surface treatment metal agent may further contain a V compound and a Zr compound. In the coating step, the method for coating the surface-treating metal agent is not limited, and for example, coating can be performed using a roll coater, a bar coater, a spray, or the like.
[0045] In this embodiment, the Si compound contained in the surface treatment metal agent may be, for example, a Si compound obtained by blending a silane coupling agent (A) containing one amino group in the molecule and a silane coupling agent (B) containing one glycidyl group in the molecule at a solid concentration ratio (A) / (B) of 0.5 to 1.7. In addition, examples of F compounds contained in the surface treatment metal agent include compounds such as hydrofluoric acid HF, borofluoric acid BF4H, silicofluoric acid H2SiF6, zirconyl hydrofluoric acid H2ZrF6, and titanium hydrofluoric acid H2TiF6. The compounds may be one type or a combination of two or more types. Among these, hydrofluoric acid is more preferable. When hydrofluoric acid is used, better corrosion resistance and paintability can be obtained.
[0046] In this embodiment, the P compound contained in the surface treatment metal agent is not particularly limited, but examples thereof include phosphoric acid, ammonium phosphate, potassium phosphate, and sodium phosphate. Among these, phosphoric acid is more preferable. When phosphoric acid is used, better corrosion resistance can be obtained.
[0047] In addition, when a V compound is contained in the surface-treated steel material, examples of the V compound include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3)2, vanadium acetylacetonate V(OC(=CH2)CH2COCH3)3, vanadium trichloride VCl3, and phosphovanadomolybdic acid. In addition, a pentavalent vanadium compound reduced to a tetravalent or divalent vanadium compound by an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group can also be used.
[0048] [Heating process] In the heating process, the steel material coated with the surface treatment metal agent is heated, dried, and baked. The maximum drying temperature is preferably 60 to 200° C., and more preferably 80 to 150° C. If the maximum drying temperature is less than 60° C., the solvent in the surface-treating metal agent does not volatilize completely, which is not preferable. On the other hand, if the maximum drying temperature exceeds 200° C., the effect of drying the solvent by heating becomes saturated, which is not economical, and is therefore not preferable. In the heating step, the method of heating the surface-treating metal agent is not limited. For example, the surface-treating metal agent can be heated and dried using an induction heater or a hot air oven. The heating process includes the holding process and the heating reaction process described below. For example, by controlling these conditions, it is possible to concentrate P and F on the plating surface side and maximize the concentrations of P and F in the concentrated layer.
[0049] [In heating process, holding process] In the coating process, a surface treatment metal agent containing an F compound is applied, and then heated in the subsequent heating process, so that F is concentrated near the interface with the plating layer. In particular, when the maximum value of the F concentration in the concentrated layer is increased to a certain level or higher, it is preferable that the time until the temperature of the steel material reaches 40°C (holding time below 40°C) is 0.5 to 15.0 seconds. By setting the time until the temperature reaches 40°C (holding time) after coating to 0.5 seconds or more, the surface treatment metal agent before drying and the plating surface are in contact for a sufficient time, and the F compound contained in the surface treatment metal agent reacts with the Zn of the plating layer, forming a complex salt of F and Zn. In addition, the above reaction reduces the concentration gradient of F contained in the surface metal agent in the thickness direction before drying, so that the F compound in the surface metal agent other than the plating surface moves to the plating surface, and F is concentrated on the plating surface. If the time to reach 40°C is less than 0.5 seconds, the reaction between the F compound and Zn becomes insufficient, F is not sufficiently concentrated at the interface with the plating layer, and the ratio of the maximum F concentration to the average F concentration in the range from the surface of the coating to the interface with the plating layer does not reach 1.5 or more. It is preferable that the time to reach 40°C is 5.0 seconds or more. On the other hand, if the time to reach 40°C exceeds 15.0 seconds, the ratio of the maximum F concentration to the average F concentration in the range from the surface of the coating to the interface with the plating layer exceeds 2.3, which is not preferable.
[0050] [Heating process, heating reaction process] When P is concentrated on the plated surface side of the coating, after a surface treatment metal agent containing a P compound is applied, the steel material is held in a temperature range of 40 to less than 55°C, which is a higher temperature range than the holding process described above. The complex chlorination reaction between the P compound contained in the surface treatment metal agent and Zn on the surface of the plating layer proceeds at a temperature of 40°C or higher, but when the temperature reaches 55°C or higher, the solvent of the surface treatment metal agent evaporates and the complex chlorination reaction ends. Therefore, in the manufacturing method of the surface-treated steel material according to this embodiment, when the complex chlorination reaction between the P compound and Zn is sufficiently promoted to concentrate P on the plating layer side of the coating, it is preferable to hold the temperature range of 40 to less than 55°C for 0.5 seconds or more. The holding time is more preferably 1.0 seconds or more, and even more preferably 5.0 seconds or more. On the other hand, if the holding time exceeds 25.0 seconds, the concentration of P (maximum concentration relative to the average concentration) becomes too high, which is not preferable. The holding temperature in the heating step (holding process, heating reaction process) may include temperature changes as long as the temperature is within a predetermined temperature range.
[0051] The thickness of the thickened layer is preferably 5 to 100 nm. For example, the thickness of the surface-treated steel material is 0.05 to 2.0 g / m 2 The thickness of the concentrated layer is 5 to 100 nm by setting the time required for the temperature to reach 40°C during the holding period in the heating step to 0.5 to 25.0 seconds, and setting the holding period in the temperature range of 40 to less than 55°C during the heating reaction step to 0.5 to 15.0 seconds.
[0052] Furthermore, in order to continuously contain 1.0 atomic % or more of Zn from the surface of the coating to the interface between the coating and the plating layer, it is preferable that the time from application of the surface treatment metal agent containing Fluorine compounds until the coating dries (until the temperature reaches 55°C) is 1.0 seconds or more. Between application and drying, the Zn in the plating layer is dissolved by the Fluorine compounds contained in the surface treatment metal agent, and diffuses into the coating. If this time is 1.0 seconds or more, the coating will contain 1.0 atomic % or more of Zn. The time from application to drying is preferably 40.0 seconds or less, because the Zn concentration in the surface-treated steel material will be saturated. EXAMPLES
[0053] The plated steel sheets shown in Table 1 were prepared. A in Table 1 (galvanized steel sheet with Zn plating) is a galvanized steel sheet specified in JIS G3302:2019, and the coating weight is expressed as Z27. B in Table 1 (galvanized steel sheet with Zn-6%Al-3%Mg plating) and C (galvanized steel sheet with Zn-11%Al-3%Mg-0.2%Si plating) are both plated steel sheets specified in JIS G3323:2019, and the coating weight is expressed as K-27.
[0054] A surface treatment metal agent was applied to these plated steel sheets without degreasing after plating using a roll coater with a treatment liquid that contained a Si compound, an F compound, a P compound, and a V compound as shown in Tables 2-1 and 2-2, and further contained a V compound as required. The Si compound used was a Si compound obtained by mixing a silane coupling agent (A) containing one amino group in the molecule and a silane coupling agent (B) containing one glycidyl group in the molecule at a solid concentration ratio (A) / (B) of 1.7. In the table, V1 and V2 in the V compounds represent the following: V1: Vanadium oxysulfate VOSO4 V2: Vanadium oxyacetylacetonate VO)OC(=CH2)CH2CO In the F compounds, F1 and F2 represent the following: F1: Hydrofluoric acid F2: Zirconium hydrofluoric acid F3: Titanium hydrofluoric acid
[0055] After the surface treatment metal agent was applied, the plated steel sheet was controlled so that the holding temperature below 40°C, the holding temperature between 40 and 55°C, the time from application to drying, and the maximum temperature reached were as shown in Tables 2-1 and 2-2 to form a coating.
[0056] [Table 1]
[0057] [Table 2-1]
[0058] [Table 2-2]
[0059] For the obtained surface-treated steel material, the following were measured by the above-mentioned method using TEM-EDS: whether the coating was composed of Si, C, O, P, F, and Zn; whether there was a concentrated layer adjacent to the interface with the plating layer and, if so, its thickness; the position at which the concentration of each element was at its maximum; if P or F was at its maximum within the concentrated layer, the maximum / average values of each concentration; and the minimum concentration of Zn in the coating. However, if there was no point where the concentration of P or F was 1.1 times or more the average value (if all points were less than 1.1 times the average value), it was determined that there was "no maximum value." In such cases, the maximum / average values were not calculated. Specifically, a sample was cut out from the coating using the cryo-FIB method, and the constituent elements, the ratio of the constituent elements, the thickness of the coating, and the thickness of the concentrated layer were measured using a TEM (a field emission transmission electron microscope manufactured by JEOL: JEM-2100F, accelerating voltage 200 kV) and an EDS (a JEOL JED-2300T manufactured by JEOL). From the results, the ratio of the maximum P concentration to the average P concentration in the thickness direction, the ratio of the maximum F concentration to the average F concentration in the thickness direction, the minimum Zn concentration in the coating, etc. were calculated. The results are shown in Tables 3-1 and 3-2.
[0060] The obtained surface-treated steel materials were evaluated for flat plate corrosion resistance, Erichsen processed area corrosion resistance, and paint adhesion in the following manner. The results are shown in Tables 4-1 and 4-2.
[0061] "Plate corrosion resistance" Flat test pieces were prepared, and each test piece was subjected to a salt spray test in accordance with JIS Z 2371:2015. The occurrence of white rust on the surface after 48 hours (the proportion of the area of the test piece where white rust occurred) was evaluated. <Evaluation criteria> 3: Rust occurs on 10% or less of the total area 2: Rust occurs on more than 10% but not more than 30% of the total area 1: Rust occurs on more than 30% of the total area The test was performed with n=3, and if two or more items scored 3 or above on the evaluation criteria, the plate corrosion resistance was determined to be excellent.
[0062] "Corrosion resistance of Erichsen processed parts" Flat test pieces were prepared and subjected to an Erichsen test (7 mm extrusion), after which a salt spray test in accordance with JIS Z 2371:2015 was performed for 72 hours, and the occurrence of white rust was observed. <Evaluation criteria> 5: Rust occurs in less than 3% of the processed area 4: Rust occurs in 3% to less than 10% of the processed area 3: Rust occurs in 10% to less than 20% of the processed area 2: Rust occurs in 20% to less than 40% of the processed area 1: Rust occurs on 40% or more of the processed area The test was performed with n=3, and if two or more items had an evaluation standard of 4 or higher, the Erichsen processed part was judged to have excellent corrosion resistance.
[0063] "Paint adhesion test" A flat test piece was prepared, and a melamine alkyd paint was bar-coated so that the film thickness after drying would be 20 μm, and baked for 20 minutes at 120° C. Cuts were made in a grid pattern spaced 1 mm apart, and the adhesion was evaluated based on the percentage of remaining pieces (remaining pieces / cut pieces: 100 pieces). <Evaluation criteria> 3: Remaining number 95% or more and 100% or less 2: Remaining number is 80% or more but less than 95% 1: Less than 80% remaining The test was performed with n=3, and if at least one evaluation criterion was 3 or more, it was determined that the paint adhesion was excellent.
[0064] [Table 3-1]
[0065] [Table 3-2]
[0066] [Table 4-1]
[0067] [Table 4-2]
[0068] As can be seen from Tables 1 to 4-2, when the coating contained Si, C, O, P, F, and Zn as constituent elements, had a P-enriched layer adjacent to the interface with the plating layer, and showed the maximum P concentration within the enriched layer, the flat plate corrosion resistance, the Erichsen processed area corrosion resistance, and the paint adhesion were all excellent. On the other hand, in the cases where there is no predetermined thickened layer or where the thickened layer does not show the maximum value of P (Nos. 14 to 18), the flat plate corrosion resistance, the Erichsen processed area corrosion resistance, and the paint adhesion are poor. [Explanation of symbols]
[0069] 1. Surface-treated steel 11 Steel plate 12 Plating layer 13 Coating 14 Protective layer
Claims
1. A steel plate, A zinc-containing plating layer formed on the steel sheet; A coating formed on the plating layer, The coating contains Si, C, O, P, F, and Zn as constituent elements, the coating has a concentrated layer in which the concentration of P is higher than the average concentration of P in the range from the surface of the coating to the interface between the coating and the plating layer in the thickness direction, The concentrated layer is adjacent to the interface with the plating layer, When an EDS line analysis is performed on the concentration of P from the surface of the coating to the interface between the coating and the plating layer, a maximum value of the P concentration is shown in the concentrated layer, When an EDS line analysis is performed on the concentration of F from the surface of the coating to the interface between the coating and the plating layer, a maximum value of the concentration of F is shown in the concentrated layer, a ratio of the maximum value of the F concentration to an average concentration of F in a range from the surface of the coating to the interface between the coating and the plating layer is 1.5 or more and 2.3 or less, The chemical composition of the plating layer is, in mass%, Al: 4.0% to less than 25.0%; Mg: 0% to less than 12.5% Sn: 0% to 20%, Bi: 0% to less than 5.0% In: 0% to less than 2.0% Ca: 0% to 3.0%, Y: 0% to 0.5%, La: 0% to less than 0.5%, Ce: 0% to less than 0.5% Si: 0% to less than 2.5%; Cr: 0% to less than 0.25% Ti: 0% to less than 0.25% Ni: 0% to less than 0.25% Co: 0% to less than 0.25% V: 0% to less than 0.25%, Nb: 0% to less than 0.25% Cu: 0% to less than 0.25% Mn: 0% to less than 0.25%; Fe: 0% to 5.0%, Sr: 0% to less than 0.5% Sb: 0% to less than 0.5% Pb: 0% to less than 0.5% B: 0% to less than 0.5%, and The balance is composed of Zn and impurities. Surface treated steel.
2. a ratio of the maximum value to the average concentration of P is 1.2 or more and 2.0 or less; The surface-treated steel material according to claim 1.
3. The thickness of the concentrated layer is 5 nm or more and 100 nm or less. The surface-treated steel material according to claim 1 or 2.
4. when EDS line analysis is performed on the concentration of Zn from the surface of the coating to the interface between the coating and the plating layer, Zn is continuously detected, and the concentration of Zn is 1.0 atomic % or more. The surface-treated steel material according to any one of claims 1 to 3.
Citation Information
Patent Citations
Manufacture of force-cooled superconducting cable
JP1986091806A
Oscillation circuit
JP1987072207A
Surface treatment liquid and manufacturing method of surface-treated steel plate and surface-treated steel plate
JP2020066793A
Chromate-free surface-treated metal materials with excellent corrosion resistance, heat resistance, fingerprint resistance, conductivity, paintability, and resistance to black residue during processing.
JP4776458B2
Surface-treated steel sheet having chemical conversion resin coating and process for producing the same