Fluororesin sheets, copper-clad laminates, circuit boards and antennas

A fluororesin sheet with specific elemental ratios and plasma treatment addresses the issues of high linear expansion and adhesion in high-frequency boards, achieving low CTE and improved adhesion to copper foil, thereby reducing warping and defects.

JP7568991B2Active Publication Date: 2024-10-17DAIKIN INDUSTRIES LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024010739
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-11-09
Filing Date
2024-01-29
Publication Date
2024-10-17
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

Existing fluororesin sheets used in high-frequency printed wiring boards face challenges with high linear expansion coefficients and inadequate adhesion to copper foil, leading to warping and circuit defects, despite surface treatments like annealing and hydrophilization.

Method used

A fluororesin sheet containing polytetrafluoroethylene and silica particles with an oxygen element ratio of 3.0 atomic% or more, nitrogen element ratio of 1.35 atomic% or more, and silicon element ratio of 0.5 atomic% or more, treated with plasma to enhance surface functional groups, achieving low linear expansion and improved adhesion.

Benefits of technology

The solution results in a fluororesin sheet with a low coefficient of linear expansion (CTE) and enhanced peel strength to copper foil, reducing substrate warpage and circuit defects while maintaining low dielectric loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568991000001
    Figure 0007568991000001
  • Figure 0007568991000002
    Figure 0007568991000002
Patent Text Reader

Abstract

To provide: a fluororesin sheet which achieves a balance between a low coefficient of linear expansion (CTE) and improved adhesion between a surface of the sheet and a smooth copper foil; and a copper-clad laminate obtained using the same.SOLUTION: This fluororesin sheet contains a fluororesin and silica particles. On one surface or both surfaces of the sheet, the oxygen element ratio, as measured using X-Ray photoelectron spectroscopy (XPS), is 3.0 atomic% or more. The coefficient of linear expansion (CTE) of the sheet is 100 ppm / °C or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a fluororesin sheet, a copper-clad laminate, a circuit board, and an antenna. [Background technology]

[0002] There is a demand for high frequency printed wiring boards with small transmission loss, and it is known to use a fluororesin film in such high frequency printed wiring boards (Patent Document 1, etc.).

[0003] In such printed wiring boards, the fluororesin film is subjected to a surface treatment to improve adhesion to the copper foil. Patent Document 2 proposes that a fluororesin film be subjected to a surface treatment and an annealing treatment to improve adhesion to a copper foil. Patent Document 3 proposes that the surface of a fluororesin substrate is hydrophilized to have an amino group and a hydroxyl group, thereby improving adhesion to a metal foil. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-8260 A [Patent Document 2] Patent Publication No. 2022-112028 [Patent Document 3] JP 2022-114351 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present disclosure is to provide a fluororesin sheet that combines a low coefficient of linear expansion (CTE) with improved adhesion to copper foil having a smooth surface, and a copper-clad laminate using the same. [Means for solving the problem]

[0006] The present disclosure relates to Polytetrafluoroethylene and silica particles, and the fluororesin sheet has an oxygen element ratio of 3.0 atomic% or more on one or both sides when measured by X-ray photoelectron spectroscopy (XPS) and a coefficient of linear expansion (CTE) of 100 ppm / °C or less.

[0007] Change Moreover, it is preferable that the nitrogen element ratio on the above-mentioned surface is 1.35 atomic % or more as measured by XPS. Furthermore, it is preferable that the silicon element ratio on the surface of the fluororesin sheet is 0.5 atomic % or more when measured by XPS.

[0008] Furthermore, it is preferable that the surface of the fluororesin sheet has a static contact angle of 105° or less when a 2 μL droplet is landed on the surface and measured 1 second after the droplet is landed.

[0009] The silica particles are preferably spherical silica. As the silica particles, it is preferable to use silica particles treated with a silane coupling agent. The silica particles preferably have an average particle size of 10 μm or less.

[0010] The fluororesin sheet of the present disclosure preferably does not contain glass fibers. The content of the silica particles in the total amount of the fluororesin sheet is preferably 30% by mass or more. The content of the silica particles in the total amount of the fluororesin sheet is preferably 50% by mass or more. The content of the silica particles in the total amount of the fluororesin sheet is preferably 50% by mass or more and 65% by mass or less.

[0011] The fluororesin sheet preferably has a dielectric loss tangent value of 0.0015 or less at 10 GHz. The fluororesin sheet preferably has a thickness of 5 to 250 μm.

[0012] The present disclosure also relates to a method for producing the fluororesin sheet, which comprises mixing fluororesin particles and silica particles to form a film, and then performing a surface treatment. Also, the method for producing a fluororesin sheet is preferably one in which a film is formed using a composition substantially consisting of fluororesin particles and filler particles containing at least silica particles, and the film is then surface-treated.

[0013] The present disclosure also relates to a copper clad laminate having a copper foil and the above-mentioned fluororesin sheet as essential layers. The surface roughness (Rz) of the copper foil is preferably 2.0 μm or less. The copper foil preferably has a surface roughness (Rq) of 0.01 to 0.15 μm. It is preferable that the copper foil and the fluororesin sheet are directly laminated together, and the peel strength of the interface between the copper foil having a surface roughness (Rz) of 2.0 μm or less and the fluororesin sheet is 0.5 kN / m or more.

[0014] The present disclosure also relates to a method for producing the copper clad laminate, comprising laminating the fluororesin sheet and copper foil, heating the laminate at 180 to 390°C, and press-molding the laminate at a pressure of 0.5 to 5 MPa under vacuum or in an inert gas atmosphere.

[0015] The present disclosure also relates to a circuit board having the copper clad laminate. The present disclosure is also an antenna formed from the circuit board. The antenna is preferably a millimeter wave antenna for mobility applications. Effect of the Invention

[0016] The fluororesin sheet of the present disclosure combines a low coefficient of linear expansion (CTE) with improved adhesion to copper foil having a smooth surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present disclosure will now be described in detail. For high-frequency boards of 5G and above, a smooth interface between the fluororesin sheet and copper foil reduces transmission loss and improves the characteristics of the high-frequency board. For this reason, good adhesion between the fluororesin sheet and copper foil with a smooth surface is required.

[0018] However, sheets made of fluororesin alone have a high linear expansion coefficient, which may cause warping of the board or defects in the circuit. In particular, in sheets made of polytetrafluoroethylene (PTFE) resin alone, functional groups containing oxygen and the like are difficult to form even when surface treatment is performed, and therefore sufficient adhesion to copper foil, which has a smooth surface, is not obtained, and further improvement is required. Such problems arise because functional groups are difficult to generate on the surface of polytetrafluoroethylene resin, and the generated functional groups are also prone to molecular motion, so that the functional groups move from the surface to the inside of the resin and are difficult to be exposed to the surface, making it difficult to obtain the effects of surface treatment.

[0019] The present disclosure has discovered that by performing a surface treatment such as plasma treatment on the surface of a fluororesin sheet containing fluororesin and silica particles and increasing the oxygen element ratio on the surface of the fluororesin sheet, good adhesion can be achieved between the fluororesin sheet and copper foil having a smooth surface with Rz of 2.0 μm or less.

[0020] In the present disclosure, by including silica particles, when the fluororesin sheet is subjected to a surface treatment, the silica surface can also have functional groups derived from the surface treatment, so that the oxygen atom ratio of the fluororesin sheet surface can be increased. This improves the adhesion between the fluororesin sheet and the copper foil, and the peel strength of the adhesive surface can be improved. Furthermore, in the present disclosure, the linear expansion coefficient of the fluororesin sheet can be further reduced by using a composite product of the fluororesin and silica particles. In this manner, the fluororesin sheet of the present disclosure can achieve both a low linear expansion coefficient and good peel strength.

[0021] The present disclosure relates to a fluororesin sheet containing fluororesin and silica particles, which has an oxygen element ratio of 3.0 atomic% or more as measured by X-ray photoelectron spectroscopy (XPS) and a linear expansion coefficient (CTE) of 100 ppm / °C or less. As described above, by making the fluororesin sheet contain fluororesin and silica particles, the oxygen element ratio on the surface of the fluororesin sheet can be increased, and therefore good adhesion to copper foil with a smooth surface is possible. In addition, the linear expansion coefficient (CTE) is low, and the occurrence of warpage of the substrate and defects in the circuit can be sufficiently suppressed.

[0022] The fluororesin sheet of the present disclosure has an oxygen element ratio of 3.0 atomic% or more on one or both sides thereof as measured by X-ray photoelectron spectroscopy (XPS). In particular, the oxygen element ratio of the sheet surface that adheres to the copper foil as measured by X-ray photoelectron spectroscopy (XPS) should be 3.0 atomic% or more. By having the oxygen element ratio of 3.0 atomic% or more, the sheet bonds with the surface of the copper foil, improving the peel strength against the copper foil. The oxygen atomic ratio is preferably 3.0 atomic % or more, more preferably 5.0 atomic % or more, and even more preferably 10.0 atomic % or more. There is no particular upper limit, but in consideration of the effect on productivity and other physical properties, it is preferably 25.0 atomic % or less.

[0023] Specifically, the measurement by X-ray photoelectron spectroscopy (XPS) is carried out using a scanning X-ray photoelectron spectroscopic analyzer (XPS / ESCA) PHI5000VersaProbeII (manufactured by ULVAC-PHI, Inc.).

[0024] In the fluororesin sheet of the present disclosure, in the surface having an oxygen element ratio of 3.0 atomic % or more as measured by X-ray photoelectron spectroscopy (XPS), the nitrogen element ratio is preferably 1.35 atomic % or more as measured by X-ray photoelectron spectroscopy (XPS). The nitrogen atomic ratio is more preferably 1.35 atomic % or more, further preferably 2.5 atomic % or more, and most preferably 3.0 atomic % or more. By increasing the nitrogen element ratio on the surface of the fluororesin sheet, which contributes to adhesion, it is possible to obtain sufficient peel strength with the copper foil without impairing the dielectric properties. There is no particular upper limit, but in consideration of the effect on productivity and other physical properties, it is preferably 25.0 atomic % or less.

[0025] In the fluororesin sheet of the present disclosure, in the surface having an oxygen element ratio of 3.0 atomic % or more as measured by X-ray photoelectron spectroscopy (XPS), the silicon element ratio is preferably 0.5 atomic % or more as measured by X-ray photoelectron spectroscopy (XPS). The silicon atomic ratio is more preferably 1.0 atomic % or more, further preferably 1.5 atomic % or more, and most preferably 2.0 atomic % or more. In this way, the silicon element ratio on the surface of the fluororesin sheet is high, which contributes to adhesion, and thus silica particles that can be surface-treated are exposed, thereby increasing the peel strength with the copper foil. There is no particular upper limit, but in consideration of the effect on other physical properties such as productivity and strength, it is preferably 10.0 atomic % or less.

[0026] In the fluororesin sheet of the present disclosure, on a surface having an oxygen element ratio of 3.0 atomic% or more as measured by X-ray photoelectron spectroscopy (XPS), the static contact angle of water measured 1 second after landing of a 2 μL droplet is preferably 105° or less, more preferably 103° or less, and even more preferably 100° or less. By satisfying such a range, new functional groups are generated in the fluororesin sheet, and the peel strength with the copper foil is increased.

[0027] The static contact angle of water was measured using a contact angle meter ("DropMaster" manufactured by Kyowa Interface Science Co., Ltd.) at 23° C., with a droplet amount of 2 μL, and one second after the droplet landed.

[0028] The fluororesin sheet of the present disclosure has a coefficient of linear expansion (CTE) of not more than 100 ppm / ° C. Having a CTE within the above range is preferable in that the fluororesin sheet has low shrinkage and excellent dimensional stability. The upper limit is more preferably 70 ppm / ° C., even more preferably 50 ppm / ° C., and even more preferably 40 ppm / ° C. The lower limit is preferably 10 ppm / ° C., and more preferably 18 ppm / ° C.

[0029] The linear expansion coefficient in this specification is determined by performing TMA measurement in a tensile mode using a TMA-7100 (manufactured by Hitachi High-Tech Science Corporation), using a fluororesin sheet cut into a length of 20 mm, width of 5 mm and thickness of 150 μm as a sample piece, setting the chuck distance to 10 mm, applying a load of 49 mN, and measuring the displacement of the sample from 0 to 150°C at a heating rate of 2°C / min.

[0030] (Fluorine resin) Fluorine resins have low dielectric properties and can therefore be suitably used in the present disclosure.

[0031] The fluororesin that can be used in the present disclosure is not particularly limited, and examples thereof include polytetrafluoroethylene (PTFE), tetrafluoroethylene [TFE] / hexafluoropropylene [HFP] copolymer [FEP], TFE / alkyl vinyl ether copolymer [PFA], TFE / HFP / alkyl vinyl ether copolymer [EPA], TFE / chlorotrifluoroethylene [CTFE] copolymer, TFE / ethylene copolymer [ETFE], polyvinylidene fluoride [PVdF], tetrafluoroethylene having a molecular weight of 300,000 or less [LMW-PTFE], etc. These fluororesins may be used alone or in combination of two or more. Among them, polytetrafluoroethylene (PTFE) is particularly preferable from the viewpoint of low dielectric properties and low linear expansion coefficient. PTFE having fibrillation is preferable. PTFE having fibrillation means PTFE that can be paste-extruded from unsintered polymer powder.

[0032] The PTFE may be modified polytetrafluoroethylene (hereinafter referred to as modified PTFE), homopolytetrafluoroethylene (hereinafter referred to as homoPTFE), or a mixture of modified PTFE and homoPTFE. From the viewpoint of maintaining good moldability of polytetrafluoroethylene, the content of modified PTFE in the polymeric PTFE is preferably 10% by mass or more and 98% by mass or less, and more preferably 50% by mass or more and 95% by mass or less.

[0033] The homo-PTFE is not particularly limited, and homo-PTFE disclosed in JP-A-53-60979, JP-A-57-135, JP-A-61-16907, JP-A-62-104816, JP-A-62-190206, JP-A-63-137906, JP-A-2000-143727, JP-A-2002-201217, WO 2007 / 046345 pamphlet, WO 2007 / 119829 pamphlet, WO 2009 / 001894 pamphlet, WO 2010 / 113950 pamphlet, WO 2013 / 027850 pamphlet, etc. can be suitably used. Among these, homo-PTFE having high stretchability and disclosed in JP-A-57-135, JP-A-63-137906, JP-A-2000-143727, JP-A-2002-201217, WO 2007 / 046345, WO 2007 / 119829, WO 2010 / 113950 and the like is preferred.

[0034] The modified PTFE is composed of TFE and a monomer other than TFE (hereinafter referred to as a modified monomer). The modified PTFE may be, but is not limited to, one that is uniformly modified by the modified monomer, one that is modified at the beginning of the polymerization reaction, one that is modified at the end of the polymerization reaction, etc. The modified PTFE is preferably a TFE copolymer obtained by subjecting a small amount of a monomer other than TFE to polymerization together with TFE within a range that does not significantly impair the properties of the TFE homopolymer.

[0035] The modified PTFE may be, for example, those disclosed in JP-A-60-42446, JP-A-61-16907, JP-A-62-104816, JP-A-62-190206, JP-A-64-1711, JP-A-2-261810, JP-A-11-240917, JP-A-11-240918, WO 2003 / 033555 pamphlet, WO 2005 / 061567 pamphlet, WO 2007 / 005361 pamphlet, WO 2011 / 055824 pamphlet, WO 2013 / 027850 pamphlet, etc., which can be suitably used. Among these, modified PTFEs having high stretchability and disclosed in JP-A-61-16907, JP-A-62-104816, JP-A-64-1711, JP-A-11-240917, WO 2003 / 033555, WO 2005 / 061567, WO 2007 / 005361, WO 2011 / 055824 and the like are preferred.

[0036] The modified PTFE contains TFE units based on TFE and modified monomer units based on a modified monomer. The modified monomer units are a part of the molecular structure of the modified PTFE and are derived from the modified monomer. The modified PTFE contains the modified monomer units in an amount of preferably 0.001 to 0.500 mass%, more preferably 0.01 to 0.30 mass%, of the total monomer units. The total monomer units are the parts derived from all monomers in the molecular structure of the modified PTFE.

[0037] The modifying monomer is not particularly limited as long as it can be copolymerized with TFE, and examples thereof include perfluoroolefins such as hexafluoropropylene (HFP), chlorofluoroolefins such as chlorotrifluoroethylene (CTFE), hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride (VDF), perfluorovinyl ethers, perfluoroalkylethylenes (PFAE), ethylene, etc. The modifying monomer used may be one type or multiple types.

[0038] The perfluorovinyl ether is not particularly limited, and examples thereof include perfluorounsaturated compounds represented by the following general formula (1). CF2 = CF-ORf (1) (In the formula, Rf represents a perfluoro organic group.)

[0039] In this specification, a perfluoro organic group is an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.

[0040] An example of the perfluorovinyl ether is perfluoro(alkyl vinyl ether) (PAVE), which is represented by the above general formula (1) in which Rf is a perfluoroalkyl group having 1 to 10 carbon atoms. The perfluoroalkyl group preferably has 1 to 5 carbon atoms. Examples of the perfluoroalkyl group in PAVE include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, a perfluorohexyl group, etc. Preferred PAVEs are perfluoropropyl vinyl ether (PPVE) and perfluoromethyl vinyl ether (PMVE).

[0041] The perfluoroalkylethylene (PFAE) is not particularly limited, and examples thereof include perfluorobutylethylene (PFBE), perfluorohexylethylene (PFHE), and the like.

[0042] The modifying monomer in the modified PTFE is preferably at least one selected from the group consisting of HFP, CTFE, VDF, PAVE, PFAE and ethylene.

[0043] The fluororesin is preferably non-melt processable. Non-melt processable means that the resin does not have sufficient fluidity even when heated to the melting point or higher, and cannot be molded by a melt molding method generally used for resins. PTFE corresponds to this.

[0044] In the present disclosure, it is preferable to use particles of such non-melt-processable fluororesin and form them into a fluororesin sheet by a molding method that fibrillates the particles. The molding method will be described later.

[0045] The PTFE preferably has a standard specific gravity (SSG) of 2.0 to 2.3. When such PTFE is used, a PTFE membrane having high strength (cohesion and puncture strength per unit thickness) is easily obtained. PTFE having a large molecular weight has a long molecular chain, and therefore it is difficult to form a structure in which the molecular chains are regularly arranged. In this case, the length of the amorphous part increases, and the degree of entanglement between the molecules increases. When the degree of entanglement between the molecules is high, the PTFE membrane is unlikely to deform under an applied load and is considered to exhibit excellent mechanical strength. In addition, when a PTFE having a large molecular weight is used, a PTFE membrane having a small average pore size is easily obtained.

[0046] The lower limit of the SSG is more preferably 2.05, and even more preferably 2.1.The upper limit of the SSG is more preferably 2.25, and even more preferably 2.2.

[0047] Standard specific gravity (SSG) was measured by preparing a sample in accordance with ASTM D-4895-89 and measuring the specific gravity of the resulting sample by the water displacement method.

[0048] In this embodiment, the molecular weight (number average molecular weight) of the PTFE constituting the PTFE particles is, for example, in the range of 2 million to 12 million. The lower limit of the molecular weight of the PTFE may be 3 million or 4 million. The upper limit of the molecular weight of the PTFE may be 10 million.

[0049] The number average molecular weight of PTFE can be measured by a method based on standard specific gravity and a method based on dynamic viscoelasticity when melted. The method based on standard specific gravity can be performed by a water displacement method based on ASTM D-792 using a sample molded based on ASTM D-4895 98. The method based on dynamic viscoelasticity is described, for example, by S. Wu in Polymer Engineering & Science, 1988, Vol. 28, 538 and the same document, 1989, Vol. 29, 273.

[0050] The PTFE preferably has a refractive index in the range of 1.2 to 1.6. By having such a refractive index, it is preferable in terms of low dielectric constant. The refractive index can be adjusted to be within the above range by a method of adjusting the polarizability or flexibility of the main chain. The lower limit of the refractive index is more preferably 1.25, more preferably 1.30, and most preferably 1.32. The upper limit of the refractive index is more preferably 1.55, more preferably 1.50, and most preferably 1.45.

[0051] The refractive indexes are values ​​measured using a refractometer (Abbemat 300).

[0052] The PTFE preferably has a maximum endothermic peak temperature (crystalline melting point) of 340±7°C.

[0053] The PTFE may be a low-melting-point PTFE having a maximum peak temperature of 338°C or lower on an endothermic curve on a crystalline melting curve measured by a differential scanning calorimeter, or a high-melting-point PTFE having a maximum peak temperature of 342°C or higher on an endothermic curve on a crystalline melting curve measured by a differential scanning calorimeter.

[0054] The low melting point PTFE powder is a powder particle produced by emulsion polymerization, and has the above-mentioned maximum endothermic peak temperature (crystalline melting point), a dielectric constant (ε) of 2.08 to 2.2, and a dielectric tangent (tan δ) of 1.9×10 -4~4.0×10 -4 Examples of commercially available products include Polyflon fine powders F201, F203, F205, F301, and F302 manufactured by Daikin Industries, Ltd., CD090 and CD076 manufactured by Asahi Glass Co., Ltd., and TF6C, TF62, and TF40 manufactured by DuPont.

[0055] The high melting point PTFE powder is also a powder particle produced by emulsion polymerization, and has the above-mentioned maximum endothermic peak temperature (crystalline melting point), a dielectric constant (ε) of 2.0 to 2.1, and a dielectric tangent (tanδ) of 1.6×10 -4 ~2.2×10 -4 As commercially available products, for example, Polyflon fine powder F104 and F106 manufactured by Daikin Industries, Ltd., CD1, CD141, and CD123 manufactured by Asahi Glass Co., Ltd., and TF6 and TF65 manufactured by DuPont are listed.

[0056] The powder in which both PTFE polymer particles are secondary aggregated usually has an average particle size of 250 to 2000 μm. In particular, granulated powder obtained by granulation using a solvent is preferred from the viewpoint of improving the flowability when filling a mold during preforming.

[0057] Powder-shaped PTFE particles that satisfy the above-mentioned parameters can be obtained by a conventional manufacturing method, for example, by following the manufacturing methods described in International Publication No. 2015-080291 and International Publication No. 2012-086710.

[0058] (Silica particles) The fluororesin sheet of the present disclosure must contain silica particles. The shape of the silica particles is not particularly limited, but it is particularly preferred that the silica particles are spherical. The spherical shape is preferred because it is easy to process uniformly during drilling, has a small specific surface area, and has low transmission loss. In the present disclosure, it is most preferred to use spherical silica.

[0059] The spherical silica means that the particle shape is close to a perfect sphere, and specifically, the sphericity is preferably 0.80 or more, more preferably 0.85 or more, even more preferably 0.90 or more, and most preferably 0.95 or more. The sphericity is calculated by taking a photograph with an SEM and calculating the value from the area and perimeter of the observed particle as (sphericity) = {4π x (area) ÷ (perimeter) 2}. The closer to 1, the closer to a perfect sphere. Specifically, the average value measured for 100 particles using an image processing device (Spectris Corporation: FPIA-3000) is used.

[0060] The spherical silica used in the present disclosure preferably has a D90 / D10 of 2 or more (preferably 2.3 or more, 2.5 or more) and a D50 of 10 μm or less when the volume is integrated from the smallest particle size. Furthermore, it is preferable that the D90 / D50 is 1.5 or more (more preferably 1.6 or more). It is preferable that the D50 / D10 is 1.5 or more (more preferably 1.6 or more). It is more preferable that the D50 is 5 μm or less. Since the small particle size spherical silica can enter the gaps between the large particle size spherical silica, it is possible to achieve excellent filling properties and high fluidity. In particular, it is preferable that the particle size distribution has a high frequency on the side of small particle size compared to a Gaussian curve. The particle size can be measured by a laser diffraction scattering type particle size distribution measuring device. In addition, since coarse particles make it difficult to form a thin sheet, it is preferable that the coarse particles having a particle size of a certain size or more are removed by a filter or the like.

[0061] The above-mentioned spherical silica preferably has a water absorption of 1.0% or less, more preferably 0.5% or less. The water absorption is based on the mass of the silica particles when dry. The water absorption is measured by leaving a sample in a dry state at 40°C and 80% RH for 1 hour, and measuring the water generated by heating at 200°C using a Karl Fischer water content measuring device, and then calculating the water absorption.

[0062] In addition, each parameter of the spherical silica described above can also be measured using the above-mentioned method after heating the fluororesin sheet at 600°C for 30 minutes in an air atmosphere to burn off the fluororesin and extracting the spherical silica particles.

[0063] The silica particles are preferably surface-treated. By previously subjecting the silica particles to a surface treatment, interactions can be generated between the silica particles, and the linear expansion coefficient of the fluororesin sheet can be reduced.

[0064] The surface treatment is not particularly limited, and any known surface treatment can be used.Specific examples include treatment with a silane coupling agent such as epoxysilane, aminosilane, isocyanatesilane, vinylsilane, acrylicsilane, hydrophobic alkylsilane, phenylsilane, and fluorinated alkylsilane having a reactive functional group, plasma treatment, and fluorination treatment.Among them, treatment with a silane coupling agent is preferred.

[0065] In the present disclosure, it is preferable to use silica particles treated with a silane coupling agent. By treating silica particles with a silane coupling agent, the linear expansion coefficient can be reduced, which is advantageous in that it improves adhesion to copper foil. In addition, by treating with a silane coupling agent, the polar functional groups present on the silica particle surface react, and the amount of polar functional groups is reduced, resulting in excellent electrical properties. Furthermore, the functional groups contained in the silane coupling agent react with the copper foil surface, thereby increasing the peel strength with the copper foil.

[0066] Examples of the silane coupling agent include epoxy silanes such as γ-glycidoxypropyltriethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, amino silanes such as aminopropyltriethoxysilane and N-phenylaminopropyltrimethoxysilane, isocyanate silanes such as 3-isocyanatepropyltrimethoxysilane, vinyl silanes such as vinyltrimethoxysilane, and acrylic silanes such as acryloxytrimethoxysilane.

[0067] The average particle size of the silica particles is preferably 10 μm or less, which is preferable because the surface roughness of the sheet is low when the average particle size of the silica particles is 10 μm or less. The upper limit of the average particle size of the silica particles is more preferably 8 μm or less, and further preferably 5 μm or less. In addition, the lower limit of the average particle size of the silica particles is not particularly limited, but is preferably 0.5 μm or more. If the average particle size is less than 0.5 μm, the filler tends to aggregate, making it difficult to obtain a sufficient effect. The average particle size here is the D50 value measured by a laser analysis type particle size distribution analyzer.

[0068] The silica particles may be commercially available silica particles that satisfy the above-mentioned properties. Examples of commercially available silica particles include Denka fused silica FB grade (manufactured by Denka Co., Ltd.), Denka fused silica SFP grade (manufactured by Denka Co., Ltd.), Excelica (manufactured by Tokuyama Corporation), high-purity synthetic spherical silica particles Admafine (manufactured by Admatechs Co., Ltd.), Admanano (manufactured by Admatechs Co., Ltd.), and Admafuse (manufactured by Admatechs Co., Ltd.).

[0069] The content of the silica particles in the total amount of the fluororesin sheet is preferably 30% by mass or more. This is preferable because it is possible to maintain a low dielectric constant and low loss while lowering the linear expansion coefficient. In addition, when PTFE is used as the fluororesin, functional groups of oxygen and nitrogen are unlikely to be formed in PTFE even when plasma treated, but the presence of silica particles allows the silica surface to have functional groups derived from the surface treatment. As a result, the oxygen atom ratio on the surface of the fluororesin sheet can be increased, the adhesion between the fluororesin sheet and the copper foil is improved, and the peel strength of the adhesive surface can be improved. The amount of silica particles is more preferably 35% by mass or more, even more preferably 50% by mass or more, and even more preferably 55% by mass or more. The upper limit of the amount of silica particles is not particularly limited, but is preferably 70% by mass or less, more preferably 68% by mass or less, and even more preferably 65% ​​by mass or less.

[0070] (Sheet) The fluororesin sheet of the present disclosure preferably has a dielectric loss tangent of 0.0015 or less at 10 GHz. By setting the dielectric loss tangent within this range, it is preferable that the loss of electrical signals in the circuit can be kept low. The dielectric loss tangent is more preferably 0.0012 or less, and even more preferably 0.0011 or less. On the other hand, the lower limit of the dielectric loss tangent is preferably 0.00001.

[0071] The fluororesin sheet of the present disclosure preferably has a relative dielectric constant of 3.5 or less at 10 GHz. Having the relative dielectric constant within this range is preferable in terms of low dielectric loss. The upper limit of the relative dielectric constant is more preferably 3.2, and even more preferably 3.1, while the lower limit of the relative dielectric constant is preferably 2.0, and more preferably 2.5.

[0072] In this specification, the relative permittivity (Dk) and dielectric loss tangent (Df) at 10 GHz were determined by measuring Dk and Df at 25° C. and 10 GHz using a split cylinder type dielectric constant / dielectric loss tangent measuring device (manufactured by EM Lab).

[0073] The fluororesin sheet of the present disclosure preferably has a thickness of 5 to 250 μm. The lower limit of the thickness is more preferably 15 μm or more, and even more preferably 30 μm or more. The upper limit of the thickness is more preferably 230 μm or less, and even more preferably 200 μm or less. The thickness can be selected in consideration of the balance between the electrical properties and the linear expansion coefficient of the laminate.

[0074] The fluororesin sheet of the present disclosure may contain components other than the fluororesin and silica particles. The components to be contained are not particularly limited, and examples thereof include fluorine-free thermosetting resins and thermoplastic resins. The fluororesin sheet of the present disclosure preferably does not contain glass fibers. By not containing glass fibers or cloth made of glass fibers, the fluororesin sheet can be made thinner and has the advantage of being more flexible and easy to use in applications where it is used while being bent.

[0075] In the present disclosure, fillers other than silica particles may be used as long as they do not impede the purpose of the present disclosure. The fillers used are not particularly limited, and include organic fillers selected from polyphenyl ester, polyphenylene sulfide, polyimide, polyether ether ketone, polyphenylene, polyamide, and wholly aromatic polyester resin, ceramics, talc, mica, aluminum oxide, zinc oxide, tin oxide, titanium oxide, calcium carbonate, calcium oxide, magnesium oxide, potassium titanate, calcium fluoride, boron nitride, barium sulfate, molybdenum disulfide, and potassium carbonate whiskers. Two or more of these may be used in combination.

[0076] (Method of manufacturing fluororesin sheet) The fluororesin sheet of the present disclosure can be obtained, for example, by mixing the above-mentioned fluororesin particles and silica particles to form a film and then performing a surface treatment. The method for forming the film is not limited, but can be performed by paste extrusion molding, powder rolling molding, etc.

[0077] As described above, it is preferable to use non-melt processable fluororesin particles as the fluororesin particles used in the fluororesin sheet of the present disclosure. When using such fluororesin particles, it is preferable to form them into a sheet by fibrillating powdered PTFE as a raw material.

[0078] The powdered PTFE preferably has a primary particle size of 0.05 to 10 μm. The use of such a powder has the advantage of excellent moldability and dispersibility. The primary particle size here is a value measured in accordance with ASTM D 4895.

[0079] The powdered PTFE preferably contains 50% by mass or more, more preferably 80% by mass or more, of polytetrafluoroethylene resin having a secondary particle diameter of 500 μm or more. By containing PTFE having a secondary particle diameter of 500 μm or more within this range, there is an advantage in that a fluororesin sheet with high strength can be produced. By using PTFE with a secondary particle size of 500 μm or more, a sheet with lower resistance and excellent toughness can be obtained.

[0080] The lower limit of the secondary particle diameter is more preferably 300 μm, and even more preferably 350 μm. The upper limit of the secondary particle diameter is more preferably 700 μm or less, and even more preferably 600 μm or less. The secondary particle diameter can be determined, for example, by a sieving method.

[0081] The powdered PTFE has an average primary particle size of preferably 50 nm or more, more preferably 100 nm or more, even more preferably 150 nm or more, and particularly preferably 200 nm or more, since this allows the production of a sheet with higher strength and excellent homogeneity. The larger the average primary particle diameter of PTFE, the more suppressed the increase in paste extrusion pressure when the powder is used for paste extrusion molding, and the better the moldability. The upper limit is not particularly limited, but may be 500 nm. From the viewpoint of productivity in the polymerization step, it is preferably 350 nm.

[0082] The above average primary particle diameter can be determined by preparing a calibration curve of the transmittance of 550 nm projected light per unit length of an aqueous dispersion of PTFE obtained by polymerization, the polymer concentration of which is adjusted to 0.22% by mass, and the average primary particle diameter determined by measuring the unidirectional diameter in a transmission electron microscope photograph, measuring the above transmittance for the aqueous dispersion to be measured, and then based on the calibration curve.

[0083] The PTFE particles used in the present disclosure may have a core-shell structure.The PTFE particles having a core-shell structure may include modified polytetrafluoroethylene, which contains a core of high molecular weight polytetrafluoroethylene and a shell of lower molecular weight polytetrafluoroethylene or modified polytetrafluoroethylene in the particle.The modified polytetrafluoroethylene may include, for example, the polytetrafluoroethylene described in JP-A-2005-527652.

[0084] The specific methods for the above paste extrusion molding and powder rolling molding are not particularly limited, but the general methods are described below.

[0085] (Paste extrusion molding) The method for producing the fluororesin sheet may include a step (1a) of mixing powdered fluororesin particles obtained using a hydrocarbon-based surfactant, silica particles, and an extrusion aid, a step (1b) of paste extrusion molding the resulting mixture, a step (1c) of rolling the extrudate obtained by extrusion molding, a step (1d) of drying the rolled sheet, and a step (1e) of firing the dried sheet to obtain a molded product. The paste extrusion molding can also be carried out by adding conventionally known additives such as pigments and fillers to the fluororesin particles and silica particles.

[0086] The extrusion aid is not particularly limited, and generally known ones can be used, such as hydrocarbon oils.

[0087] (Powder rolling molding) The fluororesin sheet can also be formed by powder rolling. Powder rolling is a method of applying a shear force to powdered fluororesin particles to fibrillate them and form them into a sheet. The method may include a step of subsequently firing the particles to obtain a molded body. More specifically, A step (1) of applying a shear force to a raw material composition containing fluororesin particles and filler particles while mixing the raw material composition. A step (2) of forming the mixture obtained by the step (1) into a bulk form; and A step (3) of rolling the bulk mixture obtained in the step (2) into a sheet. The above-mentioned manufacturing method can be used to obtain the above-mentioned polymerizable compound. The method may further include a step (4) of firing the sheet-like material obtained above at 200 to 400° C. for 1 to 60 minutes. Additionally, step (2) may be omitted.

[0088] When a fluororesin sheet is manufactured by the powder rolling molding method, it is preferable to form a film using a composition that does not contain a liquid component and is substantially composed of fluororesin particles and filler particles including at least silica particles. Note that "substantially composed of fluororesin particles and filler particles including at least silica particles" means that the content of components other than the fluororesin particles and the filler particles is 3 mass% or less based on the total amount of the composition. The filler particles include at least silica particles, and other filler particles are preferably aluminum oxide, zinc oxide, titanium oxide, calcium carbonate, magnesium oxide, etc. Filler particles other than silica particles may not be used, or one type may be used, or two or more types may be mixed and used. The filler particles other than silica particles are preferably 0.1 to 80 mass% of the filler particles. It is particularly preferable to mix and mold only fluororesin particles and silica particles.

[0089] The fluororesin sheet before surface treatment obtained by the above-mentioned manufacturing method for a fluororesin sheet preferably has an oxygen element ratio of 1.5 atomic % or more at least on the surface to be surface-treated, as measured by X-ray photoelectron spectroscopy (XPS). The presence of oxygen element on the surface of the fluororesin sheet before surface treatment enables good adhesion to copper foil having a smooth surface. In addition, such a range is preferable in order to set the oxygen element ratio of the fluororesin sheet after surface treatment in the above-mentioned specific range as measured by X-ray photoelectron spectroscopy (XPS). The oxygen atomic ratio is preferably 1.65 atomic % or more, more preferably 1.7 atomic % or more, and even more preferably 1.8 atomic % or more. There is no particular upper limit, but in consideration of the effect on productivity and other physical properties, it is preferably 4.9 atomic % or less. The method for adjusting the oxygen element ratio of the fluororesin sheet before surface treatment to fall within the above range is not particularly limited, and may be controlled, for example, by adjusting the blending amount of silica particles or the molding method.

[0090] The fluororesin sheet before surface treatment preferably has a silicon element ratio of 0.2 atomic% or more at least on the surface to be surface-treated, as measured by X-ray photoelectron spectroscopy (XPS). The presence of silicon element on the surface of the fluororesin sheet before surface treatment enables good adhesion to copper foil having a smooth surface. This range is also preferable so that the silicon element ratio of the fluororesin sheet after surface treatment, as measured by X-ray photoelectron spectroscopy (XPS), is preferably 0.5 atomic% or more. The silicon element ratio is preferably 0.3 atomic % or more, more preferably 0.5 atomic % or more, and even more preferably 0.7 atomic % or more. There is no particular upper limit, but in consideration of the effect on productivity and other physical properties, it is preferably 2.0 atomic % or less. The silicon element ratio of the fluororesin sheet before surface treatment can be adjusted to fall within the above range by, for example, adjusting the blending amount of silica particles.

[0091] (Surface treatment) The fluororesin sheet obtained by the above method can be made to satisfy the above requirements by performing a surface treatment on one or both sides of the sheet under appropriate conditions. Generally, it is difficult for a fluororesin to adhere to copper foil. For this reason, in the present disclosure, a surface treatment is performed on the fluororesin sheet to improve lamination properties. Generally, such a surface treatment is performed by increasing the amount of oxygen atoms on the resin surface.

[0092] The specific method for the above surface treatment is not particularly limited, and any known method can be used. The surface treatment of the fluororesin sheet can be carried out by conventional discharge treatment such as plasma discharge treatment, corona discharge treatment, glow discharge treatment, sputtering treatment, etc. Among these, plasma treatment is preferable.

[0093] The plasma treatment is a treatment in which the fluororesin sheet on the outer surface thereof is etched by bringing the fluororesin sheet into contact with plasma, thereby adding oxygen atoms, nitrogen atoms, and the like to the outer surface of the fluororesin sheet. For example, the surface free energy can be controlled by introducing oxygen gas, nitrogen gas, hydrogen gas, helium gas, argon gas, or the like into the discharge atmosphere.

[0094] Alternatively, the surface to be modified may be exposed to an atmosphere of an organic compound-containing inert gas, which is an inert gas containing an organic compound, and a high-frequency voltage is applied between the electrodes to cause a discharge, thereby generating active species on the surface, and then the surface treatment may be performed by introducing a functional group of the organic compound or graft polymerizing a polymerizable organic compound.

[0095] The organic compound in the organic compound-containing inert gas includes polymerizable or non-polymerizable organic compounds containing oxygen atoms, such as vinyl esters such as vinyl acetate and vinyl formate; acrylic esters such as glycidyl methacrylate; ethers such as vinyl ethyl ether, vinyl methyl ether, and glycidyl methyl ether; carboxylic acids such as acetic acid and formic acid; alcohols such as methyl alcohol, ethyl alcohol, phenol, and ethylene glycol; ketones such as acetone and methyl ethyl ketone; carboxylic esters such as ethyl acetate and ethyl formate; acrylic acids such as acrylic acid and methacrylic acid. Among these, vinyl esters, acrylic esters, and ketones are preferred because the modified surface is less likely to be deactivated, that is, because they have a long life, and because they are easy to handle in terms of safety. In particular, vinyl acetate and glycidyl methacrylate are preferred.

[0096] The concentration of the organic compound in the organic compound-containing inert gas varies depending on the type of the organic compound, the type of fluororesin to be surface-treated, etc., but is usually 0.1 to 3.0% by volume, preferably 0.1 to 1.0% by volume, more preferably 0.15 to 1.0% by volume, and even more preferably 0.30 to 1.0% by volume. The discharge conditions may be appropriately selected depending on the desired degree of surface treatment, the type of fluororesin, the type and concentration of the organic compound, etc. Usually, the discharge rate is 50 W·min / m 2 More than 1500W min / m 2 Less than 70W·min / m 2 More than 1400W min / m 2 Discharge treatment is carried out within the following range. The treatment temperature can be any temperature within the range of 0° C. to 100° C. A temperature of 80° C. or less is preferable due to concerns about stretching and wrinkling of the fluororesin sheet.

[0097] The fluororesin sheet of the present disclosure that has been surface-treated as described above can be used as a sheet for a circuit board by laminating it with other substrates. A laminate may also be formed by bonding copper foil to one or both sides of the above-mentioned fluororesin sheet. The present disclosure also relates to a copper clad laminate having a copper foil and the above-mentioned fluororesin sheet as essential layers. As described above, the fluororesin sheet containing the fluororesin and silica particles of the present disclosure has excellent adhesiveness. Therefore, a laminate in which the surface-treated surface of the fluororesin sheet of the present disclosure is directly laminated to the copper foil is preferred.

[0098] The copper foil preferably has a surface roughness (Rz) of 2.0 μm or less. When the surface roughness (Rz) is 2.0 μm or less, the interface between the copper foil and the fluororesin sheet becomes smooth, the metal interface conductivity becomes high, and the transmission loss is preferably small. At least the surface of the copper foil that is bonded to the fluororesin sheet described above has an Rz of 2.0 μm or less, and the Rz of the other surface is not particularly limited. The fluororesin sheet of the present disclosure has excellent adhesion to copper foil having a high smoothness of Rz 2.0 μm or less, further Rz 1.0 μm or less, and even further Rz 0.5 μm or less.

[0099] The above Rz is the sum of the highest point (maximum peak height: Rp) and the deepest point (maximum valley depth: Rv). The above Rz is the ten-point average roughness defined in JIS-B0601. In this specification, the above Rz is a value measured using a surface roughness meter (product name: Surfcom 470A, manufactured by Tokyo Seiki Co., Ltd.) with a measurement length of 4 mm.

[0100] The copper foil preferably has a surface roughness (Rq) of 0.01 to 0.15 μm. It is preferable that Rq is within the above range, since the metal interface conductivity can be increased and the transmission loss can be reduced satisfactorily. The copper foil may have an Rq of 0.01 to 0.15 μm on at least the surface that is bonded to the above-mentioned fluororesin sheet, and the other surface is not particularly limited in Rq. The Rq of the surface that is bonded to the fluororesin sheet is more preferably 0.015 to 0.1 μm, and even more preferably 0.03 to 0.08 μm. The above Rq is the root mean square height. In this specification, the above Rq is a value measured with a stylus surface roughness measuring instrument (product name: SE600A, manufactured by Kosaka Laboratory) with a measurement length of 4 mm.

[0101] The thickness of the copper foil is not particularly limited, but is preferably 1 to 100 μm, more preferably 5 to 50 μm, and even more preferably 9 to 35 μm.

[0102] The copper foil is not particularly limited, and specific examples thereof include rolled copper foil and electrolytic copper foil.

[0103] The copper foil having Rz of 2.0 μm or less and / or Rq of 0.01 to 0.15 μm is not particularly limited, and commercially available products can be used. Examples of such commercially available copper foils include electrolytic copper foil CF-T9DA-SV-18 (thickness 18 μm / Rz 0.85 μm / Rq 0.05 μm) (manufactured by Fukuda Metal Foil & Powder Co., Ltd.).

[0104] The copper foil may be surface-treated to increase the peel strength with the fluororesin sheet of the present disclosure.

[0105] The surface treatment is not particularly limited, but may be a silane coupling treatment, a plasma treatment, a corona treatment, a UV treatment, an electron beam treatment, etc., and the reactive functional group of the silane coupling agent is not particularly limited, but from the viewpoint of adhesion to the resin substrate such as the fluororesin sheet of the present disclosure, it is preferable to have at least one selected from an amino group, a (meth)acrylic group, a mercapto group, and an epoxy group at the end. In addition, the hydrolyzable group is not particularly limited, but may be an alkoxy group such as a methoxy group or an ethoxy group. The copper foil used in the present disclosure may have an anti-rust layer (such as an oxide film such as chromate), a heat-resistant layer, etc. formed thereon.

[0106] The surface-treated copper foil having a surface treatment layer of the above-mentioned silane compound on the copper foil surface can be produced by preparing a solution containing the silane compound and then surface treating the copper foil with this solution.

[0107] The copper foil may have a roughening treatment layer on the surface thereof from the viewpoint of improving adhesion to a resin substrate. In addition, if there is a risk that the roughening treatment will degrade the performance required in the present disclosure, the amount of roughening particles electrodeposited on the copper foil surface can be reduced as necessary, or the roughening treatment can be omitted.

[0108] Between the copper foil and the surface treatment layer, one or more layers selected from the group consisting of a heat-resistant treatment layer, a rust-proofing treatment layer, and a chromate treatment layer may be provided in order to improve various properties. These layers may be a single layer or multiple layers.

[0109] When the copper clad laminate of the present disclosure is formed by directly laminating the surface-treated surface of a fluororesin sheet and a copper foil, it is preferable that the peel strength of the interface between the copper foil and the fluororesin sheet is 0.5 kN / m or more. By using the fluororesin sheet of the present disclosure, the above-mentioned peel strength can be achieved. By setting the peel strength to 0.5 kN / m or more, the sheet can be suitably used as a copper-clad laminate or a circuit board, and the peel strength is preferably 0.7 kN / m or more. The upper limit of the peel strength is not particularly limited, but may be 3.0 kN / m or less. The peel strength here means the peel strength measured under the conditions described in the Examples.

[0110] In the case of a laminate in which a copper foil is bonded to the surface-treated surface of a fluororesin sheet that has been surface-treated on only one side, a separate surface treatment may be applied to the untreated side of the fluororesin sheet in order to improve the adhesion between the laminate and other materials.

[0111] The copper clad laminate of the present disclosure may further include layers other than the copper foil and the fluororesin sheet. The layers other than the copper foil and the fluororesin sheet are preferably layers made of at least one resin selected from the group consisting of polyimide, modified polyimide, liquid crystal polymer, polyphenylene sulfide, cycloolefin polymer, polystyrene, epoxy resin, bismaleimide, polyphenylene oxide, modified polyphenylene ether, polyphenylene ether, and polybutadiene.

[0112] The layer made of the resin, which is a layer other than the copper foil and the fluororesin sheet, may contain reinforcing fibers. The reinforcing fibers are not particularly limited, but for example, glass cloth, particularly low dielectric type, is preferable.

[0113] The layers other than the copper foil and the fluororesin sheet are not particularly limited as long as they are made of the above-mentioned resins, and the layers other than the copper foil and the fluororesin sheet preferably have a thickness of 12.5 to 260 μm.

[0114] In the copper clad laminate of the present disclosure, the copper foil layer may be formed on one or both sides of the rolled sheet. Methods for forming the copper foil layer include laminating (adhering) copper foil to the surface of the rolled sheet, vapor deposition, plating, and the like. The method for laminating the copper foil includes a method using heat pressing, etc. The heat pressing temperature is from the melting point of the sheet -150°C to the melting point of the sheet +40°C. The heat pressing time is, for example, 1 to 30 minutes.

[0115] For example, a suitable method is to laminate a fluororesin sheet and copper foil, heat the laminate at 180 to 390° C., and press mold the laminate at a pressure of 0.5 to 5 MPa in vacuum or in an inert gas atmosphere to produce a copper clad laminate. By performing press molding under such conditions, the fluororesin sheet does not deteriorate and can be bonded to the copper foil.

[0116] When obtaining the above-mentioned laminate configuration, the fluororesin sheet of the present disclosure is used by adhering copper foil to one or both sides. As described above, the fluororesin sheet of the present disclosure has excellent adhesiveness. Therefore, it also has excellent adhesiveness to copper foil having a high smoothness of Rz 2.0 μm or less.

[0117] Conventionally, copper foils used for circuit boards have been given a certain degree of unevenness on their surfaces to ensure adhesion to fluororesin sheets. However, in high-frequency applications, the presence of unevenness on the surface of copper foil is undesirable because it causes loss of electrical signals. The above laminate can obtain suitable adhesion even to copper foils with high smoothness, and is a laminate that can be suitably used as a circuit board.

[0118] The copper clad laminate of the present disclosure is used as a circuit board without any particular limitations on its application. The present disclosure also relates to a circuit board having the copper clad laminate.

[0119] Since the copper clad laminate of the present disclosure is also used as a circuit board, it is preferable that the metal interface conductivity is high. It is preferably 1.00 (1e7 S / m) or more, more preferably 3.00 (1e7 S / m) or more, and even more preferably 5.00 (1e7 S / m) or more. There is no particular upper limit, but it is preferably 6.00 (1e7 S / m) or less.

[0120] Since the copper clad laminate of the present disclosure is also used as a circuit board, it is preferable that the transmission loss is close to 0. The transmission loss at a frequency of 67 GHz is preferably −4.20 dB / 100 mm or more, more preferably −4.00 dB / 100 mm or more, and even more preferably −3.30 dB / 100 mm or more.

[0121] A circuit board is a plate-shaped component for electrically connecting electronic components such as semiconductors and capacitor chips and simultaneously arranging and fixing them in a limited space. The configuration of a circuit board formed from the derivative or copper-clad laminate of the present disclosure is not particularly limited. The circuit board may be any of a rigid board, a flexible board, and a rigid-flexible board. The circuit board may be any of a single-sided board, a board, a double-sided board, and a multilayer board (such as a pulled-up board). In particular, it can be suitably used for flexible boards and rigid boards. When the sheet of the present disclosure does not contain glass fiber or cloth made of glass fiber, it is suitable for flexible boards. In particular, it can be suitably used as a printed circuit board for high frequencies of 10 GHz or more.

[0122] In this disclosure, the high-frequency circuit does not only refer to a circuit that transmits only high-frequency signals, but also includes a circuit that has a transmission line that converts a high-frequency signal into a low-frequency signal and outputs the generated low-frequency signal to the outside, a transmission line for supplying power to drive high-frequency compatible components, and other transmission lines that transmit signals other than high-frequency signals, which are arranged on the same plane.The circuit can also be used as a circuit board for an antenna, a filter, etc. The present disclosure also relates to an antenna formed from the circuit board, and is particularly suitable as a millimeter wave antenna for mobility such as automobiles and aircraft.

[0123] The circuit board is not particularly limited, and can be produced by a general method using the above-mentioned copper clad laminate.

[0124] The fluororesin sheet and copper-clad laminate of the present disclosure are used as electric and electronic components, for example, antennas used in electronic devices and communication devices such as ETC, GPS, wireless LAN, and mobile phones, high-speed transmission connectors, CPU sockets, millimeter wave and quasi-millimeter wave radars such as collision prevention radars, RFID tags, capacitors, inverter parts, cable covering materials, insulating materials for secondary batteries such as lithium-ion batteries, speaker diaphragms, etc.

[0125] Examples of the high-speed communication compatible substrate include a base station antenna substrate, an antenna distribution substrate, a substrate for a remote radio head (RRH) which is a radio part of a wireless base station, a substrate for a control part or a baseband part (BBU: Base Band Unit) of a wireless base station, a transceiver substrate for high-speed communication, a substrate for a radio network controller (RNC), a substrate for a high-speed transmitter, a substrate for a high-speed receiver, a substrate for a high-speed signal multiplexing circuit, a substrate for WiFig using the 60 GHz band, and a substrate for data transfer used in a server for a data center. Examples of the high-speed communication compatible substrate include an antenna substrate, for example, a substrate for a massive multi-element antenna (Massive MIMO) for large-capacity communication required in the 5G and later standards. Further, a power receiving antenna for space transmission type wireless power supply by microwaves can also be mentioned. The fluororesin sheet of the present disclosure has good adhesion to a non-roughened copper foil with low transmission loss, so that when an antenna is obtained by processing a copper clad laminate including the fluororesin sheet of the present disclosure and a non-roughened copper foil, the gain is improved, and therefore the fluororesin sheet is particularly suitable for an antenna.

[0126] The fluororesin sheet of the present disclosure can be used not only as an insulator for a substrate but also as an insulator for a signal line coating material, for example, as an insulating coating material (e.g., insulating tube) for a waveguide for transmitting high-speed signals, a QSFP cable for a high-speed LAN, a coaxial cable for high-speed communication (e.g., SFP+ cable, QSFP+ cable, etc.), a coaxial cable for low loss, etc.

[0127] When using such high frequencies, materials used in electrical components such as connectors and communication devices such as casings are required to have stable electrical properties such as low relative dielectric constant (εr) and low dielectric tangent (tanδ). The fluororesin sheet of the present disclosure can also be used as an insulating material for such materials.

[0128] The fluororesin sheet of the present disclosure can also be used as an insulating material for connector printed wiring boards that require soldering. The fluororesin sheet of the present disclosure has excellent heat resistance, so problems are unlikely to occur even at high temperatures during soldering.

[0129] In dielectric waveguides, materials with low dielectric loss are required to transmit high-frequency millimeter waves or submillimeter waves with low loss. The fluororesin sheet of the present disclosure can also be used as an insulating material for dielectric waveguides that transmit millimeter waves, submillimeter waves, etc. Examples of dielectric waveguides include cylindrical dielectric lines, rectangular dielectric lines, elliptical dielectric lines, tubular dielectric lines, image lines, insulator image lines, trapped image lines, rib guides, strip dielectric lines, inverted strip lines, H guides, nonradiative dielectric lines (NRD guides), etc.

[0130] In this disclosure, mobility refers to all means and methods related to movement and transportation, including automobiles in general, such as private cars, buses, taxis, and trucks, as well as two-wheeled vehicles, such as motorcycles, bicycles, and mopeds, railways, senior cars, and compact personal mobility vehicles for one person.Mobility is not necessarily limited to vehicles that move on the ground, and may also be vehicles that move in the air or underwater.

[0131] The laminate for a circuit board may further include a base layer laminated on the copper foil layer and the above-mentioned fluororesin sheet. The base layer is not particularly limited, but examples thereof include a fabric layer made of glass fiber and a resin film layer.

[0132] The resin film used as the substrate layer is preferably a heat-resistant resin film or a thermosetting resin film. Examples of the heat-resistant resin film include polyimide, modified polyimide, liquid crystal polymer, polyphenylene sulfide, etc. Examples of the thermosetting resin include those containing epoxy resin, bismaleimide, polyphenylene oxide, modified polyphenylene ether, polyphenylene ether, polybutadiene, etc. The heat-resistant resin film and the thermosetting resin film may contain reinforcing fibers. The reinforcing fibers are not particularly limited, but for example, glass cloth, particularly low dielectric type, is preferable.

[0133] The heat-resistant resin film and the thermosetting resin film are not particularly limited in terms of dielectric properties, linear expansion coefficient, water absorption coefficient, and other properties, but for example, the dielectric constant at 20 GHz is preferably 3.8 or less, more preferably 3.4 or less, and even more preferably 3.2 or less. The dielectric loss tangent at 20 GHz is preferably 0.0030 or less, more preferably 0.0025 or less, and even more preferably 0.0020 or less. The linear expansion coefficient is preferably 100 ppm / °C or less, more preferably 70 ppm / °C or less, and even more preferably 40 ppm / °C or less. The water absorption coefficient is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.1% or less.

[0134] When a copper clad laminate, which essentially contains a fluororesin sheet and copper foil, is laminated with a substrate layer such as a resin film layer, the copper clad laminate can be laminated by adhering the fluororesin sheet layer side of the copper clad laminate to the substrate layer. In this case, the copper clad laminate may be used after a surface treatment is performed on the fluororesin sheet layer side before lamination to improve adhesion performance. The surface treatment here is not particularly limited, and examples thereof include the above-mentioned plasma treatment.

[0135] In the above laminate, the order in which the copper foil layer, the base material, and the above-mentioned fluororesin sheet are laminated and the manufacturing method are not particularly limited, and a layer configuration according to the purpose can be adopted. Specific examples of the lamination order include a base layer / fluororesin sheet / copper foil layer, a copper foil layer / fluororesin sheet / base layer / fluororesin sheet / copper foil layer, and a copper foil layer / base layer / fluororesin sheet / base layer / copper foil layer. If necessary, other layers may also be included. EXAMPLES

[0136] The present disclosure will be specifically described below based on examples. However, the present invention is not limited to the following examples. In the following examples, "parts" and "%" respectively represent "parts by mass" and "% by mass" unless otherwise specified.

[0137] Each of the obtained samples was evaluated based on the following criteria.

[0138] [Thickness of fluororesin sheet] Measurements were taken using a micrometer.

[0139] [XPS measurement of fluororesin sheet surface] The measurements were performed using a scanning X-ray photoelectron spectroscopy (XPS / ESCA) PHI5000VersaProbeII (ULVAC-PHI, Inc.).

[0140] Coefficient of Linear Expansion (CTE) TMA measurements were performed in tensile mode using a TMA-7100 (Hitachi High-Tech Science Corporation). A fluororesin sheet cut to a length of 20 mm, width of 5 mm, and thickness of 150 μm was used as a sample piece. The chuck distance was set to 10 mm, and the linear expansion coefficient was calculated from the displacement of the sample from 0 to 150°C at a heating rate of 2°C / min while applying a load of 49 mN.

[0141] [Dielectric constant and dielectric loss tangent of fluororesin sheet] The dielectric constant and dielectric loss tangent were measured at 25°C and 10 GHz using a split cylinder type dielectric constant / dielectric loss tangent measuring device (manufactured by EM Lab).

[0142] [Static contact angle of water] The static contact angle of water of the prepared fluororesin sheet was measured using a contact angle meter ("DropMaster" manufactured by Kyowa Interface Science Co., Ltd.) at 23°C, with a droplet volume of 2 μL, and 1 second after the droplet landed.

[0143] [Peel Strength] After the surface treatment, copper foil (CF-T9DA-SV-18, Rz = 0.85 μm, Rq = 0.05 μm, made by Fukuda Metal Foil Powder Co., Ltd.) was placed on top and bottom of the fluororesin sheet so that the treated surfaces were in close contact with the fluororesin sheet, and the sheets were then pressurized and heated in a vacuum heat press (360°C, 2.5 MPa, 300 s) to prepare samples. The obtained sample was cut into a strip of 10 mm width, and the peel strength was measured using a Tensilon universal testing machine (manufactured by Shimadzu Corporation) by gripping the unbonded portion of the strip sample with the upper and lower chucks of the Tensilon and pulling it at a speed of 50 mm per minute, and the obtained value was taken as the peel strength.

[0144] <How to make sheets A to G> (Paste extrusion molding) PTFE powder (average particle size: 500 μm, apparent density: 460 g / L, standard specific gravity: 2.17) and silica particles shown in Table 1 were weighed out to have the mass ratio shown in Table 1, and mixed in a mixer in the presence of dry ice. The temperature during mixing was -10°C or lower. Oil (Isopar H) was added at 18 to 23% to the obtained mixed powder, mixed, and aged for about 5 hours. The aged composition was preformed under a pressure of 3 MPa, and the preformed body was extruded at 40° C. and 50 mm / min to obtain an extrusion sample. The extruded sample was rolled with two rolls to obtain a sample with a film thickness of 125 μm, and then passed through a drying roll at 200° C. and dried. Furthermore, it was confirmed that it was possible to produce a sample with a film thickness of 30 μm by adjusting the gap and pressure between the two rolls.

[0145] <How to make Sheet H> (Powder rolling molding) PTFE powder (average particle size: 500 μm, apparent density: 460 g / L, standard specific gravity: 2.17) and silica particles shown in Table 1 were weighed out to obtain the mass ratio shown in Table 1, and stirred in a Wonder Crusher at room temperature with a setting of 6 for 30 seconds twice. The resulting mixture was rolled with two rolls (roll gap: set to 100 μm, roll temperature: 100° C.) to obtain a sample with a film thickness of 130 μm.

[0146] In each example, as shown in Table 1, spherical silica was used, such as SC6500-SQ (average particle size 2.1 μm) manufactured by Admatechs Co., Ltd., and SC6500-SQ (average particle size 2.1 μm) manufactured by Admatechs Co., Ltd. that had been surface-treated with 3-aminopropyltriethoxysilane (a treatment amount of 0.5% by mass or 1% by mass relative to the mass of the silica particles).

[0147] [Table 1]

[0148] (Examples 1 to 10) (Fluororesin sheet surface treatment) A fluororesin sheet was placed between the upper and lower electrodes in a treatment chamber (direct type plasma surface treatment device, manufactured by Air Water Corporation) equipped with upper and lower electrodes, and the treatment chamber was filled with the following mixed gas atmosphere. Then, discharge plasma treatment was performed on the surface of the fluororesin sheet for the treatment time shown in Table 2. (Treatment atmosphere) A: A mixture of argon, helium, and oxygen B: A mixture of argon, helium, nitrogen and oxygen The elemental composition of the surface-treated fluororesin sheet was measured by XPS.

[0149] Comparative Example 1 For sheet A, no surface treatment was performed, and the elemental composition was measured by XPS.

[0150] (Comparative Examples 2 to 4) The discharge plasma treatment of the surface of the fluororesin sheet was carried out in the same manner as in Example 5, except that sheets E to G were used. The elemental composition of the surface-treated fluororesin sheet was measured by XPS.

[0151] The results of Examples 1 to 10 and Comparative Examples 1 to 4 are shown in Table 2.

[0152] [Table 2]

[0153] [Metal interface conductivity measurement] The sheet prepared in Example 5 was overlaid with copper foil (CF-T9DA-SV-18, manufactured by Fukuda Metal Foil Powder) so that the treated surface of the foil was in close contact with the sheet, and the foil was inserted into a vacuum heat press, heated from room temperature to 360°C under vacuum, and pressed at 360°C with a pressure of 3MPa to prepare a double-sided copper-clad laminate. From the prepared double-sided copper-clad laminate, a circular dielectric sample (no copper on both sides) and a circular dielectric sample (circular copper foil patterning on one side) were prepared, and the metal layer interface conductivity (1e7 S / m) was measured in the frequency range of 14.5 GHz to 111.5 GHz using a balanced disk resonator method. The average metal layer interface conductivity of the double-sided copper-clad laminate prepared in Example 5 was 5.66 (1e7 S / m), which was equivalent to the reference copper disk.

[0154] In addition, the average metal layer interface conductivity was similarly measured using a commercially available RO3003 (manufactured by Rogers), which is a double-sided copper-clad laminate of a composite sheet of fluororesin and filler, and was found to be 0.56 (1e7 S / m). Therefore, it was clear that the double-sided copper-clad laminate using the sheet produced in Example 5 had a higher metal interface conductivity than commercially available double-sided copper-clad laminates.

[0155] [Transmission loss measurement] Copper foil (CF-T9DA-SV-18, Rz = 0.85 μm, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) was placed on top and bottom of the fluororesin sheet produced in Example 5 so that the treated surfaces were in close contact with the fluororesin sheet, and the sheets were inserted into a vacuum heat press. The temperature was increased from room temperature to 360°C under vacuum, and then the sheets were pressed at 360°C under a pressure of 3 MPa to produce a double-sided copper-clad laminate.

[0156] A microstrip line was used to form a transmission line on the prepared double-sided copper-clad laminate. The 50 and 68 GHz signals on the printed circuit board were processed using a network analyzer (Keysight Technologies, "E8361A"), and the S21 parameter, which indicates the transmission loss, was measured using a Universal Test Fixture as a probe. The characteristic impedance of the line was set to 50 Ω, and the length of the transmission line on the printed circuit board was set to 100 mm, and the transmission loss was measured. As a measure of transmission loss, we used the "S21-parameter," which is one of the circuit network parameters used to express the characteristics of high-frequency electronic circuits and components. The closer this value is to 0, the smaller the transmission loss is.

[0157] The transmission loss was -2.42 dB / 100 mm at a frequency of 50 GHz and -2.96 dB / 100 mm at a frequency of 67 GHz. In addition, similar transmission loss measurements were performed using the commercially available RO3003G2 (manufactured by Rogers), which is a double-sided copper-clad laminate of a composite sheet of fluororesin and filler. The transmission loss was -3.47 dB / 100 mm at a frequency of 50 GHz and -4.53 dB / 100 mm at a frequency of 67 GHz. Therefore, it was clear that the double-sided copper-clad laminate using the fluororesin sheet produced in Example 5 had lower transmission loss than commercially available double-sided copper-clad laminates.

[0158] The above experimental results show that the fluororesin sheets of the examples have a low CTE and can be well bonded to copper foil with high smoothness, and that laminates with copper foil with high smoothness have high metal interface conductivity and low transmission loss, making them suitable for use as circuit board materials. [Industrial Applicability]

[0159] The fluororesin sheet of the present disclosure can be suitably used for copper-clad laminates for circuit boards.

Claims

1. A fluororesin sheet comprising polytetrafluoroethylene and silica particles, A fluororesin sheet having an oxygen element ratio of 3.0 atomic % or more on one or both sides thereof as measured by X-ray photoelectron spectroscopy (XPS) and a coefficient of linear expansion (CTE) of 100 ppm / ° C. or less.

2. 2. The fluororesin sheet according to claim 1, wherein the nitrogen element ratio on said surface is 1.35 atomic % or more when measured by X-ray photoelectron spectroscopy (XPS).

3. 3. The fluororesin sheet according to claim 1, wherein the surface has a silicon element ratio of 0.5 atomic % or more as measured by X-ray photoelectron spectroscopy (XPS).

4. 3. The fluororesin sheet according to claim 1, wherein the static contact angle of water on said surface is 105° or less, measured one second after a 2 μL droplet is deposited on said surface.

5. 3. The fluororesin sheet according to claim 1, wherein the silica particles are spherical silica.

6. 3. The fluororesin sheet according to claim 1, wherein the silica particles are silica particles treated with a silane coupling agent.

7. 3. The fluororesin sheet according to claim 1, wherein the silica particles have an average particle size of 10 μm or less.

8. 3. The fluororesin sheet according to claim 1 or 2, which does not contain glass fibers.

9. 3. The fluororesin sheet according to claim 1, wherein the content of the silica particles in the total amount of the fluororesin sheet is 30 mass % or more.

10. 3. The sheet according to claim 1, wherein the content of the silica particles in the total amount of the fluororesin sheet is 50% by mass or more.

11. 3. The sheet according to claim 1, wherein the content of the silica particles in the total amount of the fluororesin sheet is from 50% by mass to 65% by mass.

12. 3. The fluororesin sheet according to claim 1, which has a dielectric loss tangent of 0.0015 or less at 10 GHz.

13. 3. The fluororesin sheet according to claim 1, having a thickness of 5 to 250 μm.

14. 3. A method for producing a fluororesin sheet according to claim 1 or 2, comprising mixing fluororesin particles and silica particles to form a film, and then performing a surface treatment.

15. The method for producing a fluororesin sheet according to claim 14, characterized in that a film is formed using a composition substantially consisting of fluororesin particles and filler particles containing at least silica particles, and then the surface is treated.

16. 3. A copper clad laminate comprising a copper foil and the fluororesin sheet according to claim 1 or 2 as essential layers.

17. The copper clad laminate according to claim 16, wherein the surface roughness (Rz) of the copper foil is 2.0 μm or less.

18. The copper clad laminate according to claim 16, wherein the surface roughness (Rq) of the copper foil is 0.01 to 0.15 μm.

19. 17. The copper clad laminate according to claim 16, wherein the copper foil and the fluororesin sheet are directly laminated together, and the peel strength of the interface between the copper foil and the fluororesin sheet is 0.5 kN / m or more.

20. A method for producing a copper clad laminate according to claim 16, comprising laminating the fluororesin sheet according to claim 1 and a copper foil, heating the laminate at 180 to 390°C, and press-molding the laminate at a pressure of 0.5 to 5 MPa under vacuum or in an inert gas atmosphere.

21. A circuit board comprising the copper clad laminate of claim 16.

22. 22. An antenna formed from the circuit board of claim 21.

23. 23. The antenna of claim 22, which is a millimeter wave antenna for mobility.

Citation Information

Patent Citations

  • Printed wiring board for high frequency use

    JP2015008260A

  • Insulating resin material, insulating resin material with metal layer using the same, and wiring board

    JP2021061406A

  • Fluororesin film, copper-clad laminate and substrate for circuits

    JP2022112028A

  • Low-dielectric metal-clad fluororesin substrate and method of manufacturing the same

    JP2022114351A

  • Liquid composition and method for producing film and laminate using the liquid composition

    JP2022140517A