Bioelectrode composition, bioelectrode, method for producing bioelectrode, and reaction complex
The bioelectrode composition, combining ionic polymers and carbon particles with specific salts and resins, addresses conductivity and biocompatibility issues, ensuring stable signal transmission and adhesion, suitable for long-term wearable devices.
Patent Information
- Application Number
- JP2021170179
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-05
- Filing Date
- 2021-10-18
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-10-18
AI Technical Summary
Existing bioelectrodes for wearable devices face challenges in maintaining conductivity and biocompatibility over long-term use, often causing skin allergies and losing conductivity when wet or dry, while being costly and lacking flexibility and adhesion.
A bioelectrode composition comprising a reaction complex of ionic polymers and carbon particles, with specific repeating units and additives, forming a biocontact layer that maintains conductivity and biocompatibility, even when wet or dry, using ammonium, lithium, sodium, or silver salts of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide, combined with adhesive resins and conductive powders.
The bioelectrode composition ensures stable electrical signal transmission with high sensitivity and biocompatibility, maintaining conductivity without significant decrease, even when worn for extended periods, and is lightweight and cost-effective.
Smart Images

Figure 0007569298000117 
Figure 0007569298000118 
Figure 0007569298000119
Abstract
Description
[Technical field]
[0001] The present invention relates to a bioelectrode that can be brought into contact with the skin of a living body and detect a bodily condition such as heart rate by an electrical signal from the skin, a method for producing the same, and a bioelectrode composition that is suitably used for the bioelectrode. [Background technology]
[0002] In recent years, the development of wearable devices has progressed with the spread of IoT (Internet of Things). Typical examples are watches and glasses that can connect to the Internet. In addition, wearable devices that can constantly monitor the condition of the body are needed in the medical and sports fields, and these are expected to be growth fields in the future.
[0003] In the medical field, wearable devices that monitor the state of the body's organs by sensing weak currents, such as in electrocardiograms, which detect the movement of the heart through electrical signals, are being considered. In electrocardiograms, electrodes coated with conductive paste are attached to the body to perform the measurement, but this is a one-time, short-term measurement. In contrast, the aim of developing medical wearable devices such as those mentioned above is to develop devices that constantly monitor the health state for several weeks in a row. Therefore, the bioelectrodes used in medical wearable devices are required to have no change in conductivity even when used for long periods of time and to be free of skin allergies. In addition to these, they are also required to be lightweight and to be able to be manufactured at low cost.
[0004] Wearable medical devices include those that are attached to the body and those that are incorporated into clothing. As a type that is attached to the body, a bioelectrode that uses a water-soluble gel containing water and electrolytes, which are the materials for the conductive paste mentioned above, has been proposed (Patent Document 1). The water-soluble gel contains sodium, potassium, and calcium as electrolytes in a water-soluble polymer that holds water, and converts changes in ion concentration from the skin into electricity. On the other hand, as a type that is incorporated into clothing, a method has been proposed in which a conductive polymer such as PEDOT-PSS (Poly-3,4-ethylenedioxythiophene-Polystyrenesulfonate) or cloth with silver paste incorporated into the fibers is used as an electrode (Patent Document 2).
[0005] However, when using the above-mentioned water-soluble gel containing water and electrolytes, there is a problem that the conductivity is lost when the water dries out. On the other hand, when using metals with a high ionization tendency such as copper, there is a problem that some people may develop skin allergies, and when using conductive polymers such as PEDOT-PSS, there is a problem that the conductive polymer is highly acidic and therefore may develop skin allergies, and the conductive polymer may peel off from the fibers during washing.
[0006] In addition, because of their excellent electrical conductivity, the use of metal nanowires, carbon black, carbon nanotubes, and the like as electrode materials has also been considered (Patent Documents 3, 4, 5). Metal nanowires have a high probability of contact between wires, so they can conduct electricity with a small amount of additive. However, metal nanowires are thin materials with sharp tips, which can cause skin allergies. Thus, even if the material itself does not cause an allergic reaction, the shape and irritation of the material can cause the material to have poor biocompatibility, making it difficult to achieve both electrical conductivity and biocompatibility.
[0007] Metal films are highly conductive and one would think they would function as excellent bioelectrodes, but this is not necessarily the case. When the heart beats, not only a weak current is released from the skin, but sodium ions, potassium ions, and calcium ions are also released. For this reason, it is necessary to convert the change in ion concentration into electric current, but precious metals, which are difficult to ionize, are inefficient at converting ions from the skin into electric current. Therefore, bioelectrodes using precious metals have high impedance and there is high resistance to electrical current passing through the skin.
[0008] On the other hand, batteries to which ionic liquids have been added are being considered (Patent Document 6). Ionic liquids are characterized by high thermal and chemical stability and excellent electrical conductivity, and are being widely used in batteries. However, since ionic liquids with small molecular weights as shown in Patent Document 6 dissolve in water, when a bioelectrode to which this has been added is used, the ionic liquid is extracted by sweat from the skin, which not only reduces electrical conductivity but also penetrates the skin and causes rough skin.
[0009] In addition, a battery using a lithium salt of a polymer-type sulfonimide is being studied (Non-Patent Document 1). However, although lithium is applied to batteries because of its high ion mobility, it is not a biocompatible material. Furthermore, a lithium salt of fluorosulfonic acid pendant on silicone is also being studied (Non-Patent Document 2).
[0010] When the bioelectrode is separated from the skin, it is no longer able to obtain information from the body. Furthermore, even a change in the contact area causes a fluctuation in the amount of electricity passing through, and the baseline of the electrocardiogram (electrical signal) fluctuates. Therefore, in order to obtain a stable electrical signal from the body, it is necessary for the bioelectrode to be in constant contact with the skin and for the contact area to remain constant. For this reason, it is preferable for the bioelectrode to have adhesive properties. It is also necessary for the bioelectrode to have elasticity and flexibility so that it can follow the expansion and contraction and bending changes of the skin.
[0011] A bioelectrode is being considered in which the part that comes into contact with the skin is made of silver chloride, and the part that conducts to the device is laminated with silver. Solid silver chloride has no adhesive power to the skin and is not elastic, so its ability to collect biosignals decreases, especially when the human body moves. For this reason, a laminated film of silver chloride and silver is used as a bioelectrode with a water-soluble gel laminated between the skin. In this case, the aforementioned gel will dry out and cause deterioration.
[0012] It has been reported that when carbon black is mixed with an epoxy resin, the curing reaction proceeds at a lower temperature than when only the epoxy resin is used. This is because the crosslinking reaction proceeds at a lower temperature due to the reaction between the carboxyl groups and epoxy groups present on the carbon black surface (Non-Patent Document 3).
[0013] A lithium-ion battery using graphene oxide as a conductive additive has been reported (Patent Document 7). In this case, graphene oxide is used as a binder to improve the dispersibility and conductivity of the positive electrode material such as lithium cobalt oxide. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] International Publication No. WO2013-039151 [Patent Document 2] JP 2015-100673 A [Patent Document 3] Japanese Patent Application Publication No. 5-095924 [Patent Document 4] JP 2003-225217 A [Patent Document 5] JP 2015-019806 A [Patent Document 6] Special Publication No. 2004-527902 [Patent Document 7] JP 2020-140973 A [Non-patent literature]
[0015] [Non-Patent Document 1] J.Mater.Chem.A,2016,4,p10038-10069 [Non-Patent Document 2] J. of the Electrochemical Society, 150(8) A1090-A1094 (2003) [Non-Patent Document 3] Polymer Papers Vol.41, No.10, p597-603(1984) Summary of the Invention [Problem to be solved by the invention]
[0016] The present invention has been made to solve the above problems, and aims to provide a bioelectrode composition capable of forming a biocontact layer for a bioelectrode that has excellent electrical conductivity and biocompatibility, is lightweight, can be produced at low cost, and does not significantly decrease in conductivity whether wetted with water or dried; a bioelectrode in which a biocontact layer is formed from the bioelectrode composition; and a method for producing the same. [Means for solving the problem]
[0017] In order to solve the above problems, the present invention provides A bioelectrode composition comprising: (A) a reaction complex of an ionic polymer material and carbon particles; The component (A) contains carbon particles bonded to a polymer having a repeating unit having a structure selected from the group consisting of the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide.
[0018] Such a bioelectrode composition can provide a bioelectrode composition capable of forming a biocontact layer for a bioelectrode that has excellent electrical conductivity and biocompatibility, is lightweight, can be produced at low cost, and does not significantly decrease in electrical conductivity whether it is wetted with water or dried.
[0019] The carbon particles are preferably selected from carbon black, carbon nanotubes, graphite, and graphene.
[0020] Such carbon particles can be suitably used.
[0021] In addition, it is preferable that the repeating unit having a structure selected from the group consisting of the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide has a structure represented by any of the following general formulas (1)-1 to (1)-4. [ka] (In the formula, Rf1 and Rf2 are a hydrogen atom, a fluorine atom, an oxygen atom, a methyl group, or a trifluoromethyl group. When Rf1 and Rf2 are oxygen atoms, Rf1 and Rf2 are one oxygen atom bonding to one carbon atom to form a carbonyl group. Rf3 and Rf4 are a hydrogen atom, a fluorine atom, or a trifluoromethyl group. At least one of Rf1 to Rf4 is a fluorine atom or a trifluoromethyl group. Rf5, Rf6, and Rf7 are a fluorine atom or a linear or branched alkyl group having 1 to 4 carbon atoms and having at least one fluorine atom. m is an integer of 1 to 4. M + is an ion selected from ammonium ion, lithium ion, sodium ion, potassium ion, and silver ion.
[0022] Furthermore, the repeating unit having a structure selected from the group consisting of the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide is preferably one or more selected from the repeating units a1 to a7 represented by the following general formula (2). [ka] (In the formula, R 1 , R 3 , R 5 , R 8 , R 10 , R 11 and R 13 are each independently a hydrogen atom or a methyl group, R 2 , R 4 , R 6 , R 9 , R 12 and R 14 R each independently represents a single bond, or a linear, branched or cyclic hydrocarbon group having 1 to 13 carbon atoms which may have either an ester group or an ether group, or both. 7 is a linear or branched alkylene group having 1 to 4 carbon atoms; R 7 In the formula, one or two of the hydrogen atoms may be substituted with a fluorine atom. Each of X1, X2, X3, X4, X6, and X7 is independently a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group, and X5 is a single bond, an ether group, or an ester group. Y is an oxygen atom, -NR 19 - group, and R 19 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 4 may be bonded to form a ring. m is an integer of 1 to 4. a1, a2, a3, a4, a5, a6, and a7 each satisfy 0≦a1≦1.0, 0≦a2≦1.0, 0≦a3≦1.0, 0≦a4≦1.0, 0≦a5≦1.0, 0≦a6≦1.0, and 0≦a7≦1.0, <a1+a2+a3+a4+a5+a6+a7≦1.0である。M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion. Rf5, Rf6, and Rf7 are a fluorine atom, or a linear or branched alkyl group having 1 to 4 carbon atoms, and have at least one fluorine atom.
[0023] In addition, it is preferable that the component (A) contains a complex obtained by reacting carbon particles with a polymer that reacts with carbon particles and that is copolymerized with a repeating unit b1 having an oxirane group or an oxetane group, or a repeating unit b2 having an isocyanate group, as represented by the following general formula (4), in addition to the repeating unit represented by the general formula (2): [ka] (In the formula, R 20 , R 24 is a hydrogen atom or a methyl group, X8 is a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group, X9 is an ester group, R 21 R is a single bond, a linear, branched or cyclic alkylene group having 1 to 20 carbon atoms, or a phenylene group, which may contain an ether group, an ester group or a hydroxyl group. 22 are hydrogen atoms or identical or non-identical alkyl groups having 1 to 4 carbon atoms, and R 21 R may be bonded to form a ring. 23 is a methylene group or an ethylene group, and R 21 R may be bonded to form a ring. 25 R is a linear or branched alkylene group having 1 to 20 carbon atoms, and may have an ether group. 26 is a single bond or a methylene group. B is an isocyanate group, which may be a blocked isocyanate group. 0≦b1<1.0, 0≦b2<1.0, 0 <b1+b2<1.0である。)
[0024] Furthermore, the component (A) is preferably one in which 100 parts by mass of carbon particles are reacted with 5 parts by mass or more of a polymer that reacts with the carbon particles.
[0025] Furthermore, the component (A) preferably contains, as the ammonium ion constituting the ammonium salt, an ammonium ion represented by the following general formula (3). [ka] (In the formula, R101d , R 101e , R 101f , R 101g R is a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 13 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , R 101d and R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e and R 101d and R 101e and R 101f is an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the ring.
[0026] In such a bioelectrode composition, an ionic polymer material (hereinafter, the ionic polymer material is also referred to as an ionic polymer) is pendant to the carbon particles, thereby improving both ionic conductivity and electronic conductivity, and not only improving the sensitivity of the bioelectrode, but also preventing the ionic polymer from being extracted from the bioelectrode membrane, preventing a decrease in sensitivity of the biosignal due to extraction, and reducing skin permeability and skin irritation, thereby more effectively preventing the ionic polymer from passing through the skin and causing allergies.
[0027] It is preferable that the adhesive composition further contains a tackifying resin as component (B).
[0028] The component (B) is preferably at least one selected from a silicone resin, a (meth)acrylate resin, and a urethane resin.
[0029] Such a device can be in constant contact with the skin and can provide a stable electrical signal for a long period of time.
[0030] The component (B) preferably contains a diorganosiloxane having an alkenyl group and an organohydrogenpolysiloxane having a SiH group.
[0031] The component (B) further includes R x SiO (4-x) / 2 It is preferable that the silicone resin contains a silicone resin having a unit (R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and x is in the range of 2.5 to 3.5) and a SiO2 unit.
[0032] Such a composition can be suitably used as a bioelectrode composition.
[0033] Furthermore, the component (C) preferably contains a polymeric compound having an ionic repeating unit.
[0034] In addition, it is preferable that the ionic repeating unit of the component (C) contains a repeating unit having a structure selected from the group consisting of the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide, as represented by the following general formula (2): [ka] (In the formula, R 1 , R 3 , R 5 , R 8 , R 10 , R 11 and R 13 are each independently a hydrogen atom or a methyl group, R 2 , R 4 , R 6 , R 9 , R 12 and R 14R each independently represents a single bond, or a linear, branched or cyclic hydrocarbon group having 1 to 13 carbon atoms which may have either an ester group or an ether group, or both. 7 is a linear or branched alkylene group having 1 to 4 carbon atoms; R 7 In the formula, one or two of the hydrogen atoms may be substituted with a fluorine atom. Each of X1, X2, X3, X4, X6, and X7 is independently a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group, and X5 is a single bond, an ether group, or an ester group. Y is an oxygen atom, -NR 19 - group, and R 19 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 4 may be bonded to form a ring. m is an integer of 1 to 4. a1, a2, a3, a4, a5, a6, and a7 each satisfy 0≦a1≦1.0, 0≦a2≦1.0, 0≦a3≦1.0, 0≦a4≦1.0, 0≦a5≦1.0, 0≦a6≦1.0, and 0≦a7≦1.0, <a1+a2+a3+a4+a5+a6+a7≦1.0である。M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion. Rf5, Rf6, and Rf7 are a fluorine atom, or a linear or branched alkyl group having 1 to 4 carbon atoms, and have at least one fluorine atom.
[0035] A bioelectrode composition containing a polymer compound having such a repeating unit can further improve the effects of the present invention.
[0036] Furthermore, it is preferable that the component (D) contains carbon powder and / or metal powder.
[0037] The carbon powder is preferably at least one of carbon black, graphite, and carbon nanotubes.
[0038] The metal powder is preferably a metal powder selected from the group consisting of gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium.
[0039] The metal powder is preferably silver powder.
[0040] This will result in even better electrical conductivity.
[0041] It is preferable that the component (E) further contains an organic solvent.
[0042] In this case, the coating properties of the bioelectrode composition are further improved.
[0043] Furthermore, the present invention provides a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, wherein the biocontact layer is a cured product of the bioelectrode composition.
[0044] The bioelectrode of the present invention is a bioelectrode that has excellent electrical conductivity and biocompatibility, is lightweight, can be manufactured at low cost, and does not experience a significant decrease in electrical conductivity even when wetted or dried.
[0045] In addition, the conductive substrate preferably contains one or more metals selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
[0046] In the bioelectrode of the present invention, such a conductive substrate can be particularly suitably used.
[0047] Furthermore, the present invention provides a method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, in which the bioelectrode composition is applied to the conductive substrate and cured to form the biocontact layer.
[0048] The manufacturing method of the bioelectrode of the present invention makes it possible to easily manufacture a bioelectrode that has excellent conductivity and biocompatibility, is lightweight, and can be manufactured at low cost, and whose conductivity does not decrease significantly even when it gets wet or dried.
[0049] In addition, the method for manufacturing a bioelectrode preferably uses, as the conductive base material, one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and a conductive polymer.
[0050] In the method for producing a bioelectrode of the present invention, such a conductive substrate can be particularly suitably used.
[0051] The present invention also provides a reaction complex between an ionic polymer material and carbon particles, the reaction complex being carbon particles bonded to a polymer having a repeating unit having a structure selected from the group consisting of the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide.
[0052] The carbon particles are preferably selected from carbon black, carbon nanotubes, graphite, and graphene.
[0053] By modifying the carbon particles with an ionic polymer, the carbon particles become particularly useful as a component of a bioelectrode composition that can form a biocontact layer for a bioelectrode that can transmit ions and electrical signals released from the skin to the device with high sensitivity and efficiency (i.e., excellent conductivity), does not cause allergies even when worn on the skin for a long period of time (i.e., excellent biocompatibility), and does not significantly decrease in conductivity whether wetted or dried. Effect of the Invention
[0054] As described above, the bioelectrode composition containing the carbon particles (reaction complex of an ionic polymer material and carbon particles) bound to the ionic polymer of the present invention can efficiently transmit electrical signals from the skin to the device (i.e., has excellent electrical conductivity), is not likely to cause allergies even when worn on the skin for a long period of time (i.e., has excellent biocompatibility), is lightweight, can be manufactured at low cost, and can form a biocontact layer for a bioelectrode that does not significantly decrease in electrical conductivity even when wet or dried. Furthermore, the electrical conductivity can be further improved by adding an ionic polymer compound or a conductive powder (carbon powder, metal powder), and a bioelectrode with particularly high adhesive strength and high elasticity can be manufactured by combining it with a resin having adhesiveness and elasticity. Furthermore, the elasticity and adhesiveness to the skin can be improved by additives, and the elasticity and adhesiveness can be adjusted by appropriately adjusting the composition of the resin and the thickness of the biocontact layer.
[0055] Furthermore, the bioelectrode of the present invention can achieve both electrical conductivity and biocompatibility due to the carbon particles bonded to the above-mentioned ionic polymer, and since it is also adhesive, the contact area with the skin is constant, making it possible to obtain electrical signals from the skin stably and with high sensitivity.
[0056] Furthermore, the manufacturing method of the bioelectrode of the present invention makes it possible to easily manufacture, at low cost, the bioelectrode of the present invention, which has excellent conductivity and biocompatibility, is lightweight, and whose conductivity does not decrease significantly whether it is wetted with water or dried. [Brief description of the drawings]
[0057] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a bioelectrode of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the bioelectrode of the present invention attached to a living body. [Diagram 3] FIG. 2 is a schematic diagram of a bioelectrode produced in an example of the present invention after printing. [Figure 4] FIG. 2 is a schematic diagram showing one of the bioelectrodes produced in the examples of the present invention cut out and with an adhesive layer attached. [Diagram 5] FIG. 2 is a diagram showing the locations where electrodes and a ground are attached to the human body when measuring a biosignal in an embodiment of the present invention. [Figure 6] 1 is an electrocardiogram waveform obtained using a bioelectrode according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0058] As described above, there has been a need to develop a bioelectrode composition capable of forming a biocontact layer for a bioelectrode that has high electrical conductivity and excellent biocompatibility for generating highly sensitive and low-noise biosignals, is lightweight, can be manufactured at low cost, does not significantly decrease in electrical conductivity whether wetted with water or dried, and leaves no residue on the skin after being peeled off from the skin; a bioelectrode in which a biocontact layer is formed from the bioelectrode composition; and a method for manufacturing the same.
[0059] Sodium, potassium, and calcium ions are released from the skin surface in tandem with the heartbeat. The bioelectrode must convert the increase or decrease in the ions released from the skin into an electrical signal. To do this, a material with excellent ionic conductivity is required to transmit the increase or decrease in ions. The electrical potential of the skin surface also fluctuates in tandem with the heartbeat. This potential fluctuation is slight, so electronic conductivity is also required to transmit a weak current to the device.
[0060] Water-soluble gels containing sodium chloride or potassium chloride have high ionic and electronic conductivity, but lose their conductivity when the water dries up. The conductivity also decreases when sodium chloride or potassium chloride dissolves out of the bioelectrode during bathing or showering.
[0061] Bioelectrodes using metals such as gold and silver detect only weak currents and have low ionic conductivity, making them less sensitive as bioelectrodes. Carbon has electronic conductivity like metals, but its electronic conductivity is lower than that of metals, making it less sensitive as a bioelectrode.
[0062] Conductive polymers such as PEDOT-PSS have both electronic and ionic conductivity, but their ionic conductivity is low due to their low polarization.
[0063] The salts of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide have high polarizability and high ionic conductivity. The aim of the present invention is to achieve high ionic and electronic conductivity by combining these with carbon particles.
[0064] In order to stably obtain biosignals by attaching the electrode to the skin, the electrode film needs to be adhesive. On the other hand, if the electrode film is left on the skin after being attached for a long time and then peeled off, it may cause rashes or rough skin. In order to prevent the residue from being left on the skin, it is necessary to make the electrode film in the form of an ionic polymer bonded to carbon particles, and this led to the present invention.
[0065] The present inventors propose a bioelectrode composition containing an ionic polymer bound to carbon particles, and a bioelectrode obtained by curing the same.
[0066] When the acidity of the acid that forms the neutralized salt is high, the ions are strongly polarized, improving ionic conductivity. This is why lithium salts of bis(trifluoromethanesulfonyl)imide acid and tris(trifluoromethanesulfonyl)methide acid show high ionic conductivity in lithium-ion batteries. On the other hand, the higher the acid strength of the acid before it becomes a neutralized salt, the stronger the bioirritation of the salt. In other words, there is a trade-off between ionic conductivity and bioirritation. However, salts to be applied to bioelectrodes must have both high ionic conductivity and low bioirritation.
[0067] The larger the molecular weight of an ionic compound, the less the skin permeability and the less irritation to the skin. For this reason, the ionic compound is preferably a polymer type with a high molecular weight. Therefore, the present inventors have come up with the idea that by polymerizing the ionic compound into a form having a polymerizable double bond and further adding a reaction complex in which the polymerized ionic polymer and carbon particles are bonded, no residue is left even when the ionic compound is peeled off after being attached to the skin for a long time.
[0068] Furthermore, the inventors have discovered that by mixing this salt with, for example, a silicone-, acrylic-, or urethane-based adhesive (resin), the adhesive can be in constant contact with the skin and a stable electrical signal can be obtained for a long period of time.
[0069] In order to construct a highly sensitive bioelectrode, not only high ionic conductivity is important, but also high electronic conductivity. Adding metal powder or carbon powder is effective in increasing electronic conductivity.
[0070] That is, the present invention provides: A bioelectrode composition comprising: (A) a reaction complex of an ionic polymer material and carbon particles; The component (A) is a bioelectrode composition containing carbon particles bonded to a polymer having a repeating unit having a structure selected from the group consisting of the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide.
[0071] The present invention will be described in detail below, but the present invention is not limited thereto.
[0072] <Bioelectrode composition> The bioelectrode composition of the present invention contains (A) a reaction complex of an ionic polymer material and carbon particles, and preferably (B) an adhesive resin. Each component will be described in more detail below. In the following, the reaction complex of the ionic polymer material and carbon particles will be referred to as "component (A)", the adhesive resin as "component (B)", the blended ionic polymer as "component (C)", the conductive powder as "component (D)", the organic solvent as "component (E)", and other additives as "component (F)".
[0073] [(A) Reaction complex (salt) of ionic polymer material and carbon particles] In the bioelectrode composition of the present invention, the reaction complex salt (A) between an ionic polymer material and carbon particles is carbon particles bonded to a polymer (ionic polymer) having a repeating unit having a structure selected from the group consisting of ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide. Preferably, the polymer further has a repeating unit having an oxirane group, oxetane group, or isocyanate group, and is a material in which the polymer is bonded to carbon particles by reaction.
[0074] The structure of the ammonium salt, lithium salt, sodium salt, potassium salt, or silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide is preferably one represented by the following general formulas (1)-1 to (1)-4. [ka] (In the formula, Rf1 and Rf2 are a hydrogen atom, a fluorine atom, an oxygen atom, a methyl group, or a trifluoromethyl group. When Rf1 and Rf2 are oxygen atoms, Rf1 and Rf2 are one oxygen atom bonding to one carbon atom to form a carbonyl group. Rf3 and Rf4 are a hydrogen atom, a fluorine atom, or a trifluoromethyl group. At least one of Rf1 to Rf4 is a fluorine atom or a trifluoromethyl group. Rf5, Rf6, and Rf7 are a fluorine atom or a linear or branched alkyl group having 1 to 4 carbon atoms and having at least one fluorine atom. m is an integer of 1 to 4. M + is an ion selected from ammonium ion, lithium ion, sodium ion, potassium ion, and silver ion.
[0075] The repeating unit having a structure selected from the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of fluorosulfonic acid represented by general formula (1)-1 or (1)-2, fluorosulfonimide represented by (1)-3, and N-carbonylfluorosulfonamide represented by (1)-4 is preferably one or more selected from repeating units a1 to a7 represented by general formula (2) below. [ka] (In the formula, R 1 , R 3 , R 5 , R 8 , R 10 , R 11 and R 13 are each independently a hydrogen atom or a methyl group, R 2 , R 4 , R 6 , R 9 , R 12 and R 14 R each independently represents a single bond, or a linear, branched or cyclic hydrocarbon group having 1 to 13 carbon atoms which may have either an ester group or an ether group, or both. 7 is a linear or branched alkylene group having 1 to 4 carbon atoms; R 7In the formula, one or two of the hydrogen atoms may be substituted with a fluorine atom. Each of X1, X2, X3, X4, X6, and X7 is independently a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group, and X5 is a single bond, an ether group, or an ester group. Y is an oxygen atom, -NR 19 - group, and R 19 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 4 may be bonded to form a ring. m is an integer of 1 to 4. a1, a2, a3, a4, a5, a6, and a7 each satisfy 0≦a1≦1.0, 0≦a2≦1.0, 0≦a3≦1.0, 0≦a4≦1.0, 0≦a5≦1.0, 0≦a6≦1.0, and 0≦a7≦1.0, <a1+a2+a3+a4+a5+a6+a7≦1.0である。M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion. Rf5, Rf6, and Rf7 are a fluorine atom, or a linear or branched alkyl group having 1 to 4 carbon atoms, and have at least one fluorine atom.
[0076] Among the repeating units a1 to a7 represented by the above general formula (2), specific examples of the fluorosulfonate monomer for obtaining the repeating units a1 to a5 are shown below.
[0077] [ka]
[0078] [ka]
[0079] [ka]
[0080] [ka]
[0081]
change
[0082]
change
[0083]
change
[0084]
change
[0085]
change
[0086]
change
[0087]
change
[0088]
change
[0089]
change
[0090]
change
[0091]
change
[0092] [ka]
[0093] [ka]
[0094] [ka]
[0095] [ka]
[0096] [ka]
[0097] [ka]
[0098] Specific examples of the fluorosulfonimide salt monomer for obtaining the repeating unit a6 represented by the above general formula (2) include those shown below.
[0099] [ka]
[0100] [ka]
[0101] [ka]
[0102] [ka]
[0103] [ka]
[0104] Specific examples of the N-carbonylfluorosulfonamide salt monomer for obtaining the repeating unit a7 represented by the above general formula (2) include those shown below.
[0105] [ka]
[0106] [ka] (In the formula, R 1 , R 3 , R 5 , R 8 , R 10 , R 11 , and R 13 As mentioned above.)
[0107] In addition, the component (A) contains, as an ammonium ion constituting an ammonium salt, particularly M in the repeating unit a (repeating units a1 to a7). + It is preferable that the ammonium ion (ammonium cation) is contained in the following general formula (3). [ka] (In the formula, R 101d , R 101e , R 101f , R 101gR is a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 13 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , R 101d and R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e and R 101d and R 101e and R 101f is an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the ring.
[0108] Specific examples of the ammonium ion represented by the above general formula (3) include the following.
[0109] [ka]
[0110] [ka]
[0111] [ka]
[0112] [ka]
[0113] [ka]
[0114]
change
[0115]
change
[0116]
change
[0117]
change
[0118]
change
[0119]
change
[0120]
change
[0121]
change
[0122]
change
[0123]
change
[0124]
change
[0125] As the ammonium ion represented by the above general formula (3), a tertiary or quaternary ammonium ion is particularly preferred.
[0126] (Repeating units b1, b2) The ionic polymer in the present invention preferably contains, in addition to the repeating units a1 to a7, a repeating unit b1 having an oxirane group or oxetane group, or a repeating unit b2 having an isocyanate group, as represented by the following general formula (4). [ka] (In the formula, R 20 , R 24 is a hydrogen atom or a methyl group, X8 is a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group, X9 is an ester group, R 21 R is a single bond, a linear, branched or cyclic alkylene group having 1 to 20 carbon atoms, or a phenylene group, which may contain an ether group, an ester group or a hydroxyl group. 22 are hydrogen atoms or identical or non-identical alkyl groups having 1 to 4 carbon atoms, and R 21 R may be bonded to form a ring. 23 is a methylene group or an ethylene group, and R 21 R may be bonded to form a ring. 25 R is a linear or branched alkylene group having 1 to 20 carbon atoms, and may have an ether group. 26 is a single bond or a methylene group. B is an isocyanate group, which may be a blocked isocyanate group. 0≦b1<1.0, 0≦b2<1.0, 0 <b1+b2<1.0である。)
[0127] Specific examples of monomers for obtaining the repeating unit b1 represented by formula (4) include those shown below.
[0128] [ka]
[0129] [ka]
[0130] Specific examples of monomers for obtaining the repeating unit b2 represented by formula (4) include those shown below.
[0131] [ka] Here, R 20 , R 24 is as mentioned above.
[0132] By copolymerizing the repeating units b1 and b2, the ionic polymer reacts with the carbon particles to form a composite with the carbon.
[0133] (Repeating unit c) In addition to the repeating units a1 to a7, b1, and b2, the ionic polymer in component (A) of the bioelectrode composition of the present invention can also be copolymerized with a repeating unit c having a glyme chain in order to improve electrical conductivity. Specific examples of monomers for obtaining the repeating unit c having a glyme chain are shown below. When the bioelectrode of the present invention is a dry electrode, copolymerization of a repeating unit having a glyme chain can promote the movement of ions released from the skin within the dry electrode film, thereby increasing the sensitivity of the dry electrode.
[0134] [ka]
[0135] [ka]
[0136] [ka]
[0137] [ka] R is a hydrogen atom or a methyl group.
[0138] (Repeating unit d) In addition to the repeating units a1 to a7, b1, b2, and c described above, the ionic polymer in the component (A) of the bioelectrode composition of the present invention can also be copolymerized with a hydrophilic repeating unit d having a hydroxyl group, a carboxyl group, an ammonium salt, a betaine, an amide group, a pyrrolidone, a lactone ring, a lactam ring, a sultone ring, a sodium salt of sulfonic acid, or a potassium salt of sulfonic acid in order to improve electrical conductivity. Specific examples of monomers for obtaining the hydrophilic repeating unit d are shown below. By copolymerizing repeating units containing these hydrophilic groups, the sensitivity of the ions released from the skin can be increased, and the sensitivity of the dry electrode can be increased.
[0139] [ka]
[0140] [ka] R is a hydrogen atom or a methyl group.
[0141] (Repeating unit e) The ionic polymer in the component (A) in the bioelectrode composition of the present invention can have a repeating unit e that imparts adhesiveness. Specific examples of monomers from which the repeating unit e can be obtained include the following:
[0142] [ka]
[0143] [ka]
[0144] [ka]
[0145] [ka]
[0146] [ka]
[0147] (Repeating unit f) The ionic polymer in the component (A) of the bioelectrode composition of the present invention can have a silicon-containing repeating unit f in addition to the repeating units selected from the above a1 to a7, b1, b2, and c to e. Specific examples of monomers for obtaining the silicon-containing repeating unit f include the following.
[0148] [ka] n is a number between 0 and 100.
[0149] [ka]
[0150] (Repeating unit g) The ionic polymer in component (A) of the bioelectrode composition of the present invention can have a fluorine-containing repeating unit g in addition to the repeating units selected from the above a1 to a7, b1, b2, and c to f.
[0151] Specific examples of monomers from which the fluorine-containing repeating unit g can be obtained include the following.
[0152] [ka]
[0153] [ka]
[0154] [ka]
[0155] [ka]
[0156] [ka]
[0157] [ka]
[0158] [ka] Here, R is a hydrogen atom or a methyl group.
[0159] One method for synthesizing the ionic polymer in component (A) (polymer compound before reacting with carbon particles) is to heat-polymerize desired monomers from among the monomers that give the repeating units a1 to a7, b1, b2, c, d, e, f, and g in an organic solvent with the addition of a radical polymerization initiator to obtain a copolymer polymer compound.
[0160] Examples of the organic solvent used during polymerization include toluene, benzene, tetrahydrofuran, diethyl ether, dioxane, etc. Examples of the polymerization initiator include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl 2,2-azobis(2-methylpropionate), benzoyl peroxide, lauroyl peroxide, etc. The heating temperature is preferably 50 to 80°C, and the reaction time is preferably 2 to 100 hours, more preferably 5 to 20 hours.
[0161] Here, the ratios of the repeating units a1 to a7, b1, b2, c, d, e, f, g in the ionic polymer in component (A) are as follows: 0 ≦ a1 ≦ 1.0, 0 ≦ a2 ≦ 1.0, 0 ≦ a3 ≦ 1.0, 0 ≦ a4 ≦ 1.0, 0 ≦ a5 ≦ 1.0, 0 ≦ a6 ≦ 1.0, 0 ≦ a7 ≦ 1.0, 0 < a1 + a2 + a3 + a4 + a5 + a6 + a7 ≦ 1.0, 0 ≦ b1 < 1.0, 0 ≦ b2 < 1.0, 0 ≦ b1 + b2 < 1.0, 0 ≦ c < 1.0, 0 ≦ d < 1.0, 0 ≦ e < 0.9, 0 ≦ f < 0.9, 0 ≦ g < 0.9, a1 + a2 + a3 + a4 + a5 + a6 + a7 + b1 + b2 + c + d + e + f + g ≦ 1, preferably 0 ≦ a1 ≦ 0.9, 0 ≦ a2 ≦ 0.9, 0 ≦ a3 ≦ 0.9, 0 ≦ a4 ≦ 0.9, 0 ≦ a5 ≦ 0.9, 0 ≦ a6 ≦ 0.9, 0 ≦ a7 ≦ 0.9, 0.01 ≦ a1 + a2 + a3 + a4 + a5 + a6 + a7 ≦ 0.99, 0 ≦ b1 ≦ 0.8, 0 ≦ b2 ≦ 0.8, 0.001 ≦ b1 + b2 ≦ 0.8, 0 ≦ c ≦ 0.8, 0 ≦ d ≦ 0.8, 0 ≦ e < 0.8, 0 ≦ f < 0.8, 0 ≦ g < 0.8, more preferably 0 ≦ a1 ≦ 0.8, 0 ≦ a2 ≦ 0.8, 0 ≦ a3 ≦ 0.8, 0 ≦ a4 ≦ 0.8, 0 ≦ a5 ≦ 0.8, 0 ≦ a6 ≦ 0.8, 0 ≦ a7 ≦ 0.8, 0.02 ≦ a1 + a2 + a3 + a4 + a5 + a6 + a7 ≦ 0.95, 0 ≦ b1 ≦ 0.7, 0 ≦ b2 ≦ 0.7, 0.01 ≦ b1 + b2 ≦ 0.7, 0 ≦ c ≦ 0.7, 0 ≦ d ≦ 0.5, 0 ≦ e < 0.3, 0 ≦ f < 0.7, 0 ≦ g < 0.7.
[0162] In the case of an isocyanate in which the repeating unit b2 is not blocked, if the repeating units b1 and b2 are not present in the same molecule, b1 and b2 will not react within the polymer molecule, and the reaction with the carbon particles will proceed sufficiently. For this reason, it is preferable that b1 and b2 are not copolymerized. It is also preferable that an ionic polymer in which b1 is copolymerized is not blended with an ionic polymer in which b2 is copolymerized, since b1 and b2 will not react between the molecules, and the reaction with the carbon particles will proceed sufficiently.
[0163] For example, a1+a2+a3+a4+a5+a6+a7+b1+b2+c+d+e+f+g=1 means that in a polymer compound containing repeating units a1, a2, a3, a4, a5, a6, a7, b1, b2, c, d, e, f, and g, the total amount of the repeating units a1, a2, a3, a4, a5, a6, a7, b1, b2, c, d, e, f, and g is 100 mol % based on the total amount of all repeating units. a1+a2+a3+a4+a5+a6+a7+b1+b2+c+d+e+f+g<1 means that the total amount of repeating units a1, a2, a3, a4, a5, a6, a7, b1, b2, c, d, e, f and g is less than 100 mol% based on the total amount of all repeating units, and other repeating units are present in addition to a1, a2, a3, a4, a5, a6, a7, b1, b2, c, d, e, f and g.
[0164] The molecular weight of the ionic polymer in the component (A) is preferably 500 or more as weight average molecular weight, more preferably 1,000 or more and 1,000,000 or less, and even more preferably 2,000 or more and 500,000 or less. In addition, if the amount of ionic monomer (residual monomer) that is not incorporated into the ionic polymer after polymerization is small, there is no risk of it penetrating into the skin and causing allergies in a biocompatibility test, so it is preferable to reduce the amount of the residual monomer. The amount of the residual monomer is preferably 10 parts by mass or less relative to 100 parts by mass of the total ionic polymer in the component (A). In addition, the ionic polymer may be used alone, or two or more types with different molecular weights, dispersities, and polymerized monomers may be used in combination. The molecular weight (Mw) and dispersity (Mw / Mn) can be confirmed by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.
[0165] Examples of carbon particles include carbon black, carbon nanotubes, graphite, and graphene. Carbon nanotubes and graphene may have a single-layer structure or a multi-layer structure. Furthermore, it is preferable that the carbon particles have a reactive group such as a hydroxyl group, a carboxyl group, or an amino group.
[0166] When the ionic polymer in component (A) has an oxirane group, oxetane group, or isocyanate group, these react with and bond to the hydroxyl group, carboxyl group, or amino group on the surface of the carbon particles.
[0167] The component (A) is preferably a product obtained by reacting 5 parts by mass or more of an ionic polymer with 100 parts by mass of carbon particles, and more preferably a product obtained by reacting 5 parts by mass or more of a polymer reactive with carbon particles copolymerized with a repeating unit b1 having an oxirane group or an oxetane group, or a repeating unit b2 having an isocyanate group, as shown in general formula (4), with 100 parts by mass of carbon particles.
[0168] By pendantly attaching the ionic polymer to the carbon particles, both the ionic conductivity and electronic conductivity are improved, which not only improves the sensitivity of the bioelectrode, but also prevents the ionic polymer from being extracted from the bioelectrode membrane, preventing a decrease in the sensitivity of the biosignal due to extraction. Furthermore, the permeability to the skin is reduced, reducing irritation to the skin, making it more likely that the ionic polymer will pass through the skin and cause allergies.
[0169] The ionic polymer reacts with the carbon particles, and the ionic polymer adheres to the surface of the carbon particles through chemical bonds. In the reaction between the ionic polymer and the carbon nanotubes, the ionic polymer may react across multiple carbon nanotubes, forming a bucky gel structure.
[0170] The reaction for compounding the ionic polymer and the carbon particles is carried out by mixing the ionic polymer and the carbon particles and carrying out the reaction at room temperature or by heating. The reaction can be accelerated by heating, but if the heating temperature is too high, the ionic polymer will decompose, so the heating temperature is preferably 200°C or less.
[0171] A catalyst for accelerating the reaction can also be added. When the ionic polymer has an oxirane group or an oxetane group and the carbon particles have a carboxyl group, examples of the catalyst include pyridine, 2-ethylimidazole, tertiary amines, and metal compounds such as zinc 2-ethylhexanoate and aluminum acetylacetonate. When the ionic polymer has an isocyanate group or a blocked isocyanate group, the reaction can be accelerated by adding a tin-based catalyst.
[0172] In the bioelectrode composition of the present invention, the blending amount of the (A) component is preferably 0.1 to 300 parts by mass, more preferably 1 to 200 parts by mass, per 100 parts by mass of the (B) component described below. The (A) component may be used alone or in combination of two or more kinds.
[0173] In some cases, the oxirane, oxetane, and isocyanate groups contained in the ionic polymer are not consumed in the reaction with the carbon particles. In this case, the oxirane and oxetane groups are coupled with each other or form a dialcohol group by a ring-opening reaction. Even in this case, the performance as a bioelectrode is not reduced and the irritation to the skin is not increased. In order to inactivate the unreacted oxirane, oxetane, and isocyanate groups after the reaction with the carbon particles, they can be reacted with water, alcohol, or a carboxylic acid compound.
[0174] [(B) Adhesive resin] The adhesive resin (B) blended in the bioelectrode composition of the present invention is a component that is compatible with the reaction complex (salt) of the ionic polymer material (A) and carbon particles to prevent the salt from eluting, holds a conductive improver such as metal powder, carbon powder, silicon powder, or lithium titanate powder, and exhibits adhesiveness. If the ionic polymer material in the component (A) has adhesiveness, the adhesive resin (B) is not necessarily required. The resin of the component (B) may be any resin other than the above-mentioned component (A), and is preferably either a thermosetting resin or a photocurable resin, or both, and is particularly preferably one or more selected from silicone-based (silicone resin), acrylic-based ((meth)acrylate resin), and urethane-based (urethane resin) resins.
[0175] Examples of adhesive silicone-based resins include those that are cured by addition reaction or radical crosslinking reaction. Examples of the addition reaction cured type include diorganosiloxane having an alkenyl group, RSiO, as described in JP 2015-193803 A. 0.5 and SiO2 units, organohydrogenpolysiloxane having a plurality of SiH groups, platinum catalyst, addition reaction inhibitor, and organic solvent. In addition, as the radical crosslinking reaction curing type, for example, diorganopolysiloxane which may or may not have alkenyl groups, R3SiO 0.5and those containing an MQ resin having SiO2 units, an organic peroxide, and an organic solvent, where R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms.
[0176] It is also possible to use a polysiloxane-resin integrated compound formed by condensing polysiloxane with silanols at the polymer end or side chain with MQ resin. MQ resin contains a lot of silanols, so adding this improves adhesive strength, but since it is not crosslinkable, it is not molecularly bonded to the polysiloxane. By integrating polysiloxane and resin as described above, adhesive strength can be increased.
[0177] In addition, modified siloxanes having a group selected from amino groups, oxirane groups, oxetane groups, polyether groups, hydroxy groups, carboxyl groups, mercapto groups, methacryl groups, acrylic groups, phenol groups, silanol groups, carboxylic anhydride groups, aryl groups, aralkyl groups, amide groups, ester groups, and lactone rings can be added to silicone resins. By adding modified siloxanes, the dispersibility of component (A) in the silicone resin is improved. The modified siloxanes may be modified at one end, both ends, or the side chains of the siloxane.
[0178] The adhesive acrylic resin may be, for example, one having a hydrophilic (meth)acrylic acid ester or a long-chain hydrophobic (meth)acrylic acid ester as a repeating unit, as described in JP 2016-011338 A. In some cases, a (meth)acrylic acid ester having a functional group or a (meth)acrylic acid ester having a siloxane bond may be copolymerized.
[0179] As the adhesive urethane-based resin, for example, one having a urethane bond and a polyether or polyester bond, a polycarbonate bond, or a siloxane bond, as described in JP 2016-065238 A, can be used.
[0180] In addition, in order to prevent the decrease in conductivity due to the detachment of the (A) component from the biocontact layer, in the bioelectrode composition of the present invention, it is preferable that the resin of the (B) component has high compatibility with the above-mentioned (A) component. In addition, in order to prevent the peeling of the biocontact layer from the conductive substrate, it is preferable that the resin of the (B) component has high adhesion to the conductive substrate in the bioelectrode composition of the present invention. In order to make the resin of the (B) component highly compatible with the conductive substrate and salt, it is effective to use a resin with high polarity. Examples of such resins include resins having one or more selected from ether bonds, ester bonds, amide bonds, imide bonds, urethane bonds, thiourethane bonds, and thiol groups, or polyacrylic resins, polyamide resins, polyimide resins, polyurethane resins, and polythiourethane resins. On the other hand, since the biocontact layer contacts the living body, it is easily affected by sweat from the living body. Therefore, in the bioelectrode composition of the present invention, it is preferable that the resin of the (B) component has high water repellency and is difficult to hydrolyze. In order to make the resin of the (B) component highly water repellent and difficult to hydrolyze, it is effective to use a resin containing silicon.
[0181] Silicon-atom-containing polyacrylic resins include polymers having silicone in the main chain and polymers having silicon atoms in the side chain, and both can be used suitably. As the polymer having silicone in the main chain, siloxane or silsesquioxane having a (meth)acrylpropyl group can be used. In this case, the (meth)acryl portion can be polymerized and cured by adding a photoradical generator.
[0182] Suitable examples of polyamide resins containing silicon atoms include polyamide silicone resins described in JP 2011-079946 A and U.S. Patent No. 5,981,680 A. Such polyamide silicone resins can be synthesized by combining, for example, a silicone having amino groups at both ends or a non-silicone compound having amino groups at both ends with a non-silicone having carboxyl groups at both ends or a silicone having carboxyl groups at both ends.
[0183] Alternatively, polyamic acid obtained by reacting a carboxylic anhydride with an amine before cyclization may be used. An epoxy or oxetane crosslinking agent may be used to crosslink the carboxyl groups of the polyamic acid, or the carboxyl groups may be esterified with hydroxyethyl (meth)acrylate to perform photoradical crosslinking of the (meth)acrylate portion.
[0184] As the polyimide resin containing silicon atoms, for example, the polyimide silicone resin described in JP-A-2002-332305 can be suitably used. Polyimide resins have a very high viscosity, but the viscosity can be reduced by blending a (meth)acrylic monomer as a solvent and a crosslinking agent.
[0185] Examples of polyurethane resins containing silicon atoms include polyurethane silicone resins. In such polyurethane silicone resins, crosslinking by urethane bonds can be performed by blending and heating a compound having isocyanate groups at both ends and a compound having hydroxyl groups at the ends. In this case, it is necessary to contain silicon atoms (siloxane bonds) in either or both of the compound having isocyanate groups at both ends and the compound having hydroxyl groups at the ends. Alternatively, as described in JP 2005-320418 A, a urethane (meth)acrylate monomer can be blended with polysiloxane to perform photocrosslinking. In addition, a polymer having both siloxane bonds and urethane bonds and a (meth)acrylate group at the end can also be photocrosslinked. In particular, the silicone chain attached to the side chain and the polyurethane main chain described in JP 2018-123304 A and JP 2019-70109 A are preferred because they have high strength and high elasticity.
[0186] The polythiourethane resin containing silicon atoms can be obtained by reacting a compound having a thiol group with a compound having an isocyanate group, and any one of them may contain a silicon atom. In addition, if the compound has a (meth)acrylate group at the end, it can be photocured.
[0187] In the silicone resin, the above-mentioned diorganosiloxane having an alkenyl group, RSiO 0.5 In addition to MQ resins having SiO2 units and organohydrogenpolysiloxanes having multiple SiH groups, the compatibility with the above-mentioned salts is improved by adding modified siloxanes having groups selected from amino groups, oxirane groups, oxetane groups, polyether groups, hydroxyl groups, carboxyl groups, mercapto groups, methacryl groups, acrylic groups, phenol groups, silanol groups, carboxylic anhydride groups, aryl groups, aralkyl groups, amide groups, ester groups, and lactone rings.
[0188] Diorganosiloxanes having alkenyl groups and organohydrogenpolysiloxanes having multiple SiH groups can be crosslinked by an addition reaction in the presence of a platinum catalyst.
[0189] Examples of platinum catalysts include platinum catalysts such as chloroplatinic acid, alcohol solutions of chloroplatinic acid, reaction products of chloroplatinic acid and alcohol, reaction products of chloroplatinic acid and olefin compounds, reaction products of chloroplatinic acid and vinyl group-containing siloxane, platinum-olefin complexes, platinum-vinyl group-containing siloxane complexes, platinum group metal catalysts such as rhodium complexes and ruthenium complexes, etc. Furthermore, these catalysts may be used in the form of a solution or dispersion in an alcohol-based, hydrocarbon-based, or siloxane-based solvent.
[0190] The amount of the platinum catalyst added is preferably within a range of 5 to 2,000 ppm, and particularly preferably 10 to 500 ppm, per 100 parts by mass of the resin of component (B).
[0191] In the bioelectrode composition of the present invention, the blending amount of the (B) component is preferably 0 to 2000 parts by mass, more preferably 10 to 1000 parts by mass, per 100 parts by mass of the reaction complex (A) of the ionic polymer material and the carbon particles. In addition, each of the (B) components may be used alone or in combination of two or more kinds.
[0192] When an addition-curing silicone resin is used, an addition reaction inhibitor may be added as a quencher to prevent the platinum catalyst from acting in the solution and in a low-temperature environment before heat curing after coating formation. Specific examples include 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclohexanol, 3-methyl-3-trimethylsiloxy-1-butyne, 3-methyl-3-trimethylsiloxy-1-pentyne, 3,5-dimethyl-3-trimethylsiloxy-1-hexyne, 1-ethynyl-1-trimethylsiloxycyclohexane, bis(2,2-dimethyl-3-butynoxy)dimethylsilane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, and 1,1,3,3-tetramethyl-1,3-divinyldisiloxane.
[0193] The amount of the addition reaction inhibitor added is preferably within the range of 0 to 10 parts by mass, and particularly preferably 0.05 to 3 parts by mass, per 100 parts by mass of the resin of component (B).
[0194] Among these, it is more preferable that the resin of component (B) contains a diorganosiloxane having an alkenyl group and an organohydrogenpolysiloxane having a SiH group, and further R x SiO (4-x) / 2 It is particularly preferred that the silicone resin contains a silicone resin having a SiO2 unit (R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and x is in the range of 2.5 to 3.5).
[0195] As described later, the biocontact layer is a cured product of the bioelectrode composition. By curing, the adhesion of the biocontact layer to both the skin and the conductive substrate is improved. The curing method is not particularly limited, and a general method can be used, for example, heat and / or light, or a crosslinking reaction using an acid or base catalyst. The crosslinking reaction can be carried out by appropriately selecting a method described in, for example, Crosslinking Reaction Handbook, Nakayama Hiroharu, Maruzen Publishing (2013), Chapter 2, p. 51 to p. 371.
[0196] [(C) Blended ionic polymer] In addition to the component (A), an ionic polymer (blended ionic polymer) can be added to the bioelectrode composition of the present invention. The repeating units of the blended ionic polymer can be those described in the ionic polymer in the component (A), particularly those represented by the general formula (2). The amount of the blended ionic polymer added is preferably in the range of 0.1 to 100 parts by mass per 100 parts by mass of the resin in the component (B).
[0197] [(D) Conductive powder] [Metal powder] In order to enhance electronic conductivity, the bioelectrode composition of the present invention may contain, as component (D), a metal powder selected from gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium. The amount of metal powder added is preferably within the range of 1 to 50 parts by mass per 100 parts by mass of the resin of component (B).
[0198] As the type of metal powder, gold, silver, and platinum are preferred from the viewpoint of electrical conductivity, and silver, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, and chromium are preferred from the viewpoint of cost. From the viewpoint of biocompatibility, noble metals are preferred, and from these viewpoints overall, silver is the most preferred.
[0199] The shape of the metal powder can be spherical, disk-like, flake-like, or needle-like, but the addition of flake-like powder is the most conductive and is preferred. The size of the metal powder is 100 μm or less, and the tap density is 5 g / cm. 3 Below, the specific surface area is 0.5m 2 Flakes with a relatively low density and large specific surface area of 100 / g or more are preferred.
[0200] [Carbon powder] A carbon material (carbon powder) can be added as a conductivity improver. Examples of the carbon material include carbon black, graphite, carbon nanotubes, and carbon fibers. The carbon nanotubes may be either single-walled or multi-walled, and the surface may be modified with an organic group. The amount of the carbon material added is preferably in the range of 1 to 50 parts by mass per 100 parts by mass of the resin of component (B).
[0201] [Silicon powder] Silicon powder can be added to the bioelectrode composition of the present invention in order to increase the sensitivity of ion reception. Examples of silicon powder include powders made of silicon, silicon monoxide, and silicon carbide. The particle size of the powder is preferably smaller than 100 μm, and more preferably 1 μm or less. Since finer particles have a larger surface area, they can receive more ions, resulting in a highly sensitive bioelectrode. The amount of silicon powder added is preferably in the range of 1 to 50 parts by mass per 100 parts by mass of the resin of component (B).
[0202] [Lithium titanate powder] Lithium titanate powder can be added to the bioelectrode composition of the present invention in order to increase the sensitivity of ion reception. Lithium titanate powder includes Li2TiO3, LiTiO2, and Li4Ti5O with a spinel structure. 12The molecular formula of the lithium titanate powder is as follows, and a spinel structure is preferable. Lithium titanate particles composited with carbon can also be used. The particle size of the powder is preferably smaller than 100 μm, more preferably 1 μm or less. Since finer particles have a larger surface area, they can receive more ions, resulting in a highly sensitive bioelectrode. These may be composite powders with carbon. The amount of lithium titanate powder added is preferably in the range of 1 to 50 parts by mass per 100 parts by mass of the resin of component (B).
[0203] [(E) Organic solvent] In addition, an organic solvent can be added as component (E) to the bioelectrode composition of the present invention. Specific examples of the organic solvent include toluene, xylene, cumene, 1,2,3-trimethylbenzene, 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, styrene, α-methylstyrene, butylbenzene, sec-butylbenzene, isobutylbenzene, cymene, diethylbenzene, 2-ethyl-p-xylene, 2-propyltoluene, 3-propyltoluene, 4-propyltoluene, 1,2,3,5-tetramethyltoluene, 1,2,4,5-tetramethyltoluene, tetrahydrofuran, and the like. naphthalene, 4-phenyl-1-butene, tert-amylbenzene, amylbenzene, 2-tert-butyltoluene, 3-tert-butyltoluene, 4-tert-butyltoluene, 5-isopropyl-m-xylene, 3-methylethylbenzene, tert-butyl-3-ethylbenzene, 4-tert-butyl-o-xylene, 5-tert-butyl-m-xylene, tert-butyl-p-xylene, 1,2-diisopropylbenzene, 1,3-diisopropylbenzene, 1,4-diisopropylbenzene, Aromatic hydrocarbon solvents such as isopropylbenzene, dipropylbenzene, pentamethylbenzene, hexamethylbenzene, hexylbenzene, and 1,3,5-triethylbenzene, n-heptane, isoheptane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, 1,6-heptadiene, 5-methyl-1-hexyne, norbornane, norbornene, dicyclopentadiene, 1-methyl-1,4-cyclohexadiene, 1-heptyne, 2-heptyne, cycloheptane, and cyclohexene. butene, 1,3-dimethylcyclopentane, ethylcyclopentane, methylcyclohexane, 1-methyl-1-cyclohexene, 3-methyl-1-cyclohexene, methylenecyclohexane, 4-methyl-1-cyclohexene, 2-methyl-1-hexene, 2-methyl-2-hexene, 1-heptene, 2-heptene, 3-heptene, n-octane, 2,2-dimethylhexane, 2,3-dimethylhexane, 2,4-dimethylhexane, 2,5-dimethylhexane, 3,3-dimethylhexane, 3,4-Dimethylhexane, 3-ethyl-2-methylpentane, 3-ethyl-3-methylpentane, 2-methylheptane, 3-methylheptane, 4-methylheptane, 2,2,3-trimethylpentane, 2,2,4-trimethylpentane, cyclooctane, cyclooctene, 1,2-dimethylcyclohexane, 1,3-dimethylcyclohexane, 1,4-dimethylcyclohexane, ethylcyclohexane, vinylcyclohexane, isopropylcyclopentane, 2,2-dimethyl-3-hexene, 2,4-dimethyl-1-hexene, 2,5-dimethyl-1- Hexene, 2,5-dimethyl-2-hexene, 3,3-dimethyl-1-hexene, 3,4-dimethyl-1-hexene, 4,4-dimethyl-1-hexene, 2-ethyl-1-hexene, 2-methyl-1-heptene, 1-octene, 2-octene, 3-octene, 4-octene, 1,7-octadiene, 1-octyne, 2-octyne, 3-octyne, 4-octyne, n-nonane, 2,3-dimethylheptane, 2,4-dimethylheptane, 2,5-dimethylheptane, 3,3-dimethylheptane, 3,4-dimethylheptane, 3,5-dimethylheptane, 4-ethylhexene, ethylheptane, 2-methyloctane, 3-methyloctane, 4-methyloctane, 2,2,4,4-tetramethylpentane, 2,2,4-trimethylhexane, 2,2,5-trimethylhexane, 2,2-dimethyl-3-heptene, 2,3-dimethyl-3-heptene, 2,4-dimethyl-1-heptene, 2,6-dimethyl-1-heptene, 2,6-dimethyl-3-heptene, 3,5-dimethyl-3-heptene, 2,4,4-trimethyl-1-hexene, 3,5,5-trimethyl-1-hexene, 1-ethyl-2-methylcyclohexane, 1-ethyl-3 -Methylcyclohexane, 1-ethyl-4-methylcyclohexane, propylcyclohexane, isopropylcyclohexane, 1,1,3-trimethylcyclohexane, 1,1,4-trimethylcyclohexane, 1,2,3-trimethylcyclohexane, 1,2,4-trimethylcyclohexane, 1,3,5-trimethylcyclohexane, allylcyclohexane, hydrindane, 1,8-nonadiene, 1-nonyne, 2-nonyne, 3-nonyne, 4-nonyne, 1-nonene, 2-nonene, 3-nonene, 4-nonene, n-decane, 3,3-dimethyloctane, 3,5-dimethyloctane, 4,4-dimethyloctane, 3-ethyl-3-methylheptane, 2-methylnonane, 3-methylnonane, 4-methylnonane, tert-butylcyclohexane, butylcyclohexane, isobutylcyclohexane, 4-isopropyl-1-methylcyclohexane, pentylcyclopentane, 1,1,3,5-tetramethylcyclohexane, cyclododecane, 1-decene, 2-decene, 3-decene, 4-decene, 5-decene, 1,9-decadiene, decahydronaphthalene, 1-decene, 2-decene, 3-decene, 4-decene, 5-decene, 1, 5,9-Decatriene, 2,6-dimethyl-2,4,6-octatriene, limonene, myrcene, 1,2,3,4,5-pentamethylcyclopentadiene, α-phellandrene, pinene, terpinene, tetrahydrodicyclopentadiene, 5,6-dihydrodicyclopentadiene, 1,4-decadiyne, 1,5-decadiyne, 1,9-decadiyne, 2,8-decadiyne, 4,6-decadiyne, n-undecane, amylcyclohexane, 1-undecene, 1,10-undecadiene, 1-undecyne, 3-undecyne, 5-undecyne, tricyclo[6.2.1.0, 2,7]Undec-4-ene, n-dodecane, 2-methylundecane, 3-methylundecane, 4-methylundecane, 5-methylundecane, 2,2,4,6,6-pentamethylheptane, 1,3-dimethyladamantane, 1-ethyladamantane, 1,5,9-cyclododecatriene, 1,2,Aliphatic hydrocarbon solvents such as 4-trivinylcyclohexane and isoparaffin; ketone solvents such as cyclohexanone, cyclopentanone, 2-octanone, 2-nonanone, 2-heptanone, 3-heptanone, 4-heptanone, 2-hexanone, 3-hexanone, diisobutyl ketone, methylcyclohexanone, and methyl n-pentyl ketone; alcohol solvents such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monopentyl ether, and diethylene glycol monoheptyl ether. Examples of the solvent include ether solvents such as ethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, diisopropyl ether, diisobutyl ether, diisopentyl ether, di-n-pentyl ether, methylcyclopentyl ether, methylcyclohexyl ether, di-n-butyl ether, di-sec-butyl ether, diisopentyl ether, di-sec-pentyl ether, di-tert-amyl ether, di-n-hexyl ether, and anisole; ester solvents such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate; lactone solvents such as γ-butyrolactone; and water.
[0204] The amount of the organic solvent added is preferably within a range of 10 to 50,000 parts by mass per 100 parts by mass of the resin of the component (B).
[0205] [(F) Other additives] In addition to the platinum catalyst and the addition reaction control agent described in the (B) component section, the bioelectrode composition of the present invention can also be mixed with a crosslinking agent, a crosslinking catalyst, an ionic additive, and further with silica particles, polyether silicone, and polyglycerin silicone. Silica particles have a hydrophilic surface and are compatible with hydrophilic ionic polymers, polyether silicone, and polyglycerin silicone, and can improve the dispersibility of ionic polymers, polyether silicone, and polyglycerin silicone in hydrophobic silicone adhesives. Silica particles can be used preferably in either dry or wet processes.
[0206] [Crosslinking agent] An epoxy-based crosslinking agent can be added to the bioelectrode composition of the present invention. In this case, the crosslinking agent is a compound having multiple epoxy groups or oxetane groups in one molecule. The amount of the crosslinking agent to be added is 1 to 30 parts by mass per 100 parts by mass of the resin of component (B).
[0207] [Crosslinking catalyst] A catalyst for crosslinking epoxy groups or oxetane groups can also be added to the bioelectrode composition of the present invention. In this case, the catalysts described in paragraphs 0027 to 0029 of JP-A-2019-503406 can be used. The amount of the catalyst added is 0.01 to 10 parts by mass per 100 parts by mass of the resin of component (B).
[0208] [Ionic additives] The bioelectrode composition of the present invention can be added with an ionic additive to increase ionic conductivity. In consideration of biocompatibility, sodium chloride, potassium chloride, calcium chloride, magnesium chloride, saccharin sodium salt, acesulfame potassium, sodium carboxylate, potassium carboxylate, calcium carboxylate, sodium sulfonate, potassium sulfonate, calcium sulfonate, sodium phosphate, potassium phosphate, calcium phosphate, magnesium phosphate, betaine, and salts disclosed in JP-A-2018-44147, JP-A-2018-59050, JP-A-2018-59052, and JP-A-2018-130534 can be mentioned.
[0209] [Silicone compounds having polyglycerin structure] In the bioelectrode composition of the present invention, a silicone compound having a polyglycerin structure can be added in order to improve the moisture retention of the membrane and improve the sensitivity and ion conductivity of ions released from the skin. The amount of the silicone compound having a polyglycerin structure is preferably 0.01 to 100 parts by mass, more preferably 0.5 to 60 parts by mass, per 100 parts by mass of the total of the (A) component and the (B) component. The silicone compound having a polyglycerin structure may be used alone or in a mixture of two or more types.
[0210] The silicone compound having a polyglycerin structure is preferably one represented by the following general formulas (4)' and (5)'.
[0211] [ka] (In formulas (4)' and (5)', R 1 are each independent and may be the same or different, each independently represent a hydrogen atom, a linear or branched alkyl group having 1 to 50 carbon atoms, or a phenyl group, each independently represent a silicone chain represented by the general formula (6)' ... 2R′ is a group having a polyglycerin group structure represented by formula (4)′-1 or formula (4)′-2, 3 ' are each independent and may be the same or different, 1 ' group or the R 2 ' group, R 4 ' are each independent and may be the same or different, 1 ' group, the R 2 R is a ' group or an oxygen atom. 4 If ' is an oxygen atom, then two R 4 The a' groups may be bonded to form a single ether group to form a ring together with the silicon atom. a' may be the same or different and is 0 to 100, b' is 0 to 100, and a'+b' is 0 to 200. However, when b' is 0, R 3 At least one of the R 2 In formulae (4)'-1, (4)'-2, (5)', and (6)', R 5 ' is an alkylene group having 2 to 10 carbon atoms or an aralkylene group having 7 to 10 carbon atoms; R 6 ', R 7 ' is an alkylene group having 2 to 6 carbon atoms, and R 7 ' may be an ether bond, c' is 0 to 20, and d' is 1 to 20.
[0212] Examples of such silicone compounds having a polyglycerin structure include the following.
[0213] [ka]
[0214] [ka]
[0215] [ka]
[0216] [ka]
[0217] [ka]
[0218] [ka]
[0219] [ka]
[0220] [ka]
[0221] [ka]
[0222] [ka] (wherein a', b', c' and d' are as defined above).
[0223] A bioelectrode composition containing a silicone compound having such a polyglycerin structure can exhibit better moisturizing properties, and as a result, can form a biocontact layer that can exhibit better sensitivity to ions released from the skin.
[0224] As described above, the bioelectrode composition of the present invention can efficiently transmit electrical signals from the skin to the device (i.e., has excellent electrical conductivity), is not likely to cause allergies even when worn on the skin for a long period of time (i.e., has excellent biocompatibility), is lightweight, can be manufactured at low cost, and can form a biocontact layer for a bioelectrode that does not significantly decrease in electrical conductivity even when wet or dried. In addition, the electrical conductivity can be further improved by adding a conductive powder (carbon powder, metal powder), and a bioelectrode with particularly high adhesive strength and high elasticity can be manufactured by combining it with a resin having adhesiveness and elasticity. Furthermore, the elasticity and adhesiveness to the skin can be improved by additives, and the elasticity and adhesiveness can be adjusted by appropriately adjusting the composition of the resin and the thickness of the biocontact layer.
[0225] <Bioelectrode> The present invention also provides a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, wherein the biocontact layer is a cured product of the bioelectrode composition of the present invention described above.
[0226] The bioelectrode of the present invention will be described in detail below with reference to the drawings, but the present invention is not limited thereto.
[0227] FIG. 1 is a schematic cross-sectional view showing an example of the bioelectrode of the present invention. The bioelectrode 1 of FIG. 1 has a conductive substrate 2 and a biocontact layer 3 formed on the conductive substrate 2. The biocontact layer 3 is made of a cured product of the bioelectrode composition of the present invention. The ionic reaction complex 4 constituting the biocontact layer 3 is a complex of the ionic polymer material and carbon particles (for example, carbon particles modified with the ionic polymer). The biocontact layer 3 can further contain an adhesive resin 6 other than the ionic reaction complex 4 and a blended ionic polymer 5. Hereinafter, with reference to FIGS. 1 and 2, a case where the biocontact layer 3 is a layer in which the ionic reaction complex 4 and the blended ionic polymer 5 are dispersed in the adhesive resin 6 will be described, but the bioelectrode of the present invention is not limited to this embodiment.
[0228] When using such a bioelectrode 1 of Fig. 1, as shown in Fig. 2, the biocontact layer 3 (i.e., a layer in which the ionic reaction complex 4 and the blended ionic polymer 5 are dispersed in the adhesive resin 6) is brought into contact with a living body 7, and an electrical signal is extracted from the living body 7 by the ionic reaction complex 4 and the blended ionic polymer 5, and the electrical signal is conducted to a sensor device or the like (not shown) via the conductive substrate 2. In this way, the bioelectrode of the present invention can achieve both electrical conductivity and biocompatibility by the above-mentioned ionic reaction complex 4, and has adhesiveness so that the contact area with the skin is constant, and electrical signals from the skin can be obtained stably and with high sensitivity.
[0229] Each of the constituent materials of the bioelectrode of the present invention will be described in more detail below.
[0230] [Conductive base material] The bioelectrode of the present invention has a conductive substrate. This conductive substrate is usually electrically connected to a sensor device or the like, and conducts an electrical signal extracted from a living body via a living body contact layer to the sensor device or the like.
[0231] The conductive substrate is not particularly limited as long as it is conductive, but it is preferable that the conductive substrate contains at least one material selected from the group consisting of gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
[0232] The conductive substrate is not particularly limited and may be a hard conductive substrate, a flexible conductive film, a fabric coated with a conductive paste, or a fabric with a conductive polymer kneaded in. The conductive substrate may be flat or uneven, or may be a mesh of woven metal wires, and may be appropriately selected depending on the application of the bioelectrode.
[0233] [Bio-contact layer] The bioelectrode of the present invention has a biocontact layer formed on a conductive substrate. This biocontact layer is the part that actually comes into contact with the living body when the bioelectrode is used, and has electrical conductivity and adhesiveness. The biocontact layer is a cured product of the bioelectrode composition of the present invention described above, that is, an adhesive resin layer made of a cured product of a composition containing the above-mentioned component (A) and, if necessary, components (B), (C), (D), (E), and (F).
[0234] The adhesive strength of the living body contact layer is preferably in the range of 0.5 N / 25 mm to 20 N / 25 mm. The adhesive strength is generally measured by the method shown in JIS Z 0237. A metal substrate such as SUS (stainless steel) or a PET (polyethylene terephthalate) substrate can be used as the substrate, but human skin can also be used for measurement. The surface energy of human skin is lower than that of metals and various plastics, and is close to that of Teflon (registered trademark), making it difficult to adhere to the skin.
[0235] The thickness of the biocontact layer of the bioelectrode is preferably 1 μm to 5 mm, more preferably 2 μm to 3 mm. The thinner the biocontact layer, the weaker the adhesive strength, but the more flexible it is, the lighter it is, and the better it fits to the skin. The thickness of the biocontact layer can be selected based on the balance between adhesiveness and texture on the skin.
[0236] In addition, in the bioelectrode of the present invention, similar to conventional bioelectrodes (for example, the bioelectrode described in JP 2004-033468 A), a separate adhesive film may be provided on the biocontact layer to prevent the bioelectrode from peeling off from the living body during use. When providing a separate adhesive film, it is sufficient to form the adhesive film using an adhesive film material such as an acrylic type, a urethane type, or a silicone type. In particular, the silicone type has high oxygen permeability, so that the skin can breathe while it is attached, and has high water repellency, so that the adhesiveness is less likely to decrease due to sweat, and further, is less irritating to the skin, so it is preferable. In addition, in the bioelectrode of the present invention, as described above, peeling off from the living body can be prevented by adding an adhesive imparting agent to the bioelectrode composition or using a resin that has good adhesiveness to the living body, so that the above-mentioned separate adhesive film is not necessarily required.
[0237] When the bioelectrode of the present invention is used as a wearable device, the wiring between the bioelectrode and the sensor device and other components are not particularly limited, and for example, those described in JP 2004-033468 A can be applied.
[0238] As described above, the bioelectrode of the present invention has a biocontact layer formed of the cured product of the bioelectrode composition of the present invention, so that the bioelectrode can efficiently transmit electrical signals from the skin to the device (i.e., has excellent electrical conductivity), is not likely to cause allergies even when worn on the skin for a long period of time (i.e., has excellent biocompatibility), is lightweight, can be manufactured at low cost, and does not significantly decrease in electrical conductivity even when wet or dried. In addition, the electrical conductivity can be further improved by adding a conductive powder, and a bioelectrode with particularly high adhesive strength and high elasticity can be manufactured by combining it with a resin having adhesiveness and elasticity. Furthermore, the elasticity and adhesiveness to the skin can be improved by additives, and the elasticity and adhesiveness can be adjusted by appropriately adjusting the composition of the resin and the thickness of the biocontact layer. Therefore, such a bioelectrode of the present invention is particularly suitable as a bioelectrode used in a medical wearable device.
[0239] <Manufacturing method of bioelectrodes> The present invention also provides a method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, in which the bioelectrode composition of the present invention described above is applied to the conductive substrate and cured to form the biocontact layer.
[0240] The conductive substrate and the like used in the method for producing a bioelectrode of the present invention may be the same as those described above.
[0241] The method for applying the bioelectrode composition onto the conductive substrate is not particularly limited, but suitable methods include, for example, dip coating, spray coating, spin coating, roll coating, flow coating, doctor coating, screen printing, flexographic printing, gravure printing, and inkjet printing.
[0242] The resin curing method is not particularly limited and may be appropriately selected depending on the components (A) and (B) used in the bioelectrode composition, but it is preferable to cure the resin by, for example, heat or light, or both. In addition, a catalyst that generates an acid or base may be added to the bioelectrode composition to cause a crosslinking reaction and cure the resin.
[0243] The temperature for heating is not particularly limited and may be appropriately selected depending on the components (A) and (B) used in the bioelectrode composition, but is preferably about 50 to 250°C, for example.
[0244] In addition, when heating and light irradiation are combined, heating and light irradiation may be performed simultaneously, or heating may be performed after light irradiation, or light irradiation may be performed after heating. In addition, air drying may be performed before heating after coating in order to evaporate the solvent.
[0245] After the film has hardened, applying water droplets or spraying water vapor or mist on the surface improves its compatibility with the skin, allowing for quick biosignals to be obtained. Water mixed with alcohol can also be used to reduce the size of the vapor or mist droplets. The film surface can also be wetted by contacting it with absorbent cotton or cloth soaked in water.
[0246] The water that wets the surface of the cured film may contain a salt, and the water-soluble salt that is mixed with the water is selected from sodium salts, potassium salts, calcium salts, magnesium salts, and betaines.
[0247] Specifically, the water-soluble salt may be a salt selected from sodium chloride, potassium chloride, calcium chloride, magnesium chloride, saccharin sodium salt, acesulfame potassium, sodium carboxylate, potassium carboxylate, calcium carboxylate, sodium sulfonate, potassium sulfonate, calcium sulfonate, sodium phosphate, potassium phosphate, calcium phosphate, magnesium phosphate, and betaine. Note that the above-mentioned components (A) and (C) are not included in the water-soluble salt.
[0248] More specifically, in addition to the above, sodium acetate, sodium propionate, sodium pivalate, sodium glycolate, sodium butyrate, sodium valerate, sodium caproate, sodium enanthate, sodium caprylate, sodium pelargonate, sodium caprate, sodium undecylate, sodium laurate, sodium tridecylate, sodium myristate, sodium pentadecylate, sodium palmitate, sodium margarate, sodium stearate, sodium benzoate, disodium adipate, disodium maleate, disodium phthalate, sodium 2-hydroxybutyrate, sodium 3-hydroxybutyrate, sodium 2-oxobutyrate, sodium gluconate, methane Examples of betaines include sodium sulfonate, sodium 1-nonanesulfonate, sodium 1-decanesulfonate, sodium 1-dodecanesulfonate, sodium 1-undecanesulfonate, sodium cocoyl ethionate, sodium lauroyl methyl alanine, sodium cocoyl methyl taurate, sodium cocoyl glutamate, sodium cocoyl sarcosine, sodium lauroyl methyl taurate, laumidopropyl betaine, potassium isobutyrate, potassium propionate, potassium pivalate, potassium glycolate, potassium gluconate, potassium methanesulfonate, calcium stearate, calcium glycolate, calcium gluconate, calcium 3-methyl-2-oxobutyrate, and calcium methanesulfonate. Betaine is a general term for intramolecular salts, specifically a compound in which three methyl groups are added to the amino group of an amino acid, and more specifically, trimethylglycine, carnitine, and proline betaine can be mentioned.
[0249] The water that wets the surface of the cured film may further contain a monohydric alcohol or polyhydric alcohol having 1 to 4 carbon atoms. The alcohol is preferably selected from ethanol, isopropyl alcohol, ethylene glycol, diethylene glycol, triethylene glycol, glycerin, polyethylene glycol, polypropylene glycol, polyglycerin, diglycerin, or a silicone compound having a polyglycerin structure, and it is more preferable that the silicone compound having a polyglycerin structure is one represented by the above general formula (4)' or (5)'.
[0250] The pretreatment method using a water-soluble salt-containing aqueous solution can wet the bioelectrode membrane after hardening by spraying, dispensing water droplets, etc. It can also be wetted in a high temperature and high humidity state such as a sauna. After wetting, in order to prevent drying, a protective film can be further laminated on the permeation layer to cover it. Since the protective film needs to be peeled off just before applying it to the skin, it can be coated with a release agent or a peelable Teflon (registered trademark) film can be used. For long-term storage, the dry electrode covered with the release film is preferably sealed in a bag covered with aluminum or the like. In order to prevent drying in the aluminum-covered bag, it is preferable to seal moisture in it.
[0251] Before attaching the bioelectrode of the present invention to the skin, the skin side can be moistened with water, alcohol, etc., or the skin can be wiped with a cloth or absorbent cotton containing water, alcohol, etc. The above-mentioned salt can also be contained in the water or alcohol.
[0252] As described above, the manufacturing method of the bioelectrode of the present invention makes it possible to easily manufacture, at low cost, the bioelectrode of the present invention which has excellent conductivity and biocompatibility, is lightweight, and whose conductivity does not decrease significantly whether it is wetted with water or dried. EXAMPLES
[0253] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these. In the following, "Me" represents a methyl group and "Vi" represents a vinyl group.
[0254] (ionic polymer) Ionic polymers 1 to 14, blended ionic polymer 1, and comparative ionic polymer 1, which were blended as ionic materials (conductive materials) in the bioelectrode composition solution, were synthesized as follows. A 30% by mass cyclopentanone solution of each monomer was placed in a reaction vessel and mixed, and the reaction vessel was cooled to -70°C under a nitrogen atmosphere, and degassed under reduced pressure and nitrogen blowing were repeated three times. After heating to room temperature, 0.02 mol of azobisisobutyronitrile (AIBN) was added as a polymerization initiator per mol of the total monomers, and the mixture was heated to 60°C and reacted for 15 hours. The composition of the obtained polymer was determined after drying the solvent. 1 The molecular weight (Mw) and dispersity (Mw / Mn) of the obtained polymer were confirmed by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent. The ionic polymers 1 to 14, blend ionic polymer 1, and comparative ionic polymer 1 thus synthesized are shown below.
[0255] Ionic Polymer 1 Mw=38,800 Mw / Mn=1.91 [ka]
[0256] Ionic Polymer 2 Mw=24,600 Mw / Mn=1.85 [ka]
[0257] Ionic Polymer 3 Mw=54,300 Mw / Mn=1.95 [ka]
[0258] Ionic Polymer 4 Mw=25,500 Mw / Mn=1.89 [ka] (The number of repetitions in the formula indicates the average value.)
[0259] Ionic Polymer 5 Mw=23,100 Mw / Mn=1.61 [ka]
[0260] Ionic Polymer 6 Mw=16,400 Mw / Mn=1.98 [ka]
[0261] Ionic Polymer 7 Mw=42,100 Mw / Mn=2.11 [ka] (The number of repetitions in the formula indicates the average value.)
[0262] Ionic Polymer 8 Mw=19,800 Mw / Mn=1.91 [ka] (The number of repetitions in the formula indicates the average value.)
[0263] Ionic Polymer 9 Mw=21,300 Mw / Mn=2.05 [ka] (The number of repetitions in the formula indicates the average value.)
[0264] Ionic Polymer 10 Mw=22,400 Mw / Mn=1.74 [ka]
[0265] Ionic Polymer 11 Mw=26,600 Mw / Mn=1.99 [ka]
[0266] Ionic Polymer 12 Mw=21,500 Mw / Mn=1.75 [ka]
[0267] Ionic Polymer 13 Mw=22,100 Mw / Mn=1.69 [ka] (The number of repetitions in the formula indicates the average value.)
[0268] Ionic Polymer 14 Mw=24,500 Mw / Mn=1.64 [ka] (The number of repetitions in the formula indicates the average value.)
[0269] Ionic Polymer 15 Mw=44,800 Mw / Mn=1.99 [ka] (The number of repetitions in the formula indicates the average value.)
[0270] Ionic Polymer 16 Mw=48,600 Mw / Mn=1.96 [ka] (The number of repetitions in the formula indicates the average value.)
[0271] Ionic Polymer 17 Mw=62,600 Mw / Mn=1.99 [ka] (The number of repetitions in the formula indicates the average value.)
[0272] Blend ionic polymer 1 and comparative ionic polymer 1 for comparison are shown below.
[0273] Blended ionic polymer 1 Mw=39,100 Mw / Mn=1.91 [ka] (The number of repetitions in the formula indicates the average value.)
[0274] Comparative ionic polymer 1 Mw=26,900 Mw / Mn=1.99 [ka]
[0275] (Composite carbon particles) 5 g of carbon black (Denka Black Li-400 manufactured by Denka Corporation) and 1 g of pyridine were added to 100 g of methyl isobutyl ketone (MIBK) and stirred, and 5 g of a 30 wt % cyclopentanone solution of ionic polymer 1 was dropped thereinto. After stirring at 60°C for 20 hours, the solvent was dried to synthesize ionic polymer 1 composite carbon black.
[0276] In a similar manner, ionic polymer 2 composite carbon black to ionic polymer 13 composite carbon black, ionic polymer 15 composite carbon black, ionic polymer 16 composite carbon black, ionic polymer 17 composite carbon black, and comparative ionic polymer 1 composite carbon black were synthesized.
[0277] 5 g of carbon black (Denka Black Li-400 manufactured by Denka Corporation) was added to 100 g of methyl isobutyl ketone (MIBK) and stirred, and 5 g of a 30 wt % cyclopentanone solution of ionic polymer 14 and 0.01 g of tributyltin were added dropwise thereto, and the mixture was stirred at 60°C for 20 hours, after which the solvent was dried to synthesize ionic polymer 14 composite carbon black.
[0278] 5 g of carboxylated multi-walled carbon nanotubes (SIGMA-Aldrich) and 1 g of pyridine were added to 100 g of methyl isobutyl ketone (MIBK) and stirred, and 5 g of a 30 wt % cyclopentanone solution of ionic polymer 8 was dropped into the mixture. After stirring at 60°C for 20 hours, the solvent was dried to synthesize ionic polymer 8 composite carbon nanotubes.
[0279] 5 g of graphene oxide (SIGMA-Aldrich) and 1 g of pyridine were added to 100 g of methyl isobutyl ketone (MIBK) and stirred, and 5 g of a 30 wt% cyclopentanone solution of ionic polymer 8 was dropped into the mixture. After stirring at 60°C for 20 hours, the solvent was dried to synthesize ionic polymer 8 composite graphene.
[0280] 5 g of graphite (SIGMA-Aldrich, size 20 μm or less) and 1 g of pyridine were added to 100 g of methyl isobutyl ketone (MIBK) and stirred, and 5 g of a 30 wt % cyclopentanone solution of ionic polymer 8 was dropped into the mixture. After stirring at 60°C for 20 hours, the solvent was dried to synthesize ionic polymer 8 composite graphite.
[0281] Siloxane compounds 1 to 4 that were blended as silicone resins in the bioelectrode composition solution are shown below. (Siloxane Compound 1) The viscosity of a 30% toluene solution was 27,000 mPa·s, the alkenyl group content was 0.007 mol / 100 g, and the vinyl group-containing polydimethylsiloxane whose molecular chain ends were blocked with SiMe2Vi groups was designated as siloxane compound 1. (Siloxane compound 2) Me3SiO 0.5 Polysiloxane (Me3SiO 0.5 A 60% toluene solution of siloxane compound 2 (SiO2 unit / SiO2 unit = 0.8) was used as the siloxane compound 2. (Siloxane Compound 3) 40 parts by mass of vinyl-containing polydimethylsiloxane whose molecular chain ends are capped with OH, whose viscosity in a 30% toluene solution is 42,000 mPa s and whose alkenyl group content is 0.007 mol / 100 g, Me3SiO 0.5 Polysiloxane (Me3SiO 0.5 A solution consisting of 100 parts by mass of a 60% toluene solution of 1,2-dichloro-2,4-diphenyl-2,4-tetramethylphenyl-2,5-diphenyl-2,6-diphenyl-2,7-diphenyl-2,8-diphenyl-2,7-diphenyl-2,8-diphenyl-2,6-diphenyl-2,7 ... (Siloxane Compound 4) As the methyl hydrogen silicone oil, KF-99 manufactured by Shin-Etsu Chemical Co., Ltd. was used.
[0282] Polyglycerin silicone compounds (polyglycerin compounds) 1 to 7 are shown below.
[0283] [ka]
[0284] The organic solvents contained in the bioelectrode composition solution are shown below. Isopar G: Isoparaffinic solvent, manufactured by Standard Oil Isopar M: Isoparaffinic solvent, manufactured by Standard Oil
[0285] The lithium titanate powder, platinum catalyst, and conductivity enhancer (carbon black, carbon nanotubes, and metal powder) that were blended as additives in the bioelectrode composition solution are shown below. Metal powder Silver powder: Sigma-Aldrich silver flakes, diameter 10 μm Lithium titanate powder, spinel: Sigma-Aldrich, size 200nm or less Platinum catalyst: CAT-PL-50T manufactured by Shin-Etsu Chemical Co., Ltd. Carbon black: Denka Black Li-400 manufactured by Denka Multi-walled carbon nanotubes: Sigma-Aldrich, diameter 110-170 nm, length 5-9 μm
[0286] [Examples 1 to 20, Comparative Examples 1 to 3] Ionic polymer composite carbon particles, resin, blended ionic polymer, organic solvent, and additives (platinum catalyst, conductivity enhancer, etc.) were blended in the compositions shown in Tables 1 and 2 to prepare bioelectrode composition solutions (bioelectrode composition solutions 1 to 20, comparative bioelectrode composition solutions 1 to 3).
[0287] [Table 1]
[0288] [Table 2]
[0289] (Preparation of bioelectrodes) As shown in FIG. 3, a conductive paste manufactured by Fujikura Kasei, Dotite FA-333, was coated on ST-604 of a thermoplastic urethane (TPU) film 20 manufactured by Bemis by screen printing, and baked in an oven at 120° C. for 10 minutes to print a keyhole-shaped conductive pattern 2 with a diameter of 2 cm. The bioelectrode composition solution shown in Tables 1 and 2 was applied by screen printing on the circular part on top of the film, air-dried at room temperature for 10 minutes, and then baked in an oven at 125° C. for 10 minutes to evaporate the solvent and harden the film to form a biocontact layer 3, which was used as a bioelectrode 1. Next, as shown in FIG. 4, the thermoplastic urethane film 20 on which the bioelectrode 1 was printed was cut out, and a double-sided tape 21 was attached to the film, to prepare three bioelectrode samples 10 for each composition solution.
[0290] (Measurement of the thickness of the biological contact layer) The thickness of the biocontact layer of the bioelectrode prepared above was measured using a micrometer. The results are shown in Table 3.
[0291] (Measurement of biological signals) The conductive wiring pattern made of conductive paste of the bioelectrode was connected with a portable electrocardiograph HCG-901 manufactured by Omron Healthcare Co., Ltd. with a conductive wire, and the positive electrode of the electrocardiograph was attached to the LA position of the human body in Figure 5, the negative electrode to the LL position, and the earth to the RA position. Immediately after attachment, electrocardiogram measurement was started, and the time until the electrocardiogram waveform (ECG signal) consisting of P, Q, R, S, and T waves shown in Figure 6 appeared was measured. The results are shown in Table 3.
[0292] [Table 3]
[0293] As shown in Table 3, in Examples 1 to 20 in which a biocontact layer was formed using the bioelectrode composition of the present invention containing a complex of an ionic polymer and carbon particles, a biosignal could be obtained in a short time after application to the body. On the other hand, in the case of adding only carbon particles or in the case of Comparative Examples 1 and 3 in which no ionic component with a specific structure was contained, a biosignal could not be obtained. In the case of Comparative Example 2 in which only an ionic polymer was added, it took a long time for a biosignal to appear after application to the skin.
[0294] From the above, a bioelectrode having a biocontact layer formed using the bioelectrode composition of the present invention has excellent electrical conductivity, biocompatibility, and adhesion to conductive substrates, and has high ionic conductivity, allowing biosignals to be obtained immediately after being attached to the skin.
[0295] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0296] 1...bioelectrode, 2...conductive substrate (conductive pattern), 3...biocontact layer, 4...ionic reaction complex, 5...blended ionic polymer, 6...adhesive resin, 7...Body, 10...Bioelectrode sample, 20...Thermoplastic urethane film, 21...Double-sided tape.
Claims
1. A bioelectrode composition comprising: (A) a reaction complex of an ionic polymer material and carbon particles; the component (A) contains carbon particles chemically bonded to a polymer having a repeating unit having a structure selected from the group consisting of an ammonium salt, a lithium salt, a sodium salt, a potassium salt, and a silver salt of any one of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide; The repeating unit has a structure represented by any one of the following general formulas (1)-1 to (1)-4: A bioelectrode composition, characterized in that the component (A) is obtained by reacting 100 parts by mass of carbon particles with 5 parts by mass or more of a polymer that reacts with the carbon particles. [Formula 1] (In the formula, Rf 1 and Rf 2 are a hydrogen atom, a fluorine atom, an oxygen atom, a methyl group, or a trifluoromethyl group. When Rf 1 and Rf 2 are oxygen atoms, Rf 1 and Rf 2 are one oxygen atom bonding to one carbon atom to form a carbonyl group. Rf 3 and Rf 4 are a hydrogen atom, a fluorine atom, or a trifluoromethyl group. One or more of Rf 1 to Rf 4 are a fluorine atom or a trifluoromethyl group. Rf 5 , Rf 6 , and Rf 7 are a fluorine atom or a linear or branched alkyl group having 1 to 4 carbon atoms and having at least one fluorine atom. m is an integer of 1 to 4. M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion.)
2. 2. The bioelectrode composition according to claim 1, wherein the carbon particles are selected from the group consisting of carbon black, carbon nanotubes, graphite, and graphene.
3. The repeating unit having a structure selected from the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide is one or more selected from the repeating units a1 to a7 represented by the following general formula (2): The bioelectrode composition according to claim 1 or 2. [chemical 2] (In the formula, R 1 , R 3 , R 5 , R 8 , R 10 , R 11 and R 13 are each independently a hydrogen atom or a methyl group, R 2 , R 4 , R 6 , R 9 , R 12 and R 14 R each independently represents a single bond, or a linear, branched or cyclic hydrocarbon group having 1 to 13 carbon atoms which may have either an ester group or an ether group, or both. 7 is a linear or branched alkylene group having 1 to 4 carbon atoms; R 7 One or two of the hydrogen atoms in X may be substituted with a fluorine atom. 1 , X 2 , X 3 , X 4 , X 6 , and X 7 each independently represents a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group; X 5 is a single bond, an ether group, or an ester group. Y is an oxygen atom, -NR 19 - group, and R 19 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 4may be bonded to form a ring. m is an integer of 1 to 4. a1, a2, a3, a4, a5, a6 and a7 are within the ranges of 0≦a1≦1.0, 0≦a2≦1.0, 0≦a3≦1.0, 0≦a4≦1.0, 0≦a5≦1.0, 0≦a6≦1.0, 0≦a7≦1.0, and 0<a1+a2+a3+a4+a5+a6+a7≦1.
0. M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion. 5 , Rf 6 , Rf 7 is a fluorine atom or a linear or branched alkyl group having 1 to 4 carbon atoms and having at least one fluorine atom.
4. The bioelectrode composition according to claim 3, characterized in that the component (A) contains a complex obtained by reacting carbon particles with a polymer that reacts with carbon particles and is copolymerized with a repeating unit b1 having an oxirane group or an oxetane group, or a repeating unit b2 having an isocyanate group, as shown in the following general formula (4): [C3] (In the formula, R 20 , R 24 is a hydrogen atom or a methyl group, and X 8 is a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group; 9 is an ester group, R 21 R is a single bond, a linear, branched or cyclic alkylene group having 1 to 20 carbon atoms, or a phenylene group, which may contain an ether group, an ester group or a hydroxyl group. 22 are hydrogen atoms or identical or non-identical alkyl groups having 1 to 4 carbon atoms, R 21 may be bonded to form a ring. 23 is a methylene group or an ethylene group, and R 21 may be bonded to form a ring. 25 R is a linear or branched alkylene group having 1 to 20 carbon atoms, which may have an ether group. 26is a single bond or a methylene group. B is an isocyanate group, which may be a blocked isocyanate group. 0≦b1<1.0, 0≦b2<1.0, 0<b1+b2<1.
0.
5. The bioelectrode composition according to any one of claims 1 to 4, characterized in that the component (A) contains an ammonium ion represented by the following general formula (3) as an ammonium ion constituting the ammonium salt: [C4] (In the formula, R 101d , R 101e , R 101f , R 101g R each represents a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 13 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , R 101d and R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e and R 101d and R 101e and R 101f is an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the ring.
6. The bioelectrode composition according to any one of claims 1 to 5, further comprising an adhesive resin as component (B).
7. 7. The bioelectrode composition according to claim 6, wherein the component (B) is at least one selected from the group consisting of silicone resins, (meth)acrylate resins, and urethane resins.
8. 8. The bioelectrode composition according to claim 6, characterized in that the component (B) contains a diorganosiloxane having an alkenyl group and an organohydrogenpolysiloxane having a SiH group.
9. The component (B) further includes R x SiO (4-x)/2 units (R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and x is in the range of 2.5 to 3.5) and SiO 2 9. The bioelectrode composition according to claim 8, which contains a silicone resin having a unit.
10. The bioelectrode composition according to any one of claims 1 to 9, further comprising, as component (C), a polymer compound having an ionic repeating unit.
11. The ionic repeating unit of the component (C) is a repeating unit having a structure selected from the ammonium salt, lithium salt, sodium salt, potassium salt, and silver salt of any of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide represented by the following general formula (2). The bioelectrode composition according to claim 10. [C5] (In the formula, R 1 , R 3 , R 5 , R 8 , R 10 , R 11 and R 13 are each independently a hydrogen atom or a methyl group, R 2 , R 4 , R 6 , R 9 , R 12 and R 14 R each independently represents a single bond, or a linear, branched or cyclic hydrocarbon group having 1 to 13 carbon atoms which may have either an ester group or an ether group, or both. 7 is a linear or branched alkylene group having 1 to 4 carbon atoms; R 7 One or two of the hydrogen atoms in X may be substituted with a fluorine atom. 1 , X 2 , X 3 , X 4 , X 6 , and X 7 each independently represents a single bond, a phenylene group, a naphthylene group, an ether group, an ester group, or an amide group; X 5 is a single bond, an ether group, or an ester group. Y is an oxygen atom, -NR 19 - group, and R 19 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; R 4 may be bonded to form a ring. m is an integer of 1 to 4. a1, a2, a3, a4, a5, a6 and a7 are within the ranges of 0≦a1≦1.0, 0≦a2≦1.0, 0≦a3≦1.0, 0≦a4≦1.0, 0≦a5≦1.0, 0≦a6≦1.0, 0≦a7≦1.0, and 0<a1+a2+a3+a4+a5+a6+a7≦1.
0. M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion. 5 , Rf 6 , Rf 7 is a fluorine atom or a linear or branched alkyl group having 1 to 4 carbon atoms and having at least one fluorine atom.
12. The bioelectrode composition according to any one of claims 1 to 11, further comprising carbon powder and / or metal powder as component (D).
13. 13. The bioelectrode composition according to claim 12, wherein the carbon powder is at least one of carbon black, graphite, and carbon nanotubes.
14. 14. The bioelectrode composition according to claim 12, wherein the metal powder is selected from the group consisting of gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium.
15. 15. The bioelectrode composition according to claim 14, wherein the metal powder is silver powder.
16. The bioelectrode composition according to any one of claims 1 to 15, further comprising an organic solvent as component (E).
17. A bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, the bioelectrode being characterized in that the biocontact layer is a cured product of the bioelectrode composition according to any one of claims 1 to 16.
18. The bioelectrode according to claim 17, characterized in that the conductive base material contains one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
19. A method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, comprising applying a bioelectrode composition according to any one of claims 1 to 16 onto the conductive substrate and curing the composition to form the biocontact layer.
20. The method for manufacturing a bioelectrode according to claim 19, characterized in that the conductive base material contains one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
21. A reaction complex between an ionic polymer material and carbon particles, the reaction complex being carbon particles chemically bonded to a polymer having a repeating unit having a structure selected from the group consisting of an ammonium salt, a lithium salt, a sodium salt, a potassium salt, and a silver salt of any one of fluorosulfonic acid, fluorosulfonimide, and N-carbonylfluorosulfonamide; The repeating unit has a structure represented by any one of the following general formulas (1)-1 to (1)-4: A reaction complex, characterized in that the component (A) is obtained by reacting 100 parts by mass of carbon particles with 5 parts by mass or more of a polymer that reacts with the carbon particles. [C6] (In the formula, Rf 1 and Rf 2 are a hydrogen atom, a fluorine atom, an oxygen atom, a methyl group, or a trifluoromethyl group. When Rf 1 and Rf 2 are oxygen atoms, Rf 1 and Rf 2 are one oxygen atom bonding to one carbon atom to form a carbonyl group. Rf 3 and Rf 4 are a hydrogen atom, a fluorine atom, or a trifluoromethyl group. One or more of Rf 1 to Rf 4 are a fluorine atom or a trifluoromethyl group. Rf 5 , Rf 6 , and Rf 7 are a fluorine atom or a linear or branched alkyl group having 1 to 4 carbon atoms and having at least one fluorine atom. m is an integer of 1 to 4. M + is an ion selected from an ammonium ion, a lithium ion, a sodium ion, a potassium ion, and a silver ion.)
22. 22. The reactive composite of claim 21, wherein the carbon particles are selected from carbon black, carbon nanotubes, graphite, and graphene.
Citation Information
Patent Citations
Wireless wearable neural signal detectiondevice and system
CN110811594A
Conductive millable urethane rubber electrode
JP1993095924A
Silicone rubber composition for living body electrode and electrode for living body
JP2003225217A
Long-life conjugated polymer electrochemical device incorporating ionic liquid
JP2004527902A
Biocompatible electrode structure and manufacturing method therefor, and device and manufacturing method therefor
JP2015019806A