Method for producing vanadium dioxide particles having a surface protective layer
A surface protective layer of Al oxide or hydroxide on vanadium dioxide particles addresses the degradation issue, ensuring stable silicone resin performance over time by inhibiting oxidation.
Patent Information
- Application Number
- JP2023136049
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-24
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2039-10-11
AI Technical Summary
Vanadium dioxide particles dispersed in silicone resin deteriorate and deform over long-term storage, especially under high temperature and humidity conditions, leading to degradation of the silicone resin.
A surface protective layer containing at least an oxide or hydroxide of Al is formed on vanadium dioxide particles using a precursor such as metal alkoxide or β-diketone complex, which suppresses the oxidation of vanadium dioxide and thereby stabilizes the silicone resin.
The silicone resin maintains its integrity and stability over long-term storage, preventing deformation and deterioration even in harsh environments.
Smart Images

Figure 0007569423000002 
Figure 0007569423000003 
Figure 0007569423000001
Abstract
Description
[Technical field]
[0001] The present invention relates to vanadium dioxide particles having a surface protective layer that can be maintained without corroding a silicone resin even when stored for a long period of time. The present invention relates to a method for producing the same. [Background technology]
[0002] Vanadium dioxide or substituted vanadium dioxide, in which some of the vanadium ions in vanadium dioxide are replaced with other metal ions, undergoes a phase transition from a semiconductor to a metal above a certain temperature, and its use as a heat storage material that utilizes the absorption and release of heat that accompanies this phase transition is being investigated. In utilizing vanadium dioxide and substituted vanadium dioxide, it has been considered to disperse these particles in a resin and use them as a bulk material.
[0003] For example, it has been disclosed that vanadium dioxide particles having heat storage properties are mixed with silicone resin and molded (see Patent Documents 1 and 2). Also, although not a heat storage material, it has been disclosed that when vanadium dioxide is used as a thermochromic material, a surface protective layer is provided on vanadium dioxide particles in order to prevent deterioration of the thermochromic properties (see Patent Document 3).
[0004] Since electronic devices generate heat and can cause malfunctions, heat dissipation compounds such as silicone resin heat dissipation sheets and tubes are used to protect electronic devices from heat and to conduct the generated heat to heat dissipation components to dissipate it so that they can function normally. Some heat dissipation sheets and tubes are made of silicone resin with added thermally conductive fillers such as alumina and magnesia. It is also known that vanadium dioxide particles are kneaded into the silicone resin as a heat storage material to slow down the rate at which heat is transferred.
[0005] However, the inventors have discovered that when vanadium dioxide particles, which have heat storage properties, are mixed with silicone resin and molded to form a silicone resin heat dissipation sheet intended to be filled between heat dissipation components and aid in heat dissipation, a problem occurs in that the silicone resin changes in quality and becomes deformed when the vanadium dioxide particles are dispersed in the silicone resin and stored for an extended period of time.
[0006] As a technology relating to heat storage sheets, for example, Patent Document 4 discloses that a heat storage silicone material contains an organopolysiloxane, thermally conductive particles, and a heat storage material, and the heat storage material is heat storage material particles obtained by microencapsulating a heat storage substance having a melting point of 0 to 100°C, and contains 100 to 2000 parts by weight of thermally conductive particles per 100 parts by weight of organopolysiloxane and has a thermal conductivity of 0.2 to 10 W / m K, and this heat storage silicone material is obtained by mixing and crosslinking a silicone base polymer component (A), a crosslinking component (B), a catalyst, thermally conductive particles, and 100 to 500 parts by weight of the microencapsulated heat storage material particles per 100 parts by weight of the total of the (A+B) components. However, the heat storage silicone material described in Patent Document 4 is subject to deterioration of the silicone resin when stored for a long period of time. quality No solution to this problem is presented. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2015 / 087620 [Patent Document 2] International Publication No. 2016 / 111139 [Patent Document 3] JP 2013-75806 A [Patent Document 4] JP 2014-208728 A Summary of the Invention [Problem to be solved by the invention]
[0008] We have discovered a new problem when vanadium dioxide particles are dispersed in a silicone resin: when the vanadium dioxide particles are dispersed in the silicone resin and stored for a long period of time, the silicone resin changes in quality and becomes deformed. Patent Documents 1 and 2 describe the surface treatment of vanadium dioxide particles with alkoxysilane or alkyl titanate in order to suppress inhibition of curing when vanadium dioxide particles are dispersed in silicone resin and cured. However, even with this surface treatment, the silicone resin deteriorates and deforms when stored for a long period of time, particularly under high temperature and high humidity conditions. The present invention has a surface protective layer that can solve the above-mentioned problems. Method for producing vanadium dioxide particles The purpose is to provide. [Means for solving the problem]
[0009] The present inventors have discovered that by providing the surface of vanadium dioxide particles with a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al, it is possible to obtain the excellent effect of suppressing deterioration of a silicone resin even when vanadium dioxide is dispersed in the silicone resin, and have completed the present invention.
[0010] That is, the present invention provides the following. (1) At least one of an oxide or hydroxide of Al formed from a precursor containing Al is included. 1. A method for producing vanadium dioxide particles having a surface protective layer, comprising the steps of: A step of mixing a surface treatment liquid containing an Al-containing precursor, which is a metal alkoxide or a derivative thereof, or a β-diketone complex or a derivative thereof, with vanadium dioxide particles to prepare a mixed liquid; removing the solvent in which the precursor is dissolved or dispersed from the mixture; a step of forming a surface protective layer containing at least an oxide or hydroxide of Al on the vanadium dioxide particles from which the solvent has been removed, by heat treating the vanadium dioxide particles at a temperature of 105 to 300° C., which is equal to or higher than the boiling point of the solvent in which the precursor is dissolved or dispersed; A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al, which is formed from a precursor containing Al, . (2) The method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al according to (1), characterized in that the vanadium dioxide particles contain tungsten. (3) A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al as described in (1) or (2), characterized in that the molar ratio of Al ions to the constituent cations contained in the oxide or hydroxide of the surface protective layer is 50 mol % or more. (4) A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al according to any one of (1) to (3), characterized in that the vanadium dioxide particles are produced by carbon reduction of vanadium pentoxide. Effect of the Invention
[0011] According to the present invention, vanadium dioxide particles can be obtained that make it difficult for silicone resin to deteriorate even when stored for long periods of time, so that a silicone resin sheet or silicone resin compound having the vanadium dioxide particles dispersed therein can be used stably for long periods of time. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing an example of the present invention in which a silicone resin molded body did not deteriorate or deform even in a high-temperature and high-humidity environment. [Diagram 2] FIG. 1 is a diagram showing a comparative example in which a silicone resin molded body deteriorates, flows, and deforms in a high-temperature and high-humidity environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present inventors have investigated the cause of the deterioration and breakdown of silicone resin when a silicone resin heat dissipation sheet containing vanadium dioxide particles is stored for a long period of time. As a result, they have found that the deterioration of silicone resin is most likely caused by the progression of surface oxidation of vanadium dioxide particles. As described above, it has been found that the deterioration and breakdown of silicone resin cannot be suppressed even by surface treatment with alkoxysilane or alkyl titanate, which can suppress the inhibition of curing of silicone resin. As a result of further investigation, the present inventors have found that a vanadium dioxide-containing silicone resin heat dissipation sheet and heat dissipation compound can be produced in which the silicone resin does not deteriorate even when stored for a long period of time by forming a surface protective layer on the surface of vanadium dioxide particles by a specified method, and have completed the present invention. That is, the above problem can be solved by providing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al. As described above, as the surface oxidation of vanadium dioxide particles progresses, the silicone resin deteriorates and breaks down; however, by forming a surface protective layer containing at least an aluminum oxide or hydroxide on the surface of the vanadium dioxide particles, the progress of the surface oxidation of the vanadium dioxide particles can be inhibited. As a result, the deterioration of the silicone resin is inhibited even when the particles are stored for long periods of time in a high-temperature, high-humidity environment.
[0014] The Al-containing precursor of the present invention is one that can form an Al-containing hydroxide or oxide when used as a surface protective layer, and examples thereof include metal alkoxides or derivatives thereof, β-diketone complexes or derivatives thereof, diamine complexes or derivatives thereof, diol complexes or derivatives thereof, alkanolamine complexes or derivatives thereof, etc. Among these, metal alkoxides or derivatives thereof, or β-diketone complexes or derivatives thereof are preferred.
[0015] More preferably, the surface protective layer contains aluminum oxide (alumina). The surface protective layer may be a single layer or a multilayer. The surface protective layer preferably has a layer containing aluminum oxide. The surface protective layer may be formed on at least a part of the surface of the vanadium dioxide particle, or may be formed so as to cover the entire surface of the vanadium dioxide particle. Since this can further suppress the oxidation of the vanadium dioxide particle, it is preferable that the surface protective layer is formed so as to cover the entire surface of the vanadium dioxide particle.
[0016] The molar ratio of Al (the molar ratio of Al ions to the constituent cations) contained in the oxide or hydroxide of the surface protective layer is 50 mol % or more, preferably 60 mol % or more, and more preferably 80 mol % or more. The molar ratio of Al in the surface protective layer can be determined, for example, by measuring with an energy dispersive X-ray analysis (EDS system manufactured by Oxford). The oxide or hydroxide composition of the surface protective layer is preferably Al alone or a combination of Al and Zr. The surface protective layer can sufficiently obtain the effects of the present invention using Al alone, but by combining Al with Zr, a dense surface protective layer is formed, making it easier to obtain the effects of the present invention. The surface protective layer preferably has an aluminum oxide (Al2O3) content of 1.0% by mass or more relative to the vanadium dioxide particles of the substrate. If the content is 3.0% by mass or more, the effect of the present invention can be fully achieved. There is no particular upper limit, but if the content is 50% by mass or more, the heat storage capacity may not be sufficient.
[0017] In terms of the average thickness of the surface protective layer, any thickness that produces the effects of the present invention is acceptable, but it is more preferably 0.05 μm or more, and even more preferably 0.1 μm or more. If it is 20 μm or more, the heat storage effect obtained decreases, so it is more preferably less than 20 μm, even more preferably less than 10 μm, and even more preferably less than 6 μm. In other words, in terms of the relationship between the surface protective layer and the vanadium dioxide particles, the configuration of the vanadium dioxide particles having a surface protective layer of the present invention can be expressed as follows: a surface protective layer containing at least an oxide or hydroxide of Al and having an average thickness of 0.05 μm or more and less than 20 μm is formed on the surface of the vanadium dioxide particles, the molar ratio of Al contained in the oxide or hydroxide of the surface protective layer is 50 mol % or more, and the content of Al contained in the surface protective layer relative to the vanadium dioxide particles is 1.0 mass % or more and less than 50 mass %, calculated as Al2O3.
[0018] The manufacturing method of the present invention includes the steps of mixing vanadium dioxide particles with a surface treatment liquid containing an Al-containing precursor, removing the solvent from the mixed liquid, and forming a surface protective layer containing at least an oxide or hydroxide of Al on the vanadium dioxide particles from which the solvent has been removed. According to the above-mentioned production method, vanadium dioxide particles having a surface protective layer can be obtained, so that oxidation of the vanadium dioxide particles is suppressed and it is believed that the silicone resin can be maintained without deterioration even when stored for a long period of time.
[0019] In the above surface treatment step, examples of a method for mixing the surface treatment liquid with the vanadium dioxide particles include a method in which the vanadium dioxide particles are dispersed in the surface treatment liquid and mixed therewith, and a method in which the surface treatment liquid is sprayed onto the vanadium dioxide particles. The mixing conditions are not particularly limited as long as the method can uniformly disperse vanadium dioxide particles, can adhere the surface treatment liquid to the surface of vanadium dioxide particles, etc. Examples of the method for dispersing vanadium dioxide particles in the surface treatment liquid include magnetic stirrer stirring, mechanical stirring with a motor, gas bubbling, liquid circulation, ultrasonic dispersion, rotational dispersion such as with a ball mill or a rotary mixer, or a combination of the above methods.
[0020] In the present invention, the solvent used in the surface treatment liquid may be any solvent capable of dissolving or dispersing the precursor, and may be, for example, an organic solvent, water, etc. Examples of the organic solvent include toluene, methyl ethyl ketone, alcohols, etc. Preferred are alcohols such as methanol, ethanol, isopropanol, butanol, etc. Among these, it is more preferable to use 2-butanol.
[0021] The step of removing the solvent from the mixture may use filtration, sedimentation, centrifugation, drying, or a combination of the above methods. The drying may be performed under normal pressure or under reduced pressure. The temperature during drying is preferably from room temperature to 200°C. In the step of forming a surface protective layer on the vanadium dioxide particles from which the solvent has been removed, the vanadium dioxide particles from which the solvent has been removed are heated to a temperature equal to or higher than the boiling point of the solvent, preferably at a temperature of 105°C or higher, and more preferably at a temperature of 200 to 300°C.
[0022] The present invention Produced by the manufacturing methodThe vanadium dioxide particles (hereinafter also simply referred to as vanadium dioxide particles) preferably have a heat storage property. Vanadium dioxide exists in various crystal phases, but it is preferable for it to undergo a reversible phase transition between monoclinic and tetragonal crystals (rutile type). For example, the phase transition temperature of pure vanadium dioxide is about 68°C. The vanadium dioxide particles also include substituted vanadium dioxide particles in which some of the vanadium atoms are substituted with atoms of tungsten, molybdenum, niobium, tantalum, thallium, tin, rhenium, iridium, osmium, ruthenium, germanium, chromium, iron, gallium, aluminum, fluorine, phosphorus, or the like.
[0023] The phase transition temperature can be adjusted, for example, by substituting a portion of the vanadium atoms in vanadium dioxide with at least one element selected from tungsten, molybdenum, niobium, and tantalum. Thus, the heat storage temperature can be controlled by appropriately selecting vanadium dioxide particles or substituted vanadium dioxide particles, or by appropriately selecting the type of atoms substituted and the substitution rate in the substituted vanadium dioxide particles.
[0024] When the above-mentioned substituted vanadium dioxide is used, the preferable lower limit of the substitution rate of metal atoms is 0.1 atomic % and the preferable upper limit is 10 atomic %. When the substitution rate is 0.1 atomic % or more, the phase transition temperature of the above-mentioned substituted vanadium dioxide can be easily adjusted, and when it is 10 atomic % or less, an excellent heat storage capacity can be ensured. The substitution rate is a percentage that represents the ratio of the number of substituted atoms to the total number of vanadium atoms and the number of substituted atoms. The substitution element is preferably tungsten from the viewpoint of the efficiency of varying the heat storage temperature.
[0025] The surface protective layer containing at least an oxide or hydroxide of Al formed in the above surface treatment step plays a role in suppressing oxidation of the vanadium dioxide particles.
[0026] Vanadium dioxide particles having a surface protective layer obtained by the production method of the present invention can be contained in a silicone heat dissipation sheet that contains at least an oxide or hydroxide of Al.
[0027] the above The content of the vanadium dioxide particles having the above-mentioned surface protective layer in the silicone heat dissipation sheet is, for example, preferably 0.001% by mass lower and 95% by mass upper, based on 100% by mass of the heat dissipation sheet. The necessity for the upper and lower limits lies in the range necessary for retaining the vanadium dioxide particles in the silicone heat dissipation sheet. The content of vanadium dioxide particles having the above surface protective layer makes it possible to obtain a heat dissipation sheet having excellent heat storage properties.
[0028] the above The heat dissipation sheet is made of silicone resin as its base material. As the silicone resin, a conventionally known silicone resin can be used. The silicone resin may be used alone or in combination of two or more kinds. Vanadium Dioxide Particles The vanadium dioxide particles may be produced by any method, but vanadium dioxide particles produced by carbon reduction of vanadium pentoxide are more preferable from the viewpoint of mass productivity. Vanadium Dioxide Particles The particle size may be any, but the average particle size is preferably 0.07 μm to 250 μm. Also, crushed particles obtained by crushing larger particles may be used. EXAMPLES
[0029] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0030] Example 1 (1) Method for forming a surface protective layer (coating) 50 g of alkyl acetoacetate aluminum diisopropylate (product name PLENACT AL-M, manufactured by Ajinomoto Fan Techno Co., Ltd.) was dissolved in 500 ml of MEK (methyl ethyl ketone). 1,000 g of VO2 particles (average particle size: 80 μm) were immersed in this liquid and stirred. After stirring and mixing, the mixture was concentrated to dryness using a rotary evaporator. Further, it was dried in a vacuum dryer at 40° C. for 24 hours. Next, the VO2 particles were taken out and dried at 80℃ for 1 h. By heat treatment (baking) at 200℃ for 6 hours, VO2 particles with a surface protective layer containing at least an oxide or hydroxide of Al were produced. The Al content in the surface protective layer of the VO2 particles was measured by energy dispersive X-ray analysis (EDS system, manufactured by Oxford), and was found to be 3.0 mass% in terms of Al2O3. The thickness of the surface protective layer was measured by a field emission scanning electron microscope (JEOL JSM-7900F), and was found to be 2 μm on average. The molar ratio of Al in the surface protective layer was 50 mol %.
[0031] (2) Mixing into silicone resin After the above treatment, the VO2 particles having the above surface protective layer were kneaded into silicone resin (product name TSE3062, manufactured by Momentive) in a ratio of silicone resin:VO2 = 50 parts by mass:50 parts by mass, and molded into a cylindrical shape with a diameter of 5 mm and a height of 30 mm, producing a silicone resin molded body kneaded with VO2 particles having a surface protective layer. The content of the vanadium dioxide particles in the silicone resin molded article was 50% by mass.
[0032] (3) Durability test of silicone resin molded body The VO2 particles having a surface protective layer containing at least an oxide or hydroxide of Al obtained above are Silicone resin molded body A durability test was carried out for a comparative example of a silicone resin molding incorporating VO2 particles without a surface protective layer prepared in the same manner as above by holding the molded body at 80°C x 80% (humidity) x 14 days, and the test results were evaluated.
[0033] As shown in FIG. 1, VO2 particles having a surface protective layer containing at least an oxide or hydroxide of Al were The silicone resin molded body is However, the silicone resin molding did not deteriorate, flow, or lose its shape. On the other hand, as shown in FIG. 2, the silicone resin molded body of the comparative example, in which VO2 particles without a surface protective layer were kneaded, flowed and could not maintain its shape. Thus, it was confirmed that applying the surface protective layer of the present invention to the VO2 particles to be kneaded into the silicone resin is effective in suppressing deterioration of the silicone resin.
[0034] Example 2 (1) Method for forming a surface protective layer (coating) 50 g of alkyl acetoacetate aluminum diisopropylate (product name PLENACT AL-M, manufactured by Ajinomoto Fan Techno Co., Ltd.) was dissolved in 500 ml of MEK (methyl ethyl ketone). 1,000 g of VO2 particles (average particle size: 80 μm) were immersed in this liquid and stirred. After stirring and mixing, the mixture was concentrated to dryness using an evaporator. Further, it was dried in a vacuum dryer at 40° C. for 24 hours.
[0035] (2) Mixing into silicone resin After the above treatment, the VO2 particles prepared in (1) above were kneaded into silicone resin (product name TSE3062, manufactured by Momentive Corporation) in a ratio of silicone resin:VO2 = 50 parts by mass:50 parts by mass, and molded into a cylindrical shape with a diameter of 5 mm and a height of 30 mm, producing a silicone resin molded body kneaded with the VO2 particles.
[0036] (3) Durability test of silicone resin molded body The silicone resin molded body kneaded with the VO2 particles prepared in (1) above was subjected to a durability test by maintaining it at 80°C x 80% (humidity) x 14 days in the same manner as in Example 1, and the test results were evaluated.
[0037] Although it did not flow like the comparative silicone resin molding (see Figure 2) which contained VO2 particles without a surface protective layer, it did deform slightly. In this way, it was confirmed that in the method of forming (coating) a surface protective layer on VO2 particles kneaded into silicone resin, further heat treatment (baking) at a temperature of 200 to 300°C is effective in suppressing deterioration of the silicone resin.
[0038] Example 3 (1) Method for forming a surface protective layer (coating) 50 g of alkyl acetoacetate aluminum diisopropylate (product name PLENACT AL-M, manufactured by Ajinomoto Fan Techno Co., Ltd.) was dissolved in 500 ml of MEK (methyl ethyl ketone). 1,000 g of VO2 particles (average particle size: 80 μm) were immersed in this liquid and stirred. After stirring and mixing, the mixture was concentrated to dryness using an evaporator. Further, it was dried in a vacuum dryer at 40° C. for 24 hours. The VO2 particles were then taken out and dried at 80°C for 1 h.
[0039] (2) Mixing into silicone resin After the above treatment, the VO2 particles were kneaded into silicone resin (product name TSE3062, manufactured by Momentive) in a ratio of silicone resin:VO2 = 50 parts by mass:50 parts by mass, and molded into a cylindrical shape with a diameter of 5 mm and a height of 30 mm, producing a silicone resin molded body kneaded with the VO2 particles.
[0040] (3) Durability test of silicone resin molded body The silicone resin molded body kneaded with the VO2 particles obtained above was subjected to a durability test by maintaining it at 80°C x 80% (humidity) x 14 days, and the test results were evaluated.
[0041] Although there was no flowing as in the comparative example of the silicone resin molded body kneaded with VO2 particles without a surface protective layer (see FIG. 2), there was a slight deformation, however, the deformation was smaller than that in Example 2. As is clear from the comparison of Examples 1 to 3, in the method of forming (coating) a surface protective layer on VO2 particles kneaded into silicone resin, it was confirmed that drying for 1 hour at 80°C is effective, and further heat treatment (baking) at a temperature of 200 to 300°C is effective in suppressing deterioration of the silicone resin.
[0042] Example 4 (1) Method for forming a surface protective layer (coating) A predetermined amount of aluminum sec-butoxide was dissolved in 500 ml of methoxyethanol. 1,000 g of VO2 particles (average particle size: 80 μm) were immersed in this liquid and stirred. After stirring and mixing, the mixture was concentrated to dryness using a rotary evaporator. Further, it was dried in a vacuum dryer at 40° C. for 24 hours. Next, the VO2 particles were taken out, dried at 80°C for 1 h, and then heat-treated at 250°C for 6 h to produce VO2 particles with a surface protective layer. (2) Mixing into silicone resin The same method as in Example 1 was used. (3) Durability test of silicone resin molded body The same method as in Example 1 was used. The Al content in the surface protective layer of the VO2 particles was measured by energy dispersive X-ray analysis (EDS system, manufactured by Oxford), and was found to be 3.0 mass% in terms of Al2O3. The thickness of the surface protective layer was measured by a field emission scanning electron microscope (JEOL JSM-7900F), and was found to be 2 μm on average. The molar ratio of Al in the surface protective layer was 50 mol %.
[0043] In the above (1), VO2 particles with different average thicknesses of the surface protective layer were prepared by changing the amount of aluminum sec-butoxide (0.04, 0.05, 0.1, 1.5, 6.5, 6, 10, 20 μm), and a durability test of the silicone resin molded body was performed. As a result, all VO2 particles were effective in suppressing the deterioration of the silicone resin compared to VO2 particles without a surface protective layer. When the surface protective layer was 0.04 μm thick, slight deformation occurred in some cases. On the other hand, when the thickness was 20 μm, no deformation occurred, but the amount of heat storage per mass was smaller.
[0044] Example 5 (1) Method for forming a surface protective layer (coating) 50 g of aluminum ethyl acetoacetate diisopropylate was dissolved in 500 ml of methyl ethyl ketone. 1,000 g of VO2 particles (average particle size: 80 μm) were immersed in this liquid and stirred. After stirring and mixing, the mixture was concentrated to dryness using a rotary evaporator. Further, it was dried in a vacuum dryer at 40° C. for 24 hours. Next, the VO2 particles were taken out, dried at 80°C for 1 h, and then heat-treated at 300°C for 6 h to produce VO2 particles with a surface protective layer. (2) Mixing into silicone resin The same method as in Example 1 was used. (3) Durability test of silicone resin molded body The same method as in Example 1 was used. The Al content in the surface protective layer of the VO2 particles was measured by energy dispersive X-ray analysis (EDS system, manufactured by Oxford), and was found to be 3.0 mass% in terms of Al2O3. The thickness of the surface protective layer was measured by a field emission scanning electron microscope (JEOL JSM-7900F), and was found to be 2 μm on average. The molar ratio of Al in the surface protective layer was 50 mol %.
[0045] As in Figure 1, the silicone resin molded body into which the VO2 particles having a surface protective layer were kneaded did not deteriorate, flow, or lose its shape. In this way, it was confirmed that applying the surface protective layer of the present invention, which contains at least an oxide or hydroxide of Al, to the VO2 particles to be kneaded into the silicone resin is effective in suppressing deterioration of the silicone resin. In addition, in the above (1), similar results were obtained when the material was heat-treated at 400°C for 6 hours, but when the material was heat-treated at 500°C for 6 hours, some of the VO2 particles were oxidized to form V2O5.
[0046] Example 6 Predetermined amounts of aluminum sec-butoxide and zirconium n-butoxide were dissolved in 500 ml of methoxyethanol in a mass ratio of 4:1. 1,000 g of VO2 particles (average particle size: 80 μm) were immersed in this liquid and stirred. After stirring and mixing, the mixture was concentrated to dryness using a rotary evaporator. Further, it was dried in a vacuum dryer at 40° C. for 24 hours. Next, the VO2 particles were taken out, dried at 80°C for 1 h, and then heat-treated at 250°C for 6 h to produce VO2 particles with a surface protective layer. (2) Mixing into silicone resin The same method as in Example 1 was used. (3) Durability test of silicone resin molded body The same method as in Example 1 was used. The Al content in the surface protective layer of the VO2 particles was measured by energy dispersive X-ray analysis (EDS system, manufactured by Oxford), and was found to be 3.0 mass% in terms of Al2O3. The thickness of the surface protective layer was measured by a field emission scanning electron microscope (JEOL JSM-7900F), and was found to be 2 μm on average. The molar ratio of Al in the surface protective layer was 50 mol %.
[0047] In the above (1), VO2 particles with different average thicknesses of the surface protective layer were prepared (0.04, 0.05, 0.1, 1.5, 6 μm) in the same manner as in Example 4, and a durability test was performed on the silicone resin molded body. As a result, all of the VO2 particles were effective in suppressing the deterioration of the silicone resin compared to VO2 particles without a surface protective layer, and even a surface protective layer with a thickness of 0.04 μm did not cause deformation.
[0048] Comparative Example 1 Instead of the aluminum coupling agent in Example 1, a silane coupling agent (manufactured by Momentive Corp., product name Silquest A-2120 Silane) was used, and the deterioration suppression effect of the silicone resin was confirmed by a durability test in the same manner as in Example 1. As a result, as in Figure 2, the silicone resin deteriorated, flowed, and lost its shape.
[0049] Comparative Example 2 Instead of the aluminum coupling agent used in Example 1, an organic titanium compound (product name PLENACT TTS, manufactured by AJINOMOTO FAN TECHNO CO., LTD.) was used, and the deterioration suppression effect of the silicone resin was confirmed by a durability test in the same manner as in Example 1. As a result, as in Figure 2, the silicone resin deteriorated, flowed, and lost its shape.
[0050] The test results are summarized in Table 1. As shown in Table 1, it was confirmed that VO2 particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al have a silicone resin deterioration effect, while the other particles have no effect of inhibiting the deterioration of the silicone resin, and the resin deteriorates, flows, and loses its shape. In the column for "Silicone resin deterioration inhibition effect" in Table 1, an "O" mark indicates that in a durability test of 80°C x 80% (humidity) x 14 days, the silicone resin molded body did not flow and maintained its shape (see Figure 1), and an "X" mark indicates that in the durability test under the same conditions, the silicone resin molded body flowed and was unable to maintain its shape (see Figure 2).
[0051] [Table 1]
[0052] Example 7 The vanadium dioxide used in Examples 1-6 and Comparative Examples 1-2 was vanadium dioxide particles produced by carbon reduction of vanadium pentoxide, but vanadium dioxide particles produced by hydrogen reduction of vanadium pentoxide were used. Specifically, V2O5 was reduced with 4% H2 / Ar at 700°C for 48 hours to prepare V2O3. The V2O3 and V2O5 were mixed and fired in a vacuum furnace at 1000°C for 48 hours to produce vanadium dioxide. In the same manner as in Example 1, vanadium dioxide having a surface protective layer was produced. Furthermore, similarly to Example 1, a silicone resin molded body having a surface protective layer and into which VO2 particles were kneaded was produced.
[0053] As a result of evaluation in the same manner as in Example 1, it was found that the silicone resin molded body incorporating VO2 particles having a surface protective layer containing at least an oxide or hydroxide of Al did not deteriorate or flow, resulting in loss of shape. On the other hand, the silicone resin molded body kneaded with VO2 particles that did not have a surface protective layer flowed and was unable to maintain its shape.
[0054] Example 8 Vanadium dioxide with different transition temperatures (tungsten-doped vanadium dioxide) was prepared by mixing a predetermined amount of tungsten oxide with vanadium pentoxide and then reducing it with carbon. Transition temperature 2℃(V 0.976 W 0.024 O2), 20℃(V 0.982 W 0.018 O2), 40℃(V 0.991 W 0.009 Vanadium dioxide having a surface protective layer was produced in the same manner as in Example 1 using vanadium dioxide having a surface protective layer. Furthermore, similarly to Example 1, a silicone resin molded article having a surface protective layer and into which vanadium dioxide particles were kneaded was produced.
[0055] As a result of evaluation in the same manner as in Example 1, it was found that the silicone resin molded body incorporating (tungsten-doped) VO2 particles having a surface protective layer containing at least an oxide or hydroxide of Al did not deteriorate or flow, causing the shape to collapse. On the other hand, the silicone resin molded body kneaded with VO2 particles that did not have a surface protective layer flowed and was unable to maintain its shape.
Claims
1. A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al, comprising the steps of: A step of mixing a surface treatment liquid containing an Al-containing precursor, which is a metal alkoxide or a derivative thereof, or a β-diketone complex or a derivative thereof, with vanadium dioxide particles to prepare a mixed liquid; removing the solvent, which is the surface treatment liquid in which the precursor is dissolved or dispersed, from the mixed liquid; a step of forming a surface protective layer containing at least an oxide or hydroxide of Al on the vanadium dioxide particles from which the solvent has been removed at a temperature of 105 to 300° C., which is equal to or higher than the boiling point of the solvent, which is the surface treatment liquid in which the precursor is dissolved or dispersed; 1. A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al, which is formed from a precursor containing Al,
2. A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al as described in claim 1, characterized in that the vanadium dioxide particles contain tungsten.
3. A method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al as described in claim 1 or 2, characterized in that the molar ratio of Al ions to the constituent cations contained in the oxide or hydroxide of the surface protective layer is 50 mol % or more.
4. The method for producing vanadium dioxide particles having a surface protective layer containing at least an oxide or hydroxide of Al formed from a precursor containing Al according to any one of claims 1 to 3, characterized in that the vanadium dioxide particles are vanadium dioxide particles produced by carbon reduction of vanadium pentoxide.
Citation Information
Patent Citations
Nano-alumina-coated vanadium dioxide nanoparticle and preparation method thereof
CN105668625A
Amorphous alumina-coated vanadium dioxide nanometer powder and preparation method thereof
CN108002442A
Surface modified inorganic minute particle and its usage and method of modifying surface of inorganic minute particle
JP2001240769A
Thermochromic film and thermochromic glass
JP2004346260A
Inorganic-organic composite thermoplastic material and optical element
JP2006213895A