Glossy paint, glittering coating film, glittering laminated coating film and coated objects

The glitter paint formulation with scaly indium particles, plasticizer, and solvent addresses the cost and transmittance issues of traditional indium-based paints, ensuring glitter and high radio wave transmittance, suitable for diverse applications.

JP7569595B1Active Publication Date: 2024-10-18OHASHI CHEM INDS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024084008
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-18
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

Existing glitter paints using indium particles are expensive and reduce radio wave transmittance as the pigment weight concentration increases, limiting their industrial application.

Method used

A glitter paint formulation comprising scaly indium particles, a plasticizer (preferably dioctyl maleate or diethyl succinate), and a solvent, with optional dispersant, where the indium particles are present in a range of 20 to 70% by weight, ensuring sufficient glitter and high radio wave transmittance even with a relatively low indium content, and excluding polymers with molecular weights over 10,000 as binder resins.

Benefits of technology

The formulation achieves glittering effects with reduced indium usage, maintaining high radio wave transmittance and stability, thus providing cost-effective and functional coatings for various objects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569595000001
    Figure 0007569595000001
  • Figure 0007569595000002
    Figure 0007569595000002
Patent Text Reader

Abstract

The object of the present invention is to provide a glittering paint, a glittering coating film, a glittering multilayer coating film, and a coated article that can ensure glittering even when a relatively small amount of indium particles is blended. [Solution] A glittering paint comprising scaly indium particles, a plasticizer, and a solvent, wherein the scaly indium particles are contained in an amount of 20 to 70% by weight based on 100% by weight of the solid content of the glittering paint, and the plasticizer is an aliphatic dibasic acid ester and is contained in an amount of 10 to 85% by weight based on 100% by weight of the solid content of the glittering paint.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glittering paint, a glittering coating film, a glittering multi-layer coating film, and a coated article.

[0002] Electroless plating and vapor deposition are known methods for imparting brilliance (mirror finish) to plastic housings, etc. However, due to concerns about the environmental impact of plating and the need for expensive capital investment and low productivity of vapor deposition, various methods for forming mirror designs other than these have been investigated.

[0003] Methods for forming such mirror designs include, for example, a method using silver colloid or a silver complex solution.

[0004] However, these methods also have problems such as poor weather resistance and corrosion resistance, making it difficult to widely deploy them for industrial use.

[0005] In recent years, therefore, a method of imparting brilliance by using a paint containing indium particles has been investigated.

[0006] For example, Patent Document 1 describes a coated article having: "(a) an undercoat coating layer formed from an undercoat paint, which is provided directly or indirectly on a substrate; and (b) a metal-containing coating layer, which is provided directly or indirectly on the undercoat coating layer, and which has a pigment weight concentration (PWC) of evaporated indium thin film flakes of 72.7% or more, wherein the undercoat paint is (α) a two-component curable coating material containing an isocyanate compound as a curing agent; (β) acrylic lacquer, (γ) Melamine-based paint, or (δ) an active energy ray-curable coating material containing a (meth)acrylic compound having two or more (meth)acryloyl groups in one molecule and forming a three-dimensional network structure by crosslinking and curing, and a polymerization initiator, wherein the (meth)acrylic compound is a diacrylate compound and a urethane (meth)acrylate, The vapor-deposited indium thin film flakes have an average thickness of 0.100 μm or less and 0.010 μm or more, and a cumulative 50% volume particle size D50 of 1.00 μm or less; a volumetric particle size distribution showing a relationship between the particle size of the vapor-deposited indium thin film flakes and the volume fraction of the vapor-deposited indium thin film flakes at the particle size, the volumetric particle size distribution having a first peak and a second peak having a particle size larger than that of the first peak; a volume V1 of the vapor-deposited indium thin film flake at the first peak and a volume V2 of the vapor-deposited indium thin film flake at the second peak satisfy (V1 / V2)×100≧25%, a particle size P1 of the deposited indium thin film flakes at the first peak and a particle size P2 of the deposited indium thin film flakes at the second peak satisfy 6.0≦P2 / P1≦12; The coated article is characterized in that the radio wave transmittance of the coated article is 75% or more in both the 24 GHz band and the 78 GHz band. This makes it possible to provide a coated article having a coating film that is excellent in mirror design and radio wave transmittance and has a low coating film formation temperature. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 7146311 Summary of the Invention [Problem to be solved by the invention]

[0008] However, indium particles are a very expensive material, which means that paints and coatings tend to be expensive.

[0009] In order to ensure high brilliance, for example, as described in Patent Document 1 above, it was necessary to incorporate indium particles (vapor-deposited indium thin film flakes in Patent Document 1) to the extent that the pigment weight concentration (the weight percentage of pigment in 100 weight percent of paint solids) exceeded 70 weight percent. On the other hand, with regard to radio wave transmittance, which is one of the characteristics of coatings using indium particles, there was a tendency for the radio wave transmittance to decrease as the pigment weight concentration of the indium particles increased.

[0010] The present invention has been made in consideration of the above-mentioned matters, and aims to provide a glittering paint, a glittering coating film, a glittering laminated coating film, and a coated article that can ensure glittering even when the amount of indium particles is relatively small. [Means for solving the problem]

[0011] In order to solve the above problems, a glittering paint is provided that comprises scaly indium particles, a plasticizer, and a solvent. Specific embodiments are listed below.

[0012] (Embodiment 1) A glittering paint comprising scaly indium particles, a plasticizer, and a solvent, wherein the scaly indium particles are contained in an amount of 20 to 70% by weight based on 100% by weight of the solid content of the glittering paint, and the plasticizer is an aliphatic dibasic acid ester and is contained in an amount of 10 to 85% by weight based on 100% by weight of the solid content of the glittering paint. The content of the scaly indium particles is preferably 25 to 60% by weight, and more preferably 30 to 50% by weight, based on 100% by weight of the solid content of the glittering coating material.

[0013] This bright paint can ensure sufficient brightness even if the content of the scaly indium particles is relatively small, at 20 to 70% by weight, relative to 100% by weight of the solid content of the bright paint. In addition, since the content of flaky indium particles is relatively small, the radio wave transmittance is also excellent.

[0014] (Aspect 2) The photoluminescent coating according to aspect 1, wherein the plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU).

[0015] This glittering paint can ensure even greater glittering even when the content of the scaly indium particles is relatively small.

[0016] (Embodiment 3) The glittering paint according to embodiment 1 or 2, which does not contain a polymer as a binder resin. Here, "polymer" refers to one with a molecular weight of 10,000 or more. Furthermore, "not containing a polymer as a binder resin" means that it does not substantially contain a "polymer" as a binder resin, and is intended to exclude, for example, a case where a "polymer" is used as a surface treatment agent for scaly indium particles, resulting in the luster paint containing a "polymer." More specifically, for example, it means that 100% by weight of the paint solids does not contain 5% by weight or more of a polymer with a molecular weight of 10,000 or more.

[0017] This glittering paint can ensure even greater glittering even when the content of the scaly indium particles is relatively small.

[0018] (Aspect 4) The glittering paint according to any one of Aspects 1 to 3, further comprising a dispersant. The content of the dispersant is preferably 5 to 30% by weight, more preferably 10 to 25% by weight, and most preferably 15 to 20% by weight, as solids content, based on 100% by weight of the paint solids content.

[0019] This bright paint has high dispersibility of the scaly indium particles, and the paint has improved stability.

[0020] (Aspect 5) The glittering paint according to any one of Aspects 1 to 4, wherein the plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU), and the glittering paint further contains a dispersant.

[0021] This glittering paint can ensure even greater glittering even when the content of the scaly indium particles is relatively small.

[0022] (Embodiment 6) A glittering paint comprising scaly indium particles, a plasticizer, a dispersant, and a solvent, wherein the scaly indium particles are contained in an amount of 20 to 70% by weight based on 100% by weight of the solid content of the glittering paint, and the plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU) and is contained in an amount of 10 to 85% by weight based on 100% by weight of the solid content of the glittering paint. The content of the scaly indium particles is preferably 25 to 60% by weight, and more preferably 30 to 50% by weight, based on 100% by weight of the solid content of the glittering coating material.

[0023] This glittering paint can ensure even greater glittering even when the amount of flaky indium particles blended is relatively small.

[0024] (Aspect 7) A glittering coating film comprising scaly indium particles and a plasticizer, wherein the scaly indium particles are contained in an amount of 20 to 70% by weight based on 100% by weight of the glittering coating film, and the plasticizer is an aliphatic dibasic acid ester and is contained in an amount of 10 to 85% by weight based on 100% by weight of the glittering coating film. Again, the content of the scaly indium particles is preferably 25 to 60% by weight, more preferably 30 to 50% by weight, based on 100% by weight of the solid content of the glittering paint.

[0025] This bright coating film can ensure sufficient brightness even if the content of the scaly indium particles is relatively low, ie, 20 to 70% by weight based on 100% by weight of the bright coating film. In addition, since the content of flaky indium particles is relatively small, the radio wave transmittance is also excellent.

[0026] (Embodiment 8) The glossy coating film according to embodiment 7, wherein the plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU).

[0027] This bright coating film can ensure even greater brightness even when the content of the scaly indium particles is relatively small.

[0028] (Embodiment 9) The glossy coating film according to embodiment 7 or 8, which does not contain a polymer as a binder resin. Here, "polymer" refers to one with a molecular weight of 10,000 or more. Furthermore, "not containing a polymer as a binder resin" means that it does not substantially contain a "polymer" as a binder resin, and is intended to exclude, for example, a "polymer" used as a surface treatment agent for scaly indium particles, which ends up being contained in the luster paint. For example, it means that 100% by weight of the paint solids does not contain 5% by weight or more of a polymer with a molecular weight of 10,000 or more.

[0029] This bright coating film can ensure even greater brightness even when the content of the scaly indium particles is relatively small.

[0030] (Aspect 10) The glittering coating film according to any one of Aspects 7 to 9, further comprising a dispersant. The content of the dispersant is preferably 5 to 30% by weight, more preferably 10 to 25% by weight, and most preferably 15 to 20% by weight, based on 100% by weight of the glittering coating film.

[0031] This bright coating film has high dispersibility of the flaky indium particles.

[0032] (Aspect 11) The glossy coating film according to any one of Aspects 7 to 10, wherein the plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU), and the coating film further comprises a dispersant.

[0033] This bright coating film can ensure even greater brightness even when the content of the scaly indium particles is relatively small.

[0034] (Embodiment 12) A glittering coating film comprising scaly indium particles, a plasticizer, and a dispersant, wherein the scaly indium particles are contained in an amount of 20 to 70% by weight based on 100% by weight of the glittering coating film, and the plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU) and is contained in an amount of 10 to 85% by weight based on 100% by weight of the glittering coating film. Again, the content of the scaly indium particles is preferably 25 to 60% by weight, more preferably 30 to 50% by weight, based on 100% by weight of the solid content of the glittering paint.

[0035] This bright coating film can ensure even greater brightness even when the content of the scaly indium particles is relatively small. In addition, since the content of flaky indium particles is relatively small, the radio wave transmittance is also excellent.

[0036] (Aspect 13) A glossy laminate coating film comprising an undercoat coating film, a glossy coating film according to any one of aspects 7 to 12 formed on the undercoat coating film, and a topcoat coating film formed on the glossy coating film.

[0037] This glittering multilayer coating film can ensure sufficient glittering even if the content of the scaly indium particles in the glittering coating film is relatively low. In addition, since the content of flaky indium particles in the glittering coating is relatively small, the coating also has excellent radio wave transmittance.

[0038] (Embodiment 14) A coated article having the glittering laminate coating film according to embodiment 13.

[0039] This coating can ensure sufficient brilliance. Furthermore, the laminated coating film of the coated object has excellent radio wave transmittance. Effect of the Invention

[0040] According to the present invention, it is possible to provide a glittering paint, a glittering coating film, a glittering multilayer coating film and a coated article which are capable of ensuring glittering even when the blending amount of indium particles is relatively small. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] The following describes examples of the glittering paint, the glittering coating film, the glittering laminated coating film, and the coated article. The present invention is not limited to the following embodiments.

[0042] First, the glittering paint will be illustrated. The glittering paint is composed of scaly indium particles, a plasticizer, and a solvent. The glittering paint may contain a dispersant in addition to these materials. Each element will be illustrated below.

[0043] 1. Scaly indium particles The scaly indium particles are a material for imparting brilliance to a brilliance coating film obtained by applying a brilliance paint, etc. As the scaly indium particles, for example, flaky indium particles made of indium with a purity of 95% or more can be used.

[0044] The scaly indium particles have a generally flat surface and a generally uniform thickness in a direction perpendicular to the flat surface, and the thickness is very thin and the length of the flat surface (the length of the longest part) is very long. More specifically, the term "scaly" refers to an indium particle having a very large aspect ratio (average particle size / thickness), for example, an aspect ratio of 2 to 1,000. Here, the average particle size refers to the 50% particle size (D50%) measured by a laser diffraction scattering method.

[0045] The thickness of the scaly indium particles is preferably 0.005 to 2 μm, more preferably 0.01 to 0.1 μm. Scaly indium particles having a thickness of 0.005 μm or more increase the gloss of the coating film. On the other hand, if the thickness of the scaly indium particles is 2 μm or less, the appearance of the coating film can be maintained good. In particular, if the thickness of the scaly indium particles is 0.1 μm or less, a coating film with a more metallic tone can be easily obtained. The thickness of the scaly indium particles is measured using an electron microscope.

[0046] The average particle size of the scaly indium particles is preferably 0.01 to 10 μm, more preferably 0.01 to 2 μm. If the average particle size of the scaly indium particles is 0.01 μm or more, it is easy to obtain scaly indium particles having a thickness of 0.01 μm or less. On the other hand, if the average particle size of the scaly indium particles is 10 μm or less, it is easy to obtain a smooth metallic coating film.

[0047] The scaly indium particles may be used in the form of a liquid or paste dispersed in a solvent such as an organic solvent. The surfaces of the scaly indium particles may be treated with a surface treatment agent such as a fatty acid or a silane coupling agent, or may be coated with a transparent resin.

[0048] Examples of the scaly indium particles include those obtained by pulverizing a vapor-deposited indium thin film obtained by vapor deposition or a rolled indium thin film obtained by rolling into a scaly shape, etc. Among these, those obtained by pulverizing a vapor-deposited indium thin film are preferred in that a coating film having a more metallic tone can be easily obtained. The evaporated indium thin film can be obtained, for example, by evaporating indium onto a substrate film such as polyethylene terephthalate to form an evaporated indium thin film on the substrate film, and then peeling the formed evaporated indium thin film from the substrate film. The evaporated indium thin film can be pulverized into amorphous particles to form flaky indium particles. As the thus obtained scaly indium particles, for example, Leaf Powder (registered trademark) manufactured by Oike Kogyo Co., Ltd. is commercially available.

[0049] The scaly indium particles (leaf powder manufactured by Oike Kogyo Co., Ltd.) are flaky indium particles made of indium with a purity of 95% or more, and are characterized in that in a volume-based particle size distribution showing the relationship between the particle size of the indium particles and the volume fraction of the indium particles in the particle size, the flaky indium particles have a first peak and a second peak having a particle size larger than the first peak, the volume V1 of the indium particles at the first peak and the volume V2 of the indium particles at the second peak satisfy the following formula, (V1 / V2) × 100 ≧ 25%, the particle size P1 of the indium particles at the first peak and the particle size P2 of the indium particles at the second peak satisfy the following formula, 6.0 ≦ P2 / P1 ≦ 12, and the cumulative 50% volume particle size D50 of the indium particles is 0.70 μm or less.

[0050] 2. Plasticizers Next, an example of the plasticizer will be described. In the glittering paint, an aliphatic dibasic acid ester is used as the plasticizer.

[0051] (1) Aliphatic dibasic acid esters The aliphatic dibasic acid ester can be obtained by esterifying an aliphatic dibasic acid such as adipic acid, azelaic acid, maleic acid, or sebacic acid with an alcohol. Examples of aliphatic dibasic acid esters include dibutyl adipate (DBA), diisobutyl adipate (DIBA), di-2-ethylhexyl adipate (DOA), diisononyl adipate (DINA), diisodecyl adipate (DIDA), bis-2-ethylhexyl azelaate (DOZ), dibutyl sebacate (DBS), di-2-ethylhexyl sebacate (DOS), diisononyl sebacate (DINS), dioctyl maleate (DOM), and diethyl succinate (DESU).

[0052] Among these aliphatic dibasic acid esters, dioctyl maleate (DOM) and diethyl succinate (DESU) are preferred in terms of brilliance. The mechanism by which the brilliance is improved by the combination of dioctyl maleate (DOM) and diethyl succinate (DESU) is unclear, but it is hypothesized that this is related to the symmetrical structure of the molecules. For example, it is thought that the orientation of the scaly indium particles is improved due to molecular symmetry.

[0053] 3. Dispersants Next, an example of a dispersant will be described. A dispersant is an optional component in a glittering paint. However, in order to suppress the aggregation of the scaly indium particles and to maintain the particles stably dispersed in the glittering paint, it is preferable to add a dispersant.

[0054] In the glittering paint, any dispersant can be used as long as it can stably disperse the scaly indium particles. However, it is not preferable to add a large amount of a dispersant with a high molecular weight (e.g., a molecular weight exceeding 10,000) in terms of glittering.

[0055] In general, examples of dispersants include alkyl ether sulfates such as ammonium polyoxyethylene styrenated phenyl ether sulfate, sodium polyoxyalkylene decyl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, ammonium polyoxyethylene isodecyl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, ammonium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene alkyl ether sulfate, ammonium polyoxyethylene oleyl cetyl ether sulfate, and sodium polyoxyethylene oleyl cetyl ether sulfate, alkyl sulfate ester salts, alkyl benzene sulfonates, alkyl phthalene sulfonates, and polyoxyethylene alkyl ether sulfates. Known examples of such alkyl phosphate esters include alkyl ether phosphate esters, polyoxyethylene alkyl ether phosphate esters, polyoxyethylene lauryl ether phosphate esters, polyoxyethylene alkyl ether phosphates, polyoxyethylene tridecyl ether phosphate esters, and polyoxyethylene styrenated phenyl ether phosphate esters; alkyl ether acetates, such as polyoxyethylene alkyl ether acetates and sodium polyoxyethylene lauryl ether acetate; and alkyl succinates, such as disodium lauryl sulfosuccinate, disodium polyoxyethylene alkyl sulfosuccinate, disodium polyoxyethylene lauryl sulfosuccinate, and polyoxyethylene alkyl sulfosuccinates.

[0056] Examples of commercially available dispersants that can be used include S-LEAM C-2091I (NOF Corporation), S-LEAM AD-374M (NOF Corporation), S-LEAM MP-071K (NOF Corporation), as well as S-LEAM SP-0201 (NOF Corporation), S-LEAM C20931 (NOF Corporation), S-LEAM 221P (NOF Corporation), S-LEAM AD-3172M (NOF Corporation), BYK-392 (BYK), DISPERBYK-2000 (BYK), DISPERBYK-2200 (BYK), and DISPERBYK-2155 (BYK).

[0057] 4. Solvent Next, examples of the solvent will be described below. The solvent is used to disperse the scaly indium particles and the plasticizer, and to adjust the viscosity of the glittering paint to optimize the applicability.

[0058] The solvent can be appropriately selected in consideration of the compatibility with the plasticizer used in the glittering paint, the dispersibility of the flaky indium particles, the drying temperature, the drying time, etc. The solvent includes organic solvents as well as water. When forming a glittering coating film on various plastic housings, it is desirable to select a solvent so that the glittering paint dries at a drying temperature of about 80±5° C. and within one hour, preferably within 30 minutes.

[0059] Examples of the organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, ester-based solvents, glycol ether-based solvents, phenol-based solvents, aliphatic or aromatic hydrocarbon-based solvents, aliphatic or aromatic chlorinated hydrocarbon-based solvents, sulfur-containing compound-based solvents, nitrogen-containing compound-based solvents, etc. These may be used alone or in combination of two or more.

[0060] 5. Glitter paint Next, the glittering paint will be described by way of example. The glittering paint is obtained by blending and mixing predetermined amounts of scaly indium particles, a plasticizer, and a solvent. In addition to these materials, a dispersant, an additive, etc. may be added.

[0061] [Scaly indium particles] The scaly indium particles are blended in an amount of 20 to 70% by weight based on 100% by weight of the solid content of the glittering paint.The scaly indium particles are blended in an amount of preferably 25 to 60% by weight, more preferably 30 to 55% by weight, and most preferably 30 to 50% by weight based on 100% by weight of the solid content of the glittering paint.

[0062] [Plasticizer] The aliphatic dibasic acid ester as a plasticizer is blended so as to be 10 to 85% by weight (solid content) in the 100% by weight solid content of the glittering paint. The aliphatic dibasic acid ester as a plasticizer is blended so as to be preferably 15 to 80% by weight (solid content) in the 100% by weight solid content of the glittering paint. To explain the amount of plasticizer in more detail, when a dispersant described below is not used, the amount of plasticizer is preferably 25 to 80% by weight, more preferably 30 to 75% by weight, and most preferably 33 to 72% by weight, based on 100% by weight of the solids content of the paint. On the other hand, when a dispersant described later is blended, the amount of plasticizer blended is preferably 15 to 60% by weight, more preferably 20 to 55% by weight, and most preferably 25 to 50% by weight, based on 100% by weight of the solid content of the paint.

[0063] [Dispersant] The dispersant is an optional component. When a dispersant is blended, it is blended preferably in an amount of 30% by weight or less, more preferably 25% by weight or less, based on 100% by weight of the solid content of the glittering paint. When a dispersant is blended, the lower limit of the blending amount is not particularly limited, but it can be 10% by weight or more or 15% by weight or more, based on 100% by weight of the solid content of the glittering paint.

[0064] [solvent] The solvent is blended, for example, so that the glossy paint has a viscosity that allows the desired coatability to be obtained. Note that the coatability may vary depending on the type of solvent.

[0065] [others] The glittering paint may also contain small amounts of various additives. It is preferable that the luster paint does not contain a polymer as a binder resin. "Polymer" refers to a material with a molecular weight of 10,000 or more. Furthermore, "does not contain a polymer as a binder resin" means that the material does not substantially contain a "polymer" as a binder resin, and is intended to exclude, for example, a material in which a "polymer" is used as a surface treatment agent for scaly indium particles, resulting in the luster paint containing a "polymer." For example, it means that the luster paint does not contain 5% by weight or more of a polymer with a molecular weight of 10,000 or more in 100% by weight of the paint solids.

[0066] 6. Bright coating film Next, the glossy coating film will be illustrated. The glossy coating film is obtained by applying the above-mentioned glossy paint to the surface of the object to be coated and drying (volatilizing the solvent). The glossy coating film is composed of scaly indium particles and a plasticizer. In addition to these materials, the glossy coating film may also contain a dispersant, etc. When forming a glossy coating film on various plastic housings, the coating is dried or cured at a temperature of about 80±5° C. for within one hour.

[0067] 7.Glitter laminated coating film Next, the glittering multilayer coating film will be illustrated. The glittering multilayer coating film is composed of an undercoat coating film, the glittering coating film formed on the undercoat coating film, and a topcoat coating film formed on the glittering coating film.

[0068] [Undercoat] The undercoat coating film is a coating film formed on the surface of a substrate, and is usually obtained by applying an undercoat paint to the substrate and drying it. There are no particular limitations on the undercoat coating film, so long as it ensures adhesion to the substrate, has a certain degree of surface smoothness, and provides good applicability of the glittering paint.

[0069] As the undercoat paint, for example, a two-liquid type clear paint can be used. Considering the formation of a laminated coating film on various plastic housings, it is preferable to use an undercoat paint that dries or hardens at a drying temperature of about 80±5°C and within one hour. The applied film thickness of the undercoat paint is preferably 10 to 35 μm, more preferably 20 to 25 μm, depending on the solid content of the undercoat paint.

[0070] [Glitter coating film] The above-mentioned glittering paint is applied on the undercoat and dried to form the glittering paint film. The glittering paint and the glittering paint film are as described above, and therefore a detailed description thereof will be omitted. The infrared absorptivity of the glittering paint is preferably 30 to 80%, more preferably 45 to 75%, depending on the solid content of the glittering paint. Since the thickness of the glittering paint is 1 μm or less, an electromagnetic film thickness gauge cannot be used. As a result of various investigations, it was found that the infrared absorptivity is proportional to the film thickness of the glittering paint, and the above-mentioned quantification was carried out. The infrared absorptivity was measured using an optical transmittance measuring instrument DST-2501 manufactured by Toa System Create Co., Ltd. As a measurement sample, a transparent acrylic resin plate was used, and the glittering paint was applied to it and dried to form a glittering paint film, and the infrared absorptivity was measured. The glittering paint was applied with a spray gun.

[0071] [Topcoat] The topcoat coating film is a coating film formed on the surface of the glittering coating film, and is usually obtained by applying a topcoat paint to the glittering coating film and drying it. There are no particular limitations on the topcoat coating film as long as it has adhesion to the glittering coating film and has a certain degree of surface smoothness.

[0072] As the topcoat paint, for example, a two-liquid type clear paint can be used. Considering the formation of a laminated coating film on various plastic housings, it is preferable to use a topcoat paint that dries or hardens at a drying temperature of about 80±5°C and within one hour. The applied film thickness of the topcoat paint is preferably 8 to 32 μm, more preferably 18 to 22 μm, depending on the solid content of the topcoat paint. 8.Painted items

[0073] Finally, a coated article will be described by way of example. A coated article is an article in which the multilayer coating film is formed on a part or the whole of an object to be coated. The area on which the multilayer coating film is formed has high luster.

[0074] The object to be coated on which the multilayer coating film is formed is not particularly limited, and examples thereof include the exterior and interior parts of automobiles, automobile parts such as bumpers and front grilles, exterior parts of electrical products such as mobile phones and information terminal devices, housing parts such as makeup palettes and cosmetic palettes, and fishing tackle such as reels and lures.

[0075] The material of these objects to be coated is not particularly limited, but examples thereof include various metal materials such as iron and aluminum, various resin materials such as ABS resin and polyethylene resin, various plastic materials such as FRP, various inorganic materials such as glass and cement, and various fibrous materials such as paper and cloth. EXAMPLES

[0076] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. In the examples, the ratios and the like are based on weight.

[0077] Example 1 A glittering paint was prepared based on the recipe of Example 1 in Table 1 below. In Table 1, the figures in parentheses for the amounts of indium, plasticizer, and dispersant used are the amounts of solids. In Tables 1 and 2, the scaly indium particle content (wt %) is the content (wt %) of scaly indium particles in 100 wt % of the solid content of the luster paint, and is generally referred to as pigment weight concentration (PWC). Also, the plasticizer content (wt %) is the content (wt %) of the plasticizer solid content in 100 wt % of the paint solid content of the luster paint.

[0078] First, a scaly indium particle solution (Oike Kogyo Co., Ltd., "Product No.: Leaf Powder 49CJ-1120") was mixed as scaly indium, and dioctyl maleate (Daihachi Chemical Industry Co., Ltd., "Product No.: DOM"), an aliphatic dibasic acid ester, was mixed as a plasticizer, and thinner No. 5600 (Ohashi Chemical Industry Co., Ltd.) was further mixed as a solvent (diluent). After that, the mixture was thoroughly stirred until it was homogenous, and the glittering paint of Example 1 was obtained. Incidentally, 100% by weight of the flaky indium particle solution contains 20% by weight of flaky indium particles. In addition, in order to ensure accuracy in blending, the plasticizer and dispersant described below are blended in the form of a solution (10% solids) diluted 10 times with thinner No. 5600.

[0079] Then, a primer paint was applied onto the ABS resin plate, which was the object to be painted, and then dried to form a primer coating film. On top of that, the glossy paint of Example 1 was applied and dried to form a glossy coating film. The undercoat paint used was Fine Finish (NXT) Undercoat Clear (manufactured by Ohashi Chemical Industry Co., Ltd.) mixed with hardener IP-60 (manufactured by Ohashi Chemical Industry Co., Ltd.) and thinner No. 6820 (manufactured by Ohashi Chemical Industry Co., Ltd.) in a weight ratio of 60:10:48. This was applied to an ABS resin plate (film thickness 20 to 25 μm) and dried at 80°C for 30 minutes to obtain an undercoat coating film. A glittering paint was applied onto the obtained undercoat film, and dried at 80°C for 30 minutes to obtain a glittering coating film. The infrared absorptivity of the glittering coating film was 45 to 75%.

[0080] Finally, a topcoat paint was applied on the obtained glossy coating film, and then dried to form a topcoat coating film, obtaining a glossy laminated coating film. As the topcoat paint, Fine Finish (NXT) topcoat clear (manufactured by Ohashi Chemical Industry Co., Ltd.) was mixed with hardener IP-60 (manufactured by Ohashi Chemical Industry Co., Ltd.) and thinner No. 6820 (manufactured by Ohashi Chemical Industry Co., Ltd.) in a weight ratio of 80:10:88, and this was applied on the glossy coating film (film thickness 18 to 22 μm), and dried at 80°C for 30 minutes to obtain a topcoat coating film. As a result, a glittering multi-layer coating film consisting of the undercoat coating film, the glittering coating film and the topcoat coating film was obtained.

[0081] The resulting multilayer coating film was evaluated for gloss value, L value, and adhesion, as well as for the appearance of the coating film.

[0082] The gloss value was measured according to JIS Z8741-1997 Specular Gloss Measurement Method. The measurement was performed at angles of 20°, 60°, and 85° using a MULTI GLOSS 268 Plus made by Konica Minolta, Inc. A value of 700 or more at a measurement angle of 20° was rated as ○.

[0083] The L value was measured using a spectrophotometer CM-600d manufactured by Konica Minolta, Inc. A measured value of 60 or more was evaluated as ○.

[0084] Adhesion was evaluated using the so-called cross-cut tape peel test (JIS K5600-2014), and those that did not peel were rated as ○. The appearance of the coating film was rated as a reference only, since it may be affected by the application conditions, but those that did not receive a good rating for appearance were rated as △, even if other ratings were good.

[0085] The multilayer coating film using the glittering paint of Example 1 achieved very good evaluation results.

[0086] [Table 1]

[0087] (Example 2) (Example 3) This is an example in which the blending amount of dioctyl maleate as a plasticizer is increased based on the blending amount of Example 1.

[0088] The multilayer coating films using the glittering paints of Examples 2 and 3 both achieved very good evaluation results.

[0089] (Example 4) (Example 5) (Example 6) This example is based on the formulation of Example 1, but the plasticizer was changed from dioctyl maleate to diethyl succinate (Daihachi Chemical Industry Co., Ltd., "Product No.: DESU"), which is also an aliphatic dibasic acid ester, and the amount of the plasticizer mixed was varied.

[0090] The multilayer coating films using the glittering paints of Examples 4, 5 and 6 all achieved very good evaluation results.

[0091] (Comparative Example 1) (Comparative Example 2) (Comparative Example 3) This example is based on the formulation of Example 1, but the plasticizer was changed from dioctyl maleate, an aliphatic dibasic acid ester, to an adipic acid-based polyester (DIC Corporation, product number: W-2340-S), and the amount of plasticizer added was varied.

[0092] The multilayer coating films using the glittering paints of Comparative Examples 1, 2 and 3 did not give very good evaluation results.

[0093] (Comparative Example 4) to (Comparative Example 12) These are comparative examples in which various dispersants were added in place of the plasticizer and the amounts added were varied based on the formulation of Example 1. The dispersants used were S-ream C-2091I (NOF Corporation), S-ream MP-071K (NOF Corporation), and S-ream AD-374M (NOF Corporation).

[0094] Of Comparative Examples 4 to 12, the multilayer coating film using the glitter paint of Comparative Example 7 was relatively good in terms of gloss value and L value, but the system containing only a dispersant did not receive a very good evaluation compared to the system containing a plasticizer.

[0095] Comparative Example 13 This is a comparative example in which neither a plasticizer nor a dispersant was added.

[0096] The multi-layer coating film using the glittering paint of Comparative Example 13 also did not give very good evaluation results.

[0097] From the above, it was found that the evaluation results of the system containing the aliphatic dibasic acid esters dioctyl maleate (DOM) or diethyl succinate (DESU) as a plasticizer were good.

[0098] Next, a dispersant was added to the plasticizer-based system to carry out prototype evaluation. The recipe and evaluation results are shown in Table 2.

[0099] [Table 2]

[0100] Example 7 This system is based on the formulation of Example 1, but with the addition of a dispersant.

[0101] Although the multilayer coating film using the glossy paint of Example 1, which did not contain a dispersant, showed better results, the multilayer coating film using the glossy paint of Example 7 also showed very good evaluation results.

[0102] Example 8 This is a system based on the formulation of Example 7, with the amount of plasticizer increased.

[0103] The multilayer coating film using the glittering paint of Example 8 also showed very good evaluation results.

[0104] (Example 9) (Example 10) (Example 11) Based on the formulation of Example 7, this system has been modified by changing the type and amount of dispersant used.

[0105] The multilayer coating films using the glittering paints of Examples 9, 10, and 11 all showed favorable evaluation results.

[0106] (Example 12) to (Example 17) Based on the formulations of Examples 7 to 11, this is an example in which the plasticizer was changed from dioctyl maleate to diethyl succinate (Daihachi Chemical Industry Co., Ltd., "Product No.: DESU"), which is also an aliphatic dibasic acid ester.

[0107] The multilayer coating films using the glittering coating materials of Examples 12 to 17 also showed good evaluation results.

[0108] (Comparative Example 14) to (Comparative Example 18) Based on the formulations of Examples 7 to 11, the plasticizer was changed from dioctyl maleate, an aliphatic dibasic acid ester, to an adipic acid polyester (DIC Corporation, Product No. W-2340-S).

[0109] The multilayer coating films using Comparative Examples 14 to 18, which are systems in which an adipic acid-based polyester was blended as a plasticizer, did not generally give very good evaluation results.

[0110] In addition, preliminary studies have shown that photoluminescent paints containing materials with large molecular weights are prone to cloudiness and reduced color development through verification experiments in which polymers are added.

[0111] Furthermore, when the radio wave transmittance (attenuation and transmittance in the 24 GHz band and the 78 GHz band) of the laminated coating film of each Example was confirmed, good results were obtained in all cases.

[0112] The present invention has been described above with reference to specific embodiments and examples, but the present invention is not limited to the above-mentioned embodiments, and various changes and modifications can be made by those skilled in the art without departing from the scope of the claims attached to the application of this application.

Claims

1. Scaly indium particles; A plasticizer; A glittering paint comprising a solvent, The scaly indium particles are The glittering paint contains 20 to 70% by weight of the solid content of the glittering paint (100% by weight), The plasticizer is An aliphatic dibasic acid ester, which is contained in an amount of 30 to 80% by weight based on 100% by weight of the solid content of the glittering paint; Bright paint.

2. Scaly indium particles; A plasticizer; A dispersant; A glittering paint comprising a solvent, The scaly indium particles are The content of the luster paint is 30 to 55% by weight based on 100% by weight of the solid content of the luster paint, The plasticizer is The aliphatic dibasic acid ester is contained in an amount of 20 to 55% by weight based on 100% by weight of the solid content of the glittering paint, The dispersant is The content is 10 to 30% by weight based on 100% by weight of the solid content of the glittering paint. Bright paint.

3. The plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU); The glittering paint according to claim 1.

4. The plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU); The glittering paint according to claim 2.

5. Scaly indium particles; A glittering coating film comprising a plasticizer, The scaly indium particles are The glittering coating film contains 20 to 70% by weight of the glittering coating film (100% by weight), The plasticizer is an aliphatic dibasic acid ester, the content of which is 30 to 80% by weight in 100% by weight of the glittering coating film; Bright coating film.

6. Scaly indium particles and A plasticizer; A dispersant; A glittering coating film consisting of The scaly indium particles are The content of the luster coating film is 30 to 55% by weight based on 100% by weight of the luster coating film, The plasticizer is an aliphatic dibasic acid ester, the content of which is 20 to 55% by weight per 100% by weight of the glittering coating film; The dispersant is The glittering coating film is contained in an amount of 10 to 30% by weight based on 100% by weight of the glittering coating film. Bright coating film.

7. The plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU); The glittering coating film according to claim 5.

8. The plasticizer is dioctyl maleate (DOM) or diethyl succinate (DESU); The glittering coating film according to claim 6.

9. A primer coating and The glossy coating film according to any one of claims 5 to 8 formed on the undercoat coating film; A topcoat coating film formed on the glossy coating film; A glossy multilayer coating film having the above properties.

10. A coated object having the photoluminescent laminate coating film described in claim 9.

Citation Information

Patent Citations

  • Painted object, method of manufacturing painted object, and paint set

    JP7146311B1

  • JPP7146311B

  • JPP7406176B