Manufacturing method of CO2 immobilization material and CO2 immobilization product

The method addresses the inefficiencies in existing carbon dioxide immobilization methods by using specific mineral compounds and disaccharides to promote carbonation at controlled temperatures and humidity, achieving high carbonation rates and reducing emissions.

JP7569777B2Active Publication Date: 2024-10-18DENKA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021171812
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-10-18
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

Existing methods for immobilizing carbon dioxide in concrete do not provide effective conditions for carbonation treatment, particularly with moisture content set at 1.5% or more and temperature at 75 to 175°C, lacking disclosure on suitable materials and conditions.

Method used

A method using γ-2CaO·SiO2, 3CaO·2SiO2, α-CaO·SiO2, and non-hydraulic compounds like calcium magnesium silicate, with Li content of 0.001 to 1.0% by mass, and disaccharides like trehalose, promotes carbonation at temperatures below 75°C and humidity above 50%RH, forming vaterite and enhancing carbonation.

Benefits of technology

The method effectively immobilizes carbon dioxide in concrete, achieving high carbonation rates and reducing greenhouse gas emissions by utilizing industrial by-products and disaccharides to enhance carbonation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569777000001
    Figure 0007569777000001
  • Figure 0007569777000002
    Figure 0007569777000002
  • Figure 0007569777000003
    Figure 0007569777000003
Patent Text Reader

Abstract

To provide a CO2 immobilization material capable of immobilizing CO2 by carbonation and a method for producing a CO2 immobilization material.SOLUTION: Provided is a CO2 immobilization material comprising one or more non-hydraulic compounds selected from the group consisting of γ-2CaO SiO2, 3CaO 2SiO2, α-CaO SiO2 and calcium magnesium silicate. The CO2 immobilization material comprises Li. The Li content in the CO2 immobilization material is 0.001 to 1.0 mass% in terms of oxide. Also provided is a method for producing a CO2 immobilization product in which carbonization of the CO2 immobilization material is performed at 75°C or lower and / or 50% RH or greater.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a CO2 immobilization material and a method for producing a CO2 immobilized product. [Background technology]

[0002] As an effort to reduce greenhouse gas emissions, concrete products that forcibly absorb or carbonate CO2 during manufacturing (hereinafter referred to as CO2 absorption concrete) have been put into practical use in some areas. CO2 absorption concrete, a type of CCUS technology (short for Carbon dioxide Capture, Utilization and Storage), was also mentioned in the "Carbon Recycling Technology Roadmap" announced by the Ministry of Economy, Trade and Industry in 2019, and technological development is being carried out to expand its use.

[0003] Patent Document 1 discloses a method for forcibly absorbing or carbonating CO2 during the production of concrete. Specifically, the method includes a contacting step of contacting a carbon dioxide-containing gas with a cementitious hardened body to fix the carbon dioxide contained in the carbon dioxide-containing gas in the cementitious hardened body. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-15659 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the fixation method of Patent Document 1 sets the moisture content in the carbon dioxide-containing gas to 1.5% or more and the temperature to 75 to 175° C., and does not disclose or suggest any material that can fix CO2.

[0006] In view of the above, an object of the present invention is to provide a CO2 immobilization material capable of immobilizing CO2 by carbonation treatment and a method for producing a CO2 immobilized product. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have come up with the following invention and found that the above problems can be solved.

[0008] [1] A CO2 fixation material comprising one or more non-hydraulic compounds selected from the group consisting of γ-2CaO SiO2, 3CaO 2SiO2, α-CaO SiO2, and calcium magnesium silicate, wherein the CO2 fixation material contains Li, and the Li content is 0.001 to 1.0 mass% in terms of oxide. [2] A CO2 fixation material comprising one or more non-hydraulic compounds selected from the group consisting of γ-2CaO·SiO2, 3CaO·2SiO2, α-CaO·SiO2, and calcium magnesium silicate, and a disaccharide. [3] The CO2 immobilization material according to [1] or [2], wherein the CaO / SiO2 molar ratio in the non-hydraulic compound is 0.8 to 2.3. [4] The CO2 fixation material according to [1], further comprising a disaccharide. [5] The CO2 fixation material according to any one of [1], [2] and [4], containing 0.5 to 10 parts by mass of the disaccharide per 100 parts by mass of the CO2 fixation material. [6] The CO2 fixation material according to any one of [1], [2], [4], and [5], wherein the disaccharide contains trehalose. [7] A method for producing a CO2 immobilization material, comprising carbonation treatment of the CO2 immobilization material described in any one of [1] to [6] at 75°C or lower and / or 50% RH or higher. Effect of the Invention

[0009] According to the present invention, it is possible to provide a CO2 immobilization material capable of immobilizing CO2 by carbonation treatment and a method for producing a CO2 immobilized product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [CO2 fixation material] The CO2 fixation material according to the embodiment of the present invention includes a first CO2 fixation material and a second CO2 fixation material.

[0011] <The first CO2 fixation material> The first CO2 fixation material contains one or more non-hydraulic compounds selected from the group consisting of γ-2CaO·SiO2, 3CaO·2SiO2, α-CaO·SiO2, and calcium magnesium silicate. The first CO2 fixation material further contains Li, and the content of Li is 0.001 to 1.0% in terms of oxide. It is presumed that this predetermined amount of Li promotes the generation of vaterite, a type of calcium carbonate, during the carbonation of CSH (calcium silicate hydrate), and it is considered that a denser hardened state can be easily obtained by carbonation (salt) curing.

[0012] Here, "Li is contained in the CO2 fixation material" refers to a state in which the non-hydraulic compounds in the CO2 fixation material contain Li2O as a chemical composition (their presence can be confirmed by ICP atomic emission spectroscopy), but Li2O is not identified by X-ray diffraction measurement (no clear Li2O peak is seen), and it does not simply mean that the non-hydraulic compounds and Li compounds are physically mixed. This state can be obtained by mixing the respective raw materials and subjecting them to heat treatment at high temperatures of 1,000°C or higher. Each component will be explained below.

[0013] (γ-2CaO SiO2) γ-2CaO SiO2 is known as a low-temperature phase of the compound represented by 2CaO SiO2, and is completely different from the high-temperature phases α-2CaO SiO2, α'-2CaO SiO2, and β-2CaO SiO2. Although all of these are represented by 2CaO SiO2, they have different crystal structures and densities.

[0014] (3CaO 2SiO2) 3CaO·2SiO2 is a mineral called rankinite, which is a pseudowollastonite containing CaO. It is a chemically stable mineral with no hydration activity, but has a large CO2 fixation effect.

[0015] (α-CaO SiO2) α-CaO·SiO2 (α-type wollastonite) is known as a high-temperature phase among the compounds expressed as CaO·SiO2, and is completely different from the low-temperature phase β-CaO·SiO2. Although both are expressed as CaO·SiO2, they have different crystal structures and densities.

[0016] Naturally occurring wollastonite is a low-temperature phase of β-CaO SiO2. β-CaO SiO2 has needle-shaped crystals and is used as an inorganic fibrous material such as wollastonite fiber, but it does not have the CO2 fixation effect of α-CaO SiO2 in this embodiment.

[0017] (Calcium Magnesium Silicate) Calcium magnesium silicate is a general term for CaO-MgO-SiO2 compounds, but in this embodiment, merwinite represented by 3CaO·MgO·2SiO2 (C3MS2) is preferred, as merwinite can achieve a large CO2 fixation effect.

[0018] The non-hydraulic compound may be one or more kinds, but the Li content in the non-hydraulic compound (the total when there are multiple kinds) is 0.001 to 1.0% in oxide conversion, preferably 0.005 to 1.0%, more preferably 0.010 to 0.90%, and even more preferably 0.015 to 0.80%. If the Li content is less than 0.001% in oxide conversion, the carbonation promotion effect cannot be obtained. If it exceeds 1.0%, the cost becomes high. The Li content in oxide conversion can be measured by the method described in the Examples.

[0019] Among the non-hydraulic compounds listed above, γ-2CaO·SiO2 is particularly preferable because it requires less energy to grind than other compounds due to the powdering phenomenon known as dusting that occurs during production, and because it has a large long-term CO2 fixation effect.

[0020] The non-hydraulic compound according to the present embodiment is obtained by blending a CaO raw material, a SiO2 raw material, a MgO raw material, and a Li raw material in a predetermined molar ratio and heat treating them. Examples of the CaO raw material include calcium carbonate such as limestone, calcium hydroxide such as slaked lime, by-product slaked lime such as acetylene by-product slaked lime, fine powder generated from waste concrete blocks, concrete sludge (dehydrated cake) generated in ready-mixed concrete plants and concrete product plants, incineration ash (coal ash, woody biomass, urban waste incineration ash, sewage sludge incineration ash, etc.), steel slag (converter slag, electric furnace slag, etc.), etc. Examples of the SiO2 raw material include silica stone, clay, and various siliceous dusts generated as industrial by-products such as silica fume and fly ash. Examples of the MgO raw material include magnesium hydroxide, basic calcium carbonate, dolomite, etc. Also, examples of the Li raw material include lithium carbonate, etc. In addition, if the CaO raw material, SiO2 raw material, and MgO raw material contain Li, there is no need to add a new Li raw material. In order to reduce non-energy-derived CO2 emissions during heat treatment, one or more types of industrial by-products containing CaO, such as by-product slaked lime, fine powder generated from waste concrete blocks, concrete sludge, municipal waste incineration ash, and sewage sludge incineration ash, can be used. Among these, the use of by-product slaked lime, which contains fewer impurities than other industrial by-products, is even more preferable.

[0021] Examples of by-product slaked lime include acetylene by-product slaked lime such as by-product slaked lime (wet type and dry type depending on the acetylene gas production method) produced in the acetylene gas production process by the calcium carbide method, and by-product slaked lime contained in the dust captured in the wet dust collection process of a calcium carbide electric furnace. By-product slaked lime contains, for example, 65 to 95% (preferably 70 to 90%) calcium hydroxide, 1 to 10% calcium carbonate, and 0.1 to 6.0% (preferably 0.1 to 3.0%) iron oxide. These ratios can be confirmed by fluorescent X-ray measurement and mass loss (Ca(OH)2: around 405°C to 515°C, CaCO3: around 650°C to 765°C) determined by differential thermogravimetry (TG-DTA). The volume average particle diameter measured by laser diffraction / scattering method is about 50 to 100 μm. Furthermore, the moisture content measured by the loss on drying method in JIS K 0068 "Method for measuring moisture content of chemical products" is preferably 10% or less. In addition, sulfur compounds such as CaS, A12S3, and CaC2·CaS may be contained, but the content is preferably 2% or less.

[0022] The heat treatment at a high temperature of 1,000° C. or higher is not particularly limited, but can be carried out, for example, by using a rotary kiln, an electric furnace, etc. The heat treatment temperature is not uniquely determined, but is usually carried out in the range of about 1,000 to 1,800° C., and often in the range of about 1,200 to 1,600° C.

[0023] In this embodiment, the above-mentioned industrial by-products containing non-hydraulic compounds can also be used. In this case, impurities coexist. Examples of such industrial by-products include steel slag.

[0024] The CaO raw material, SiO2 raw material, and MgO raw material may contain impurities, but this is not a problem as long as the effects of the present invention are not hindered. Specific examples of impurities include Al2O3, Fe2O3, TiO2, MnO, Na2O, K2O, S, P2O5, F, B2O3, and chlorine. Coexisting compounds include free calcium oxide, calcium hydroxide, calcium aluminate, calcium aluminosilicate, calcium ferrite, calcium aluminoferrite, calcium phosphate, calcium borate, magnesium silicate, leucite (K2O, Na2O)·Al2O3·SiO2, spinel MgO·Al2O3, magnetite Fe3O4, and sulfur compounds such as CaS, A12S3, and CaC2·CaS.

[0025] Of these impurities, the content of S (sulfur) in the non-hydraulic compound is preferably 1.0% or less, more preferably 0.7% or less, and even more preferably 0.5% or less, calculated as oxide (SO3). A content of 1.0% or less provides a sufficient carbonation (salt) promotion effect, and also allows the setting and hardening properties to be within an appropriate range. The content of S calculated as oxide (SO3) can be measured by fluorescent X-ray measurement. Note that S (sulfur) may be present in the non-hydraulic compound at about 2% calculated as oxide.

[0026] In this fixing material, the content of non-hydraulic compounds (the content in the total amount when multiple types are included) is preferably 65% ​​or more, more preferably 70% or more, and even more preferably 75% or more. Note that hydraulic 2CaO·SiO2 other than γ-2CaO·SiO2 can be mixed in, up to a maximum of 35%.

[0027] The content of γ-2CaO·SiO2 in the non-hydraulic compound is preferably 35% or more, more preferably 45% or more. The upper limit of the content of γ-2CaO·SiO2 is not particularly limited. Among steelmaking slags, electric furnace reduction slag or stainless steel slag, which has a high content of γ-2CaO·SiO2, is preferable.

[0028] The CaO / SiO2 molar ratio in the non-hydraulic compound is preferably 0.8 to 2.3, and more preferably 1.2 to 2.3. The molar ratio of 0.8 to 2.3 can further promote carbonation.

[0029] In addition, in order to make the effect of the immobilization material more easily manifest, it is preferable that the chemical components of the immobilization material contain 0.001 to 1.0 part of Li2O, 45 to 70 parts of CaO, 30 to 55 parts of SiO2, and 0 to 10 parts of Al2O3 per 100 parts of the CO2 immobilization material. The content of Li2O can be measured by the method described in the examples below. The contents of CaO, SiO2, and Al2O3 can be measured by fluorescent X-rays. As chemical components, it is more preferable that the CO2 fixation material contains 0.002 to 0.5 parts of Li2O, 60 to 70 parts of CaO, 30 to 45 parts of SiO2, and 0.5 to 5 parts of Al2O3 per 100 parts of the CO2 fixation material. Furthermore, as chemical components, the total amount of Li2O, CaO, SiO2, and Al2O3 is preferably 90 parts or more, and more preferably 95 to 100 parts, in 100 parts of the CO2 fixation material.

[0030] The amount of non-hydraulic compounds in the immobilizing material can be determined by the Rietveld method using powder X-ray diffraction.

[0031] The water content of the CO2 fixation material is preferably 10% by mass or less, and more preferably 0.01 to 10% by mass, in order to maintain an appropriate level of contact between the surface of the non-hydraulic compound and the carbon dioxide-containing gas. This can be calculated from the difference in mass between the sample before drying and the mass after drying by heating at 105°C. The moisture content of the CO2 fixation material can be adjusted by adding an appropriate amount of water and stirring after drying by heating at 105°C.

[0032] The average particle size of the CO2 fixation material is preferably 1 to 100 μm, and more preferably 1 to 70 μm. By setting the average particle size to 1 to 70 μm, it is possible to promote the dissolution of Ca into the water on the particle surface and promote the carbonation reaction. The average particle size can be determined by measuring with a laser diffraction / scattering type particle size distribution measuring device.

[0033] In addition, the Blaine specific surface area of ​​the CO2 fixation material (especially when γ-2CaO·SiO2 is used) is 1,000 to 10,000 cm 2 / g, and 2,500 to 10,000 cm 2 / g. It is more preferable that the specific surface area is 2,500 to 10,000 cm 2 / g, the contact area between the particles and the water on the particle surface increases, promoting the dissolution of Ca and accelerating the carbonation reaction. The specific surface area can be determined by measurement using a Blaine air permeation device described in JIS R 5201.

[0034] The CO2 fixation material preferably further contains a disaccharide such as trehalose, maltose, or sucrose to form a chelate with Ca dissolved in the water on the particle surface and promote further dissolution. Among them, it is more preferable to contain trehalose, which has a high effect of promoting the carbonation reaction.

[0035] From the viewpoint of the carbonation reaction acceleration effect, the disaccharide is preferably contained in an amount of 0.5 to 10 parts by mass, more preferably 5 to 10 parts by mass, per 100 parts by mass of the non-hydraulic compound. In addition, the content of trehalose in the disaccharide is preferably 90% by mass or more, more preferably 95% by mass or more, in order to obtain a sufficient carbonation acceleration effect.

[0036] Here, the fixation of CO2 means that the material is carbonated and CO2 forms a carbonate compound with the material. Here, the carbonation rate can be calculated as the ratio of the CaO component in the CO2 fixation material to the theoretically fixed CO2 as follows.

[0037] Formula (1): Carbonation rate = (ΔM × 56.08) / (M × w CaO ×44.01) Here, ΔM: mass increase due to carbonation [g], M: mass of the CO2 fixation material before carbonation [g], w CaO : CaO in the CO2 fixation material before carbonation [wt%] In the above formula, the increase in mass due to carbonation refers to the mass obtained by subtracting the sample weight before carbonation from the sample weight after carbonation. CaO in the CO2 fixation material before carbonation can be measured by fluorescent X-ray analysis.

[0038] <The second CO2 fixation material> The second CO2 fixation material contains one or more non-hydraulic compounds selected from the group consisting of γ-2CaO·SiO2, 3CaO·2SiO2, α-CaO·SiO2, and calcium magnesium silicate, and a disaccharide.

[0039] Disaccharides such as trehalose, maltose, and sucrose form chelates with Ca dissolved in water from the surface of the CO2 immobilization material particles, promoting further dissolution, and therefore enhancing the effect of promoting the carbonation reaction. From the viewpoint of further enhancing the effect of promoting the carbonation reaction, it is preferable to include trehalose.

[0040] As described above, since the second CO2 fixation material contains disaccharides, CO2 can be fixed by carbonation treatment even if the CO2 fixation material does not contain a specified amount of Li, as in the first CO2 fixation material.

[0041] In addition, the second CO2 fixation material can adopt the configuration and preferred aspects of the first CO2 fixation material as appropriate, so long as it is essential that the second CO2 fixation material contains a non-hydraulic compound and a disaccharide.

[0042] [Method of manufacturing CO2 fixation] The method for producing a CO2 immobilization material according to the present invention is a method for carrying out a carbonation treatment of a CO2 immobilization material at 75°C or lower and / or 50% RH or higher. The method of carbonation treatment is not particularly limited, but examples include a method in which the treatment is performed by appropriately heating and / or humidifying (adding water) in a carbon dioxide-containing gas atmosphere to a temperature of 75°C or less and / or 50% RH or more.

[0043] The temperature in the carbonation treatment is preferably from 5 to 75° C., more preferably from 5 to 50° C. The relative humidity is preferably from 50 to 100% RH, more preferably from 90 to 100% RH.

[0044] The carbon dioxide-containing gas may be exhaust gas generated from a cement factory or a coal-fired power plant, exhaust gas generated during exhaust treatment in a paint factory, etc. The proportion of carbon dioxide in the carbon dioxide-containing gas is preferably 5% by volume or more, more preferably 10% by volume or more, and even more preferably 15% by volume or more. The carbon dioxide-containing gas may contain moisture (water vapor).

[0045] The CO2 immobilization material produced in the above manner can be used, for example, as a cement additive, or can be used as it is as a material for mortar or concrete aggregate, roadbed material, embankment material, backfill material, etc. In other words, not only can carbon dioxide in the atmosphere be effectively immobilized in the CO2 immobilization material, but it can also be effectively utilized as a concrete material. EXAMPLES

[0046] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. Note that the CO2 fixation material may be simply called the "fixation material."

[0047] [Experimental Example 1] CO2 fixation materials A to F were prepared as follows. CO2 fixation material A: γ-2CaO SiO2. First-grade reagent calcium carbonate and first-grade reagent silicon dioxide were mixed in a molar ratio of 2:1, and then first-grade reagent lithium carbonate was mixed in such a way that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,400°C for 2 hours and allowed to stand at room temperature until the Blaine specific surface area reached 4,000 cm. 2 / g of CO2 fixation material A was produced.

[0048] CO2 fixation material B: 3CaO 2SiO2. First-grade reagent calcium carbonate and first-grade reagent silicon dioxide were mixed in a molar ratio of 3:2, and then first-grade reagent lithium carbonate was mixed in such a way that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,400°C for 2 hours and allowed to stand at room temperature until the Blaine specific surface area reached 4,000 cm. 2 / g of CO2 fixation material B was produced.

[0049] CO2 fixation material C: α-CaO SiO2. First-grade reagent calcium carbonate and first-grade reagent silicon dioxide were mixed in a 1:1 molar ratio, and then first-grade reagent lithium carbonate was mixed in such a way that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,500°C for 2 hours and allowed to stand at room temperature until the Blaine specific surface area reached 4,000 cm. 2 / g of CO2 fixation material C was produced.

[0050] CO2 fixation material D: 3CaO·MgO·2SiO2. First-grade reagent calcium carbonate, first-grade reagent magnesium oxide, and first-grade reagent silicon dioxide were mixed in a molar ratio of 3:1:2, and then first-grade reagent lithium carbonate was mixed in such a way that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,400°C for 2 hours and allowed to stand at room temperature until the Blaine specific surface area reached 4,000 cm. 2 / g of CO2 fixation material D was produced.

[0051] CO2 fixation material E: γ-2CaO SiO2. Reagent grade calcium carbonate and reagent grade silicon dioxide were mixed in a molar ratio of 2:1, heat-treated at 1,400°C for 2 hours, and allowed to cool to room temperature until the Blaine specific surface area reached 4,000 cm. 2 / g γ-2CaO SiO2 was prepared.

[0052] CO2 fixation material F: Li2O+γ-2CaO SiO2. Reagent grade calcium carbonate and reagent grade silicon dioxide were mixed in a molar ratio of 2:1, heat-treated at 1,400°C for 2 hours, and allowed to cool to room temperature until the Blaine specific surface area was 4,000 cm 2 / g γ-2CaO SiO2 was prepared. In addition, first-grade reagent lithium carbonate was heat-treated at 1,400°C for 2 hours and then left to cool to room temperature to produce Li2O powder. Li2O powder (reagent grade lithium carbonate heat-treated at 1,400℃ for 2 hours) was mixed with γ-2CaO SiO2 so that the Li2O content was 0.1% (internal substitution), to prepare CO2 fixation material F. The oxide-equivalent Li content of each CO2 fixation material was measured using an ICP emission spectrometer (VISTA-PRO, Hitachi High-Tech Science Corporation). The absolute calibration curve method using a diluted ICP mixture (XSTC-22, SPEX Corporation) confirmed that the Li content was the same as the amount of the material. The measurement conditions were as follows: ·Li measurement wavelength: 670.783nm BG correction: Fitting curve method Standard solution for calibration curve: Dilute SPEX XSTC-22 ICP mixture and use Calibration range: 0-5mg / L (0mg / L, 0.1mg / L, 0.5mg / L, 1mg / (5-point calibration curve of 5 mg / L, 5 mg / L) Quantitative analysis using absolute calibration curve method

[0053] 25 g of each of the CO2 fixation materials A to F was placed in each plastic cup, and carbonation was carried out in a temperature and humidity controlled room under conditions of 20°C, 80% RH, and a carbon dioxide concentration of 20% by volume. After carbonation for each of the specified periods shown in Table 1, the mass of the sample was measured after drying at 105°C for 24 hours, and the carbonation rate was calculated from the change in mass before and after carbonation using the above-mentioned formula (1). The results are shown in Table 1.

[0054] [Table 1]

[0055] [Experimental Example 2] In the preparation of CO2 fixation materials A and C in Experiment 1, CO2 fixation materials A-1 to A-7 and CO2 fixation materials C-1 to C-7 were prepared in the same manner as in the preparation of CO2 fixation materials A and C in Experiment 1, except that reagent grade lithium carbonate was mixed so that the Li content in the mixture was 0.0005%, 0.002%, 0.006%, 0.1%, 0.15%, 0.8%, 0.9%, 1.0%, and 1.1% (each by internal substitution) in terms of oxide (Li2O). Each CO2 fixation material was evaluated in the same manner as in Experiment 1. The results are shown in Table 2.

[0056] [Table 2]

[0057] [Experimental Example 3] CO2 fixation materials G to I were prepared as follows. CO2 fixation material G: First-grade reagent calcium carbonate and first-grade reagent silicon dioxide were mixed at a CaO / SiO2 molar ratio of 1.2, and then first-grade reagent lithium carbonate was mixed so that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,400°C for 2 hours and allowed to cool to room temperature, resulting in a Blaine specific surface area of ​​4,000 cm. 2 / g of CO2 fixation material G was produced.

[0058] CO2 fixation material H: First-grade reagent calcium carbonate and first-grade reagent silicon dioxide were mixed at a CaO / SiO2 molar ratio of 1.8, and then first-grade reagent lithium carbonate was mixed so that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,400°C for 2 hours and allowed to cool to room temperature, resulting in a Blaine specific surface area of ​​4,000 cm. 2 / g of CO2 fixation material H was produced.

[0059] CO2 fixation material I: First-grade reagent calcium carbonate and first-grade reagent silicon dioxide were mixed at a CaO / SiO2 molar ratio of 2.3, and then first-grade reagent lithium carbonate was mixed so that the Li content of the mixture was 0.1% (internal substitution) in terms of oxide (Li2O). The mixture was then heat-treated at 1,400°C for 2 hours and allowed to cool to room temperature until the Blaine specific surface area reached 4,000 cm. 2 / g of CO2 fixation material I was produced.

[0060] Powder X-ray diffraction measurements were performed on the CO2 fixation material produced. The measurement results were analyzed using quantitative software to determine the mineral composition. The powder X-ray diffraction device used was Rigaku's fully automatic multipurpose X-ray diffraction device "SmartLab," and the quantitative software used was Rigaku's "SmartlabStudio II."

[0061] The carbonation rate of each CO2 fixation material prepared in the same manner as in Experimental Example 1 was calculated. The results are shown in Table 3.

[0062] [Table 3]

[0063] [Experimental Example 4] Carbonation was carried out in the same manner as in Experimental Example 1, except that various assistants were added and mixed to 100 parts by mass of the CO2 fixation material A in the prescribed ratios shown in Table 3. The carbonation rate was calculated. The results are shown in Table 4.

[0064] [Table 4]

[0065] [Experimental Example 5] Carbonation was carried out in the same manner as in Experimental Example 1, except that the carbonation conditions in the constant temperature and humidity chamber were changed from 20°C and 80% RH to those shown in Table 5, and the carbonation rate was calculated. The results are shown in Table 5.

[0066] [Table 5]

[0067] The results in Table 1 show that the CO2 fixation material of the present invention achieves a high carbonation rate. The results in Table 2 show that a high carbonation rate was obtained when the Li content was 0.001 to 1.0 mass% calculated as the oxide (Li2O). From the results in Table 3, a good carbonation rate was obtained when the CaO / SiO2 molar ratio was 1.0 to 2.3. The results in Table 4 show that the carbonation effect was greater when disaccharides were added. In particular, the carbonation effect was greater when trehalose was added. From the results in Table 5, a good carbonation rate was obtained by setting the carbonation temperature at 75° C. or lower and / or 50% RH or higher.

[0068] [Experimental Example 6] Carbonation was carried out in the same manner as in Experimental Example 1, except that various assistants were added and mixed to 100 parts by mass of the CO2 fixation material E in the prescribed ratios shown in Table 6. The carbonation rate was calculated. The results are shown in Table 6.

[0069] [Table 6]

[0070] The results in Table 6 show that the carbonation effect was greater when disaccharides were added, and especially when trehalose was added. [Industrial Applicability]

[0071] The CO2 immobilization material of the present invention can be carbonated at a temperature of 75°C or lower and / or a humidity of 50% RH or higher to immobilize CO2. The CO2 immobilized product obtained by carbonating the CO2 immobilization material can be used in the fields of civil engineering and construction, for example, as a cement additive, and can be effectively used as it is as a material for mortar or concrete aggregate, roadbed material, embankment material, backfill material, etc.

Claims

1. γ-2CaO.SiO 2 , 3CaO・2SiO 2 , α-CaO.SiO 2 , and CO containing one or more non-hydraulic compounds selected from the group consisting of 3CaO, MgO, and 2SiO2 2 The immobilization material comprises: 2 The immobilizing material contains Li, and the Li content is 0.001 to 1.0 mass % in terms of oxide. The term "Li is contained in the CO 2 immobilizing material" refers to a CO 2 immobilizing material in which the non-hydraulic compound in the CO 2 immobilizing material contains Li 2 O as a chemical composition, but Li 2 O is not identified by X-ray diffraction measurement. 2 Immobilization material.

2. γ-2CaO.SiO 2 , 3CaO・2SiO 2 , α-CaO.SiO 2 and 3CaO.MgO.2SiO2, and one or more non-hydraulic compounds selected from the group consisting of disaccharides, and the disaccharides are contained in an amount of 0.5 to 10 parts by mass per 100 parts by mass of the non-hydraulic compound. 2 Immobilization material.

3. CaO / SiO in the non-hydraulic compound 2 3. The CO according to claim 1 or 2, wherein the molar ratio is 0.8 to 2.

3. 2 Immobilization material.

4. The CO of claim 1 further comprising a disaccharide. 2 Immobilization material.

5. The CO 2 The CO immobilization method according to claim 4, wherein the disaccharide is contained in an amount of 0.5 to 10 parts by mass per 100 parts by mass of the immobilization material. 2 Immobilization material.

6. The CO according to any one of claims 2, 4 and 5, wherein the disaccharide comprises trehalose. 2 Immobilization material.

7. The CO according to any one of claims 1 to 6 is used at 75°C or less and / or 50% RH or more. 2 CO for carbonation treatment of immobilized materials 2 Method for producing immobilized material.

Citation Information

Patent Citations

  • Stabilization method of carbon dioxide

    JP2020015659A

  • METHOD FOR PRODUCING γ-2CaO• SiO 2

    WO2014002727A1