Conductive laminate, touch panel, and method for manufacturing conductive laminate

A conductive laminate with low-water organic films and optional inorganic films and supports addresses the issue of wire disconnection in high-temperature environments, enhancing durability and reliability.

JP7569914B2Active Publication Date: 2024-10-18FUJIFILM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023188104
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-26
Filing Date
2023-11-02
Publication Date
2024-10-18
Estimated Expiration
2040-02-19

AI Technical Summary

Technical Problem

Conductive laminates with thin metal wires experience disconnection when exposed to high-temperature environments, which is not effectively addressed by existing technologies.

Method used

The conductive laminate is configured with organic films having a water content of less than 3.00%, and optionally includes an inorganic film and a support, with specific metal compositions and layer structures to enhance adhesion and protect the metal wires.

Benefits of technology

The laminate effectively suppresses disconnection of thin metal wires in high-temperature conditions, ensuring durability and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569914000002
    Figure 0007569914000002
  • Figure 0007569914000003
    Figure 0007569914000003
  • Figure 0007569914000004
    Figure 0007569914000004
Patent Text Reader

Abstract

To provide a conductive laminate body which can suppress breakage of a metal thin wire when it is set under a high-temperature environment, a touch panel, and a method for manufacturing the conductive laminate body.SOLUTION: The conductive laminate body includes a first organic film, a metal thin wire on the first organic film, and a second organic film covering the metal thin wire. The metal thin wire includes a blackening layer, an adhesive layer, and a metal conductive layer in this order from the first organic film side. The first and second organic films contain water in a concentration of less than 3.00%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive laminate, a touch panel, and a method for manufacturing a conductive laminate. [Background technology]

[0002] Conductive substrates having fine metal wires are widely used for various applications such as touch panels, solar cells, and EL (electroluminescence) elements. In particular, the rate at which touch panels are installed in mobile phones and portable game devices has been increasing in recent years, and the demand for conductive substrates for capacitive touch panels capable of multi-point detection is growing rapidly. For example, Patent Document 1 discloses a touch panel sensor in which a blackening layer and copper wiring are disposed on a substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-206315 A Summary of the Invention [Problem to be solved by the invention]

[0004] Typically, for the purpose of protecting the thin metal wires, an organic film may be disposed so as to cover the thin metal wires disposed on the organic film. The present inventors have investigated the properties of a conductive laminate obtained by disposing an adhesive layer between the blackened layer and the metal conductive layer and further disposing an organic film on the obtained thin metal wires in order to improve the adhesion between the blackened layer and the metal conductive layer, and have found that when the conductive laminate is left in a high-temperature environment, breakage of the thin metal wires may occur. This breakage of the thin metal wires does not depend on the width of the thin wires.

[0005] In view of the above circumstances, an object of the present invention is to provide a conductive laminate in which breakage of thin metal wires is suppressed when the laminate is left standing in a high-temperature environment. Another object of the present invention is to provide a method for manufacturing a touch panel and a conductive laminate. [Means for solving the problem]

[0006] As a result of extensive investigation into the above problems, the present inventors have found that the above problems can be solved by the following configuration.

[0007] (1) a first organic film; A thin metal wire disposed on the first organic film; a second organic film disposed so as to cover the thin metal wires; the thin metal wire includes, from the first organic film side, a blackening layer, an adhesion layer, and a metal conductive layer in this order; A conductive laminate, wherein the moisture content of the first organic film and the second organic film is less than 3.00%. (2) The conductive laminate according to (1), which has a moisture content of less than 1.00%. (3) The conductive laminate according to (1) or (2), wherein the blackening layer and the adhesion layer contain the same metal atoms. (4) The conductive laminate according to any one of (1) to (3), wherein the first organic film and the second organic film are made of the same material. (5) The conductive laminate according to any one of (1) to (4), wherein the line width of the thin metal wires gradually decreases from the first organic film side toward the second organic film side. (6) The conductive laminate according to any one of (1) to (5), in which an inorganic film containing at least one metal atom selected from the group consisting of Si, Al, and Ti is disposed between the thin metal wires and the second organic film so as to cover the thin metal wires. (7) The conductive laminate according to (6), wherein the inorganic film contains at least one selected from the group consisting of SiO2, SiON, SiN, Al2O3, and TiO2. (8) The conductive laminate according to any one of (1) to (7), wherein the metal conductive layer contains at least one metal atom selected from the group consisting of Cu, Al, and Ag. (9) The conductive laminate according to any one of (1) to (8), wherein the blackening layer contains at least one metal atom selected from the group consisting of Mo, Nb, Cr, Ti, and W. (10) The conductive laminate according to any one of (1) to (9), further comprising a support on the side of the first organic film opposite to the second organic film side. (11) The conductive laminate according to (10), wherein the support is a glass substrate. (12) A touch panel comprising the conductive laminate according to any one of (1) to (11). (13) forming a first organic film; forming a thin metal wire on the first organic film; forming a second organic film so as to cover the thin metal wires; the thin metal wire includes, from the first organic film side, a blackening layer, an adhesion layer, and a metal conductive layer in this order; A method for producing a conductive laminate, wherein the first organic film and the second organic film have a moisture content of less than 3.00%. Effect of the Invention

[0008] According to the present invention, it is possible to provide a conductive laminate in which breakage of thin metal wires is suppressed when the conductive laminate is left standing in a high-temperature environment. Moreover, according to the present invention, it is possible to provide a touch panel and a method for manufacturing a conductive laminate. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view of a first embodiment of a conductive laminate. [Diagram 2] FIG. 2 is a partial plan view showing a mesh pattern formed of intersecting thin metal wires. [Diagram 3] FIG. 4 is a cross-sectional view of a second embodiment of a conductive laminate. [Figure 4] FIG. 4 is a cross-sectional view of a third embodiment of a conductive laminate. [Diagram 5] FIG. 2 is a schematic diagram of a metal wiring pattern formed in an embodiment. [Figure 6]FIG. 2 is a schematic diagram of a metal wiring pattern formed in an embodiment. [Figure 7] FIG. 2 is a schematic diagram of a metal wiring pattern formed in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Preferred embodiments of the present invention will now be described. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In addition, in this specification, the term "organic film" (the first organic film to the third organic film described below) means a film containing carbon atoms, and may contain heteroatoms other than carbon atoms (e.g., silicon atoms, nitrogen atoms, oxygen atoms, etc.). A feature of the conductive laminate of the present invention is that it uses an organic film having a low moisture content. In the present invention, by surrounding the metal thin wire including the adhesive layer and the metal conductive layer with an organic film having a low moisture content, peeling between the adhesive layer and the metal conductive layer is suppressed, and disconnection is suppressed.

[0011] First Embodiment A first embodiment of the conductive laminate of the present invention will be described below with reference to the drawings. Fig. 1 shows a cross-sectional view of the first embodiment of the conductive laminate of the present invention. The conductive laminate 10A includes a first organic film 12, a thin metal wire 14A, and a second organic film 16. The thin metal wire 14A includes, from the first organic film 12 side, a blackening layer 20, an adhesion layer 22, and a metal conductive layer 24, in this order. The thin metal wire 14A disposed on the first organic film 12 is covered with the second organic film 16. That is, the thin metal wire 14A is surrounded by the first organic film 12 and the second organic film 16. When the conductive laminate 10A is applied to a touch panel, it is preferable to arrange the conductive laminate 10A in the touch panel so that the blackening layer 20 in the thin metal wire 14A is arranged on the viewing side of the metal conductive layer 24. Each member included in the conductive laminate 10A will be described in detail below.

[0012] (1st organic film) The first organic film is one of the members that supports the thin metal wires. The water content of the first organic film is less than 3.00%. In particular, from the viewpoint of suppressing breakage of the thin metal wires when the conductive laminate is left in a high-temperature environment (hereinafter, also simply referred to as "the viewpoint of superior effects of the present invention"), it is preferably less than 1.00%, and more preferably 0.40% or less. There is no particular lower limit, but it is often 0.001% or more. The moisture content can be measured by conditioning the measurement object for 24 hours in an environment of a temperature of 25° C. and a humidity of 50%, and measuring the moisture content by the Karl Fischer method (150° C., evaporation method). In this specification, "Karl Fischer method (150°C, evaporation method)" means that the moisture content was measured by a moisture evaporation method at a vaporization temperature of 150°C using a Karl Fischer moisture meter in accordance with JIS K0113.

[0013] The thickness of the first organic film is not particularly limited, but in terms of obtaining better effects of the present invention, the thickness is preferably 0.5 to 5.0 μm, and more preferably 1.0 to 3.0 μm.

[0014] The material constituting the first organic film is not particularly limited as long as it satisfies the above-mentioned moisture content, and is preferably a resin. For example, (meth)acrylic resin, polystyrene resin, polyolefin resin, fluororesin, polyimide resin, fluorinated polyimide resin, polyurethane resin, polyether ether ketone resin, polycarbonate resin, and silicon-containing resin can be mentioned, and (meth)acrylic resin or silicon-containing resin is preferable. The term "(meth)acrylic resin" includes both acrylic resin and methacrylic resin. The silicon-containing resin refers to an organic resin that contains silicon atoms. Examples of the silicon-containing resin include polysilazanes having an organic group and organic resins that contain a silsesquioxane structure.

[0015] In order to reduce the water content in the organic film, the (meth)acrylic resin preferably has a carbon ring. Examples of the carbon ring include an aliphatic ring such as a cyclohexane ring, and an aromatic ring such as a benzene ring, a naphthalene ring, a fluorene ring, an anthracene ring, and a phenanthrene ring. The carbocycle may be a monocyclic or polycyclic ring. The carbon ring is preferably a benzene ring or a fluorene ring, and more preferably a fluorene ring.

[0016] Monomers that can form the repeating units contained in the (meth)acrylic resin include acrylic acid esters such as methyl acrylate, ethyl acrylate, and butyl acrylate, and methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate. The (meth)acrylic resin may be a homopolymer of one type of (meth)acrylic acid derivative, a copolymer of two or more types of (meth)acrylic acid derivatives, or a copolymer of these with other monomers copolymerizable therewith. The weight average molecular weight Mw of the (meth)acrylic resin is preferably 20,000 or more, and more preferably 25,000 or more, and is preferably 600,000 or less, and more preferably 350,0000 or less, in terms of superior effects of the present invention. The weight average molecular weight (hereinafter abbreviated as Mw) is a value calculated as polystyrene by gel permeation chromatography (GPC). Specific measurement conditions for GPC include the following. GPC equipment: HLC-8320 (Tosoh Corporation) Column: TSK gel SuperHZM-H, TSK gel SuperHZ4000, TSK gel SuperHZ2000 (Tosoh Corporation, 4.6 mm ID (inner diameter) x 15.0 cm) Eluent: tetrahydrofuran (THF)

[0017] The (meth)acrylic resin may be one produced by a known method, or may be a commercially available product, such as Delpet 60N and 80N (manufactured by Asahi Kasei Chemicals Corporation), and Dianale BR80, BR83, BR85, BR88, BR95, BR110, and BR113 (manufactured by Mitsubishi Rayon Co., Ltd.).

[0018] When the material constituting the first organic film is a resin, the resin may have a crosslinked structure. An example of a method for forming a resin having a crosslinked structure is a method in which a polyfunctional monomer is cured to obtain a resin. The type of polymerizable group that the polyfunctional monomer has is not particularly limited, but examples include radically polymerizable groups (for example, (meth)acryloyl groups) and cationic polymerizable groups. The number of polymerizable groups that the polyfunctional monomer has is not particularly limited, but is preferably 2 or more, and more preferably 3 to 6.

[0019] When a monomer is used in producing the first organic film, a polymerization initiator may be used in combination as necessary. The polymerization initiator is selected from the most suitable initiators depending on the polymerization type, and examples of the polymerization initiator include radical polymerization initiators and cationic polymerization initiators.

[0020] The method for forming the first organic film is not particularly limited, and includes known methods. For example, the method includes forming a coating film using a composition containing a specific monomer, curing the coating film to form the first organic film, applying a composition containing a specific resin, and drying the composition as necessary to form the first organic film, and melting the resin to form a film.

[0021] (Thin metal wire) The thin metal wire includes a blackening layer, an adhesion layer, and a metal conductive layer. Each layer will be described in detail below. The blackening layer is a layer for suppressing light reflection and reducing the visibility of the thin metal wires. The material constituting the blackening layer is not particularly limited, and known materials can be used. In particular, the blackening layer preferably contains at least one metal atom selected from the group consisting of Mo, Nb, Cr, Ti, W, Ni, Ta, V, Fe, Co, Cu, Sn, and Mn, and more preferably contains at least one metal atom selected from the group consisting of Mo, Nb, Cr, Ti, and W. The blackening layer may contain atoms other than the above metal atoms (for example, carbon atoms, oxygen atoms, nitrogen atoms, and hydrogen atoms). The blackening layer may contain a metal element consisting of the above-mentioned metal atoms, or a metal alloy consisting of two or more kinds of metal atoms. The blackening layer may also contain an oxide, nitride, or oxynitride of the above-mentioned metal atoms.

[0022] The thickness of the blackened layer is not particularly limited, but from the viewpoints of being able to sufficiently suppress light reflection and being excellent in industrial applications, the thickness is preferably from 1 to 100 nm, and more preferably from 3 to 30 nm.

[0023] The adhesion layer is a layer for ensuring adhesion between the blackening layer and the metal conductive layer. The material constituting the adhesion layer is not particularly limited, and known materials can be used. Among them, the adhesion layer preferably contains at least one metal atom selected from the group consisting of Mo, Nb, Cr, Ti, W, Ni, Ta, V, Fe, Co, Cu, Sn, and Mn, and more preferably contains at least one metal atom selected from the group consisting of Mo, Nb, Cr, Ti, and W. The adhesion layer may contain atoms other than the above metal atoms (for example, carbon atoms, oxygen atoms, nitrogen atoms, and hydrogen atoms). The adhesion layer may contain a metal element consisting of the above-mentioned metal atoms, or a metal alloy consisting of two or more kinds of metal atoms. The adhesion layer may also contain an oxide, nitride, or oxynitride of the above-mentioned metal atoms.

[0024] In order to improve the adhesion between the adhesion layer and the blackening layer, it is preferable that the blackening layer and the adhesion layer contain the same metal atoms. Even if the adhesive layer and the blackening layer have the same constituents, their functions may differ due to differences in density. The densities of the adhesive layer and the blackening layer may vary depending on the conditions under which they are formed (for example, the conditions of the sputtering method).

[0025] The thickness of the adhesive layer is not particularly limited, but in terms of obtaining a better effect of the present invention, the thickness is preferably from 1 to 100 nm, and more preferably from 20 to 60 nm.

[0026] The metal conductive layer is a member capable of imparting electrical conductivity to the conductive laminate. The material constituting the metal conductive layer is not particularly limited, and known materials can be used. Among them, the metal conductive layer preferably contains at least one metal atom selected from the group consisting of Cu, Al, Ag, Pt, Ni, and Pd, and more preferably contains at least one metal atom selected from the group consisting of Cu, Al, and Ag. The metal conductive layer may contain a simple metal made of the above-mentioned metal atoms, or a metal alloy made of two or more kinds of metal atoms.

[0027] The thickness of the metal conductive layer is not particularly limited, but from the viewpoint of electrical conductivity, the thickness is preferably from 10 to 700 nm, and more preferably from 100 to 600 nm.

[0028] The thin metal wire may include layers other than the blackening layer, the adhesion layer, and the metal conductive layer. For example, the thin metal wire may include an adhesion layer and a protective layer on the surface of the metal conductive layer opposite to the adhesion layer side. The adhesion layer disposed between the metal conductive layer and the protective layer is a layer for ensuring adhesion between the two. The structure of the adhesion layer can be the structure of the adhesion layer disposed between the above-mentioned blackening layer and the metal conductive layer.

[0029] The protective layer is a layer that has the role of protecting the metal conductive layer. The protective layer may have the same structure as the blackening layer described above.

[0030] The shape of the thin metal wire is not particularly limited, but it is preferable that the line width of the thin metal wire gradually decreases from the first organic film side toward the second organic film side (see FIG. 1). In other words, the thin metal wire preferably has a tapered cross-sectional shape. When the thin metal wire has the above shape, the thin metal wire becomes more difficult to see. The angle (θ1 in FIG. 1; hereinafter also referred to as the taper angle) between the inclined surface of the thin metal wire having a tapered cross section and the surface of the first organic film is not particularly limited, but is preferably 60 to 80°. The line width of the blackening layer on the first organic film side may be different from the line width of the metal conductive layer on the first organic film side, and the ratio of the line width W2 of the metal conductive layer on the first organic film side to the line width W1 of the blackening layer on the first organic film side {(W2 / W1)×100(%)} (see FIG. 1) is preferably 90 to 99.9%. If within the above range, the thin metal lines become less visible.

[0031] The line width of the metal thin wire is not particularly limited, and is preferably 30 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, particularly preferably 9 μm or less, most preferably 7 μm or less, preferably 0.5 μm or more, and more preferably 1.0 μm or more. Within the above range, an electrode that is low in resistance and difficult to see can be formed. Note that the line width of the thin metal wires refers to the largest line width of the thin metal wires. In the case of thin metal wires having a tapered cross-sectional shape as shown in FIG. 1, the line width of the blackening layer on the first organic film side corresponds to the line width of the thin metal wires.

[0032] The thickness of the thin metal wire is not particularly limited, and is preferably 0.01 to 20 μm, more preferably 0.01 to 10 μm, and even more preferably 0.01 to 5 μm. If the thickness is within the above range, an electrode that has low resistance and is difficult to see can be formed.

[0033] The thin metal wires may form a pattern, and the pattern is not particularly limited, and is preferably a triangle such as an equilateral triangle, an isosceles triangle, or a right-angled triangle; a quadrilateral (e.g., a square, a rectangle, a rhombus, a parallelogram, or a trapezoid); a (regular) n-gon such as a (regular) hexagon or a (regular) octagon; a circle; an ellipse; a star; or a geometric figure combining these, and more preferably a mesh-like shape (mesh pattern).

[0034] The mesh shape includes a shape including a plurality of openings 18 formed by intersecting thin metal wires 14, as shown in Fig. 2. The length L of one side of the openings 18 is not particularly limited, but is preferably 1500 µm or less, more preferably 1300 µm or less, even more preferably 1000 µm or less, preferably 5 µm or more, more preferably 30 µm or more, and even more preferably 80 µm or more. When the length of one side of the opening is within the above range, the transparency of the conductive laminate is improved.

[0035] In FIG. 2, the opening 18 has a diamond shape, but may have other shapes. For example, it may be a polygon (for example, a triangle, a rectangle, a hexagon, or a random polygon). In addition, the shape of one side may be a straight line, a curved shape, or an arc shape. In the case of an arc shape, for example, two opposing sides may be outwardly convex arc shapes, and the other two opposing sides may be inwardly convex arc shapes. In addition, the shape of each side may be a wavy line shape in which an outwardly convex arc and an inwardly convex arc are continuous. Of course, the shape of each side may be a sine curve.

[0036] In terms of visible light transmittance, the mesh pattern formed of the thin metal wires has an aperture ratio of preferably 85% or more, more preferably 90% or more, and even more preferably 95% or more. The aperture ratio corresponds to the proportion of the area on the first organic film excluding the area where the thin metal wires are located to the whole area.

[0037] The method for forming the thin metal wires is not particularly limited, and includes known methods such as sputtering, ion plating, and vapor deposition. As a method for forming the thin metal wires at the predetermined positions, there are known methods, such as forming a blackening layer, an adhesion layer, and a metal conductive layer all over the first organic film by a sputtering method, forming a patterned resist film on the metal conductive layer, and removing the blackening layer, adhesion layer, and metal conductive layer at the openings of the resist film to arrange the thin metal wires at the predetermined positions. The unnecessary layers may be removed by either wet etching (eg, etching using an etching solution) or dry etching.

[0038] (Second organic film) The second organic film, together with the above-mentioned first organic film, is one of the members that support the thin metal wires. The configuration of the second organic film is the same as that of the first organic film described above. For example, the range of the moisture content of the second organic film is the same as that of the first organic film described above. The thickness of the second organic film is preferably 0.5 to 5.0 μm, and more preferably 1.0 to 3.0 μm, in order to cover the thin metal wires and to provide a smooth surface of the second organic film. Furthermore, the preferred embodiments of the material constituting the second organic film are the same as the preferred embodiments of the material constituting the first organic film. The method for forming the second organic film is the same as the method for forming the first organic film described above.

[0039] In order to obtain a more excellent effect of the present invention, it is preferable that the first organic film and the second organic film are made of the same material, which improves the adhesion between the first organic film and the second organic film.

[0040] The conductive laminate can be produced by a known method. Among these, it is preferable to manufacture the thin film by a method including the steps of forming a first organic film, forming thin metal wires on the first organic film, and forming a second organic film so as to cover the thin metal wires. The specific manufacturing methods for each of the members (first organic film, thin metal wires, second organic film) are as described above.

[0041] The conductive laminate may include other members than those mentioned above. For example, a conductive portion other than the thin metal wires (for example, conductive terminal portions disposed on both ends of a mesh pattern made of thin metal wires) may be disposed between the first organic film and the second organic film.

[0042] <Second embodiment> A second embodiment of the conductive laminate of the present invention will be described below with reference to the drawings. Fig. 3 shows a cross-sectional view of the second embodiment of the conductive laminate of the present invention. The conductive laminate 10B includes a first organic film 12, fine metal wires 14A, an inorganic film 26, and a second organic film 16. The fine metal wires 14A include, from the first organic film 12 side, a blackening layer 20, an adhesion layer 22, and a metal conductive layer 24, in this order. The conductive laminate 10B has a similar configuration to the conductive laminate 10A except for the inorganic film 26, and the same components are given the same reference numerals and descriptions thereof are omitted. The inorganic film 26 will be described in detail below.

[0043] (Inorganic membrane) The inorganic film is a film disposed between the first organic film and the second organic film so as to cover the thin metal wires. By disposing the inorganic film, the effects of the present invention are more excellent. The material constituting the inorganic film is not particularly limited, and preferably contains at least one metal atom selected from the group consisting of Si, Al, and Ti. The inorganic film may contain atoms other than the above metal atoms (for example, carbon atoms, oxygen atoms, nitrogen atoms, and hydrogen atoms). The inorganic film may contain an oxide, nitride, or oxynitride of the above-mentioned metal atoms, and preferably contains at least one selected from the group consisting of SiO2, SiON, SiN, Al2O3, and TiO2.

[0044] The thickness of the inorganic film is not particularly limited, and is preferably from 10 to 1000 nm, more preferably from 20 to 200 nm.

[0045] As shown in FIG. 3, the inorganic film may be disposed so as to cover the first organic film and the thin metal wires, or may be disposed so as to cover only the thin metal wires. The method for forming the inorganic film is not particularly limited, and includes known methods such as sputtering, ion plating, chemical vapor deposition (CVD), and liquid phase growth methods such as plating and the sol-gel method.

[0046] <Third embodiment> The third embodiment of the conductive laminate of the present invention will be described below with reference to the drawings. Fig. 4 shows a cross-sectional view of the third embodiment of the conductive laminate of the present invention. The conductive laminate 10C includes a support 28, a first organic film 12, fine metal wires 14A, a second organic film 16, fine metal wires 14B, an inorganic film 26, and a third organic film 30. The fine metal wires 14A and 14B include, from the first organic film 12 side, a blackening layer 20, an adhesion layer 22, and a metal conductive layer 24, in this order. When the conductive laminate 10C is applied to a touch panel, it is preferable to arrange the conductive laminate 10C in the touch panel so that the blackened layer 20 in the thin metal wires 14A is arranged on the viewing side of the metal conductive layer 24. In other words, it is preferable to arrange the support 28 on the viewing side in the touch panel. In this case, the support 28 may constitute the touch surface of the touch panel. The first organic film 12, the thin metal wires 14A, and the second organic film 16 in the conductive laminate 10C correspond to the first organic film 12, the thin metal wires 14A, and the second organic film 16, respectively, of the conductive laminate 10A, and their explanations will be omitted. In the following, the support 28, the thin metal wires 14B (hereinafter also referred to as "second thin metal wires"), the inorganic film 26, and the third organic film 30 included in the conductive laminate 10C will be described in detail.

[0047] (Support) The support is a member for supporting other members, more specifically, it functions as a member when the first organic film is formed. The type of the support is not particularly limited, and examples thereof include a glass substrate and a resin substrate. From the viewpoints of transparency and light resistance, a glass substrate is preferred. In addition, examples of materials constituting the resin substrate include thermoplastic resins. Examples of the thermoplastic resins include polyester resins such as polyethylene terephthalate, methacrylic resins, methacrylic acid-maleic acid copolymers, polystyrene resins, transparent fluororesins, polyimide, fluorinated polyimide resins, polyamide resins, polyamideimide resins, polyetherimide resins, cellulose acylate resins, polyurethane resins, polyether ether ketone resins, polycarbonate resins, alicyclic polyolefin resins, polyarylate resins, polyethersulfone resins, polysulfone resins, cycloolefin copolymers, fluorene ring-modified polycarbonate resins, alicyclic modified polycarbonate resins, and fluorene ring-modified polyester resins. The thickness of the support is not particularly limited, and is often 25 to 500 μm. The total light transmittance of the support is preferably 85 to 100%.

[0048] In addition, a temporary support (peelable support) can also be used as the support. When a temporary support is used as the support, the member disposed on the temporary support can be transferred to another object to be pasted. In this case, peeling occurs between the temporary support and the first organic film, and the temporary support can be separated.

[0049] (Second metal thin wire) The second thin metal wire is a thin wire disposed between the second organic film and the third organic film. The configuration of the second thin metal wires is similar to the configuration of the thin metal wires explained in the above-mentioned first embodiment.

[0050] (Inorganic membrane) The inorganic film is a film disposed between the second organic film and the third organic film so as to cover the second thin metal wires. By disposing the inorganic film, the effects of the present invention are more excellent. The configuration of the inorganic film is the same as that of the inorganic film described in the above-mentioned second embodiment.

[0051] (Third organic film) The third organic film is a film disposed so as to cover the second thin metal wires. The configuration of the third organic film is the same as the configuration of the first organic film described above in the first embodiment. For example, the range of the water content of the third organic film is the same as the range of the water content of the first organic film described above. The preferred range of the thickness of the third organic film is the same as the preferred range of the thickness of the first organic film described above. Furthermore, the preferred embodiments of the material constituting the third organic film are the same as the preferred embodiments of the material constituting the first organic film. The method for forming the third organic film is the same as the method for forming the first organic film described above.

[0052] The conductive laminate of the present invention can be suitably used for a touch panel. The type of touch panel having the conductive laminate of the present invention is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a surface-type capacitive touch panel, a projected capacitive touch panel, and a resistive touch panel. Note that the touch panel includes so-called touch sensors and touch pads. The above touch panel is applied to various display devices (such as liquid crystal display devices and organic electroluminescence display devices). EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0054] <Example 1> (Preparation of the support) The surface of a 10 cm square glass substrate (Corning, Eagle XG glass) was subjected to UV (ultraviolet) ozone treatment for 5 minutes. The obtained glass substrate was then immersed in an aqueous solution of 30% by mass of Clean Ace manufactured by AS ONE Corporation, and the surface of the glass substrate was scrubbed and washed using Bellclean manufactured by AION Corporation. The obtained glass substrate was then immersed in pure water, and the surface of the glass substrate was scrubbed and washed using Bellclean in the same manner as above. The obtained glass substrate was then air-blowed and dried at 200°C for 30 minutes.

[0055] (First organic film formation) Trimethylolpropane triacrylate (manufactured by Toagosei Co., Ltd.) and a photopolymerization initiator (ESACURE KTO46 manufactured by Lamberti Co., Ltd.) were mixed in a ratio of 95.5% by mass:4.5% by mass, and then dissolved in methyl ethyl ketone to a solids concentration of 10% by mass to obtain a composition for forming an organic film. Next, the organic film-forming composition was applied onto the glass substrate that had been cleaned as described above using an applicator bar (effective width 20 mm) of a Tester Sangyo automatic coater PI1210, and then dried at 120° C. for 3 minutes to form a coating film. The coating speed was 100 mm / sec. Next, the coating was irradiated with UV light (600 mJ / cm ) using a metal halide lamp MAL625NL manufactured by Japan Battery Co., Ltd. under conditions of an oxygen concentration of 200 ppm by volume and a temperature of 80°C. 2 ) to obtain a cured film. The cured film was then dried under vacuum at 80° C. for 12 hours to obtain a first organic film (thickness: 1.5 μm).

[0056] (First metal thin wire formation) A MoNb film (Mo content: 80 mass %, Nb content: 20 mass %) having a thickness of 10 nm was formed on the obtained first organic film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 7 Pa, the power was 7 kW, and the deposition rate was 0.8 nm / min. Next, a MoNb film (Mo content: 80 mass %, Nb content: 20 mass %) having a thickness of 40 nm was formed on the MoNb film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 8 Pa, the power was 8 kW, and the deposition rate was 0.6 nm / min. Next, a Cu film with a thickness of 200 nm was formed on the MoNb film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 5 Pa, the power was 5 kW, and the deposition rate was 0.4 nm / min. Next, a CuNi film (Cu content: 75 mass %, Ni content: 25 mass %) having a thickness of 80 nm was formed on the Cu film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 6 Pa, the power was 6 kW, and the deposition rate was 0.8 nm / min. Next, a MoNb film (Mo content: 80 mass %, Nb content: 20 mass %) having a thickness of 100 nm was formed on the CuNi film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 4 Pa, the power was 4 kW, and the deposition rate was 0.5 nm / min. In the magnetron sputtering method, argon was used as the inert gas. Next, OAP manufactured by Tokyo Ohka Kogyo Co., Ltd. was applied onto the formed laminated film. Next, Novolak OFPR800 manufactured by Tokyo Ohka Kogyo Co., Ltd. was further applied as a patterning resist. The above application was performed using a spin coater 1H-D7 manufactured by Mikasa Co., Ltd. After the above application, the film was dried at 90°C for 3 minutes to obtain a resist film with a thickness of 1 μm. Next, the resist film was irradiated with light for 10 seconds using a mesh photomask and a mask aligner MA-20 (mercury light source) manufactured by Mikasa Co., Ltd. Thereafter, the resist film was immersed in a 2.38% aqueous solution of NMD-W manufactured by Tokyo Ohka Kogyo Co., Ltd. for 5 minutes, then immersed in pure water for 1 minute, and dried at 120°C for 3 minutes to obtain a patterned resist film. The glass substrate having the patterned resist film was immersed in an etching solution (ferric chloride solution manufactured by Toagosei Co., Ltd.) kept at 50°C for 1 minute, then immersed in pure water for 5 minutes, blown with air, and dried at 120°C for 3 minutes to obtain a mesh-like metal wire as shown in Figure 2. The formed thin metal wire contained a MoNb film (blackening layer), a MoNb film (adhesion layer), a Cu film (metal conductive layer), a CuNi film (adhesion layer), and a MoNb film (protection layer) in this order. The thin metal wire had a tapered cross-sectional shape as shown in Figure 1, the line width of the thin metal wire (corresponding to the line width of the blackening layer on the first organic film side) was 4.0 μm, the taper angle θ1 was 70°, and the ratio of the line width W2 of the metal conductive layer on the first organic film side to the line width W1 of the blackening layer on the first organic film side was 97%. 5, 20 units 44 were arranged on the first organic film, each unit 44 being made of a mesh pattern 40 formed from the mesh-like first thin metal wires and two resistance measurement terminals 42 sandwiching the mesh pattern 40. The length of one side of the mesh-like opening of the mesh pattern was 500 μm, and the angle of one of the diamond-shaped openings (angle θ2 in FIG. 2) was 65°. The size of the resistance measurement terminals 42 was 2 mm × 1 mm, and the interval between each unit 44 was 2 mm.

[0057] (Second organic film formation) On the first organic film on which the thin metal wires were formed, a second organic film having a thickness of 2.5 μm was formed in the same manner as in the above (formation of the first organic film).

[0058] (Second metal thin wire formation) A mesh-like second thin metal wire was formed on the second organic film in the same manner as in the above (first thin metal wire), except that the mesh-like second thin metal wire was formed so that the intersections of the mesh pattern formed by the first thin metal wire were positioned at the openings of the mesh pattern formed by the second thin metal wire. 6, 20 units 44 were arranged on the second organic film, each unit being composed of a mesh pattern 40 formed from the mesh-like second thin metal wires and two resistance measurement terminals 42 sandwiching the mesh pattern 40. The size of the resistance measurement terminals 42 was 2 mm×1 mm, and the interval between each unit 44 was 2 mm. Note that the arrangement direction of the units is different in FIG. 5 and FIG. 6, and the arrangement direction of the units of the second thin metal wires was set to be perpendicular to the arrangement direction of the units of the first thin metal wires.

[0059] (Inorganic film formation) A SiO2 film having a thickness of 50 nm was formed by plasma CVD on the second organic film on which the second thin metal wires were disposed. In the plasma CVD method, silane gas, hydrogen gas, and oxygen gas were used as raw material gas. The flow rates of silane gas, hydrogen gas, and oxygen gas were 100 sccm, 1000 sccm, and 200 sccm, respectively. The degree of vacuum was 50 Pa, the substrate temperature was 30°C, the electrode input power was 6.5 kW, and the deposition rate was 10 nm / min.

[0060] (Third organic film formation) On the SiO2 film, a second organic film having a thickness of 2.0 μm was formed according to the same procedure as that described above (formation of the first organic film).

[0061] By the above procedure, a conductive laminate 1 was obtained as shown in Fig. 4. When the conductive laminate 1 was observed from above, a mesh pattern was found to be arranged as shown in Fig. 7.

[0062] <Example 2> A conductive laminate 2 was obtained in the same manner as in Example 1, except that the manufacturing conditions for each layer in the above (formation of first thin metal wires) were changed as shown below (manufacturing conditions 2). The first and second thin metal wires in the conductive laminate 2 included a Mo2N film (blackened layer), a Mo film (adhesion layer), an Al film (metal conductive layer), a Mo film (adhesion layer), and a Mo2N film (protective layer) in that order.

[0063] (Manufacturing condition 2) A MoN film having a thickness of 10 nm was formed on the obtained first organic film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 1 Pa, the power was 10 kW, and the deposition rate was 0.5 nm / min. Next, a Mo film with a thickness of 40 nm was formed on the MoN film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30°C, and a vacuum degree of 5.0×10 -2 The pressure was 8 Pa, the power was 8 kW, and the deposition rate was 0.6 nm / min. Next, an Al film with a thickness of 200 nm was formed on the Mo film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 6 Pa, the power was 6 kW, and the deposition rate was 0.4 nm / min. Next, a Mo film with a thickness of 80 nm was formed on the Al film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30° C., and a vacuum degree of 5.0×10 -2 The pressure was 4 Pa, the power was 4 kW, and the deposition rate was 0.3 nm / min. Next, a MoN film with a thickness of 100 nm was formed on the Mo film by magnetron sputtering. The conditions for the magnetron sputtering were a magnetic field strength of 1000 Gauss, a substrate temperature of 30°C, and a vacuum degree of 5.0×10 -2 The pressure was 7 Pa, the power was 7 kW, and the deposition rate was 0.4 nm / min. In the magnetron sputtering method, nitrogen was used as the reactive gas and argon was used as the inert gas.

[0064] <Examples 3 to 5> Conductive laminates 3 to 5 were obtained in the same manner as in Example 1, except that the materials shown in Table 1 were used instead of trimethylolpropane triacrylate.

[0065] <Examples 6 to 7> Conductive laminates 6 to 7 were obtained in the same manner as in Example 1, except that the above procedure (formation of the first organic film) was changed as follows. In the conductive laminates 6 to 7, the first organic film, the second organic film, and the third organic film were all formed using the materials shown in Table 1. The thicknesses of the first organic film, the second organic film, and the third organic film of the conductive laminates 6 to 7 were the same as the thicknesses of the first organic film, the second organic film, and the third organic film of the conductive laminate 1.

[0066] (First organic film formation) BR113 (manufactured by Mitsubishi Rayon Co., Ltd.) or BR95 (manufactured by Mitsubishi Rayon Co., Ltd.) was dissolved in methyl ethyl ketone to a solid content concentration of 10 mass % to obtain a composition for forming an organic film. Next, the organic film-forming composition was applied onto the glass substrate that had been cleaned as described above using an applicator bar (effective width 20 mm) in a Tester Sangyo automatic coater PI1210, and then dried at 120° C. for 3 minutes to form a first organic film. The coating speed was 100 mm / sec.

[0067] <Example 8> A conductive laminate 8 was obtained in the same manner as in Example 1, except that the above procedure (formation of the first organic film) was changed as follows. In the conductive laminate 8, the first organic film to the third organic film were all formed using the materials shown in Table 1. The first organic film to the third organic film of the conductive laminate 8 had the same thickness as the first organic film to the third organic film of the conductive laminate 1.

[0068] (First organic film formation) Using an applicator bar (effective width 20 mm) on a Tester Sangyo automatic coater PI1210, Silplus HT100 (manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.) was applied onto the glass substrate that had been cleaned as described above, and then the substrate was dried at 120°C for 3 minutes to form a coating film. The coating speed was 100 mm / sec. Next, the coating was irradiated with UV light (1000 mJ / cm ) using a metal halide lamp MAL625NL manufactured by Japan Battery Co., Ltd. under conditions of an oxygen concentration of 200 ppm by volume. 2 ) to obtain a cured film.

[0069] <Examples 9 to 12> Conductive laminates 9 to 12 were obtained following the same procedure as in Example 1, except that the above procedure (forming the first organic film) was changed as follows, and the line width of the thin metal wire (corresponding to the line width on the first organic film side of the blackened layer) and the thickness of the metal conductive layer were changed as shown in Table 1. In the conductive laminates 9 to 12, the first organic film, the second organic film, and the third organic film were all formed using the materials shown in Table 1. The thicknesses of the first organic film, the second organic film, and the third organic film of the conductive laminate 9 were the same as the thicknesses of the first organic film, the second organic film, and the third organic film of the conductive laminate 1.

[0070] (First organic film formation) A dibutyl ether solution of 20% by mass of catalyst-free perhydropolysilazane (AQUAMICA NN120-20: manufactured by AZ Electronic Materials Co., Ltd.) and a dibutyl ether solution containing 5% by mass (solid content) of an amine catalyst (N,N,N',N'-tetramethyl-1,6-diaminohexane) (AQUAMICA NAX120-20: manufactured by AZ Electronic Materials Co., Ltd.) were mixed to prepare an organic film-forming composition. The content of the amine catalyst in the obtained organic film-forming composition was 1% by mass relative to the total solid content. Next, the organic film-forming composition was applied onto the above-cleaned glass substrate using an applicator bar (effective width 20 mm) of a Tester Sangyo automatic coater PI1210, and then dried at 120° C. for 3 minutes to form a coating film. The coating speed was 100 mm / sec. Next, the coating was irradiated with UV light (5000 mJ / cm) using a metal halide lamp MAL625NL manufactured by Japan Battery Co., Ltd. under conditions of an oxygen concentration of 200 ppm by volume and a temperature of 100°C. 2 ) to obtain a cured film. The obtained cured film was then dried at 80° C. for 12 hours to obtain a first organic film.

[0071] <Example 13> A conductive laminate 13 was obtained in the same manner as in Example 9, except that the manufacturing conditions for each layer in the above (formation of first thin metal wires) were changed to the above (manufacturing conditions 2).

[0072] <Comparative Examples 1 to 3> Conductive laminates C1 to C3 were obtained in the same manner as in Example 1, except that the monomers shown in Table 1 were used instead of trimethylolpropane triacrylate. In Comparative Example 3, styrene and A9300 were mixed in a mass ratio of 1:1.

[0073] <Evaluation> (Moisture content evaluation) An organic film (thickness: 1.5 μm) was produced on a glass support according to the procedures in Examples 1 to 13 and Comparative Examples 1 to 3 (formation of first organic film). The obtained organic film was scraped off from the glass support and left to stand for 24 hours under an environment of 25°C temperature and 50% humidity, and the moisture content of the obtained organic film was measured by the Karl Fischer method (150°C, evaporation method) using the apparatus AQV-2100 manufactured by Hiranuma Sangyo Co., Ltd. The results are summarized in Table 1.

[0074] (Disconnection evaluation) 100 conductive laminates were produced for each of the example and comparative example. After leaving the conductive laminate for one week in an environment of 50°C, a probe was applied to the resistance measurement terminals on both ends of each unit, and the resistance value was measured with a resistance measuring device. If even one unit out of a total of 40 units in each conductive laminate was broken, it was counted as the number of breaks. Of the 100 samples measured, 10 or more samples with broken wires were given a score of 1, 3 to 9 samples with broken wires were given a score of 2, 1 to 2 samples with broken wires were given a score of 3, and 0 samples with broken wires were given a score of 4.

[0075] The symbols in the "Materials" column in Table 1 represent the following: TMPTA: Trimethylolpropane triacrylate (manufactured by Toagosei Co., Ltd.) AD-TMP: Ditrimethylolpropane tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) A-DCP: Tricyclodecane dimethanol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.) EA-0250P: 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene (Osaka Gas Chemicals) BR-113: Dianall BR-113 (manufactured by Mitsubishi Rayon Co., Ltd.) BR95: Dianale BR-95 (manufactured by Mitsubishi Rayon Co., Ltd.) Silplus HT100: Silplus HT100 (manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.) Polysilazane: A mixture of a dibutyl ether solution of perhydropolysilazane (AQUAMICA NN120-20: manufactured by AZ Electronic Materials Co., Ltd.) and a dibutyl ether solution containing an amine catalyst (N,N,N',N'-tetramethyl-1,6-diaminohexane) (AQUAMICA NAX120-20: manufactured by AZ Electronic Materials Co., Ltd.) A9300: Ethoxylated isocyanuric acid triacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0076] "Moisture content" in Table 1 indicates the moisture content of the organic films (first organic film to third organic film) in each conductive laminate. The "Thin Metal Wire" column in Table 1 indicates that the thin metal wire formed includes a MoNb film (blackened layer), a MoNb film (adhesion layer), a Cu film (metal conductive layer), a CuNi film (adhesion layer), and a MoNb film (protective layer), and indicates that the thin metal wire formed includes a Mo2N film (blackened layer), a Mo film (adhesion layer), an Al film (metal conductive layer), a Mo film (adhesion layer), and a Mo2N film (protective layer), and is indicated as "B." In Table 1, "Width of thin metal wire (μm)" indicates the width of the thin metal wire (the width of the blackening layer on the first organic film side). In Table 1, "Thickness of metal conductive layer (nm)" indicates the thickness of the metal conductive layer in the thin metal wire.

[0077] [Table 1]

[0078] As shown in Table 1, the conductive laminate of the present invention exhibits the desired effects. In particular, it was confirmed that when the moisture content of the organic film is less than 1.00% (particularly when it is 0.40% or less), a more excellent effect is exhibited. [Explanation of symbols]

[0079] 10A, 10B, 10C Conductive laminate 12 First organic film 14A,14B Fine metal wire 16 Second organic film 18 Openings 20 Blackened layer 22 Adhesion layer 24 Metal Conductive Layer 26 Inorganic membrane 28 Support 30 Third organic film 40 Mesh Pattern 42 Resistance measurement terminal 44 units

Claims

1. A first organic film; a thin metal wire disposed on the first organic film; a second organic film disposed so as to cover the thin metal wire; the thin metal wire includes a blackening layer, an adhesion layer, and a metal conductive layer in this order from the first organic film side, the water content of the first organic film and the second organic film is 0.25% or more and less than 3.00%, The conductive laminate, wherein the first organic film has a thickness of 0.5 to 5.0 μm.

2. The conductive laminate according to claim 1 , wherein the moisture content is less than 1.00%.

3. The conductive laminate described in claim 1 or 2, wherein the material constituting the first organic film is an acrylic resin, a methacrylic resin, or a silicon-containing resin.

4. 4. The conductive laminate according to claim 1, wherein the blackening layer and the adhesion layer contain the same metal atoms.

5. 5. The conductive laminate according to claim 1, wherein the first organic film and the second organic film are made of the same material.

6. 6. The conductive laminate according to claim 1, wherein the line width of the thin metal wires gradually decreases from the first organic film side toward the second organic film side.

7. The conductive laminate according to any one of claims 1 to 6, wherein an inorganic film containing at least one type of metal atom selected from the group consisting of Si, Al, and Ti is disposed between the thin metal wires and the second organic film so as to cover the thin metal wires.

8. The inorganic film is SiO 2 , SiON, SiN, Al 2 O 3 , and TiO 2 The conductive laminate according to claim 7 , comprising at least one selected from the group consisting of:

9. The conductive laminate according to any one of claims 1 to 8, wherein the metal conductive layer contains at least one metal atom selected from the group consisting of Cu, Al, and Ag.

10. The conductive laminate according to any one of claims 1 to 9, wherein the blackening layer contains at least one metal atom selected from the group consisting of Mo, Nb, Cr, Ti, and W.

11. The conductive laminate according to any one of claims 1 to 10, further comprising a support on the side of the first organic film opposite to the second organic film side.

12. a second thin metal wire disposed on a side of the second organic film opposite to the first organic film; a third organic film disposed so as to cover the second thin metal wires, the second thin metal wire includes a blackening layer, an adhesion layer, and a metal conductive layer in this order from the first organic film side, The conductive laminate according to claim 11 , wherein the third organic film has a moisture content of less than 3.00%.

13. The conductive laminate according to claim 11 or 12, wherein the support is a glass substrate.

14. A touch panel comprising the conductive laminate according to any one of claims 1 to 13.

15. forming a first organic film; forming a thin metal wire on the first organic film; forming a second organic film so as to cover the thin metal wires; the thin metal wire includes a blackening layer, an adhesion layer, and a metal conductive layer in this order from the first organic film side, the water content of the first organic film and the second organic film is 0.25% or more and less than 3.00%, The method for producing a conductive laminate, wherein the first organic film has a thickness of 0.5 to 5.0 μm.

16. A method for manufacturing a conductive laminate as described in claim 15, wherein the material constituting the first organic film is an acrylic resin, a methacrylic resin, or a silicon-containing resin.

Citation Information

Patent Citations

  • Touch sensing electrode structure and method of manufacturing same

    EP2983072A1

  • Film-shaped touch panel sensor and method for manufacturing the same

    JP2013206315A

  • Electrode film, method for producing the same, and image display device

    JP2014150118A

  • Wiring board, touch panel, color filter substrate, and display device

    JP2017211826A

  • Touch window

    KR1020150134010A