Method for acid hydrolysis of pure polylaurolactam
The method of hydrolyzing PA12 with sulfuric acid at controlled temperatures and pressures effectively addresses the challenge of incomplete conversion in existing methods, achieving nearly complete conversion to ω-aminolauric acid, especially with low laurolactam and ω-aminolauric acid contents.
Patent Information
- Application Number
- JP2023517409
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-16
- Filing Date
- 2021-09-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-14
AI Technical Summary
The hydrolysis of polylaurolactam (PA12) is technically demanding due to its high stability, and existing methods do not achieve complete conversion efficiently, particularly when the starting material is low in laurolactam and ω-aminolauric acid.
Hydrolyzing polylaurolactam with sulfuric acid at specific temperatures (125°C to 190°C, preferably 140°C to 180°C) and pressures (1 to 100 bar) with controlled sulfuric acid content, optionally followed by an alkali hydroxide step to enhance conversion.
This method achieves nearly quantitative conversion of PA12 to ω-aminolauric acid, even with low laurolactam and ω-aminolauric acid contents, improving upon previous methods by ensuring high yields and efficient processing.
Smart Images

Figure 0007569929000001 
Figure 0007569929000002 
Figure 0007569929000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an improved process for the acid hydrolysis of polylaurolactam with sulfuric acid. As starting material, polylaurolactam which is to be recycled and which is characterized by a low content of laurolactam is particularly suitable.
[0002] 2. Background of the Invention Polylaurolactam (CAS number: 24937-16-4; also known as nylon 12, polyamide 12, hereafter abbreviated as "PA12") is an industrially important polymer.
[0003] PA12 comprises a repeat unit of the following structure (I): * The bonds indicated by ( ) are the bonds between adjacent repeat units. ** ) to the bond indicated. [ka]
[0004] PA12 is valued in applications especially for its high hydrolytic stability and, in terms of this property, is clearly different from short-chain polyamides such as polycaprolactam (CAS number: 25038-54-4; alternative name: polyamide 6; hereinafter abbreviated as "PA6") or poly-(N,N'-hexamethylene adipamide) / poly-(hexamethylene adipamide) (CAS number: 32131-17-2; alternative name: polyamide 66; hereinafter abbreviated as "PA66").
[0005] PA6 and PA66 absorb several times more water due to the higher density of amide groups, and the reaction equilibrium in the case of short chain polyamides is much more biased in favor of the monomer, so that the hydrolysis can proceed much faster. Recycling of these materials requires cleavage of the amide bond, which is usually carried out under acid or base catalysis to give the defined monomer units.
[0006] The first approaches to chemical recycling of nylon 66 have been undertaken for as long as these materials have existed.
[0007] US 2,872,420 describes a method for recovering nylon 66 from waste materials using sulfuric acid, which shows that high purity sulfuric acid has only a small effect on the molecular weight of the polyamide and can therefore be used for purification by dissolution and precipitation.
[0008] Recycling of nylon 6 is a special case since the monomer caprolactam can be separated off from the reaction mixture by distillation and the reaction can be brought to high conversions even with non-quantitative addition of acid or base.
[0009] Treatment of PA6 and PA66 with base or mineral acid in the presence of water at relatively high temperatures leads to their decomposition into monomeric units.
[0010] US 2,407,896 A and US 3,069,465 A describe the hydrolysis of PA66 with sulfuric acid.
[0011] WO 97 / 00846 A1 describes the hydrolysis of PA66 with nitric acid.
[0012] US 2,840,606 A describes the alkaline hydrolysis of short chain AABB type polyamides. Under alkaline catalysis, the diamines and diacids as components are reformed at temperatures above 160° C. The addition of an aliphatic alcohol accelerates the reaction.
[0013] While the hydrolysis of PA6 is successful using the methods described in the prior art, the workup of aqueous solutions of this amino acid is difficult, since the short-chain ω-aminocarboxylic acids are readily soluble both as salts and as free acids, and thus their purification requires the distillation of large amounts of water.
[0014] In Chinese Patent Publication No. 102399363 (CN102399363 A), SO4 2- The hydrolysis of nylon 6 by hydrolytic degradation with solid acids having groups has been described. A route to produce hot melt adhesives therefrom has been described. The reaction does not result in complete conversion.
[0015] DE 1240087B describes the work-up of longer-chain ω-amino carboxylic acids, such as ω-aminododecanoic acid.
[0016] Recycling of polyamide 12 by hydrolysis is more technically demanding due to its relatively high stability.
[0017] JP55-108453 A describes the degradation of polyamide 12 by adding water and phosphoric acid during extrusion, but only aims at reducing the molecular weight to a value above that of the monomer. Accordingly, the degradation does not proceed to aminolauric acid.
[0018] DE 693 09 709 T2 describes the hydrolysis and oxidation of polyamides. Possible polyamides are PA6, PA66 and PA12. The reaction is based on the presence of dissolved nitroso groups in the hydrolysis medium.
[0019] DE 3401415 A describes the post-treatment of waste streams from the production of laurolactam. The waste streams consist of a mixture of laurolactam, oligo- and polyamides and further impurities. They can be converted to ω-aminolauric acid by acid- or base-catalyzed hydrolysis.
[0020] It has now been found that the hydrolysis in the process described in DE-A 34 01 415 is facilitated by laurolactam as plasticizer. However, PA12 waste in most cases does not contain laurolactam.
[0021] In addition, US Pat. No. 4,170,588 A describes a method for hydrolyzing polylaurolactam with sulfuric acid at 80° C.
[0022] Accordingly, it was an object of the present invention to provide an improved process for the hydrolysis of polyamide 12 waste.
[0023] A method for solving this problem has now surprisingly been found.
[0024] Brief description of the invention Accordingly, the present invention relates to a method for hydrolyzing polylaurolactam, comprising the steps of: Polylaurolactam is cleaved with sulfuric acid to ω-aminolauric acid at a temperature of 125°C to 190°C, preferably 140°C to 180°C, more preferably 150°C to 170°C, and even more preferably 160°C to 165°C.
[0025] Detailed Description of the Invention It has surprisingly been found that the hydrolysis of polylaurolactam with sulfuric acid proceeds in higher yields than the methods described in the prior art.
[0026] The polylaurolactam used in the method according to the present invention is not particularly limited. Preferably, recyclable materials (PA12 waste) are used.
[0027] The polylaurolactam is especially used as powder, because its hydrolysis can be promoted by increasing surface area.Suitable powdered PA12 is described, for example, in EP 0 911 142 A1.For this purpose, PA12 can be ground into powder by using methods known to those skilled in the art before being used in the method according to the present invention.
[0028] The PA12 used in accordance with the present invention comprises repeat units of structure (I) shown above, where the repeat units ( * The bonds indicated by ( ) are the bonds between adjacent repeat units. ** ) to the bond indicated. Preferably, the PA12 used according to the invention has a molecular weight of 1000 to 10 6 g / mol, preferably 3000 to 200000 g / mol, more preferably 15000 to 150000 g / mol, more preferably 25000 to 120000 g / mol, even more preferably 40000 to 95000 g / mol, more preferably 80000 g / mol.
[0029] In particular, the present invention is suitable for hydrolysis of polylaurolactam with low laurolactam content.Preferably, polylaurolactam is used with laurolactam content of <4.9% by weight, preferably <4.0% by weight, more preferably <3.0% by weight, even more preferably <1.0% by weight, and even more preferably <0.01% by weight, based on the sum of the masses of PA12 and laurolactam, respectively.
[0030] In particular, the present invention is suitable for the hydrolysis of polylaurolactams with a low content of ω-aminolauric acid.Preferably, polylaurolactams are used with a content of ω-aminolauric acid of <4.9% by weight, preferably <4.0% by weight, more preferably <3.0% by weight, even more preferably <1.0% by weight, and even more preferably <0.3% by weight, based on the sum of the masses of PA12 and ω-aminolauric acid, respectively.
[0031] This distinguishes the present process, in particular from the process in DE-A 34 01 415, in which residues from the laurolactam production are hydrolyzed to give a high proportion of laurolactam in the starting material which can be hydrolyzed.
[0032] In contrast, the hydrolysis with sulfuric acid in the process according to the invention is particularly suitable for the use of recyclable materials which are characterized by a low content of laurolactam and ω-aminolauric acid.
[0033] The hydrolysis can be carried out by methods known to those skilled in the art.
[0034] The temperature in the method according to the present invention is from 125°C to 190°C, preferably from 140°C to 180°C, more preferably from 150°C to 170°C, and even more preferably from 160°C to 165°C.
[0035] The pressure in the process according to the invention is preferably in the range from 1 bar to 100 bar, preferably from 10 bar to 60 bar.
[0036] Typically, the polylaurolactam to be hydrolyzed is charged into a reaction vessel, such as an autoclave lined with a precious metal, such as gold or stainless steel, and mixed with the sulfuric acid.
[0037] The sulfuric acid is usually in the form of an aqueous solution, and the content of sulfuric acid in the aqueous solution is not particularly limited.
[0038] The content of sulfuric acid in the aqueous solution is preferably within the range of 10 to 90% by weight, preferably 20 to 80% by weight, more preferably 30 to 50% by weight, and even more preferably 35 to 40% by weight.
[0039] The ratio of sulfuric acid used to polylaurolactam used is not limited.In particular, sulfuric acid is used in such an amount that the weight ratio of sulfuric acid used to PA12 used is within the range of 1:0.1-1:1, preferably within the range of 1:0.2-1:0.8, preferably within the range of 1:0.3-1:0.7, more preferably within the range of 1:0.4-1:0.6, and even more preferably within the range of 1:0.45-1:0.51.
[0040] The process according to the invention is preferably carried out until at least 30% by weight, preferably at least 50% by weight, more preferably at least 70% by weight, even more preferably at least 90% by weight, even more preferably at least 99% by weight of the PA12 used has been reacted.
[0041] In an alternative special embodiment of the process according to the invention, after 1 to 99% by weight, preferably 30 to 90% by weight, preferably 50 to 70% by weight, of the PA12 used has been reacted, an alkali hydroxide is added to neutralize the sulfuric acid (i.e. in particular to adjust the pH to 7 in the reaction mixture), then another alkali hydroxide is added and the remaining PA12 is reacted with this other alkali hydroxide as hydrolysis catalyst.
[0042] As alkali hydroxide, in particular lithium hydroxide, sodium hydroxide or potassium hydroxide, preferably potassium hydroxide, is used.
[0043] In this alternative embodiment, it is taken advantage of the fact that hydrolysis of PA12 with a low content of laurolactam or the very similar ω-aminolauric acid with sulfuric acid works very well. When the PA12 has been degraded to a certain extent, the remaining hydrolytic cleavage can then be carried out in a subsequent step with an alkali hydroxide.
[0044] This further step can then preferably be carried out as described in DE-A 3 4 01 415.
[0045] In particular, the alkali hydroxide is used in such an amount that after neutralization with the sulfuric acid, the weight ratio of unconverted polylaurolactam to the remaining alkali hydroxide is within the range of 1:0.1 to 1:1, preferably within the range of 1:0.2 to 1:0.8, preferably within the range of 1:0.3 to 1:0.7, more preferably within the range of 1:0.4 to 1:0.6, and even more preferably within the range of 1:0.45 to 1:0.51.
[0046] The temperature in the subsequent step is preferably within the range of 160°C to 280°C, preferably 180°C to 250°C, and more preferably 200°C to 230°C.
[0047] The pressure in the subsequent steps is preferably in the range of 1 bar to 100 bar, preferably 10 bar to 60 bar.
[0048] In the subsequent step, the alkali hydroxide is preferably used as an aqueous solution, more preferably at a concentration of 1 to 10% by weight of alkali hydroxide.
[0049] If this further step is carried out, further work-up of the cleaved PA12 can be carried out as described in DE-A 34 01 415.
[0050] The following examples illustrate the invention but do not limit it in any way. EXAMPLES
[0051] The depolymerization of PA12 with contents of laurolactam and ω-aminolauric acid of <1%, respectively, was investigated under various catalyst and temperature conditions.
[0052] The following catalysts were tested: KOH, H2SO4, H3PO4.
[0053] Conversion was determined by the reaction of 1 The carbonyl group was determined by H-NMR.
[0054] The following tests were performed: 1. Comparative test V1: H3PO4, 320℃ 6.66 mg of PA12 powder was placed in a gold-coated autoclave. Then, 6.8 mg of H3PO4 (85%) and 6.30 mg of water were added and the autoclave was sealed. The autoclave was heated to 320°C in an oven and the reaction mixture was kept at this temperature for 4 hours. Then, the mixture was cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 96%.
[0055] 2. Comparative test V2: H3PO4, 300℃ 5.9 mg of PA12 powder was placed in a gold-coated autoclave. Then, 4.25 mg of H3PO4 (85%) and 5.23 mg of water were added and the autoclave was sealed. The autoclave was heated to 300°C in an oven and the reaction mixture was kept at this temperature for 4 hours. Then, the mixture was cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 85%.
[0056] 3. Comparative test V3: H3PO4, 250℃ 7.17 mg of PA12 powder was placed in a gold-coated autoclave. Then, 4.98 mg of H3PO4 (85%) and 6.23 mg of water were added and the autoclave was sealed. The autoclave was heated to 250°C in an oven and the reaction mixture was kept at this temperature for 4 hours. Then, the mixture was cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 88%.
[0057] 4. Comparative test V4: H3PO4, 220℃ 6.95 mg of PA12 powder was placed in a gold-coated autoclave. Then, 4.6 mg of H3PO4 (85%) and 6.30 mg of water were added and the autoclave was sealed. The autoclave was heated to 220°C in an oven and the reaction mixture was kept at this temperature for 4 hours. Then, the mixture was cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 87%.
[0058] 5. Comparative test V5: H3PO4, 200℃ 7.27 mg of PA12 powder was placed in a gold-coated autoclave. 5.43 mg of H3PO4 (85%) and 6.20 mg of water were then added and the autoclave was sealed. The autoclave was heated to 200°C in an oven and the reaction mixture was kept at this temperature for 4 hours. The mixture was then cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 100%.
[0059] 6. Example E1 according to the present invention: H2SO4, 180°C 6.5 mg of PA12 powder was placed in a gold-coated autoclave. 8.62 mg of H2SO4 (35%) was then added and the autoclave was sealed. The autoclave was heated to 180°C in an oven and the reaction mixture was kept at this temperature for 4 hours. The mixture was then cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 100%.
[0060] 7. Example E2 according to the present invention: H2SO4, 160°C 6.61 mg of PA12 powder was placed in a gold-coated autoclave. 8.63 mg of H2SO4 (35%) was then added and the autoclave was sealed. The autoclave was heated to 160°C in an oven and the reaction mixture was kept at this temperature for 4 hours. The mixture was then cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of KOH. The mixture was dried at 80°C and 200 mbar. The conversion of the PA12 was 98%.
[0061] 8. Comparative test V6 (corresponding to DE 3407415 A1): KOH, 320° C. 30.0 g of PA12 powder was placed in a nickel-lined autoclave. Then, 18.95 g of KOH solution (50%) in water was added and the autoclave was sealed. The autoclave was pressurized with nitrogen to 28 bar and heated to 320° C. The reaction mixture was kept at this temperature for 4 hours. Then, the mixture was cooled to room temperature at a rate of 100 K / min and the pressure was released. The reaction mixture was removed from the reactor, dissolved in water and neutralized by adding 13 g of sulfuric acid. The mixture was dried at 70° C. and 100 mbar. The conversion of the PA12 was 94%.
[0062] 9. Comparative test V7 (corresponding to DE 3407415): KOH, 300°C 7.42 mg of PA12 powder was placed in a gold-coated autoclave. 4.03 mg of KOH solution (50%) in water was then added and the autoclave was sealed. The autoclave was heated to 300° C. in an oven. The reaction mixture was kept at this temperature for 4 hours and then cooled to room temperature at a rate of 100 K / min. The mixture was then cooled to room temperature. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of phosphoric acid. The mixture was dried at 70° C. and 100 mbar. The conversion of the PA12 was 78%.
[0063] 10. Comparative test V8 (corresponding to German Patent Application Publication No. 3407415): KOH, 280°C 7.17 mg of PA12 powder was placed in a gold-coated autoclave. 4.42 mg of KOH solution (50%) in water was then added and the autoclave was sealed. The autoclave was heated to 280° C. in an oven. The reaction mixture was kept at this temperature for 4 hours and then cooled to room temperature at a rate of 100 K / min. The mixture was then cooled to room temperature. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of phosphoric acid. The mixture was dried at 70° C. and 100 mbar. The conversion of the PA12 was 78%.
[0064] 11. Comparative test V9 (corresponding to DE 3407415): KOH, 280°C 6.80 mg of PA12 powder was placed in a gold-coated autoclave. 0.95 mg of KOH solution (50%) in water was then added and the autoclave was sealed. The autoclave was heated to 320° C. in an oven. The reaction mixture was kept at this temperature for 4 hours and then cooled to room temperature at a rate of 100 K / min. The mixture was then cooled to room temperature. The reaction mixture was removed from the reactor and neutralized by adding 1 g of water and a stoichiometric amount of phosphoric acid. The mixture was dried at 70° C. and 100 mbar. The conversion of the PA12 was 2%.
[0065] 12. Comparative test V10: No catalyst, 320℃ 7.62 mg of PA12 powder was placed in a nickel-lined autoclave. 3.91 mg of water was then added and the autoclave was sealed. The autoclave was heated to 320° C. in an oven. The reaction mixture was kept at this temperature for 4 hours and then cooled to room temperature at a rate of 100 K / min. The reaction mixture was removed from the reactor and dried at 80° C. and 200 mbar. The conversion of the PA12 was 6%.
[0066] Table 1 below summarizes the results of the tests and comparative tests. Table 1 [Table 1]
[0067] From these results it is clear that the addition of H2SO4 leads to an almost quantitative conversion, especially at low temperatures, i.e. already at 190°C and 160°C.
[0068] 13. Temperature dependence of hydrolysis of PA12 in sulfuric acid To investigate the temperature dependence of the hydrolysis of PA12 in sulfuric acid, the following test series was carried out: PA12 powder and H2SO4 (35%) were added into a gold-lined autoclave in the amounts listed in Table 2 below. The autoclave was then sealed. The autoclave was heated in an oven to the respective temperature T listed in Table 2 below (heating rate 5 K / min) and the reaction mixture was kept at this temperature for 4 hours. The mixture was then cooled to room temperature at a rate of 5 K / min. The residual content of PA12 was then determined.
[0069] Table 2 [Table 2]
[0070] Based on the test results shown in Table 2, it is clear that the hydrolysis of PA12 with sulfuric acid in the temperature range of 125°C to 190°C (E3-E5; E6-E8) proceeds surprisingly efficiently. In comparison, the hydrolysis at a temperature of 80° C. (comparative tests V11, V13) carried out in the prior art (US Pat. No. 4,170,588) is unproductive. Comparative tests V12 and V14 further demonstrate that at a temperature of 230° C. the residual content of PA12 rises again, so that the efficiency of the conversion falls again.
Claims
1. A method for hydrolyzing polylaurolactam, comprising cleaving polylaurolactam with an aqueous solution of sulfuric acid at a temperature of 125° C. to 190° C. to ω-aminolauric acid; the polylaurolactam being a PA12 waste having a laurolactam content of less than 4.9% by weight and / or a ω-aminolauric acid content of less than 4.9% by weight, The content of sulfuric acid in the aqueous solution is within the range of 10 to 90% by weight, and The process wherein the weight ratio of sulfuric acid used to polylaurolactam used is in the range of 1:0.1 to 1:
1.
2. The polylaurolactam is 1000 to 10 6 The method of claim 1 , wherein the cation exchange copolymer has a molar mass in g / mol.
3. 3. The process according to claim 1 or 2, wherein the pressure is between 1 bar and 100 bar.
4. 4. The method according to claim 1, wherein after 1 to 99% by weight of the polylaurolactam used has been reacted, an alkali hydroxide is added to neutralize the sulfuric acid, and then another alkali hydroxide is added to react the remaining polylaurolactam with the other alkali hydroxide.
5. The method according to claim 4, wherein an alkali hydroxide is used in a subsequent step in such an amount that after neutralization of the sulfuric acid, the alkali hydroxide remains in an amount such that the weight ratio of unconverted polylaurolactam to the remaining alkali hydroxide is in the range of 1:0.1 to 1:
1.
6. 6. The method according to claim 4 or 5, wherein the temperature in the subsequent step is in the range of 160°C to 280°C.
7. 7. The method according to claim 4, wherein the pressure in the subsequent step is in the range of 1 to 100 bar.
Citation Information
Patent Citations
JP1973075544A
Method of stabilizing selected molding or nonnmolding plastics
JP1978028642A
Crystalline polyester amide copolymer and its production
JP1984102924A
Production of fine particle of crude polyamide copolymer