Method for evaluating heat-resistant adhesion
The method of impregnating tire cords with an adhesive composition and using micro-XAFS measurement for penetration thickness calculation addresses the inefficiencies of existing adhesion evaluation methods, providing a quick and accurate assessment of heat-resistant adhesion for tire performance.
Patent Information
- Application Number
- JP2020216858
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-25
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Existing methods for evaluating heat-resistant adhesion between tire cords and rubber compositions are time-consuming, costly, and require significant man-hours, making them inefficient for tire performance assessment.
A method involving impregnating a tire cord with an adhesive composition, preparing a cross-sectional sample, and using micro-XAFS measurement to calculate the penetration thickness of the adhesive composition through X-ray absorption coefficient mapping, allowing for quantitative evaluation of heat-resistant adhesion.
Enables simple and quantitative assessment of heat-resistant adhesion without complex tests, improving the evaluation efficiency and correlating well with traditional peel tests, thereby enhancing tire development.
Smart Images

Figure 0007571540000004 
Figure 0007571540000005 
Figure 0007571540000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for evaluating heat-resistant adhesion between a tire cord and a rubber composition. [Background technology]
[0002] The heat-resistant adhesion of tire cords in rubber is very important for maintaining tire performance such as durability. To date, methods have been used to evaluate such heat-resistant adhesion, such as performing a drum durability test after tire molding, or performing a peel test using a test piece in which an organic fiber cord and rubber are vulcanized together. However, these methods have the problem of requiring test man-hours and test time, which are costly.
[0003] Patent Document 1 describes a method for easily evaluating the decrease in interfacial adhesive strength of a tire cord-rubber composite by reproducing the destruction mode of a tire on a laboratory scale. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-2780 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method for easily evaluating the heat-resistant adhesion between a tire cord and a rubber composition. [Means for solving the problem]
[0006] As a result of extensive investigations, the present inventors have found that it is possible to simply and quantitatively evaluate the heat-resistant adhesion between a tire cord and a rubber composition by impregnating a tire cord with an adhesive composition and measuring the penetration depth by a prescribed method, and have thus completed the present invention.
[0007] That is, the present invention provides [1] A method for evaluating heat-resistant adhesion between a tire cord and a rubber composition, comprising: a cross-sectional sample preparation step of impregnating a tire cord with an adhesive composition and cutting the impregnated product at a predetermined thickness to prepare a cross-sectional sample for evaluation; and a penetration depth calculation step of calculating a penetration thickness of the adhesive composition from a surface of the tire cord for the cross-sectional sample obtained by the cross-sectional sample preparation step, [2] The evaluation method according to [1], wherein the cross-sectional sample preparation step includes an embedding preparation step of embedding the impregnated material in a resin before cutting the impregnated material, and the cutting of the embedded material is performed perpendicular to the length direction of the cord; the penetration thickness calculation step includes a stack image acquisition step of acquiring a series of X-ray absorption coefficient mapping images of the cross-sectional sample by a micro-XAFS measurement device while changing the photon energy of X-rays in a region near the absorption edge of the element of interest; an adhesive composition image preparation step of acquiring an X-ray absorption coefficient mapping image of the adhesive composition from the stack image by performing singular value decomposition using the XAFS spectra of the tire cord, the adhesive composition, and the resin for embedding the cord as standard spectra; and an adhesive composition image analysis step of calculating the penetration thickness of the adhesive composition from the surface of the tire cord from the adhesive composition image. [3] The evaluation method according to [2], further comprising an analysis region selection step between the cross-sectional sample preparation step and the stack image acquisition step, in which the cross-sectional sample is spatially scanned with a micro-XAFS measurement device by fixing the photon energy of X-rays in a region near the absorption edge of an element of interest, thereby obtaining an X-ray absorption coefficient mapping image at the photon energy, and selecting an area where the absorption intensity of the adhesive composition is strong from the X-ray absorption coefficient mapping image as an analysis region. [4] The evaluation method according to [3], wherein the micro-XAFS measurement device used in the analysis area determination step and the stack image acquisition step is an STXM. [5] The brightness of the X-rays in the analysis area determination step and the stack image acquisition step is 10 10 (photons / s / mrad2 / mm 2 / 0.1% bw) or more, [6] The evaluation method according to any one of [3] to [5], wherein in the analysis area determination process and the stack image acquisition process, the element of interest is at least one selected from the group consisting of carbon, oxygen, and nitrogen. Effect of the Invention
[0008] According to the present invention, the heat-resistant adhesion between a tire cord and a rubber composition can be evaluated simply and quantitatively without carrying out complicated peel tests, drum durability tests, or the like. [Brief description of the drawings]
[0009] [Figure 1] This is an X-ray absorption coefficient mapping image of a cross-sectional sample of Code 1 obtained by irradiating it with a 287 eV X-ray microbeam. [Diagram 2] This is a standard XAFS spectrum of the embedding resin near the carbon K absorption edge. [Diagram 3] 1 is a standard XAFS spectrum of adhesive composition 1 near the carbon K absorption edge. [Figure 4] This is the PET code's standard XAFS spectrum near the carbon K absorption edge. [Diagram 5] 1 shows X-ray absorption coefficient mapping images of (a) the embedding resin, (b) adhesive composition 1, (C) the PET code, and (d) the above three components after singular value decomposition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The method of evaluating heat-resistant adhesion between a tire cord and a rubber composition disclosed herein includes a cross-sectional sample preparation step of impregnating a tire cord with an adhesive composition and cutting the impregnated product at a predetermined thickness to prepare a cross-sectional sample for evaluation; and a penetration depth calculation step of calculating the penetration thickness of the adhesive composition from the tire cord surface for the cross-sectional sample obtained in the cross-sectional sample preparation step.
[0011] Preferably, the cross-sectional sample preparation step includes an embedment preparation step of embedding the impregnated material in a resin before cutting the impregnated material, and the cutting of the embedded material is performed perpendicular to the length direction of the cord; the penetration thickness calculation step includes a stack image acquisition step of acquiring a series of X-ray absorption coefficient mapping images of the cross-sectional sample by a micro-XAFS measurement device while changing the photon energy of X-rays in a region near the absorption edge of the element of interest; an adhesive composition image preparation step of acquiring an X-ray absorption coefficient mapping image of the adhesive composition from the stack image by performing singular value decomposition using the XAFS spectra of the tire cord, the adhesive composition, and the resin for embedding the cord as standard spectra; and an adhesive composition image analysis step of calculating the penetration thickness of the adhesive composition from the surface of the tire cord from the adhesive composition image.
[0012] More preferably, between the cross-sectional sample preparation step and the stack image acquisition step, the method further includes an analysis region selection step of: fixing the photon energy of X-rays in a region near the absorption edge of an element of interest using a micro-XAFS measurement device, spatially scanning the cross-sectional sample to obtain an X-ray absorption coefficient mapping at that photon energy, and selecting, from the X-ray absorption coefficient mapping image, a region where the absorption intensity by the adhesive composition is strong as an analysis region.
[0013] The analysis area selected in the analysis area selection step is preferably an area including filaments located inside the second layer counting from the outside among the filaments constituting the tire cord.
[0014] The micro-XAFS measurement device used in the analysis region determining step and the stack image acquiring step is preferably an STXM.
[0015] The intensity of the X-rays in the analysis region determination step and the stack image acquisition step is 10 10 (photons / s / mrad 2 / mm2 / 0.1%bw) or more is preferable.
[0016] In the analysis region determining step and the stack image acquiring step, the element of interest is preferably at least one selected from the group consisting of carbon, oxygen, and nitrogen.
[0017] The heat-resistant adhesion evaluation method according to one embodiment of the present disclosure will be described in detail below. However, the following description is an example for explaining the present disclosure, and is not intended to limit the technical scope of the present invention to the described range. In this specification, when a numerical range is indicated using "~", the numerical range includes both ends of the range.
[0018] <Cross-section sample preparation process> This is a process in which a tire cord is impregnated with an adhesive composition, and the impregnated product is cut to a predetermined thickness to prepare a cross-sectional sample for evaluation.
[0019] (Production of tire cord) The tire cord is not particularly limited as long as it is generally usable in the tire industry, and examples thereof include organic fiber cord, glass fiber cord, steel cord, etc. The material of the organic fiber cord is not particularly limited, but thermoplastics are preferred. Thermoplastics include polyamide, polyester, polyolefins such as polypropylene and polyethylene, polycarbonate, polyacrylate, styrene resins such as ABS resin, vinyl chloride resin, etc., and polyamide and polyester are preferred. The steel cord includes single-twist steel cords with a 1×n configuration, layer-twist steel cords with a k+m configuration, etc. (n is an integer of 1 to 27, k is an integer of 1 to 10, m is an integer of 1 to 3, etc.).
[0020] The adhesive composition is not particularly limited as long as it can be used to bond tire cords and rubber, and examples thereof include epoxy compounds, blocked isocyanates, resorcinol-formaldehyde latex (RFL), p-chlorophenol-resorcinol-formaldehyde condensates, allylhydroxyphenyl ether-resorcinol-formaldehyde condensates, and mixtures thereof. The tire cords are impregnated with the adhesive composition by a known method.
[0021] Drying after impregnating the tire cord with the adhesive composition is carried out by a known method. The drying temperature is usually 120 to 300° C., and preferably 150 to 250° C. The drying time is usually 1 to 10 minutes, and preferably 2 to 5 minutes.
[0022] (Preparation of cross-sectional samples) A cord piece having a thickness of about several mm (preferably about 5 to 10 mm) containing the adhesive composition impregnated into a tire cord is cut out, the cord piece is embedded in a resin, and the embedded material is cut with a cryomicrotome perpendicularly to the length direction of the cord at a predetermined thickness to obtain a cross-sectional sample. The cord piece may be not only one cut out from a tire cord impregnated with the adhesive composition, but also one cut out from a tire cord-rubber composite in which a tire cord impregnated with the adhesive composition is embedded in unvulcanized rubber and vulcanized to integrate the tire cord and rubber.
[0023] <Penetration thickness calculation process> This is a step of calculating the penetration depth of the adhesive composition from the tire cord surface for the cross-sectional sample obtained by the cross-sectional sample preparation step. Although the method for measuring the penetration depth is not particularly limited, in the present disclosure, a method for calculating the penetration depth using a micro-XAFS measurement device will be described below.
[0024] (Micro-XAFS measurement) The cross-sectional sample is held on a TEM grid and subjected to micro-XAFS measurement. Examples of micro-XAFS measurement devices include a scanning transmission X-ray microscope (STXM) and an X-ray photoemission electron microscope (XPEEM). From the viewpoint of preventing damage to the sample by X-rays, an STXM is preferred. The brightness of the X-rays is 10 10 (photons / s / mrad 2 / mm 2 / 0.1%bw) or more is preferable, and 10 12 (photons / s / mrad 2 / mm 2 / 0.1%bw) or more is more preferable, and 10 14 (photons / s / mrad 2 / mm 2 / 0.1% bw) or more is more preferable. If the sample is sensitive to X-ray damage, the X-ray damage can be reduced by, for example, cooling the sample to -80°C or lower during micro-XAFS measurement.
[0025] The STXM method is a technique for measuring the amount of X-ray absorption in a micro-area and performing two-dimensional mapping of the near edge X-ray absorption fine structure (NEXAFS) by simultaneously measuring the incident light and the light (transmitted light) that has passed through the sample while scanning a slice-shaped sample with high-intensity X-rays focused by a zone plate. It is possible to perform chemical state analysis of various elements with a spatial resolution of up to several tens of nm, and is particularly suitable for mapping elements or chemical states such as carbon, nitrogen, and oxygen that have an absorption edge in the soft X-ray region. The range of photon energy of the irradiated X-ray can be appropriately selected depending on the element of interest. For example, in the case of organic materials, the photon energy of the carbon K-absorption edge region (about 280 to 320 eV) and the photon energy of the oxygen K-absorption edge region (about 520 to 570 eV) are preferably selected for measurement, but are not limited thereto.
[0026] (Analysis area selection process) The cross-sectional sample is subjected to a micro-XAFS measurement device, in a region near the absorption edge of the chemical state (element, functional group, or compound) of interest in the adhesive composition, with the photon energy of the irradiated X-ray fixed, and a certain range (for example, a region of 20 to 50 μm square) on the cross-sectional sample is spatially scanned to obtain a distribution image of the X-ray absorption coefficient at the photon energy (X-ray absorption coefficient mapping image). From the obtained X-ray absorption coefficient mapping image, a region where the amount of X-ray absorption by the adhesive composition is large is selected as an analysis region. For example, in the examples described later, FIG. 1 is an example of an X-ray absorption coefficient mapping image. In FIG. 1, the black region indicated by 1 is a region where the amount of X-ray absorption by the adhesive composition is large. Also, the round region indicated by 2 is a filament. The analysis region is preferably a region including filaments inside the second layer counting from the outside among the filaments constituting the tire cord. This is because there is a tendency that a better evaluation of heat-resistant adhesion can be performed.
[0027] (Stack image acquisition process) Using a micro-XAFS measurement device, the cross-sectional sample is spatially scanned within a selected analysis region in the vicinity of the absorption edge of the element of interest (preferably carbon) with a fixed photon energy of irradiated X-rays, thereby obtaining an X-ray absorption coefficient mapping image at that photon energy. Next, while changing the photon energy of the X-rays in the vicinity of the absorption edge of the element of interest, for example, at intervals of 0.1 to 1.0 eV, an X-ray absorption coefficient mapping image at each photon energy is obtained in the same manner as above. In this way, a set of X-ray absorption coefficient mapping images (stack images) at a series of photon energies is obtained.
[0028] (Adhesive composition image preparation process) From the obtained stack image, singular value decomposition is performed using the XAFS spectra of the tire cord, adhesive composition, and embedding resin as standard spectra to obtain X-ray absorption coefficient mapping images of the tire cord, adhesive composition, and embedding resin, respectively. Among these, the X-ray absorption coefficient mapping image of the adhesive composition is used in the next step. The standard spectrum may be obtained in advance for each of the tire cord, adhesive composition, and embedding resin using a micro-XAFS measurement device, or the standard spectrum of the tire cord, adhesive composition, and embedding resin may be extracted from a characteristic region of the stack image, respectively.
[0029] (Adhesive composition image analysis process) The singular value decomposed X-ray absorption coefficient mapping image of the adhesive composition is stored with a scale bar, and the penetration thickness of the adhesive composition impregnated into the cord portion is calculated using image analysis software. Specifically, the line connecting the points where the absorption intensity (brightness) in the X-ray absorption coefficient mapping image is the tire cord surface, and the perpendicular direction of the line is the thickness direction of the tire cord. The distance from any point on the line representing the tire cord surface to the point where the brightness is zero is the penetration thickness of the adhesive composition impregnated into the cord portion, and the maximum and minimum values are measured. The penetration thickness can be measured with higher accuracy by selecting multiple analysis areas and averaging them.
[0030] The minimum value of the penetration thickness is preferably 90 nm or more, more preferably 95 nm or more, and even more preferably 100 nm or more. When the minimum value of the penetration thickness is within the above range, the heat resistant adhesion between the tire cord and the rubber composition can be evaluated as being good.
[0031] The difference between the maximum and minimum values of the penetration thickness is preferably 50 nm or less, more preferably 40 nm or less, and even more preferably 30 nm or less. When the difference between the maximum and minimum values of the penetration thickness is within the above range, the thickness unevenness is small, and the heat-resistant adhesion between the tire cord and the rubber composition can be evaluated as being good. EXAMPLES
[0032] The present disclosure will be described based on examples, but the present disclosure is not limited to only the examples.
[0033] The various chemicals used in the Examples and Comparative Examples are listed below. Note that the various chemicals were purified according to conventional methods as necessary. Adhesive composition 1: An adhesive made by mixing an aliphatic epoxy resin with a viscosity of 150 (mPa·s) and a blocked isocyanate Adhesive composition 2: Adhesive made by mixing an aliphatic epoxy resin with a viscosity of 5000 (mPa·s) and a blocked isocyanate Adhesive composition 3: Adhesive made by mixing an aliphatic epoxy resin with a viscosity of 2600 (mPa·s) and a blocked isocyanate NR:TSR20 BR: BR150B manufactured by Ube Industries, Ltd. Carbon black: Show Black N351 manufactured by Cabot Japan Co., Ltd. Oil: Process oil X-140 manufactured by ENEOS Corporation Anti-aging agent: Nocrac 6C (N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Wax: Ozoace 355 manufactured by Nippon Seiro Co., Ltd. Zinc oxide: "Ginrei R" manufactured by Toho Zinc Co., Ltd. Stearic acid: Beads of stearic acid camellia manufactured by NOF Corporation Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. (Powdered sulfur containing 5% oil) Vulcanization accelerator: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0034] (Example) <Production of tire cord> A PET cord having 110 dtex / 2, cord diameter 0.54 nm and twist number 48 was dipped into the above adhesive compositions 1 to 3, dried at 150° C. for 2 minutes, and then heat-treated at 240° C. for 2 minutes to prepare cords 1 to 3, respectively.
[0035] <Preparation of Code Cross-Section Specimens> For Codes 1 to 3, code pieces with a thickness of about 5 to 10 mm, including the adhesive composition impregnated in the code, were cut out. After each code piece was embedded in an embedding resin, the embedded material was cut at a thickness of 200 nm perpendicular to the code length direction using a cryomicrotome. The cross-section specimens of the cut Codes 1 to 3 were mounted on a Cu grid for TEM.
[0036] <STXM Measurement> Under the following conditions, STXM measurements were performed on the PET code before the impregnation step, the adhesive composition, the embedding resin, and the cross-section specimens of Codes 1 to 3. (Measurement Location) Extreme Ultraviolet Light Research Facility BL4U, Institute for Molecular Science, National Institutes of Natural Sciences (Measurement Conditions) X-ray Luminance: 1×10 16 (photons / s / mrad 2 / mm 2 / 0.1%bw) Spectrometer: Grating (Measurement Energy) 282 to 294 eV (Carbon K Absorption Edge Region) (STXM Measurement Data Analysis Software) aXis2000 (Free Software)
[0037] First, the XAFS standard spectra in the vicinity of the carbon K-shell absorption edge of the embedding resin, Adhesive Compositions 1 to 3, and the PET code before impregnation with the adhesive composition were measured respectively (Figures 2, 3, and 4).
[0038] The cross-section specimens of Codes 1 to 3 were irradiated with an X-ray microbeam of 287 eV to obtain an X-ray absorption coefficient mapping image for selecting the analysis region. Figure 1 shows the X-ray absorption coefficient mapping image of the cross-section specimen of Code 1. Among the filaments constituting the tire code, the region including the filaments inside the second layer from the outside, which includes the region with a large X-ray absorption amount due to the adhesive composition in the X-ray absorption coefficient mapping image (the black region in Figure 1), was selected as the analysis region.
[0039] Next, the cross-sectional samples of codes 1 to 3 were irradiated with an X-ray microbeam at a fixed energy of 287 eV within the selected analysis area to obtain X-ray absorption coefficient mapping images. Furthermore, X-ray microbeams were irradiated while changing the photon energy in 0.2 eV intervals in the range of 282 to 294 eV to obtain X-ray absorption coefficient mapping images in the same manner, and these sets were used as stack images.
[0040] Singular value decomposition was performed using the obtained stack image and the standard spectrum to obtain X-ray absorption coefficient mapping images of the embedding resin, adhesive compositions 1 to 3, and the PET code. In Fig. 5, (a) shows the X-ray absorption coefficient mapping image of the embedding resin, (b) the X-ray absorption coefficient mapping image of adhesive composition 1, (c) the X-ray absorption coefficient mapping image of the PET code, and (d) shows the X-ray absorption coefficient mapping image in which the three components are color-coded.
[0041] The singular value decomposed X-ray absorption coefficient mapping images of adhesive compositions 1 to 3 were stored with a scale bar, and the penetration thickness of adhesive compositions 1 to 3 impregnated into cords 1 to 3 was calculated using image analysis software. Specifically, the line connecting the points where the absorption intensity (brightness) in the X-ray absorption coefficient mapping images was the tire cord surface, and the perpendicular direction of the line was the thickness direction of the tire cord. The distance from any point on the line representing the tire cord surface to the point where the brightness was zero was taken as the penetration thickness of the adhesive composition impregnated into the cord portion, and the maximum and minimum values were measured. The penetration thickness was calculated by selecting 3 to 4 analysis areas and averaging them. The results are shown in Table 1.
[0042] [Table 1]
[0043] (Comparative Example) <Preparation of tire cord-rubber composite test specimens> According to the formulation shown in Table 2, materials other than sulfur and vulcanization accelerator were filled in a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. so that the filling rate was 58%, and kneaded at 80 rpm until the temperature reached 140°C. Sulfur and vulcanization accelerator were added to the obtained kneaded product, and the mixture was kneaded for 5 minutes under the condition of 80°C using a two-axis open roll to obtain an unvulcanized rubber composition. The amount of sulfur in Table 2 indicates the amount of insoluble sulfur (sulfur content + oil content). Rubber sheets were prepared from the obtained unvulcanized rubber composition, and the above-mentioned cords 1 to 3 were covered from above and below with the rubber sheets, and press-vulcanized at 140°C for 40 minutes to obtain tire cord-rubber composite test pieces of Comparative Examples 1 to 3.
[0044] [Table 2]
[0045] <Moisture and heat deterioration and peeling test> In accordance with JIS K 7277:1998 "Plastics - Method for measuring the effect of exposure to moist heat, water spray and salt mist", each tire cord-rubber composite test piece of Comparative Examples 1 to 3 was subjected to moist heat aging for 150 hours under conditions of a temperature of 80°C and a humidity of 95%, and a peel test was performed in accordance with the method described in 2.4.4 of "Improvement of adhesion of PET tire cord fibers by low-temperature plasma treatment" in the Journal of the Society of Rubber Science and Technology of Japan, Vol. 63, No. 4 (1990), and the rubber coverage rate after peeling (the rate of rubber coverage on the peeled surface when the fiber cord and rubber are peeled) was measured visually. The adhesive strength was evaluated according to the following criteria, and a higher score indicates better heat-resistant adhesiveness. [Evaluation Criteria] 5 points: 100% rubber coverage on the peeled surface 4 points: Rubber coverage on the peeled surface is 75% or more but less than 100% 3 points: Rubber coverage on the peeled surface is 50% or more but less than 75% 2 points: Rubber coverage on the peeled surface is 25% or more but less than 50% 1 point: Rubber coverage on peeled surface is over 0% and less than 25% 0 points: 0% rubber coverage on the peeled surface
[0046] [Table 3]
[0047] From the results of Tables 1 and 3, it can be seen that the larger the minimum penetration thickness of the adhesive composition measured by the evaluation method of the present disclosure, and the smaller the difference between the maximum and minimum penetration thicknesses, the more improved the heat-resistant adhesion in the peel test, and that the evaluation method of the present disclosure correlates well with the evaluation of heat-resistant adhesion in the peel test. It can also be seen that the evaluation method of the present disclosure is excellent for quantitative evaluation of heat-resistant adhesion. [Industrial Applicability]
[0048] According to the present invention, it is possible to simply and quantitatively evaluate the heat-resistant adhesion between a tire cord and a rubber composition without carrying out complicated peel tests, drum durability tests, etc. Therefore, the present invention is useful in promoting the development of tires with improved heat-resistant adhesion. [Explanation of symbols]
[0049] 1 Region where the amount of X-ray absorption by the adhesive composition is large 2 Filaments
Claims
1. A method for evaluating heat resistance adhesion between a tire cord and a rubber composition, comprising the steps of: a cross-sectional sample preparation step of impregnating a tire cord with the adhesive composition and cutting the impregnated product at a predetermined thickness to prepare a cross-sectional sample for evaluation; and The evaluation method includes a penetration depth calculation step of calculating a penetration depth of the adhesive composition from a tire cord surface for the cross-sectional sample obtained in the cross-sectional sample preparation step.
2. The cross-sectional sample preparation step includes an embedding preparation step of embedding the impregnated object in a resin before cutting the impregnated object, and the cutting of the embedded object is performed perpendicular to the length direction of the cord; a stack image acquisition step of acquiring a series of X-ray absorption coefficient mapping images of the cross-sectional sample by a micro-XAFS measurement device while changing the photon energy of X-rays in a region near the absorption edge of the element of interest, in the penetration thickness calculation step; An adhesive composition image preparation step of performing singular value decomposition from the stack image using the XAFS spectra of the tire cord, the adhesive composition, and the resin for embedding the cord as standard spectra to obtain an X-ray absorption coefficient mapping image of the adhesive composition; and The evaluation method according to claim 1 , further comprising an adhesive composition image analysis step of calculating a penetration depth of the adhesive composition from a tire cord surface based on the adhesive composition image.
3. 3. The evaluation method according to claim 2, further comprising, between the cross-sectional sample preparation step and the stack image acquisition step, an analysis region selection step of: using a micro-XAFS measurement device to fix the photon energy of X-rays in a region near the absorption edge of an element of interest, spatially scan the cross-sectional sample, and obtain an X-ray absorption coefficient mapping image at the photon energy, and select a region where absorption intensity by the adhesive composition is strong from the X-ray absorption coefficient mapping image as an analysis region.
4. 4. The evaluation method according to claim 3, wherein the micro-XAFS measurement device used in the analysis area determination step and the stack image acquisition step is an STXM.
5. The brightness of the X-rays in the analysis region determination step and the stack image acquisition step is 10 10 (photons / s / mrad 2 / mm 2 5. The method according to claim 3, wherein the solubility of the cellulose acetate layer is 0.1% bw or more.
6. The evaluation method according to any one of claims 3 to 5, wherein the element of interest in the analysis area determination step and the stack image acquisition step is at least one selected from the group consisting of carbon, oxygen, and nitrogen.
Citation Information
Patent Citations
Tire cord and tire using the same
JP2010024601A
Adhesion state evaluation method of rubber wire complex, and rubber wire complex and pneumatic tire
JP2018189455A
Determination method of adhesion state, metal-rubber composite, pneumatic tire, and manufacturing method of pneumatic tire
JP2018189595A
Evaluation method of interfacial adhesion force