Electrode for enzyme sensor and enzyme sensor

The use of a carbon-based electrode with a thickness of 15 μm or less and density of 1.4 g/cm³ addresses the sensitivity and cost issues of enzyme sensors, providing a low-noise and robust solution for enzyme sensors.

JP7571658B2Active Publication Date: 2024-10-23TOYO INK MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021078325
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-06
Publication Date
2024-10-23
Estimated Expiration
2041-05-06

AI Technical Summary

Technical Problem

Existing enzyme sensors suffer from insufficient measurement sensitivity and high cost due to the use of expensive metals, and there is a need for electrodes with improved strength and reduced noise.

Method used

The electrode for enzyme sensors is composed of a working electrode with a carbon material and an aqueous resin, having a thickness of 15 μm or less and a density of 1.4 g/cm³, primarily using graphite for conductivity and cost-effectiveness.

Benefits of technology

This configuration results in an enzyme sensor electrode with low noise and high strength, enabling low-cost disposable electrodes with enhanced sensitivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571658000001
    Figure 0007571658000001
Patent Text Reader

Abstract

To provide an electrode for an enzyme sensor, that is superior in sensitivity with respect to noise of the electrode and that has high intensity, and to provide an enzyme sensor.SOLUTION: Provided is an electrode for an enzyme sensor, and an enzyme sensor using the electrode for an enzyme sensor. In the electrode for an enzyme sensor having an action electrode and a counter electrode, the action electrode comprises a carbon material and aqueous resin. Thickness of the action electrode is 15 μm or less and density is 1.4 g / cm3 or more in the electrode for an enzyme sensor. Further, in the electrode for an enzyme sensor, the carbon material contains at least black lead, and a content of the carbon material is 60 mass% or more in 100 mass% of the action electrode.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode for an enzyme sensor and an enzyme sensor. [Background technology]

[0002] Enzyme sensors that can easily measure specific components contained in biological samples such as blood and sweat, foods, cell culture media, etc., have been put to practical use. For example, there is a blood glucose sensor that detects or quantifies glucose in blood by electrochemical means. In this sensor, the glucose contained in blood is selectively oxidized by the substrate specificity of the enzyme, and a current is generated when a charge reaches an electrode via a mediator or directly, and the glucose concentration can be quantified from the current value. The electrode part of the enzyme sensor in practical use may have a metal layer formed by sputtering, plating, or the like (for example, Patent Document 1). However, the measurement sensitivity is still far from sufficient, and not using expensive metals is preferable from the viewpoints of corrosion and cost. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-045877 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide an electrode for an enzyme sensor and an enzyme sensor which are excellent in sensitivity to electrode noise and have high strength. [Means for solving the problem]

[0005] The present inventors conducted extensive research to solve the above-mentioned problems and arrived at the present invention. That is, the present invention provides an electrode for an enzyme sensor having at least a working electrode and a counter electrode disposed on a substrate, the working electrode including at least a carbon material and an aqueous resin, and the working electrode having a thickness of 15 μm or less and a density of 1.4 g / cm 3 The present invention relates to the above-mentioned enzyme sensor electrode.

[0006] The present invention also relates to the electrode for an enzyme sensor, wherein the carbon material contains at least graphite.

[0007] The present invention also relates to the above-mentioned electrode for an enzyme sensor, wherein the carbon material contained in the working electrode is 60% or more.

[0008] The present invention also relates to an enzyme sensor using the enzyme sensor electrode. Effect of the Invention

[0009] According to the present invention, in a working electrode containing a carbon material and an aqueous resin, a film thickness of 15 μm or less and a density of 1.4 g / cm 3 In this way, an enzyme sensor electrode with less noise and excellent strength can be provided. Furthermore, since the electrode is mainly made of a carbon material, a disposable electrode can be provided at low cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (Carbon materials) The carbon material in the present invention is not particularly limited, and examples thereof include graphite, carbon black, conductive carbon fibers (carbon nanotubes, carbon nanofibers, carbon fibers), graphene, fullerene, etc., which can be used alone or in combination of two or more. It is preferable to use at least graphite as the carbon material from the viewpoints of conductivity and cost.

[0011] Examples of graphite include artificial graphite and natural graphite. Artificial graphite is obtained by artificially orienting irregularly arranged micrographite crystals by heat treatment of amorphous carbon, and is generally produced using petroleum coke or coal-based pitch coke as the main raw material. As natural graphite, flake graphite, spherical graphite, scaly graphite, lump graphite, earthy graphite, etc. can be used. In addition, expanded graphite (also called expandable graphite) obtained by chemically treating scaly graphite, and expanded graphite obtained by heat treating expanded graphite to expand it and then refining or pressing it can also be used. Among these graphites, natural graphite is preferred from the viewpoint of electrical conductivity, and spherical graphite, scaly graphite, expanded graphite, and flake graphite are preferred.

[0012] The average particle size of the graphite used is preferably 0.5 to 500 μm, and particularly preferably 2 to 100 μm.

[0013] The average particle size in the present invention refers to the particle size (D50) at which the volume ratio of particles is 50% when the volume ratio of particles is accumulated from the finest particle size in the volume particle size distribution, and is measured with a general particle size distribution meter, for example, a dynamic light scattering type particle size distribution meter ("Microtrac UPA" manufactured by Nikkiso Co., Ltd.).

[0014] Examples of commercially available graphite include flake graphite such as CMX, UP-5, UP-10, UP-20, UP-35N, CSSP, CSPE, CSP, CP, CPB, UCP, J-CPB, CB-150, CB-100, ACP, ACP-1000, ACB-50, ACB-100, ACB-150, SP-10, SP-20, SP-5030, J-SP, SP-270, HOP, GR-60, LEP, F#1, F#2, and F#3 manufactured by Nippon Graphite Industries Co., Ltd., and CX-3000, FBF, BF, CBR, SSC-3000, and SSC-600 manufactured by Chuetsu Graphite Co., Ltd. , SSC-3, SSC, CX-600, CPF-8, CPF-3, CPB-6S, CPB, 96E, 96L, 96L-3, 90L-3, CPC, S-87, K-3, CF-80, CF-48, CF-32, CP-150, CP-100, CP, HF-80, HF-48, HF-32, SC-120, SC-80, SC-60, SC-32, CNP15, CNP7, Z-5F, EC1500, EC1000, EC500, EC300, EC100, EC50 manufactured by Ito Graphite Industries Co., Ltd., 10099M, PB-99 manufactured by Nishimura Graphite Co., Ltd., etc. Examples of spherical natural graphite include CGC-20, CGC-50, CGB-20, and CGB-50 manufactured by Nippon Graphite Industries Co., Ltd. Examples of amorphous graphite include Blue P, AP, AOP, and P#1 manufactured by Nippon Graphite Industries Co., Ltd., and APR, S-3, AP-6, and 300F manufactured by Chuetsu Graphite Co., Ltd. Examples of artificial graphite include PAG-60, PAG-80, PAG-120, PAG-5, HAG-10W, and HAG-150 manufactured by Nippon Graphite Industries Co., Ltd., RA-3000, RA-15, RA-44, GX-600, G-6S, G-3, G-150, G-100, G-48, G-30, and G-50 manufactured by Chuetsu Graphite Co., Ltd., and SGP-100, SGP-50, SGP-25, SGP-15, SGP-5, SGP-1, SGO-100, SGO-50, SGO-25, SGO-15, SGO-5, SGO-1, SGX-100, SGX-50, SGX-25, SGX-15, SGX-5, and SGX-1 manufactured by SEC Carbon Co., Ltd. These can be used alone or in combination of two or more kinds.

[0015] The larger the specific surface area of ​​the graphite used, the larger the area in which the electrochemical reaction occurs, which is advantageous for increasing sensitivity. Specifically, the specific surface area (BET) calculated from the amount of nitrogen adsorption is preferably 1 m 2 / g or more, more preferably 5m 2 It is preferable to use a material with a specific surface area of ​​1 m 2 If graphite with a refractive index below 300m / g is used, it may be difficult to obtain sufficient sensitivity. 2 Graphite with a molecular weight exceeding 1.0 / g may be difficult to obtain as a commercially available material.

[0016] The content of graphite in the total of 100% by mass of the carbon materials is preferably 25 to 99% by mass, and more preferably 50 to 96% by mass. Although there are no particular limitations on the carbon material other than graphite, it is preferable to use carbon black or conductive carbon fiber from the viewpoints of cost, conductivity, and the like.

[0017] Carbon black can be produced by continuously pyrolyzing a gaseous or liquid raw material in a reactor, particularly ketjen black made from ethylene heavy oil, channel black made by burning raw material gas and quenching and precipitating the flame by hitting the bottom surface of a channel steel, thermal black made from gas by periodically repeating combustion and pyrolysis, particularly acetylene black made from acetylene gas, etc. Carbon black that has been subjected to a commonly used oxidation treatment, hollow carbon, etc. can also be used. Carbon oxidation is a process in which oxygen-containing polar functional groups such as phenol groups, quinone groups, carboxyl groups, and carbonyl groups are directly introduced (covalently bonded) to the carbon surface by treating the carbon at high temperatures in air or secondary treatment with nitric acid, nitrogen dioxide, ozone, etc., and is generally carried out to improve the dispersibility of carbon. However, since the electrical conductivity of carbon generally decreases as the amount of functional groups introduced increases, it is preferable to use carbon that has not been subjected to oxidation treatment.

[0018] The larger the specific surface area of ​​the carbon black used, the more contact points there are between the carbon black particles, which is advantageous for lowering the internal resistance of the electrode. Also, the larger the specific surface area, the larger the area in which electrochemical reactions occur, which is advantageous for increasing sensitivity. Specifically, the specific surface area (BET) calculated from the amount of nitrogen adsorption is preferably 210 m 2 It is preferable to use a material with a specific surface area of ​​210 m 2 If carbon black with a conductivity below 1500m / g is used, it may be difficult to obtain sufficient conductivity. 2 Carbon black exceeding this value may be difficult to obtain as a commercially available material. The particle size of the carbon black used is preferably 0.005 to 1 μm, particularly preferably 0.01 to 0.2 μm, in terms of primary particle size, where the primary particle size is the average particle size measured with an electron microscope or the like.

[0019] Examples of commercially available carbon black include, for example, ketjen black, Tokai Carbon's Toka Black #4400, #4500, and #5500; Degussa's Printex L; Mitsubishi Chemical's #2350, #2400B, #2600B, #3050B, #3230B, #3350B, #3400B, and #5400B; Cabot's Vulcan XC-72R and Black Pearls 2000; and Timcal's Ensaco 250G furnace black; Lion Specialty Chemicals' EC-200L, EC-300J, and EC-600JD acetylene black; and Denka Black HS-100, Denka Black Li-400, and Denka Black FX-35, all of which are manufactured by Denka Co., Ltd. However, the present invention is not limited thereto, and two or more of them may be used in combination.

[0020] The conductive carbon fibers are preferably those obtained by burning petroleum-derived raw materials, but those obtained by burning plant-derived raw materials can also be used. Carbon nanotubes include single-walled carbon nanotubes, which are tubes formed of one graphene sheet and have a diameter in the nanometer range, and multi-walled carbon nanotubes, which are tubes formed of multiple graphene sheets. The diameter of single-walled carbon nanotubes is preferably 0.7-2.0 nm, and the diameter of multi-walled carbon nanotubes is preferably about 30 nm.

[0021] Examples of commercially available conductive carbon fibers and carbon nanotubes include vapor grown carbon fibers such as VGCF manufactured by Showa Denko K.K.; single-walled carbon nanotubes such as EC1.0, EC1.5, EC2.0, and EC1.5-P manufactured by Meijo Nano Carbon K.K.; FloTube9000, FloTube9100, FloTube9110, and FloTube9200 manufactured by CNano; NC7000 manufactured by Nanocyl Corporation; and 100T manufactured by Knano Corporation.

[0022] The content of the carbon material other than graphite in the total of 100% by mass is preferably 1 to 75% by mass, more preferably 4 to 50% by mass, in terms of electrical conductivity, adhesion to a non-conductive substrate, etc. The content of the carbon material contained in 100% by mass of the working electrode is preferably 50 to 98% by mass, more preferably 60 to 95% by mass.

[0023] (Water-based resin) In order to provide the dispersibility of the carbon material, the adhesion to the non-conductive substrate, and the stability of the conductive composition, at least the working electrode uses an aqueous resin as a binder that allows the aqueous solution to quickly penetrate into the electrode, taking into consideration that the measurement target is a biological sample, food, or cell culture medium. The aqueous resin is not particularly limited, and examples thereof include conductive resins such as acrylic resins, polyurethane resins, polyester resins, phenolic resins, epoxy resins, phenoxy resins, urea resins, melamine resins, silicone resins, polyaniline, and polyacetylene, celluloses, and modified or copolymerized products thereof. These aqueous resins can be used alone or in combination.

[0024] Furthermore, a curable resin, which undergoes a curing (crosslinking) reaction after the aqueous resin becomes a coating film, can also be used.

[0025] The aqueous resin may be used in combination with an aqueous emulsion. The aqueous emulsion is a dispersion in which the binder resin is not dissolved in water but is dispersed in the form of fine particles. The aqueous emulsion is not particularly limited, and examples thereof include (meth)acrylic emulsions; nitrile emulsions; urethane emulsions; diene emulsions containing diene rubbers such as SBR (styrene butadiene rubber); and fluorine-based emulsions containing fluorine-containing polymers such as PVdF (polyvinylidene fluoride) and PTFE (polytetrafluoroethylene). The average particle size of the emulsion is preferably 10 to 1000 nm, more preferably 10 to 300 nm, from the viewpoint of binding property and particle stability. The average particle size in the present invention refers to the volume average particle size, and can be measured by a dynamic light scattering method. In particular, it is preferable to use an aqueous emulsion from the viewpoint of adhesion.

[0026] <Enzyme sensor electrodes> The present invention relates to an electrode for an enzyme sensor used in an enzyme sensor having a working electrode and a counter electrode, and these electrodes can be obtained, for example, by applying an enzyme sensor electrode-forming composition containing a conductive carbon material, an aqueous resin, and, if necessary, a liquid medium, etc., to at least one surface of a substrate, and then performing a press treatment, etc., if necessary, to form a conductive layer. The electrode for an enzyme sensor is such that at least the working electrode contains a carbon material and an aqueous resin, and further the working electrode has a thickness of 15 μm or less and a density of 1.4 g / cm. 3 That's all. If necessary, an oxidoreductase or a mediator can be supported to obtain an electrode. The enzyme sensor needs to have at least a working electrode and a counter electrode, and may also have a reference electrode.

[0027] (Liquid medium) The composition for forming an enzyme sensor electrode may contain any liquid medium. The liquid medium is not particularly limited, and any known liquid medium may be used. In order to improve the dispersibility of the paste composition and the applicability of the paste composition on the substrate, a mixture of multiple types of solvents may be used. Examples of the liquid medium include organic solvents such as alcohols, glycols, cellosolves, amino alcohols, amines, ketones, carboxylic acid amides, phosphoric acid amides, sulfoxides, carboxylic acid esters, phosphoric acid esters, ethers, and nitriles, and water, etc. Among these, it is preferable to use water as the main component since an aqueous resin is used.

[0028] (Dispersant) The composition for forming an enzyme sensor electrode may use a dispersant. The dispersant functions effectively as a dispersant for carbon materials and the like, and can reduce the aggregation thereof. The dispersant is not particularly limited as long as it has the effect of reducing the aggregation of the carbon material.

[0029] Furthermore, the composition for forming an enzyme sensor electrode may contain, as necessary, a thickener, a film-forming assistant, a hardener, an antifoaming agent, a leveling agent, a preservative, a pH adjuster, an oxidoreductase, a mediator, and the like.

[0030] (Non-conductive base material) Examples of non-conductive substrates include polyester resins such as polyethylene terephthalate and polyethylene naphthalate, acrylic resins such as polymethyl methacrylate, and resin films such as polyethylene, polypropylene, polyvinyl chloride, polystyrene, polycarbonate, polyimide, polytetrafluoroethylene, perfluoroalkoxyalkane, perfluoroethylenepropene copolymer, ethylenetetrafluoroethylene copolymer, polyvinylidene fluoride, polychlorotrifluoroethylene, and ethylenechlorotrifluoroethylene copolymer. In addition to resin films, paper, cloth, and the like can also be used.

[0031] <Formation of electrodes for enzyme sensors> The electrode for the enzyme sensor can be formed by coating / printing the composition for forming the enzyme sensor electrode on the non-conductive substrate, and if necessary, performing a press treatment, etc. The method for coating / printing the composition on the non-conductive substrate is not particularly limited, and general methods such as screen printing, inkjet printing, gravure printing, knife coater, bar coater, blade coater, spray, dip coater, spin coater, roll coater, die coater, curtain coater, etc. can be applied.

[0032] After coating, rolling treatment may be performed using a lithographic press or a calendar roll, or heating may be performed to soften the conductive layer and make it easier to press. If the thickness of the electrode part (conductive layer) excluding the substrate is thin, the electrolyte will penetrate into the electrode quickly and noise can be reduced, so it is preferable that the thickness is 15 μm or less. In addition, the higher the density, the stronger the electrode will be, so a thickness of 1.4 g / cm is preferable. 3 The above is preferred.

[0033] <Enzyme sensor> The electrodes in the enzyme sensor are installed in a configuration of a working electrode and a counter electrode, or a working electrode, a counter electrode and a reference electrode. These electrodes may be prepared by forming conductive layers on different non-conductive substrates, forming conductive layers for each electrode on the same non-conductive substrate, or forming a non-conductive portion after forming a conductive layer on the same non-conductive substrate. Alternatively, the electrodes may be prepared by forming a metal layer on the non-conductive substrate in advance by metal sputtering or the like and then forming a conductive layer for each electrode. When a reference electrode is installed, it is prepared, for example, by further laminating silver or silver chloride on the top of the conductive layer. Examples of the lead portion of each electrode include a method of forming a metal layer by metal sputtering or the like, a method of extending the conductive layer, and a method of further forming a metal layer on the top or bottom of the extended conductive layer by metal sputtering or the like.

[0034] Methods for disposing the oxidoreductase or mediator include a method of incorporating the oxidoreductase and, if necessary, the mediator on the upper part of the working electrode, the counter electrode, and the reference electrode, or on the upper part and / or inside of the working electrode, a method of forming a layer containing the oxidoreductase and, if necessary, the mediator, etc. When forming a layer containing the oxidoreductase or the mediator, a hydrophilic compound and / or a hydrophilic resin may be mixed.

[0035] Examples of the uses of sensors include organic matter sensors for various organic matters, biosensors for organic matters and body fluids in biological samples such as blood, sweat, urine, feces, tears, saliva, and breath, moisture sensors for moisture, food sensors for sugar in fruits and foods, IoT sensors, environmental sensors for organic matters in the environment such as the atmosphere, rivers, and soil, animal and plant sensors for animals, insects, and plants, and cell culture sensors for monitoring medium components in cell culture. Examples of biosensors include blood glucose level sensors that sense sugar in blood, urine glucose level sensors that sense sugar in urine, fatigue level sensors and heat stroke sensors that sense lactic acid levels in sweat, and sweat and urination sensors that sense moisture in sweat and urine. Examples of uses of wearable sensors for living organisms include urination sensors and urine glucose level sensors with sensors installed in diapers, percutaneously attached sweat and heat stroke sensors, and puncture-type interstitial fluid sugar sensors.

[0036] <Oxidoreductase> The enzyme in the present invention is not particularly limited as long as it can donate and receive electrons through a reaction, and is appropriately selected depending on the detection target. Oxidases and dehydrogenases of sugars and organic acids can be used. Among them, glucose oxidase and glucose dehydrogenase, which can detect glucose contained in biological samples such as human blood and urine, may be preferable. In addition, fructose oxidase and fructose dehydrogenase, which can detect fructose, and lactate oxidase and lactate dehydrogenase, which can detect lactate, may be preferable.

[0037] <Mediator> Enzymes include direct electron transfer (DET) enzymes that can transfer electrons directly to the electrode, and enzymes that cannot transfer electrons directly. In the case of enzymes other than DET, it is necessary to use a mediator that transfers electrons generated by the oxidation of the fuel from the enzyme to the electrode. There is no particular limitation on the mediator as long as it is an oxidation-reduction substance that can transfer electrons to the electrode, and any conventionally known mediator can be used. The mediator can be used by supporting it on an electrode or by dissolving it in an electrolyte. Examples of mediators include non-metallic compounds such as tetrathiafulvalene, quinones such as hydroquinone and 1,4-naphthoquinone, ferrocene, ferricyanide, osmium complexes, and polymers modified with these compounds. EXAMPLES

[0038] The present invention will be described in more detail below with reference to examples, but the following examples are not intended to limit the scope of the invention. In the examples and comparative examples, "parts" refers to "parts by mass" and "%" refers to "% by mass" unless otherwise specified.

[0039] [Example 1] <Preparation of composition for forming enzyme sensor electrode> 3 parts by mass of water-based resin (CMC Daicel #1240 (manufactured by Daicel Chemical Industries, Ltd.)) was dissolved in 500 parts by mass of ion-exchanged water, 70 parts by mass of graphite (natural graphite J-CPB (manufactured by Nippon Graphite Co., Ltd.)) and 10 parts by mass of carbon material other than graphite (furnace black VULCAN (registered trademark) XC72 (manufactured by CABOT)) were added, and the mixture was mixed in a mixer. Then, the mixture was dispersed using a sand mill. Next, 34 parts by mass of water-dispersible resin particles ((meth)acrylic emulsion W-168 (Toyochem Co., Ltd., solid content 50% by mass)) were added, and ion-exchanged water was added appropriately and mixed in a mixer to obtain a composition for forming an enzyme sensor electrode.

[0040] <Preparation of electrodes for enzyme sensors> The enzyme sensor electrode-forming composition was applied to a non-conductive PET substrate (Lumirror (manufactured by Toray Industries, Inc.)) having a thickness of 100 μm using a doctor blade, and then heated and dried to obtain a conductive layer (1). Thereafter, pressing was performed using a roll press machine to obtain an enzyme sensor electrode (1), the film thickness was measured, and the density of the conductive layer was calculated.

[0041] By the same method as in Example 1, electrodes (2) to (9) for enzyme sensors of Examples 2 to 5 and Comparative Examples 1 and 2 shown in Table 1 were obtained. 〇: Density 1.4g / cm 3 End △: Density 1.4g / cm 3 less than

[0042] <Adhesion evaluation of electrodes> The electrodes prepared above were cut with a knife to a depth reaching from the electrode surface to the substrate, with 2 mm intervals in both the vertical and horizontal directions. Adhesive tape was applied to the cuts and immediately peeled off, and the degree of peeling of the coating was visually evaluated. The evaluation criteria are shown below. The results are shown in Table 1. ○: Almost no peeling △: "About half peeled off" (level that does not cause any problems in practical use) ×: "Most of the parts peeled off"

[0043] The enzyme sensor electrodes (1) to (9) were cut into a size of 10×20 mm, and the area other than the lower 2×2 mm was masked with tape.

[0044] <Electrochemical evaluation> The enzyme sensor electrode prepared above was used as the working electrode, and a 0.1 M phosphate buffer solution (pH 7.0) was placed in an electrolytic cell equipped with a counter electrode (platinum coil electrode) and a reference electrode (silver / silver chloride electrode), and a potential of 0.3 V (vs Ag / AgCl) was applied to measure the current value after 500 seconds to obtain the background. As shown in Table 1, the current values ​​in each example were compared as a percentage (%) of the current value at 0.3 V in the comparative example. The smaller the background current value measured with the enzyme sensor electrode, the easier it is to detect the substance to be sensed, and the higher the sensitivity. ○: Less than 50% △: 50% or more but less than 100% ×: 100% or more

[0045] [Table 1]

[0046] In all of the Examples, the background current, which becomes noise, was reduced more than in the Comparative Examples, so the electrode of the present invention can be used as a highly sensitive enzyme sensor. 3 Electrodes with a thickness of less than this are not suitable for use as electrodes for enzyme sensors due to their poor adhesion.

[0047] For the enzyme sensor electrode (5) of Example 5, a methanol solution of ferrocene as a mediator and an aqueous solution of glucose oxidase as an enzyme were dropped onto the lower 2×2 mm conductive layer that had not been masked, and the electrode was naturally dried to support the mediator and enzyme, thereby obtaining an enzyme-supported electrode for an enzyme sensor. When a potential of 0.3 V (vs Ag / AgCl) was applied in each of 0.1 M phosphate buffer solutions containing 5 mM, 10 mM, and 20 mM glucose, and the current value was measured after 10 seconds, a correlation was observed between the glucose concentration and the current value. Since the current value change depending on the substrate concentration was obtained, it can be used as a sensor. In addition, when the glucose concentration and current value were similarly confirmed for the enzyme sensor electrode (7) of Example 7, the current value was half or less compared to Example 5.

Claims

1. An electrode for an enzyme sensor having a working electrode and a counter electrode, the working electrode containing a carbon material and an aqueous resin, the working electrode having a thickness of 10 μm or less and a density of 1.4 g / cm 3 The above is an electrode for an enzyme sensor.

2. 2. The electrode for an enzyme sensor according to claim 1, wherein the carbon material contains at least graphite.

3. 3. The electrode for an enzyme sensor according to claim 1, wherein the working electrode contains a carbon material in an amount of 60% by mass or more based on 100% by mass of the working electrode.

4. An enzyme sensor using the electrode for an enzyme sensor according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Method of manufacturing biosensor

    JP2008045877A

  • Conductive laminate

    JP2018037394A

  • Conductive substrate for enzyme power generation device, electrode for enzyme power generation device and enzyme power generation device

    JP2019212575A

  • Microbial fuel cell device

    JP2020095962A

  • Soft Analyte Sensor

    JP2020506750A