Manufacturing method of SiC single crystal, SiC seed crystal and SiC ingot

By processing SiC single crystals to align with the atomic arrangement plane, the method addresses BPD issues, enhancing the quality and yield of SiC epitaxial wafers and devices.

JP7571902B2Active Publication Date: 2024-10-23RESONAC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024002798
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-11
Publication Date
2024-10-23
Estimated Expiration
2038-08-13

AI Technical Summary

Technical Problem

Basal plane dislocations (BPD) in SiC wafers, which are caused by slippage at the basal surface, cannot be sufficiently suppressed by controlling the warpage and waviness of the external shape of the SiC single crystal used as a seed crystal, leading to deterioration of device characteristics.

Method used

A method for processing SiC single crystals by measuring and aligning the atomic arrangement plane to flatten it during crystal growth, involving steps such as processing the back side of the seed crystal to follow the atomic alignment plane, using spacers or vacuum adsorption to adjust curvature, and electrical discharge machining to match the atomic arrangement plane, resulting in a SiC single crystal with minimal curvature.

Benefits of technology

The method effectively suppresses basal plane dislocations in SiC ingots and wafers, improving the quality and yield of SiC epitaxial wafers and devices by reducing BPD density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571902000005
    Figure 0007571902000005
  • Figure 0007571902000006
    Figure 0007571902000006
  • Figure 0007571902000007
    Figure 0007571902000007
Patent Text Reader

Abstract

To provide a processing method of a SiC single crystal capable of reducing curvature of an atomic arrangement plane during crystal growth.SOLUTION: A processing method of a SiC single crystal has a measurement step for measuring the shape of an atomic arrangement plane of the SiC single crystal at least along a first direction passing through a plane view center and along a second direction orthogonal to the first direction, a processing step for processing at least a first surface of the SiC single crystal along the atomic arrangement plane based on a measurement result, and a pasting step for pasting the SiC single crystal onto an installation surface by using the first surface as a pasting surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a SiC single crystal, a SiC seed crystal, and a SiC ingot. [Background technology]

[0002] Silicon carbide (SiC) has an electric breakdown field one order of magnitude larger than silicon (Si) and a band gap three times larger. Silicon carbide (SiC) also has a thermal conductivity three times higher than silicon (Si). Silicon carbide (SiC) is expected to be used in power devices, high-frequency devices, high-temperature operating devices, and other applications.

[0003] SiC epitaxial wafers, which are made by forming an epitaxial film on a SiC wafer, are used for devices such as semiconductors. The epitaxial film formed on the SiC wafer by chemical vapor deposition (CVD) becomes the active region of the SiC semiconductor device.

[0004] Therefore, there is a demand for high-quality SiC wafers that are free from damage such as cracks and have few defects. In this specification, the term "SiC epitaxial wafer" refers to a wafer after an epitaxial film is formed, and the term "SiC wafer" refers to a wafer before an epitaxial film is formed.

[0005] For example, Patent Documents 1 and 2 describe that by controlling the warpage and waviness of the outer shape of a SiC single crystal used as a seed crystal, SiC ingots and SiC wafers obtained from this seed crystal can be of high quality. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-117143 A [Patent Document 2] Patent No. 4494856 Summary of the Invention [Problem to be solved by the invention]

[0007] One of the killer defects in SiC wafers is the basal plane dislocation (BPD). Some of the BPDs in SiC wafers are inherited by SiC epitaxial wafers, and they cause a decrease in forward characteristics when a forward current is passed through the device. BPDs are defects that are thought to be caused in part by slippage that occurs on the basal plane.

[0008] As described in Patent Documents 1 and 2, BPD cannot be sufficiently suppressed even by controlling the warpage and waviness of the outer shape of the SiC single crystal used as a seed crystal. Therefore, there is a demand for reducing BPD.

[0009] The present invention has been made in view of the above problems, and has an object to provide a method for processing SiC single crystal that can reduce curvature of the atomic arrangement plane during crystal growth. [Means for solving the problem]

[0010] As a result of intensive research, the inventors have found that there is a correlation between the curvature of the atomic arrangement plane (lattice plane) of a SiC single crystal and the density of basal plane dislocations (BPDs). Therefore, they have found that the atomic arrangement plane can be flattened during crystal growth by processing the back surface of a seed crystal into a shape that follows the curvature of the atomic arrangement plane and attaching it to a flat attachment surface of a crucible. That is, in order to solve the above problems, the present invention provides the following means.

[0011] (1) A first aspect of a method for processing a SiC single crystal includes a measurement step of measuring a shape of an atomic arrangement surface of a SiC single crystal at least along a first direction passing through a center in a planar view and a second direction perpendicular to the first direction, a processing step of processing at least a first surface of the SiC single crystal along the atomic arrangement surface based on the measurement results, and an attachment step of attaching the SiC single crystal to a setting surface using the first surface as an attachment surface.

[0012] (2) In the method for processing a SiC single crystal according to the above aspect, the processing step may include a planarization step of attaching the SiC single crystal to a spacer having a curved surface that curves in a direction opposite to the curvature of the atomic arrangement surface and planarizing the atomic arrangement surface, and a face preparation step of cutting or grinding the SiC single crystal along the planarized atomic arrangement surface.

[0013] (3) In the method for processing a SiC single crystal according to the above aspect, the processing step may include a vacuum adsorption step of vacuum adsorbing the SiC single crystal onto an adsorption surface having an adsorption force that varies depending on the amount of curvature of the atomic arrangement surface, and flattening the atomic arrangement surface, and a surface preparation step of cutting or grinding the SiC single crystal along the flattened atomic arrangement surface.

[0014] (4) In the method for processing a SiC single crystal according to the above aspect, the processing step may include an electric discharge processing step of bringing the SiC single crystal close to an electrode having a shape corresponding to the atomic arrangement surface, and processing the first surface of the SiC single crystal by electric discharge.

[0015] (5) In the method for processing a SiC single crystal according to the above aspect, the SiC single crystal may have a thickness of 5 mm or less when the bonding step is performed.

[0016] (6) In the attachment step of the method for processing a SiC single crystal according to the above-described aspect, when the first surface is convexly curved toward the installation surface, the load on the outer periphery of the SiC single crystal may be made stronger than that on the inner side, and when the first surface is concavely curved toward the installation surface, the load on the inner side of the SiC single crystal may be made stronger than that on the outer periphery.

[0017] (7) The method of processing a SiC single crystal according to the above aspect may further include a depressurizing step of depressurizing the surroundings of the SiC single crystal during the attaching step.

[0018] (8) A method for producing a SiC ingot according to a second aspect, in the method for processing a SiC single crystal according to the above aspect, comprises performing crystal growth using the SiC single crystal attached to the installation surface as a seed crystal.

[0019] (9) The SiC single crystal according to the third aspect is a SiC single crystal having a maximum amount of curvature of an atomic arrangement plane of 20 μm or more, and an absolute value of the difference between the amount of warpage of the SiC single crystal and the amount of curvature of the atomic arrangement plane is 10 μm or less. Effect of the Invention

[0020] By using the method for evaluating a SiC single crystal according to the above embodiment, the atomic arrangement plane during crystal growth can be flattened, and the occurrence of basal plane dislocations (BPDs) can be suppressed. [Brief description of the drawings]

[0021] [Figure 1] 1 is a schematic diagram of a cross section of a SiC single crystal cut along a straight line passing through the center in a plan view and extending in a first direction. [Diagram 2] FIG. 2 is a diagram showing a schematic diagram of an example of an atomic arrangement plane of a SiC single crystal. [Diagram 3] FIG. 2 is a diagram showing a schematic diagram of another example of an atomic arrangement plane of a SiC single crystal. [Figure 4] 1A to 1C are diagrams for specifically explaining a method for measuring the shape of an atomic arrangement plane. [Diagram 5] 1A to 1C are diagrams for specifically explaining a method for measuring the shape of an atomic arrangement plane. [Figure 6] 1A to 1C are diagrams for specifically explaining a method for measuring the shape of an atomic arrangement plane. [Figure 7] 1A to 1C are diagrams for specifically explaining a method for measuring the shape of an atomic arrangement plane. [Figure 8] An example of determining the radius of curvature of an atomic arrangement plane from multiple XRD measurement points is shown below. [Figure 9] 11A to 11C are diagrams for specifically explaining another example of a method for measuring the shape of an atomic arrangement plane. [Figure 10] 11A to 11C are diagrams for specifically explaining another example of a method for measuring the shape of an atomic arrangement plane. [Figure 11] FIG. 2 is a schematic diagram for explaining a first processing method. [Figure 12] FIG. 2 is a schematic diagram showing an adsorption surface in plan view. [Figure 13] FIG. 11 is a schematic diagram for explaining a third processing method. [Figure 14] FIG. 11 is a schematic diagram for explaining a bonding step. [Figure 15] FIG. 1 is a schematic diagram of an example of a production apparatus used in a sublimation method. [Figure 16] 1 is a graph showing the relationship between the radius of curvature of the atomic arrangement plane of a SiC single crystal and the BPD density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for convenience, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be modified as appropriate within the scope of the present invention.

[0023] "SiC single crystal processing method" The method for processing a SiC single crystal according to this embodiment includes a measuring step, a processing step, and an attaching step. In the measuring step, the shape of the atomic arrangement surface of the SiC single crystal is measured at least along a first direction passing through the center in a plan view and a second direction perpendicular to the first direction. In the processing step, at least the first surface of the SiC single crystal is processed along the atomic arrangement surface based on the measurement results. In the attaching step, the SiC single crystal is attached to a mounting surface with the first surface of the SiC single crystal as an attaching surface. Each step will be specifically described below.

[0024] <Measurement process> FIG. 1 is a schematic diagram of a cross section of a SiC single crystal 1 cut along a straight line that passes through the center in a plan view and extends in a first direction. The first direction can be set to any direction. In FIG. 1, the first direction is set to [1-100]. In FIG. 1, the upper side corresponds to the [000-1] direction, i.e. <0001> This is the direction in which a carbon surface (C surface, (000-1) surface) appears when cut perpendicularly to the [1-100] direction. In the following, an example will be explained in which the first direction is [1-100].

[0025] Here, crystal orientations and planes are expressed using the following brackets as Miller indices. () and {} are used to represent planes. () is used to represent a specific plane, while {} is used to represent a collective term (collective plane) for equivalent planes due to the symmetry of the crystal. On the other hand, <> and [] are specifically used to represent directions. [] is used to represent a specific direction, while <> is used to represent equivalent directions due to the symmetry of the crystal.

[0026] As shown in Fig. 1, SiC single crystal 1 is a single crystal formed by aligning a plurality of atoms A. Therefore, as shown in Fig. 1, when a cut surface of the SiC single crystal is viewed microscopically, an atomic arrangement plane 2 is formed along which a plurality of atoms A are arranged. The atomic arrangement plane 2 on the cut surface is expressed as a line extending in a direction approximately parallel to the cutting direction obtained by connecting the atoms A arranged along the cut surface.

[0027] The shape of the atomic arrangement plane 2 may vary depending on the direction of the cut surface, regardless of the shape of the outermost surface of the SiC single crystal 1. Figures 2 and 3 are diagrams showing the shape of the atomic arrangement plane 2. The atomic arrangement plane 2 shown in Figure 2 is concave toward the center. Therefore, the atomic arrangement plane 2 shown in Figure 2 has the same curvature direction in the [1-100] direction and the [11-20] direction perpendicular to the [1-100] direction. In contrast, the atomic arrangement plane 2 shown in Figure 3 has a potato chip (saddle) shape that is concave on a certain cut surface and convex on a different cut surface. Therefore, the atomic arrangement plane 2 shown in Figure 3 has different curvature directions in the [1-100] direction and the [11-20] direction perpendicular to the [1-100] direction.

[0028] That is, in order to accurately grasp the shape of the atomic arrangement surface 2, it is necessary to measure the shape of the atomic arrangement surface 2 of the SiC single crystal at least along two directions (a first direction and a second direction) that pass through the center in a plan view and are perpendicular to each other. In addition, the crystal structure of the SiC single crystal 1 is hexagonal, and it is preferable to measure the shape of the atomic arrangement surface 2 along six directions symmetrical with respect to the center. If the shape of the atomic arrangement surface 2 is measured along six directions symmetrical with respect to the center, the shape of the atomic arrangement surface 2 can be obtained more precisely.

[0029] The shape of the atomic arrangement plane 2 can be measured by X-ray diffraction (XRD). The plane to be measured is determined according to the direction to be measured. If the measurement direction is [hkil], the measurement plane must satisfy the relationship of (mh mk mi n). Here, m is an integer equal to or greater than 0, and n is a natural number. For example, when measuring in the [11-20] direction, the (0004) plane is selected with m=0 and n=4, and the (22-416) plane is selected with m=2 and n=16. On the other hand, when measuring in the [11-20] direction, the (0004) plane is selected with m=0 and n=4, and the (3-3016) plane is selected with m=3 and n=16. In other words, the measurement plane may be different depending on the measurement direction, and the atomic arrangement plane 2 to be measured does not necessarily have to be the same plane. By satisfying the above relationship, it is possible to prevent the lattice curvature in the a-plane or m-plane direction, which has little effect on crystal growth, from being mistaken for the lattice curvature in the c-plane direction. The measurement may be performed on either the C-face or the Si-face, but is performed on the attachment surface (first surface) that is attached to the installation surface of the crucible.

[0030] X-ray diffraction data is acquired at five points along a predetermined direction: the center, the edge, and the midpoint between the center and the edge. If the atomic arrangement surface 2 is curved, the reflection direction of the X-ray changes, and the position of the ω angle of the peak of the X-ray diffraction image output at the center and other parts varies. The curvature direction of the atomic arrangement surface 2 can be obtained from this positional variation of the diffraction peak. Furthermore, the radius of curvature of the atomic arrangement surface 2 can be obtained from the positional variation of the diffraction peak, and the amount of curvature of the atomic arrangement surface 2 can also be obtained. The shape of the atomic arrangement surface 2 can be obtained from the curvature direction and amount of curvature of the atomic arrangement surface 2.

[0031] (Specific explanation of the method for measuring the shape of atomic arrangement planes (Method 1)) A method for measuring the curvature direction and curvature amount of the atomic arrangement plane from the XRD measurement value of the outer peripheral edge portion of a sample (hereinafter referred to as wafer 20) sliced ​​from a SiC single crystal will be specifically described. The measurement method will be described using wafer 20 as an example, but a similar method can also be used for measurement of an ingot-shaped SiC single crystal before slicing.

[0032] FIG. 4 shows a schematic cross section cut along the direction of measurement of the atomic arrangement plane, for example, the [1-100] direction, passing through the center of the plan view. If the radius of the wafer 20 is r, the horizontal length of the cross section is 2r. FIG. 4 also shows the shape of the atomic arrangement plane 22 in the wafer 20. As shown in FIG. 4, the shape of the wafer 20 itself is flat, but the atomic arrangement plane 22 may be curved. The atomic arrangement plane 22 shown in FIG. 4 is symmetrical and concavely curved. This symmetry is due to the fact that the manufacturing conditions of the SiC single crystal (ingot) are usually symmetrical with respect to the center. Note that this symmetry does not need to be perfect symmetry, but means an approximate symmetry that allows for deviations due to fluctuations in the manufacturing conditions, etc.

[0033] 5, XRD is performed on both outer peripheral edges of the wafer 20, and the difference Δθ in the X-ray diffraction peak angles between the two measured points is determined. This Δθ is the difference in the inclination of the atomic arrangement plane 22 at the two measured points. The diffraction plane used in the X-ray diffraction measurement is selected as an appropriate plane according to the cut surface, as described above.

[0034] Next, as shown in Fig. 6, the radius of curvature of the curved atomic arrangement surface 22 is calculated from the obtained Δθ. Fig. 6 shows a circle C tangent to the atomic arrangement surface at two measured locations, assuming that the curved surface of the atomic arrangement surface 22 of the wafer 20 is a part of a circle. Geometrically, from Fig. 6, the central angle φ of a sector including an arc with both ends at the tangent point is equal to the difference Δθ between the measured X-ray diffraction peak angles. The radius of curvature of the atomic arrangement surface 22 corresponds to the radius R of the arc. The radius R of the arc can be calculated by the following relational expression.

[0035]

number

[0036] Then, the amount of curvature d of the atomic arrangement surface 22 is found from the radius R of this arc and the radius r of the wafer 20. As shown in Fig. 7, the amount of curvature d of the atomic arrangement surface 22 corresponds to the radius of the arc minus the distance of the perpendicular line drawn from the center of the arc to the wafer 20. The distance of the perpendicular line drawn from the center of the arc to the wafer 20 is calculated using Pythagoras' theorem, and the following formula holds. Note that in this specification, the amount of curvature d is defined as a positive value when the radius of curvature is positive (concave surface), and as a negative value when the radius of curvature is negative (convex surface).

[0037]

number

[0038] As described above, R can be measured only from the XRD measurements of both outer edges of the wafer 20. However, when this method is used, there is a possibility that the shape may be misjudged if there is local distortion at the measurement point. For this reason, the X-ray diffraction peak angles are measured at multiple points, and the curvature per unit length is calculated using the following formula.

[0039]

number

[0040] Figure 8 shows an example of determining the radius of curvature of an atomic arrangement plane from multiple XRD measurement points. The horizontal axis in Figure 8 indicates the relative position from the center of the wafer, and the vertical axis indicates the relative diffraction peak angle of each measurement point with respect to the wafer center diffraction peak angle. Figure 8 shows an example in which the [1-100] direction of the wafer was measured, and the measurement surface was (3-3016). Measurements were taken at five locations. The five points were arranged almost in a straight line, and from the inclination of this line, dθ / dr = 8.69 × 10 -4 By applying this result to the above formula, it is possible to calculate that the concave surface has a radius of R = 66 m. From this radius and the wafer radius r (75 mm), the curvature d of the atomic arrangement surface is calculated to be 42.6 μm.

[0041] So far, we have used an example in which the atomic arrangement plane shape is concave, but the same calculation can be done for a convex surface. In the case of a convex surface, R is calculated as a negative value.

[0042] (Explanation of another method for measuring the shape of atomic arrangement surfaces (Method 2)) The shape of the atomic arrangement plane may be obtained by another method. Fig. 9 shows a schematic cross section cut along the measurement direction of the atomic arrangement plane, for example, the [1-100] direction, passing through the center of the plan view. Fig. 9 shows an example in which the shape of the atomic arrangement plane 22 is curved in a concave shape.

[0043] As shown in Fig. 9, X-ray diffraction peaks are measured at two points, the center of the wafer 20 and a point a distance x away from the center of the wafer 20. Due to the symmetry of the manufacturing conditions of the ingot, the shape of the wafer 20 can be approximately bilaterally symmetrical, and it can be assumed that the atomic arrangement surface 22 is flat at the center of the wafer 20. Therefore, if the difference in the inclination of the atomic arrangement surface 22 at the two measured points as shown in Fig. 10 is taken as Δθ, the relative position y of the atomic arrangement surface 22 can be expressed by the following equation.

[0044]

number

[0045] By measuring a plurality of points while changing the position of the distance x from the center, the relative atomic positions of the atomic arrangement surface 22 at each point between the wafer center and the measurement point can be obtained. This method determines the relative positions of atoms on the atomic arrangement surface at each measurement point. Therefore, the amount of curvature of the local atomic arrangement surface can be determined. In addition, the relative atomic positions of the atomic arrangement surface 22 on the entire wafer 20 can be displayed as a graph, which is useful for intuitively understanding the arrangement of the atomic arrangement surface 22.

[0046] Here, the measurement object has been described as a wafer 20. When the measurement object is a SiC ingot or a cut piece cut from a SiC ingot, the amount of curvature of the atomic arrangement plane can be obtained in the same manner.

[0047] Using the above-mentioned procedure, the curvature of the atomic arrangement plane 2 of the SiC single crystal is measured at least along two mutually orthogonal directions (first and second directions) that pass through the center in a plan view. By determining the curvature amount and curvature direction in each direction, it is possible to obtain a rough shape of the atomic arrangement plane 2 as shown in Figs. 2 and 3.

[0048] <Processing process> In the processing step, based on the measurement results of the measurement step, the attachment surface (first surface) of the SiC single crystal 1 is processed along the atomic arrangement surface 2. The processing method is not particularly limited, but for example, the following three methods can be used.

[0049] (First processing method) The first processing method includes a planarizing step of attaching the SiC single crystal to a spacer having a curved surface that curves in the opposite direction to the curvature of the atomic arrangement surface 2 and planarizing the atomic arrangement surface 2, and a faceting step of cutting or grinding the SiC single crystal along the planarized atomic arrangement surface 2. When using the first processing method, the thickness of the SiC single crystal is preferably 5 mm or less to allow elastic deformation.

[0050] 11 is a schematic diagram for explaining the first processing method. As shown in Fig. 11(a), a spacer 30 and a support 31 are prepared. A first surface 30A of the spacer 30 is a flat surface, and a second surface 30B is a curved surface that is curved in the opposite direction to the curvature of the atomic arrangement surface 2.

[0051] The second surface 30B of the spacer 30 may be processed after measuring the shape of the atomic arrangement surface 2 of the SiC single crystal 1, or a plurality of spacers with different curvature directions and amounts of curvature may be prepared in advance, and one of them that can best flatten the atomic arrangement surface 2 after attachment may be selected.

[0052] The spacer 30 and the support base 31 may be made of glass, ceramics, or the like. From the viewpoint of workability, it is preferable to use ceramics to manufacture the spacer 30. It is preferable to use a support base 31 that has excellent surface flatness and rigidity.

[0053] Next, as shown in FIG. 11(b), a spacer 30 is placed on a support 31, and the SiC single crystal 1 is bonded to the second surface 30B of the spacer 30. The SiC single crystal 1 is bonded so that the curvature direction of the atomic arrangement surface 2 is opposite to the curvature direction of the second surface 30B. The bonding is performed, for example, by using an adhesive. The adhesive may be a thermoplastic resin-based solid wax that is usually used in precision machining, and it is preferable to select an adhesive with strong adhesive strength. Even if the SiC single crystal is elastically deformed by the adhesive and fixed to the support 31, it can be fixed in the deformed state.

[0054] The atomic arrangement surface 2 of the SiC single crystal 1 after being bonded to the spacer 30 is flatter than the atomic arrangement surface 2 before being bonded. It is most preferable that the atomic arrangement surface 2 after being bonded to the spacer 30 is parallel to the surface of the support table 31.

[0055] Next, as shown in FIG. 11(c), the SiC single crystal 1 is cut. The cut surface is parallel to the surface of the support table 31. Since the atomic arrangement surface 2 is flattened relative to the surface of the support table 31, when the SiC single crystal 1 is cut parallel to the surface of the support table 31, the SiC single crystal 1 is necessarily cut along the flattened atomic arrangement surface 2. For example, a wire saw or the like can be used for cutting. Furthermore, in the face-finishing step, the atomic arrangement surface 2 may be face-finished by a method other than cutting. As a method other than cutting, for example, the SiC single crystal 1 may be ground from the face opposite to the support table 31.

[0056] By going through the above-mentioned process, as shown in FIG. 11(d), a SiC single crystal 10 is obtained after cutting, in which the first surface 10A is aligned with the atomic arrangement plane 2.

[0057] (Second processing method) The second processing method includes a vacuum suction step of vacuum suctioning the SiC single crystal 1 onto an adsorption surface having different suction strengths according to the amount of curvature of the atomic arrangement surface 2, and flattening the atomic arrangement surface 2, and a surface preparation step of cutting or grinding the SiC single crystal along the flattened atomic arrangement surface 2. The second processing method differs from the first processing method in that the atomic arrangement surface 2 is flattened by the difference in the strength of the suction strength without using a spacer 30. The other processing steps are the same, and will not be described. Even when using the second processing method, the thickness of the SiC single crystal is preferably 5 mm or less, which allows elastic deformation.

[0058] 12 is a schematic plan view of the suction surface 40. The suction surface 40 has a plurality of suction holes 41. In the second processing method, the atomic arrangement surface 2 is flattened by utilizing the difference in suction force of these suction holes 41.

[0059] For example, as shown in FIG. 2, when the atomic arrangement surface 2 of the SiC single crystal 1 is concave toward the center, the suction force of the suction hole 41I is made smaller than that of the other suction holes 41A to 41H. Then, the outer periphery of the atomic arrangement surface 2 is suctioned relatively stronger than the inside, and the atomic arrangement surface 2 is flattened. Also, as shown in FIG. 3, when the atomic arrangement surface 2 of the SiC single crystal 1 is a saddle shape with different curvature directions in the [1-100] direction and the [11-20] direction, the suction force of the suction hole 41 located farther from the central axis in the [11-20] direction is made larger. That is, the suction force of the suction holes 41G, 41I, 41C is made smaller than that of the suction holes 41H, 41B, 41F, 41D, and the suction force of the suction holes 41H, 41B, 41F, 41D is made smaller than that of the suction holes 41A, 41E.

[0060] As described above, the atomic arrangement surface 2 can be flattened by utilizing the difference in suction force of the suction holes 41. Then, the SiC single crystal 1 with the flattened atomic arrangement surface 2 is cut parallel to the mounting surface, as in Figures 11(c) and 11(d). Through the above process, a SiC single crystal 10 with a first surface 10A aligned with the atomic arrangement surface 2 is obtained.

[0061] (Third processing method) The third machining method includes an electric discharge machining step of bringing SiC single crystal 1 close to an electrode having a shape corresponding to atomic arrangement surface 2 and machining first surface 1A of SiC single crystal 1 by electric discharge. When using the third machining method, unlike the first and second machining methods, the thickness of SiC single crystal 1 does not matter.

[0062] Fig. 13 is a schematic diagram for explaining the third processing method. As shown in Fig. 13(a), an electrode 50 is prepared. A first surface 50A of the electrode 50 shown in Fig. 13(a), which faces the SiC single crystal 1, is a curved surface processed along the atomic arrangement plane 2.

[0063] The first surface 50A of the electrode 50 may be machined after measuring the shape of the atomic arrangement surface 2 of the SiC single crystal 1, or a plurality of electrodes with different curvature directions and amounts of curvature may be prepared in advance, and the one that is closest to the shape of the atomic arrangement surface 2 may be selected from among them.

[0064] Next, with the first surface 50A of the electrode 50 facing the SiC single crystal 1, the electrode 50 is brought closer to the SiC single crystal 1. The closer the distance between the electrode 50 and the SiC single crystal 1, the stronger the discharge, and so the first surface 1A of the SiC single crystal 1 evaporates along the shape of the first surface 50A of the electrode 50. As a result, as shown in Fig. 13(b), a SiC single crystal 10 is obtained whose first surface 10A is aligned with the atomic arrangement plane 2.

[0065] <Attachment process> Fig. 14 is a schematic diagram for explaining the bonding step. As shown in Fig. 14(a), in the bonding step, the SiC single crystal 10 is bonded to a mounting surface 60A of a mounting stand 60, with a first surface 10A of the SiC single crystal 10 obtained by processing being used as a bonding surface. The mounting stand 60 corresponds to, for example, a single crystal mounting portion of a crucible.

[0066] The thickness of the SiC single crystal 10 during the attachment step is preferably 5 mm or less. If the SiC single crystal 10 is too thick, it is difficult to cause bending during attachment, making it difficult to attach it flat to the base, and it may be difficult to arrange the atomic arrangement plane (lattice plane) of the SiC single crystal flat.

[0067] In the attachment step, the load with which the SiC single crystal 10 is pressed against the mounting surface 60A is preferably changed according to the amount of curvature of the first surface 10A relative to the mounting surface 60A. For example, when the first surface 10A of the SiC single crystal 10 is curved convexly toward the mounting surface 60A, it is preferable to make the load on the outer periphery of the SiC single crystal 10 stronger than that on the inner surface. When the first surface 10A of the SiC single crystal 10 is curved concavely toward the mounting surface 60A, it is preferable to make the load on the inner surface of the SiC single crystal 10 stronger than that on the outer periphery.

[0068] The attaching step is performed by using, for example, an adhesive, such as a thermosetting resin.

[0069] Furthermore, during the bonding process, a decompression process may be further performed before the adhesive is cured to reduce the pressure around the SiC single crystal 10. Even if air bubbles or the like are trapped in the adhesive surface, they can be degassed by creating a decompression environment. As a result, unevenness in the thickness of the adhesive when applied can be further suppressed.

[0070] In addition, it is preferable that the thermal expansion coefficient of the mounting base 60 to be attached is close to that of the SiC single crystal 10. Specifically, the difference in thermal expansion coefficient is 0.3×10 -6 / °C or less. The thermal expansion coefficient referred to here means the thermal expansion coefficient in the temperature range in which crystal growth occurs using the SiC single crystal 10 as a seed crystal, and means a temperature in the vicinity of 2000°C. For example, the thermal expansion coefficient of graphite is 4.3×10 -6 / ℃~7.1×10 -6 / ° C. Since the difference in thermal expansion coefficient between the mounting table 60 and the SiC single crystal 10 is close to each other, it is possible to prevent the SiC single crystal 10 from warping and the atomic arrangement plane 2 from curving due to the difference in thermal expansion coefficient during single crystal growth.

[0071] Then, by carrying out the bonding step as described above, it is possible to obtain SiC single crystal 10 with atomic arrangement plane 2 parallel to mounting surface 60A and with little curvature, as shown in FIG. 14(b).

[0072] "SiC single crystal" The SiC single crystal processed up to the stage before the above-mentioned bonding process is processed so that the first surface is shaped to follow the curvature of the atomic arrangement surface. As a result, as shown in FIG. 14(a), the warped shape of the first surface 10A of the SiC single crystal 10 and the curvature of the atomic arrangement surface 2 are substantially parallel. In other words, the absolute value of the difference between the amount of warping of the SiC single crystal 10 and the amount of curvature of the atomic arrangement surface 2 is 10 μm or less. Here, the "amount of warping" means the maximum value of the distance between the mounting surface and the first surface of the SiC single crystal on the mounting surface side when the SiC single crystal is placed on a flat surface. When the maximum amount of curvature of the atomic arrangement surface 2 of the SiC single crystal 10 is 20 μm or more, it is difficult to imagine that the warped shape of the first surface 10A of the SiC single crystal 10 and the curvature of the atomic arrangement surface 2 will be substantially parallel without carrying out the above-mentioned processing. In other words, SiC single crystal 10 in which the maximum curvature of the atomic arrangement plane is 20 μm or more and the absolute value of the difference between the warpage of SiC single crystal 10 and the curvature of atomic arrangement plane 2 is 10 μm or less can be achieved through the above process.

[0073] "SiC ingot manufacturing method" The method for producing a SiC ingot according to this embodiment is the same as the above-mentioned method for processing a SiC single crystal, except that crystal growth is performed using a SiC single crystal 10 attached to the mounting surface 60A as a seed crystal. The SiC ingot can be produced, for example, by sublimation. The sublimation method is a method for obtaining a large single crystal (ingot) by recrystallizing a raw material gas generated by heating the raw material on a single crystal (seed crystal).

[0074] 15 is a schematic diagram of an example of a manufacturing apparatus used in the sublimation method. The manufacturing apparatus 200 has a crucible 100 and a coil 101. A heating element (not shown) that generates heat by induction heating of the coil 101 may be provided between the crucible 100 and the coil 101.

[0075] The crucible 100 has a mounting table 60 provided at a position facing the raw material G. A SiC single crystal 10 processed by the above-mentioned SiC single crystal processing method is attached as a seed crystal to the mounting table 60. In addition, a taper guide 102 expanding in diameter from the mounting table 60 toward the raw material G is provided inside the crucible 100.

[0076] When an alternating current is applied to the coil 101, the crucible 100 is heated and a raw material gas is generated from the raw material G. The generated raw material gas is supplied along a tapered guide 102 to the SiC single crystal 10 placed on the placement table 60. The supply of the raw material gas to the SiC single crystal 10 causes crystal growth of an SiC ingot I on the main surface of the SiC single crystal 10. The crystal growth surface of the SiC single crystal 10 is preferably a carbon surface or a surface having an off angle of 10° or less from the carbon surface.

[0077] SiC ingot I inherits much of the crystal information of SiC single crystal 10. Since atomic arrangement plane 2 of SiC single crystal 10 is flattened, the occurrence of BPDs in SiC ingot I can be suppressed.

[0078] FIG. 16 is a graph showing the relationship between the radius of curvature of the atomic arrangement plane of a SiC single crystal and the BPD density. As shown in FIG. 16, there is a corresponding relationship between the radius of curvature of the atomic arrangement plane 2 and the BPD density in the SiC ingot I. The larger the radius of curvature of the atomic arrangement plane 2 (the smaller the amount of curvature of the atomic arrangement plane 2), the lower the BPD density tends to be. It is considered that a crystal with residual stress inside induces slippage of the crystal plane, which causes the atomic arrangement plane 2 to curve along with the generation of BPD. Alternatively, conversely, it is considered that the atomic arrangement plane 2 with a large amount of curvature has distortion and becomes the cause of BPD. In either case, the larger the radius of curvature of the atomic arrangement plane (i.e., the smaller the amount of curvature of the atomic arrangement plane), the lower the BPD density.

[0079] As described above, in the method for producing a SiC ingot according to the present embodiment, the atomic arrangement surface 2 of the SiC single crystal 10 used as the seed crystal is flattened, thereby suppressing the occurrence of BPDs in the SiC ingot I. Therefore, a good-quality SiC ingot I with a low BPD density can be obtained.

[0080] Finally, the obtained SiC ingot I is sliced ​​to produce SiC wafers. The cutting direction is as follows: <0001> The wafer is cut perpendicular to the C-plane or at an off angle of 0 to 10° to produce a wafer with a surface parallel to the C-plane or at an off angle of 0 to 10° from the C-plane. The surface of the wafer may be mirror-finished on the (0001) plane, i.e., the Si-plane. The Si-plane is the surface on which epitaxial growth is usually performed. Since SiC ingot I has few BPDs, it is possible to obtain SiC wafers with few BPDs. By using SiC wafers with few BPDs, which are killer defects, it is possible to obtain high-quality SiC epitaxial wafers and increase the yield of SiC devices.

[0081] In addition, when the crucible 100 is heated to sublimate the raw material G, it is preferable to rotate the crucible 100 so as to prevent anisotropy in the circumferential direction. The rotation speed is preferably 0.1 rpm or more. In addition, it is preferable to minimize the temperature change on the growth surface during growth.

[0082] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the specific embodiment, and various modifications and changes are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0083] 1,10 SiC single crystal 10A 1st side 2,22 Atomic arrangement surface 20 wafers 30 Spacer 30A 1st side 30B 2nd side 31 Support stand 40 Adsorption surface 41 Suction hole 50 electrodes 50A Page 1 60 Installation stand 60A Installation surface 100 Crucible 101 Coil 102 Taper Guide A atom I SiC ingot G raw material

Claims

1. a SiC single crystal having a main surface, the main surface being a carbon surface or having an off angle of 10° or less from the carbon surface, and the maximum curvature of the atomic arrangement plane being 20 μm or more; an absolute value of a difference between the amount of warpage of the SiC single crystal and the amount of curvature of the atomic arrangement plane is 10 μm or less; A SiC single crystal that is not attached to any other components.

2. The SiC single crystal according to claim 1 , having a thickness of 5 mm or less.

3. The SiC single crystal according to claim 1 or 2, which is in the form of an ingot.

4. a SiC seed crystal having a maximum curvature amount of an atomic arrangement plane of 20 μm or more; an absolute value of a difference between the amount of warpage of the SiC seed crystal and the amount of curvature of the atomic arrangement plane is 10 μm or less; A SiC seed crystal that is not attached to any other member.

5. The SiC seed crystal of claim 4 having a thickness of 5 mm or less.

6. The SiC seed crystal according to claim 4 or 5, comprising a main surface, the main surface being a carbon surface or having an off angle of 10° or less from the carbon surface.

7. A method for producing a SiC ingot, comprising: growing a crystal by using the SiC seed crystal according to any one of claims 4 to 6.

Citation Information

Patent Citations

  • SiC SINGLE CRYSTAL AND ITS MANUFACTURING METHOD

    JP2004269297A

  • Silicon carbide single crystal, method for producing the same, silicon carbide single crystal wafer, and silicon carbide single crystal ingot

    JP2011111372A

  • Production method of single crystal

    JP2015117143A

  • PASTING METHOD OF SiC SINGLE CRYSTAL, MANUFACTURING METHOD OF SiC INGOT, AND PEDESTAL FOR SiC SINGLE CRYSTAL GROWTH

    JP2020026374A

  • Seed crystal for silicon carbide single crystal growth, method for manufacturing the same, and method for growing crystals using the same

    JP4494856B2