Water-based inkjet inks and printed matter
A water-based inkjet ink with a specific surfactant and solvent combination addresses the challenges of ejection stability and blocking resistance on non-permeable substrates, ensuring high-quality printed images.
Patent Information
- Application Number
- JP2024053809
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing water-based inkjet inks fail to simultaneously achieve high ejection stability, suppress beading, and provide blocking resistance, especially on non-permeable substrates.
A water-based inkjet ink formulation containing a specific combination of acetylene diol-based surfactants with an HLB value of 10 or less, alkanediols with 3 to 5 carbon atoms, and glycol monoethers with 4 to 10 carbon atoms, optimized to enhance surface tension reduction and orientation speed, thereby improving ejection stability and blocking resistance.
The ink achieves excellent ejection stability, suppresses beading, and provides superior blocking resistance on non-permeable substrates, resulting in high-quality printed images.
Smart Images

Figure 0007571911000001 
Figure 0007571911000002 
Figure 0007571911000003
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an aqueous inkjet ink and a printed matter formed using the aqueous inkjet ink. [Background technology]
[0002] Digital printing methods are becoming increasingly popular as printing runs get smaller and needs become more diverse. Digital printing methods do not require plates, so they can handle small runs, reduce costs, and make it possible to downsize printing equipment.
[0003] Inkjet printing is a type of digital printing method, in which minute droplets of ink are ejected and landed on a printing substrate (also referred to simply as "substrate" in this application) from an inkjet head to form an image and / or characters on the printing substrate. Hereinafter, the printing substrate and the image and / or characters formed on the printing substrate by printing ink are collectively referred to as "printed matter." Note that the above "image" also includes solid images and seamless images such as checkered images. Compared to other digital printing methods, inkjet printing is superior in terms of the size and cost of the printing device, running costs during printing, ease of full colorization, etc., and in recent years, it has also been increasingly used in industrial printing applications.
[0004] Inks used in inkjet printing methods are diverse, including oil-based, solvent-based, active energy ray curing, and water-based. Until now, solvent-based and active energy ray curing inks have been used for industrial printing applications. However, in recent years, there has been an increasing demand for water-based inks (inks that contain water as the main component) due to concerns and responses to harmful effects on the environment and people.
[0005] In recent years, there has been an increasing demand for packaging applications such as paper containers, labels, and packaging films as an expansion of the applications of water-based inks used in inkjet printing methods (also referred to as "aqueous inkjet inks" in this application). In such packaging applications, inks that can produce printed matter with high color reproducibility and print image quality, and further withstand practical use, are required not only on poorly permeable substrates such as coated paper and art paper, but also on non-permeable substrates. Here, examples of the non-permeable substrates include polypropylene films (e.g., biaxially oriented polypropylene (OPP) films), polyethylene terephthalate (PET) films, and nylon films.
[0006] Most of the aqueous inkjet inks that have been put to practical use so far have been intended for printing on highly permeable substrates such as plain paper and specialty paper. When such aqueous inkjet inks, particularly those that have not been subjected to any of the below-mentioned procedures, are used on non-permeable substrates, the droplets that land on the substrate remain in a state of high surface tension and do not spread out. Furthermore, when adjacent aqueous inkjet ink droplets come into contact with each other in this state, a force acts on each droplet in a direction that reduces the surface area, resulting in beading. Beading is a phenomenon in which aqueous inkjet ink droplets attract each other and coalesce on the printing substrate, resulting in the appearance of a string of beads of different color shading. Prints in which beading occurs have a significantly reduced print quality.
[0007] In addition, when printing on a non-permeable substrate, the aqueous inkjet ink does not penetrate and is not absorbed into the substrate, so the droplets that land do not dry sufficiently and do not adhere well to the substrate. As a result, when the printed matter is stored in a rolled or stacked state, pressure is applied to the printed surface, causing blocking. Blocking is a phenomenon in which a part of the ink layer is taken up by the printed substrate when the printed substrate attached to the ink layer is peeled off.
[0008] As a method for improving print quality and blocking resistance (suppressing the occurrence of blocking), it is common to reduce the surface tension of the aqueous inkjet ink. For example, a surfactant or a water-soluble organic solvent is added to the aqueous inkjet ink to reduce the surface tension. However, in general, after a droplet of the aqueous inkjet ink lands on a printing substrate, the time until another droplet lands at an adjacent position is only several hundred microseconds to several tens of milliseconds. Therefore, simply adopting the above-mentioned measures to reduce the static surface tension does not allow the droplet of the aqueous inkjet ink to wet and spread sufficiently. As a result, the droplets come into contact with each other while the surface tension remains high, causing beading.
[0009] For example, Patent Document 1 discloses an aqueous inkjet ink in which a polyoxyethylene alkyl ether surfactant is used to control the dynamic surface tension. It is also disclosed that this aqueous inkjet ink can suppress feathering (a phenomenon in which the aqueous inkjet ink irregularly spreads along the fibers of a printing substrate such as fine paper) and the like, thereby obtaining a printed matter with excellent print quality, and can also suppress deterioration of ejection stability. Indeed, the aqueous inkjet ink is effective in improving the print quality of a permeable substrate such as that used in the examples of Patent Document 1. However, when the aqueous inkjet ink is used for printing on the non-permeable substrate, beading occurs due to droplets coming into contact with each other in a state where they are not sufficiently wetted and spread.
[0010] Patent Document 2 discloses an aqueous inkjet ink containing an acetylene diol surfactant having an HLB value of 3 or less and a water-soluble organic solvent having an HLB value of 8 or less. It also discloses that the use of this aqueous inkjet ink suppresses whiteout and aggregation unevenness caused by insufficient spreadability of the aqueous inkjet ink on a poorly permeable substrate, and a printed matter with excellent print quality can be obtained. Indeed, the use of the above surfactant and the above water-soluble organic solvent reduces image defects such as aggregation unevenness in printing on a poorly permeable substrate. However, when the above aqueous inkjet ink is used to print on a non-permeable substrate, the surfactant remains on the surface of the ink layer, which may cause blocking. In addition, since the above surfactant has a small HLB value and is not easily compatible with water, it is likely to be concentrated and oriented at the gas-liquid interface on the nozzle of the inkjet head. As a result, for example, during ejection, the aqueous inkjet ink may overflow from the nozzle to the outside, which may cause nozzle dropout (a phenomenon in which the aqueous inkjet ink is not ejected from the nozzle) and decrease in ejection straightness. Details of these will be described later. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2012-211260 A [Patent Document 2] JP 2017-165809 A Summary of the Invention [Problem to be solved by the invention]
[0012] As described above, until now, there has been no aqueous inkjet ink that simultaneously satisfies all of the requirements for print image quality (suppression of beading), blocking resistance, and ejection stability at high levels, particularly for non-permeable substrates.
[0013] Therefore, one embodiment of the present invention provides an aqueous inkjet ink that has excellent ejection stability, suppresses beading even on non-permeable substrates, and can give printed matter that has excellent blocking resistance. [Means for solving the problem]
[0014] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by an aqueous inkjet ink having the following composition.
[0015] That is, one embodiment of the present invention relates to an aqueous inkjet ink. Another embodiment of the present invention relates to a printed matter obtained using the aqueous inkjet ink. More specifically, the embodiments of the present invention include the following. However, the present invention is not limited to the following embodiments and includes various embodiments. [1] An aqueous inkjet ink comprising a pigment, a surfactant (A), and a water-soluble organic solvent (B), The surfactant (A) includes an acetylene diol-based surfactant (A1) having a structure represented by the following general formula (1) and an HLB value of 10 or less, the water-soluble organic solvent (B) contains an alkanediol (B1) having 3 to 5 carbon atoms and a glycol monoether (B2) having 4 to 10 carbon atoms; The water-based inkjet ink has a mass ratio ((B1) / (B2)) of the content of the alkanediols (B1) having 3 to 5 carbon atoms to the content of the glycol monoethers (B2) having 4 to 10 carbon atoms of 0.8 to 12. General formula (1): [ka] (In the general formula (1), R 1 and R 2Each of m1, m2, n1, and n2 represents an integer of 1 to 10, and the ratio (m1+n1):(m2+n2)=1:9 to 9:1. However, the addition pattern of the ethylene oxide group and the propylene oxide group in the brackets [ ] may be block or random.) [2] The aqueous inkjet ink according to [1], wherein the surfactant (A) further comprises a nonionic surfactant (A2) other than the acetylene diol-based surfactant (A1). [3] The aqueous inkjet ink according to [1] or [2], wherein the content of the acetylene diol surfactant (A1) is 0.1 to 5.0 mass % of the total amount of the aqueous inkjet ink. [4] A printed matter obtained by printing with the aqueous inkjet ink described in any one of [1] to [3].
[0016] The disclosure of this application is related to the subject matter described in Japanese Patent Application No. 2023-089969, filed on May 31, 2023, the entire disclosure of which is incorporated herein by reference. Effect of the Invention
[0017] The aqueous inkjet ink according to one embodiment of the present invention has excellent ejection stability, and even when applied to a non-permeable substrate, it is possible to provide a printed matter that suppresses beading and has excellent printed images and blocking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] An aqueous inkjet ink according to one embodiment of the present invention (hereinafter, simply referred to as "aqueous inkjet ink of this embodiment" or "ink") will be described below. Note that the present invention is not limited to the embodiment described below, and includes embodiments that can be modified without changing the essential parts of the present invention.
[0019] As described above, the aqueous inkjet ink of this embodiment having the above-mentioned configuration can simultaneously achieve high levels of ejection stability, as well as beading suppression and blocking resistance in printed matter on non-permeable substrates, etc. Although the mechanism behind this is not clear, the present inventors speculate as follows. However, the present invention is not limited to the following speculation.
[0020] In order to suppress beading and improve print quality, it is necessary to reduce the surface tension immediately after the ink lands. One method for this is to use a surfactant that has a fast orientation speed to the droplet surface (air-liquid interface). In particular, surfactants with a small molecular weight and low affinity with water have a fast orientation speed to the air-liquid interface and are effective in suppressing beading. Among these surfactants, acetylenic diol surfactants have an acetylene group in which bond rotation does not occur in the molecule. This makes them less likely to deform structurally than other surfactants such as polyoxyethylene alkyl ether surfactants. Therefore, even if a small amount is added, a sufficient amount of acetylenic diol surfactant molecules can be oriented to the air-liquid interface. From the above, from the viewpoint of improving the print quality of printed matter, it is preferable to select an acetylenic diol surfactant with a small molecular weight and low affinity with water. Examples of such compounds include unmodified acetylenic diol surfactants and ethylene oxide modified acetylenic diol surfactants (low molar adducts) as used in the above Patent Document 2.
[0021] On the other hand, such surfactants are naturally present in large amounts on the surface of the ink layer. Also, because of their low molecular weight, it is thought that the surfactant molecules move actively when affected by heat (e.g., outside temperature) or humidity. Therefore, for example, when the printed matter is rolled up and stored, blocking is likely to occur.
[0022] For example, increasing the molecular weight of the surfactant is effective in suppressing blocking. However, when the molecular weight of an ethylene oxide-modified acetylenic diol is increased, the hydrophilicity becomes too high, so that the orientation speed to the gas-liquid interface decreases, and beading occurs. In addition, when the molecular weight of an unmodified acetylenic diol-based surfactant is increased, it cannot exist stably in the aqueous inkjet ink, and there is a risk of precipitation and deterioration of ejection stability.
[0023] In addition, the aqueous inkjet ink near the nozzle of the inkjet head also has an air-liquid interface. Therefore, the surfactant may be concentrated and oriented at the air-liquid interface, causing the aqueous inkjet ink to overflow from the nozzle. For example, if the overflow of the aqueous inkjet ink from the nozzle occurs and progresses during continuous ejection, this can cause ejection defects such as nozzle clogging and reduced straight ejection.
[0024] As described above, while unmodified acetylenic diol surfactants and ethylene oxide-modified acetylenic diol surfactants (low molar adducts) are effective in improving print image quality, they have the problem of causing a decrease in properties such as blocking resistance and ejection stability.
[0025] In contrast, the aqueous inkjet ink of the present embodiment contains, as an acetylenic diol surfactant, an acetylenic diol surfactant (A1) having a structure represented by the above general formula (1) and an HLB value of 10 or less. The acetylenic diol surfactant (A1) contains not only an ethylene oxide structure but also a propylene oxide structure. Since this propylene oxide structure has both hydrophilic and hydrophobic properties, by using it together with the ethylene oxide structure to modify the acetylenic diol surfactant, precise control of the molecular weight and hydrophilicity / hydrophobicity (e.g., HLB value) becomes easy. In particular, by selecting and using an acetylenic diol surfactant (A1) having a structure represented by the above general formula (1) and an HLB value of 10 or less, it becomes possible to maintain hydrophobicity in a molecular weight range where blocking can be suppressed, and the orientation speed to the gas-liquid interface does not decrease excessively.
[0026] In addition, the alkanediols (B1) having 3 to 5 carbon atoms contained in the aqueous inkjet ink of this embodiment are considered to assist the above-mentioned effects. The alkanediols (B1) having 3 to 5 carbon atoms contain multiple hydroxyl groups and have a small molecular weight. Therefore, the alkanediols (B1) have high affinity with water, but do not have excessive affinity with the acetylenic diol surfactant (A1) having an HLB value of 10 or less. The alkanediols (B1) having 3 to 5 carbon atoms also function to retain moisture on the inkjet head nozzle. As a result, the alkanediols (B1) having 3 to 5 carbon atoms can contribute to improving the ejection stability without interfering with the orientation of the acetylenic diol surfactant (A1).
[0027] Furthermore, the aqueous inkjet ink of this embodiment contains glycol monoethers (B2) having 4 to 10 carbon atoms, and the mass ratio of the alkanediols (B1) having 3 to 5 carbon atoms and the glycol monoethers (B2) having 4 to 10 carbon atoms is specified. Although the details are not clear, glycol monoethers having an alkylene oxide structure have a high affinity with the acetylene diol surfactant (A1) having an ethylene oxide structure and a propylene oxide structure. Furthermore, since the glycol monoethers (B2) having 4 to 10 carbon atoms have a small molecular weight, it is considered that the glycol monoethers (B2) molecules are present in a state close to the acetylene diol surfactant (A1). As a result, it is possible to suppress excessive orientation of the acetylene diol surfactant (A1) at the gas-liquid interface, and it is considered that the aqueous inkjet ink does not overflow from the nozzle even during continuous ejection, and suitable ejection stability can be maintained.
[0028] On the other hand, if the orientation of the acetylenic diol surfactant (A1) is suppressed, there is a risk that beading may occur. However, the glycol monoethers (B2) having 4 to 10 carbon atoms have a smaller surface tension than water and other water-soluble organic solvents. Therefore, it is considered that in the droplets of the aqueous inkjet ink on the printing substrate, the glycol monoethers (B2) contribute to a decrease in surface tension together with the acetylenic diol surfactant (A1), thereby suppressing beading.
[0029] As described above, the ink having the configuration of the present invention can solve the above-mentioned problems simultaneously and at a high level.
[0030] Hereinafter, each component constituting the aqueous inkjet ink according to one embodiment of the present invention will be described in detail.
[0031] <Surfactant (A)> (Acetylene diol surfactant (A1)) As described above, the aqueous inkjet ink of this embodiment contains, as a surfactant, an acetylenic diol-based surfactant (A1) having a structure represented by the following general formula (1) and an HLB value of not more than 10. Since the acetylenic diol-based surfactant (A1) has an ethylene oxide structure and a propylene oxide structure, the molecular weight and hydrophilicity / hydrophobicity can be easily controlled.
[0032] General formula (1): [ka]
[0033] In general formula (1), R 1 and R 2 each represents an alkyl group having 1 to 5 carbon atoms which may be branched, EO represents an ethylene oxide group, and PO represents a propylene oxide group. In addition, m1, m2, n1, and n2 each represent an integer of 1 to 10, and (m1+n1):(m2+n2)=1:9 to 9:1. However, the addition pattern of the ethylene oxide group and the propylene oxide group in the brackets [] may be block or random.
[0034] In the above general formula 1, the values of m1, n1, m2, and n2, as well as R 1 and R 2 By changing the structure, the HLB value is adjusted to be 10 or less. In particular, in order to obtain a compound having a suitable HLB value and molecular weight (each of which will be described in detail later), the value of m1+n1 in general formula (1) is preferably 2 to 10, and the value of m2+n2 is preferably 1 to 9. Furthermore, the ratio of the number of ethylene oxide structures to the number of propylene oxide structures represented by (m1+n1):(m2+n2) is preferably 1:2 to 5:1, more preferably 1:1 to 4.5:1, and particularly preferably 1.2:1 to 4:1.
[0035] From the viewpoint of the orientation speed to the gas-liquid interface and the improvement of blocking resistance, the HLB value is 10 or less, preferably 4 to 9, and more preferably 5 to 8. When the HLB value is 10 or less, the moisture absorption of the ink layer constituting the printed matter is reduced, leading to improvement of blocking resistance. Furthermore, by using the ink in combination with an alkanediol (B1) having 3 to 5 carbon atoms and a glycol monoether (B2) having 4 to 10 carbon atoms, it is possible to simultaneously suppress beading and improve blocking resistance and ejection stability.
[0036] The HLB (Hydrophile-Lipophile Balance) value is one of the parameters that indicate the hydrophilicity or hydrophobicity of a material. There are various methods for calculating the HLB value, such as the Griffin method, the Davis method, and the Kawakami method. In this application, the HLB value of the acetylene diol surfactant (A1) is calculated using the Griffin method.
[0037] The Griffin method uses the molecular weight of the target compound to calculate the HLB value according to the following formula (2). Note that the smaller the HLB value, the more hydrophobic the target compound is, and the larger the HLB value, the more hydrophilic the compound is.
[0038] Formula (2): HLB value = 20 x (sum of molecular weights of hydrophilic parts) ÷ (molecular weight of material)
[0039] The acetylene diol surfactant (A1) having an HLB value of 10 or less may be a compound represented by the above general formula (1). Specifically, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol, hexadec-8-yne-7,10-diol, 4,7-dipropyl-dec-5-yne-4,7-diol, 6,9-dimethyl-tetradec-7-yne-6,9-diol, 3,6-diisopropyl-2,7-dimethyloct-4-yne-3,6-diol, octadec-1,1,2,3,4,5,6,7,8,9,10,11,12,13,14,15,16,17,18,19,20,21,22,23,24,25,26,27,28,29,30,31,32,33,34,35,36,37,38,39,40,41,42,43,44,45,46,47,48,49,50,51,52,53,54,55,56,57,58,60,61,72,73,74,75,76,77,82,83,94,95,96,97,98,9 ... Examples of the compounds include ethylene oxide and propylene oxide modified compounds such as keto-9-yne-8,11-diol, 7,10-dimethylhexadec-8-yne-7,10-diol, 5,8-dibutyldodec-6-yne-5,8-diol, 4,7-diisobutyl-2,9-dimethyl-dec-5-yne-4,7-diol, and 5,14-diethyl-8,11-dimethyloctadec-9-yne-8,11-diol. The compounds listed above may be used alone or in combination of two or more. These compounds may be synthesized by a known synthesis method or may be commercially available. Among these, from the viewpoint of compatibility with water and the glycol monoethers (B2), it is preferable to use compounds obtained by modifying 2,4,7,9-tetramethyl-5-decyne-4,7-diol and / or 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol with ethylene oxide and propylene oxide.
[0040] The molecular weight of the acetylene diol surfactant (A1) having a structure represented by the above general formula (1) and an HLB value of 10 or less is preferably 300 to 1,200, more preferably 400 to 900, and even more preferably 450 to 700. The acetylene diol surfactant (A1) having a molecular weight in the above range has a high orientation speed to the gas-liquid interface, so that beading can be suppressed and further deterioration of blocking resistance can be prevented. Note that the molecular weight in this application refers to the formula weight and can be determined by calculation.
[0041] The content of the acetylene diol surfactant (A1) in the aqueous inkjet ink of this embodiment is preferably 0.1 to 5.0 mass %, more preferably 0.2 to 3.5 mass %, further preferably 0.3 to 2.5 mass %, particularly preferably 0.5 to 2.0 mass %, and extremely preferably 0.5 to 1.5 mass % based on the total amount of the aqueous inkjet ink. By using within the above range, it is possible to simultaneously achieve high levels of beading suppression, ejection stability, and blocking resistance.
[0042] [Other surfactants] The aqueous inkjet ink of this embodiment may further contain another surfactant other than the acetylene diol surfactant (A1) having an HLB value of 10 or less (that is, different from the above (A1)).
[0043] In the aqueous inkjet ink of this embodiment, the other surfactant may be one or more selected from the group consisting of ionic (anionic or cationic) surfactants, amphoteric surfactants, and nonionic surfactants (excluding the acetylenic diol surfactant (A1)). In particular, from the viewpoint of compatibility with the glycol monoethers (B2) and the acetylenic diol surfactant (A1), it is preferable to use a nonionic surfactant other than the acetylenic diol surfactant (A1) (also simply referred to as "nonionic surfactant (A2)" in the present application) as the other surfactant.
[0044] <Nonionic surfactant (A2)> As the nonionic surfactant (A2), acetylene diol-based surfactants (excluding acetylene diol-based surfactant (A1)), acetylene monool-based surfactants, siloxane-based surfactants, fluorine-based surfactants, polyoxyalkylene monoalkyl ether-based surfactants (wherein the oxyalkylene group is an oxyethylene group and / or an oxypropylene group, and the number of said oxyalkylene groups is 5 to 100 and / or the number of carbon atoms in the terminal alkyl group is 5 to 22); and the like can be used. These other surfactants may be used alone or in combination of two or more.
[0045] Among them, it is preferable to use, as the nonionic surfactant (A2), one or more selected from the group consisting of acetylenic diol surfactants (excluding acetylenic diol surfactants (A1)), siloxane surfactants, and polyoxyalkylene monoalkyl ether surfactants (wherein the oxyalkylene group is an oxyethylene group and / or an oxypropylene group, and the number of the oxyalkylene group is 5 to 100, and / or the number of carbon atoms of the terminal alkyl group is 5 to 22). These are preferable in that they function similarly to glycol monoethers (B2) by being compatible with the acetylenic diol surfactant (A1) or emulsified with the acetylenic diol surfactant (A1), and can be expected to improve both discharge stability and suppress beading.
[0046] Among the above, it is preferable to use a siloxane-based surfactant as the nonionic surfactant (A2). The siloxane-based surfactant has a high compatibility with the acetylene diol-based surfactant (A1), and can greatly improve the ejection stability. In addition, after the droplets of the aqueous inkjet ink land on the printing substrate, the siloxane-based surfactant is oriented on the droplet surface with a delay from the orientation of the acetylene diol-based surfactant (A1). As a result, the droplets can be sufficiently wetted and spread, beading can be suppressed to a higher level, and blocking resistance can be improved.
[0047] From the viewpoint of improving the blocking resistance and ejection stability of the printed matter, it is preferable to use a siloxane-based surfactant and an acetylene diol-based surfactant (excluding the acetylene diol-based surfactant (A1)) in combination as the nonionic surfactant (A2). In one embodiment, the total content of the siloxane-based surfactant and the acetylene diol-based surfactant (excluding the acetylene diol-based surfactant (A1)) is preferably 20 to 850 mass%, and particularly preferably 40 to 400 mass%, relative to the content of the acetylene diol-based surfactant (A1). When the total content is adjusted to within the above range, it is possible to easily improve the beading suppression effect and blocking resistance while realizing a suitable print image quality.
[0048] In another embodiment, the content of the acetylenic diol surfactant (excluding the acetylenic diol surfactant (A1)) is preferably 10 to 250 mass % relative to the content of the acetylenic diol surfactant (A1), and particularly preferably 25 to 120 mass %. When the content is adjusted as described above, the effect of the acetylenic diol surfactant (A1) can be suitably exhibited, and the suppression of beading and blocking, as well as the improvement of discharge stability, can all be simultaneously achieved.
[0049] On the other hand, when a siloxane-based surfactant is used as the nonionic surfactant (A2), it is preferable to use it in combination with two or more siloxane-based surfactants with different orientation speeds to the interface, from the viewpoint of suppressing beading and easily obtaining a printed matter with excellent print quality. Since the orientation speed depends on the molecular structure of the surfactant, examples of the above-mentioned "two or more siloxane-based surfactants with different orientation speeds" include two or more modified siloxane-based surfactants with different modified species and / or modified positions; and / or two or more siloxane-based surfactants with different mass average molecular weights; etc. In addition, examples of the above-mentioned "two or more modified siloxane-based surfactants with different modified species and / or modified positions" include a combination of a polyether-modified siloxane-based surfactant having a polyether structure in the side chain and a polyether-modified siloxane-based surfactant having a polyether structure at both ends of the molecular chain, etc.
[0050] On the other hand, an example of the "two or more siloxane-based surfactants having different mass average molecular weights" is a combination of siloxane-based surfactants whose difference in mass average molecular weight is 800 to 15,000. From the viewpoint of obtaining printed matter with excellent print quality, the difference in mass average molecular weight is more preferably 1,200 to 12,000, and particularly preferably 1,500 to 10,000. The mass average molecular weight of the siloxane surfactant can be measured by gel permeation chromatography. Specifically, for example, it can be measured using a TSKgel column (manufactured by Tosoh Corporation) and an HLC-8120GPC (manufactured by Tosoh Corporation) equipped with an RI detector, using THF as a developing solvent.
[0051] The content of the nonionic surfactant (A2) in the aqueous inkjet ink of this embodiment is preferably 0.1 to 5.0 mass% of the total amount of the aqueous inkjet ink, more preferably 0.2 to 2.5 mass%, even more preferably 0.4 to 2.0 mass%, and particularly preferably 0.4 to 1.5 mass%. By using the nonionic surfactant (A2) within the above range, it is possible to achieve high levels of all of the suppression of beading, ejection stability, and blocking resistance.
[0052] Examples of commercially available acetylenic diol surfactants (excluding the acetylenic diol surfactants (A1)) that can be used as the nonionic surfactant (A2) are shown below. Surfynol 61, 104E, 104H, 104A, 104BC, 104DPM, 104PA, 104PG-50, 420, 440, 465, 485, SE, SE-F, Dynol 604, 607 (manufactured by Evonik), Olfine E1004, E1010, E1020, PD-001, PD-002W, PD-004, PD-005, EXP.4001, EXP.4200, EXP.4123, EXP.4300 (manufactured by Nissin Chemical Industry Co., Ltd.). The above-listed products may be used alone or in combination of two or more. These compounds may be synthesized by a conventionally known synthesis method or may be commercially available products.
[0053] Among these, from the viewpoint of compatibility with water, the alkanediols (B1) and the glycol monoethers (B2) and from the viewpoint of blocking resistance, it is preferable to use compounds obtained by modifying 2,4,7,9-tetramethyl-5-decyne-4,7-diol or 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol with ethylene oxide, such as Surfynol 465, 485, Dynol 604, 607, and Olfine E1010, 1020.
[0054] Examples of commercially available siloxane-based surfactants that can be used as the nonionic surfactant (A2) are shown below. BY16-201, FZ-77, FZ-2104, FZ-2110, FZ-2162, F-2123, L-7001, L-7002, SF8427, SF8428, SH3749, SH8400, 8032ADDITIVE, SH3773M (manufactured by Dow Corning Toray Co., Ltd.), TEGO Glide 100, TEGO Glide 410, TEGO Glide 432, TEGO Glide 435, TEGO Glide 440, TEGO Glide 450, TEGO Twin 4000, TEGO Twin4100, TEGO Wet250, TEGO Wet260, TEGO Wet270, TEGO Wet280 (manufactured by Evonik), SAG-002, SAG-503A (manufactured by Nissin Chemical Industry Co., Ltd.), BYK-331, BYK-333, BYK-345, BYK-346, BYK-347, BYK-348, BYK-349, BYK-3420, BYK-UV3500, BYK-UV3510 (manufactured by BYK-Chemie), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-6004, KF-6011, KF-6012, KF-6013, KF-6015, KF-6016, KF-6017, KF-6043, KF-615A, KF-640, KF-642, KF-643 (manufactured by Shin-Etsu Chemical Co., Ltd.). The above-listed products may be used alone or in combination of two or more. These compounds may be synthesized by a conventionally known synthesis method or may be commercially available products.
[0055] Examples of commercially available polyoxyalkylene monoalkyl ether surfactants that can be used as the nonionic surfactant (A2) are shown below. Nonion series such as Nonion K-204, 220, 230, 2100W, P-208, 210, 213, S-202, 207, 215, 220, 250 (manufactured by NOF Corp.), Emulgen series (manufactured by Kao Corp.), Tergitol L series, Tergitol X series, Tergitol TWN series (manufactured by Dow Chemical Co.). The above-listed products may be used alone or in combination of two or more. These compounds may be synthesized by a conventionally known synthesis method or may be commercially available products.
[0056] The total content of the surfactants contained in the aqueous inkjet ink of this embodiment is preferably 0.1 to 5 mass % of the total amount of the aqueous inkjet ink, more preferably 0.2 to 4.5 mass %, even more preferably 0.3 to 4 mass %, and particularly preferably 0.4 to 3.5 mass %.
[0057] <Water-soluble organic solvent (B)> The aqueous inkjet ink of this embodiment contains a water-soluble organic solvent (B). As described above, the water-soluble organic solvent (B) contains an alkanediol (B1) having 3 to 5 carbon atoms and a glycol monoether (B2) having 4 to 10 carbon atoms. In this specification, the term "water-soluble organic solvent" refers to a solvent that has a solubility of 1 mass % or more in water at 25°C and is a liquid at 25°C.
[0058] (Alkanediols having 3 to 5 carbon atoms (B1)) The alkanediols (B1) having 3 to 5 carbon atoms are considered to contribute to improving the ejection stability because they exhibit moisturizing properties without inhibiting the orientation of the acetylene diol surfactant (A1). As the alkanediols (B1) having 3 to 5 carbon atoms, 1,2-propanediol, 1,2-butanediol, 1,2-pentanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, 3-methyl-1,3-butanediol, 2,2-dimethyl-1,3-propanediol, etc. can be used. These compounds may be used alone or in combination of two or more.
[0059] The SP value of alkanediols (B1) having 3 to 5 carbon atoms is 12.0 to 14.0 (cal / cm 3) 1 / 2 and more preferably 12.5 to 14.0 (cal / cm 3 ) 1 / 2 If the alkanediol (B1) is within the above range, it will not have excessive affinity with the acetylenic diol surfactant (A1). As a result, the orientation of the acetylenic diol surfactant (A1) will not be excessively hindered, which not only improves the ejection stability but also contributes to suppressing beading.
[0060] The above "SP value" is an abbreviation for solubility parameter. In this specification, it refers to a value calculated by Fedor's estimation method (unit: cal / cm 3 ) 1 / 2 (Let us assume that) is used.
[0061] Among the alkanediols (B1) having 3 to 5 carbon atoms (preferably the alkanediols (B1) having the above-mentioned SP value), it is particularly preferable to use 1,2-propanediol and / or 1,2-butanediol. These water-soluble organic solvents are highly hydrophilic, but do not have excessive affinity with the acetylene diol surfactant (A1). Therefore, the water-soluble organic solvents do not inhibit the orientation of the acetylene diol surfactant (A1) at the gas-liquid interface, and can maximize the effect of the surfactant, which is considered to facilitate the production of a printed matter without beading. In addition, after landing on the printing substrate, these water-soluble organic solvents volatilize quickly, resulting in a printed matter with excellent drying properties and blocking resistance. In addition, these water-soluble organic solvents have the property of being less likely to destroy the dispersion state of the pigment described below, and can be used preferably from the viewpoint of preventing deterioration of the storage stability of the aqueous inkjet ink.
[0062] The content of the alkanediol (B1) having 3 to 5 carbon atoms in the aqueous inkjet ink of this embodiment is preferably 5 to 35 mass % of the total amount of the aqueous inkjet ink, more preferably 10 to 30 mass %, and even more preferably 10 to 25 mass %.
[0063] (C4-10 glycol monoethers (B2)) On the other hand, the aqueous inkjet ink of this embodiment contains glycol monoethers (B2) having 4 to 10 carbon atoms, which has high affinity with the acetylenic diol surfactant (A1) and can suppress excessive orientation, thereby improving the ejection stability. In addition, the glycol monoethers (B2) having 4 to 10 carbon atoms contribute to reducing the surface tension on the printing substrate together with the acetylenic diol surfactant (A1), thereby suppressing beading. Examples of glycol monoethers (B2) having 4 to 10 carbon atoms include ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monophenyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, and dipropylene glycol monobutyl ether. These compounds may be used alone or in combination of two or more.
[0064] Among them, it is preferable to use one or more selected from diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether. It is more preferable to use one or more selected from diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monohexyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monobutyl ether. These water-soluble organic solvents are not excessively compatible with water and are easily oriented at the gas-liquid interface. In addition, they have a moderate affinity with the acetylenic diol surfactant (A1) (and the nonionic surfactant (A2) when used), and the orientation speed of these surfactants at the gas-liquid interface is adjusted, thereby improving the discharge stability. Furthermore, they contribute to reducing the surface tension on the printing substrate together with the acetylenic diol surfactant (A1), so that beading can also be suppressed. In addition, these water-soluble organic solvents not only have excellent drying properties, but also function as film-forming assistants for the resin described below, thereby contributing to improved blocking resistance.
[0065] In particular, since the above-mentioned effects are significantly exhibited, in one embodiment, one or more compounds selected from the group consisting of propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether are preferably used as the glycol monoethers (B2). Particularly preferably, propylene glycol monomethyl ether and / or propylene glycol monoethyl ether can be used. Propylene glycol monomethyl ether and propylene glycol monoethyl ether are compounds with small molecular weights, but have a PO group like the acetylenic diol surfactant (A1). Therefore, it is considered that an interaction occurs between these water-soluble organic solvents and the acetylenic diol surfactant (A1), and they are oriented at the gas-liquid interface while maintaining a suitable compatibilized state. As a result, a modest effect is exhibited in terms of discharge stability due to moisture retention or compatibilization, and beading suppression due to improved orientation speed.
[0066] The content of the glycol monoethers (B2) having 4 to 10 carbon atoms in the aqueous inkjet ink of this embodiment is preferably 0.5 to 20 mass %, more preferably 1 to 15 mass %, and even more preferably 2 to 10 mass %, of the total amount of the aqueous inkjet ink.
[0067] In the aqueous inkjet ink of this embodiment, the affinity of the acetylenic diol surfactant (A1) is controlled, and from the viewpoint of simultaneously achieving beading suppression, ejection stability, and blocking resistance, the mass ratio ((B1) / (B2)) of the content of the alkanediols (B1) having 3 to 5 carbon atoms to the content of the glycol monoethers (B2) having 4 to 10 carbon atoms is 0.8 to 12, more preferably 1 to 8, and even more preferably 1.5 to 5. Within the above range, the affinity of the acetylenic diol surfactant (A1) is optimized, and the beading suppression effect can be maximized. In addition, the ejection stability can be improved by suppressing concentrated orientation of the surfactant at the gas-liquid interface. Furthermore, since the aqueous inkjet ink has excellent drying properties, it is possible to prevent deterioration of blocking resistance.
[0068] In order to simultaneously realize all of the improvements in ejection stability, the suppression of beading, and the improvement of blocking resistance, it is preferable to further consider the drying behavior of the water-soluble organic solvent described above. Specifically, the energy required to evaporate the alkanediol (B1) having 3 to 5 carbon atoms is preferably 1.2 to 20 times, more preferably 2.5 to 16 times, and particularly preferably 3.5 to 13 times, the energy required to evaporate the glycol monoether (B2) having 4 to 10 carbon atoms.
[0069] Although the detailed mechanism is unclear, by using the alkanediols (B1) having 3 to 5 carbon atoms and the glycol monoethers (B2) having 4 to 10 carbon atoms in combination so that the energy ratio falls within the above range, it is possible to prevent the water-soluble organic solvent from volatilizing before the effects of controlling the affinity with the acetylenic diol surfactant (A1) and adjusting the orientation speed of the acetylenic diol surfactant (A1) are achieved. In addition, as the aqueous inkjet ink dries on the printing substrate, the balance between the amount of the alkanediols (B1) and the amount of the glycol monoethers (B2) does not fluctuate significantly. As a result, it is possible to improve the ejection stability, as well as to suppress beading and improve blocking resistance in printed matter on non-permeable substrates.
[0070] The energy required to evaporate the water-soluble organic solvent can be calculated by the following formula (3).
[0071] Formula (3): VE = (BP-25) x MP x SH
[0072] In the above formula (3), VE is the energy (cal) required to evaporate the target water-soluble organic solvent contained in the aqueous inkjet ink. BP is the boiling point (°C) of the water-soluble organic solvent at 1 atmospheric pressure. MP is the content (mass%) of the water-soluble organic solvent in the aqueous inkjet ink. SH is the specific heat (cal / g·°C) of the water-soluble organic solvent at 25°C. Furthermore, a value calculated by the Missenard estimation method can be used as the specific heat.
[0073] The Missenard estimation method uses the sum of values determined according to the molecular structure and temperature of the target compound as the specific heat (cal / mol·°C) at the above temperature. However, the unit of specific heat calculated by the Missenard estimation method is "cal / mol·°C". Therefore, in the above formula (3), the specific heat value of the target compound obtained by the Missenard estimation method is divided by the molecular weight of the compound. An example of values at 25°C determined according to the above molecular structure is shown in Table 1.
[0074] [Table 1]
[0075] (Other water-soluble organic solvents) The aqueous inkjet ink of this embodiment may contain a water-soluble organic solvent other than the alkanediol (B1) having 3 to 5 carbon atoms and the glycol monoether (B2) having 4 to 10 carbon atoms (referred to as "other water-soluble organic solvents" in the present application).
[0076] In the aqueous inkjet ink of this embodiment, the other water-soluble organic solvents may include alkanediols having 6 carbon atoms; alkanetriols (having 3 to 6 carbon atoms); polyoxyalkylene diols (having oxyalkylene groups which are oxyethylene groups or oxypropylene groups and having 2 to 4 oxyalkylene groups); glycol monoethers ((poly)oxyalkylene monoalkyl ethers) (having oxyalkylene groups which are oxyethylene groups or oxypropylene groups and having 1 to 4 oxyalkylene groups and having 1 to 4 carbon atoms in the terminal alkyl group, those having 11 or more carbon atoms); glycol diethers ((poly)oxyethylene dialkyl ethers) (wherein the number of oxyalkylene groups is 1 to 4 and the number of carbon atoms in the terminal alkyl groups is 1 to 4); lactams (wherein the number of atoms constituting the lactam ring is 5 to 7. An alkyl group having 1 to 2 carbon atoms, a hydroxyalkyl group having 1 to 2 carbon atoms, or a vinyl group may be bonded to the nitrogen atom and / or carbon atom constituting the lactam ring); alkanolamines (wherein the number of amino groups is 1, the number of hydroxyl groups is 1 to 3, and the number of carbon atoms is 3 to 9); and the like can be used. These other water-soluble organic solvents exemplified above may be used alone or in combination of two or more.
[0077] In the present application, the term "(poly)oxyalkylene" refers to oxyalkylene and polyoxyalkylene.
[0078] The total content of the water-soluble organic solvents in the aqueous inkjet ink of this embodiment is preferably 5 to 50 mass %, more preferably 9 to 40 mass %, even more preferably 12 to 35 mass %, and particularly preferably 15 to 30 mass %, of the total amount of the aqueous inkjet ink.
[0079] <Resin> The water-based inkjet ink of this embodiment preferably contains a resin.
[0080] Generally, water-soluble resins and resin microparticles are known as the form of resins used in aqueous inkjet inks. In the aqueous inkjet ink of this embodiment, the resin contained in the aqueous inkjet ink of this embodiment may be a water-soluble resin or may be resin microparticles. Also, a combination of a water-soluble resin and resin microparticles may be used.
[0081] In this specification, a resin having a solubility of 1 g or more in 100 g of water at 25° C. is referred to as a “water-soluble resin”, and a resin having a solubility of less than 1 g is referred to as a “water-insoluble resin”. In addition, among the above water-insoluble resins, a resin that is dispersed in water in the form of particles and has a volume-based median diameter (also referred to as “D50” in this application) of 10 to 1,000 nm is referred to as a “resin fine particle”.
[0082] In this specification, D50 is a value measured in an environment of 25° C. using a dynamic light scattering particle size distribution measuring device such as Microtrac-Bell's “Nanotrac UPA-EX150”.
[0083] Examples of resins that can be used in the aqueous inkjet ink of this embodiment include acrylic resins, styrene resins, maleic acid (anhydride)-based resins, styrene-maleic acid (anhydride) resins, olefin-maleic acid (anhydride) resins, urethane resins, polyester resins, vinyl chloride resins, vinyl chloride-vinyl acetate resins, polyolefin resins, vinyl alcohol resins, etc. These resins may be used alone or in combination of two or more.
[0084] In this specification, the term "acrylic resin" refers to a resin using an acrylic acid ester and / or a methacrylic acid ester as a polymerizable monomer (a styrene-based monomer may also be used). Also, the term "maleic acid (anhydride)" refers to at least one selected from "maleic acid" and "maleic anhydride".
[0085] The resin is used for any purpose, for example, a pigment dispersion purpose, a binder purpose, a wax purpose, a thickening purpose, etc. Furthermore, the resin may be used for a single purpose or may have a plurality of purposes. Among these, from the viewpoint of improving blocking resistance, the above resins are preferably used for binder applications and / or pigment dispersion applications.
[0086] (binder resin) In one embodiment, the aqueous inkjet ink preferably contains a resin used as a binder (also referred to as a "binder resin" in the present application) in order to improve the coating resistance and blocking resistance of the printed matter. When the aqueous inkjet ink of this embodiment contains a binder resin, the type of resin used as the binder resin may be any of those listed above. In particular, the binder resin is preferably one or more types selected from the group consisting of acrylic resins, urethane resins, and polyester resins. Furthermore, the form of the resin preferably used is resin fine particles.
[0087] The content of the binder resin in the aqueous inkjet ink of this embodiment is preferably 0.1 to 20 mass % of the total amount of the aqueous inkjet ink, more preferably 0.2 to 15 mass %, even more preferably 0.3 to 12 mass %, and particularly preferably 0.5 to 10 mass %.
[0088] (Pigment dispersion resin) When the aqueous inkjet ink of this embodiment contains a pigment as a colorant, the blocking resistance of the printed matter can be improved by using a resin used for dispersing pigments (also referred to as "pigment dispersion resin" in this specification). In this case, the type of resin used as the pigment dispersion resin may be one of those listed above. In particular, the pigment dispersion resin is preferably one or more types selected from the group consisting of styrene-maleic anhydride resin, olefin-maleic anhydride resin, and acrylic resin.
[0089] <Coloring agent> [Pigment] The aqueous inkjet ink of the present embodiment contains a colorant. In addition, it is preferable that the colorant contains a pigment, since this can provide printed matter with high density or hiding power and excellent light resistance, water resistance, and the like.
[0090] As the pigment, any conventionally known organic or inorganic pigment can be used. For example, pigments represented by the following color index names can be used. Specifically, red pigments include CI Pigment Red 52, 5, 7, 9, 12, 17, 22, 23, 31, 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 57:1, 57:2, 112, 122, 123, 146, 147, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 184, 188, 202, 207, 209, 254, 255, 260, 264, 266, 269, 282; Violet pigments include CI Pigment Violet 19, 23, 29, 32, 36, 37, 42, 50; Orange pigments include CI Pigment Orange 1, 2, 3, 5, 7, 13, 14, 15, 16, 22, 34, 36, 38, 40, 43, 47, 48, 49, 51, 52, 53, 60, 61, 62, 64, 65, 66, 69, 71, 73; Blue pigments include CI Pigment Blue 15, 15:3, 15:4, 15:6, 16, 60, 64, and 79; As green pigments, CI Pigment Green 7, 10, 36, 48; Yellow pigments include CI Pigment Yellow 1, 2, 3, 5, 12, 13, 14, 16, 17, 24, 73, 74, 83, 87, 93, 94, 95, 97, 98, 109, 110, 111, 112, 120, 126, 127, 128, 129, 137, 138, 139, 147, 150, 151, 154, 155, 166, 167, 168, 170, 180, 185, 213; Black pigments include CI Pigment Black 1, 7, and 11; White pigments include CI Pigment White 4, 5, 6, 21, etc. These pigments may be used alone or in combination of two or more. A solid solution of two or more of the pigments listed above may also be used as a pigment.
[0091] The content of the pigment contained in the aqueous inkjet ink of this embodiment may be adjusted depending on the use of the printed matter produced using the aqueous inkjet ink. In one embodiment, the content of the pigment is preferably 0.5 to 30% by mass in the total amount of the aqueous inkjet ink. In the case of inks other than white aqueous inkjet inks (aqueous white inks), the content of the pigment is more preferably 1 to 15% by mass, and particularly preferably 1.5 to 10% by mass, from the viewpoint of obtaining a printed matter with high density without deteriorating the discharge stability of the aqueous inkjet ink. On the other hand, in the case of aqueous white inks, the content of the pigment is more preferably 5 to 25% by mass, and particularly preferably 10 to 20% by mass, from the viewpoint of obtaining a printed matter with high concealing property without deteriorating the discharge stability of the aqueous white ink.
[0092] <Other ingredients> The aqueous inkjet ink of the present embodiment may contain, in addition to the above-mentioned components, a pH adjuster, a preservative, and other additives. Examples of the other additives include a crosslinking agent, a preservative, an ultraviolet absorber, and an infrared absorber. For each of these components, one or more conventionally known compounds may be used.
[0093] <Water> The water contained in the aqueous inkjet ink of this embodiment is preferably ion-exchanged water and / or reverse osmosis water. The content of water contained in the aqueous inkjet ink is preferably 30 to 90% by mass, and particularly preferably 45 to 85% by mass, of the total amount of the aqueous inkjet ink.
[0094] <Method of manufacturing water-based inkjet ink> The aqueous inkjet ink of the present embodiment can be produced by a conventionally known method. For example, when a water-insoluble colorant (water-insoluble colorant) is used as a colorant, the water-insoluble colorant is dispersed in a medium (aqueous medium) containing at least water to produce a water-insoluble colorant dispersion. On the other hand, when a water-soluble colorant (water-soluble colorant) is used as a colorant, the water-soluble colorant is dissolved in a water-based medium to produce a water-soluble colorant aqueous solution. Then, water, a surfactant (A), a water-soluble organic solvent (B), etc. are added to the water-insoluble colorant dispersion and / or the water-soluble colorant aqueous solution, and the mixture is thoroughly stirred and mixed, and then coarse particles are removed by a method such as filtration or centrifugation. However, the method for producing the aqueous inkjet ink of the present embodiment is not limited to the above-mentioned method.
[0095] <Characteristics of water-based inkjet ink> The aqueous inkjet ink of the present embodiment preferably has a viscosity of 3 to 15 mPa·s at 25°C. In this viscosity range, droplets of the aqueous inkjet ink can be stably ejected not only from an inkjet head having an ejection frequency of about 4 to 10 KHz, but also from an inkjet head having a high ejection frequency of about 20 to 70 KHz. In particular, when the aqueous inkjet ink of the present embodiment has a viscosity of 4 to 10 mPa·s at 25°C, the aqueous inkjet ink can be stably ejected even when an inkjet head having a design resolution of 600 dpi or more is used. In this specification, the viscosity is measured in a 25°C environment using a cone-plate type rotational viscometer (E-type viscometer, cone angle 1°34') such as the "TVE25L type viscometer" manufactured by Toki Sangyo Co., Ltd.
[0096] In order to obtain an aqueous inkjet ink excellent in ejection stability and print quality of printed matter, the aqueous inkjet ink of this embodiment preferably has a static surface tension of 18 to 35 mN / m, and particularly preferably 21 to 32 mN / m, at 25° C. In this specification, the static surface tension is a value measured in an environment of 25° C. using the Wilhelmy method (plate method) with an "Automatic Surface Tensiometer CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd.
[0097] When the aqueous inkjet ink of this embodiment contains a water-insoluble colorant, in order to achieve both high levels of ejection stability and high levels of density or hiding power of the printed matter, the volume-based median diameter (D50) of the water-insoluble colorant is preferably 30 to 450 nm, more preferably 50 to 400 nm, and particularly preferably 70 to 350 nm.
[0098] <Water-based inkjet ink set> The aqueous inkjet ink of the present embodiment may be used alone, or may be used as an aqueous inkjet ink set by combining two or more aqueous inkjet inks. Examples of the aqueous inkjet ink set include a set of four aqueous inkjet inks (process color ink set) consisting of a cyan aqueous inkjet ink (aqueous cyan ink), a magenta aqueous inkjet ink (aqueous magenta ink), a yellow aqueous inkjet ink (aqueous yellow ink), and a black aqueous inkjet ink (aqueous black ink); a set of five aqueous inkjet inks obtained by adding an aqueous white ink to the process color ink set; and the like. It is preferable that all the aqueous inkjet inks constituting the aqueous inkjet ink set satisfy the requirements of the above-mentioned embodiment of the present invention.
[0099] <Ink-pretreatment liquid set> The aqueous inkjet ink of this embodiment and the aqueous inkjet ink set can also be used in a form combined with a pretreatment liquid containing an aggregating agent (in the form of an ink-pretreatment liquid set). By applying a pretreatment liquid containing an aggregating agent onto a printing substrate before printing with the aqueous inkjet ink, a layer (ink aggregating layer) can be formed that intentionally aggregates the solid components contained in the aqueous inkjet ink. By landing the aqueous inkjet ink on the ink aggregating layer, it is possible to prevent the droplets of the aqueous inkjet ink from coalescing and mixing, and to significantly improve the print quality of the printed matter.
[0100] As the flocculant, for example, water-soluble inorganic or organic salts containing polyvalent metal ions, and resins having cationic groups and in which the cationic group equivalent is greater than the anionic group equivalent can be used.
[0101] <Inkjet printing method> The aqueous inkjet ink of this embodiment is used in the inkjet printing method described above. A printing method using the inkjet printing method typically includes an ink ejection step and a drying step of the ejected ink. In the above printing method, the aqueous inkjet ink of this embodiment is ejected onto a printing substrate from an inkjet head having fine nozzles (ejection step). In addition, the aqueous inkjet ink ejected onto the printing substrate is preferably dried by a drying mechanism (drying step).
[0102] (Discharge process) One example of the operation method of the inkjet head in the ejection process is a shuttle (scan) method in which the inkjet head is scanned back and forth in a direction perpendicular to the transport direction of the printing substrate to eject and record the aqueous inkjet ink. Another example of the operation method is a single-pass method in which the aqueous inkjet ink is ejected and recorded when the printing substrate passes under a fixedly arranged inkjet head. The inkjet head equipped with the aqueous inkjet ink of this embodiment may adopt either the shuttle method or the single-pass method. Among them, the single-pass method is preferably selected because the landing position of the droplets of the aqueous inkjet ink is less likely to shift and the print quality of the printed matter is improved.
[0103] The method of ejection from the inkjet head can be selected from any known methods, such as a piezoelectric method that utilizes the volume change of a piezoelectric element, a thermal method that ejects water-based inkjet ink by bubbles generated by heating a heater, and a valve method that ejects pressurized water-based inkjet ink by opening and closing a nozzle cover (valve) with a solenoid.
[0104] The amount of droplets of the aqueous inkjet ink ejected from the inkjet head is preferably 0.5 to 20 picoliters, and particularly preferably 0.5 to 15 picoliters, from the viewpoints of reducing the drying load and improving the print quality. In addition, from the viewpoint of improving the print quality, it is preferable to adjust the printing conditions (specifically, the driving frequency and number of inkjet heads, and the printing speed). In one embodiment, the printing conditions may be adjusted so that the recording resolution of the printed matter is preferably 600 dpi or more, more preferably 1200 dpi or more.
[0105] (drying process) Examples of drying methods employed in the drying mechanism used in the drying step include heat drying, hot air drying, infrared (e.g., infrared with a wavelength of 700 to 2500 nm) drying, microwave drying, and drum drying. In the drying step, one or more of these methods can be selected and used as desired. When two or more of the above drying methods are used, the drying methods may be used separately (e.g., consecutively) or simultaneously. For example, by using the heat drying method and the hot air drying method in combination, the aqueous inkjet ink can be dried more quickly than when each method is used alone.
[0106] In particular, from the viewpoint of preventing bumping of the liquid components in the aqueous inkjet ink and obtaining a printed matter with excellent print quality, when a heat drying method is employed, the drying temperature is preferably 35 to 100° C. When a hot air drying method is employed, the hot air temperature is preferably 50 to 250° C. From the same viewpoint, when an infrared drying method is employed, it is preferable that 50% or more of the integrated value of the total output of the irradiated infrared rays is in the wavelength region of 700 to 1500 nm.
[0107] <Printed material> A printed matter according to one embodiment of the present invention has a printing substrate and a printing layer containing an image or characters formed by printing the aqueous inkjet ink of the present embodiment on the printing substrate. The printing can be suitably carried out according to an inkjet printing method. The details of the printing method and printing conditions are as described above.
[0108] (Printing base material) The printing substrate on which the aqueous inkjet ink of this embodiment is printed is not particularly limited, and any known substrate such as a permeable substrate, a poorly permeable substrate, or a non-permeable substrate can be used.
[0109] In this embodiment, the permeability of the printing substrate is judged by the amount of water absorption measured by a dynamic scanning absorptiometer. Specifically, the amount of pure water absorption measured by the following method for a contact time of 100 msec is 1 g / m 2A printing substrate with a water absorption of less than 1 g / m is called a "non-permeable substrate". 2 More than 6g / m 2 A printing substrate with a water absorption of less than 6g / m2 is called a "hardly permeable substrate." 2 The printing substrate described above is referred to as a "permeable substrate." The water absorption of the printing substrate can be measured, for example, using a dynamic scanning absorptiometer (e.g., "KM500win" manufactured by Kumagai Riki Kogyo Co., Ltd.) set under the conditions shown below, using a sample of the printing substrate approximately 15 to 20 cm square, in an environment of 23°C and 50% RH. Measurement method: Spiral Method ·Measurement start radius: 20mm Measurement end radius: 60mm ·Contact time: 10~1,000msec Number of sampling points: 19 (measured at approximately equal intervals relative to the square root of contact time) Scanning distance: 7mm Rotating table speed switching angle: 86.3 degrees Head box conditions: width 5mm, slit width 1mm
[0110] Examples of permeable substrates include uncoated paper such as sawdust paper, medium-quality paper, fine paper, and recycled paper, fabrics such as cotton, synthetic fiber fabrics, silk, hemp, and nonwoven fabrics, and leather. Among these, uncoated paper such as sawdust paper, medium-quality paper, fine paper, and recycled paper is preferably used because it can provide printed matter with excellent print quality.
[0111] Examples of non-permeable substrates or poorly permeable substrates include plastic films and sheets such as polyvinyl chloride sheets, polyethylene terephthalate (PET) films, polypropylene films, polyethylene sheets, nylon films, nylon sheets, polystyrene films, polystyrene sheets, and polyvinyl alcohol films; coated papers such as coated paper, art paper, and cast paper; metals such as aluminum, iron, stainless steel, and titanium; and glass.
[0112] The printing substrates listed above may have a smooth surface or may have an uneven surface. The printing substrates may be transparent, semi-transparent, or opaque. The printing substrates may be in the form of rolls or sheets. In addition, two or more of the printing substrates listed above may be bonded together to be used as the printing substrate. A peelable adhesive layer or the like may be provided on the opposite side of the printing surface, or an adhesive layer or the like may be provided on the printing surface after printing.
[0113] The printing surface of the printing substrates listed above may be subjected to surface modification such as corona treatment and plasma treatment. When the surface is modified, the wettability and spreadability of the aqueous inkjet ink of the present embodiment is improved, and a printed matter having excellent print quality and drying properties and excellent abrasion resistance and adhesion to the substrate can be obtained due to the uniformity of the printed surface. EXAMPLES
[0114] The aqueous inkjet ink of the present embodiment will be described in more detail below with reference to examples and comparative examples. In the following description, "parts" and "%" refer to "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0115] <Production example of binder resin 1> A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 72.4 parts of 2-butanone and substituted with nitrogen gas. The reaction vessel was heated to 80°C, and a mixture of 15 parts of styrene, 4.5 parts of methacrylic acid, 5.0 parts of 2-hydroxyethyl methacrylate, 20 parts of stearyl methacrylate, 55.5 parts of methyl methacrylate, and 4 parts of V-601 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator was added dropwise over 2 hours. After the dropwise addition, the mixture was reacted at 80°C for 3 hours, and then 0.6 parts of V-601 was added and the reaction was continued at 80°C for another 2 hours to obtain a solution of binder resin 1. After cooling the above-mentioned solution of binder resin 1 to 50°C, 4.7 parts of dimethylaminoethanol were added to neutralize the carboxyl group, and then 140 parts of water were added. Thereafter, the solution was heated to 78°C or higher, and azeotroped with water to distill off 2-butanone. The solid content was then adjusted to 30%, to obtain an aqueous solution of binder resin 1 (solid content 30%). The weight average molecular weight of the binder resin 1 was measured using a GPC (HLC-8120GPC, Tosoh Corporation) equipped with a TSKgel column (Tosoh Corporation) and an RI detector, using THF as a developing solvent, and was found to be about 17,000.
[0116] In the present application, the term "aqueous solution" refers to a solution containing an aqueous solvent (a medium consisting of a liquid containing at least water) and a component dispersed and / or dissolved in the aqueous solvent.
[0117] <Synthesis of acetylene diol surfactant 1> Acetylene diol surfactant 1 was synthesized using the method described in Example 4 of JP 2001-215690 A. Acetylene diol surfactant 1 is a compound represented by the general formula (1): 1 is a methyl group, R 2 is an isobutyl group, m1+n1 is 5, m2+n2 is 2, and it is a compound in which an ethylene oxide group and a propylene oxide group are added in block form. The HLB value of the acetylene diol surfactant 1 is 7.8, and the molecular weight is 563.
[0118] <Synthesis of acetylene diol surfactants 2-11> Acetylene diol surfactants 2 to 11 were synthesized by using the methods described in JP 2001-215690 A, Examples 6 and 14, and further adjusting the amounts of ethylene oxide and propylene oxide used. The structures and HLB values of the acetylene diol surfactants 2 to 11 are shown in Table 2.
[0119] [Table 2]
[0120] <Production of pigment dispersion> 450 g of carbon black ("PrinteX85" manufactured by Orion Engineered Carbons), 90 g of acrylic resin (a random polymer of styrene / acrylic acid / behenyl acrylate = 45 / 30 / 25 (mass ratio) in which all acid groups are neutralized with dimethylaminoethanol, acid value of about 230 mgKOH / g, mass average molecular weight of 20,000), and 2,460 g of water were put into a mixing vessel (volume 10 L) equipped with a stirrer and stirred (premixed) for 1 hour. Next, circulation dispersion of the mixture was started using "Dyno Mill" (volume 0.6 L) manufactured by Shinmaru Enterprises, which was filled with 1,800 g of zirconia beads with a diameter of 0.5 mm. Then, the D50 of the mixture was measured using the above-mentioned device at regular intervals (for example, 1 hour), and the circulation dispersion was stopped when the D50 became 120 nm or less, thereby producing a pigment dispersion liquid.
[0121] <Production of water-based inkjet inks> Using the pigment dispersion produced by the above-mentioned method, each raw material was added to a mixing vessel equipped with a stirrer so as to obtain the formulation shown in each column of Table 3. After addition, the mixture was heated to 50°C and further mixed for 1 hour, and then filtered through a membrane filter with a pore size of 0.8 μm to produce water-based inkjet inks 1 to 60.
[0122] When producing the aqueous inkjet ink, each raw material was added while stirring the mixture in the mixing vessel. In addition, the raw materials were added in the order listed in the top row of each column in Table 3. However, when producing an aqueous inkjet ink that does not contain one or more of these components, that component was not added and the next component was added in the order listed. In addition, for components that contain two or more types of raw materials, the order of addition of the raw materials within that component was arbitrary.
[0123] [Table 3]
[0124] [Table 3]
[0125] [Table 3]
[0126] [Table 3]
[0127] Here, the meanings of the abbreviations and details of the product names listed in Table 3 above are as follows: In Table 3, "bp" represents the boiling point (unit: °C), and "HLB" represents the HLB value. 1,2-PD: 1,2-propanediol (SP value: 13.5 (cal / cm 3 ) 1 / 2 , boiling point: 188℃, specific heat: 0.574cal / g ℃) 1,2-BD: 1,2-butanediol (SP value: 12.8 (cal / cm 3 ) 1 / 2 , boiling point: 191℃, specific heat: 0.559cal / g ℃) 1,3-BD: 1,3-butanediol (SP value: 12.8 (cal / cm 3 ) 1 / 2 , boiling point: 207℃, specific heat: 0.559cal / g ℃) 1,5-PentD: 1,5-pentanediol (SP value: 12.4 (cal / cm 3 ) 1 / 2 , boiling point: 239℃, specific heat: 0.526cal / g ℃) Gly: Glycerin (SP value: 16.4 (cal / cm 3 ) 1 / 2 , boiling point: 290℃, specific heat: 0.539cal / g ℃) DEG: Diethylene glycol (SP value: 15.0 (cal / cm 3 ) 1 / 2 , boiling point: 244℃, specific heat: 0.519cal / g ℃) EB: Ethylene glycol monobutyl ether (SP value: 10.8 (cal / cm 3 ) 1 / 2 , boiling point: 171℃, specific heat: 0.519cal / g ℃) PM: Propylene glycol monomethyl ether (SP value: 11.3 (cal / cm 3 ) 1 / 2 , boiling point: 121℃, specific heat: 0.557cal / g ℃) PE: Propylene glycol monoethyl ether (SP value: 10.9 (cal / cm 3 ) 1 / 2 , boiling point: 132℃, specific heat: 0.547cal / g ℃) PnP: Propylene glycol monopropyl ether (SP value: 10.7 (cal / cm 3 ) 1 / 2 , boiling point: 150℃, specific heat: 0.539cal / g ℃)
[0128] PnB: Propylene glycol monobutyl ether (SP value: 10.4 (cal / cm 3 ) 1 / 2 , boiling point: 170℃, specific heat: 0.533cal / g ℃) MDG: Diethylene glycol monomethyl ether (SP value: 11.2 (cal / cm 3 ) 1 / 2 , boiling point: 193℃, specific heat: 0.513cal / g ℃) EDG: Diethylene glycol monoethyl ether (SP value: 10.9 (cal / cm 3 ) 1 / 2 , boiling point: 202℃, specific heat: 0.510cal / g ℃) BDG: Diethylene glycol monobutyl ether (SP value: 10.5 (cal / cm 3 ) 1 / 2 , boiling point: 231℃, specific heat: 0.505cal / g ℃) HDG: Diethylene glycol monohexyl ether (SP value: 10.2 (cal / cm 3 ) 1 / 2 , boiling point: 258℃, specific heat: 0.501cal / g°C) TEB: Triethylene glycol monobutyl ether (SP value: 10.3 (cal / cm 3 ) 1 / 2 , boiling point: 278℃, specific heat: 0.497cal / g ℃)
[0129] Surfynol 440: An acetylene diol surfactant manufactured by Evonik Japan Co., Ltd. (in the general formula (1), R 1 is a methyl group, R 2 isobutyl group, m1+n1 is 3-4, m2+n2 is 0, HLB value: 8.1 (average value) Surfynol 485: An acetylene diol surfactant manufactured by Evonik Japan Co., Ltd. (in the general formula (1), R 1 is a methyl group, R 2 isobutyl group, m1+n1 is 30, m2+n2 is 0, HLB value: 17.1)
[0130] TEGO Wet 280: Siloxane surfactant manufactured by Evonik Japan BYK-3420: Siloxane surfactant manufactured by BYK Japan TEGO Glide 100: Siloxane surfactant manufactured by Evonik Japan TEGO Glide 440: Siloxane surfactant manufactured by Evonik Japan
[0131] EMAL 20C: Polyoxyethylene (3) lauryl ether sodium sulfate aqueous solution (25% solids, anionic surfactant manufactured by Kao Corporation) Proxel GXL: 1,2-benzisothiazol-3-one in dipropylene glycol (1,2-benzisothiazol-3-one:dipropylene glycol:water = 2:6:2, preservative manufactured by Arch Chemicals)
[0132] <Creating printed matter> An inkjet printing device was prepared with a Kyocera inkjet head "KJ4B-1200" (design resolution 1,200 dpi, nozzle diameter 20 μm) installed above a conveyor, and the inkjet head was filled with the aqueous inkjet ink listed in Table 2. In addition, an OPP film cut to A4 size (width 21 cm × length 30 cm) was fixed on the conveyor as a printing substrate. Thereafter, the conveyor was driven at a speed of 50 m / min, and when the printing substrate passed under the installation part of the inkjet head, the aqueous inkjet ink was discharged under the condition of a drop volume of 2 pL to print an image. Then, the printed printing substrate was immediately placed in a constant temperature incubator with a blower set at 70 °C and dried for 1 minute to produce a printed matter.
[0133] The following two types of printed matter were produced by the above method: In addition, the following two types of printed matter were produced for each of the water-based inkjet inks. Solid print: 100% print coverage (width 15cm x length 30cm) Gradient print: A gradation image with a print rate that changes continuously between 5% and 80% is printed in an area of 10cm wide x 30cm long.
[0134] [Examples 1 to 51, Comparative Examples 1 to 9] The printed matter produced by the above-mentioned method was used to carry out the following evaluations 1 and 2. The above-mentioned water-based inkjet ink was also used to carry out the following evaluation 3. The results of these evaluations are shown in Table 3.
[0135] <Evaluation 1: Beading evaluation> The gradation print produced by the above method was visually observed, and beading was evaluated by checking the printing rate at the point where unevenness in shading began to be seen. The evaluation criteria are as follows, and a rating of "C" or higher was deemed usable. (Evaluation Criteria) AA: No unevenness in shading was observed even with a print rate of 90%. A: No unevenness in shading was observed at a print rate of 80%, but unevenness in shading was observed at a print rate of 70%. B: No unevenness in shading was observed at a print rate of 70%, but unevenness in shading was observed at a print rate of 80%. C: No unevenness in shading was observed at a print rate of 60%, but unevenness in shading was observed at a print rate of 70%. D: Uneven shading was observed at a printing rate of 60%.
[0136] <Evaluation 2: Evaluation of blocking resistance> The solid print produced by the above method was cut into a 4 cm x 4 cm square, and the printed surface was then superimposed on the non-printed surface of the same printing substrate (OPP film) used for printing. The superimposed surface was then used as a test piece, and a blocking test was carried out using a constant load permanent deformation tester (Tester Sangyo Co., Ltd. "CO-201"). The conditions for the blocking test were a load of 10 kg / cm 2 The test conditions were: ambient temperature 40°C, ambient humidity 80% RH, and static time 36 hours. After 24 hours, the test piece was removed from the constant load permanent deformation tester, and the overlapping printed substrate was instantly peeled off while maintaining an angle of 90 degrees. Blocking resistance was evaluated based on the feel when peeled off (peel resistance) and the appearance of the printed surface after peeling off (visual confirmation). The evaluation criteria were as follows, and a rating of "B" or higher was deemed usable. (Evaluation Criteria) AA: There was no peel resistance, and no part of the water-based inkjet ink layer adhered to the non-printed surface of the printing substrate. A: Although there was slight resistance when peeling, no part of the water-based inkjet ink layer adhered to the non-printed surface of the printing substrate. B: Part of the water-based inkjet ink layer was attached to the non-printed surface of the printed substrate, and the extent of this was 10% or less of the area of the overlapping parts. C: Part of the water-based inkjet ink layer was attached to the non-printed surface of the printed substrate, and the extent of this was more than 10% but not more than 30% of the overlapping area. D: Part of the water-based inkjet ink layer was adhered to the non-printed surface of the printing substrate, and the extent of this was more than 30% of the area of the overlapping parts.
[0137] <Evaluation 3: Evaluation of ejection stability> The water-based inkjet ink listed in Table 2 was filled into the inkjet printing device used to produce the printouts. A nozzle check pattern was printed to confirm that there were no missing nozzles, and then 300 solid printouts were produced using the method described above. Thereafter, a nozzle check pattern was printed again and the number of missing nozzles was visually counted to evaluate the ejection stability. The evaluation criteria were as follows, with a rating of "B" or higher deemed usable. (Evaluation Criteria) AA: No missing nozzles at all A: 1 to 9 nozzles were missing B: 10 to 19 nozzles were missing C: 20 to 49 or more nozzles were missing D: 50 or more nozzles were missing
[0138] As shown in Table 3 above, the aqueous inkjet inks of Examples 1 to 51 having the configuration of the present invention were superior in ejection stability to the inks of Comparative Examples 1 to 9. Furthermore, the printed matter exhibited good suppression of beading (image quality) and also had excellent anti-blocking properties.
Claims
1. An aqueous inkjet ink comprising a pigment, a surfactant (A), and a water-soluble organic solvent (B), The surfactant (A) includes an acetylene diol-based surfactant (A1) having a structure represented by the following general formula (1) and an HLB value of 10 or less, the water-soluble organic solvent (B) contains an alkanediol (B1) having 3 to 5 carbon atoms and a glycol monoether (B2) having 4 to 10 carbon atoms; the alkanediol (B1) having 3 to 5 carbon atoms has an SP value of 12.0 to 14.0 (cal / cm 3 ) 1 / 2 as calculated by Fedor's estimation method; the mass ratio ((B1) / (B2)) of the content of the alkanediols (B1) having 3 to 5 carbon atoms to the content of the glycol monoethers (B2) having 4 to 10 carbon atoms is 0.8 to 12. General formula (1): 【Chemistry 1】 (In the general formula (1), R 1 and R 2 each represents an alkyl group having 1 to 5 carbon atoms which may be branched, EO represents an ethylene oxide group, and PO represents a propylene oxide group. In addition, m1, m2, n1, and n2 each represent an integer of 1 to 10, and (m1+n1):(m2+n2)=1:9 to 9:
1. However, the addition pattern of the ethylene oxide groups and propylene oxide groups in the parentheses may be block or random.)
2. The aqueous inkjet ink according to claim 1 , wherein the surfactant (A) further comprises a nonionic surfactant (A2) other than the acetylene diol-based surfactant (A1).
3. 3. The aqueous inkjet ink according to claim 1, wherein the content of the acetylene diol surfactant (A1) is 0.1 to 5.0 mass % of the total amount of the aqueous inkjet ink.
4. A printed matter obtained by printing with the aqueous inkjet ink according to claim 1 or 2.
Citation Information
Patent Citations
Ink jet recording ink
JP1999080639A
Recording ink and recording method using the same
JP2002285055A
Ink jet recording sheet
JP2004181760A
Inkjet recording ink, inkjet recording method, print and inkjet recording apparatus
JP2004346159A
Inkjet recording aqueous ink, ink cartridge, inkjet recording method, and inkjet recording apparatus
JP2012211260A