Method for manufacturing nitride semiconductor device

By employing coherent growth and annealing of a second nitride semiconductor layer, the method addresses the inefficiency of activating p-type impurities in nitride semiconductor layers, achieving a highly active p-type region with lower energy usage.

JP7572309B2Active Publication Date: 2024-10-23DENSO CORP +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021100863
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-17
Publication Date
2024-10-23
Estimated Expiration
2041-06-17

AI Technical Summary

Technical Problem

Existing methods struggle to effectively activate p-type impurities introduced into nitride semiconductor layers, requiring high energy and often resulting in inefficient p-type regions.

Method used

A method involving coherent growth of a second nitride semiconductor layer on a first nitride semiconductor layer, followed by annealing, to create a two-dimensional electron gas layer that activates p-type impurities with lower energy, forming a highly active p-type region.

Benefits of technology

This method efficiently activates p-type impurities with reduced energy consumption, maintaining the upper layer of the first nitride semiconductor layer as n-type, thereby forming a highly active p-type region.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572309000001
    Figure 0007572309000001
  • Figure 0007572309000002
    Figure 0007572309000002
  • Figure 0007572309000003
    Figure 0007572309000003
Patent Text Reader

Abstract

To provide a novel technique capable of activating a p-type impurity introduced into a nitride semiconductor layer.SOLUTION: A manufacturing method of a nitride semiconductor device includes a p-type impurity introduction step of introducing a p-type impurity into at least a portion of an upper layer portion of a first nitride semiconductor layer 14 to form a p-type impurity introduction region 16, a film formation step of forming a second nitride semiconductor layer 18 from an upper surface of the first nitride semiconductor layer so as to include the p-type impurity introduction region, and forming the second nitride semiconductor layer by coherent growth, and an annealing treatment step of performing annealing treatment in a state in which the second nitride semiconductor layer is formed on the first nitride semiconductor layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in this specification relates to a method for manufacturing a nitride semiconductor device including a nitride semiconductor layer. [Background technology]

[0002] In order to manufacture a nitride semiconductor device, a technique is required to introduce a p-type impurity into a nitride semiconductor layer and activate the introduced p-type impurity to form a p-type diffusion region. An example of a technique for forming a p-type diffusion region in a nitride semiconductor layer is disclosed in Patent Document 1. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-79930 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present specification provides a novel technique capable of activating p-type impurities introduced into a nitride semiconductor layer. [Means for solving the problem]

[0005] The method for manufacturing a nitride semiconductor device disclosed in this specification can include a p-type impurity introducing step of introducing a p-type impurity into at least a portion of an upper layer portion of a first nitride semiconductor layer (14) to form a p-type impurity introduced region (16), a film formation step of forming a second nitride semiconductor layer (18) from an upper surface of the first nitride semiconductor layer so as to include the p-type impurity introduced region, where the second nitride semiconductor layer is formed by coherent growth, and an annealing treatment step of performing an annealing treatment in a state where the second nitride semiconductor layer is formed on the first nitride semiconductor layer.

[0006] The energy required to activate the p-type impurity depends on the position of the Fermi level of the region into which the p-type impurity is introduced, and the closer the position of the Fermi level is to the valence band, i.e., if the region into which the p-type impurity is introduced is n-type, the lower the energy becomes. According to the above manufacturing method, by forming the second nitride semiconductor layer formed by coherent growth on the first nitride semiconductor layer, a two-dimensional electron gas layer (2DEG) is generated by piezoelectric polarization in the upper layer portion of the first nitride semiconductor layer, and the upper layer portion of the first nitride semiconductor layer can be made n-type. Therefore, at least a part of the p-type impurity introduced region formed in the upper layer portion of the first nitride semiconductor layer can be located in the n-type region. According to the above manufacturing method, an annealing process can be performed in a state in which the upper layer portion of the first nitride semiconductor layer is made n-type, so that the p-type impurity in the p-type impurity introduced region can be activated with low energy. As a result, the above manufacturing method can form a highly active p-type region. [Brief description of the drawings]

[0007] [Figure 1] 1 shows a flowchart of a part of a method for manufacturing a nitride semiconductor device. [Diagram 2] 1A and 1B are schematic cross-sectional views of a main portion of a nitride semiconductor layer in a process of a method for manufacturing a nitride semiconductor device. [Diagram 3] 1A and 1B are schematic cross-sectional views of a main portion of a nitride semiconductor layer in a process of a method for manufacturing a nitride semiconductor device. [Figure 4] 1A and 1B are schematic cross-sectional views of a main portion of a nitride semiconductor layer in a process of a method for manufacturing a nitride semiconductor device. [Diagram 5] 1A and 1B are schematic cross-sectional views of a main portion of a nitride semiconductor layer in a process of a method for manufacturing a nitride semiconductor device. [Figure 6] 1A and 1B are schematic cross-sectional views of a main portion of a nitride semiconductor layer in a process of a method for manufacturing a nitride semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, a method for manufacturing a nitride semiconductor device including a nitride semiconductor layer will be described with reference to the drawings. Hereinafter, an annealing process for activating the p-type impurities implanted in the ion implantation process among the processes for manufacturing the nitride semiconductor device will be described. For other processes among the processes for manufacturing the nitride semiconductor device, known manufacturing methods can be used.

[0009] In this specification, the "nitride semiconductor" refers to In X Al Y Ga 1-X-Y a compound defined by N (where 0 ≦ X ≦ 1, 0 ≦ Y ≦ 1). Further, aluminum gallium nitride (AlGaN) is a nitride semiconductor corresponding to X = 0 and 0 < Y < 1 in the above definition. Indium aluminum nitride (InAlN) is a nitride semiconductor corresponding to X + Y = 1, 0 < X < 1, and 0 < Y < 1 in the above definition.

[0010] FIG. 1 shows a partial flowchart of a method for manufacturing a nitride semiconductor device. FIGS. 2 to 6 schematically show cross-sectional views of main parts of the nitride semiconductor layer in the manufacturing process corresponding to the flowchart of FIG. 1.

[0011] First, as shown in FIG. 2, a semiconductor substrate 12 is prepared, and a first nitride semiconductor layer 14 of a nitride semiconductor is formed on the semiconductor substrate 12 using an epitaxial growth technique (step S1 in FIG. 1). The semiconductor substrate 12 may be any material capable of growing a nitride semiconductor crystal. In this example, the material of the semiconductor substrate 12 is gallium nitride (GaN) containing a high concentration of n-type impurities. The first nitride semiconductor layer 14 is not particularly limited, and may be formed on the semiconductor substrate 12 using, for example, MOCVD (Metal Organic Chemical Vapor Deposition) technology. In this example, the material of the first nitride semiconductor layer 14 is gallium nitride (GaN) containing a low concentration of n-type impurities.

[0012] In addition, various diffusion regions constituting functional structures that perform electrical functions are formed in the first nitride semiconductor layer 14. Examples of such functional structures include functional structures of the type called MISFET (Metal Insulator Semiconductor Field Effect Transistor) and MOSFET (Metal Oxide Semiconductor Field Effect Transistor) that perform a switching function, or functional structures of the type called diode that perform a rectifying function. The first nitride semiconductor layer 14 may correspond to a drift region constituting such MISFET and MOSFET, or may correspond to a high resistance region or cathode region constituting a diode. The following describes a method for forming a p-type diffusion region in the first nitride semiconductor layer 14. Such a p-type diffusion region may be a p-type body region or a p-type body contact region in the MISFET and MOSFET, or a p-type anode region in the diode.

[0013] Next, as shown in FIG. 3, a p-type impurity is irradiated toward a part of the upper surface of the first nitride semiconductor layer 14 using an ion implantation technique to introduce the p-type impurity into a part of the upper layer of the first nitride semiconductor layer 14, thereby forming a p-type impurity introduction region 16 (step S2 in FIG. 1). The p-type impurity introduction region 16 is formed at a position exposed on the upper surface of the first nitride semiconductor layer 14. The p-type impurity is not particularly limited, but may be, for example, magnesium (Mg). The p-type impurity may be beryllium (Be) instead of magnesium. Nitrogen (N) may be introduced into the p-type impurity introduction region 16 as necessary to promote activation.

[0014] Next, as shown in FIG. 4, a second nitride semiconductor layer 18 of a nitride semiconductor is formed on the first nitride semiconductor layer 14 using an epitaxial growth technique (step S3 in FIG. 1). The second nitride semiconductor layer 18 may be formed on the first nitride semiconductor layer 14 by coherent growth using, for example, an MOCVD technique, although it is not particularly limited thereto. Here, the coherent growth refers to a state in which, although there is a lattice mismatch between the first nitride semiconductor layer 14 and the second nitride semiconductor layer 18, when the second nitride semiconductor layer 18 is crystal-grown, the lattice of the second nitride semiconductor layer 18 is distorted, so that the second nitride semiconductor layer 18 grows while maintaining the continuity of the lattice at the interface between the first nitride semiconductor layer 14 and the second nitride semiconductor layer 18. The second nitride semiconductor layer 18 is a nitride semiconductor having a band gap different from that of the first nitride semiconductor layer 14. Typically, the second nitride semiconductor layer 18 is a nitride semiconductor having a band gap larger than that of the first nitride semiconductor layer 14. In this example, the second nitride semiconductor layer 18 is non-doped or n-type aluminum gallium nitride (AlGaN).

[0015] Since the second nitride semiconductor layer 18 is formed by coherent growth from the upper surface of the first nitride semiconductor layer 14, as shown in FIG. 4, a two-dimensional electron gas layer (2DEG) is formed by piezoelectric polarization on the first nitride semiconductor layer 14 side of the heterojunction surface between the first nitride semiconductor layer 14 and the second nitride semiconductor layer 18. Note that the E F indicates the Fermi level. In this manner, the upper layer portion of the first nitride semiconductor layer 14 is made n-type, and at least a portion of the p-type impurity introduced region 16 is disposed in this n-type region, i.e., in the two-dimensional electron gas layer (2DEG).

[0016] Next, an annealing process is performed in a state where the second nitride semiconductor layer 18 is formed on the first nitride semiconductor layer 14 (step S4 in FIG. 1). The annealing temperature is not particularly limited, but may be, for example, 1300° C. to 1500° C. The formation energy for replacing magnesium (Mg) as a p-type impurity with gallium (Ga), that is, the energy required to activate magnesium, depends on the position of the Fermi level of the p-type impurity introduction region 16. The closer the position of the Fermi level of the p-type impurity introduction region 16 is to the valence band, that is, if the p-type impurity introduction region 16 is n-type, the lower the energy required to activate magnesium. This annealing process is performed in a state where a two-dimensional electron gas layer (2DEG) is formed in the upper layer portion of the first nitride semiconductor layer 14, so that the annealing process is performed in a state where at least a part of the p-type impurity introduction region 16 is located in the n-type region. Therefore, the p-type impurity in the p-type impurity introduction region 16 can be activated with low energy. Furthermore, the maximum concentration of the p-type impurity introduced into the p-type impurity introduction region 16 is adjusted to be smaller than the maximum charge density in the two-dimensional electron gas layer (2DEG). Therefore, the upper layer portion of the first nitride semiconductor layer 14 is maintained in the n-type region during the annealing treatment. As a result, the p-type impurity introduced into the p-type impurity introduction region 16 can be activated with high efficiency.

[0017] Next, as shown in Fig. 5, the second nitride semiconductor layer 18 is removed (Step S5 in Fig. 1). When the second nitride semiconductor layer 18 is removed, the piezoelectric polarization disappears, and the p-type impurity introduced region 16 becomes a p-type region. In this manner, a highly active p-type region can be formed in the upper portion of the first nitride semiconductor layer 14.

[0018] In the above example, the second nitride semiconductor layer 18 is composed of one nitride semiconductor layer. Instead of this example, as shown in Fig. 6, the second nitride semiconductor layer 18 may be composed of a plurality of layers. Fig. 6 shows an example in which a lower nitride semiconductor layer 18a and an upper nitride semiconductor layer 18b are laminated. The lower nitride semiconductor layer 18a and the upper nitride semiconductor layer 18b are not particularly limited, but may be formed in this order by coherent growth on the first nitride semiconductor layer 14 using, for example, MOCVD technology.

[0019] For example, the lower nitride semiconductor layer 18a and the upper nitride semiconductor layer 18b may be made of AlGaN and have different aluminum composition ratios. 0.2 Ga 0.8 N, and the upper nitride semiconductor layer 18b is Al 0.4 Ga 0.6 N. When the aluminum composition ratio of the lower nitride semiconductor layer 18a in contact with the first nitride semiconductor layer 14 is small, lattice mismatch between the first nitride semiconductor layer 14 and the lower nitride semiconductor layer 18a is suppressed, and the occurrence of cracks during annealing is suppressed. When the aluminum composition ratio of the uppermost nitride semiconductor layer 18b is large, nitrogen loss from the surface of the upper nitride semiconductor layer 18b is suppressed, improving heat resistance. To ensure practical heat resistance, the aluminum composition ratio of the upper nitride semiconductor layer 18b may be 40% or more. Instead of the two distinct laminated structures of the lower nitride semiconductor layer 18a and the upper nitride semiconductor layer 18b, the second nitride semiconductor layer 18 may be configured with three or more layers such that the aluminum composition ratio increases stepwise from the first nitride semiconductor layer 14 side toward the outermost surface, or may be configured with one layer such that the aluminum composition ratio increases continuously from the first nitride semiconductor layer 14 side toward the outermost surface, or may be configured with a combination of these. In any case, the aluminum composition ratio of the second nitride semiconductor layer 18 may be configured so that the portion in contact with the first nitride semiconductor layer 14 has a minimum value and the outermost surface has a maximum value. This makes it possible to extremely satisfactorily suppress both cracking and nitrogen loss.

[0020] For example, the lower nitride semiconductor layer 18a may be indium aluminum nitride (InAlN), and the upper nitride semiconductor layer 18b may be aluminum gallium nitride (AlGaN). The charge density of the two-dimensional electron gas layer (2DEG) formed at the heterojunction surface of InAlN / GaN is higher than the charge density of the two-dimensional electron gas layer (2DEG) formed at the heterojunction surface of AlGaN / GaN. Therefore, when the lower nitride semiconductor layer 18a is indium aluminum nitride (InAlN), a high-density two-dimensional electron gas layer (2DEG) is formed in the upper layer portion of the first nitride semiconductor layer 14. Therefore, even if the p-type impurity concentration of the p-type impurity introduction region 16 is increased, an n-type region can be maintained during the annealing process, and a high-concentration p-type region can be formed in the upper layer portion of the first nitride semiconductor layer 14.

[0021] The features of the technology disclosed in this specification are summarized below. Note that the technical elements described below are independent technical elements that exhibit technical usefulness alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing.

[0022] The method for manufacturing a nitride semiconductor device disclosed in the present specification may include a p-type impurity introduction step of introducing a p-type impurity into at least a part of an upper layer portion of a first nitride semiconductor layer to form a p-type impurity introduction region, a film formation step of forming a second nitride semiconductor layer from an upper surface of the first nitride semiconductor layer so as to include the p-type impurity introduction region, the second nitride semiconductor layer being formed by coherent growth, and an annealing treatment step of performing an annealing treatment in a state in which the second nitride semiconductor layer is formed on the first nitride semiconductor layer. The second nitride semiconductor layer may be a nitride semiconductor having a band gap different from that of the first nitride semiconductor layer. Typically, the second nitride semiconductor layer may be a nitride semiconductor having a band gap larger than that of the first nitride semiconductor layer.

[0023] In the film formation step, the second nitride semiconductor layer may be formed by stacking nitride semiconductors having different composition ratios. For example, the first nitride semiconductor layer may be GaN, and the second nitride semiconductor layer may be AlGaN. In this case, in the second step, the second nitride semiconductor layer may be formed so that the aluminum composition ratio increases from the first nitride semiconductor layer side toward the outermost surface. It is possible to simultaneously suppress cracks and nitrogen loss. Alternatively, the first nitride semiconductor layer may be GaN, and the second nitride semiconductor layer may be a stack of InAlN and AlGaN. It is possible to form a high concentration p-type region in the upper layer portion of the first nitride semiconductor layer.

[0024] When the first nitride semiconductor layer is made of GaN, the annealing temperature in the annealing treatment step may be 1300° C. to 1500° C. Energy necessary for activating the p-type impurity can be applied.

[0025] In the film formation step, the second nitride semiconductor layer may be formed by utilizing an MOCVD technique.

[0026] Although specific examples of the present invention have been described above in detail, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and variations of the specific examples exemplified above. Furthermore, the technical elements described in this specification or drawings exhibit technical utility alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing. Furthermore, the technology exemplified in this specification or drawings can achieve multiple objectives simultaneously, and achieving one of these objectives is itself technically useful. [Explanation of symbols]

[0027] 12: Semiconductor substrate 14: First nitride semiconductor layer 16: p-type impurity introduction region 18: Second nitride semiconductor layer

Claims

1. A method for manufacturing a nitride semiconductor device, comprising the steps of: a p-type impurity introduction step of introducing a p-type impurity into at least a portion of an upper layer portion of the first nitride semiconductor layer (14) to form a p-type impurity introduction region (16); a deposition step of depositing a second nitride semiconductor layer (18) on an upper surface of the first nitride semiconductor layer so as to include the p-type impurity introduced region, the second nitride semiconductor layer being deposited by coherent growth; an annealing step of performing an annealing treatment in a state where the second nitride semiconductor layer is formed on the first nitride semiconductor layer; a removal step of removing the second nitride semiconductor layer after the annealing step, In the film forming step, the second nitride semiconductor layer is formed by stacking nitride semiconductors having different composition ratios.

2. the first nitride semiconductor layer is GaN; the second nitride semiconductor layer is AlGaN; The method for manufacturing a nitride semiconductor device according to claim 1 , wherein in said film forming step, said second nitride semiconductor layer is formed such that a composition ratio of aluminum increases from said first nitride semiconductor layer side toward an outermost surface.

3. the first nitride semiconductor layer is GaN; The method for manufacturing a nitride semiconductor device according to claim 1 , wherein the second nitride semiconductor layer is a stack of InAlN and AlGaN.

4. 4. The method for manufacturing a nitride semiconductor device according to claim 2, wherein the annealing temperature in the annealing step is 1300.degree. C. to 1500.degree. C.

5. 5. The method for manufacturing a nitride semiconductor device according to claim 1, wherein in said film forming step, said second nitride semiconductor layer is formed by utilizing MOCVD technology.

Citation Information

Patent Citations

  • Method for manufacturing nitride compound semiconductor and semiconductor element

    JP2003124515A

  • Field effect transistor

    JP2008124373A

  • Compound semiconductor device and manufacturing method of the same

    JP2013197313A

  • High electron mobility transistor

    JP2017041543A

  • Semiconductor device manufacturing method

    JP2018056257A