Lithium-containing oxide crystal, battery, and method for producing lithium-containing oxide crystal

By controlling the dew point and using specific growth methods, lithium-containing oxide crystals with large areas and dimensions are produced without cracks, improving the capacity and conductivity of all-solid-state batteries.

JP7572730B2Active Publication Date: 2024-10-24ORBRAY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021507388
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-21
Filing Date
2020-03-18
Publication Date
2024-10-24
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

Lithium-containing oxide crystals grown using methods like FZ and CZ suffer from cracks, limiting the production of large, high-quality crystals with low Li ion conductivity, which affects the capacity and conductivity of all-solid-state batteries.

Method used

The production method involves setting the dew point of the growth atmosphere between -70°C and -35°C, using the CZ or EFG method, to grow lithium-containing oxide crystals with a cross-sectional area of 0.38 cm² or more and a longitudinal dimension of 10 mm or more, ensuring no cracks and high conductivity.

Benefits of technology

This approach enables the production of large, crack-free lithium-containing oxide crystals, enhancing the capacity and conductivity of all-solid-state batteries, with conductivity exceeding 0.5 mS/cm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572730000001
    Figure 0007572730000001
  • Figure 0007572730000002
    Figure 0007572730000002
  • Figure 0007572730000003
    Figure 0007572730000003
Patent Text Reader

Abstract

[Problem] To provide: a lithium-containing oxide crystal which is free from cracks, while having a large area; a battery which uses this lithium-containing oxide crystal; and a method for producing this lithium-containing oxide crystal. [Solution] The present invention comprises a molten part formation step wherein at least some of the starting material of the lithium-containing oxide crystal, said starting material containing oxygen, is melted so as to form a molten part, and a growth step wherein a lithium-containing oxide crystal is grown form the molten part; the dew point of the atmosphere of the growth step is within the range of from -70°C to -35°C; and the lithium-containing oxide crystal is free from cracks, while having a cross-sectional area of 0.38 cm2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium-containing oxide crystal, a battery, and a method for producing a lithium-containing oxide crystal. [Background technology]

[0002] Lithium-ion batteries have been used for smartphone batteries, electric vehicle batteries, and the like. Conventional lithium-ion batteries use an electrolyte solution as an electrolyte through which Li (lithium) ions can move. However, it is becoming difficult to achieve higher capacity, higher voltage, higher energy density, and faster charging performance with lithium-ion batteries that use an electrolyte solution. Therefore, development of all-solid-state batteries that use solid electrolytes instead of electrolyte solutions as lithium-ion batteries that meet these various requirements is underway. Examples of solid electrolytes used in all-solid-state lithium-ion batteries include sulfide-based and oxide-based lithium ion crystals.

[0003] Sulfide-based solid electrolytes have high Li-ion conductivity and are suitable for batteries that prioritize energy density. However, there is an issue that harmful substances (hydrogen sulfide (H2S)) are released when the crystal structure of the solid electrolyte is destroyed by high temperatures. Therefore, development of oxide-based solid electrolytes is being promoted for applications that require greater safety and stability without releasing harmful substances.

[0004] On the other hand, oxide-based solid electrolytes have the problem of lower Li-ion conductivity compared to sulfide-based solid electrolytes. To apply them to bulk-type all-solid-state batteries, the conductivity at room temperature must be 10 -3 It is preferable to use an oxide-based solid electrolyte that exhibits a resistance of 10 (S / cm) or more. -3 As an example of an oxide-based solid electrolyte with a conductivity of about 10 ... 0.51 Li 0.34 TiO 2.94 Lithium-containing oxide crystals such as those mentioned above are known (for example, see Non-Patent Document 1). [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Chemistry, July 1, 2012, Internet<URL: http: / / www2.chem.osakafu-u.ac.jp / ohka / ohka2 / research / battery_li.pdf> Summary of the Invention [Problem to be solved by the invention]

[0006] However, there is a problem with lithium-containing oxide crystals in that cracks occur in crystals grown using the FZ (Floating Zone) method, the CZ (Czochralski) method, the EFG (Edge-defined Film-fed Growth) method, etc. In more detail, when at least a part of the lithium-containing oxide crystal raw material is melted to form a molten part and the lithium-containing oxide crystal is grown from the molten part, the viscosity of the molten part changes in the crystal growth direction, and the melt of the molten part suddenly breaks during growth (droops in the FZ method), causing cracks in the crystal.

[0007] In the case of lithium-containing oxide crystals, the larger the outer dimensions of the crystals to be grown, the more likely they are to develop cracks, leading to a decrease in yield. This makes it difficult to manufacture large lithium-containing oxide crystals with good crystal quality and no cracks at a high yield.

[0008] The present invention has been made in view of the above problems, and aims to provide a lithium-containing oxide crystal having a large area and no cracks, as well as a method for producing the lithium-containing oxide crystal. Further, the present invention aims to provide a battery including at least a part of the lithium-containing oxide crystal. [Means for solving the problem]

[0009] In order to solve the above problems, the lithium-containing oxide crystal of the present invention is free of cracks and has a diameter of 0.38 cm 2 The present invention is characterized in that the cross-sectional area of ​​the gas is equal to or larger than that mentioned above and contains oxygen.

[0010] Such lithium-containing oxide crystal of the present invention has a large area without cracks, and therefore it is possible to achieve high capacity and high electrical conductivity of an all-solid-state battery.

[0011] In one embodiment of the present invention, the cross-sectional area is 1.76 cm 2 More than 100cm 2 The following is the result.

[0012] In one embodiment of the present invention, the electrode has a longitudinal dimension, and the longitudinal dimension is 10 mm or more.

[0013] In order to achieve the above object, a battery of the present invention is characterized by using at least a part of any one of the lithium-containing oxide crystals described above.

[0014] In order to solve the above problems, the method for producing a lithium-containing oxide crystal of the present invention includes a melting part forming step of melting at least a part of a lithium-containing oxide crystal raw material containing oxygen to form a melting part, and a growing step of growing a lithium-containing oxide crystal from the melting part, wherein the dew point of the atmosphere in the growing step is in the range of -70°C or more and -35°C or less, and the lithium-containing oxide crystal has a thickness of 0.38 cm. 2 It is characterized by having a cross-sectional area of ​​more than or equal to this.

[0015] In one embodiment of the present invention, the dew point is set within a range of -70°C or more and -40°C or less, and the temperature is set to 1.76 cm from the molten part. 2 More than 100cm 2 The lithium-containing oxide crystal is grown to have the following area:

[0016] In one aspect of the present invention, the dew point is set within a range of −65° C. or more and −45° C. or less, and the lithium-containing oxide crystal is grown to a longitudinal dimension of 10 mm or more from the molten part.

[0017] In one embodiment of the present invention, the growing step uses a CZ method or an EFG method. Effect of the Invention

[0018] According to the present invention, it is possible to provide a lithium-containing oxide crystal having a large area and no cracks, and a method for producing the same. Also, it is possible to provide a battery including at least a part of the lithium-containing oxide crystal. [Brief description of the drawings]

[0019] [Figure 1] 1 is a cross-sectional observation photograph showing cracks generated in a lithium-containing oxide crystal. [Diagram 2] 1 is a table showing evaluations of Examples 1 and 2 and a Comparative Example of lithium-containing oxide crystals grown by the FZ method. [Diagram 3] 6(a) to 6(c) are photographs showing the appearances of the lithium-containing oxide crystals of Examples 1 and 2 and Comparative Example 1, respectively. [Figure 4] 1 is a table showing external appearance photographs of lithium-containing oxide crystals of Examples 3 to 6 and Comparative Example 2, which were grown by the FZ method while changing the dew point conditions. [Diagram 5] 1 is a table showing evaluations of Examples 7 to 10 of lithium-containing oxide crystals grown by the CZ method. [Figure 6] 6(a) to 6(d) are photographs showing the appearances of the lithium-containing oxide crystals of Examples 7 to 10, respectively. [Figure 7] 1 is a photograph showing the appearance of the lithium-containing oxide crystal of Example 11. [Figure 8] 1 is a photograph showing the appearance of the lithium-containing oxide crystal of Example 12. [Figure 9] 1 is a photograph showing the appearance of the lithium-containing oxide crystal of Example 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The first feature of this embodiment is that the lithium-containing oxide crystal is crack-free and has a size of 0.38 cm 2 or more and contains oxygen.

[0021] According to this configuration, since it has a large area without cracks, it is possible to achieve high capacity and high conductivity of the all-solid-state battery.

[0022] The second characteristic is that the cross-sectional area is 1.76 cm 2 More than 100cm 2 The following is what has been done.

[0023] According to this configuration, larger lithium-containing oxide crystals can be formed, and the capacity and conductivity of the all-solid-state battery can be further increased.

[0024] The third feature is that the electrode has a longitudinal dimension, and the longitudinal dimension is 10 mm or more.

[0025] According to this configuration, it is possible to increase the volume of the lithium-containing oxide crystal, thereby improving the productivity and achieving a further increase in the capacity and electrical conductivity of the all-solid-state battery.

[0026] A fourth feature is that the battery uses at least a part of any one of the lithium-containing oxide crystals described above.

[0027] According to this configuration, by using a large lithium-containing oxide crystal, it is possible to realize an all-solid-state battery with high conductivity of, for example, 0.5 (mS / cm) or more and high capacity.

[0028] The fifth feature is that the method for producing lithium-containing oxide crystals includes a melting part forming step of melting at least a part of a lithium-containing oxide crystal raw material containing oxygen to form a melting part, and a growing step of growing and forming lithium-containing oxide crystals from the melting part, and the dew point of the atmosphere in the growing step is in the range of -70°C or more and -35°C or less, and the lithium-containing oxide crystals have a thickness of 0.38 cm. 2 The cross-sectional area is set to be equal to or greater than the above.

[0029] According to this configuration, the lithium-containing oxide crystal containing oxygen is crack-free and has a thickness of at least 0.38 cm. 2 Furthermore, by using the obtained lithium-containing oxide crystal in a battery, it becomes possible to easily form a high-capacity battery.

[0030] The sixth feature is that the dew point is set within the range of -70°C to -40°C, and the temperature is within 1.76 cm from the molten part. 2 More than 100cm 2 The lithium-containing oxide crystal having the following area is grown and formed.

[0031] According to this configuration, larger lithium-containing oxide crystals can be formed, and the capacity and conductivity of the all-solid-state battery can be further increased.

[0032] The seventh feature is that the dew point is set within a range of -65°C to -45°C, and the lithium-containing oxide crystal is grown to a longitudinal dimension of 10 mm or more from the molten part.

[0033] According to this configuration, it is possible to increase the volume of the lithium-containing oxide crystal, thereby improving the productivity and achieving a further increase in the capacity and electrical conductivity of the all-solid-state battery.

[0034] The eighth feature is that the growth process uses the CZ method or the EFG method.

[0035] According to this configuration, the diameter of the lithium-containing oxide crystal can be increased, and the capacity and conductivity of the all-solid-state battery can be further increased.

[0036] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The same or equivalent components, members, and processes shown in each drawing are denoted by the same reference numerals, and duplicated descriptions will be omitted as appropriate.

[0037] The lithium-containing oxide crystal of this embodiment contains oxygen, has no cracks, and is 0.38 cm 2 or more, and has the general formula Li 7-x-y La3Zr 2-x-y Nb x Ta y O 12 (0.2≦x+y≦1.0, 0≦x≦1.0, 0≦y≦1.0) and has a cubic garnet structure. More preferably, the cross-sectional area is 1.76 cm 2 More than 100cm 2 The range is as follows. The lithium-containing oxide crystal has a longitudinal dimension, and the longitudinal dimension is preferably 10 mm or more. The lithium-containing oxide crystal has a large area and volume without cracks, which makes it possible to improve productivity and increase the capacity and conductivity of the all-solid-state battery. Here, high conductivity means that the conductivity of the solid electrolyte inside the battery is, for example, 0.5 (mS / cm) or more.

[0038] In this embodiment, the crack refers to a crack occurring in the lithium-containing oxide crystal that is visible by an optical microscope and exceeds 1 mm. In addition, the lithium-containing oxide crystal without cracks is preferably one in which no cracks exist throughout the as-grown crystal immediately after crystal growth, but also includes a case in which a crack-free region is partially formed. Furthermore, it also includes a case in which cracks are removed by polishing or cutting the surface after crystal growth. In addition, the cross-sectional area without cracks means the area in the direction in which the region without cracks is maximum in the lithium ion oxide crystal, but it is preferable that the cross-sectional area is a cross-sectional area in a plane perpendicular to the crystal growth direction, because this can achieve uniform crystal quality within the plane.

[0039] FIG. 1 is a cross-sectional observation photograph showing a lithium-containing oxide crystal and cracks that have occurred in the crystal. Here, the scale shown at the bottom of FIG. 1 is 1 mm, and the lithium-containing oxide crystal shown in the figure is disk-shaped with a diameter of about 7 mm. As shown in FIG. 1, when the lithium-containing oxide crystal is cut on a plane perpendicular to the growth direction, it can be seen that a plurality of cracks extend from the outer periphery of the crystal toward the inside. If the lithium-containing oxide crystal contains cracks in this way, it is not preferable because there is a risk of problems such as reduced reliability, reduced capacity, and reduced lifespan when used in an all-solid-state battery. In contrast, in a lithium-containing oxide crystal that does not have any cracks within a diameter of about 7 mm, the cracks are 0.38 cm. 2 With a cross-sectional area of ​​the above, it is possible to achieve high capacity and high conductivity of the all-solid-state battery.

[0040] First, in the manufacturing method of the lithium-containing oxide crystal of the present embodiment, various raw materials of the lithium-containing oxide crystal are prepared as a raw material preparation step, crushed, and mixed in a predetermined ratio to process the raw materials into a powder form. The crushing and mixing methods are not limited, and known methods can be used. Thereafter, in the molding step, the powdered raw materials are pressure-molded and sintered to obtain a raw material sintered body. The pressure-molding and sintering methods are not limited, and known methods can be used.

[0041] As the raw material of the lithium-containing oxide crystal, a lithium compound, a lanthanum compound, a zirconium compound, a tantalum compound, or a niobium compound can be used. As the lithium compound, for example, Li2O or Li2CO3 can be used. As the lanthanum compound, for example, La2O3 or La(OH)3 can be used. As the zirconium compound, for example, ZrO2, ZrC l4 , La2Zr2O7, Li2ZrO3, etc. Tantalum compounds include, for example, Ta2O5 and TaC l5 Examples of niobium compounds include Nb2O5, LiNbO3, and LaNbO4.

[0042] Next, in the molten part forming step, at least a part of the raw material sintered body is melted to form a molten part, and in the growth step, the molten part is cooled to grow a lithium-containing oxide crystal. The method of the molten part forming step and the growth step is not limited, and the crystal can be grown using various known melting methods, such as the FZ (Floating Zone) method, the Bridgman method, the Kyroporus method, the TSSG (Top Seeded Solution Growth) method, the LPE (Liquid Phase Epitaxy) method, the CZ (Czochralski) method, and the EFG (Edge-defined Film-fed Growth) method. In order to increase the diameter of the lithium-containing oxide crystal, it is preferable to use the CZ method or the EFG method. In the case of the growth method using a crucible, it is preferable to use Ir, which does not react with the raw material melt, as the material of the crucible.

[0043] The atmosphere used in the growth step is preferably N2, Ar, or dry air, and the dew point of the atmosphere is set to be in the range of -70°C to -35°C. In this embodiment, the dew point of the atmosphere means the temperature at which the amount of water vapor contained in the atmosphere becomes the saturated water vapor amount at the same pressure. In this embodiment and in the examples and comparative examples described later, a capacitance type dew point meter (online dew point meter TK-100 manufactured by Techne Measurement Co., Ltd.) was used to measure the dew point of the atmosphere.

[0044] The present applicant has found that the Li content in the crystal changes depending on the dew point of the atmosphere in the growth process, causing cracks. In lithium-containing oxide crystals, the change in Li content causes clouding and cracks in the appearance, resulting in variation in the characteristics within the crystal. By setting the dew point of the atmosphere in the growth process to a range of -70°C or higher and -35°C or lower, clouding and cracks are suppressed, and the variation in characteristics is suppressed, resulting in a crystal with a crystal size of 0.38 cm. 2 It is possible to obtain uniform lithium-containing oxide crystals having the above cross-sectional area.

[0045] In addition, by setting the dew point of the atmosphere in the growth process to within the range of -70°C to -40°C, the 2 More than 100cm2 It is possible to grow and form a lithium-containing oxide crystal having the following area. Furthermore, by setting the dew point of the atmosphere in the growth step within the range of -65°C or more and -45°C or less, it is possible to grow and form a lithium-containing oxide crystal with a longitudinal dimension (i.e., the length in the growth direction of the lithium-containing oxide crystal) of 10 mm or more from the molten part.

[0046] Examples of the present invention will be described below, but the present invention is not limited to the following examples. (Examples 1 and 2 and Comparative Example 1)

[0047] First, in Examples 1 and 2 and Comparative Example 1, a lithium-containing oxide crystal, Li 6.5 La3Zr 1.5 Nb 0.5 O 12 was grown. The amount of Li contained in the raw material was 108% of the Li contained in the obtained lithium-containing oxide crystal. The atmosphere during the growth step was air (dry air) at 1 atmosphere at room temperature flowing at a flow rate of 7 liters per minute, and the dew points were set to -35°C, -55°C, and -20°C in Examples 1 and 2 and Comparative Example 1, respectively. The obtained lithium-containing oxide crystal was visually inspected using an optical microscope.

[0048] 2 is a table showing the evaluation of the lithium-containing oxide crystals grown by the FZ method in Examples 1 and 2 and Comparative Example 1. The area column in FIG. 2 shows the cross-sectional area of ​​the portion where no cracks have occurred, and the length column shows the cross-sectional area of ​​0.38 cm 2 The above shows the length in the growth direction of the portion where no cracks have occurred. Figures 3(a) to (c) are photographs showing the appearance of the lithium-containing oxide crystals of Examples 1 and 2 and Comparative Example 1, respectively. The left side in Figures 3(a) to (c) is the starting side of crystal growth, and the as-grown state in which the raw material was melted and grown toward the right side is shown.

[0049] As shown in FIG. 2 and FIG. 3, in Example 1, the diameter is 7 mm and the cross-sectional area is 0.38 cm 2In Example 2, the diameter was 7 mm and the cross-sectional area was 0.38 cm. 2 In the comparative example 1, the lithium-containing oxide crystal had cracks all over the surface, and there was no region without cracks. Therefore, when the dew point was higher than -35°C, the cross-sectional area was 0.38 cm 2 It is clear that it is impossible to obtain a lithium-containing oxide crystal without the above cracks. (Examples 3 to 6 and Comparative Example 2)

[0050] Next, in Examples 3 to 6 and Comparative Example 2, the lithium-containing oxide crystal Li was prepared by the FZ method. 6.5 La3Zr 1.5 Nb 0.5 O 12 were grown. The amount of Li contained in the raw material was 108% of the Li contained in the obtained lithium-containing oxide crystal. The atmosphere during the growth step was air (dry air) at room temperature and 1 atm flowing at a flow rate of 7 liters per minute, and the dew points were set to -40°C, -43°C, -48°C, -62°C, and -68°C in Examples 3 to 6 and Comparative Example 2, respectively. The obtained lithium-containing oxide crystal was visually inspected using an optical microscope.

[0051] 4 is a table showing external appearance photographs of lithium-containing oxide crystals grown by the FZ method under different dew point conditions in Examples 3 to 6 and Comparative Example 2. In Fig. 4, the dew point is -40°C in Example 3, -43°C in Example 4, -48°C in Example 5, -62°C in Example 6, and -68°C in Comparative Example 2. In all of Examples 3 to 6, the cross-sectional area is 0.38 cm 2 There were regions where cracks were not generated within the regions. In addition, in all of Examples 3 to 6 and Comparative Example 2, the electrical conductivity was 0.65 (mS / cm) or more, and in particular, in Example 5, it was 0.85 (mS / cm). On the other hand, in Comparative Example 2, cracks were generated along the crystal growth direction of the lithium-containing oxide crystals, and there was no region without cracks.

[0052] As shown in FIG. 4, in Example 3, white turbidity due to Li deficiency was partially observed, and the cross-sectional area was 0.38 cm 2 The crack-free area was less than 10 mm. 2 The crack-free area was less than 10 mm. Therefore, by setting the dew point within the range of -65°C to -45°C, the cross-sectional area was reduced to 0.38 cm2. 2 It can be seen that a crack-free region with dimensions of 10 mm or more can be formed. (Examples 7 to 10)

[0053] Next, in Examples 7 to 10, lithium-containing oxide crystals, Li 6.5 La3Zr 1.5 Nb 0.5 O 12 and Li 6.5 La3Zr 1.5 Nb 0.25 Ta 0.25 O 12 The atmosphere during the growth step was set to N2 at 1 atm at room temperature at a flow rate of 2 to 4 liters per minute, and the dew points of Examples 7 to 10 were set to -40°C, -65°C, -66°C, and -69°C, respectively. An Ir material was used for the crucible. The obtained lithium-containing oxide crystal was visually inspected using an optical microscope.

[0054] 5 is a table showing the evaluation of Examples 7 to 10 of the lithium-containing oxide crystal grown by the CZ method. The area column in FIG. 5 shows the cross-sectional area of ​​a portion where no cracks have occurred, and the length column shows the cross-sectional area of ​​0.38 cm2 or less. 2 The above shows the length in the growth direction of the part where no cracks have occurred. 6.5 La3Zr 1.5 Nb 0.5 O 12 Example 9 is Li containing Ta. 6.5 La3Zr 1.5 Nb 0.25 Ta 0.25 O 126(a) to (d) are photographs showing the appearances of the lithium-containing oxide crystals of Examples 7 to 10, respectively. The left side in Fig. 6(a) to (d) is the starting side of crystal growth, and the as-grown state in which the raw material was melted and grown toward the right side is shown.

[0055] As shown in Fig. 5 and Fig. 6, in Example 7, the diameter was 18 mm and the cross-sectional area was 2.76 cm at the initial growth stage. 2 A crack-free area of ​​0.38 cm2 was formed. 2 There was also a 11 mm portion where no cracks had occurred. 2 A crack-free area of ​​0.38 cm2 was formed. 2 There was also a 38 mm portion where no cracks had occurred. 2 A crack-free area of ​​0.38 cm2 was formed. 2 There was also a 27 mm portion where no cracks had occurred. In Example 10, although some cracks had occurred, the diameter was 16 mm and the cross-sectional area was 2.0 cm 2 A crack-free area of ​​0.38 cm2 was formed. 2 There was still a 24mm section where no cracks had occurred.

[0056] Therefore, by setting the dew point within the range of -70°C to -40°C, the cross-sectional area is 1.76 cm 2 More than 100cm 2 It can be seen that a crack-free lithium-containing oxide crystal having the following area can be obtained. Example 11

[0057] Next, as Example 11, a lithium-containing oxide crystal, Li 6.8 La3Zr 1.8 Nb 0.2 O 12The atmosphere during the growth process was set to a condition of flowing N2 at 1 atm at a flow rate of 2 to 4 liters per minute at room temperature with a dew point of -65°C. An Ir material was used for the crucible. The obtained lithium-containing oxide crystal was visually inspected using an optical microscope.

[0058] The evaluation of Example 11 of the lithium-containing oxide crystal grown by the CZ method is shown below. Also, Fig. 7 is a photograph showing the appearance of the lithium-containing oxide crystal of Example 11. The right side in Fig. 7 is the starting side of the crystal growth, and the as-grown state in which the raw material was melted and grown toward the left side is shown.

[0059] As shown in FIG. 7, in Example 11, the crack-free region was 9.5 mm in diameter and 0.70 cm in cross-sectional area. 2 It is made of and has a cross-sectional area of ​​0.38 cm 2 There was also a portion in which no cracks had occurred that was 30 mm long in the longitudinal direction (length in the growth direction).

[0060] Therefore, by setting the dew point at -65°C, the cross-sectional area is reduced to 0.38 cm 2 It is understood that a lithium-containing oxide crystal having the above area and no cracks over a longitudinal dimension of 10 mm or more can be obtained.

[0061] As described above, in the present embodiment, it is possible to provide a lithium-containing oxide crystal having a large area without cracks and a manufacturing method thereof. In addition, it is possible to provide a battery including at least a part of the lithium-containing oxide crystal. Example 12

[0062] Next, as Example 12, a lithium-containing oxide crystal, Li 6.0 La3Zr 1.0 Nb 1.0 O 12was grown. The amount of Li contained in the raw material was 110% of the Li contained in the obtained lithium-containing oxide crystal. The atmosphere during the growth process was set to a condition of flowing N2 at 1 atm at a flow rate of 4 liters per minute at room temperature, with a dew point of -62°C. An Ir material was used for the crucible. The obtained lithium-containing oxide crystal was visually inspected using an optical microscope.

[0063] Fig. 8 is a photograph showing the appearance of the lithium-containing oxide crystal of Example 12. The left side in Fig. 8 is the starting side of the crystal growth, and the as-grown state in which the raw materials were melted and grown toward the right side is shown.

[0064] As shown in FIG. 8, in Example 12, the diameter is 7 mm and the cross-sectional area is 0.38 cm 2 There was an area of ​​11 mm, and no cracks were present within this area. (Example 13)

[0065] Next, as Example 13, a lithium-containing oxide crystal, Li 6.5 La3Zr 1.5 Ta 0.5 O 12 The atmosphere during the growth process was set to room temperature, 1 atm N2 at a flow rate of 4 liters per minute, and a dew point of -69°C. Ir material was used for the crucible. The obtained lithium-containing oxide crystal was visually inspected using an optical microscope.

[0066] Fig. 9 is a photograph showing the appearance of the lithium-containing oxide crystal of Example 13. The left side in Fig. 9 is the starting side of the crystal growth, and the as-grown state in which the raw material was melted and grown toward the right side is shown.

[0067] As shown in FIG. 9, in Example 13, the diameter is 7 mm and the cross-sectional area is 0.38 cm 2 There was a 12 mm area, and no cracks were found within that area.

[0068] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

Claims

1. A molten part forming step of melting at least a part of a lithium-containing oxide crystal raw material containing oxygen to form a molten part; A growing step of growing and forming a lithium-containing oxide crystal from the molten part, The dew point of the atmosphere in the growth step is set within a range of −65° C. or more and −45° C. or less; A method for producing a lithium-containing oxide crystal, wherein the lithium-containing oxide crystal has a cross-sectional area of ​​0.38 cm 2 or more and 1.76 cm 2 or less, and is grown to have a longitudinal dimension of 10 mm or more from the molten part.

2. A method for producing the lithium-containing oxide crystal according to claim 1, comprising the steps of: A method for producing a lithium-containing oxide crystal, wherein the growth step uses a CZ method or an EFG method.

Citation Information

Patent Citations

  • Method for manufacturing monopolarized lithium tantalate crystal and monopolarized lithium tantalate crystal

    JP2005119950A

  • Method for manufacturing oxide single crystal

    JP2006124223A

  • Rod-like seed crystal retainer

    JP2019001693A

  • Lowly symmetric garnet-related structured solid electrolyte and lithium secondary battery

    WO2017203954A1