Silicon nitride plate and its manufacturing method, composite substrate and its manufacturing method, and circuit substrate and its manufacturing method
By forming scribe lines on silicon nitride plates with a laser beam in multiple steps to minimize the oxygen-rich layer, the method addresses the issue of foreign matter generation, ensuring a good appearance and high reliability of the silicon nitride plates, composite substrates, and circuit boards.
Patent Information
- Application Number
- JP2022512241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-30
- Filing Date
- 2021-03-29
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2041-03-29
AI Technical Summary
The manufacturing process of silicon nitride plates for circuit boards generates foreign matter, such as an oxygen-rich layer, which affects the appearance and reliability of the final product, leading to potential contamination and decreased performance.
Forming scribe lines on silicon nitride plates using a laser beam in multiple steps to reduce the energy per shot, thereby minimizing the formation of an oxygen-rich layer, ensuring the silicon nitride plate maintains a good appearance and enhances reliability.
The method effectively reduces the thickness and presence of the oxygen-rich layer, preventing contamination and maintaining the appearance of the silicon nitride plate, improving its reliability and reducing facility contamination during manufacturing.
Smart Images

Figure 0007573023000002 
Figure 0007573023000003 
Figure 0007573023000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a silicon nitride plate and a manufacturing method thereof, a composite substrate and a manufacturing method thereof, and a circuit substrate and a manufacturing method thereof. [Background technology]
[0002] An insulating ceramic plate may be used for a circuit board mounted on an electronic device. The following technique, as described in Patent Document 1, is known as a method for manufacturing such a circuit board. That is, a carbon dioxide laser, a YAG laser, or the like is used to provide a scribe line on the surface of a ceramic plate, and then a metal layer is bonded to the surface to form a composite substrate. Then, the metal layer on the surface of the composite substrate is processed into a circuit pattern by etching. After that, the composite substrate is divided along the scribe lines to manufacture a plurality of circuit substrates. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-324301 A Summary of the Invention [Problem to be solved by the invention]
[0004] Silicon nitride plates are made into products or parts through various processes such as bonding with metal plates and forming circuits. As electronic devices become more and more sophisticated, the required quality level is also becoming higher and higher. Under these circumstances, there is concern that foreign matter generated during the manufacturing process may not only deteriorate the appearance of the product, but also cause a decrease in product performance.
[0005] Therefore, the present disclosure provides a silicon nitride plate that maintains a good appearance and has excellent reliability, and a method for manufacturing the same. The present disclosure also provides a composite substrate that maintains a good appearance and has excellent reliability, and a method for manufacturing the same. The present disclosure also provides a circuit board that maintains a good appearance and has excellent reliability, and a method for manufacturing the same. [Means for solving the problem]
[0006] The scribe lines on the silicon nitride plate need to have a certain depth so that the silicon nitride plate can be divided smoothly in the subsequent process. In order to form scribe lines with a certain depth, it is necessary to irradiate a laser beam with a suitable energy. However, if the energy of the laser beam becomes too high, the silicon nitride contained in the base material burns and foreign matter is generated inside the hole, which causes contamination of the silicon nitride plate.
[0007] Therefore, in one aspect, the present disclosure provides a method for producing a silicon nitride plate having a scribe line on its surface, the method comprising a step of forming a plurality of holes in the surface of a substrate containing silicon nitride with laser light to provide a scribe line, and each of the plurality of holes is formed by irradiating the laser light multiple times.
[0008] In the above manufacturing method, when forming a plurality of holes that become scribe lines, each hole is formed by irradiating the laser light multiple times. Therefore, the energy of the laser light irradiated per time (one shot) can be reduced compared to when holes are formed by irradiating only once. This makes it possible to efficiently use the laser light to form the holes, and scorching can be suppressed. Therefore, the generation of an oxygen-rich layer, which is a foreign matter, can be suppressed, and a good appearance of the silicon nitride plate can be maintained. Such a silicon nitride plate is also excellent in reliability because the amount of the oxygen-rich layer that peels off can be reduced. In addition, contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer in the subsequent process can be suppressed.
[0009] When the laser beam is irradiated in multiple steps, the energy of the laser beam per shot may be less than 15 mJ, which can sufficiently reduce the amount of an oxygen-rich layer formed inside the hole.
[0010] The opening diameter of the holes on the surface of the silicon nitride plate obtained by the above manufacturing method may be 50 μm or more, and the hole depth may be 50 μm or more. A silicon nitride plate having scribe lines formed by such holes can be divided smoothly.
[0011] The maximum thickness of the oxygen-rich layer at the bottom of the hole may be less than 8 μm, which satisfactorily reduces the oxygen-rich layer as a foreign matter and satisfactorily suppresses the generation of dirt.
[0012] The thickness of the oxygen-rich layer on the surface may be smaller than that on the inner surface of the hole, which makes it possible to sufficiently suppress contamination of the surface of the silicon nitride plate and to improve the bondability.
[0013] In one aspect, the present disclosure provides a silicon nitride plate having a scribe line on its surface, in which the thickness of an oxygen-rich layer at the bottom of a plurality of holes constituting the scribe line is less than 8 μm. In this silicon nitride plate, the oxygen-rich layer, which is a foreign matter, is sufficiently reduced. As a result, the generation of dirt can be sufficiently suppressed and a good appearance can be maintained. Such a silicon nitride plate is also excellent in reliability because the amount of the oxygen-rich layer that peels off can be reduced. In addition, contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer can be reduced.
[0014] In one aspect, the present disclosure provides a silicon nitride plate having a scribe line on its surface, in which the thickness of the oxygen-rich layer on the surface is thinner than that on the inner surfaces of a plurality of holes constituting the scribe line. Since the oxygen-rich layer on the surface of this silicon nitride plate is reduced, the generation of dirt can be sufficiently suppressed. Therefore, a good appearance can be maintained. In addition, the bondability with a member bonded to the surface of the silicon nitride plate can be improved. Therefore, the reliability is also excellent. Furthermore, since the oxygen-rich layer exposed on the surface can be reduced, the contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer can be reduced. It is noted that there may be no oxygen-rich layer on the surface at all.
[0015] The opening diameter of the holes on the surface may be 50 μm or more, and the depth of the holes may be 50 μm or more. A silicon nitride plate having scribe lines formed by such holes can be smoothly divided.
[0016] In one aspect, the present disclosure provides a method for producing a composite substrate, comprising the step of bonding a metal plate to a silicon nitride plate so as to cover the surface of the silicon nitride plate obtained by any one of the above-mentioned production methods to obtain a composite substrate. Since this composite substrate includes a silicon nitride plate obtained by any one of the above-mentioned production methods, the oxygen-rich layer, which is a foreign matter, is reduced, and a good appearance can be maintained. Such a composite substrate is also excellent in reliability because the oxygen-rich layer peeling off from the holes in the silicon nitride plate can be reduced. In addition, contamination of each production facility due to peeling and scattering of the oxygen-rich layer can be reduced.
[0017] In one aspect, the present disclosure provides a method for manufacturing a circuit board, comprising the steps of removing a portion of the metal plate in the composite substrate obtained by the above-mentioned manufacturing method, and forming an independent conductor portion for each partition portion defined by a scribe line to obtain a circuit board. Since this circuit board uses the composite substrate obtained by the above-mentioned manufacturing method, the oxygen-rich layer, which is a foreign matter, is reduced, and a good appearance can be maintained. Such a circuit board is also excellent in reliability because the oxygen-rich layer peeling off from the holes in the silicon nitride plate can be reduced. In addition, contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer can be reduced.
[0018] In one aspect, the present disclosure provides a composite substrate comprising any one of the silicon nitride plates described above and a metal plate bonded to the silicon nitride plate so as to cover the surface of the silicon nitride plate. Since the composite substrate comprises any one of the silicon nitride plates described above, the oxygen-rich layer, which is a foreign matter, is reduced, and a good appearance can be maintained. Such a composite substrate is also excellent in reliability because it is possible to reduce the amount of the oxygen-rich layer peeling off from the holes in the silicon nitride plate. In addition, it is possible to reduce contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer.
[0019] In one aspect, the present disclosure provides a circuit board comprising any one of the silicon nitride plates described above and a conductor portion provided on the surface so as to be independent of each partition portion defined by a scribe line. Since this circuit board comprises any one of the silicon nitride plates described above, foreign matter is reduced and a good appearance can be maintained. Such a circuit board is also excellent in reliability because the oxygen-rich layer peeling off from the holes in the silicon nitride plate can be reduced. In addition, contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer can be reduced. Effect of the Invention
[0020] According to the present disclosure, it is possible to provide a silicon nitride plate and a method for manufacturing the same that are highly reliable while maintaining a good appearance. It is also possible to provide a composite substrate and a method for manufacturing the same that are highly reliable while maintaining a good appearance. It is also possible to provide a circuit board and a method for manufacturing the same that are highly reliable while maintaining a good appearance. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a perspective view of a silicon nitride plate according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the silicon nitride plate of FIG. 1 taken along line II-II. [Diagram 3] FIG. 3 is a cross-sectional view of the silicon nitride plate of FIG. 1 taken along line III-III. [Figure 4] FIG. 4 is a partially enlarged view showing a scribe line provided on a portion of the surface of a silicon nitride plate. [Diagram 5] FIG. 5 is a cross-sectional view taken along line VV of the silicon nitride plate of FIG. [Figure 6] FIG. 6 is an enlarged cross-sectional view of a portion of the silicon nitride plate where a hole is formed. [Figure 7] FIG. 7 is a perspective view showing an example of a silicon nitride plate to which a brazing material is applied. [Figure 8] FIG. 8 is a perspective view of a composite substrate according to an embodiment. [Figure 9] FIG. 9 is a perspective view showing an example of a composite substrate having a resist pattern formed on the surface thereof. [Figure 10] FIG. 10 is a perspective view of a circuit board according to an embodiment. [Figure 11] FIG. 11 is an SEM photograph of the surface and cross section of the silicon nitride plate of Example 1 in which a plurality of holes constituting the scribe lines are formed. [Figure 12] FIG. 12 is an SEM photograph of the surface and cross section of the silicon nitride plate of Comparative Example 1 in which a plurality of holes constituting the scribe lines were formed. [Figure 13]FIG. 13 is a SEM photograph taken at 250 and 500 magnifications of a cross section of a silicon nitride plate with a hole formed therein. [Figure 14] FIG. 14 is a SEM photograph taken at 1000 and 2500 magnifications of a cross section of a silicon nitride plate with a hole formed therein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings as needed. However, the following embodiment is an example for explaining the present disclosure, and is not intended to limit the present disclosure to the following content. In the description, the same reference numerals are used for the same elements or elements having the same functions, and redundant descriptions are omitted as needed. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the dimensional ratios of each element are not limited to the ratios shown in the drawings.
[0023] Fig. 1 is a perspective view of a silicon nitride plate according to one embodiment. The silicon nitride plate 100 in Fig. 1 has a flat plate shape. A surface 100A of the silicon nitride plate 100 is divided into a plurality of sections by scribe lines. The surface 100A is provided with a plurality of scribe lines L1 extending along a first direction and arranged at equal intervals, and a plurality of scribe lines L2 extending along a second direction perpendicular to the first direction and arranged at equal intervals. The scribe lines L1 and L2 are perpendicular to each other.
[0024] The scribe lines L1, L2 are composed of a plurality of holes formed by laser light. Examples of the laser source include a carbon dioxide laser and a YAG laser. The scribe lines can be provided by forming a plurality of holes along a predetermined direction by intermittently irradiating the laser light from such a laser source. Note that the scribe lines L1, L2 do not have to be arranged at equal intervals, and are not limited to being perpendicular to each other. Moreover, they may be curved or bent instead of straight.
[0025] Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1, and Fig. 3 is a cross-sectional view taken along line III-III in Fig. 1. As shown in Figs. 1, 2, and 3, the partition 10 is composed of a three-dimensional area surrounded by an area on one surface 100A surrounded by scribe lines L1, L2, an area on the other surface 100B corresponding to said area, and imaginary lines VL1, VL2 drawn parallel to the thickness direction of the silicon nitride plate 100 from the scribe lines L1, L2. That is, the silicon nitride plate 100 has a plurality of partitions 10 (9 in Fig. 1) defined by the scribe lines L1 and L2.
[0026] 1, 2 and 3 show an example in which the scribe lines L1, L2 are formed only on one surface 100A of the silicon nitride plate 100, but the present invention is not limited to this example. In other words, the scribe lines L1, L2 may also be formed on the surface 100B of the silicon nitride plate 100 opposite to the surface 100A.
[0027] FIG. 4 is a partially enlarged view showing a scribe line L1 provided on a portion of the surface 100A of the silicon nitride plate 100. The scribe line L1 (L2) is composed of a plurality of holes 20 arranged along the longitudinal direction. The adjacent holes 20 may be connected to each other or may be separated from each other. The opening 20E of the hole 20 on the surface 100A may be circular. The diameter of the opening 20E, i.e., the opening diameter r, may be 50 μm or more, or may be 70 μm or more. The silicon nitride plate 100 having the scribe line L1 (L2) composed of the holes 20 having such an opening diameter r can be smoothly divided along the scribe line L1 (L2). From the viewpoint of maintaining the mechanical strength of the silicon nitride plate 100, the opening diameter r may be 300 μm or less, or may be 200 μm or less. In a modified example, the adjacent holes 20 may be separated from each other. In another modified example, the adjacent holes 20 may partially overlap each other.
[0028] 5 is a cross-sectional view of line VV in FIG. 4. That is, FIG. 5 is a cross-sectional view of the silicon nitride plate 100 cut along a plane passing through the scribe line L1 (L2) and perpendicular to the surface 100A. The hole 20 has a cone shape tapering from the opening 20E toward the inside of the silicon nitride plate 100. The hole 20 has a depth d from the opening 20E on the surface 100A to the bottom 20B. When the thickness of the silicon nitride plate 100 is 0.15 to 1 mm, the depth d may be 50 μm or more, or may be 60 μm or more. The silicon nitride plate 100 having the scribe line L1 (L2) formed by the hole 20 having such a depth d can be smoothly divided along the scribe line L1 (L2). From the viewpoint of maintaining the mechanical strength of the silicon nitride plate 100, the depth d may be half or less, or may be one-third or less of the thickness of the silicon nitride plate 100. The depth d of the multiple holes 20 may be the same or different.
[0029] Fig. 6 is a cross-sectional view showing a cross section of a portion of a silicon nitride plate where a hole 20 is formed, enlarged from Fig. 5. As shown in Fig. 6, at least a part of the inner surface of the cone-shaped hole 20 may be covered with an oxygen-rich layer 22. The oxygen-rich layer 22 is substantially not formed on the surface 100A, and the thickness of the oxygen-rich layer 22 on the surface 100A is smaller than that of the inner surface of the hole 20. This makes it possible to sufficiently suppress the generation of stains caused by the oxygen-rich layer 22. In addition, it is possible to improve the bondability with a member bonded to the surface 100A.
[0030] The maximum thickness t of the oxygen-rich layer 22 at the bottom 20B of the hole 20 may be less than 8 μm, less than 6 μm, or less than 5 μm. The oxygen-rich layer 22 is a region in which the oxygen concentration on a mass basis is three times or more higher than that of the surface 100A of the silicon nitride plate 100 in the portion where the scribe lines L1, L2 are not formed. The oxygen concentration can be measured with an EPMA (electron probe microanalyzer).
[0031] The oxygen rich layer 22 is composed of a foreign matter other than silicon nitride. The oxygen rich layer 22 may contain, for example, an oxide. The oxide may be, for example, silicon dioxide. The thickness of the oxygen rich layer 22 is usually greatest at the bottom 20B of the hole 20. Therefore, by reducing the maximum thickness t, the oxygen rich layer 22 is reduced, and contamination due to peeling of the oxygen rich layer 22 can be suppressed. Such a silicon nitride plate 100 can suppress a decrease in reliability caused by peeling of the oxygen rich layer 22. Also, contamination of each manufacturing facility due to the oxygen rich layer 22 can be reduced. The maximum thickness t is measured along a direction perpendicular to the surface 100A.
[0032] 6 shows an example in which the entire inner surface of the hole 20 is covered with the oxygen-rich layer 22, but the present invention is not limited to such an example. For example, only a part of the inner surface of the hole 20 may be covered with the oxygen-rich layer 22, or the inner surface of the hole 20 may not be covered with the oxygen-rich layer 22 at all. In this case, it is possible to prevent the occurrence of contamination due to foreign matter. Such a silicon nitride plate 100 has sufficiently excellent reliability.
[0033] As a method for producing a silicon nitride plate according to one embodiment, a method for producing a silicon nitride plate 100 will be described. The method for producing the silicon nitride plate 100 includes a step of producing a substrate containing silicon nitride, and a step of forming a plurality of holes on the surface of the substrate with a laser beam to provide scribe lines, thereby obtaining the silicon nitride plate 100.
[0034] The substrate containing silicon nitride can be manufactured by the following procedure. First, a slurry containing silicon nitride powder, binder resin, sintering aid, plasticizer, dispersant, solvent, etc. is molded to obtain a green sheet. Examples of the sintering aid include rare earth metals, alkaline earth metals, metal oxides, fluorides, chlorides, nitrates, and sulfates. These may be used alone or in combination of two or more. The use of the sintering aid can promote the sintering of the inorganic compound powder. Examples of the binder resin include methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, and (meth)acrylic resins.
[0035] Examples of the plasticizer include purified glycerin, glycerin trioleate, diethylene glycol, phthalic acid plasticizers such as di-n-butyl phthalate, and dibasic acid plasticizers such as di-2-ethylhexyl sebacate. Examples of the dispersant include poly(meth)acrylate and (meth)acrylic acid-maleate copolymer. Examples of the solvent include organic solvents such as ethanol and toluene.
[0036] Examples of the method for forming the slurry include the doctor blade method and the extrusion molding method. A green sheet is produced by such a method. The green sheet is degreased and sintered to obtain a base material containing silicon nitride. The degreasing may be performed, for example, by heating at 400 to 800°C for 0.5 to 20 hours. This makes it possible to reduce the amount of residual organic matter (carbon) while suppressing oxidation and deterioration of silicon nitride. The sintering may be performed by heating to 1700 to 1900°C in a non-oxidizing gas atmosphere such as nitrogen, argon, ammonia, or hydrogen.
[0037] The above-mentioned degreasing and sintering may be performed in a state where a plurality of green sheets are laminated. When the green sheets are laminated and degreasing and sintering are performed, a release layer made of a release agent may be provided between the green sheets in order to facilitate separation of the base material after firing. For example, boron nitride (BN) may be used as the release agent. The release layer may be formed by applying, for example, a slurry of boron nitride powder by a method such as spraying, brushing, roll coating, or screen printing. The number of green sheets to be laminated may be, for example, 8 to 100 sheets, or may be 30 to 70 sheets, from the viewpoint of efficiently mass-producing the base material while sufficiently proceeding with degreasing.
[0038] A laser beam is irradiated onto the surface of the silicon nitride-containing substrate thus obtained to form a plurality of holes. As a result, a silicon nitride plate 100 having scribe lines L1, L2 on the surface 100A is obtained as shown in Figs. 1 to 3. Examples of the laser beam include a carbon dioxide gas laser and a YAG laser. Each of the plurality of holes 20 shown in Figs. 4 and 5 is formed by irradiating the laser beam multiple times. As a result, the energy of the laser beam irradiated per shot (one shot) can be reduced compared to the case where a hole is formed by irradiating only once. Therefore, it is possible to efficiently use the laser beam to form the holes 20, and the scorching of the silicon nitride can be suppressed. As a result, the generation of the oxygen-rich layer 22 shown in Fig. 6 can be suppressed, and the good appearance of the silicon nitride plate can be maintained. Such a silicon nitride plate 100 has excellent reliability because the amount of the oxygen-rich layer 22 peeling off can be reduced. In addition, contamination of the silicon nitride plate 100 and each manufacturing facility using the same can be reduced.
[0039] The holes 20 may be formed by a burst pulse mode or a cycle pulse mode. The burst pulse mode is performed according to the following procedure. The first hole 20 is formed by irradiating the same position with a laser beam divided into a number of times. Next, the second hole 20 is formed by irradiating the same position with a laser beam divided into a number of times so as to be adjacent to the first hole 20. In this way, two holes 20 adjacent to each other are formed. This procedure is repeated a number of times to form n holes 20 (n is a positive integer of 2 or more). In this way, a scribe line L1 (L2) consisting of n holes 20 can be formed. When irradiating the laser beam twice to form one hole 20, the laser beam is irradiated divided into 2n times to form n holes 20.
[0040] The cycle pulse mode is performed, for example, in the following manner. The first to n-th holes 20 are each formed by irradiating the laser light once. After that, the first to n-th holes 20 are irradiated with the laser light once again. In this case, the laser light is irradiated 2n times to form n holes 20. The laser light may be irradiated three or more times to form each hole 20. From the viewpoint of work efficiency, the number of times (number of shots) of irradiating the laser light to form each hole 20 may be 10 or less. The method of forming the holes 20 is not limited to the above two methods. For example, the burst pulse mode and the cycle pulse mode may be combined.
[0041] The interval between multiple laser light irradiations to form one hole 20 may be 100 μsec or more (10 kHz or less) or 1000 μsec or more (1 kHz or less) to ensure cooling time for the silicon nitride plate 100 heated by the laser light irradiation.
[0042] The energy of the laser light irradiated per time, i.e., the energy per shot, may be less than 15 mJ, may be 12 mJ or less, or may be 10 mJ or less. By reducing the energy irradiated per time in this manner, the maximum thickness t of the oxygen-rich layer 22 formed on the inner surface of the hole 20 can be sufficiently reduced. From the viewpoint of efficiently forming the hole 20, the energy of the laser light irradiated per time may be 2 mJ or more, or may be 4 mJ or more.
[0043] The pulse width of the laser light may be 3 to 20 μsec, or may be 5 to 15 μsec, from the viewpoint of forming a sufficiently large hole 20 on the surface 100A of the silicon nitride plate 100 while reducing damage to the silicon nitride plate 100.
[0044] By providing the scribe lines L1, L2 in this manner, it is possible to obtain the silicon nitride plate 100. The scribe lines L1, L2 will become cutting lines when dividing the silicon nitride plate 100 (circuit board) in a later process.
[0045] In the above-mentioned method for manufacturing a silicon nitride plate, the holes 20 constituting the scribe lines L1 (L2) are each formed by irradiating the laser light multiple times. Therefore, the energy of the laser light irradiated per time (one shot) can be reduced compared to when the holes are formed by irradiating only once. This reduces the amount of foreign matter (oxygen-rich layer 22) generated on the inner surface of the hole 20, and the silicon nitride plate 100 can maintain a good appearance. Such a silicon nitride plate 100 is also excellent in reliability because the oxygen-rich layer 22 can be reduced. In addition, contamination of each manufacturing facility due to peeling and scattering of the oxygen-rich layer 22 in the later process can be suppressed.
[0046] A manufacturing method for a composite substrate according to one embodiment uses the above-mentioned silicon nitride plate 100. That is, this manufacturing method includes a step of laminating a pair of metal plates so as to cover the surfaces 100A and 100B of the silicon nitride plate 100, respectively, and bonding the pair of metal plates to the silicon nitride plate 100 to obtain a composite substrate. The metal plates may have a flat plate shape similar to that of the silicon nitride plate 100. The pair of metal plates are bonded to the surfaces 100A and 100B of the silicon nitride plate 100, respectively, via a brazing material.
[0047] Specifically, first, a paste-like brazing material is applied to a pair of surfaces 100A, 100B of a silicon nitride plate 100 by a roll coater method, a screen printing method, a transfer method, or the like. The brazing material contains, for example, metal components such as silver and titanium, an organic solvent, and a binder. The viscosity of the brazing material may be, for example, 5 to 20 Pa·s. The content of the organic solvent in the brazing material may be, for example, 5 to 25 mass %, and the content of the binder may be, for example, 2 to 15 mass %.
[0048] Fig. 7 is a perspective view showing an example of a silicon nitride plate 100 to which a brazing material 40 has been applied. As shown in Fig. 7, the brazing material 40 may be applied independently to each partition 10. Fig. 7 shows only the front surface 100A side, but the brazing material 40 may be applied to the front surface 100B side as well. In a modified example, the brazing material may be applied to the entire surfaces 100A and 100B.
[0049] In this way, a metal plate is bonded to the surface 100A and the surface 100B of the silicon nitride plate 100 coated with the brazing material 40 to obtain a bonded body. Then, the silicon nitride plate 100 and the pair of metal plates are sufficiently bonded to obtain a composite substrate by heating in a heating furnace. The heating temperature may be, for example, 700 to 900°C. The atmosphere in the heating furnace may be an inert gas such as nitrogen, and may be under reduced pressure below atmospheric pressure or under vacuum. The heating furnace may be a continuous type that continuously produces a plurality of bonded bodies, or may be a batch type that produces one or a plurality of bonded bodies. Heating may be performed while pressing the bonded bodies in the stacking direction.
[0050] The silicon nitride plate 100 has a reduced oxygen-rich layer 22 on the inner surface of the holes 20 that define the scribe lines L1, L2, making it possible to obtain a composite substrate with a good appearance. In addition, scattering of the oxygen-rich layer during firing is suppressed, making it possible to reduce contamination inside the heating furnace. In addition, since the amount of peeled-off oxygen-rich layer 22 can be reduced, it is possible to improve the bonding between the metal plate and the silicon nitride plate 100.
[0051] FIG. 8 is a perspective view of a composite substrate according to an embodiment. The composite substrate 200 includes a pair of metal plates 110 arranged to face each other, and a silicon nitride plate 100 between the pair of metal plates 110. The pair of metal plates 110 are joined to the silicon nitride plate 100 so as to cover the surface 100A and the surface 100B of the silicon nitride plate 100. The metal plate 110 may be a copper plate. The silicon nitride plate 100 and the metal plate 110 may have the same shape and size or may have different shapes and sizes. The composite substrate 200 can be manufactured by the above-mentioned manufacturing method. Since the oxygen-rich layer 22 formed in the hole 20 of the silicon nitride plate 100 is reduced, a good appearance can be maintained. Since the oxygen-rich layer 22 is reduced, such a composite substrate 200 has excellent reliability. In addition, contamination of the composite substrate 200 and each manufacturing facility using the same can be reduced.
[0052] In one embodiment of the method for manufacturing a circuit board, following the above-mentioned method for manufacturing a composite board, a process is performed in which a part of the metal plate in the composite board is removed to form an independent conductor part for each partition part. This process may be performed by, for example, photolithography. Specifically, first, a photosensitive resist is printed on the surface of the composite board. Then, an exposure device is used to form a resist pattern having a predetermined shape. The resist may be negative or positive. Uncured resist is removed by, for example, washing.
[0053] Fig. 9 is a perspective view showing an example of a composite substrate 200 having a resist pattern 30 formed on the front surface 200A. Although Fig. 9 shows only the front surface 200A side, a similar resist pattern may be formed on the front surface 200B side as well. The resist pattern 30 is formed on the front surface 200A and the front surface 200B in regions corresponding to each partition portion 10 of the silicon nitride plate 100.
[0054] After forming the resist pattern 30, the portions of the metal plate 110 that are not covered by the resist pattern 30 are removed by etching. This exposes the surfaces 100A and 100B of the silicon nitride plate 100 in those portions. Thereafter, the resist pattern 30 is removed to form independent conductor portions for each partition portion 10. Through the above steps, a circuit board is obtained.
[0055] The silicon nitride plate 100 has a reduced oxygen-rich layer 22 on the inner surface of the holes 20 that define the scribe lines L1, L2, making it possible to obtain a circuit board with a good appearance. In addition, the amount of peeled oxygen-rich layer 22 can be reduced, making it possible to suppress contamination of the inside of an exposure device, etc. Also, the bonding strength between the conductor and the silicon nitride plate 100 can be improved.
[0056] 10 is a plan view of a circuit board according to one embodiment. The circuit board 300 includes a silicon nitride plate 100 and conductors 50 arranged to face each other with the silicon nitride plate 100 in between. The conductors 50 are provided on the front surface 100A and the front surface 100B independently for each partition 10. That is, a pair of conductors 50 arranged to face each other is provided for each partition 10.
[0057] The circuit board 300 is cut along the scribe lines L1, L2 and divided into a plurality of divided boards. The divided boards are used as components of a power module, for example. Electronic components are mounted on the conductor parts 50 in the divided boards. The circuit board 300 can be manufactured by the above-mentioned manufacturing method. In the above-mentioned manufacturing method, the silicon nitride plate 100 in which the oxygen-rich layer 22 on the inner surface of the hole 20 is reduced is used, so that the circuit board 300 and its divided boards can maintain good appearances. When the divided boards are manufactured, the inner surfaces of the holes 20 that constituted the scribe lines L1, L2 are exposed to the outer edge. Therefore, by using the silicon nitride plate 100 in which the oxygen-rich layer 22 on the inner surface of the hole 20 is reduced, it is possible to maintain good appearances of not only the divided boards but also the power module on which the divided boards are mounted. In addition, the reliability of the power module can be improved.
[0058] Although several embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. For example, the shapes of the conductors 50 provided in each partition 10 do not need to be the same, and each partition 10 may have a different shape. In addition, the silicon nitride plate and the composite substrate may have a shape other than a rectangular prism shape.
[0059] Any surface treatment may be applied to the conductor portion 50 of the circuit board 300. For example, a part of the surface of the conductor portion 50 may be covered with a protective layer such as a solder resist, and the other part of the surface of the conductor portion 50 may be plated. EXAMPLES
[0060] [Preparation of silicon nitride plate with scribe lines] Example 1 A flat silicon nitride plate (length x width x thickness = 139.7 mm x 190.5 mm x 0.32 mm) was prepared. A carbon dioxide gas laser processing machine was used to form multiple holes in a line along one direction on the surface of this silicon nitride plate, providing scribe lines. The multiple holes were formed by irradiating the same position with laser light twice in burst pulse mode (number of shots: 2). The energy and pulse width of the laser light per shot were as shown in Table 1.
[0061] Comparative Example 1 A silicon nitride plate of the same shape and material as in Example 1 was prepared. A carbon dioxide gas laser processing machine was used to form a plurality of holes aligned in one direction on the surface of this silicon nitride plate, providing scribe lines. Each hole was formed by irradiating the laser light only once (number of shots: 1). The energy and pulse width of the laser light per shot were as shown in Table 1.
[0062] [Evaluation of holes that make up scribe lines 1] Fig. 11 shows SEM photographs of the surface and cross section of the silicon nitride plate of Example 1 in which a plurality of holes constituting scribe lines are formed. SEM photograph A in Fig. 11 shows the surface of the silicon nitride plate of Example 1 in which a plurality of holes 20 are formed. SEM photograph B in Fig. 11 shows the cross section of the silicon nitride plate of Example 1 in which a plurality of holes 20 are formed. That is, SEM photograph B shows a cross section when the silicon nitride plate is cut along a plane perpendicular to the surface on which the scribe lines are formed and passing through the scribe lines.
[0063] Fig. 12 shows SEM photographs of the surface and cross section of the silicon nitride plate of Comparative Example 1 in which a plurality of holes constituting scribe lines are formed. SEM photograph A in Fig. 12 shows the surface of the silicon nitride plate of Comparative Example 1 in which a plurality of holes 20 are formed. SEM photograph B in Fig. 12 shows a cross section of the silicon nitride plate of Comparative Example 1 in which a plurality of holes 20 are formed. That is, SEM photograph B shows a cross section when the silicon nitride plate is cut along a plane perpendicular to the surface on which the scribe lines are provided and passing through the scribe lines.
[0064] Fig. 13 is a SEM photograph taken at 250x and 500x magnification of the cross section of the silicon nitride plate in which a hole was formed of Example 1 and Comparative Example 1. Fig. 14 is a SEM photograph taken at 1000x and 2500x magnification of the cross section of the silicon nitride plate in which a hole was formed of Example 1 and Comparative Example 1. Figs. 13 and 14 show a cross section of the silicon nitride plate cut along a plane perpendicular to the surface on which the scribe lines are formed and perpendicular to the longitudinal direction of the scribe lines.
[0065] As shown in Figures 13 and 14, in Comparative Example 1, it was confirmed that the inner surface of the hole was covered with a layer that was whiter than the color of silicon nitride. When this white layer was analyzed by EPMA, it was confirmed that it contained oxygen. In other words, it was confirmed that the white layer was an oxygen-rich layer that contained more oxygen than the inside of the silicon nitride plate. The maximum thickness t of the oxygen-rich layer at the bottom of the hole was measured to be 10 μm.
[0066] On the other hand, in Example 1, the thickness of the oxygen-rich layer (oxygen concentration was the same as in Comparative Example 1) on the inner surface and bottom of the hole was thinner than in Comparative Example 1. The maximum thickness t of the oxygen-rich layer at the bottom of the hole was 3 μm. This confirmed that the oxygen-rich layer formed on the inner surface of the hole could be reduced by irradiating the laser light multiple times when forming the hole.
[0067] [Evaluation of holes that make up scribe lines 2] The portions of the surfaces of the silicon nitride plates of Example 1 and Comparative Example 1 where the scribe lines were formed were observed with an optical microscope (magnification: 250 times), and the opening diameter r of the hole 20 was measured. The results are shown in Table 1. Furthermore, the silicon nitride plates of Example 1 and Comparative Example 1 were folded along the scribe lines to obtain cross sections as shown in SEM photographs B of Figs. 11 and 12. The cross sections were observed with an optical microscope (magnification: 250 times), and the depth d of the hole 20 was measured. The results are shown in Table 1.
[0068] [Table 1]
[0069] In the silicon nitride plate of Example 1, the thickness of the oxygen-rich layer formed at the bottom of the hole constituting the scribe line was significantly smaller than that of Comparative Example 1. Such a silicon nitride plate is capable of suppressing contamination due to peeling of the oxygen-rich layer and maintaining a good appearance. In addition, it is possible to suppress the decrease in reliability due to peeling of the oxygen-rich layer and reduce contamination of each manufacturing facility. [Industrial Applicability]
[0070] According to the present disclosure, it is possible to provide a silicon nitride plate and a method for manufacturing the same that are highly reliable while maintaining a good appearance. It is also possible to provide a composite substrate and a method for manufacturing the same that are highly reliable while maintaining a good appearance. It is also possible to provide a circuit board and a method for manufacturing the same that are highly reliable while maintaining a good appearance. [Explanation of symbols]
[0071] 10...partition, 20...hole, 20B...bottom, 20E...opening, 22...oxygen-rich layer, 30...resist pattern, 40...soldering material, 100...silicon nitride plate, 100A, 100B...surface, 110...metal plate, 200...composite substrate, 200A, 200B...surface, 300...circuit board, L1, L2...scribe line, VL1, VL2...virtual line.
Claims
1. A method for manufacturing a silicon nitride plate having a scribe line on a surface thereof, comprising the steps of: The method includes a step of forming a plurality of holes having bottoms on a surface of a substrate containing silicon nitride by using a laser beam to provide the scribe lines; Each of the plurality of holes is formed by irradiating the laser light a plurality of times, The method for manufacturing a silicon nitride plate, wherein the oxygen-rich layer on the surface is thinner than that on the inner surface of the hole.
2. 2. The method for producing a silicon nitride plate according to claim 1, wherein the energy of the laser light per irradiation is less than 15 mJ when the laser light is irradiated in a plurality of times.
3. 3. The method for manufacturing a silicon nitride plate according to claim 1, wherein the opening diameter of the holes on the surface is 50 μm or more, and the depth of the holes is 50 μm or more.
4. The method for producing a silicon nitride plate according to any one of claims 1 to 3, wherein the maximum thickness of the oxygen-rich layer at the bottom of the hole is less than 8 µm.
5. A method for manufacturing a silicon nitride plate described in any one of claims 1 to 4, wherein the depth of the hole is 1 / 3 or less of the thickness of the silicon nitride plate.
6. A silicon nitride plate having a scribe line on a surface thereof, A silicon nitride plate, wherein at least a portion of the inner surfaces of the multiple holes constituting the scribe line are covered with an oxygen-rich layer, the thickness of the oxygen-rich layer is greatest at the bottom of the hole, and the thickness of the oxygen-rich layer at the bottom is less than 8 μm.
7. A silicon nitride plate having a scribe line on a surface thereof, A silicon nitride plate, wherein the oxygen-rich layer on the surface is thinner than the thickness of the inner surface of a plurality of holes having bottoms that form the scribe line.
8. 8. The silicon nitride plate according to claim 6, wherein the opening diameter of the holes on the surface is 50 μm or more, and the depth of the holes is 50 μm or more.
9. A method for producing a composite substrate, comprising a step of bonding a metal plate to the silicon nitride plate obtained by the method for producing a composite substrate according to any one of claims 1 to 5 so as to cover the surface of the silicon nitride plate.
10. 10. A method for manufacturing a circuit board, comprising the steps of removing a portion of the metal plate in a composite substrate obtained by the manufacturing method according to claim 9, and forming an independent conductor portion for each partition portion defined by the scribe lines to obtain a circuit board.
11. A silicon nitride plate according to any one of claims 6 to 8, a metal plate bonded to the silicon nitride plate so as to cover the surface.
12. A silicon nitride plate according to any one of claims 6 to 8, a conductor portion provided on the surface so as to be independent for each partition portion defined by the scribe lines.
Citation Information
Patent Citations
Ceramic member and method of manufacturing the same and electronic component using the ceramic member
JP2006321702A
Method for manufacturing nitride ceramics circuit board
JP2007324301A
Ceramic assembled board
JP2014042066A
Silicon nitride ceramic aggregate substrate and manufacturing method therefor, and manufacturing method for silicon nitride sintered substrate
JP2017028192A
Method for roughening substrate, method for surface-treating substrate, method for producing spray-coated member, and spray-coated member
WO2016170895A1