Method for preparing and using glass-ceramics
By controlling primary crystallization temperature and time, the method addresses irregular deformation in glass covers, enhancing transmittance and yield through precise density and crystal growth management.
Patent Information
- Application Number
- JP2023549050
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-29
- Filing Date
- 2022-07-29
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2042-07-29
AI Technical Summary
Conventional glass covers for smartphones undergo irregular deformation during secondary crystallization, leading to reduced yield and material waste.
A method for preparing crystallized glass involving primary crystallization at controlled temperature and time conditions (x1, t) within specific ranges, followed by secondary crystallization, to achieve desired density (2.440g/cm³ ≦ y1 ≦ 2.490g/cm³) and controlled crystal growth, reducing deformation and improving yield.
The method effectively reduces deformation during secondary crystallization, enhances glass transmittance, and improves product yield by controlling primary crystallization parameters.
Smart Images

Figure 0007573119000004 
Figure 0007573119000001 
Figure 0007573119000002
Abstract
Description
[Technical field]
[0001] The present disclosure is in the field of glass preparation, and in particular relates to crystallized glass, its preparation method and uses. [Background technology]
[0002] With the advent of the information age, the portability and ease of use of smart devices are of particular importance, and mobile phones have become the most promising smart terminal devices at present. More and more new materials are being used in the design and manufacturing of smartphones, and cover glass is one of them. Mobile phone cover glass started from 2D, passed through the 2.5D era, and entered the new 3D era, which not only beautifies the appearance of mobile phones, but also greatly improves the tactile experience of users.
[0003] Glass is ideal for screen covers due to its excellent mechanical properties and light transmission. However, covers made of traditional glass could no longer meet people's demands, and so crystallized glass was born, a new development in cover glass. New materials bring not only new experiences, but also new challenges.
[0004] For covers with a predetermined shape (e.g., rounded), secondary heating is often required for crystallization. In the secondary crystallization, the crystallized glass is prone to irregular deformation, which can lead to reduced yields and waste of material. How to suppress the amount of deformation of crystallized glass prepared by secondary crystallization is a technical problem to be solved in this field. Summary of the Invention
[0005] The present disclosure has been made in view of the problems in the prior art, and has as an object to provide a method for preparing crystallized glass, the method comprising the steps of: Step (1): Nucleation is performed on a glass sheet, and then primary crystallization is performed, and the temperature of the primary crystallization is set to x 1 , the time of primary crystallization is t, The temperature of the primary crystallization x 1 and the time t of primary crystallization must satisfy the following conditions: (i) -a×t+652≦x 1 ≦-a×t+667 where a is a constant and 0.1≦a≦0.25, t is 10 to 300 minutes, and the crystallization temperature x 1 The unit is °C, (ii)y 1 =0.0029x 1 +b where y 1 is the glass density after the first crystallization, and 2.440 g / cm 3 ≦y 1 ≦2.490g / cm 3 And then, b is a constant and is 0.55 <b<0.60となる。 Step (2): A secondary crystallization is performed on the glass sheet after the primary crystallization.
[0006] The present disclosure provides a method for controlling the density y of a glass sheet after primary crystallization by controlling the temperature and time of primary crystallization for the glass sheet that requires secondary crystallization. 1 is 2.440g / cm 3 ≦y 1 ≦2.490g / cm 3 The desired type of crystal phase and the growth rate of the crystals are obtained so as to satisfy the above requirement and to approach the density after secondary crystallization. This reduces the amount of deformation during secondary crystallization and improves the product yield.
[0007] The principle is that when the glass reaches the corresponding density through primary crystallization, the crystal growth inside the glass becomes relatively slow and enters a lag stage, so that the glass does not expand significantly from a macroscopic point of view. 3 If the density is less than 2.490 g / cm, the crystal phase inside the glass does not grow or transform sufficiently, and the deformation rate of the crystallized glass increases due to secondary crystallization. 3In the above cases, the crystalline phase inside the glass has completely grown and transformed, but excessive growth of the crystalline phase occurs after secondary crystallization. In this case, the deformation ratio of the glass decreases, but the optical properties such as the light transmittance of the glass deteriorate.
[0008] Said glass sheet can be understood as a glass sheet obtained from glass raw materials after melting, forming and low-temperature treatment. The specific preparation process typically includes, but is not limited to, weighing and mixing glass raw materials. In the melt forming of glass, its forming method includes, but is not limited to, float method, overflow method, roll-out method, pouring method, etc. The formed glass plate is annealed and low-temperature treated to obtain a glass sheet of the same size.
[0009] As a preferred technical proposal, the time t of the primary crystallization is 10 to 300 minutes (e.g., 25 minutes, 40 minutes, 55 minutes, 70 minutes, 95 minutes, 110 minutes, 135 minutes, 155 minutes, 195 minutes, 210 minutes, 240 minutes, 270 minutes, 290 minutes, etc.), preferably 50 to 200 minutes, more preferably 80 to 150 minutes, and even more preferably 90 to 120 minutes. The glass density after the primary crystallization is 2.447 g / cm 3 ≦y 1 ≦2.455g / cm 3 and preferably 2.455 g / cm 3 ≦y 1 ≦2.460g / cm 3 , more preferably 2.460 g / cm 3 ≦y 1 ≦2.481g / cm 3 , and more preferably 2.481 g / cm 3 ≦y 1 ≦2.490g / cm 3 Meet the following.
[0010] The density of the glass after the first crystallization is 2.440 g / cm 3 ≦y 1 ≦2.455g / cm 3If the above condition is satisfied, the effect of controlling the deformation rate of the secondary crystallized glass to 1.2% to 1.8% can be further obtained. The density of the glass after the primary crystallization is 2.455 g / cm 3 ≦y 1 ≦2.460g / cm 3 If the above condition is satisfied, the effect of controlling the deformation rate of the secondary crystallized glass to 1.0% to 1.2% can be further obtained. The density of the glass after the primary crystallization is 2.460 g / cm 3 ≦y 1 ≦2.481g / cm 3 If the above condition is satisfied, the effect of controlling the deformation rate of the secondary crystallized glass to 0% to 1.0% can be further obtained. The density of the glass after the primary crystallization is 2.481 g / cm 3 ≦y 1 ≦2.490g / cm 3 If the above condition is satisfied, it is possible to obtain an additional effect of controlling the deformation rate of the secondary glass-ceramics to 0.0% to 0.5%.
[0011] As a preferred technical proposal, the nucleation temperature is 520 to 580°C (e.g., 525°C, 530°C, 535°C, 540°C, 545°C, 550°C, 560°C, 565°C, 570°C, 575°C, etc.), preferably 545 to 575°C, more preferably 550 to 570°C. The nucleation time is preferably 180 to 360 minutes (e.g., 190 minutes, 195 minutes, 205 minutes, 225 minutes, 240 minutes, 245 minutes, 260 minutes, 280 minutes, 300 minutes, 310 minutes, 320 minutes, 330 minutes, etc.), more preferably 200 to 280 minutes, and even more preferably 220 to 250 minutes.
[0012] A suitable nucleation temperature can achieve uniform nucleation.
[0013] As a preferred technical solution, the process of secondary crystallization includes a temperature increasing stage, a thermoforming stage and a temperature decreasing stage in sequence.
[0014] The secondary crystallization process is carried out in stages, allowing precise control over the temperature at each stage, reducing or eliminating the impact of processing equipment instability on material performance, further improving the consistency of the processed finished product, and increasing product yield.
[0015] As a preferred technical solution, the temperature increasing step is performed by increasing the temperature from room temperature to 10 to 60 °C / min The temperature is increased to the first target temperature at a rate of 20 to 50. °C / min , more preferably 30 to 40 °C / min The first target temperature is 650 to 750°C, preferably 670 to 730°C, and more preferably 680 to 710°C.
[0016] In a preferred technical solution, the thermoforming step is performed by increasing the temperature from a first target temperature to a second target temperature at a temperature increase rate of 15-50° C. / min, preferably 20-40° C. / min, more preferably 30-40° C. / min.
[0017] The second target temperature is 680 to 800°C, preferably 700 to 780°C, more preferably 720 to 750°C, and further preferably 730 to 740°C.
[0018] As a preferred technical solution, the temperature lowering step is performed by lowering the temperature by 30 to 50 degrees from the second target temperature. °C / min The temperature is lowered to room temperature at a rate of preferably 35 to 45 °C / min , more preferably 38 to 40 °C / min It is.
[0019] A proper temperature change curve can reduce the impact of processing equipment on glass. On the one hand, it can prevent glass cracking caused by rapid cooling and heating, and on the other hand, it can prevent the increase in work time and the decrease in production efficiency caused by too slow heating and cooling. In addition, controlling the temperature change curve can also improve the optical properties of glass.
[0020] In a preferred technical solution, the glass sheet is a lithium aluminosilicate glass.
[0021] Preferably, the glass sheet contains 3 to 7 mol% Al. 2 O 3 , 0.5 to 5 mol% ZrO 2 , 10~25mol% Li 2 O, 0.5-5 mol% Na 2 O, 0.5-2mol% P 2 O 5 , 0.1 to 2 mol% B 2 O 3 , 65-72mol% SiO 2 Contains:
[0022] The preferred technical solution is Al in the glass sheet. 2 O 3 The content is 4 to 6 mol %, and preferably 4.5 to 5.5 mol %.
[0023] The preferred technical solution is ZrO 2 The content is 1 to 4 mol %, and preferably 2.5 to 3.5 mol %.
[0024] The preferred technical solution is Li of glass sheet. 2 The O content is 14 to 20 mol %, preferably 16 to 19 mol %, and more preferably 17 to 18 mol %.
[0025] As a preferred technical solution, the Na 2 The O content is 0.7 to 3.2 mol %, and preferably 1.0 to 2.5 mol %.
[0026] The preferred technical solution is the P 2 O 5 The content is 0.8 to 1.5 mol %, and preferably 1 to 1.3 mol %.
[0027] As a preferred technical solution, glass sheet B 2 O 3 The content is 0.5 to 1.5 mol %, and preferably 0.8 to 1.2 mol %.
[0028] As a preferred technical solution, the SiO 2 The content is 67 to 71 mol %, preferably 68 to 70 mol %.
[0029] A second object of the present disclosure is to provide a crystallized glass prepared by the method described in the first object.
[0030] The present disclosure relates to a cover for a mobile phone, a watch, a tablet, or an in-vehicle display. one The third object of the present invention is to provide a use of the crystallized glass prepared by the method described in the above.
[0031] Compared with the prior art, the present disclosure has at least the following beneficial effects: The present disclosure provides a method for controlling the density y of a glass sheet after primary crystallization by controlling the temperature and time of primary crystallization for the glass sheet that requires secondary crystallization. 1 is 2.440g / cm 3 ≦y 1 ≦2.490g / cm 3 and approach the density after secondary crystallization. This reduces the amount of deformation during secondary crystallization, and the resulting glass has excellent light transmittance and improves product yield. [Brief description of the drawings]
[0032]
Figure 1
[0033] The technical solution according to the present disclosure will be further described below with reference to specific embodiments. As will be appreciated by those skilled in the art, the examples are merely for the purpose of providing a better understanding of the present disclosure and are not intended to limit the present disclosure.
[0034] Example 1 The crystallized glass is prepared by the following method. Step (1): 5mol% Al 2 O 3 , 2.7mol% ZrO 2 , 14.9mol% Li 2 O, 2.1 mol% Na 2 O, 1.6 mol% P 2 O 5 , 0.75 mol% B 2 O 3 , the remainder being SiO 2 Based on a glass recipe containing the above, glass raw materials were weighed and mixed to obtain a raw material mixture.
[0035] Step (2): The raw material mixture was molded and cooled to obtain a glass sheet. The molding method was to melt the mixture at 1650°C for 5 hours, then pour it into a mold preheated to 200°C and mold it. The cooling method was to anneal the mixture at 580°C for 24 hours, and then cool the annealing furnace to room temperature. The size of the glass sheet produced was 159 x 74 x 0.60 mm.
[0036] Step (3): The glass sheet was subjected to nucleation at 555° C. for 280 minutes and primary crystallization at 645° C. for 100 minutes.
[0037] Step (4): The glass sheet after the primary crystallization was subjected to secondary crystallization to obtain a crystallized glass. The secondary crystallization was performed at room temperature for 20 °C / min The temperature was raised to 700°C at a rate of 25°C. °C / min The temperature was raised to 800°C at a rate of 20°C. °C / min The temperature was lowered to room temperature at a rate of 0.15.
[0038] Example 2 The difference from Example 1 is that the primary crystallization temperature in step (3) is 640° C. and the primary crystallization time is 100 minutes.
[0039] Example 3 The difference from Example 1 is that the primary crystallization temperature in step (3) is 635° C., and the primary crystallization time is 100 minutes.
[0040] Example 4 The difference from Example 1 is that the primary crystallization temperature in step (3) is 650° C. and the primary crystallization time is 100 minutes.
[0041] Example 5 The difference from Example 1 is that the primary crystallization temperature in step (3) is 637° C., and the primary crystallization time is 90 minutes.
[0042] Example 6 The difference from Example 1 is that the primary crystallization temperature in step (3) is 642° C., and the primary crystallization time is 90 minutes.
[0043] Example 7 The difference from Example 1 is that the primary crystallization temperature in step (3) is 647° C., and the primary crystallization time is 90 minutes.
[0044] Example 8 The difference from Example 1 is that the primary crystallization temperature in step (3) is 652° C., and the primary crystallization time is 90 minutes.
[0045] Example 9 The difference from Example 1 is that the primary crystallization temperature in step (3) is 635° C., and the primary crystallization time is 120 minutes.
[0046] Example 10 The difference from Example 1 is that the primary crystallization temperature in step (3) is 640° C., and the primary crystallization time is 120 minutes.
[0047] Example 11 The difference from Example 1 is that the primary crystallization temperature in step (3) is 655° C. and the primary crystallization time is 100 minutes.
[0048] Example 12 The difference from Example 1 is that the primary crystallization temperature in step (3) is 636° C. and the primary crystallization time is 300 minutes.
[0049] Example 13 The difference from Example 1 is that the primary crystallization temperature in step (3) is 650° C., and the primary crystallization time is 10 minutes.
[0050] Example 14 The difference from Example 1 is that the glass recipe in step (1) contains 7.0 mol% Al 2 O 3 , 0.5mol% ZrO 2 , 25.0mol% Li 2 O, 0.5 mol% Na 2 O, 2.0 mol% P 2 O 5 , 2.0 mol% B 2 O 3 , the remainder being SiO 2 It will contain:
[0051] Example 15 The difference from Example 1 is that the glass recipe in step (1) contains 3.0 mol% Al 2 O 3 , 5.0mol% ZrO 2 , 10mol% Li 2 O, 5.0 mol% Na 2 O, 0.5mol% P 2 O 5 , 0.1 mol% B 2 O 3 , the remainder being SiO 2 It will contain:
[0052] Example 16 The difference from Example 1 is that the nucleation temperature in step (3) is 520° C. and the nucleation time is 360 minutes.
[0053] In step (4), the temperature is increased from room temperature to 10 °C / min The temperature was raised to 650°C at a rate of 15°C. °C / min The temperature was increased to 680°C at a rate of 10 °C / min The temperature is then lowered to room temperature at a rate of .
[0054] Example 17 The difference from Example 1 is that the nucleation temperature in step (3) is 580° C. and the nucleation time is 180 minutes.
[0055] In step (4), the temperature is increased from room temperature to 60 °C / min The temperature was increased to 750°C at a rate of 50°C. °C / min The temperature was raised to 850°C at a rate of 850 ℃ to 50 °C / min The temperature is then lowered to room temperature at a rate of .
[0056] Comparative Example 1 The difference from Example 1 is that the primary crystallization temperature in step (3) is 630° C., and the primary crystallization time is 150 minutes.
[0057] Comparative Example 2 The difference from Example 1 is that the primary crystallization temperature in step (3) is 675° C. and the primary crystallization time is 100 minutes.
[0058] Comparative Example 3 The difference from Example 1 is that the primary crystallization temperature in step (3) is 635° C., and the primary crystallization time is 50 minutes.
[0059] Performance test: (1) Density measurement: The measurement method is to immerse the glass sheet to be measured in a mixed solution of ethanol:pure water = 1:1 for 30 minutes, then clean it with an ultrasonic cleaner (XDQ 5090ST, Dongguan Xingdaqiang Ultrasonic Equipment Co., Ltd.) for 10 minutes, wipe off the liquid on the surface with a dust-free cloth, and measure the density with a density meter (ELECTRONIC DEN DENSIMEETER SD-200L, Japan). The density after primary crystallization and the density after secondary crystallization are measured.
[0060] (2) Size change: The test method is to measure the two-dimensional size of the glass after secondary crystallization using a two-dimensional image measuring device (MY-YXCL-4030 (±0.01 mm)). Specifically, the test method is to measure three sets of data at 1 / 4, 1 / 2, and 3 / 4 positions on the long side (a schematic diagram of the measurement positions is shown in Figure 1). Thirty data points are obtained from 10 test sheets, and the maximum value (L max , mm) and minimum value (L min , mm), and calculate the difference between the maximum and minimum values to determine the size change y 2 (mm), The deformation ratio is calculated using JPEG0007573119000001.jpg1239. The deformation ratio represents the concentration of size change after secondary crystallization of the glass of the lot. A larger deformation ratio means a larger size change, and a smaller deformation ratio means a smaller size change.
[0061] (3) Light transmittance: As a test method, the crystallized glass sheet is washed in an ultrasonic cleaner under the following conditions: washing time: 5-10 minutes, cleaning agent used: 10 times diluted general detergent, washing temperature: 45℃-65℃, washing frequency: 20KHZ-40KHZ, and the light transmittance of the crystallized glass by wavelength is measured using a haze meter in accordance with "GB / T7962.12-2010 Test method for colorless optical glass Part 12: Spectral transmittance". The haze meter used in this disclosure is a spectrophotometer CM-3600A manufactured by Konica Minolta Japan.
[0062] Table 1 shows the relevant parameters and test results of the primary crystallization. [Table 1] JPEG0007573119000003.jpg144166
[0063] Table 1 reveals the following: The temperature x of the primary crystallization carried out in Examples 1 to 17 1 and time t both satisfy the following conditions:
[0064] Condition (i): -a×t + 652 ≤ x 1 ≤ -a×t + 667. However, a is a constant and 0.1 ≤ a ≤ 0.25, t is between 10 and 300 minutes, and the crystallization temperature x 1 is in the unit of °C.
[0065] Condition (ii): y 1 = 0.0029x 1 + b. However, y 1 is the glass density after primary crystallization and 2.440 g / cm 3 ≤ y 1 ≤ 2.490 g / cm 3 holds. b is a constant and 0.55 < b < 0.60. The deformation rate of the produced crystallized glass is less than 1.5% in all cases, and the light transmittance is 89% or more. Also, within the limited range of the glass density after primary crystallization, as the density increases, the deformation rate of the glass after secondary crystallization gradually decreases, and the corresponding light transmittance increases.
[0066] In Comparative Example 1, the temperature and time of primary crystallization satisfy Condition (i), but the temperature and density after primary crystallization do not satisfy Condition (ii). It can be seen that the deformation rate of the glass after secondary crystallization becomes as large as 1. 8 8% and the light transmittance is poor.
[0067] In Comparative Example 2, the temperature and time of primary crystallization do not satisfy Conditions (i) and (ii), and the density after primary crystallization exceeds 2.490 g / cm 3 . Although a relatively small deformation rate can be obtained, it can be seen that the light transmittance becomes poor.
[0068] In Comparative Example 3, the temperature and time of primary crystallization do not satisfy Conditions (i) and (ii). It can be seen that the deformation rate of the glass after secondary crystallization becomes as large as 1.53% and the light transmittance is poor.
[0069] The above-described embodiments are only some of the embodiments of the present disclosure, and are not all of the embodiments. The detailed description of the embodiments of the present disclosure merely shows selected embodiments of the present disclosure, and does not limit the scope of the present disclosure to be protected. All other embodiments that a person skilled in the art can obtain based on the embodiments of the present disclosure without using his / her inventive ability are all within the scope of protection of the present disclosure.
Claims
1. A method for preparing crystallized glass, comprising the steps of: Step (1): Nucleation is performed on a glass sheet, and then primary crystallization is performed, where the temperature of the primary crystallization is x 1 When the time of the primary crystallization is t, the temperature of the primary crystallization x 1 and the time t of the primary crystallization satisfy the following conditions (i) and (ii), (i)-a×t+652≦x 1 ≦-a×t+667 where a is a constant and 0.1≦a≦0.25, t is 10 to 300 minutes, and the primary crystallization temperature x 1 The unit is °C, (ii)y 1 =0.0029x 1 +b Here, y 1 is the glass density after the primary crystallization, and 2.440 g / cm 3 ≦y 1 ≦2.490g / cm 3 where b is a constant and 0.55<b<0.60; and Step (2): performing secondary crystallization on the glass sheet after the primary crystallization; The glass sheet is a lithium aluminosilicate glass, The glass sheet contains 3-7 mol % Al 2 O 3 , 0.5-5 mol % ZrO 2 , 10-25 mol % Li 2 O, 0.5-5 mol % Na 2 O, 0.5-2 mol % P 2 O 5 , 0.1-2 mol % B 2 O 3 , and 65-72 mol % SiO 2 . A method for preparing crystallized glass.
2. The density of the glass after the primary crystallization is 2.447 g / cm 3 ≦y 1 ≦2.490g / cm 3 and preferably 2.455 g / cm 3 ≦y1≦2.490g / cm 3 , more preferably 2.460 g / cm 3 ≦y1≦2.490g / cm 3 , more preferably 2.481 g / cm 3 ≦y1≦2.490g / cm 3 is 2. The method according to claim 1 .
3. The nucleation temperature is 520 to 580° C., preferably 545 to 575° C., more preferably 550 to 570° C., and the nucleation time is 180 to 360 minutes, preferably 200 to 280 minutes, more preferably 220 to 250 minutes.
2. The method according to claim 1 .
4. The secondary crystallization process includes a temperature increase stage, a thermoforming stage, and a temperature decrease stage in this order.
2. The method according to claim 1 .
5. In the temperature increasing step, the temperature is increased from room temperature to a first target temperature at a rate of 10 to 60° C. / min; Here, the first target temperature is 650 to 750° C.
5. The method according to claim 4 .
6. In the thermoforming step, the temperature is increased from a first target temperature to a second target temperature, where the temperature increase rate is 15-50° C. / min, and the second target temperature is 680-850° C.
5. The method according to claim 4 .
7. In the temperature decreasing step, the temperature is decreased from the second target temperature to room temperature at a rate of 10 to 50° C. / min.
5. The method according to claim 4 .
8. Used for mobile phone covers, watch covers, tablet covers, and car display covers Use of glass-ceramics prepared by the method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Locally reinforced glass product and processing method thereof
CN111253087A
Black lithium silicate glass ceramic
JP2021505503A
Crystallized glass of three-dimensional shape, chemically strengthened glass of three-dimensional shape, and method for producing crystallized glass of three-dimensional shape and chemically strengthened glass of three-dimensional shape
WO2019167850A1