Method for preparing quartz glass plane TEM sample by adopting FIB

By using U-shaped cutting inclination angle and reverse cutting technology in the process of preparing quartz glass flat TEM samples in FIB, the problems of high energy and spot control in traditional methods are solved, and efficient and accurate sample preparation is achieved, and the quality of the sample is improved. stability.

CN119064103AActive Publication Date: 2024-12-03HUBEI SINOPHORUS ELECTRONIC MATERIALS CO LTD

Patent Information

Application Number
CN202411202740.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

When traditional FIB prepares quartz glass flat TEM samples, it is difficult to control due to high energy and beam spot size, resulting in large damage to the sample, low preparation accuracy, and difficult to completely repair the problem of uneven thickness after treatment, which affects sample quality and performance.

Method used

After FIB etching, the ion beam cutting angle and strength are gradually adjusted through U-shaped cutting tilt angle and reverse cutting technology, combined with nano robot and gas injection system, fine grinding and purge processing is formed to form a high-quality quartz glass flat TEM sample.

Benefits of technology

It improves the preparation efficiency and quality of the sample, reduces the degree of damage, ensures thickness uniformity and imaging quality, and reduces the damage caused by imaging errors and electron beam irradiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064103A_ABST
    Figure CN119064103A_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a quartz glass plane TEM sample by adopting FIB, and belongs to the technical field of semiconductor manufacturing. The method comprises the following steps: S1, sample pretreatment; s2, FIB etching is carried out; s3, wedge-shaped correction: gradually adjusting the cutting angle and strength of the ion beam through a U-shaped cutting tilt angle method, reducing the wedge-shaped degree of the wedge-shaped sample sheet in the step S2, and preparing a sample sheet with an initial observation area; s4, fine grinding: introducing a back-cutting technology, and separating an observation area from the sample sheet by controlling a nano manipulator and a tungsten welding technology to form an independent TEM sample; and S5, carrying out sample post-treatment. By optimizing ion beam parameters and processing steps and introducing an improved back-cutting technical means, the problems of thick amorphous layer, large damage and low efficiency during sample preparation in the prior art are solved, and the preparation efficiency and quality of the TEM sample are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of semiconductor manufacturing, and in particular to a method for preparing a quartz glass plane TEM sample by adopting FIB. Background Art

[0002] As a common optical and electronic material, quartz glass faces many difficulties in preparing transmission electron microscope (TEM) samples due to its high hardness and low conductivity. Although traditional mechanical grinding and ion thinning methods can prepare samples that meet the requirements to a certain extent, they have problems such as long preparation cycle, complex operation, and large sample damage. Especially when preparing planar samples, due to the hardness and brittleness of the material, it is easy to produce defects such as cracks and fractures during the preparation process, which seriously affects the quality and observability of the samples.

[0003] As an emerging micro-nano processing technology, focused ion beam technology (FIB) has the advantages of high precision, high efficiency, and non-contact processing, providing new possibilities for the preparation of high-quality quartz glass planar TEM samples.

[0004] In the existing quartz glass plane TEM sample preparation technology, FIB is widely used due to its advantages of high precision and non-contact processing, such as the invention patent with application number 201910003403.4. The steps of preparing TEM samples using FIB include sample pretreatment, FIB etching, sample post-processing and other links.

[0005] The pretreatment stage mainly involves the fixation of the sample and the enhancement of its conductivity, such as using conductive glue to fix the sample on the sample stage and performing gold spraying to improve the conductivity of the sample.

[0006] In the FIB etching stage, the traditional approach is to directly use a focused ion beam to etch the sample to remove unwanted parts and form the desired observation area. However, due to the high hardness and low conductivity of quartz glass, the traditional FIB etching method often faces problems such as excessive energy leading to large sample damage and difficult control of the beam spot size leading to low preparation accuracy.

[0007] In the sample post-processing stage, the prepared TEM samples are usually cleaned and purged to remove residual FIB etching products and impurities. However, since samples prepared by traditional methods may have problems such as damage and uneven thickness, the post-processing process is often difficult to completely repair these problems, affecting the quality and performance of the final sample.

[0008] At present, the traditional FIB preparation method still has some problems, such as high ion beam energy resulting in severe sample damage, and the difficulty in controlling the ion beam spot size resulting in low sample preparation accuracy. Therefore, it is necessary to improve and optimize the traditional FIB preparation method to meet the needs of TEM sample preparation for difficult-to-process materials such as quartz glass. Summary of the invention

[0009] In view of the above problems, the present invention provides a method for preparing a quartz glass plane TEM sample by using FIB.

[0010] The method for preparing a quartz glass plane TEM sample using FIB comprises the following steps: S1. Sample pretreatment: fix the quartz glass sample on the sample stage and perform gold spraying on the quartz glass sample to enhance conductivity; S2, FIB etching: Use FIB technology to etch the quartz glass sample to obtain a wedge-shaped sample slice with an initial observation area; S3, wedge correction: by using the U-shaped cutting tilt angle method, the cutting angle and intensity of the ion beam are gradually adjusted to reduce the wedge degree of the wedge-shaped sample slice in step S2, so as to obtain a sample slice with an initial observation area; S4, fine grinding: introduce the inverted cutting technology, and separate the observation area from the sample slice by manipulating the nanomanipulator and tungsten welding technology to form an independent TEM sample; S5, sample post-processing: the TEM sample prepared in step S4 is purged and cleaned to remove the amorphous layer and the damaged layer on the surface, so as to obtain the quartz glass plane TEM sample.

[0011] The method for preparing a quartz glass plane TEM sample by using FIB provided by the present invention reduces charge accumulation and electron beam damage by enhancing the conductivity of the quartz glass sample in sample pretreatment; for the wedge-shaped sample slice after FIB treatment, a method of reducing the wedge degree by using a U-shaped cutting tilt angle is proposed for the first time, and the parallelism of the sample is further improved by combining the inverted cutting technology, thereby avoiding imaging errors caused by sample unevenness; finally, a purging treatment and a cleaning treatment are performed to ensure the cleanliness of the sample surface and reduce damage caused by electron beam irradiation, thereby improving the final imaging quality.

[0012] Preferably, in step S1, the step of fixing the quartz glass sample on the sample stage specifically includes the following steps: fixing the quartz glass sample on the sample stage with conductive C glue, and bonding the sample to the sample stage with conductive Cu glue. Since the conductivity of quartz glass is poor, the sample is wrapped with conductive Cu glue.

[0013] Preferably, in step S1, the gold spraying treatment specifically comprises the following steps: performing gold spraying treatment on the fixed quartz glass sample, leaving only the target processing area unsprayed with gold, so as to enhance the conductivity.

[0014] Preferably, in step S2, the FIB etching specifically includes the following steps: S201, perform precise tungsten layer deposition, set the electron beam voltage to 2 kV, the current to 6.4 nA, and plate a tungsten layer with a thickness of 0.3 μm on the target processing area of ​​the quartz glass sample as a protective layer; the tungsten layer can protect the sample surface from damage during subsequent ion beam processing and improve processing accuracy; S202, tilt the sample stage to 52°, set the energy of the ion beam to 10-20 keV, and continue ion beam deposition. Through precise ion beam energy control, the damage to the quartz glass sample can be reduced, the cutting accuracy can be ensured, and the microstructure integrity of the sample can be maintained; S203, setting the voltage and current of the ion beam to a low beam current of 30 kV and 2.5 nA respectively, and processing deep pits in the vertical direction in the adjacent areas on the upper and lower sides of the tungsten layer; S204, performing Cross-Sectional Shaping (CCS) refinement on the upper edge and the lower edge of the tungsten layer when the sample stage tilt angle is 50° and 54°, respectively, to obtain a wedge-shaped sample slice with an initial observation area.

[0015] Preferably, in step S3, the U-shaped cutting tilt angle method specifically includes the following steps: when the sample stage returns to the 0° position, the wedge-shaped sample slice is cut into a cantilever beam shape; then, the tilt angle of the sample stage is adjusted from 0° to -10°, and the wedge-shaped sample slice is continued to be thinned to obtain a sample slice with an initial observation area.

[0016] The U-shaped cutting tilt angle method can effectively reduce the thickness of the other side of the wedge-shaped sample slice after processing by precisely controlling the angle of the sample stage and the parameters of the ion beam, precisely controlling the cutting and thinning process of the wedge-shaped sample slice, effectively reducing the wedge degree of the wedge-shaped sample slice, and obtaining a thinner and more uniform sample slice.

[0017] Preferably, in step S3, during the thinning process, the tilt angle is set to ±1.5°, the thinning voltage is maintained at 25-30 kV, and the sample is finely polished by using a method of gradually reducing the ion beam current.

[0018] Through precise control of the tilt angle and ion beam current, high-precision thinning of wedge-shaped sample slices is achieved, which not only improves processing accuracy and preparation efficiency, but also optimizes sample morphology and reduces sample damage. By setting the tilt angle, the interaction between the ion beam and the sample surface is precisely controlled, thereby achieving a more uniform and fine polishing effect.

[0019] Further preferably, when the thickness of the wedge-shaped sample slice is greater than 200 nm, the ion beam current is 0.23 nA; when the thickness of the wedge-shaped sample slice is 100-200 nm, the ion beam current is 80 pA; when the thickness of the wedge-shaped sample slice is 80-100 nm, the ion beam current is 40 pA.

[0020] The method of gradually reducing the ion beam current for different thicknesses avoids excessive processing when the sample is close to the target thickness, reduces ion beam damage on the sample surface, maintains the microstructural integrity of the sample, and can complete the thinning process more effectively and efficiently.

[0021] Preferably, in step S3, the thickness of the prepared sample slice is 80-100 nm, which is suitable for TEM observation, and can ensure the penetration of the electron beam and meet the requirements of high-resolution imaging.

[0022] In order to further improve the quality of the sample and the observation effect, the sample was finely polished by gradually reducing the ion beam voltage, which specifically included the following steps: when the wedge-shaped sample slice was less than 100 nm, it was first thinned under the conditions of 5 kV and 15 pA, and then continued to be thinned under the conditions of 2 kV and 9 pA until the tungsten layer gradually became thinner and had good light transmittance under the conditions of 3 kV, ensuring that the impurities in the amorphous layer had been removed and the sample was finely polished.

[0023] Preferably, in step S3, an in-situ nanomanipulator and a gas injection system (GIS) are simultaneously combined to precisely control the cutting and thinning process of the sample.

[0024] Preferably, in step S4, the inverted cutting technology specifically includes the following steps: after completing the wedge correction in step S3, adjust the relative position of the nanomanipulator and the sample slice, rotate the nanomanipulator 180°, cut off the wedge-shaped part of the sample slice with an ion beam, adjust the sample slice and the copper column to the same plane, use tungsten material to weld them, and then cut off the cantilever arm to obtain a TEM sample.

[0025] Preferably, in step S5, the purging and cleaning treatment specifically includes the following steps: tilting the sample stage to ±3°, setting the ion beam voltage to 5 kV and the current to 15 pA, purging the front and rear surfaces of the TEM sample obtained in step S4 for 30 s each, and repeating the purging 2 to 3 times; then continuing to tilt the sample stage to ±5°, setting the ion beam voltage to 2 kV and the current to 9 pA, and purging the front and rear surfaces of the TEM sample for 10 to 60 s each.

[0026] Compared with the prior art, the beneficial effects of the present invention are: 1. The method for preparing a quartz glass plane TEM sample using FIB provided by the present invention improves the sample preparation efficiency. The present invention adopts an improved undercutting technology, which can quickly and accurately prepare a high-quality quartz glass plane TEM sample and reduce the preparation time. 2. The method for preparing a quartz glass plane TEM sample using FIB provided by the present invention reduces the degree of damage to the sample. The present invention reduces the damage to the sample and improves the quality and stability of the sample by optimizing the parameters of the FIB and the etching process. 3. The method for preparing a quartz glass plane TEM sample using FIB provided by the present invention improves the thickness uniformity of the sample. The present invention adopts an improved undercutting technology to achieve precise control of the sample thickness, thus avoiding the problem of uneven sample thickness in the traditional method. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a planar TEM sample image of the quartz glass prepared in Example 1. DETAILED DESCRIPTION

[0028] The technical scheme of the present invention is further described below by way of examples. The raw materials used in the examples can be purchased from the market or prepared by conventional methods.

[0029] Example 1 A method for preparing a quartz glass plane TEM sample using FIB, comprising the following steps: S1. Sample pretreatment: Fix the quartz glass sample on the sample stage with conductive C glue, and use conductive Cu glue to adhere the sample to the sample stage. Since the conductivity of quartz glass is poor, wrap the sample with conductive Cu glue; then use an ion sputtering device to spray gold on the fixed quartz glass sample, leaving only the target processing area without gold spraying to enhance conductivity.

[0030] S2, FIB etching: In the FIB equipment, the quartz glass sample is initially cut by precisely controlling the focused ion beam, which specifically includes the following steps: S201, performing precise tungsten layer deposition, setting the voltage of the electron beam to 2 kV and the current to 6.4 nA, and coating a tungsten layer with a thickness of 0.3 μm on the target processing area of ​​the quartz glass sample as a protective layer; S202, tilting the sample stage to 52°, setting the energy of the gallium ion source ion beam to 10-20 keV, and continuing ion beam deposition to reduce damage to the quartz glass sample and ensure cutting accuracy; S203, setting the voltage and current of the ion beam to a low beam current of 30 kV and 2.5 nA respectively, and processing deep pits in the vertical direction in the adjacent areas on the upper and lower sides of the tungsten layer; S204, performing Cross-Sectional Shaping (CCS) refinement on the upper edge and the lower edge of the tungsten layer when the sample stage tilt angle is 50° and 54°, respectively, to obtain a wedge-shaped sample slice with an initial observation area.

[0031] S3, wedge correction: Due to the hard and brittle characteristics of quartz glass, a wedge-shaped sample is formed after the initial cutting. In order to reduce the wedge degree of the wedge-shaped sample slice in step S2, the cutting and thinning process of the sample is precisely controlled by combining the in-situ nanomanipulator and the gas injection system (GIS), which specifically includes the following steps: When the sample stage returns to the position of 0°, the wedge-shaped sample slice is cut into a cantilever beam shape; then, the tilt angle of the sample stage is adjusted from 0° to -10°, and the wedge-shaped sample slice is continued to be thinned. During the thinning process, the tilt angle is set to ±1.5°, and the thinning voltage is maintained at 30 kV. The sample is finely polished by gradually reducing the ion beam current, that is, when the thickness of the wedge-shaped sample slice is greater than 200 nm, the ion beam current is 0.23 nA; when the thickness of the wedge-shaped sample slice is 100-200 nm, the ion beam current is 80 pA; when the thickness of the wedge-shaped sample slice is 80-100 nm, the ion beam current is 40 pA; a sample slice with a thickness of 80-100 nm and an initial observation area is obtained; In order to further improve the quality of the sample and the observation effect, the sample was finely polished by gradually reducing the ion beam voltage, which specifically included the following steps: when the wedge-shaped sample slice was less than 100 nm, it was first thinned under the conditions of 5 kV and 15 pA, and then continued to be thinned under the conditions of 2 kV and 9 pA until the tungsten layer gradually became thinner and had good light transmittance under the conditions of 3 kV, ensuring that the impurities in the amorphous layer had been removed and the sample was finely polished.

[0032] S4. Fine polishing: Introduce the reverse cutting technology, and separate the observation area from the sample slice by manipulating the nanomanipulator and tungsten welding technology. Specifically, the following steps are included: After completing the wedge correction in step S3, adjust the relative position of the nanomanipulator and the sample slice, rotate the nanomanipulator 180°, cut off the wedge-shaped part of the sample slice with an ion beam, adjust the sample slice and the copper column to the same plane, use tungsten material for welding, and then cut off the cantilever arm to obtain a TEM sample.

[0033] S5, sample post-processing: the TEM sample prepared in step S4 is purged and cleaned to remove the amorphous layer and the damaged layer on the surface, specifically comprising the following steps: the sample stage is tilted to ±3°, the ion beam voltage is set to 5 kV, the current is 15 pA, the front and rear surfaces of the TEM sample prepared in step S4 are purged for 30 s respectively, and the purging is repeated 2 to 3 times; then the sample stage is further tilted to ±5°, the ion beam voltage is set to 2 kV, the current is 9 pA, the front and rear surfaces of the TEM sample are purged for 60 s respectively, and the process can be stopped at any time according to the actual situation of the sample to retain the original structure and characteristics of the sample, and the quartz glass plane TEM sample is obtained.

[0034] The prepared quartz glass plane TEM sample was tested. Figure 1 As shown, through TEM observation, the prepared quartz glass plane TEM sample meets the observation requirements. If necessary, steps S3 to S5 can be repeated to improve the observation effect.

[0035] It should be understood that the above embodiments are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of the present application.

Claims

1. A method for preparing a quartz glass plane TEM sample using FIB, characterized in that: The following steps are involved: S1. Sample pretreatment: fix the quartz glass sample on the sample stage and perform gold spraying on the quartz glass sample; S2, FIB etching: Use FIB technology to etch the quartz glass sample to obtain a wedge-shaped sample slice with an initial observation area; S3, wedge correction: by using the U-shaped cutting tilt angle method, the cutting angle and intensity of the ion beam are gradually adjusted to reduce the wedge degree of the wedge-shaped sample slice in step S2, so as to obtain a sample slice with an initial observation area; S4, fine grinding: introduce the inverted cutting technology, and separate the observation area from the sample slice by manipulating the nanomanipulator and tungsten welding technology to form an independent TEM sample; S5, sample post-processing: the TEM sample prepared in step S4 is purged and cleaned to remove the amorphous layer and the damaged layer on the surface, so as to obtain the quartz glass plane TEM sample.

2. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S1, the quartz glass sample is fixed on the sample stage, which specifically includes the following steps: fixing the quartz glass sample on the sample stage with conductive C glue, and bonding the sample to the sample stage with conductive Cu glue. Since the conductivity of quartz glass is poor, the sample is wrapped with conductive Cu glue.

3. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S1, the gold spraying treatment specifically includes the following steps: performing gold spraying treatment on the fixed quartz glass sample, and only retaining the target processing area without being gold sprayed.

4. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S2, the FIB etching specifically includes the following steps: S201, performing precise tungsten layer deposition, setting the voltage of the electron beam to 2 kV and the current to 6.4 nA, and coating a tungsten layer with a thickness of 0.3 μm on the target processing area of ​​the quartz glass sample as a protective layer; S202, tilt the sample stage to 52°, set the energy of the ion beam to 10-20 keV, and continue ion beam deposition to reduce damage to the quartz glass sample and ensure cutting accuracy; S203, setting the voltage and current of the ion beam to a low beam current of 30 kV and 2.5 nA respectively, and processing deep pits in the vertical direction in the adjacent areas on the upper and lower sides of the tungsten layer; S204, when the tilt angle of the sample stage is 50° and 54°, respectively, the upper edge and the lower edge of the tungsten layer are refined by Cross-Sectional Shaping to obtain a wedge-shaped sample slice with an initial observation area.

5. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S3, the U-shaped cutting tilt angle method specifically includes the following steps: when the sample stage returns to the 0° position, the wedge-shaped sample slice is cut into a cantilever beam shape; then, the tilt angle of the sample stage is adjusted from 0° to -10°, and the wedge-shaped sample slice is continued to be thinned to obtain a sample slice with an initial observation area.

6. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S3, during the thinning process, the tilt angle is set to ±1.5°, the thinning voltage is maintained at 25-30 kV, and the sample is finely polished by gradually reducing the ion beam current.

7. The method for preparing a quartz glass planar TEM sample using FIB according to claim 6, characterized in that: When the thickness of the wedge-shaped sample slice is greater than 200 nm, the ion beam current is 0.23 nA; when the thickness of the wedge-shaped sample slice is 100-200 nm, the ion beam current is 80 pA; when the thickness of the wedge-shaped sample slice is 80-100 nm, the ion beam current is 40 pA.

8. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S3, the sample is finely polished by gradually reducing the ion beam voltage, which specifically includes the following steps: when the wedge-shaped sample slice is less than 100 nm, it is first thinned under the conditions of 5 kV and 15 pA, and then thinned again under the conditions of 2 kV and 9 pA until the tungsten layer gradually becomes thinner and has good light transmittance under the condition of 3 kV, ensuring that the impurities in the amorphous layer have been removed and the sample is finely polished.

9. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S4, the inverted cutting technology specifically includes the following steps: after completing the wedge correction in step S3, adjust the relative position of the nanomanipulator and the sample slice, rotate the nanomanipulator 180°, cut off the wedge-shaped part of the sample slice with an ion beam, adjust the sample slice and the copper column to the same plane, weld them with tungsten material, and then cut off the cantilever arm to obtain a TEM sample.

10. The method for preparing a quartz glass planar TEM sample using FIB according to claim 1, characterized in that: In step S5, the purging and cleaning treatment specifically includes the following steps: tilting the sample stage to ±3°, setting the ion beam voltage to 2~5 kV, the current to 9~15 pA, purging the front and rear surfaces of the TEM sample obtained in step S4 for 10~30 s respectively, and repeating the purging 2~3 times; then continue to tilt the sample stage to ±5°, set the ion beam voltage to 2 kV, the current to 9 pA, and purge the front and rear surfaces of the TEM sample for 30~60 s respectively.

Citation Information

Patent Citations

  • Method for preparing triethylenemelamine (TEM) sample

    CN103308365A

  • Device and method for preparing gradient nanostructure material transmission electron microscope sample

    CN114062081A

  • Sample rotating system and method

    CN115602514A

  • Preparation of FIB-TEM sample using SOG inSemiconductor wafer

    KR1020030041602A

  • Method for producing TEM specimen

    KR1020140077350A

Cited By

  • Method for preparing TEM pore sample by using focused ion beam

    CN119666504A

  • A method for preparing TEM pore samples using focused ion beam

    CN119666504B

  • TEM sample preparation method

    CN121298381A