Metal coloring solution for chemical conversion treatment and metal coloring treatment method
A metal coloring liquid using permanganic acid and phosphates directly colors metal surfaces in yellow to brown tones, addressing inefficiencies in conventional methods by eliminating oxide film formation and enhancing processing efficiency.
Patent Information
- Application Number
- JP2020116562
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-06
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-07-06
AI Technical Summary
Conventional methods for coloring metal surfaces in yellow to brown tones require multiple processing steps and the formation of an oxide film, leading to inefficiencies.
A metal coloring liquid containing permanganic acid or its salt, inorganic acids or their salts, and condensed phosphates is used to directly color metal surfaces in yellow to brown tones through chemical conversion treatment, eliminating the need for oxide film formation and electrolysis.
The method achieves efficient coloring of metal surfaces in yellow to brown tones with improved adhesion and processing efficiency, without the need for additional film formation steps.
Smart Images

Figure 0007573232000001 
Figure 0007573232000002 
Figure 0007573232000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal coloring solution for chemical conversion treatment and a metal coloring treatment method. [Background technology]
[0002] 2. Description of the Related Art Conventionally, in coloring various metals, particularly aluminum or aluminum alloys, a method for obtaining a yellow to brown color tone has generally been by anodization or by adsorbing a dye onto an anodized film.
[0003] For example, Patent Document 1 discloses a method for electrolytic coloring of aluminum and aluminum alloys, which is characterized in that a colored film formed on the surface of aluminum or aluminum alloy substrate by electrolytic coloring or natural coloring is made into a film structure capable of electrolytic coloring, and then electrolytic coloring is performed to obtain a film of a new color tone by superimposing colors. It is described that such a configuration can provide an electrolytic coloring method capable of obtaining various colors including various intermediate colors that cannot be obtained by conventional electrolytic coloring methods. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 110895 / 1989 [Patent Document 2] Patent No. 6004217 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the past, in order to color a metal surface in a yellow to brown color tone, for example, in the case of aluminum or an aluminum alloy, it was necessary to use anodizing. That is, in order to color a metal surface in a yellow to brown color tone, it is necessary to use a metal having an oxide film on the surface, which requires many processing steps, and there is a demand for improvement in processing efficiency.
[0006] Furthermore, Patent Document 2 discloses a treatment agent for coloring the surface of aluminum or an aluminum alloy gold, but there is room for further research and development in coloring metal surfaces in yellow to brown tones by chemical conversion treatment.
[0007] In view of such problems, the present invention has an object to provide a metal coloring liquid for chemical conversion treatment and a metal coloring treatment method that are capable of coloring a metal surface in a yellow to brown color tone with good treatment efficiency. [Means for solving the problem]
[0008] As a result of intensive research conducted by the inventors to solve the above-mentioned problems, it has been found that by carrying out treatment with a metal coloring liquid for chemical conversion treatment that contains permanganic acid or a salt thereof, either or both of an inorganic acid and a salt thereof, and a condensed phosphate, it is possible to color a metal surface in a yellow to brown color tone with good treatment efficiency.
[0009] One aspect of the present invention, which was completed based on the above findings, is a metal coloring solution for chemical conversion coating, which contains permanganic acid or a salt thereof, either or both of an inorganic acid and a salt thereof, and a condensed phosphate.
[0010] In one embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the permanganic acid or a salt thereof is permanganic acid, sodium permanganate, potassium permanganate, zinc permanganate, magnesium permanganate, calcium permanganate, ammonium permanganate, or a combination thereof.
[0011] In another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the inorganic acid and the salt thereof are phosphoric acid, sulfuric acid, nitric acid, carbonic acid, hydrochloric acid, and salts thereof, or combinations thereof.
[0012] In yet another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the condensed phosphate is potassium pyrophosphate, sodium tripolyphosphate, or a combination thereof.
[0013] In still another embodiment of the metal coloring solution for chemical conversion treatment of the present invention, the content of the permanganic acid or a salt thereof is 0.5 to 50 g / L.
[0014] In still another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the content of the inorganic acid and the salt thereof is 0.5 to 100 g / L.
[0015] In still another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the content of the condensed phosphate is 1 to 150 g / L.
[0016] In yet another embodiment, the metal coloring liquid for chemical conversion treatment of the present invention further contains an oxoacid or a salt thereof.
[0017] In still another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the oxoacid or a salt thereof is perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, boric acid, or a salt thereof, or a combination thereof.
[0018] In still another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the total content of the oxoacid or a salt thereof is 0.5 to 100 g / L.
[0019] In yet another embodiment of the metal coloring liquid for chemical conversion treatment of the present invention, the metal to be treated is at least one selected from the group consisting of aluminum, aluminum alloys, copper, copper alloys, iron, iron alloys, zinc, zinc alloys, magnesium, and magnesium alloys.
[0020] In another aspect, the present invention provides a metal coloring treatment method including a step of coloring a metal by chemical conversion treatment using the metal coloring liquid for chemical conversion treatment of the present invention.
[0021] In one embodiment of the metal coloring treatment method of the present invention, in the step of coloring the metal by chemical conversion treatment, the metal is colored by immersing the metal in the metal coloring solution for chemical conversion treatment at 10°C to 80°C for 30 seconds to 20 minutes. Effect of the Invention
[0022] According to the present invention, it is possible to provide a metal coloring solution for chemical conversion treatment and a metal coloring treatment method that are capable of coloring a metal surface in a yellow to brown color tone with good treatment efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, embodiments of the metal coloring liquid for chemical conversion treatment and the metal coloring treatment method of the present invention will be described, but the present invention should not be interpreted as being limited thereto, and various changes, modifications, and improvements can be made based on the knowledge of those skilled in the art without departing from the scope of the present invention.
[0024] [Metal coloring solution for chemical conversion treatment] The metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention contains permanganic acid or a salt thereof, either or both of an inorganic acid and a salt thereof, and a condensed phosphate. By using the metal coloring liquid for chemical conversion treatment containing permanganic acid or a salt thereof, either or both of an inorganic acid and a salt thereof, and a condensed phosphate, a film (colored film) can be formed on the metal surface by simply immersing the metal to be treated in the metal coloring liquid for chemical conversion treatment, and thus the metal surface can be colored in a yellow to brown color tone. Therefore, when coloring the metal surface in a yellow to brown color tone, it is not necessary to form an oxide film on the surface of the metal, and it is not necessary to color the metal surface by electrolysis, and the treatment efficiency is improved. In addition, according to the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention, the adhesion of the film (colored film) formed on the metal surface is also improved.
[0025] (Metal to be treated) The metal to be treated (metal to be treated) whose surface is to be colored with the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention may be at least one selected from the group consisting of aluminum, aluminum alloy, copper, copper alloy, iron, iron alloy, zinc, zinc alloy, magnesium, and magnesium alloy. The metal to be treated may be the metal itself, or may be, for example, a plating of the metal formed on the surface of a metal substrate such as an iron-based material or an iron-based part.
[0026] (Permanganic acid or its salts) As permanganic acid or a salt thereof, permanganic acid, sodium permanganate, potassium permanganate, zinc permanganate, magnesium permanganate, calcium permanganate, ammonium permanganate, or a combination thereof can be used. As permanganic acid or a salt thereof, sodium permanganate and potassium permanganate are more preferable.
[0027] The content of permanganic acid or a salt thereof in the metal coloring solution for chemical conversion treatment according to the embodiment of the present invention depends on the type of metal to be treated and the degree of yellow to brown color to be colored, and can be, for example, 0.5 to 50 g / L. Basically, the lower the content of permanganic acid or a salt thereof, the more the metal surface can be colored in a light yellow to dark yellow color. Also, the higher the content of permanganic acid or a salt thereof, the more the metal surface can be colored in a light brown to dark brown color. The content of permanganic acid or a salt thereof is more preferably 1 to 30 g / L, and more preferably 2 to 20 g / L.
[0028] The metal coloring solution for chemical conversion treatment according to the embodiment of the present invention may contain an oxoacid or a salt thereof, as described below. However, in the case of a metal coloring solution for chemical conversion treatment that does not contain these components, it is possible to color metal surfaces, particularly aluminum and aluminum alloys, in a more aesthetically pleasing yellow to brown color tone.
[0029] (Inorganic acids and their salts) The inorganic acid and its salt are preferably phosphoric acid, sulfuric acid, nitric acid, carbonic acid, hydrochloric acid, and their salts, or combinations thereof. As the salts of phosphoric acid, sulfuric acid, nitric acid, carbonic acid, and hydrochloric acid, metal salts or ammonium salts thereof can be used. As the inorganic acid and its salt, trisodium phosphate, nitric acid, copper nitrate, and zinc chloride are more preferable.
[0030] The content of the inorganic acid and its salt in the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention depends on the type of metal to be treated and the degree of yellow to brown color to be colored, and can be, for example, 0.5 to 100 g / L. Basically, the lower the content of the inorganic acid and its salt, the more the metal surface can be colored in a light yellow to deep yellow color. Also, the higher the content of the inorganic acid and its salt, the more the metal surface can be colored in a light brown to deep brown color. The content of the inorganic acid and its salt is more preferably 1 to 30 g / L, and more preferably 2 to 20 g / L.
[0031] (Condensed phosphate) The condensed phosphate is preferably potassium pyrophosphate, sodium tripolyphosphate, or a combination thereof. The content of the condensed phosphate depends on the type of metal to be treated and the degree of yellow to brown color to be colored, and may be, for example, 1 to 150 g / L. Basically, the lower the content of the condensed phosphate, the more the metal surface can be colored in a light yellow to dark yellow color. Also, the higher the content of the condensed phosphate, the more the metal surface can be colored in a light brown to dark brown color. The content of the condensed phosphate is more preferably 3 to 50 g / L, and more preferably 4 to 40 g / L.
[0032] (Oxoacid or its salt) The metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention may further contain an oxoacid or a salt thereof. Even if the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention contains an oxoacid or a salt thereof, it can color the metal surface to be treated in a yellow to brown color tone with good treatment efficiency. Furthermore, by containing an oxoacid or a salt thereof, the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention can color the surface of metals such as copper, copper alloys, iron, iron alloys, zinc, and zinc alloys in a more aesthetically pleasing yellow to brown color tone.
[0033] The oxoacid or its salt is preferably perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, boric acid, or a salt thereof, or a combination thereof. As the salt of perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, or boric acid, a metal salt or an ammonium salt thereof can be used.
[0034] The total content of oxoacids or salts thereof in the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention can be 0.5 to 100 g / L. Basically, the smaller the total content of oxoacids or salts thereof, the more the metal surface can be colored in a light yellow to deep yellow tone. Also, the larger the total content of oxoacids or salts thereof, the more the metal surface can be colored in a light brown to deep brown tone. The total content of oxoacids or salts thereof is more preferably 1 to 50 g / L, and more preferably 10 to 30 g / L.
[0035] (aqueous medium) The metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention may be a mixture of the above-mentioned various components with an aqueous medium. The aqueous medium refers to a medium mainly composed of water. Examples of the aqueous medium include a medium mainly composed of water and containing an organic solvent such as alcohol miscible with water. The aqueous medium may contain various components that act advantageously to improve some properties of the colored surface of the metal during preparation of the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention, during storage of the metal coloring liquid for chemical conversion treatment, or after coloring the metal surface, or various components that do not substantially inhibit the effects of the present invention, as necessary. For example, pH adjusters, storage stabilizers, etc. are specific examples of such components.
[0036] [Metal coloring treatment method] Next, the metal coloring treatment method according to the embodiment of the present invention will be described in detail. First, a bath containing the metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention is prepared. Next, the metal to be treated is immersed in the metal coloring liquid for chemical conversion treatment while controlling the temperature of the metal coloring liquid for chemical conversion treatment in the bath. After a predetermined time has elapsed, the metal to be treated is pulled out of the bath to obtain a metal whose surface is colored in a yellow to brown color tone. Thus, according to the metal coloring treatment method according to the embodiment of the present invention, the metal to be treated can be colored in a yellow to brown color tone simply by immersing it in the metal coloring liquid for chemical conversion treatment. Therefore, when coloring the metal surface in a yellow to brown color tone, it is not necessary to form an oxide film on the surface of the metal, and it is not necessary to color the metal by electrolysis, and the treatment efficiency is improved.
[0037] Furthermore, in the metal coloring treatment method according to an embodiment of the present invention, in addition to immersing the metal to be treated in the metal coloring liquid for chemical conversion treatment, the surface of the metal to be treated may be colored by contacting the surface of the metal to be treated with the metal coloring liquid for chemical conversion treatment, for example, by a spraying process using the metal coloring liquid for chemical conversion treatment.
[0038] The treatment temperature with the metal colored liquid for chemical conversion treatment is preferably in the range of 10 to 80° C., more preferably in the range of 10 to 60° C., and even more preferably in the range of 30 to 60° C. If the treatment temperature is 10° C. or higher, the reaction rate of the surface treatment increases, and if it is 80° C. or lower, a decrease in the liquid level of the metal colored liquid for chemical conversion treatment due to evaporation can be suppressed.
[0039] The treatment time with the metal coloring liquid for chemical conversion treatment is preferably in the range of 30 seconds to 20 minutes, more preferably in the range of 1 minute to 20 minutes, and even more preferably in the range of 1 minute to 10 minutes. Basically, the shorter the treatment time, the more the metal surface can be colored in a light yellow to dark yellow tone. Also, the longer the treatment time, the more the metal surface can be colored in a light brown to dark brown tone.
[0040] When performing metal surface treatment, it is possible to improve the appearance, corrosion resistance, and reactivity of the metal to be treated with the metal coloring liquid for chemical conversion treatment by first degreasing, activating, and conditioning the surface of the metal to be treated.
[0041] After the metal surface treatment, post-treatment may be performed with a coating agent containing one or more of the group consisting of silicon, resin, and wax. There are no particular limitations on these coating agents as long as they do not affect the desired color tone of the metal surface, and coating agents containing resins such as acrylic resin, olefin resin, alkyd resin, urea resin, epoxy resin, melamine resin, fluororesin, polyethylene, polyvinyl chloride, polystyrene, polypropylene, methacrylic resin, phenolic resin, polyester resin, polyurethane, polyamide, polycarbonate, silicate, colloidal silica, etc. may be used. The resin concentration is preferably 0.01 to 800 g / L, but the appropriate concentration varies depending on the type of resin. Specific examples of coating agents include Cosmo Coat (trade name, Kansai Paint Co., Ltd.), Hi-Seal 272 (trade name, Nippon Hyomen Kagaku Co., Ltd.), Stron JS Coat (trade name, Nippon Hyomen Kagaku Co., Ltd.), Tryner TR-170 (trade name, Nippon Hyomen Kagaku Co., Ltd.), Finigard (trade name, Coventya Co., Ltd.), etc. Specific examples of acrylic resins include Hirotite (trade name, Hitachi Chemical Co., Ltd.) and Aroset (trade name, Nippon Shokubai Co., Ltd.), and examples of olefin resins include Flothane (trade name, Sumitomo Seika Chemicals Co., Ltd.), PES (trade name, Nippon Unicar Co., Ltd.), Chemipearl (trade name, Mitsui Chemicals Inc.), and Sunfine (trade name, Asahi Kasei Corporation).
[0042] The metal coloring liquid for chemical conversion treatment according to the embodiment of the present invention can be used for the purpose of coloring a metal surface in a desired color, imparting a desired aesthetic appearance, imparting distinguishability, etc. Any form of metal to be treated can be used, and is not particularly limited, and examples of such metals include ornaments, fastening members such as buttons and zippers, and in-vehicle parts. In addition, the shape of the metal to be treated is also not limited, and any form can be used. EXAMPLES
[0043] Examples of the present invention are given below, but these are provided for a better understanding of the present invention and are not intended to limit the present invention.
[0044] [Test Example 1: Coloring test of aluminum and aluminum alloys] (Examples 1 to 83, 90, and 91) Test pieces (metal pieces to be treated) were prepared as follows: JIS A5052 (aluminum-magnesium alloy), A2017 (aluminum-copper alloy), and ADC12 (aluminum die-casting). The surfaces of the test pieces were degreased and washed with water, in that order. Next, a bathtub was prepared containing a metal coloring liquid for chemical conversion treatment having the liquid composition shown in Tables 1 to 6 and 8. Pure water was used as the aqueous medium for the metal coloring liquid for chemical conversion treatment. Next, the test pieces were immersed in the metal coloring liquid for chemical conversion treatment in a bath with the temperature controlled to the values shown in Tables 1 to 6 and 8. After immersion for the time shown in Tables 1 to 6 and 8, the test pieces were taken out. Next, the surfaces of the test pieces were washed with water and then dried.
[0045] In addition, for Examples 90 and 91, the test pieces after forming the film (colored film) by immersion were washed with water, coated, and dried. Stron JS Coat (a coating agent manufactured by Nippon Hyomen Kagaku Co., Ltd.) was used for the coating treatment of Example 90, and TR-170 (a coating agent manufactured by Nippon Hyomen Kagaku Co., Ltd.) was used for the coating treatment of Example 91.
[0046] [Test Example 2: Coloring test of copper and copper alloys] (Examples 84 to 85) As test pieces (metal pieces to be treated), JIS C2600P (brass) and C1100P (pure copper) were prepared, and the surfaces of the test pieces were degreased and washed with water in that order. Next, a bathtub was prepared containing a metal coloring liquid for chemical conversion treatment having the liquid composition shown in Table 7. Pure water was used as the aqueous medium for the metal coloring liquid for chemical conversion treatment. Next, the test piece was immersed in the metal coloring liquid for chemical conversion treatment in a bath controlled at the temperature shown in Table 7. After immersion for the time shown in Table 7, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.
[0047] [Test Example 3: Coloring test of zinc and zinc alloys] (Examples 86 to 87) JIS ZDC2 (zinc die-cast) and zinc-plated material were prepared as test pieces (metal pieces to be treated), and the surfaces of the test pieces were degreased and washed with water. The zinc-plated material was a JIS SPCC (rolled steel plate) specified by JIS that was used as a base material and was plated with zincate zinc to a thickness of 8 μm. In addition, 9000ABS manufactured by Nippon Hyomen Kagaku Co., Ltd. was used as a brightener for the zincate zinc plating. Next, a bathtub was prepared containing a metal coloring liquid for chemical conversion treatment having the liquid composition shown in Table 7. Pure water was used as the aqueous medium for the metal coloring liquid for chemical conversion treatment. Next, the test piece was immersed in the metal coloring liquid for chemical conversion treatment in a bath controlled at the temperature shown in Table 7. After immersion for the time shown in Table 7, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.
[0048] [Test Example 4: Coloring test of iron and iron alloys] (Example 88) A JIS SPCC (rolled steel plate) was prepared as a test piece (metal piece to be treated), and the surface of the test piece was degreased and washed with water in that order. Next, a bathtub was prepared containing a metal coloring liquid for chemical conversion treatment having the liquid composition shown in Table 7. Pure water was used as the aqueous medium for the metal coloring liquid for chemical conversion treatment. Next, the test piece was immersed in the metal coloring liquid for chemical conversion treatment in a bath controlled at the temperature shown in Table 7. After immersion for the time shown in Table 7, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.
[0049] [Test Example 5: Coloring test of magnesium and magnesium alloys] (Example 89) A JIS AZ31 (magnesium-zinc alloy) was prepared as a test piece (metal piece to be treated), and the surface of the test piece was degreased and washed with water in that order. Next, a bathtub was prepared containing a metal coloring liquid for chemical conversion treatment having the liquid composition shown in Table 7. Pure water was used as the aqueous medium for the metal coloring liquid for chemical conversion treatment. Next, the test piece was immersed in the metal coloring liquid for chemical conversion treatment in a bath controlled at the temperature shown in Table 7. After immersion for the time shown in Table 7, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.
[0050] [Test Example 6] (Comparative Examples 1 to 4) The metals shown in Table 9 were prepared as test pieces (metal pieces to be treated), and the surfaces of the test pieces were degreased and washed with water in that order. Next, a bathtub was prepared containing a metal coloring liquid for chemical conversion treatment having the liquid composition shown in Table 9. Pure water was used as the aqueous medium for the metal coloring liquid for chemical conversion treatment. Next, the test piece was immersed in the metal coloring liquid for chemical conversion treatment in a bath controlled at a temperature shown in Table 9. After immersion for the time shown in Table 9, the test piece was taken out. Next, the surface of the test piece was washed with water and then dried.
[0051] [Various evaluations] For the test pieces prepared in Examples 1 to 91 and Comparative Examples 1 to 4, color tone evaluation and adhesion evaluation were performed as follows.
[0052] (Color Tone Evaluation) The surface color tone of the test piece was evaluated visually according to the following criteria: A: Yellow with uniform and aesthetically pleasing processing appearance B: A deeper yellow color than A, with a uniform and aesthetically pleasing processed appearance C: A lighter yellow than A, with a uniform and aesthetically pleasing processed appearance D: Brown with uniform and aesthetically pleasing processed appearance E: Darker brown than D, with a uniform and aesthetically pleasing processed appearance F: A lighter brown than D, with a uniform and aesthetically pleasing processed appearance G: No coloring
[0053] (Adhesion evaluation) The surface of the test piece was cut with a cutter into 10 × 10 squares (100 squares in total), and the number of squares in which the colored film did not come off when Scotch tape (registered trademark) was applied and peeled off was counted. The size of one square was 1 mm x 1 mm in length x width. In each table, the result is shown as (the number of squares where the colored film did not peel off) / 100, and the greater the number of squares where the colored film did not peel off, the higher the adhesion of the colored film.
[0054] For Examples 1 to 91 and Comparative Examples 1 to 4, the test conditions and evaluation results are shown in Tables 1 to 9.
[0055] [Table 1]
[0056] [Table 2]
[0057] [Table 3]
[0058] [Table 4]
[0059] [Table 5]
[0060] [Table 6]
[0061] [Table 7]
[0062] [Table 8]
[0063] [Table 9]
[0064] From the above results, it was confirmed that, as in Examples 1 to 91, the metal coloring solution for chemical conversion treatment containing permanganic acid or a salt thereof, either or both of an inorganic acid and a salt thereof, and a condensed phosphate can color a metal surface in a yellow to brown color tone with good treatment efficiency. On the other hand, it was confirmed that, as in Comparative Examples 1 to 4, if the metal coloring solution for chemical conversion treatment does not contain permanganic acid or a salt thereof, either or both of an inorganic acid and a salt thereof, and a condensed phosphate, the metal surface cannot be colored in a yellow to brown color tone.
Claims
1. Permanganic acid or a salt thereof, An inorganic acid and / or a salt thereof; A condensed phosphate; Including, the permanganic acid or a salt thereof is permanganic acid, sodium permanganate, potassium permanganate, zinc permanganate, magnesium permanganate, calcium permanganate, ammonium permanganate, or a combination thereof; The inorganic acid and its salt are phosphoric acid, sulfuric acid, nitric acid, carbonic acid, hydrochloric acid, and their salts, or combinations thereof; the condensed phosphate is a combination of potassium pyrophosphate and sodium tripolyphosphate, The content of the permanganic acid or a salt thereof is 0.5 to 50 g / L, The content of the inorganic acid and its salt is 0.5 to 100 g / L; The content of the condensed phosphate is 1 to 150 g / L, The metal to be treated is at least one selected from the group consisting of aluminum, aluminum alloys, copper, copper alloys, iron, iron alloys, zinc, and zinc alloys; Metal coloring liquid for chemical conversion coating.
2. 2. The metal coloring solution for chemical conversion coating according to claim 1, further comprising an oxoacid or a salt thereof.
3. 3. The metal coloring liquid for chemical conversion treatment according to claim 2, wherein the oxoacid or a salt thereof is perchloric acid, chloric acid, chlorous acid, hypochlorous acid, bromic acid, boric acid, a salt thereof, or a combination thereof.
4. 4. The metal coloring solution for chemical conversion treatment according to claim 2, wherein the total content of the oxoacid or a salt thereof is 0.5 to 100 g / L.
5. A metal coloring treatment method comprising a step of coloring a metal by chemical conversion treatment using the metal coloring liquid for chemical conversion treatment according to any one of claims 1 to 4.
6. 6. The metal coloring treatment method according to claim 5, wherein in the step of coloring the metal by chemical conversion treatment, the metal is colored by immersing the metal in the metal coloring solution for chemical conversion treatment at 10°C to 80°C for 30 seconds to 20 minutes.
Citation Information
Patent Citations
Method for forming golden yellow film on surface of aluminum alloy
CN104894552A
Coloring of aluminum
JP1979107438A
Alignment pattern of semiconductor device
JP1985004217A
Electrolytic coloring method of aluminum and aluminum alloy
JP1985110895A
Surface treatment method for aluminum alloy
JP2004169120A