Seed crystal adhesion layer, method for manufacturing laminate using same, and method for manufacturing wafer

By employing a seed crystal adhesive layer with controlled thermal expansion properties, the stress-induced warpage and crystallinity issues in silicon carbide wafer production are mitigated, resulting in high-quality ingots and wafers with reduced defects.

JP7573259B2Active Publication Date: 2024-10-25株式会社 アイン クリスタル
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2020080840
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-22
Filing Date
2020-04-30
Publication Date
2024-10-25
Estimated Expiration
2040-04-30

AI Technical Summary

Technical Problem

The conventional methods for growing silicon carbide single crystals face issues due to stress caused by the difference in thermal expansion coefficients between the seed crystal holder and the adhesive layer, leading to warpage and decreased crystallinity during wafer processing.

Method used

A seed crystal adhesive layer with specific volume and area changes (Sg and Vr values) is applied, which minimizes stress by allowing partial separation during the growth and cooling processes, using a carbonized and graphitized adhesive layer with controlled thermal expansion characteristics.

Benefits of technology

This approach results in silicon carbide ingots and wafers with reduced warpage and improved crystallinity, enabling the production of high-quality wafers with minimal defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573259000021
    Figure 0007573259000021
  • Figure 0007573259000022
    Figure 0007573259000022
  • Figure 0007573259000023
    Figure 0007573259000023
Patent Text Reader

Abstract

To provide a seed crystal adhesion layer and a production method of a laminate applying the same.SOLUTION: A seed crystal adhesion layer 100 minimizes a stress applied to an ingot 130 at a unique graphitization shrinkage, and can separate only a part of the grown ingot 130 from a seed crystal holder 120, but can prevent complete separation. Further, the ingot 130 manufactured by applying the seed crystal adhesion layer 100, and a processed wafer can show an excellent warpage value.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a seed crystal adhesive layer, a method for producing a laminate using the seed crystal adhesive layer, and a method for producing a wafer. [Background technology]

[0002] Silicon carbide (SiC) is a semiconductor with a wide band gap of 2.2 eV to 3.3 eV, and due to its excellent physical and chemical properties, research and development of it as a semiconductor material is progressing.

[0003] Methods for producing silicon carbide single crystals include liquid phase epitaxy (LPE), chemical vapor deposition (CVD), and physical vapor transport (PVT). Among them, the physical vapor transport method is a method in which silicon carbide raw material is charged into a crucible, a seed crystal consisting of silicon carbide single crystal is placed on the upper end of the crucible, and the crucible is heated by induction heating to sublimate the raw material and grow silicon carbide single crystal on the seed crystal. The physical vapor transport method is the most widely used method because it has a high growth rate and can produce silicon carbide in the form of an ingot.

[0004] Meanwhile, in the past, in order to grow silicon carbide single crystals, an adhesive layer has been formed between a seed crystal and a seed crystal holder. However, during growth of a silicon carbide single crystal ingot, stress may be applied to the ingot due to a difference in thermal expansion coefficient between the seed crystal holder and the adhesive layer, which may result in problems such as increased warpage and decreased crystal quality when processed into a wafer.

[0005] Examples of such methods for producing silicon carbide include "Method for growing single crystal silicon carbide" disclosed in Korean Patent Publication No. 10-2015-0075220 and "Method for producing single crystal silicon carbide" disclosed in Korean Patent Publication No. 10-1392639. Summary of the Invention [Problem to be solved by the invention]

[0006] The purpose of the embodiment is to provide a seed crystal adhesive layer capable of producing an ingot of excellent quality by minimizing the generation of stress caused by the difference in thermal expansion coefficient between the support and the adhesive layer, and a method for manufacturing a laminate using the same.

[0007] An object of the embodiment is to minimize the occurrence of stress caused by the difference in thermal expansion coefficient between the support and the adhesive layer, thereby manufacturing ingots, wafers, etc. with high quality. [Means for solving the problem]

[0008] In order to achieve the above object, in one embodiment, the seed crystal adhesion layer has a Vr represented by the following formula 1, and has a Vr of 28% / mm 3 It has a Vr value of equal to or greater than 1.

[0009] [Formula 1] JPEG0007573259000001.jpg734

[0010] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at room temperature,

[0011] [Formula 2] JPEG0007573259000002.jpg741

[0012] In the formula 2, A1 is the area (mm 2 ) and A2 is the area (mm 2 ) was measured at room temperature.

[0013] The Sg value may be 8.5% or more.

[0014] The seed crystal adhesion layer before carbonization was 1.69 g / cm 2 It can support more than this weight.

[0015] The graphitized seed crystal adhesion layer has a thickness of 1.97 g / cm 2 It can support more than this weight.

[0016] The seed crystal adhesion layer before carbonization may be in the form of a coating layer or a film layer.

[0017] The seed crystal adhesion layer may have a Vg value of 56% or more, where Vg is represented by the following formula 3:

[0018] [Formula 3] JPEG0007573259000003.jpg745

[0019] In the above formula 3, V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) was measured at room temperature.

[0020] The seed crystal adhesion layer may have a thickness of 3 μm or more.

[0021] A part or the whole of one surface of the seed crystal adhesion layer may be adhered to a surface having a thermal expansion coefficient of 6 or less at 293.15 to 473.15K.

[0022] The seed crystal adhesion layer can i) comprise an adhesive resin, or ii) comprise an adhesive resin and a filler.

[0023] The adhesive resin may have a residual carbon content of 5 to 50% by weight.

[0024] The graphitized seed crystal adhesive layer may be obtained by subjecting the seed crystal adhesive layer before carbonization to a heat treatment at a temperature of 2000° C. or higher.

[0025] The seed crystal adhesion layer before carbonization has an area of ​​7.85×10 3 mm 2 It may be more than that.

[0026] The graphitized seed crystal adhesion layer has a surface area of ​​5.50×10 3 mm 2 It may be more than that.

[0027] In order to achieve the above object, a method for manufacturing a laminate according to one embodiment includes the steps of:

[0028] a lamination step of providing a seed crystal adhesive layer before carbonization on one surface of a support or one surface of a seed crystal, and providing a laminate including the seed crystal adhesive layer interposed between the support and the seed crystal;

[0029] a carbonization step of subjecting the uncarbonized seed crystal adhesive layer to a carbonization heat treatment so that the laminate includes a carbonized seed crystal adhesive layer;

[0030] The seed crystal adhesion layer has a Vr value represented by the following formula 1 of 28% / mm 3 It may be more than that.

[0031] [Formula 1] JPEG0007573259000004.jpg734

[0032] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at room temperature,

[0033] [Formula 2] JPEG0007573259000005.jpg741

[0034] In the formula 2, A1 is the area (mm 2 ) and A2 is the area (mm 2 ) was measured at room temperature.

[0035] The carbonization heat treatment may be carried out at a temperature of 500°C to 900°C.

[0036] The method for producing the laminate may further include a graphitization heat treatment step after the carbonization step.

[0037] The graphitization heat treatment step is a step of subjecting the laminate to a graphitization heat treatment at a temperature of 2000° C. or higher so that the laminate includes a graphitized seed crystal adhesion layer.

[0038] The graphitization heat treatment step may include growing an ingot on one side of the seed crystal.

[0039] The graphitized seed crystal adhesion layer includes opposing first and second sides.

[0040] The first surface and the second surface each have a joining surface bonded to the opposing surface.

[0041] The graphitized seed crystal adhesion layer can have a first bonding surface and a second bonding surface bonded to opposing surfaces.

[0042] The first bonding surface is a bonding surface where the first surface is in direct contact with a surface opposite to the first surface, and the second bonding surface is a bonding surface where the second surface is in direct contact with a surface opposite to the second surface.

[0043] The surface opposite to the second surface may be one surface of the seed crystal, and a sum of an area of ​​the first bonding surface and an area of ​​the second bonding surface may be 0.95 times or less of a sum of an area of ​​the first surface and an area of ​​the second surface.

[0044] In order to achieve the above object, a method for manufacturing a wafer according to one embodiment includes a grinding step of grinding an edge of an ingot grown on one surface of the seed crystal;

[0045] and a sawing step of sawing the ground ingot to provide wafers.

[0046] In order to achieve the above object, a laminate according to one embodiment comprises:

[0047] a seed crystal adhesion layer having a first surface and a second surface; a support overlying the first surface; and a seed crystal underlying the second surface;

[0048] The first surface and one surface of the support face each other, and the second surface and one surface of the seed crystal contact each other,

[0049] the seed crystal adhesion layer is a carbonized seed crystal adhesion layer;

[0050] The carbonized seed crystal adhesive layer is obtained by carbonizing a seed crystal adhesive layer before carbonization,

[0051] The seed crystal adhesion layer before carbonization is a seed crystal adhesion layer that is a coating layer or a film layer,

[0052] the carbonized seed crystal adhesion layer is graphitized by heat treatment at a temperature of 2000° C. or more to form a graphitized seed crystal adhesion layer;

[0053] the change in area of ​​the seed crystal adhesive layer is the difference between the area of ​​the graphitized seed crystal adhesive layer and the area of ​​the seed crystal adhesive layer before carbonization;

[0054] the change in area of ​​the seed crystal is a change in area of ​​one face of the seed crystal before and after the heat treatment,

[0055] the change in area of ​​the support is a change in area of ​​one surface of the support before and after the heat treatment,

[0056] The change in area of ​​the seed crystal adhesion layer is greater than the change in area of ​​the seed crystal or the change in area of ​​the support,

[0057] The graphitized seed crystal adhesion layer may have a portion of the first surface or a portion of the second surface separated from an adjacent surface.

[0058] In the laminate, one surface of the support may have a thermal expansion coefficient of 6 or less at 293.15 to 473.15K.

[0059] In the laminate, one surface of the seed crystal may have a thermal expansion coefficient of 4 or less at 293.15 to 473.15K.

[0060] The graphitized seed crystal adhesion layer may have an area reduced during the heat treatment and the cooling process after the heat treatment.

[0061] The seed crystal adhesion layer before carbonization is 1.69 g / cm 2 It can support more than this weight.

[0062] The graphitized seed crystal adhesion layer has a density of 1.97 g / cm 2 It can support more than this weight.

[0063] The stack may include an ingot grown from the other side of the seed crystal.

[0064] The seed crystal adhesive layer of the laminate has a bonding surface bonded to an opposing surface, a first bonding surface being a bonding surface where the first surface and the opposing surface contact, and a second bonding surface being a bonding surface where the second surface contacts one surface of the seed crystal that the second surface faces, and the sum of the area of ​​the first bonding surface and the area of ​​the second bonding surface may be 0.95 times or less of the sum of the area of ​​the first surface and the area of ​​the second surface.

[0065] The seed crystal adhesive layer of the laminate has a bonding surface bonded to an opposing directly contacting surface, a first bonding surface being a surface where the first surface and the opposing surface are in contact, and a second bonding surface being a surface where the second surface is in contact with one surface of the seed crystal.

[0066] The area of ​​the first bonding surface may be 0.3 times or more the area of ​​the first surface.

[0067] The area of ​​the second bonding surface may be 0.3 times or more the area of ​​the second surface.

[0068] The seed crystal adhesion layer of the laminate is 28% / mm 3 The Vr value may be equal to or greater than 1, and the Vr may be expressed by the following formula 1.

[0069] [Formula 1] JPEG0007573259000006.jpg734

[0070] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at room temperature,

[0071] [Formula 2] JPEG0007573259000007.jpg741

[0072] In the formula 2, A1 is the area (mm 2 ) and A2 is the area (mm 2 ) was measured at room temperature.

[0073] The seed crystal of the stack has an area of ​​7.85×10 3 mm 2 It may be more than that.

[0074] One surface of the seed crystal of the laminate may have a surface roughness (Ra) of 5 μm or less.

[0075] In order to achieve the above object, a method for producing an ingot according to one embodiment includes the steps of:

[0076] A preparation step of disposing the source material and the laminate facing each other in a reaction vessel having an internal space;

[0077] a growing step of sublimating the source material by adjusting the temperature, pressure and gas atmosphere of the inner space to provide an ingot grown from the laminate;

[0078] and a cooling step of cooling the reaction vessel to recover the ingot or a stack further including the ingot;

[0079] The laminate includes a seed crystal adhesion layer having a first surface and a second surface; a support positioned above the first surface; and a seed crystal positioned below the second surface;

[0080] the first surface and one surface of the support face each other,

[0081] the second surface and one surface of the seed crystal are in contact with each other,

[0082] In the preparation step, the seed crystal adhesion layer is a carbonized seed crystal adhesion layer;

[0083] The carbonized seed crystal adhesive layer is obtained by carbonizing a seed crystal adhesive layer before carbonization,

[0084] The seed crystal adhesion layer before carbonization is a seed crystal adhesion layer that is a coating layer or a film layer,

[0085] In the growing step, the seed crystal adhesion layer is a graphitized seed crystal adhesion layer;

[0086] the change in area of ​​the seed crystal adhesive layer is the difference between the area of ​​the graphitized seed crystal adhesive layer and the area of ​​the seed crystal adhesive layer before carbonization;

[0087] the change in area of ​​the seed crystal is a change in area of ​​one face of the seed crystal before and after the heat treatment,

[0088] the change in area of ​​the support is a change in area of ​​one surface of the support before and after the heat treatment,

[0089] The change in area of ​​the seed crystal adhesion layer is greater than the change in area of ​​the seed crystal or the change in area of ​​the support,

[0090] The graphitized seed crystal adhesion layer may be such that a portion of the first surface or a portion of the second surface is separated from the adjacent surface.

[0091] In the method for producing an ingot, the area of ​​the graphitized seed crystal bonding layer may be reduced by 8.5% or more based on the area of ​​the seed crystal bonding layer before carbonization.

[0092] In the method for producing an ingot, the seed crystal adhesion layer has a bonding surface bonded to an opposing surface, and the first bonding surface is a bonding surface where the opposing surface of the first surface is in contact with each other;

[0093] The second bonding surface may be a bonding surface that is in direct contact with one surface of the seed crystal opposite to the second surface, and an area of ​​the first bonding surface after the cooling step may be 0.3 times or more the area of ​​the first surface, and an area of ​​the second bonding surface may be 0.3 times or more the area of ​​the second surface.

[0094] In the method for producing the ingot, the wafer produced from the ingot can have a warpage value of 55 μm or less.

[0095] In the method for producing an ingot, the ingot may be a SiC single crystal ingot.

[0096] In order to achieve the above object, a method for manufacturing a wafer according to one embodiment includes the steps of:

[0097] A preparation step of disposing a raw material and a laminate produced by the laminate production method in a reaction vessel having an internal space so as to face each other;

[0098] a growing step of sublimating the source material by adjusting the temperature, pressure and gas atmosphere of the inner space to provide an ingot grown from the laminate;

[0099] a cooling step of cooling the reaction vessel to recover the ingot or a stack including the ingot;

[0100] a grinding step of grinding an edge of the recovered ingot;

[0101] and a sawing step of sawing the ground ingot to provide wafers.

[0102] In order to achieve the above object, a method for manufacturing a wafer according to one embodiment includes the steps of:

[0103] a grinding step of grinding an edge of the ingot produced by the ingot production method;

[0104] and a sawing step of sawing the ground ingot to provide wafers. Effect of the Invention

[0105] The seed crystal bonding layer according to an embodiment can minimize stress applied to the ingot, and the grown ingot can be only partially but not completely separated from the seed crystal bonding layer. In addition, the silicon carbide ingot manufactured by applying the seed crystal bonding layer according to an embodiment and the wafer processed therefrom can exhibit good warpage values.

[0106] The stack of one embodiment minimizes the stress applied to the ingot and allows the grown ingot to only partially detach from the seed crystal adhesion layer, and not to separate completely.

[0107] According to the ingot manufacturing method of the embodiment, the manufactured silicon carbide ingot and the wafer processed therefrom can exhibit good warpage values.

[0108] The wafer manufacturing method according to one embodiment can produce excellent quality wafers from a silicon carbide ingot. [Brief description of the drawings]

[0109] [Figure 1] FIG. 1 is a conceptual diagram illustrating the inside of a reaction vessel after a silicon carbide ingot has been grown in the prior art. [Diagram 2] 1A and 1B are schematic conceptual diagrams showing an example of the interior of a reaction vessel after an ingot is grown by applying a seed crystal adhesion layer according to an embodiment of the present invention; [Diagram 3] FIG. 2 is a conceptual diagram illustrating a laminate to which a seed crystal adhesion layer according to one embodiment is applied. [Figure 4] 1 is a conceptual diagram illustrating an example of a silicon carbide single crystal growth apparatus to which a seed crystal adhesion layer according to an embodiment of the present invention is applied. [Diagram 5] The photographs show (a) application of a resin composition, (b) formation of an adhesive layer, (c) carbonization, and (d) graphitization in that order. [Figure 6] 1 is a graph showing the warpage value of a wafer depending on the cutting position of an ingot in a comparative example (a) and an example (b). [Figure 7] 6 is a photograph showing the results of XRD mapping of a wafer in the comparative example (a) and the example (b). [Figure 8] FIG. 1 is a conceptual diagram showing the forms (c1) and (c2) of a seed crystal adhesion layer (a) being separated from a seed crystal and a support by shrinkage (b) after heat treatment according to one embodiment. BEST MODE FOR CARRYING OUT THEINVENTION

[0110] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the following, the preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily understand the present invention. However, the present invention may be embodied in many different forms and is not limited to the preferred embodiments described herein. The same reference numerals are used throughout the specification to refer to similar parts.

[0111] In this specification, when a certain configuration "includes" another configuration, this does not mean to exclude the other configurations, unless specifically stated to the contrary, but rather means that the other configurations may also be included.

[0112] In this specification, when a certain component is said to be "connected" to another component, this includes not only the case where the component is "directly connected" but also the case where the component is "connected via another component between them."

[0113] In this specification, the term "B is located on A" means that B is located on A in direct contact therewith, or that B is located on A with another layer located therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.

[0114] As used herein, the term "combinations thereof" contained in a Markush form expression means a mixture or combination of one or more selected from the group of components set forth in the Markush form expression, and is meant to include one or more selected from the group of components.

[0115] In this specification, the phrase "A and / or B" means "A, B, or A and B."

[0116] In this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from each other, unless otherwise specified.

[0117] In this specification, the term "singular" is to be construed as including the singular or plural as the context requires, unless otherwise specified.

[0118] The present invention will now be described in more detail.

[0119] While researching a method for producing a high-quality ingot with fewer defects, the inventors of the present invention discovered that a seed crystal adhesive layer that satisfies a predetermined graphitization shrinkage rate can be used in the process of growing a single crystal using physical vapor transport (PVT), a sublimation method, to produce an ingot of excellent quality, and thus completed the present invention.

[0120] Seed crystal adhesive layer In order to achieve the above object, the seed crystal bonding layer 100 according to one embodiment comprises: Vr is expressed by the following formula 1, and is 28% / mm 3 The Vr value may be greater than or equal to 1.

[0121] [Formula 1] JPEG0007573259000008.jpg734

[0122] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at room temperature,

[0123] [Formula 2] JPEG0007573259000009.jpg741

[0124] In the formula 2, A1 is the area (mm 2 ) and A2 is the area (mm 2 ) was measured at room temperature.

[0125] The seed crystal adhesive layer before carbonization is the seed crystal adhesive layer before the seed crystal adhesive layer is graphitized at a temperature of at least 2000° C. The composition and manufacturing method of the seed crystal adhesive layer will be described later.

[0126] The seed crystal adhesive layer before carbonization may be a seed crystal adhesive layer that is a coating layer or a seed crystal adhesive layer that is a film layer. The seed crystal adhesive layer that is a coating layer and the seed crystal adhesive layer that is a film layer will be described later.

[0127] The seed crystal adhesive layer before carbonization is semi-transparent because the adhesive resin is polymerized. The seed crystal adhesive layer before carbonization is amorphous carbon, and is different from the opaque seed crystal adhesive layer after carbonization. The adhesive resin will be described later.

[0128] The graphitized seed crystal bonding layer is a seed crystal bonding layer graphitized at the temperature. The volume of the seed crystal bonding layer before carbonization is reduced as it becomes a graphitized seed crystal bonding layer.

[0129] The Sg value is the percentage of the area of ​​the seed crystal adhesion layer 100 before carbonization that has changed due to graphitization. The change may be shown as a decrease.

[0130] The area of ​​the seed crystal adhesive layer before carbonization may be the area relative to the bonding surface attached to the adherend (support, seed crystal, etc.) The area of ​​the graphitized seed crystal adhesive layer refers to the area of ​​the seed crystal adhesive layer excluding the area of ​​the seed crystal adhesive layer before carbonization that has shrunk due to graphitization.

[0131] The area, thickness and volume of the graphitized seed crystal adhesion layer may be measured at room temperature, which may be 20°C to 30°C, specifically 25°C.

[0132] The Sg value may be 8.5% or more, or may be 9% or more. The Sg value may be 11% or more, or may be 16% or more. The Sg value may be 30% or less. The Sg value may be 27% or less, or may be 21% or less.

[0133] If the Sg value exceeds 30%, the seed crystal, including the ingot grown and cooled using the seed crystal adhesive layer 100, may be completely separated from the seed crystal adhesive layer, which may damage the ingot, and the area of ​​the seed crystal adhesive layer separated from the seed crystal or support may be excessive, which may reduce the quality of the ingot.

[0134] If the Sg value is less than 8.5%, the warp value of the ingot may not be good due to stress between the seed crystal containing the grown ingot and the seed crystal adhesive layer or between the seed crystal and the support.

[0135] When the Sg value satisfies the above range, partial separation can be effectively performed between the seed crystal adhesive layer and the adherend (support, seed crystal, etc.) during the process of growing and cooling the ingot through sublimation at a temperature of 2000° C. or more, thereby minimizing the stress applied to the ingot to be manufactured. When the Sg value is 16% to 21%, the quality of the ingot to be manufactured can be further improved.

[0136] The Sg value may be measured by a method such as that described in the following Experimental Examples, but is not limited thereto.

[0137] When the Vr value in Equation 1 is within the range described below, the generation of stress can be further reduced when the seed crystal adhesion layer 100 is applied to produce an ingot, so that a high-quality ingot can be grown and recovered.

[0138] The Vr value is 28 % / mm 3 or more, or 28.7 % / mm 3 The Vr value may be 38.3 or more. % / mm 3 or more, or 52.3 % / mm 3 The Vr value may be 154.5 or more. % / mm 3 The Vr value may be 77.8 or less. % / mm3 or less than 63.8 % / mm 3 It may be the following.

[0139] The Vr value is 154.5 % / mm 3 If the temperature exceeds this range, the defect density of the ingot grown using the seed crystal adhesion layer 100 may become so high that the ingot produced may become completely detached from the seed crystal adhesion layer, potentially damaging the ingot itself.

[0140] The Vr value is 28 % / mm 3 If it is less than this, the ingot grown by applying the seed crystal adhesive layer will be susceptible to stress due to the difference in thermal expansion coefficient between the seed crystal adhesive layer and the adherend (support, seed crystal, etc.), and the quality of the ingot produced may not be good.

[0141] When the Vr value satisfies the above range, the stress applied to the ingot being manufactured and the defects caused thereby can be minimized, and the seed crystal can be effectively partially separated from the seed crystal bonding layer during the ingot manufacturing process.

[0142] The Vr value is 53.7 % / mm 3 ~64.1 % / mm 3 If so, the quality of the produced ingot can be further improved.

[0143] The Vr value may be measured by a method such as that described in the following Experimental Examples, but is not limited thereto.

[0144] When the seed crystal adhesive layer 100 is a seed crystal adhesive layer before carbonization, it may be a seed crystal adhesive layer that is a coating layer or a seed crystal adhesive layer that is a film layer. The seed crystal adhesive layer that is a coating layer may be a seed crystal adhesive layer in a form in which a liquid adhesive resin composition is applied, and the seed crystal adhesive layer that is a film layer may be a seed crystal adhesive layer in a form in which the adhesive resin composition is applied and then cured.

[0145] The seed crystal adhesion layer 100 before carbonization had a viscosity of 1.69 g / cm 2 The seed crystal adhesion layer 100 before carbonization can support a weight of 10.7 g / cm 2 Can support a weight of more than 15.4g / cm 2 By supporting a weight in the above range, a layered body including the seed crystal adhesion layer 100 interposed between the seed crystal and the support can be stably disposed at the upper end inside the reaction vessel before the growth of an ingot.

[0146] The seed crystal adhesive layer 100, which is a coating layer, may include an adhesive resin, or may include an adhesive resin and a filler. The seed crystal adhesive layer 100, which is a coating layer, may further include a solvent.

[0147] The seed crystal adhesion layer, which is the coating layer, may be formed by applying a liquid adhesive resin composition containing an adhesive resin having a predetermined solid content and drying it.

[0148] The solid content may be 16% by weight to 27% by weight, or 18% by weight to 25% by weight, based on the total adhesive resin composition. The solid content may be 18% by weight to 22% by weight, based on the total adhesive resin composition.

[0149] The adhesive resin composition having the above solid content can easily form the seed crystal adhesive layer on the adherend, and can provide a seed crystal adhesive layer having the above Sg and Vr values.

[0150] The solvent may include one selected from the group consisting of dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethanol, methanol, acetone, and combinations thereof, but may be applied without limitation as long as it is applicable to the production of the adhesive resin composition and the seed crystal adhesive layer, and is not limited to the above examples.

[0151] The film layer, the seed crystal adhesive layer 100, may include an adhesive resin, or may include an adhesive resin and a filler.

[0152] The seed crystal adhesive layer 100 which is the film layer can be provided by applying the liquid adhesive resin composition and subjecting it to a curing heat treatment.

[0153] The adhesive resin may be graphitized along with the growth of the ingot in a growth temperature atmosphere in which the growth of the ingot including the sublimation of the source material is performed. The adhesive resin may be one that can at least partially maintain adhesion to the seed crystal and the support at the growth temperature of the ingot.

[0154] The residual carbon content of the adhesive resin may be 5 wt% to 50 wt%, or 10 wt% to 30 wt%. The seed crystal adhesive layer using the adhesive resin having the residual carbon content in the above range can be effectively graphitized in the ingot growing step, and can help the seed crystal adhesive layer to be partially separated in the recovery step after the ingot is grown.

[0155] Specifically, the adhesive resin may include one selected from the group consisting of polyacrylic resin, polyacrylonitrile resin, phenol resin, epoxy resin, polyvinyl chloride resin, and combinations thereof.

[0156] The filler may be one selected from the group consisting of graphite, coke, carbon black, carbon nanotubes, graphene, and combinations thereof. The filler can control the degree of shrinkage during graphitization of the seed crystal bonding layer 100.

[0157] The average particle size of the filler (D 50 The average particle size (D 50 The average particle diameter (D 50 ) may be 250 nm to 550 nm, or may be 280 nm to 520 nm.

[0158] When the filler has such a particle size, the adhesive properties of the seed crystal adhesive layer 100 can be maintained at the same level or higher while minimizing the effect of stress applied to the ingot, and the change characteristics of the volume and area of ​​the seed crystal adhesive layer due to temperature can be more easily controlled.

[0159] The amount of the filler added may be 0.5% by weight or more, or 1% by weight or more, based on the entire solution containing the adhesive resin. The amount of the filler added may be 10% by weight or less, or 6% by weight or less, based on the entire solution containing the adhesive resin. Within the range of the amount of the filler added, the adhesive properties and area change properties of the seed crystal adhesive layer 100 can be more easily controlled.

[0160] When the filler is added, the adhesive resin may be one selected from the group consisting of polyacrylic acid resin, polyacrylonitrile resin, phenolic resin, and cresol novolac type resin. Also, when the filler is added, the adhesive resin may be polyacrylic acid resin or polyacrylonitrile resin.

[0161] In this case, by applying the resin to the seed crystal adhesive layer 100, the adherends, that is, the seed crystal 110 and the support 120, maintain an optimal bonding area with the graphitized seed crystal adhesive layer during the growth and cooling of the ingot, but are partially separated, thereby efficiently reducing the stress applied to the ingot and producing a higher quality ingot.

[0162] The seed crystal adhesive layer 100 may include a bonding surface to which the surface facing the adherend (support, seed crystal, etc.) is bonded, and the bonding surface includes a first surface which is one surface of the seed crystal adhesive layer 100, and a second surface which is the other surface.

[0163] Specifically, a support 120 can be positioned above the seed crystal adhesive layer, one side of the support can face the first side of the seed crystal adhesive layer, and they can be bonded to each other. A seed crystal 110 can be positioned below the seed crystal adhesive layer, one side of the seed crystal can face and contact the second side of the seed crystal adhesive layer.

[0164] The seed crystal adhesion layer 100 and the object to be adhered (support, seed crystal, etc.) are adhered to each other.

[0165] The thermal expansion coefficient of the adherend (×10 -6 / °C) may be 6 or less at 293.15K to 473.15K. -6 / °C) may be 5 or less, or 4.5 or less at 293.15K to 473.15K. -6 / °C) may be 1 or more, 2 or more, or 3 or more at 293.15K to 473.15K. -6 / °C) may be 3.7 to 4.2 at 293.15K to 473.15K.

[0166] When the seed crystal adhesive layer is applied to an adherend (seed crystal, support, etc.) that satisfies the above-mentioned range of thermal expansion coefficient, partial separation between the seed crystal adhesive layer and the adherend can be more appropriately induced during the heating and cooling process for growing the ingot.

[0167] The surface roughness (Ra) of one surface of the adherend to which the seed crystal adhesive layer 100 is adhered may be 5 μm or less, or 0.01 nm or more.

[0168] The seed crystal 110 can be applied in different ways depending on the characteristics of the ingot to be grown.

[0169] When the ingot is a silicon carbide ingot, a silicon carbide seed crystal can be applied. For example, 4H-SiC wafer, 6H-SiC wafer, 3C-SiC wafer, 15R-SiC wafer, etc. can be applied, and any ingot can be grown by sublimation at a temperature of 2000°C or higher.

[0170] The seed crystal 110 can be applied differently depending on the size of the ingot to be grown. The diameter of the ingot may be 4 inches or more, 5 inches or more, or 6 inches or more. The diameter of the ingot may be 4 inches to 12 inches, 4 inches to 10 inches, or 6 inches to 8 inches. The seed crystal can be appropriately applied depending on the characteristics of the ingot.

[0171] The seed crystal 110 may be one capable of growing a 4H-SiC single crystal, and for example, a seed crystal of a 4H-SiC crystal whose front surface from which an ingot grows is the C-plane (000-1) may be used.

[0172] The support 120 may be applied for the purpose of placing the seed crystal 110 together with the seed crystal adhesion layer 100 in the upper part of the inner space of a reaction vessel for growing an ingot.

[0173] The support 120 may be made of graphite or may be made of the same material as the crucible of the reaction vessel used to grow the ingot, and may be formed integrally with or separately from the lid of the reaction vessel.

[0174] The graphitized seed crystal adhesive layer 100 can be provided by heat treating the seed crystal adhesive layer in an inert atmosphere such as nitrogen or argon gas at a pressure of 10 torr to 50 torr, at a temperature increase rate of 5° C. / min to 10° C. / min, and at a temperature of 2000° C. to 2600° C. for 1 hour to 100 hours. Specifically, the graphitized seed crystal adhesive layer 100 can be provided by heat treating the seed crystal adhesive layer in an argon atmosphere of 30 torr at a temperature increase rate of 10° C. / min, and at a temperature of 2600° C. for 10 hours.

[0175] The area, volume, etc. of the graphitized seed crystal adhesion layer are based on values ​​measured at a temperature of 25°C.

[0176] Generally, the growth of the ingot and / or the graphitization of the seed crystal bonding layer is performed by a heat treatment process at high temperature, and the area, volume, etc. of the graphitized seed crystal bonding layer are measured after a cooling process. The cooling process may be performed by applying a cooling rate of 5°C / min to 10°C / min to the graphitized seed crystal bonding layer. The cooling may be performed under the condition of an argon or nitrogen atmosphere of 5 to 750 torr.

[0177] The graphitized seed crystal adhesion layer 100 has a viscosity of 1.97 g / cm 2 Can support a weight of more than 12.5g / cm 2 The graphitized seed crystal adhesion layer can support a weight of 51.3 g / cm 2 It can support the following weight: 35.9g / cm 2 By supporting a weight in this range, even if the graphitized seed crystal adhesion layer is partially separated from the adherend after the ingot is grown and cooled, the ingot can be prevented from being completely separated.

[0178] The seed crystal adhesion layer 100 may have a Vg value represented by the following formula 3 of 56% or more and 71% or less.

[0179] [Formula 3] JPEG0007573259000010.jpg741

[0180] In the above formula 3, V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) was measured at room temperature.

[0181] V1 and V2 in the formula 3 may be the same as the values ​​in the formula 1, and the graphitization conditions and the volume measurement conditions in the formula 3 are also the same as those described above.

[0182] When the seed crystal bonding layer 100 satisfies the Sg and Vr value ranges and the Vg value range, the desired partial separation can be easily induced while maintaining sufficient adhesion to the adherend during the ingot growth and cooling steps, and an ingot with further reduced stress-induced defects can be manufactured.

[0183] The thickness of the seed crystal adhesive layer 100 may be 3 μm or more. The thickness of the seed crystal adhesive layer 100 may be 5 μm or more, or 10 μm or more. The thickness may be 100 μm or less. The thickness may be 80 μm or less, or 70 μm or less. Within the above thickness range, a seed crystal adhesive layer of a uniform thickness overall can be stably formed, and the adherends, such as the seed crystal 110 and the support 120, can be more stably adhered.

[0184] The seed crystal adhesion layer 100 before carbonization (in the form of a coating layer or film layer) has an area of ​​7.85×10 3 mm 2 or more, or 17.6 x 10 3 mm 2 The seed crystal adhesion layer before carbonization may have an area of ​​70.6×104 mm 2 or less, or 40.9 x 10 4 mm 2 Within the above area and thickness ranges, adhesion can be stably performed, and partial separation of the seed crystal adhesion layer from the adherend can be effectively performed during growth and cooling of the ingot.

[0185] The area of ​​the graphitized seed crystal adhesion layer 100 is 5.50×10 3 mm 2 or more, or 12.3 x 10 3 mm 2 It may be 49.4 x 10 or more. 3 mm 2 or less, or 28.6 x 10 3 mm 2 When the graphitized seed crystal adhesion layer has such an area range, the graphitized seed crystal adhesion layer can be more easily partially separated from the adherend.

[0186] The volume of the seed crystal adhesive layer changes during the heating and cooling process, and at this time, tensions in opposite directions temporarily act on the interface between the seed crystal adhesive layer and the adherend, which is thought to temporarily weaken the adhesive force of the seed crystal adhesive layer to adhere to the adherend, causing partial separation of the seed crystal adhesive layer. At this time, if an ingot is located on the other side of the seed crystal and its weight increases, the partial separation can be more effectively performed.

[0187] The partial separation of the seed crystal adhesive layer can substantially eliminate stress caused by the difference in thermal expansion (or thermal contraction) rate during heating and cooling, and can significantly reduce defects caused in the ingot due to stress.

[0188] Such a volume change characteristic of the seed crystal adhesive layer is believed to have at least two reasons. One is that the adhesive resin contained in the seed crystal adhesive layer before carbonization is reduced in volume as it goes through the carbonization and graphitization process. The other is that the graphitized seed crystal adhesive layer is thermally contracted during cooling, resulting in a volume reduction.

[0189] Such a feature of the seed crystal adhesion layer has an even more excellent effect when it has a thermal expansion (or thermal contraction) property in an appropriate range with respect to the adherend.

[0190] However, since it is practically difficult to measure the thermal expansion coefficient (or coefficient of thermal expansion) at temperatures above 2000°C, the above presents the thermal expansion coefficient of the adherend (support, seed crystal, etc.) within the measurable temperature range.

[0191] Referring to Figures 1 and 2, a silicon carbide ingot grown using a conventional adhesive layer 10 (Figure 1) and an ingot 130 using a seed crystal adhesive layer 100 according to one embodiment (Figures 2(a) and (b)) can be seen.

[0192] As shown in FIG. 1, conventionally, stress may be applied to a silicon carbide ingot during heating and cooling processes in the growth process of the silicon carbide ingot due to a difference in thermal expansion coefficient between a support 120 and a seed crystal 110.

[0193] 2(a) and (b) show a shape in which partial separation occurs between the support 120 and the seed crystal 110 due to shrinkage of the seed crystal adhesion layer 100. This can suppress warping of the reaction vessel cover 140 located on the top of the support, and minimize stress applied to the ingot due to the difference in thermal expansion coefficient with the support.

[0194] During the ingot growth process, a polycrystal 131 may be formed surrounding the outer periphery of the seed crystal, the seed crystal adhesive layer, and the support, and then as the seed crystal adhesive layer shrinks, a portion of the polycrystal may break off.

[0195] As the ingot grows and cools, the graphitized seed crystal bonding layer 100 shrinks, as shown in FIG. 8 (FIG. 8(b), the black arrows represent the shrinkage of the bonding layer), and partial separation between the adherend and the seed crystal bonding layer may occur (FIGS. 8(c1) and (c2)).

[0196] When the remaining unseparated adhesive area between the graphitized seed crystal adhesive layer and the adherend is 95% or less of the area of ​​the graphitized seed crystal adhesive layer (i.e., when the separated area is more than 5%), the desired partial separation can be considered to have occurred.

[0197] The remaining unseparated adhesion area may be 90% or less, or 77% or less, of the area of ​​the graphitized seed crystal adhesion layer. The remaining unseparated adhesion area may be 30% or more, or 45% or more, of the area of ​​the graphitized seed crystal adhesion layer. When the graphitized seed crystal adhesion layer has the range of the remaining unseparated adhesion area, partial separation between the seed crystal adhesion layer and the adherend can be effectively performed during the growth and cooling of an ingot, and the seed crystal adhesion layer, which is the unseparated adhesion surface, can support the seed crystal and the ingot located on the other side of the seed crystal so that they are not completely separated.

[0198] Manufacturing method of laminate A method for manufacturing a laminate according to another embodiment includes the steps of:

[0199] a lamination step of providing a seed crystal adhesive layer 100 before carbonization on one surface of a support 120 or one surface of a seed crystal 110, and providing a laminate including the seed crystal adhesive layer interposed between the support and the seed crystal; and a carbonization step of subjecting the uncarbonized seed crystal adhesive layer to a carbonization heat treatment to provide a laminate including a carbonized seed crystal adhesive layer.

[0200] The carbonization step may further include a heat treatment step.

[0201] The heat treatment step is a step of producing a laminate including a graphitized seed crystal adhesion layer by subjecting the laminate to a graphitization heat treatment at a temperature of 2000° C. or higher.

[0202] The seed crystal adhesion layer has a Vr value represented by the following formula 1 of 28% / mm 3 It may be more than that.

[0203] [Formula 1] JPEG0007573259000011.jpg734

[0204] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at room temperature,

[0205] [Formula 2] JPEG0007573259000012.jpg741

[0206] In the formula 2, A1 is the area (mm 2 ) and A2 is the area (mm 2 ) was measured at room temperature.

[0207] The seed crystal adhesion layer includes a first side and a second side.

[0208] The seed crystal adhesive layer before carbonization includes a seed crystal adhesive layer that is a coating layer, or a seed crystal adhesive layer that is a film layer.

[0209] The carbonized seed crystal adhesive layer may be one obtained by subjecting the seed crystal adhesive layer which is a coating layer or the seed crystal adhesive layer which is a film layer to a carbonization heat treatment.

[0210] The lamination step is a step of providing a seed crystal adhesive layer before carbonization on one surface of the support 120 or one surface of the seed crystal 110, and providing a laminate including the seed crystal adhesive layer interposed between the support and the seed crystal.

[0211] The stack can include the seed crystal adhering layer, the support overlying a first side of the seed crystal adhering layer, and the seed crystal underlying a second side of the seed crystal adhering layer.

[0212] The seed crystal 110 and the support 120 in the lamination step are the same as the seed crystal and the support described as the adherend in the description of the seed crystal adhesion layer.

[0213] The seed crystal adhesive layer 100 in the lamination step is a seed crystal adhesive layer before carbonization, which may be in the form of a coating layer or a film layer, as described in the description of the seed crystal adhesive layer.

[0214] When the seed crystal adhesive layer 100 in the lamination step is a seed crystal adhesive layer that is a coating layer, the seed crystal adhesive layer that is a coating layer may be a liquid having a predetermined weight percent solid content by mixing the adhesive resin and the solvent.

[0215] When the seed crystal adhesive layer 100 in the lamination step is a seed crystal adhesive layer that is a coating layer, it may be a coating layer obtained by partially removing the solvent from the liquid seed crystal adhesive layer and drying it.

[0216] When the adhesive resin is a polyacrylic acid resin, a polyacrylonitrile resin, or a cresol novolac type resin, it may have a solid content of 16% to 27% by weight when mixed with a solvent, and the solid content may be 18% to 25% by weight, or 18% to 22% by weight.

[0217] By using an adhesive resin composition having the solid content, a seed crystal adhesive layer 100 that satisfies the Sg and Vr values ​​while having stable workability can be produced.

[0218] When the seed crystal adhesive layer 100 (seed crystal adhesive layer before carbonization) in the lamination step is in the form of a coating layer, the seed crystal adhesive layer in the form of a coating layer may be formed by applying an adhesive resin composition onto one surface of the support 120 or the seed crystal 110. Specifically, the application may be a method of applying a general liquid substance, and spin coating may be used, but is not limited thereto.

[0219] The coating thickness in the coating may be 3 μm or more, 5 μm or more, or 10 μm or more. The coating thickness may be 100 μm or less, 80 μm or less, or 70 μm or less. Within the above coating thickness range, the adherends such as the seed crystal 110 and the support 120 can be stably adhered, and the seed crystal and the support can be appropriately separated only partially in the subsequent step.

[0220] When the seed crystal adhesive layer 100 (seed crystal adhesive layer before carbonization) in the lamination step is in the form of a film layer, the seed crystal adhesive layer which is the film layer can be provided by subjecting the seed crystal adhesive layer which is the coating layer to a curing heat treatment.

[0221] The curing heat treatment temperature may be 100° C. to 450° C., 120° C. to 420° C., or 150° C. to 420° C. The heat treatment time may be 1 hour to 10 hours.

[0222] If the heat treatment temperature is less than 100° C., the degree of crosslinking of the seed crystal adhesive layer in the form of a film layer may be insufficient, and if the heat treatment temperature is more than 450° C., the degree of volume change of the seed crystal adhesive layer in the form of a film layer may decrease in the subsequent process.

[0223] As shown in FIG. 3, the seed crystal adhesive layer 100 may be formed on a support 120, and a seed crystal 110 may be placed on the seed crystal adhesive layer to provide a laminate.

[0224] The support 120 may be a seed crystal holder or may be a lid 140 for the reaction vessel.

[0225] The support 120 may be formed separately from or integrally with the lid 140 of the reaction vessel.

[0226] In conventional methods, a pressurizing step may be applied when manufacturing a laminate including an adhesive layer interposed between a seed crystal and a support, but the method for manufacturing a laminate according to one embodiment can omit the pressurizing step.

[0227] The carbonization step is a step of subjecting the uncarbonized seed crystal adhesive layer 100 to a carbonization heat treatment to provide a laminate including a carbonized seed crystal adhesive layer.

[0228] The carbonization heat treatment temperature of the carbonization step may be 500° C. or more, or 600° C. or more. The carbonization heat treatment temperature may be 900° C. or less, or 800° C. or less. Within the carbonization heat treatment temperature range, the seed crystal adhesion layer 100 can be easily carbonized and energy waste can be minimized.

[0229] The carbonization step can be carried out in an inert gas atmosphere such as argon or nitrogen, at a pressure of 1 torr to 750 torr for 1 hour to 10 hours.

[0230] The method may further include a cooling step of cooling the laminate after the carbonization step, and the laminate may be cooled to room temperature of 20°C to 30°C.

[0231] The carbonization step may further include a heat treatment step.

[0232] The heat treatment step is a step of producing a laminate including a graphitized seed crystal adhesion layer by subjecting the laminate to a graphitization heat treatment at a temperature of 2000° C. or higher.

[0233] The temperature of the heat treatment step may be 2000° C. or more, 2200° C. or more, or 2300° C. or more. The temperature may be 2600° C. or less, or 2500° C. or less. In the above temperature range, graphitization of the seed crystal adhesion layer can be effectively performed.

[0234] The heat treatment step may be performed in an inert atmosphere at a pressure of 1 torr to 200 torr and at a temperature rise rate of 1°C / min to 10°C / min for 1 hour to 100 hours. The heat treatment step may be performed at a pressure of 10 torr to 50 torr and at a temperature rise rate of 5°C / min to 10°C / min for 5 hours to 48 hours. Within the above temperature, pressure and temperature rise rate ranges, the graphitization treatment of the seed crystal adhesion layer 100 can be performed more efficiently.

[0235] The seed crystal adhesive layer 100 graphitized in the heat treatment step may have a first surface and a second surface, and may have a bonding surface bonded to an adherend. The first surface is one surface of the graphitized seed crystal adhesive layer, and the second surface is the other surface of the graphitized seed crystal adhesive layer.

[0236] The seed crystal bonding layer graphitized in the heat treatment step may have a bonding surface bonded to the opposing surface, and the bonding surface may include a first bonding surface and a second bonding surface.

[0237] The first bonding surface is a bonding surface that is in contact with a surface opposite to the first surface, and may be a bonding surface where the first surface and one surface of the support are in direct contact with each other.

[0238] The second bonding surface is a surface that directly contacts one surface of the seed crystal that faces the second surface.

[0239] When the sum of the areas of the first and second bonding surfaces is equal to or smaller than a predetermined multiple of the sum of the areas of the first and second surfaces, it can be considered that partial separation has occurred.

[0240] The sum of the areas of the first and second bonding surfaces may be 0.95 times or less than the sum of the areas of the first and second surfaces, or 0.90 times or less. The sum of the areas of the first and second bonding surfaces may be 0.77 times or less than the sum of the areas of the first and second surfaces.

[0241] The sum of the area of ​​the first bonding surface and the area of ​​the second bonding surface may be 0.30 times or more, or 0.45 times or more, the sum of the area of ​​the first surface and the area of ​​the second surface.

[0242] When the sum of the area of ​​the first bonding surface and the area of ​​the second bonding surface is within the above range, when the seed crystal adhesive layer is applied to grow an ingot, stress between the ingot and the support that may occur due to thermal expansion (thermal contraction) during the growth and cooling of the ingot can be minimized, and an ingot of better quality can be provided.

[0243] After the heat treatment step, as shown in Fig. 8, due to shrinkage caused by graphitization of the seed crystal bonding layer 100 (Fig. 8(b)), partial separation (Figs. 8(c1) and (c2)) may occur between the support 120 and the seed crystal bonding layer and between the seed crystal 110 and the seed crystal bonding layer. This can minimize stress applied to the seed crystal and the ingot due to the difference in thermal expansion coefficient between the support and the seed crystal.

[0244] The heat treatment step may be performed simultaneously with a growing step of growing an ingot on one surface of the seed crystal, or the heat treatment step may be performed sequentially with graphitizing the seed crystal adhesion layer and growing the ingot.

[0245] The growing step may be performed by disposing the source material 300 in the lower part of the inner space of a reaction vessel and the stack in the upper part, with the other surface of the seed crystal of the stack facing the source material 300 .

[0246] An example of an ingot manufacturing apparatus is shown in schematic form in Fig. 4. Referring to Fig. 4, the reaction vessel may be surrounded and fixed by a heat insulating material 400, and the heat insulating material surrounding the reaction vessel may be located within a reaction chamber 420 such as a quartz tube. The temperature of the inner space of the reaction vessel may be controlled by a heating means 500 provided outside the heat insulating material and the reaction chamber.

[0247] The reaction vessel may be any suitable vessel for growing the silicon carbide ingot 130, and specifically, a graphite crucible may be used.

[0248] The reaction vessel may include a body including an internal space and an opening, and a lid corresponding to the opening and sealing the internal space. The lid may be configured such that the laminate is disposed on a surface facing the internal space of the reaction vessel, and one surface of a support 120 for the laminate may be in contact with the lid.

[0249] The growth step of the heat treatment step can be performed by heating the reaction vessel and the internal space of the reaction vessel by the heating means 500, and the growth of the ingot can be induced by depressurizing the internal space and injecting a predetermined amount of inert gas simultaneously with or separately from the heating.

[0250] The temperature, pressure, atmosphere and heating rate of the growth step of the heat treatment step may be the same as those described in the heat treatment step.

[0251] The ingot 130 manufactured through the growth step of the heat treatment step can simplify the cutting process for separating the ingot from the laminate. The separated ingot can be processed into wafers by external grinding using an external grinding device, slicing to a certain thickness, and then grinding the edge and grinding the surface, polishing, etc.

[0252] Wafers manufactured from the ingot may have a warp value of 55 μm or less, or an average warp value of 30 μm or less for wafers manufactured from the ingot. An ingot having such characteristics can be used to manufacture wafers with excellent physical properties. The warp value can be measured by applying the method described in the following experimental examples.

[0253] The method for manufacturing the laminate may further include a cooling step of cooling the laminate manufactured in the heat treatment step.

[0254] The cooling step can be carried out for 24 to 48 hours at a cooling rate of 1° C. / min to 10° C. / min. The cooling step can be carried out in a state where the pressure in the internal space is increased to 700 torr to 800 torr.

[0255] The Sg value in formula 2 and the Vr value in formula 1 in the manufacturing method of the laminate are as described in the explanation of the seed crystal adhesion layer 100, and the measurement process is as described in the experimental example section below, but is not limited thereto.

[0256] The laminate manufactured by the laminate manufacturing method has a seed crystal bonding layer 100 having the specific Vr and Sg values, and partial separation between the adherends occurs due to shrinkage of the seed crystal bonding layer. When the heat treatment step of the laminate manufacturing method includes an ingot growth step, an ingot of excellent quality can be manufactured.

[0257] Laminate A laminate according to another embodiment includes: The substrate includes a seed crystal adhesion layer 100 having a first side and a second side; a support 120 having one side positioned above the first side; and a seed crystal 110 positioned below the second side.

[0258] The first surface and one surface of the support may face each other.

[0259] The second surface and one surface of the seed crystal 110 may be in contact with each other.

[0260] The carbonized seed crystal adhesive layer is obtained by carbonizing the seed crystal adhesive layer before carbonization.

[0261] The seed crystal adhesive layer before carbonization may be a seed crystal adhesive layer that is a coating layer or a film layer.

[0262] The carbonized seed crystal bonding layer is graphitized by heat treatment at a temperature of 2000° C. or higher to form a graphitized seed crystal bonding layer.

[0263] The change in area of ​​the seed crystal adhering layer is the difference between the area of ​​the graphitized seed crystal adhering layer and the area of ​​the seed crystal adhering layer before carbonization.

[0264] The change in area of ​​the seed crystal 110 is the change in area of ​​one surface of the seed crystal before and after the heat treatment.

[0265] The change in area of ​​the support 120 is the change in area of ​​one surface of the support before and after the heat treatment.

[0266] The change in area of ​​the seed crystal adhesion layer 100 can be greater than the change in area of ​​the seed crystal or the change in area of ​​the support.

[0267] In the graphitized seed crystal adhesion layer 100, a part of the first surface or a part of the second surface is separated from the adjacent surface.

[0268] After heat treatment at 2000°C or higher, the change in area of ​​the seed crystal adhesion layer 100 measured at room temperature compared to the area of ​​the seed crystal adhesion layer before the heat treatment may be greater than the change in area of ​​the support 120 or the change in area of ​​the seed crystal 110.

[0269] After the seed crystal bonding layer 100 is heat-treated at 2000° C. or higher, a part of the first surface or a part of the second surface is separated from the adjacent surface without being directly bonded thereto.

[0270] Specifically, the seed crystal adhesive layer 100 before the heat treatment at 2000° C. or higher may be a seed crystal adhesive layer before carbonization, and the seed crystal adhesive layer after the heat treatment is a graphitized seed crystal adhesive layer.

[0271] The change in area of ​​the seed crystal bonding layer 100 is the difference between the area of ​​the graphitized seed crystal bonding layer and the area of ​​the seed crystal bonding layer before carbonization.

[0272] The change in area of ​​the seed crystal bonding layer 100 may be the area of ​​the seed crystal bonding layer before carbonization minus the area of ​​the graphitized seed crystal bonding layer.

[0273] The seed crystal adhesive layer 100 before carbonization may be a seed crystal adhesive layer that is a coating layer, or a seed crystal adhesive layer that is a film layer.

[0274] The seed crystal adhesion layer 100 may be heat-treated at 2000° C. or more, cooled to room temperature, and graphitized to reduce its area.

[0275] The specific description of the seed crystal 110, the support 120 and the characteristics thereof are the same as the description of the seed crystal and the support described as the adherend in the description of the seed crystal adhesion layer and the manufacturing method thereof.

[0276] The surface of the support 120 in contact with the first surface may have a thermal expansion coefficient of 6 or less at 293.15 to 473.15 K, and the explanation related to the thermal expansion coefficient of the support or the surface in contact with the first surface is the same as the explanation for the adherend described above.

[0277] The surface of the seed crystal 110 in direct contact with the second surface may have a thermal expansion coefficient of 4 or less at 293.15 to 473.15 K. A more detailed explanation related to the thermal expansion coefficient of the seed crystal or the surface in contact with the second surface is the same as the explanation for the adherend described above.

[0278] The stack may include an ingot 130 grown from the other side of the seed crystal 110 .

[0279] The seed crystal adhesion layer 100 may be a seed crystal adhesion layer before carbonization.

[0280] Specific descriptions such as the seed crystal adhesive layer 100 before carbonization and the weight supported by the seed crystal adhesive layer before carbonization are the same as those described above.

[0281] The carbonized seed crystal adhesive layer 100 may be obtained by subjecting the seed crystal adhesive layer before carbonization to a carbonization heat treatment, and may have substantially no bubbles formed on its surface.

[0282] The seed crystal adhesion layer 100 may be the graphitized seed crystal adhesion layer after the graphitization heat treatment.

[0283] The specific description of the graphitization and the graphitized seed crystal adhesion layer 100 is as described above.

[0284] As described above, the area of ​​the graphitized seed crystal bonding layer 100 may decrease during the heat treatment and the cooling process after the heat treatment.

[0285] The seed crystal adhesive layer 100 may have bonding surfaces bonded to opposing surfaces that are in direct contact with each other. The first bonding surface is a surface where the first surface is in direct contact with one surface of the support 120, and the second bonding surface is a surface where the second surface is in direct contact with one surface of the seed crystal 110. The characteristics, such as the sum of the first bonding surface and the second bonding surface being 0.95 times or less of the sum of the first surface and the second surface, are as described above.

[0286] The seed crystal bonding layer 100 may have the above-mentioned Vr, Sg, and Vg characteristics, the specific description of which is as described above.

[0287] The seed crystal adhesive layer 100 may have a thickness of 3 μm or more, and the thickness of the seed crystal adhesive layer and the like are as described above.

[0288] The specific details of the area of ​​the seed crystal 110, the area of ​​the support 120, the area of ​​the seed crystal adhesion layer 100, etc. are as described above.

[0289] The specific details of the roughness of the seed crystal 110 and the roughness of the support 120 are as described above.

[0290] Ingot manufacturing method A method for producing an ingot according to another embodiment includes the steps of: A preparation step of disposing the source material and the laminate facing each other in a reaction vessel having an internal space; a growing step of sublimating the source material by adjusting the temperature, pressure and gas atmosphere of the inner space to provide an ingot grown from the laminate; and a cooling step of cooling the reaction vessel to recover the ingot or a stack including the ingot.

[0291] When the ingot is a silicon carbide ingot, the source material may include any one selected from the group consisting of carbon, silicon, silicon carbide, and combinations thereof.

[0292] The ingot may further include a dopant in the raw material, and the dopant may be any material that can be used as a dopant without any limitations.

[0293] The specific description of the configuration of the laminate and the features of each component is as described above.

[0294] The preparation of the laminate in the preparation step can be performed by a method such as the lamination step of the above-mentioned laminate manufacturing method, or the lamination step and the carbonization step.

[0295] The temperature, pressure and gas atmosphere in the internal space in the growing step are as described above.

[0296] The explanation of the stack further including the ingot in the cooling step, the explanation of the cooling rate, etc. are the same as those described above.

[0297] The area of ​​the graphitized seed crystal bonding layer may be reduced by 8.5% or more based on the area of ​​the seed crystal bonding layer before carbonization of the laminate. When the area is reduced in this manner, the seed crystal bonding layer is partially separated from the ingot or the seed crystal including the ingot, thereby minimizing the influence of stress that may occur during thermal expansion and thermal contraction, and an ingot having better physical properties can be manufactured.

[0298] The specific description of the ingot is as described above.

[0299] The ingot may be a silicon carbide ingot.

[0300] The ingot may be a silicon carbide single crystal ingot.

[0301] By applying the seed crystal adhesion layer, the laminate, and the like, a higher quality silicon carbide ingot can be provided.

[0302] Wafer and method for manufacturing the same A method for manufacturing a wafer according to another embodiment includes the steps of: a grinding step of grinding an edge of the ingot 130 produced by the ingot production method; and a sawing step of sawing the ground ingot to provide wafers.

[0303] The grinding step may involve grinding from the edge of the ingot 130 inwardly to remove 5% or more of its cross-sectional area.

[0304] The grinding step can be performed by grinding the silicon carbide ingot from its bottom surface where the seed crystal and the ingot 130 contact, toward the other surface, which is the surface of the growth termination portion, and toward the central axis, so as to have a uniform cross section.

[0305] The cutting step can cut the ingot so as to have a predetermined off angle with respect to the bottom surface or the (0001) plane of the ingot.

[0306] The off angle of the cutting step may be 0° to 10°.

[0307] The cutting step may be performed so that the thickness of the wafer is 300 μm to 600 μm.

[0308] The method for manufacturing the wafer may further include a planarization step of planarizing a thickness of the wafer provided after the cutting step.

[0309] The method for manufacturing the wafer may further include a grinding step of grinding the edge of the wafer, which is provided after the cutting step.

[0310] The method for manufacturing the wafer may further include a surface treatment step of etching and polishing the surface of the wafer provided after the cutting step.

[0311] The planarizing step, grinding step and surface treatment step may be performed in a suitable order according to a conventional method, and may be performed in the order of planarizing step-grinding step-surface treatment step.

[0312] The method for producing a wafer may be a method for producing a silicon carbide wafer.

[0313] The ingot may be a silicon carbide ingot, and may be a substantially single crystal silicon carbide ingot.

[0314] The wafer may be a silicon carbide wafer.

[0315] The silicon carbide wafer has the characteristics described below.

[0316] The silicon carbide wafer may have an off angle of -1.5° to +1.5° with respect to a reference angle, -1.0° to +1.0° with respect to the reference angle, -0.1° to +0.1° with respect to the reference angle, or -0.05° to +0.05° with respect to the reference angle, based on a wafer having an off angle of any one angle selected from 0° to 10° with respect to the (0001) plane.

[0317] A silicon carbide wafer having an off angle of 0° with respect to the (0001) plane may have a rocking angle of -1.0° to +1.0° with respect to a reference angle, -0.5° to +0.5° with respect to a reference angle, -0.1° to +0.1° with respect to a reference angle, or -0.05° to +0.05° with respect to a reference angle. An ingot having such characteristics has excellent crystalline properties.

[0318] A silicon carbide wafer having an off angle of 4° with respect to the (0001) plane may have a rocking angle of -1.0° to +1.0° with respect to a reference angle, -0.5° to +0.5° with respect to a reference angle, -0.1° to +0.1° with respect to a reference angle, or -0.05° to +0.05° with respect to a reference angle. An ingot having such characteristics has excellent crystalline properties.

[0319] A silicon carbide wafer having an off angle of 8° with respect to the (0001) plane may have a rocking angle of -1.0° to +1.0° with respect to a reference angle, -0.5° to +0.5° with respect to a reference angle, -0.1° to +0.1° with respect to a reference angle, or -0.05° to +0.05° with respect to a reference angle. An ingot having such characteristics has excellent crystalline properties.

[0320] The rocking angle, the meaning of the off angle being X°, the meaning of the rocking angle being "-1 to +1° with respect to the reference angle", the omega angle and how to handle them may be the same as those described above.

[0321] The present invention will be described in more detail with reference to the following specific examples. The following examples are merely illustrative for the purpose of aiding understanding of the present invention, and are not intended to limit the scope of the present invention.

[0322] Preparation of seed crystal adhesion layer and graphitized seed crystal adhesion layer Adhesive resin: polyacrylic resin, polyacrylonitrile resin, phenol resin, and trimethylsilyl ether group-containing cresol novolak resin as shown in the following chemical formula 1 were included.

[0323] [ka]

[0324] (In the above Chemical Formula 1, n is an integer of 1 to 1000.)

[0325] Filler: Average particle size (D 50 ) was 400 nm in diameter.

[0326] Solvents: dimethylformamide and ethanol.

[0327] Preparation of liquid adhesive composition: Adhesive resin compositions were prepared by mixing the adhesive resins to have the ratio and solid content shown in Table 1. In the case of phenolic resin, liquid phenolic resin was used.

[0328] 3, the liquid composition was applied by spin coating onto the support 120 or the seed crystal 110 in the thickness and area shown in Table 1, and then heat-treated in a muffle furnace at the temperature shown in Table 1. The support 120 used had a surface roughness (Ra) of 0.1 to 5 μm, and the seed crystal 110 used had a surface roughness (Ra) of 0.01 to 5 nm.

[0329] Preparation of graphitized seed crystal adhesive layer: The prepared seed crystal adhesive layer was graphitized in an induction heating furnace at a temperature corresponding to the conditions in Table 1.

[0330] Silicon carbide ingot growth As shown in Fig. 4 as an example of a silicon carbide ingot manufacturing apparatus, a silicon carbide raw material 300 was charged into the lower part of the internal space of a reaction vessel. The liquid composition used in manufacturing the seed crystal bonding layer 100 was interposed between a support 120 and a 6-inch 4H silicon carbide seed crystal 110 to a thickness of 10 µm, and the liquid composition was formed into a film at a temperature of 250°C in a muffle furnace to provide a laminate. This was heat-treated at a temperature of 600°C to provide a laminate in which the seed crystal bonding layer was carbonized.

[0331] The stacked body was placed in the upper part of the internal space of a reaction vessel, with the C-plane ((000-1) plane) of the silicon carbide seed crystal of the stacked body facing the silicon carbide raw material in the lower part of the internal space.

[0332] The reaction vessel was sealed and its exterior was surrounded by a heat insulating material 400, and then the reaction vessel was placed in a reaction chamber 420 equipped with a heating coil as a heating means 500.

[0333] The internal space of the reaction vessel was depressurized to adjust to a vacuum atmosphere, and argon gas was injected to make the internal space reach atmospheric pressure, after which the internal space was depressurized again and the temperature of the internal space was increased to 2200-2600°C at a heating rate of 5-10°C / min.

[0334] A silicon carbide ingot was grown on the silicon carbide seed crystal surface facing the silicon carbide raw material for 100 hours under a pressure condition of 5 torr, and then cooled to 25°C at a cooling rate of 10°C / min in an argon gas atmosphere of 5 to 760 torr.

[0335] Measurement and evaluation method of seed crystal adhesion layer and laminate 1) Sg: The original area A1 of the seed crystal bonding layer was measured under the conditions in Table 1, and the area A2 of the silicon carbide ingot after graphitization heat treatment and cooling to room temperature was measured under the manufacturing conditions thereof, and this was applied to Equation 2 to calculate.

[0336] 2) Thickness change: The thickness of the seed crystal adhesive layer was measured under the conditions in Table 1, and the thickness was measured after the silicon carbide ingot was graphitized under the manufacturing conditions and cooled to room temperature, and the thickness change was calculated. The thickness was measured using a dial gauge.

[0337] 3) Vr: The original volume V1 of the seed crystal bonding layer and the volume V2 of the silicon carbide ingot after being subjected to the graphitization heat treatment and cooled to room temperature under the manufacturing conditions thereof were calculated using the area value of 1) and the thickness of 2), and were calculated by applying the calculated volume to Equation 1.

[0338] 4) Vg: Calculated by applying the V1 and V2 values ​​in 3) above to Equation 3 above.

[0339] 5) Bonding area after graphitization: The degree of the gap between the seed crystal bonding layer and the adherend (support, seed crystal) cooled after the graphitization heat treatment under the manufacturing conditions of the silicon carbide ingot was measured using a 0.02 mm gap gauge.

[0340] Physical property evaluation of wafers produced from silicon carbide ingots 1) Evaluation of warp value: Using AutoScan 200 from MTI Instruments, Inc., the ingot was cut into individual parts (the distance when the seed crystal surface is viewed as No. 0), and the warp value of the wafer to which an off angle of 4° was applied was measured.

[0341] 2) Evaluation of wafer surface: A high-resolution X-ray diffraction analysis system (HR-XRD system, Rigaku's SmartLab High Resolution X-ray Diffraction System) was used to prepare a wafer with an off-angle of 4° based on the (0001) plane of the ingot, and the [11-20] direction of the wafer was aligned with the X-ray path. The X-ray source optic and X-ray detector optic angles were set to 2θ (35 to 36°), and the omega (ω, or theta θ, X-ray detector optic) angle was adjusted according to the off-angle of the wafer to perform measurement. Specifically, the omega angle was 17.8111° based on 0° off, the omega angle was 13.811° based on 4° off, and the omega angle was 9.8111° based on 8° off. The X-ray power was 9kW, the X-ray target was Cu, and the Goniometer resolution was 0.0001°. The full width at half maximum (FWHM) of the rocking curve was measured based on the angle at maximum intensity, and each was evaluated in arcsec. Measurements were performed at 167 points at intervals of 10 mm on the surface of the wafer. The results are shown in FIG.

[0342] [Table 1] (PAA: polyacrylic acid, PAN: polyacrylonitrile, TMSCN: cresol novolac containing trimethylsilyl ether groups, the amount of filler added is the value assuming the entire liquid composition containing the adhesive resin as 100% by weight.)

[0343] [Table 2] (Partial separation: After heat treatment (growth step), the bonding surface between the graphitized seed crystal adhesive layer and the adherend is 95% or less of the cross-sectional area of ​​the graphitized seed crystal adhesive layer. Average wafer warpage (μm): 30 or less is good, 31 to 59 is normal, 60 or more is bad. "-" indicates that it was not measured.)

[0344] Referring to Tables 1 and 2, the samples using acrylic resin, acrylic resin with added filler, phenolic resin without added filler, and cresol novolac resin had Sg values ​​of 9.12% to 27.2% and Vr values ​​of 28.1% to 30.0%, respectively. % / mm 3 ~152.7 % / mm 3 The samples using phenol resin and cresol novolac resin with 2% by weight of filler added when the entire liquid composition is considered to be 100% by weight showed Sg value of 8.42% or less and Vr value of 27.8% or less. % / mm 3 The following is shown.

[0345] For samples using acrylic resin with a solid content of 18 to 22 wt% to which filler was added, the Sg value was 16.42% to 21.08% and the Vr value was 53.7%. % / mm 3 ~64.1 % / mm 3 The average warpage value of the wafers manufactured from the ingots subjected to the above conditions was good.

[0346] In addition, the Sg value is 8.42% or less, and the Vr value is 27.8 % / mm3 When the seed crystal adhesive layer described below was applied, the ingot (seed crystal) was not partially separated from the adherend (seed crystal, support). However, in the examples, the bonding area between the graphitized seed crystal adhesive layer and the adherend was 95% or less of the bonding area before the graphitization heat treatment, confirming that partial separation occurred.

[0347] 6 is a graph showing the warpage of wafers according to the relative distance (wafer no.) from the seed crystal when cutting the wafers from the manufactured ingots. Referring to FIG. 6, the wafers manufactured from the ingots grown under the conditions of Comparative Example 3(a) had an average warp value of 98 μm or more, and the wafers manufactured from the ingot part (wafer no. 2) near the seed crystal had a warp value of 140 μm or more. The wafers manufactured from the ingots grown under the conditions of Example 10(b) had a warp value of 45 μm or less and an average warp value of 30 μm or less for the ingot part (wafer no. 2) near the seed crystal.

[0348] FIG. 7 is a photograph showing the results of XRD mapping of the wafer in Comparative Example 3(a) and Example 10(b). The intervals of the squares on the x-axis and y-axis in FIG. 7 are 10 mm, respectively. Referring to FIG. 7, the wafer (Wafer No. 8) cut from the ingot manufactured under the conditions of Comparative Example 3(a) at a distance of 5 mm from the seed crystal surface showed a maximum value of 153.7 arcsec, a minimum value of 42.9 arcsec, and an average value of 63.5 arcsec, and the curvature was 14.3 m. The wafer (Wafer No. 8) cut from the ingot manufactured under the conditions of Example 10(b) at a distance of 5 mm from the seed crystal surface showed a maximum value of 106.9 arcsec, a minimum value of 19.7 arcsec, and an average value of 27.1 arcsec, and the curvature was -19.1 m, and it can be seen that the wafers manufactured from Example 10 are of good quality.

[0349] That is, it was confirmed that the ingots and wafers manufactured by applying a seed crystal adhesion layer satisfying a specific Vr value are excellent in quality.

[0350] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the appended claims also fall within the scope of the present invention. [Explanation of symbols]

[0351] 10 Conventional seed crystal adhesion layer 100 seed crystal adhesive layer 110 Seed Crystal 120 Support 130 Ingot, Silicon carbide ingot 131 Polycrystalline, silicon carbide polycrystalline 140 Lid 300 Raw materials, silicon carbide raw materials 400 Insulation 420 Reaction Chamber 500 Heating means

Claims

1. Vr is expressed by the following formula 1, and is 28% / mm 3 ~154.5% / mm 3 A seed crystal adhesion layer having a Vr value of [Formula 1] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at 25°C, [Formula 2] In the formula 2, A1 is the area (mm 2 ) and A2 is the area of ​​the graphitized seed crystal adhesion layer (mm 2 ) measured at 25°C, The graphitized seed crystal adhesive layer is obtained by heat-treating the seed crystal adhesive layer before carbonization in an inert atmosphere at a pressure of 10 torr to 50 torr, at a temperature increase rate of 5° C. / min to 10° C. / min, and at a temperature of 2400° C. to 2600° C. for 1 hour to 100 hours; The area and volume of the graphitized seed crystal adhesive layer are based on those measured at a temperature of 25° C. after a cooling process, and the cooling process is performed on the graphitized seed crystal adhesive layer at a cooling rate of 5° C. / min to 10° C. / min under an argon or nitrogen atmosphere of 5 to 750 torr; The graphitized seed crystal adhesion layer has a thickness of 1.97 g / cm 2 Supports a weight of more than One surface of the adherend to which the seed crystal adhesion layer is adhered has a surface roughness (Ra) of 5 μm or less and 0.01 nm or more; The thermal expansion coefficient of the adherend (×10 -6 / °C) is 6 or less from 293.15K to 473.15K.

2. 2. The seed crystal adhesion layer of claim 1, wherein the Sg value is 8.5% or greater.

3. The seed crystal adhesion layer before carbonization was 1.69 g / cm 2 The seed crystal adhesion layer of claim 1 , which supports a weight of at least

4. 2. The seed crystal adhesion layer according to claim 1, wherein Vg is represented by the following formula 3 and has a Vg value of 56% or more: [Formula 3] In the formula 3, V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at 25°C, The graphitized seed crystal adhesive layer is obtained by heat-treating the seed crystal adhesive layer before carbonization in an inert atmosphere at a pressure of 10 torr to 50 torr, at a temperature increase rate of 5° C. / min to 10° C. / min, and at a temperature of 2400° C. to 2600° C. for 1 hour to 100 hours; The volume of the graphitized seed crystal adhesive layer is based on the volume measured at a temperature of 25° C. after a cooling process, and the cooling process is performed on the graphitized seed crystal adhesive layer at a cooling rate of 5° C. / min to 10° C. / min under an argon or nitrogen atmosphere of 5 to 750 torr; The graphitized seed crystal adhesion layer has a thickness of 1.97 g / cm 2 Supports a weight of more than One surface of the adherend to which the seed crystal adhesion layer is adhered has a surface roughness (Ra) of 5 μm or less and 0.01 nm or more; The thermal expansion coefficient of the adherend (×10 -6 / °C) is 6 or less from 293.15K to 473.15K.

5. 10. The seed crystal adhesion layer of claim 1, comprising: i) an adhesive resin; or ii) an adhesive resin and a filler.

6. The seed crystal adhesive layer according to claim 5, wherein the adhesive resin has a residual carbon amount of 5 to 50% by weight.

7. The seed crystal adhesion layer before carbonization has an area of ​​7.85 × 10 3 mm 2 The seed crystal adhesion layer according to claim 1 .

8. The graphitized seed crystal adhesion layer has an area of ​​5.50×10 3 mm 2 The seed crystal adhesion layer according to claim 1 .

9. A lamination step of providing a seed crystal adhesive layer before carbonization on one surface of a support or one surface of a seed crystal, and providing a laminate including the seed crystal adhesive layer interposed between the support and the seed crystal; A carbonization step of subjecting the seed crystal adhesive layer before carbonization to a carbonization heat treatment so that the laminate includes a carbonized seed crystal adhesive layer; The seed crystal adhesion layer has a Vr value represented by the following formula 1 of 28% / mm 3 A method for producing a laminate, the method comprising the steps of: [Formula 1] In the above formula 1, Sg (%) is the value of the following formula 2, and V1 is the volume (mm 3 ) and V2 is the volume of the graphitized seed crystal adhesion layer (mm 3 ) measured at 25°C, [Formula 2] In the formula 2, A1 is the area (mm 2 ) and A2 is the area of ​​the graphitized seed crystal adhesion layer (mm 2 ) measured at 25°C, The graphitized seed crystal adhesive layer is obtained by heat-treating the seed crystal adhesive layer before carbonization in an inert atmosphere at a pressure of 10 torr to 50 torr, at a temperature increase rate of 5° C. / min to 10° C. / min, and at a temperature of 2400° C. to 2600° C. for 1 hour to 100 hours; The area and volume of the graphitized seed crystal adhesive layer are based on those measured at a temperature of 25° C. after a cooling process, and the cooling process is performed on the graphitized seed crystal adhesive layer at a cooling rate of 5° C. / min to 10° C. / min under an argon or nitrogen atmosphere of 5 to 750 torr; The graphitized seed crystal adhesion layer has a thickness of 1.97 g / cm 2 Supports a weight of more than One surface of the adherend to which the seed crystal adhesion layer is adhered has a surface roughness (Ra) of 5 μm or less and 0.01 nm or more; The thermal expansion coefficient of the adherend (×10 -6 / °C) is 6 or less at 293.15K to 473.15K.

10. The method for producing a laminate according to claim 9, wherein the carbonization heat treatment is carried out at a temperature of 500°C to 900°C.

11. Further comprising a heat treatment step after the carbonization step, 10. The method for producing a laminate according to claim 9, wherein the heat treatment step is a step of subjecting the laminate to a graphitization heat treatment at a temperature of 2400°C to 2600°C so that the laminate includes a graphitized seed crystal adhesion layer.

12. The method for manufacturing a laminate according to claim 11 , wherein the heat treatment step includes a process of growing an ingot on one surface of the seed crystal.

13. the graphitized seed crystal adhesion layer includes a first surface and a second surface opposed to one another; the graphitized seed crystal bonding layer having a first bonding surface and a second bonding surface bonded to opposing surfaces; the first bonding surface is a bonding surface where the first surface is in contact with a surface opposite to the first surface, the second bonding surface is a bonding surface where the second surface is in contact with a surface opposite to the second surface, the surface opposite to the second surface is one surface of the seed crystal, The method for producing a laminate according to claim 9 , wherein a sum of an area of ​​the first bonding surface and an area of ​​the second bonding surface is 0.95 times or less of a sum of an area of ​​the first surface and an area of ​​the second surface.

14. A preparation step of disposing a raw material and a laminate manufactured according to claim 9 so as to face each other in a reaction vessel having an internal space; a growing step of sublimating the source material by adjusting a temperature, pressure and gas atmosphere of the inner space to provide an ingot grown from the laminate; a cooling step of cooling the reaction vessel to recover the ingot or a stack including the ingot; a grinding step of grinding the edge of the recovered ingot; and cutting the ground ingot to provide wafers.