Carbide and cutting tools
The cemented carbide composition with tungsten carbide and dispersed MxW1-xCyNy particles addresses the challenge of fracture resistance and breakage resistance during low-speed machining, improving tool performance in cutting tools.
Patent Information
- Application Number
- JP2021062899
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-04-01
AI Technical Summary
Cemented carbides used in cutting tools face challenges in providing excellent fracture resistance and breakage resistance during low-speed machining, particularly for small-diameter drills.
A cemented carbide composition comprising first hard phase particles of tungsten carbide and second hard phase particles of a solid solution represented by MxW1-xCyNy, where M is a metal element from Group 4, Group 5, chromium, or molybdenum, with specific atomic ratios and particle sizes, dispersed within a binder phase of iron or nickel, enhancing mechanical properties.
The cemented carbide exhibits improved fracture resistance and breakage resistance during low-speed machining, leading to enhanced tool life and performance in applications like small-diameter drills.
Smart Images

Figure 0007574719000002 
Figure 0007574719000003 
Figure 0007574719000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to hardmetals and cutting tools. [Background technology]
[0002] Conventionally, cemented carbide having a hard phase mainly composed of tungsten carbide (WC) and a binder phase mainly composed of an iron group element has been used as a material for cutting tools. In recent years, a technology has been developed to improve the wear resistance and chipping resistance of cemented carbide by further adding a second hard phase composed of a metal nitride (for example, International Publication No. WO 2017 / 191744 (Patent Document 1)). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 191744 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, work materials have become increasingly difficult to cut in cutting processes, and there is a demand for cemented carbide alloys that have excellent resistance to chipping and breakage even in low-speed cutting, particularly in the field of small-diameter drills.
[0005] Therefore, an object of the present disclosure is to provide a cemented carbide that, when used as a tool material, has excellent chipping resistance and breakage resistance even in low-speed machining. [Means for solving the problem]
[0006] The cemented carbide of the present disclosure is A cemented carbide comprising a hard phase and a binder phase, the hard phase comprises first hard phase particles and second hard phase particles; the first hard phase particles are made of tungsten carbide; The second hard phase particles are x W1-x C 1-y N y and M is at least one metal element selected from the group consisting of Group 4 elements, Group 5 elements, chromium, and molybdenum of the periodic table; The x is equal to or greater than 0.20 and equal to or less than 0.70, The y is equal to or greater than 0 and equal to or less than 0.90, the binder phase contains at least one iron group element selected from the group consisting of iron, cobalt, and nickel; The second hard phase particles have an area-based 50% cumulative number particle size of 0.1 μm or more and 1.0 μm or less, The second hard phase particles are present in a dispersed state and are a cemented carbide.
[0007] The cutting tool of the present disclosure is a cutting tool including the above-described cemented carbide. Effect of the Invention
[0008] When used as a tool material, the cemented carbide of the present disclosure can have excellent chipping resistance and breakage resistance even in low-speed machining. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a diagram illustrating a cross section of a cemented carbide according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram showing a method for line analysis of second hard phase particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. (1) The present disclosure relates to a cemented carbide having a hard phase and a binder phase, the hard phase comprises first hard phase particles and second hard phase particles; the first hard phase particles are made of tungsten carbide; The second hard phase particles are x W 1-x C 1-y N y and M is at least one metal element selected from the group consisting of Group 4 elements, Group 5 elements, chromium, and molybdenum of the periodic table; The x is equal to or greater than 0.20 and equal to or less than 0.70, The y is equal to or greater than 0 and equal to or less than 0.90, the binder phase contains at least one iron group element selected from the group consisting of iron, cobalt, and nickel; The second hard phase particles have an area-based 50% cumulative number particle size of 0.1 μm or more and 1.0 μm or less, The second hard phase particles are present in a dispersed state and are a cemented carbide.
[0011] When used as a tool material, the cemented carbide of the present disclosure can have excellent chipping resistance and breakage resistance even in low-speed machining.
[0012] (2) the x is equal to or greater than 0.40 and equal to or less than 0.70; The second hard phase particles preferably have an area-based 50% cumulative number particle size of 0.1 μm or more and 0.5 μm or less.
[0013] This further improves the chipping resistance and breakage resistance of the cemented carbide.
[0014] (3) The first hard phase particles preferably have an area-based 50% cumulative number grain size of 0.1 μm or more and 1.5 μm or less, which further improves the chipping resistance and breakage resistance of the cemented carbide.
[0015] (4) It is preferable that the cemented carbide does not contain either or both of chromium and vanadium, which further improves the chipping resistance and breakage resistance of the cemented carbide.
[0016] (5) The present disclosure relates to a cutting tool including the above-mentioned cemented carbide. The cutting tool of the present disclosure has excellent chipping resistance and breakage resistance even in low-speed machining.
[0017] [Details of the embodiment of the present disclosure] Specific examples of the cemented carbide and cutting tool of the present disclosure will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference numerals represent the same or corresponding parts. Furthermore, dimensional relationships such as length, width, thickness, and depth have been appropriately changed for clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.
[0018] In this specification, the expression "A to B" means the upper and lower limits of a range (i.e., A or more and B or less). When no unit is specified for A and a unit is specified only for B, the unit of A and the unit of B are the same.
[0019] In this specification, the "10% cumulative number particle size based on the area of the particles" is referred to as "D10", the "50% cumulative number particle size based on the area of the particles" is referred to as "D50", and the "90% cumulative number particle size based on the area of the particles" is referred to as "D90".
[0020] In this specification, when a compound is expressed by a chemical formula, unless the atomic ratio is specifically limited, it is intended to include any conventionally known atomic ratio and is not necessarily limited to the stoichiometric range. For example, when "WC" is written, the ratio of the number of atoms constituting WC includes any conventionally known atomic ratio.
[0021] [Embodiment 1: Carbide] <Cemented carbide> A cemented carbide according to one embodiment of the present disclosure (hereinafter also referred to as "the present embodiment") will be described with reference to Fig. 1. Fig. 1 is a diagram that illustrates a cross section of the cemented carbide according to the present embodiment. The cemented carbide of this embodiment is a cemented carbide having a hard phase and a binder phase 3, The hard phase has first hard phase particles 1 and second hard phase particles 2, The first hard phase particles 1 are made of tungsten carbide, The second hard phase particles 2 are M x W 1-x C 1-y N y and M is at least one metal element selected from the group consisting of Group 4 elements, Group 5 elements, chromium, and molybdenum of the periodic table; x is equal to or greater than 0.20 and equal to or less than 0.70; y is equal to or greater than 0 and equal to or less than 0.90, The binder phase 3 contains at least one iron group element selected from the group consisting of iron, cobalt, and nickel, The second hard phase particles 2 have an area-based 50% cumulative number particle size of 0.1 μm or more and 1.0 μm or less, The second hard phase particles are dispersed in the cemented carbide.
[0022] When used as a tool material, the cemented carbide of this embodiment can have excellent chipping resistance and breakage resistance even in low-speed machining.
[0023] <Hard phase> In the cemented carbide of this embodiment, the hard phase includes first hard phase particles and second hard phase particles.
[0024] <First hard phase particles> (Composition of first hard phase particles) The first hard phase particles are made of tungsten carbide (WC). Here, the first hard phase particles being made of tungsten carbide means that the first hard phase particles are substantially made of tungsten carbide. Specifically, the first hard phase particles preferably contain 99.9 mass% or more of tungsten carbide.
[0025] In addition to tungsten carbide, the first hard phase particles may contain inevitable impurity elements and trace amounts of impurity elements mixed in during the manufacturing process of WC, as long as the effects of the present disclosure are exhibited. Examples of these impurity elements include molybdenum (Mo) and chromium (Cr). The content of the impurity elements in the first hard phase particles (the total content when there are two or more types of impurity elements) is preferably less than 0.1 mass%. The content of the impurity elements in the first hard phase particles is measured by ICP (Inductively Coupled Plasma) emission spectrometry (measuring device: Shimadzu Corporation's "ICPS-8100" (trademark)).
[0026] (D50 of first hard phase particles) The first hard phase particles preferably have an area-based 50% cumulative number grain size (D50) of 0.1 μm or more and 1.5 μm or less, which improves the chipping resistance and breakage resistance of the cemented carbide.
[0027] The lower limit of D50 of the first hard phase particles is preferably 0.1 μm or more, and more preferably 0.2 μm or more. From the viewpoint of improving chipping resistance and breakage resistance, the upper limit of D50 of the first hard phase particles is preferably 1.5 μm or less, more preferably 1.2 μm or less, and even more preferably 1.0 μm or less. D50 of the first hard phase particles is preferably 0.1 μm or more and 1.5 μm or less, more preferably 0.2 μm or more and 1.2 μm or less, and even more preferably 0.2 μm or more and 1.0 μm or less.
[0028] The method for measuring the particle size of each first hard phase particle to calculate the D50 of the first hard phase particle is as follows. First, a sample having a smooth cross section is obtained by processing the cemented carbide with a CP (Cross Section Polisher) using an argon ion beam. The cross section is imaged at 10,000 times magnification using a field emission scanning electron microscope (FE-SEM) (measuring device: "JSM-7000F" (trademark) manufactured by JEOL Ltd.) to obtain an electron microscope image (SEM-BSE image) of the cross section.
[0029] The electron microscope image (SEM-BSE image) is subjected to EDX mapping by an energy dispersive X-ray spectrometer (EDX) attached to the field emission scanning electron microscope (FE-SEM), thereby identifying the first hard phase particles, the second hard phase particles, and the binder phase. In the EDX mapping image, the region where tungsten exists corresponds to the first hard phase particles. In the EDX mapping image, the region where at least one metal element selected from the group consisting of Group 4 elements, Group 5 elements, chromium, and molybdenum of the periodic table exists corresponds to the second hard phase particles. In this specification, the Group 4 elements of the periodic table include titanium (Ti), zirconium (Zr), and hafnium (Hf), and the Group 5 elements of the periodic table include vanadium (V), niobium (Nb), and tantalum (Ta). In the EDX mapping image, the region containing at least one iron group element selected from the group consisting of iron, cobalt, and nickel corresponds to the binder phase.
[0030] The electron microscope image is input to a computer, and image processing is performed using image analysis software ("Mac-View" (trademark) manufactured by Mountech Co., Ltd.), and the circle equivalent diameter (Heywood diameter: equivalent circle diameter with equal area) of each of all the first hard phase particles observed in the electron microscope image (SEM-BSE image) is calculated. The image processing conditions are as follows. (Image processing conditions) Particle shape: non-spherical Detection sensitivity: 5 Detection angle: 0.7 Scanning density: 7 x 1 High Cut: Disabled Low Cut: Inverted
[0031] In calculating the D50 of the first hard phase particles, 10 arbitrary electron microscope images (10 fields of view) are prepared for one cross section of the cemented carbide such that no overlapping portions are captured. The average of the D50 of the first hard phase particles in the 10 fields of view is defined as the D50 of the first hard phase particles in the cemented carbide.
[0032] As far as the applicant has measured, it has been confirmed that there is no variation in the results even if the measurement field of view is set arbitrarily.
[0033] D10, D50 and D90 of the second hard phase particles described below can also be calculated in the same manner as above by taking the second hard phase particles as the measurement subject in the above electron microscope image.
[0034] (Content of first hard phase particles) The content of the first hard phase particles in the cemented carbide of this embodiment is preferably 80 volume % or more and 99 volume % or less. When the content of the first hard phase particles in the cemented carbide is 80 volume % or more, the mechanical strength of the cemented carbide is improved. Here, "mechanical strength" means the mechanical strength including various properties of the cemented carbide such as wear resistance, chipping resistance, breakage resistance, and bending strength. When the content of the first hard elementary particles in the cemented carbide is 99 volume % or less, the toughness of the cemented carbide is improved. The content of the first hard phase particles in the cemented carbide is more preferably 83 volume % or more and 97 volume % or less, and further preferably 85 volume % or more and 95 volume % or less.
[0035] The content (volume %) of the first hard phase particles in the cemented carbide is measured as follows: The first hard phase particles, the second hard phase particles, and the binder phase are identified by performing EDX mapping on an electron microscope image (SEM-BSE image) of a cross section of a sample made of cemented carbide in the same manner as in the above-mentioned method for measuring the particle size of the first hard phase particles.
[0036] The electron microscope image is imported into a computer and image processing is performed using image analysis software (Mac-View (trademark) manufactured by Mountech Co., Ltd.). The area ratio of the first hard phase particles identified by the EDX mapping is measured using the entire measurement field (length 9 μm × width 12 μm) as the denominator. The image processing conditions are the same as those used in the measurement method for the particle size of the first hard phase particles. By regarding the area of the first hard phase particles as continuous in the depth direction of the cross section, the area ratio can be regarded as the content (volume %) of the first hard phase particles in the measurement field.
[0037] In the method for measuring the content of the first hard phase particles, five electron microscope images (five fields of view) are prepared for one cross section of the cemented carbide such that no overlapping imaged portions appear. The five fields of view are one field of view in the center of the cross section and four fields of view located above, below, left and right of the first field of view. The average of the contents of the first hard phase particles in the five fields of view is defined as the content (volume %) of the first hard phase particles in the cemented carbide.
[0038] As far as the applicant has measured, it has been confirmed that there is no variation in the results even if the measurement field of view is set arbitrarily.
[0039] The content (volume %) of the second hard phase particles and the content (volume %) of the binder phase in the cemented carbide described below can also be measured in the same manner as above by measuring the second hard phase particles and the binder phase in the above measurement field of view.
[0040] <Second hard phase particles> (Morphology, composition and atomic ratio of second hard phase particles) The second hard phase particles are M x W 1-x C 1-y N y Here, M is at least one metal element selected from the group consisting of Group 4 elements (titanium (Ti), zirconium (Zr), hafnium (Hf)) of the periodic table, Group 5 elements (vanadium (V), niobium (Nb), tantalum (Ta)), chromium (Cr) and molybdenum (Mo), x is 0.20 or more and 0.70 or less, and y is 0 or more and 0.90 or less. When the cemented carbide contains second hard phase particles and x and y are in the above ranges, the particle strength of the second hard phase particles is excellent and the interface strength between particles in the cemented carbide is excellent, so that the cemented carbide can have excellent chipping resistance and breakage resistance.
[0041] The above M is preferably at least one metal element selected from the group consisting of Ti, Zr, Hf, Nb, Ta and Mo. The above M is more preferably at least one metal element selected from the group consisting of Ti, Zr and Nb.
[0042] The above x is preferably 0.40 or more and 0.70 or less. This further improves the chipping resistance and breakage resistance of the cemented carbide. The above x is more preferably 0.41 or more and 0.69 or less, and even more preferably 0.42 or more and 0.68 or less.
[0043] From the viewpoint of making the second hard phase particles fine, the above y is 0 or more and 0.90 or less, preferably 0.20 or more and 0.80 or less, and more preferably 0.30 or more and 0.70 or less.
[0044] The composition of the second hard phase particles is not particularly limited, but examples thereof include TiWC, TiWCN, ZrWC, ZrWCN, NbWC, NbWCN, TiNbWC, and TiNbWCN.
[0045] The methods for measuring the morphology, composition and atomic ratio of the second hard phase particles are as follows (A1) to (H1). (A1) In a manner similar to the above-mentioned method for measuring the particle size of the first hard phase particles, the first hard phase particles, the second hard phase particles, and the binder phase are identified by performing EDX mapping on an electron microscope image (SEM-BSE image) of a cross section of a sample made of cemented carbide.
[0046] (B1) The second hard phase particles identified above are subjected to line analysis using an energy dispersive X-ray spectrometer (EDX) attached to a field emission scanning electron microscope (FE-SEM). The line analysis will be specifically described with reference to FIG. 2.
[0047] (C1) FIG. 2 is a diagram showing a method of line analysis of second hard phase particles. In FIG. 2, X indicates the center of gravity of the second hard phase particle, and a1 to a8 indicate measurement points. First, the above-mentioned electron microscope image is imported into a computer, and image processing is performed using image analysis software ("Mac-View" (trademark) manufactured by Mountec Co., Ltd.) to identify the center of gravity X of any one second hard phase particle. The image processing conditions are the same as the image processing conditions in the above-mentioned method for measuring the particle size of the first hard phase particle. Here, the center of gravity X is identified based on the shape of the second hard phase particle in the above-mentioned electron microscope image. An arbitrary line L1 passing through the center of gravity X is drawn. The intersections (measurement points) a1 and a8 of the outer edge of the second hard phase particle and the line L1 are identified. The positions (measurement points) a2 to a7 that divide the line segment connecting a1 and a8 into seven equal parts are identified.
[0048] (D1) EDX analysis is carried out at each of the measurement points a1 to a8, and the composition of the second hard phase particles and the proportion (atomic %) of each element at each measurement point are calculated.
[0049] (E1) At least one metal element (M x W 1-x C 1-y N y The maximum ratio of M max (atomic %) and minimum value M min (atomic %) and M max -M min When the content of the second hard phase particles is less than 40 atomic %, the morphology of the second hard phase particles is determined to be a solid solution.
[0050] (F1) The above judgment in (E1) is carried out for any 10 second hard phase particles. In this specification, when 6 or more of the 10 second hard phase particles are judged to be in a solid solution, it is judged that "in the cemented carbide, the morphology of the second hard phase particles is a solid solution", that is, "in the cemented carbide, the second hard phase particles are (M x W 1-x C 1-y N yIn the present specification, the term "hard alloy" refers to a hard alloy in which the second hard phase particles are composed of a solid solution represented by M x W 1-x C 1-y N y "The composition of the second hard phase particles in the cemented carbide is a solid solution represented by the formula: M x W 1-x C 1-y N y and the percentage of the number of second hard phase particles consisting of a solid solution to the total number of second hard phase particles in the cemented carbide is more than 50%.
[0051] (G1) The average value of the ratio of each element at the eight measurement points obtained in (D1) above is determined as the ratio of each element in the second hard phase particle, thereby specifying the composition of the second hard phase particle and the ratio of each element.
[0052] (H1) The composition of the second hard phase particles and the ratio of each element in (G1) above are specified for any 10 second hard phase particles. In this specification, the average value of the ratio of each element in the 10 second hard phase particles is defined as the ratio of each element in the second hard phase particles of the cemented carbide. This specifies the composition of the second hard phase particles and the ratio of each element in the cemented carbide.
[0053] As far as the applicant has measured, it has been confirmed that there is no variation in the results even if the measurement field of view is set arbitrarily.
[0054] The composition of tungsten carbide in the first hard phase particles and the composition of the binder phase described below can also be measured by the same method as above by measuring the first hard phase particles and the binder phase in the electron microscope image.
[0055] (D50 of second hard phase particles) The second hard phase particles have an area-based 50% cumulative number grain size (D50) of 0.1 μm or more and 1.0 μm or less, which improves the chipping resistance and breakage resistance of the cemented carbide.
[0056] The lower limit of D50 of the second hard phase particles is 0.1 μm or more, and can be 0.15 μm or more. From the viewpoint of improving chipping resistance and breakage resistance, D50 of the second hard phase particles is 1.0 μm or less, preferably 0.5 μm or less, more preferably 0.4 μm or less, and even more preferably 0.3 μm or less. D50 of the second hard phase particles is preferably 0.1 μm or more and 0.5 μm or less, more preferably 0.15 μm or more and 0.4 μm or less, and even more preferably 0.15 μm or more and 0.3 μm or less.
[0057] (D10 / D90 of second hard phase particles) The ratio D10 / D90 of the 10% cumulative number particle size (D10) to the 90% cumulative number particle size (D90) based on the area of the second hard phase particles is preferably 0.1 or more and 0.5 or less. This makes the particle size distribution of the second hard phase particles sharp, the second hard phase particles do not aggregate, and the structure of the cemented carbide becomes homogenous, improving the chipping resistance and breakage resistance. The D10 / D90 of the second hard phase particles is more preferably 0.1 or more and 0.4 or less.
[0058] The D10, D50 and D90 of the second hard phase particles can be calculated in the same manner as the above-mentioned method for measuring D50 of the first hard phase particles, by measuring the second hard phase particles in an electron microscope image.
[0059] (Dispersion state of second hard phase particles) In the cemented carbide of this embodiment, the second hard phase particles are dispersed. In this specification, "the second hard phase particles are dispersed in the cemented carbide" means that the second hard phase particles are uniformly dispersed in the cemented carbide without bias. Also, "the second hard phase particles are unevenly distributed in the cemented carbide" means that the second hard phase particles are unevenly distributed in the cemented carbide. A method for determining whether the second hard phase particles are dispersed or unevenly distributed in the cemented carbide will be described below. The determination method is as follows (A2) to (D2).
[0060] (A2) In the same manner as in the above-mentioned method for measuring the particle size of the first hard phase particles, EDX mapping is performed on an electron microscope image (SEM-BSE image) of a cross section of a sample made of cemented carbide to identify the first hard phase particles, the second hard phase particles, and the binder phase.
[0061] (B2) Next, in the above electron microscope image (9 μm×12 μm), a total of 48 unit regions R are provided by arranging six square unit regions R with sides of 1.5 μm in the vertical direction and eight in the horizontal direction.
[0062] (C2) The number of second hard phase particles identified by the EDX mapping present inside each unit region R is counted by performing image analysis using image analysis software (Mac-View (trademark) manufactured by Mountech Co., Ltd.). The image processing conditions are the same as those in the method for measuring the particle size of the first hard phase particles described above. When a second hard phase particle is present across two or more adjacent unit regions R, the second hard phase particle is counted as being included in the unit region R with the fewest number of second hard phase particles among the unit regions R that are across. In addition, when the shape of the second hard phase particle indicates that the second hard phase particle is formed by bonding two second hard phase particles, the number of the second hard phase particle is counted as one.
[0063] (D2) Next, the total number of second hard phase particles present inside a total of 48 unit regions R is counted, and the percentage of the number of second hard phase particles present inside each unit region R with respect to the total number is calculated.
[0064] Since a total of 48 unit regions R are provided in the above electron microscope image, when the second hard phase particles are uniformly dispersed in the cemented carbide without bias, the percentage of the number of the second hard phase particles in each unit region R is 2.08% (1 / 48×100%). In this specification, when the number of unit regions R in which the percentage of the number of the second hard phase particles in the unit region R is less than 0.5% or more than 5% among the total of 48 unit regions R is 14 or less, it is determined that the second hard phase particles are dispersed and present in the cemented carbide. On the other hand, when the number of unit regions R in which the percentage of the number of the second hard phase particles in the unit region R is less than 0.5% or more than 5% among the total of 48 unit regions R is 15 or more, it is determined that the second hard phase particles are unevenly distributed in the cemented carbide.
[0065] As far as the applicant has measured, it has been confirmed that there is no variation in the results even if the measurement field of view is arbitrarily set for the same measurement sample.
[0066] In the cemented carbide of this embodiment, out of a total of 48 unit regions R, the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% is 14 or less. That is, the second hard phase particles are dispersed in the cemented carbide. This improves the chipping resistance and breakage resistance of the cemented carbide.
[0067] Of the total 48 unit regions R, the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% is preferably 13 or less, more preferably 12 or less, and even more preferably 10 or less.
[0068] (Content of second hard phase particles) The content of the second hard phase particles in the cemented carbide of this embodiment is preferably 0.5 volume % or more and 3.0 volume % or less. When the content of the second hard phase particles in the cemented carbide is 0.5 volume % or more, the wear resistance is improved. When the content of the second hard elementary particles in the cemented carbide is 3.0 volume % or less, the strength is improved. The content of the second hard phase particles in the cemented carbide is more preferably 0.8 volume % or more and 2.5 volume % or less, and further preferably 1.0 volume % or more and 2.0 volume % or less.
[0069] The content (volume %) of second hard phase particles in the cemented carbide can be calculated in the same manner as the above-mentioned method for measuring the content (volume %) of first hard phase particles, by measuring the second hard phase particles in an electron microscope image.
[0070] <Binded phase> (Composition of the binder phase) The binder phase contains at least one iron group element selected from the group consisting of iron, cobalt, and nickel, and the content of the iron group element in the binder phase is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 98 mass% or more, and most preferably 100 mass%.
[0071] The binder phase may contain, other than the iron group elements, inevitable impurity elements mixed in from the first hard phase particles and the second hard phase particles, and trace amounts of impurity elements, etc., as long as the effect of the present disclosure is exhibited. Examples of these impurity elements include tungsten (W) and titanium (Ti). The content of the impurity elements in the binder phase (the total content when there are two or more kinds of impurity elements) is preferably less than 1 mass%. The content of the impurity elements in the binder phase is measured by ICP (Inductively Coupled Plasma) emission spectrometry (measuring device: Shimadzu Corporation's "ICPS-8100" (trademark)).
[0072] (Binder phase content) The content of the binder phase in the cemented carbide of this embodiment is preferably 0.5% by volume or more and 20% by volume or less. When the content of the binder phase in the cemented carbide is 0.5% by volume or more, the adhesive strength between the first hard phase particles, the second hard phase particles and the binder phase is improved, and the toughness of the cemented carbide is improved. When the content of the binder phase in the cemented carbide is 20% by volume or less, the hardness of the cemented carbide is improved. The content of the binder phase in the cemented carbide is more preferably 1% by volume or more and 18% by volume or less, and further preferably 5% by volume or more and 15% by volume or less.
[0073] The binder phase content (volume %) in the cemented carbide can be calculated in the same manner as the above-mentioned method for measuring the first hard phase particle content (volume %), by measuring the binder phase in an electron microscope image.
[0074] <Chromium and vanadium> The cemented carbide of this embodiment preferably does not contain either or both of chromium and vanadium. That is, the cemented carbide of this embodiment preferably does not contain chromium, or the cemented carbide of this embodiment preferably does not contain vanadium, or the cemented carbide of this embodiment preferably does not contain chromium and vanadium. Chromium carbide (Cr 3 C 2 ) and vanadium carbide (VC) have a grain growth inhibitory effect, and therefore have been used as grain growth inhibitors in the manufacture of conventional ultrafine cemented carbide. However, when chromium precipitates as carbide in the cemented carbide, it tends to become the starting point of breakage. In addition, vanadium in the cemented carbide exists at the interface between particles, so the strength of the cemented carbide tends to decrease. Therefore, when the cemented carbide does not contain one or both of chromium and vanadium, the fracture resistance and breakage resistance of the cemented carbide are improved. In addition, when the second hard phase particles contain one or both of chromium and vanadium, it is preferable that the binder phase does not contain one or both of chromium and vanadium in the region other than the second hard phase particles of the cemented carbide.
[0075] The chromium and vanadium contents in the cemented carbide are measured by ICP (Inductively Coupled Plasma) emission spectrometry (measuring device: Shimadzu Corporation's "ICPS-8100" (trademark)). In this specification, when the chromium content is below the detection limit in the ICP analysis, it is determined that "the cemented carbide does not contain chromium," and when the vanadium content is below the detection limit, it is determined that "the cemented carbide does not contain vanadium."
[0076] [Embodiment 2: Cutting tool] The cutting tool of this embodiment includes the above-mentioned cemented carbide. The cutting tool preferably includes a cutting edge made of the above-mentioned cemented carbide. In this specification, the cutting edge means a part involved in cutting, and in the cemented carbide, means a region surrounded by the cutting edge ridge and an imaginary surface that is 2 mm away from the cutting edge ridge to the cemented carbide side and is tangent to the cutting edge ridge.
[0077] Examples of cutting tools include cutting tools, drills, end mills, indexable cutting tips for milling, indexable cutting tips for turning, metal saws, gear cutting tools, reamers, taps, etc. In particular, the cutting tool of the present embodiment can exhibit excellent effects in the case of a small-diameter drill for machining printed circuit boards.
[0078] The cemented carbide of the present embodiment may constitute the entirety of these tools, or may constitute a part of them. Here, "constitute a part" refers to a mode in which the cemented carbide of the present embodiment is brazed to a predetermined position of any substrate to form a cutting edge.
[0079] The cutting tool of this embodiment may further include a hard film that covers at least a part of the surface of the substrate made of cemented carbide. Examples of the hard film include diamond-like carbon and diamond.
[0080] [Embodiment 3: Method for manufacturing a cemented carbide alloy] The cemented carbide of the embodiment 1 can be typically manufactured by carrying out the steps of preparing raw material powder, mixing, molding, sintering, and cooling in the above-mentioned order. Each step will be described below.
[0081] <Preparation process> The preparation step is a step of preparing raw material powders of all materials constituting the cemented carbide, including tungsten carbide powder, hydride powder of a metal element selected from the group consisting of Group 4 elements, Group 5 elements, chromium, and molybdenum in the periodic table (hereinafter also referred to as "metal hydride"), graphite powder, and iron group element powder.
[0082] (tungsten carbide powder) The average particle size of the tungsten carbide powder is preferably 0.1 μm or more and 1.5 μm or less. When the average particle size of the tungsten carbide powder is fine as in the above range, the dispersibility of the second hard phase particles in the cemented carbide can be improved. In this specification, the average particle size of the powder is measured using a particle size distribution measuring device (MT330EX (trademark)) manufactured by Microtrac.
[0083] (Metal hydride powder) The metal hydride powder may be, for example, titanium hydride (TiH 2 ), zirconium hydride (ZrH 2 ), and niobium hydride (NbH). The metal element in the metal hydride powder serves as a supply source for the metal element M in the second hard phase particles.
[0084] The average particle size of the metal hydride powder is preferably 0.1 μm or more and 1.0 μm or less, so that agglomerates of the second hard phase particles are less likely to form in the cemented carbide.
[0085] (Graphite powder) The graphite powder may be any known one. Of these, it is preferable to use natural graphite. The carbon in the graphite powder serves as a carbon source for the second hard phase particles.
[0086] The average particle size of the graphite powder is preferably 10 nm or more and 100 nm or less, so that agglomerates of the graphite powder are less likely to form in the cemented carbide.
[0087] The iron group element powder includes iron powder, cobalt powder, and nickel powder. The iron group element powder is a raw material for the binder phase.
[0088] The average particle size of the iron group element powder is preferably 0.1 μm or more and 1.5 μm or less, because this makes it difficult for agglomerates of the binder phase to form in the cemented carbide.
[0089] <Mixing process> The mixing step is a step of mixing the raw material powders prepared in the preparation step to obtain a mixed powder.
[0090] The ratio of the tungsten carbide powder in the mixed powder is preferably, for example, 88 mass % or more and 99 mass % or less.
[0091] The ratio of the metal hydride powder in the mixed powder is preferably, for example, 0.1 mass % or more and 1.0 mass % or less.
[0092] The ratio of graphite powder in the mixed powder is preferably, for example, 0.05% by mass or more and 0.3% by mass or less. In this embodiment, carbon in CO gas in the sintering step described below is used together with graphite powder as a carbon source for the second hard phase particles. Therefore, the ratio of graphite powder in the mixed powder can be made small as described above. Therefore, it is possible to suppress the inhomogeneity of the sintered body structure and the decrease in strength caused by the remaining carbon not incorporated in the second hard phase particles.
[0093] The proportion of the iron group element powder in the mixed powder is preferably, for example, 0.3 mass % or more and 15 mass % or less.
[0094] The mixing is preferably carried out using a bead mill for 0.5 to 24 hours, which can prevent excessive pulverization and prevent the particle size distribution of the mixed powder from becoming broad.
[0095] After the mixing step, the mixed powder may be granulated as necessary. By granulating the mixed powder, the mixed powder can be easily filled into a die or a mold during the molding step described below. A known method can be used for granulation. For example, a commercially available granulator such as a spray dryer or an extrusion granulator can be used.
[0096] <Forming process> The molding step is a step of forming the mixed powder obtained in the mixing step into a predetermined shape to obtain a molded body. The molding method and molding conditions in the molding step can be general methods and conditions. The predetermined shape can be a cutting tool shape (for example, a round bar for a small drill).
[0097] <Sintering process> The sintering step is a step in which the compact obtained in the molding step is sintered to obtain a cemented carbide. 2 The mixture is heated at a temperature of 1350 to 1500°C for 60 to 120 minutes in a gas mixture containing N gas and carbon monoxide (CO) gas. 2 The volume ratio of N to CO is 2 If the total of N and CO is 100% by volume, 2 It is preferable that the amount of CO is 20 volume % or more and 50 volume % or less, and the amount of CO is 50 volume % or more and 80 volume % or less. The carbon in the CO gas used here serves as a carbon source in the second hard phase particles.
[0098] Next, the heated compact is immersed in nitrogen (N 2 The mixture is heated and pressurized in a 1350 to 1500°C atmosphere at a pressure of 3 to 10 kPa for 60 to 120 minutes to obtain a cemented carbide. By applying pressure, it is possible to suppress the occurrence of large defects in the cemented carbide. 2 By heating and pressurizing in gas, the amount of nitrogen in the second hard phase particles increases, and the dispersibility of the second hard phase particles in the cemented carbide can be improved.
[0099] In the sintering process, metal hydride powder, tungsten carbide powder, graphite powder and N 2The gas is first dissolved in a binder phase made of iron group elements, and these constituent elements form a complex, which is then precipitated as a solid solution by the subsequent cooling process. It is believed that this solid solution is the second hard phase particles. When a metal hydride powder is used, the complex is less likely to coarsen and less likely to aggregate in the sintering process. This makes it possible to improve the dispersibility of the second hard phase particles in the cemented carbide. This was newly discovered by the present inventors as a result of extensive research. Note that in conventional methods for producing cemented carbide, metal oxides (TiO 2 However, when metal oxides are used, oxygen tends to remain in the cemented carbide, reducing its strength.
[0100] <Cooling process> The cooling step is a step of cooling the cemented carbide after the sintering is completed. The cooling conditions are not particularly limited, and general conditions can be used.
[0101] <Additional Notes> The above description includes the following additional embodiments. [Appendix 1] The cemented carbide of the present disclosure preferably contains 88 vol % to 99 vol % first hard phase particles, 0.2 vol % to 2.5 vol % second hard phase particles, and 0.5 vol % to 20 vol % binder phase. The cemented carbide of the present disclosure preferably contains 80% to 99% by volume of first hard phase particles, 0.5% to 3.0% by volume of second hard phase particles, and 0.5% to 20% by volume of a binder phase.
[0102] [Appendix 2] In the cemented carbide of the present disclosure, of the total 48 unit regions R, the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% is preferably 13 or less. In the cemented carbide of the present disclosure, of the total 48 unit regions R, the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% is preferably 12 or less. In the cemented carbide of the present disclosure, of the total 48 unit regions R, the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% is preferably 10 or less. EXAMPLES
[0103] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.
[0104] [Samples a to d, Samples A to H] <Preparation of cemented carbide> (preparation process) The raw powders are tungsten carbide powder, metal hydride powder, natural graphite powder, and chromium carbide (Cr 3 C 2 ) powder, vanadium carbide (VC) powder, and cobalt (Co) powder were prepared. The average particle size of the tungsten carbide (WC) powder was 1.0 μm. Metal hydride (TiH 2 The average particle size of the natural graphite powder (LONZA's "Graphite Powder") is 0.5 μm. The average particle size of the chromium carbide (Cr 3 C 2 The average particle size of the vanadium carbide (VC) powder is 0.8 μm. The average particle size of the cobalt (Co) powder is 0.8 μm. The WC powder, metal hydride powder, chromium carbide powder, vanadium carbide powder, and cobalt powder are commercially available products.
[0105] (Mixing process) The raw material powders were mixed to obtain a mixed powder, in which the ratio of each raw material powder in the mixed powder was as follows: Metal hydride (TiH 2 ) Powder: 0.2~2.0% by mass Natural graphite powder: 0.1 to 2.5% by mass Cobalt (Co) powder: 4.5 to 5% by mass Chromium carbide (Cr 3 C 2 ) Powder: 0.3% by mass (only sample G is included) Vanadium carbide (VC) powder: 0.1% by mass (only sample H is included) Tungsten carbide powder: Remainder (Adjust so that tungsten carbide powder occupies the remainder of the powder mixture.) The mixture was mixed in a bead mill for 12 hours, and the resulting mixed powder was granulated using a spray dryer.
[0106] (molding process) The obtained granules were press molded into a rod-shaped compact.
[0107] (Sintering process) The compact is subjected to N 2 N gas and CO gas 2 The compact was heated and pressurized for 60 minutes at a pressure of 2 to 50 kPa and a temperature of 1500° C. in a mixed gas having a volume ratio of 0.25 to 1 / CO (volume ratio). The compact was then sintered in nitrogen gas at a temperature of 1500° C. and a pressure of 2 to 50 kPa for 60 minutes to obtain a cemented carbide.
[0108] (cooling process) The cemented carbide was slowly cooled in an argon (Ar) gas atmosphere.
[0109] [Sample I] For sample I, a round bar-shaped cemented carbide was produced by the method described in Patent Document 1.
[0110] (preparation process) The raw powders were WC powder (average particle size 2.6 μm), TiC powder (average particle size 0.7 μm), TaC powder (average particle size 0.6 μm), Cr 3 C 2 Powder (average particle size: 0.9 μm) and Co powder (average particle size: 0.4 μm) were prepared.
[0111] (Mixing process) The raw material powders were mixed together to obtain a mixed powder. The mixing was carried out together with a solvent in an attritor (rotation speed: 250 rpm) for 1 hour. The obtained mixed powder was granulated using a spray dryer.
[0112] (molding process) The obtained granules were press molded into a rod-shaped compact.
[0113] (Sintering process) The compact was heated in Ar gas at a temperature of 1330° C. for 2 hours to obtain a round bar-shaped cemented carbide alloy.
[0114] (cooling process) The cemented carbide was slowly cooled in an argon (Ar) gas atmosphere.
[0115] [Sample J] Sample J is a metal hydride (TiH 2 ) powder, TiO 2 A round bar-shaped cemented carbide was produced in the same manner as in Samples a to d, except that the powder was used and argon gas was used during sintering.
[0116] <Evaluation> (D50 of first hard phase particles and second hard phase particles) For each sample, the 50% cumulative particle size (D50) based on area of the first hard phase particles and the second hard phase particles was measured. The specific measurement method is described in the first embodiment, and the description will not be repeated. The results are shown in the "D50 (μm)" column of "First hard phase particles" and the "D50 (μm)" column of "Second hard phase particles" of "Cemented carbide" in Table 1. Note that no measurement was performed for samples with "-" in the "D50 (μm)" column.
[0117] (D10 / D90 of second hard phase particles) For each sample, the D10 / D90 of the second hard phase particles was measured. The specific measurement method is described in the first embodiment, so the description will not be repeated. The results are shown in the "D10 / D90" column of "Second hard phase particles" under "Cemented carbide" in Table 1.
[0118] (Morphology, composition and atomic ratio of second hard phase particles) The morphology, composition and atomic ratio of the second hard phase particles were measured for each sample. The specific measurement method is described in the first embodiment, so the description will not be repeated. The second hard phase particles of Samples a to d and Samples A to I were solid solutions. The second hard phase particles of Sample J had a double structure.
[0119] The composition and atomic ratio of the second hard phase particles are shown in Table 1 under "Composition Ti" under "Second hard phase particles" under "Cemented carbide". x W 1-x C 1-y N y For example, in sample a, the composition Ti x W 1-x C 1-y N y In this case, x=0.42 and y=0.40, i.e., the composition is Ti 0.42 W 0.58 C 0.60 N 0.40 The composition of the second hard phase particles in sample I was TiWC. Since sample J had a double structure, the composition was not measured.
[0120] (Chromium and vanadium content) The mass-based content of chromium and vanadium was measured for each sample of cemented carbide. The specific measurement method is described in the first embodiment, and therefore the description thereof will not be repeated.
[0121] It was confirmed that sample G contained chromium, and sample H contained vanadium. The other samples were confirmed to contain neither chromium nor vanadium.
[0122] (Determination of the dispersion state of second hard phase particles) For each sample, it was determined whether the second hard phase particles were dispersed or unevenly distributed in the cemented carbide. The specific method of determination is described in the first embodiment, and therefore the description will not be repeated. When the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% is 14 or less out of a total of 48 unit regions R, it is determined that the second hard phase particles are dispersed in the cemented carbide. When the number of unit regions R is 15 or more, it is determined that the second hard phase particles are unevenly distributed in the cemented carbide. The results are shown in "Dispersion / Imbalanced (number)" of "Second Hard Phase Particles" of "Cemented Carbide" in Table 1. In the column, the number in parentheses indicates the number of unit regions R in which the percentage of the number of second hard phase particles in the unit regions R is less than 0.5% or more than 5% out of a total of 48 unit regions R.
[0123] (Composition of cemented carbide) It was confirmed that the cemented carbide of Samples a to d and Samples A to H contains 88 volume % to 99 volume % of first hard phase particles, 0.2 volume % to 2.5 volume % of second hard phase particles, and 0.5 volume % to 20 volume % of binder phase. The specific confirmation method is described in the first embodiment, and the description thereof will not be repeated.
[0124] (Cutting test) The tip of the round bar made of cemented carbide of each sample was sharpened to prepare a small-diameter drill with a cutting diameter of φ0.3 mm. Ten drills were prepared for each sample. The drills were used to drill holes in a commercially available printed wiring board for in-vehicle use. The conditions for drilling were a rotation speed of 100 krpm and a feed rate of 1.0 m / min. These conditions correspond to low-speed processing. The presence or absence of chipping and the cutting edge condition of the drill after drilling 2000 holes were observed. The average number of chippings in the 10 drills is shown in the "Number of chippings" column of "Cutting test" in Table 1. The smaller the number of chippings, the better the chipping resistance and breakage resistance. The cutting edge condition of the drill after the cutting test is shown in the "Cutting edge condition" column. Furthermore, it was judged whether or not it could be used continuously after the cutting test. The results are shown in the "Can it be used continuously" column.
[0125] [Table 1]
[0126] <Consideration> The cemented carbide alloys of samples a to d and samples F to H correspond to examples. The drills made of cemented carbide alloys of samples a and b had zero chipping, and were in a state in which they could be used further after the cutting test. The drills made of cemented carbide alloys of samples c and d had one chipping, which was very small, and were in a state in which they could be used further after the cutting test. The drills made of cemented carbide alloys of sample F (D50 of the first hard phase particles was 1.6 μm), sample G (containing chromium), and sample H (containing vanadium) had two to three chipping, and were in a state in which they could be used further after the cutting test.
[0127] That is, it was confirmed that the drills made of cemented carbide of Samples a to d and Samples F to H have excellent chipping resistance and breakage resistance and have long tool life even in low-speed machining. Among them, Samples a to d showed very excellent chipping resistance and breakage resistance with the number of chipping being 0 or 1.
[0128] The cemented carbide samples A to E correspond to comparative examples. The drills made of the cemented carbide samples A to E had 6 to 8 chippings, and were in a state where they could not be used continuously after the cutting test.
[0129] The cemented carbide of sample I corresponds to a comparative example. The drill made of the cemented carbide of sample I broke before drilling 1000 holes. This is presumably because when metal carbide powder is used as the raw material, the raw material powder of the second hard phase particles tends to become coarse and aggregate during the sintering process. Also, it is presumed that when coarse-grained WC powder is used as the raw material, the dispersibility of the second hard phase particles decreases.
[0130] The cemented carbide of sample J corresponds to a comparative example. The drill made of the cemented carbide of sample J broke before drilling 1000 holes. This is presumably because oxygen remains in the cemented carbide when metal oxide powder is used as the raw material, which reduces the strength of the cemented carbide. In addition, it is presumed that when the carbon source of the second hard phase particles is only the blended carbon, the remaining carbon that was not incorporated into the second hard phase particles causes the sintered body structure to become non-homogenous and the strength to decrease.
[0131] Although the embodiments and examples of the present disclosure have been described above, it is intended from the outset that the configurations of the above-described embodiments and examples may be appropriately combined or modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered as limiting. The scope of the present invention is indicated by the claims, not by the embodiments and examples described above, and is intended to include the meaning equivalent to the claims and all modifications within the scope. [Explanation of symbols]
[0132] 1 1st hard phase particle 2 Second hard phase particles 3 Bonded phase L1 Any line passing through the center of gravity X of the second hard phase particle a1~a8 measurement points R unit area
Claims
1. A cemented carbide comprising a hard phase and a binder phase, the hard phase comprises first hard phase particles and second hard phase particles; the first hard phase particles are made of tungsten carbide; The second hard phase particles are x W 1-x C 1-y N y and M is at least one metal element selected from the group consisting of Group 4 elements, Group 5 elements, chromium, and molybdenum of the periodic table; The x is 0.40 or more and 0.70 or less, The y is 0 or more and 0.90 or less, the binder phase contains at least one iron group element selected from the group consisting of iron, cobalt, and nickel; the second hard phase particles have an area-based 50% cumulative number particle diameter of 0.1 μm or more and 0.5 μm or less; The second hard phase particles are present in a dispersed state.
2. 2. The cemented carbide according to claim 1, wherein the first hard phase particles have an area-based 50% cumulative number grain size of 0.1 μm or more and 1.5 μm or less.
3. 3. The cemented carbide of claim 1 or claim 2, wherein the cemented carbide is free of one or both of chromium and vanadium.
4. A cutting tool comprising the cemented carbide according to any one of claims 1 to 3.
Citation Information
Patent Citations
Cemented carbide and method of making the same
JP2005126824A
Tungsten carbide-based sintered body and abrasion resistant member using the same
JP2012229138A
Cemented carbide and cutting tool
WO2017191744A1