Zn-Al-Mg-Si coated steel sheet

The Zn-Al-Mg-Si plated steel sheet addresses chemical conversion and blistering issues by controlling the microstructure to suppress surface alloy phases and form oxide phases inside, enhancing corrosion resistance and joint integrity with aluminum alloys.

JP7574972B1Active Publication Date: 2024-10-29JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024532587
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-03-05
Publication Date
2024-10-29
Estimated Expiration
2044-03-05

AI Technical Summary

Technical Problem

Existing Zn-plated steel sheets face challenges in chemical conversion treatment properties and blistering under the coating film from edges, particularly in dissimilar metal joints with aluminum alloy parts, which are critical for lightweight automobile construction.

Method used

A Zn-Al-Mg-Si plated steel sheet with controlled composition and microstructure, where Mg2Si alloy phase is suppressed on the surface and formed inside the plating layer, and SiO2 oxide phase is formed inside, enhancing corrosion resistance and suppressing blistering.

Benefits of technology

The solution provides excellent chemical conversion treatment properties and superior corrosion resistance at dissimilar joints with aluminum alloys, effectively preventing blistering and improving overall corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574972000003
    Figure 0007574972000003
  • Figure 0007574972000004
    Figure 0007574972000004
  • Figure 0007574972000001
    Figure 0007574972000001
Patent Text Reader

Abstract

The present invention provides a Zn-Al-Mg-Si plated steel sheet that is excellent in chemical conversion treatability, suppression of blistering under the paint film, and corrosion resistance at dissimilar joints. The Zn-Al-Mg-Si plated steel sheet of the present invention has a base steel sheet and a plating layer formed on at least one side of the base steel sheet, the plating layer having a composition, by mass%, of 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn2 ternary eutectic structure, and in a backscattered electron image at a magnification of 5000 times obtained with a scanning electron microscope at an accelerating voltage of 7.0 kV, needle-shaped Mg2Si alloy phases are present on the ternary eutectic structure at a number density of 100,000 particles / mm 2 When the same method was used with an accelerating voltage of 15.0 kV, the number density of the needle-like Mg2Si alloy phase was less than 500 / mm 2 The number density of the needle-shaped SiO2 oxide phase is 100,000 pieces / mm 2 The present invention is characterized in that:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Zn-Al-Mg-Si plated steel sheet. [Background technology]

[0002] Zinc plating, which suppresses the corrosion of iron through sacrificial corrosion protection, is excellent in rust prevention performance and economy, and is widely used to manufacture steel materials with high corrosion resistance. In particular, hot-dip galvanized steel materials, in which a plating layer is formed by immersing a steel material in molten zinc, have a simpler manufacturing process and a lower product price than electrogalvanized steel materials, and therefore demand is increasing across industries such as automobiles, home appliances, and building materials. However, due to the worsening of air pollution and corrosive environments associated with industrial advancement, and the depletion of zinc resources due to a significant increase in zinc usage, there has been a demand for plated steel materials that are more corrosion resistant than conventional zinc plating and that also require less zinc.

[0003] Patent Document 1 discloses a Zn-Al-Mg-plated steel material in which elements such as aluminum (Al) and magnesium (Mg) are added to zinc (Zn) to improve the corrosion resistance of the steel material. Patent Document 2 reports that the corrosion resistance of the flat and end surfaces of the plated steel material is improved compared to that of a conventional Zn-Al-Mg-plated steel sheet by adding silicon (Si) to the Zn-Al-Mg-plated layer. Patent Document 3 reports that the plating layer of a Zn-Al-Mg-plated steel sheet is given fracture toughness and corrosion resistance after processing is improved by adding Si to the plating layer and concentrating Si at the interface between the plating layer and the base steel sheet. Patent Document 4 reports that a resin film containing fine silica (SiO2) is formed on the surface of the plating layer of a Zn-Al-Mg-plated steel sheet, which strengthens the film and improves the workability and corrosion resistance of the processed part. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 4-147955 [Patent Document 2] JP 2005-82834 A [Patent Document 3] Patent Publication No. 2021-508771 [Patent Document 4] JP 2004-338397 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, further improvements were required in the chemical conversion treatability of plated steel sheets and in the suppression of blistering under the paint film from the edges.In addition, as the use of aluminum alloy sheets and aluminum die castings in automobile bodies is increasing in order to drastically reduce the weight of automobiles, corrosion resistance at dissimilar joints between plated steel sheet members and aluminum alloy members has become apparent as a new required property, and corrosion resistance at dissimilar joints with aluminum alloy members has been desired.

[0006] In view of the above problems, an object of the present invention is to provide a Zn-Al-Mg-Si plated steel sheet which has excellent chemical conversion treatability, sufficiently suppresses under-coat blistering from the edges, and has excellent corrosion resistance at dissimilar joints in contact with an aluminum alloy at a processed portion. [Means for solving the problem]

[0007] The present inventors have made intensive studies to solve the above problems, and have found the following. In a Zn-Al-Mg-Si-plated steel sheet, excellent chemical conversion treatability can be obtained by suppressing the formation of an Mg2Si alloy phase in the surface layer of the plating layer. On the other hand, the formation of an SiO2 oxide phase in the surface layer of the plating layer can improve the corrosion resistance of dissimilar joints at the contact portion with the aluminum alloy of the processed portion. In addition, the formation of an Mg2Si alloy phase inside the plating layer can suppress the undercoat blister from the sheared end after painting. As a method for producing such a plated steel sheet, a salt water application process is performed after plating of the base steel sheet, thereby reducing the Mg2Si alloy phase in the surface layer of the plating layer and forming an SiO2 oxide phase instead.

[0008] That is, the gist and configuration of the present invention are as follows.

[0009] [1] A steel sheet having a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, the plating layer has a composition containing, in mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, and has a Zn-Al-MgZn2 ternary eutectic structure; In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases having a long side length of 0.5 μm or more were observed on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 pieces / mm 2 Less than (0 pieces / mm 2 (including In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases having a long side length of 0.5 μm or more were observed on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 500 pieces / mm 2 There are more than In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped SiO2 oxide phases having a long side length of 0.5 μm or more were observed on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 pieces / mm 2 A Zn-Al-Mg-Si-plated steel sheet characterized in that the above-mentioned components are present. Effect of the Invention

[0010] ADVANTAGE OF THE PRESENT DISCLOSURE According to the present invention, there can be provided a Zn-Al-Mg-Si plated steel sheet which has excellent chemical conversion treatability, sufficiently suppresses under-coat blistering from the edges, and has excellent corrosion resistance at dissimilar joints in contact with aluminum alloys at processed sections. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1(a) is a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of a plating layer with an electron beam at an accelerating voltage of 7.0 kV in one embodiment of the present invention, and FIG. 1(b) to (e) are the Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, obtained by composition analysis using EDS. [Diagram 2] FIG. 1(a) is a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of a plating layer with an electron beam at an accelerating voltage of 15.0 kV in one embodiment of the present invention, and FIG. 1(b) to (f) are the Mg distribution, Si distribution, Al distribution, Zn distribution, and O distribution, respectively, obtained by composition analysis using EDS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the Zn-Al-Mg-Si-plated steel sheet according to the present invention will be described. Note that the embodiment described below is one example of the present invention, and the configuration of the present invention is not limited to this specific example.

[0013] A Zn-Al-Mg-Si-plated steel sheet according to one embodiment of the present invention comprises a base steel sheet and a plating layer formed on at least one surface of the base steel sheet. The plating layer has a composition, by mass%, of 0.50-3.00% Mg, 0.10-3.00% Al, 0.010-0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, and a Zn-Al-MgZn2 ternary eutectic structure. Furthermore, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases having a long side length of 0.5 μm or more are present on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 pieces / mm 2 Less than (0 pieces / mm 2 In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases having a long side length of 0.5 μm or more are present on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 500 pieces / mm 2 or more, and in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped SiO2 oxide phases having a long side length of 0.5 μm or more are present on the Zn-Al-MgZn2 ternary eutectic structure at a number density of 100,000 pieces / mm 2 The present invention is characterized in that:

[0014] The type of the base steel sheet used in the present invention is not particularly limited, and for example, a hot-rolled steel sheet or hot-rolled steel strip that has been pickled and descaled, or a cold-rolled steel sheet or cold-rolled steel strip obtained by cold rolling the hot-rolled steel sheet or hot-rolled steel strip can be used. There is also no particular limit to the thickness of the base steel sheet, but it is preferably 0.7 to 2.0 mm.

[0015] Next, the composition of the Zn-Al-Mg-Si based plating layer in the present invention will be described.

[0016] When the content of Mg in the plating layer is less than 0.50% by mass, the number density of the Mg2Si alloy phase and the SiO2 oxide phase is not sufficient in the backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using the scanning electron microscope, and the effect of suppressing the bulging under the coating film from the edge and improving the corrosion resistance of the dissimilar joint at the contact part with the aluminum alloy of the processed part is insufficient. Therefore, the content of Mg in the plating layer is 0.50% by mass or more, and preferably 1.00% by mass or more. On the other hand, when the content of Mg in the plating layer exceeds 3.00% by mass, a brittle lump-like MgZn2 phase is formed, the plating layer becomes brittle, the adhesion decreases, and the workability and the corrosion resistance of the processed part may deteriorate. Therefore, the content of Mg in the plating layer is 3.00% by mass or less, and preferably 2.50% by mass or less.

[0017] When the content of Al in the coating layer is less than 0.10% by mass, the Zn-Al-MgZn2 ternary eutectic structure is not formed in the coating layer, and the Mg2Si alloy phase is not sufficiently formed, so that the effect of suppressing blistering under the coating from the edge is reduced. Therefore, the content of Al in the coating layer is set to 0.10% by mass or more, and preferably 0.50% by mass or more. On the other hand, when the content of Al in the coating layer exceeds 3.00% by mass, peeling of the coating occurs from the sheared edge of the plated steel sheet, and suppression of blistering under the coating is insufficient. Therefore, the content of Al in the coating layer is set to 3.00% by mass or less, and preferably 2.00% by mass or less.

[0018] When the content of Si in the plating layer is 0.010% by mass or more, it forms an Mg2Si alloy phase together with Mg in the plating layer, contributing to improving the corrosion resistance of the plating layer. This is believed to be due to the following action. That is, since the Mg2Si alloy phase is active, it reacts with water in a corrosive environment and decomposes, and in the plating structure of the Zn-Al-MgZn2 ternary eutectic described below, it sacrificially protects the metal structure containing one or more of the Zn phase, Al phase, and MgZn2 alloy phase. At the same time, the resulting corrosion product of Mg forms a protective film and suppresses further corrosion. Under the coating film, the progress of bimetallic corrosion with Fe occurring at the sheared end of the plated steel sheet is suppressed, so that the blister that appears on the coating surface occurring from the sheared end is suppressed. In order to obtain the above effect, the content of Si in the plating layer is 0.010% by mass or more, and preferably 0.050% by mass or more. If the Si content is less than 0.010% by mass, the Mg2Si alloy phase is not sufficiently formed in the plating layer, making it difficult to suppress the blistering under the coating film that occurs from the sheared end. On the other hand, if the Si content in the plating layer exceeds 0.20% by mass, a large amount of Mg2Si alloy phase is formed even in the surface layer of the plating layer. The Mg2Si alloy phase is easily oxidized to become an oxide layer, which tends to block and inhibit the adhesion of the chemical conversion treatment agent, and there is a concern that the chemical conversion treatment property will decrease. Therefore, the Si content in the plating layer is 0.20% by mass or less, and preferably 0.15% by mass or less.

[0019] If the Fe content in the coating layer exceeds 0.30 mass%, the growth of the alloy layer formed at the interface between the base steel sheet and the coating layer increases, and workability decreases. Therefore, the Fe content in the coating layer is set to 0.30 mass% or less, and preferably 0.20 mass% or less. On the other hand, the lower limit of the Fe content in the coating layer is not particularly limited, and may be 0.00 mass%.

[0020] The balance of the composition of the plating layer other than the above consists of Zn and unavoidable impurities.

[0021] Next, the structure of the Zn-Al-Mg-Si based coating layer will be described. The coating layer in the present invention has a Zn-Al-MgZn2 ternary eutectic coating structure, and contains a Mg2Si alloy phase in the coating structure. The coating structure may further contain a Zn phase, an Al phase, or a MgZn2 alloy phase.

[0022] If the Mg2Si alloy phase of the Zn-Al-Mg-Si-based plating layer is present in a large amount in the surface layer of the plating layer, there is a concern that the chemical conversion treatment property may be reduced. Therefore, it is preferable that the Mg2Si alloy phase is not formed in the surface layer of the plating layer. On the other hand, if the Mg2Si alloy phase is formed inside the plating layer, it suppresses plating corrosion that occurs at the sheared end after painting, suppresses the progress of corrosion under the coating film, and suppresses blistering under the coating film that occurs from the sheared end. For this reason, it is preferable that the Mg2Si alloy phase is not formed on the surface layer of the plating layer, but is formed inside the plating layer.

[0023] In the present invention, the phrase "the Mg2Si alloy phase is not formed in the surface layer of the plating layer" means that in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, no needle-shaped Mg2Si alloy phase with a long side length of 0.5 μm or more is observed in the Zn-Al-MgZn2 ternary eutectic structure. 2 If the number density of the Mg2Si alloy phase formed in the surface layer of the coating layer is more than 100,000 / mm 2 Less than 0 pieces / mm 2 It is more preferable that:

[0024] In the present invention, the phrase "the Mg2Si alloy phase is formed inside the plating layer" means that, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped Mg2Si alloy phases with a long side length of 0.5 μm or more are observed on the Zn-Al-MgZn2 ternary eutectic structure.2 When the thickness is more than 500 mm, the effect of suppressing the blistering under the coating from the sheared edge after coating can be obtained. Therefore, the number density of the Mg2Si alloy phase formed inside the coating layer is 500 pieces / mm 2 More than 1200 pieces / mm 2 On the other hand, the upper limit of the number density of the Mg2Si alloy phase formed inside the plating layer is not particularly limited, but the number density is generally 2500 pieces / mm 2 The result is as follows.

[0025] Furthermore, when the Mg2Si alloy phase inside the plating layer is corroded, a SiO2 oxide phase is formed inside the plating layer. When the SiO2 oxide phase formed inside the plating layer is present together with Zn in a corrosive environment, it promotes the production of basic zinc chloride, which has a strong protective effect, and contributes to improving corrosion resistance. Furthermore, the SiO2 oxide phase strengthens the plating layer, suppresses the occurrence of cracks under external stress and the progression of corrosion after the occurrence of cracks, thereby improving the corrosion resistance of the processed part. Therefore, it is preferable that a SiO2 oxide phase is formed inside the plating layer.

[0026] In the present invention, the expression "the SiO2 oxide phase is formed inside the plating layer" means that, in a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, needle-shaped SiO2 oxide phases with a long side length of 0.5 μm or more are observed on the Zn-Al-MgZn2 ternary eutectic structure. 2 If the density is more than 100,000 / mm, the corrosion resistance of the processed part is obtained. Therefore, the number density of the SiO2 oxide phase formed inside the plating layer is 100,000 / mm 2 More than 150,000 pieces / mm 2 On the other hand, the upper limit of the number density of the SiO2 oxide phase formed inside the plating layer is not particularly limited, but the number density is generally 380,000 pieces / mm 2 The result is as follows.

[0027] The formation of the SiO2 oxide phase requires the control of the Si content in the plating bath components, the control of the reductivity (O2 concentration control) when plating the surface of the base steel sheet, and post-treatment processes after plating. If such control and post-treatment processes are insufficient, the Mg2Si alloy phase may be too much in the surface layer of the plating layer, reducing the chemical conversion treatability, or the Mg2Si alloy phase may be too little inside the plating layer, causing blistering from the sheared edge after painting to be uncontrollable, or the SiO2 oxide phase may not be sufficiently formed inside the plating layer, reducing the corrosion resistance of the processed part.

[0028] 1(a) to (e) show backscattered electron images (5000x) and EDS analysis results observed when the surface of the plating layer of the Zn-Al-Mg-Si-plated steel sheet produced in one embodiment of the present invention was irradiated with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope. FIG. 1(a) is a backscattered electron image of the Zn-Al-Mg-Si-plated layer, and (b) to (e) are the Mg distribution, Si distribution, Al distribution, and Zn distribution, respectively, analyzed by EDS. As shown in FIG. 1(a) to (e), the Mg2Si alloy phase has a needle-like shape where the distributions of Mg and Si overlap, and it can be seen that it is in the Zn-Al-MgZn2 ternary eutectic structure.

[0029] 2(a) to (f) show backscattered electron images (5000x) and EDS analysis results observed when the surface of the plating layer of the Zn-Al-Mg-Si-plated steel sheet manufactured in one embodiment of the present invention is irradiated with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope. FIG. 2(a) is a backscattered electron image of the Zn-Al-Mg-Si-plated layer, and (b) to (f) are Mg distribution, Si distribution, Al distribution, Zn distribution, and O distribution, respectively, analyzed using EDS. As shown in FIG. 2(a) to (f), the Si distribution has a needle-like shape, and the O distribution overlaps with the distributions of Mg, Si, and Al. The SiO2 oxide phase has a needle-like shape where the distributions of Si and O overlap, and it can be seen that it is in the Zn-Al-MgZn2 ternary eutectic structure.

[0030] [Manufacturing method of Zn-Al-Mg-Si plated steel sheet] Next, a method for producing a Zn-Al-Mg-Si-plated steel sheet according to one embodiment of the present invention will be described. The method for producing a Zn-Al-Mg-Si-plated steel sheet according to one embodiment of the present invention includes the steps of immersing a base steel sheet in a plating bath containing, in mass%, 0.50 to 3.00% Mg, 0.10 to 3.00% Al, 0.010 to 0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities, to perform a plating treatment on the base steel sheet, performing gas wiping on the base steel sheet after the plating treatment to adjust the adhesion amount of the plating layer formed on the base steel sheet, and performing salt water coating treatment on the surface of the plated steel sheet after the gas wiping. The method for cooling the plated steel sheet after gas wiping and before the salt water coating treatment is not particularly limited, but various methods such as air cooling, air-water cooling, and water cooling can be applied.

[0031] By carrying out a saltwater coating process on the surface of plated steel sheet, the plated layer is etched and the Mg2Si alloy phase present inside the plated layer is oxidized. When the Mg2Si alloy phase is oxidized, Mg, which has a lower natural potential in a saltwater environment, is selectively dissolved and eluted from the plated layer. As a result, the remaining Si is oxidized and becomes an oxide, forming a SiO2 oxide phase. When this SiO2 oxide phase formed inside the plated layer is present together with Zn in a corrosive environment, it promotes the production of basic zinc chloride, which has a strong protective effect, and contributes to improving corrosion resistance.

[0032] In the method for producing a Zn-Al-Mg-Si plated steel sheet according to the present invention, the base steel sheet to be plated is the same as that described above for the base steel sheet.

[0033] When the annealing heat treatment is performed on the base steel sheet before the plating treatment, if the H2 concentration in the furnace atmosphere during annealing is 1 volume % or more, the oxides on the surface of the base steel sheet can be suitably reduced. Therefore, the H2 concentration in the furnace atmosphere during annealing is preferably 1 volume % or more. On the other hand, if the H2 concentration in the furnace atmosphere during annealing is 10 volume % or less, the manufacturing cost can be suitably suppressed. Therefore, the H2 concentration in the furnace atmosphere during annealing is preferably 10 volume % or less. In addition, the furnace atmosphere during annealing is preferably a mixed gas containing H2 and the balance consisting of N2. The temperature of the annealing heat treatment is not particularly limited, but is preferably 600 to 850°C. In addition, the time of the annealing heat treatment is not particularly limited, but is preferably 10 to 60 seconds.

[0034] The plating bath used in the production of the Zn-Al-Mg-Si plated steel sheet according to the present invention has a composition containing, in mass%, 0.50-3.00% Mg, 0.10-3.00% Al, 0.010-0.20% Si, and 0.30% or less Fe, with the balance being Zn and unavoidable impurities. The explanation of each component in the plating bath is the same as the explanation of each component of the plating layer described above. The composition of the plating bath and the composition of the applied plating layer are equivalent.

[0035] The coating weight of the plating layer in the plating process is set at 15g / m from the viewpoint of corrosion resistance. 2 It is preferable that the thickness is 30 g / m or more. 2 On the other hand, the coating weight of the plating layer is preferably 100 g / m or more. 2 If the coating weight of the plating layer is less than 100 g / m, the manufacturing cost can be suppressed favorably. 2It is preferable that the temperature of the plating bath during plating is 430 to 540°C. If the plating bath temperature is less than 430°C, the fluidity of the plating bath may decrease, which may hinder uniform plating coverage. For this reason, the temperature of the plating bath is preferably 430°C or higher. On the other hand, if the temperature of the plating bath exceeds 540°C, there is a risk of an increase in oxides on the surface of the plating bath due to oxidation of Mg in the plating bath, and erosion of the refractory material in the plating bath by Al and Mg. For this reason, the temperature of the plating bath is preferably 540°C or lower, more preferably 530°C or lower.

[0036] In order to prevent the Mg2Si alloy phase from being formed in the surface layer of the plating layer and to form a large amount of it inside the plating layer, it is effective to reduce the reducing property of the gas used in gas wiping. When H2 is used as the mixed gas used in gas wiping, the reducing property becomes very high. When the H2 concentration is 1% by volume or more and the amount of Si in the plating bath is low, even if the salt water treatment process is performed, Mg2Si in the plating layer is not easily oxidized, and a sufficient amount of SiO2 oxide phase is not formed, making it difficult to obtain the desired corrosion resistance of the processed part. As a result of intensive research by the present inventors on this point, it was found that the higher the O2 concentration during gas wiping and the lower the reducing property of the gas, the less likely the Mg2Si alloy phase is to be formed in the surface layer of the plating layer and the more likely it is to be formed inside the plating layer. As a result, it is possible to reduce the SiO2 oxide phase in the surface layer of the plating layer and increase the SiO2 oxide phase inside the plating layer during corrosion due to the salt water treatment process. Therefore, it is preferable to use a mixed gas containing O2 and N2, or air (air) as the gas type used in gas wiping. The gas wiping is preferably performed in an atmospheric environment.

[0037] When the gas used in gas wiping is a mixed gas containing O2 and N2, if the O2 concentration is 3% by volume or more, even if the Si content in the plating bath is low, the Mg2Si alloy phase is preferably formed inside the plating layer, and the effect of contributing to improving corrosion resistance is preferably obtained. Therefore, the O2 concentration of the mixed gas used in gas wiping is preferably 3% by volume or more. On the other hand, if the O2 concentration is 15% by volume or less, the manufacturing cost can be preferably suppressed. Therefore, the O2 concentration of the mixed gas used in gas wiping is preferably 15% by volume or less. In addition, the mixed gas may contain H2, and if the H2 concentration of the mixed gas used in gas wiping is 7% by volume or more, the generation of the Mg2Si alloy phase in the surface layer of the plating layer is preferably suppressed, the Mg2Si alloy phase is formed inside the plating layer, and the formation of the SiO2 oxide phase inside the plating layer during the salt water application treatment process is preferably promoted.

[0038] Gas wiping may be performed using air, and even in this case, even if the amount of Si in the plating bath is low, an Mg2Si alloy phase is preferably formed inside the plating layer. During the salt water application process after gas wiping with air, the formation of an SiO2 oxide phase is preferably promoted inside the plating layer, and the effect of contributing to the improvement of corrosion resistance is preferably obtained.

[0039] The method of applying salt water to the surface of the plated steel sheet after adjusting the coating weight is not particularly limited, but a method of applying salt water to the surface of the plated steel sheet, leaving it for a predetermined time, and then washing and drying to corrode and oxidize the plating layer of the plated steel sheet may be used. The salt water used in the salt water application treatment is not particularly limited, but an aqueous solution of sodium chloride (NaCl) is preferable from the viewpoint of manufacturing costs. The salt water concentration is also not particularly limited, but it is preferably 0.5 mass% or more and 5.0 mass% or less from the viewpoint of manufacturing costs. In addition, the leaving time of the salt water application treatment is preferably 0.5 hours or more from the viewpoint of sufficiently oxidizing the plating layer. On the other hand, if the leaving time exceeds 2 hours, the corrosion of the plating layer may progress extremely, the plating coating weight may decrease, and the corrosion resistance may deteriorate. Therefore, the leaving time of the salt water application treatment is preferably 2 hours or less, and more preferably 1 hour or less.

[0040] Regarding steps and conditions not described in the present invention, conventional methods can be used. EXAMPLES

[0041] Using an ultra-low carbon cold-rolled steel sheet with a thickness of 0.8 mm as the base steel sheet, all the Zn-Al-Mg-Si plated steel sheets to be used as samples were manufactured using hot-dip plating equipment. Each sample was plated using variously changed plating bath compositions, and the temperature of the plating bath was set to 450°C, 30°C higher than the solidification start temperature estimated from the Zn-Al-Mg-Si quaternary equilibrium phase diagram. The base steel sheet was heated in an H2 (5% by volume) + N2 atmosphere, and the temperature of the base steel sheet when immersed in the plating bath was set to the same temperature as the plating bath temperature, and hot-dip plating was performed in the plating bath for 1 second. Thereafter, the thickness of the plating layer was reduced to 7 μm (50 g / m) by adjusting the flow rate of the wiping gas. 2 The temperature was controlled to a constant temperature (equivalent to 100°C). Some samples were further subjected to a salt water coating treatment by immersing them in an aqueous solution of 0.5% by weight NaCl for 1 hour, followed by washing and drying. Table 1 shows the plating bath composition, wiping gas composition, and plating layer composition. In addition, for the salt for salt water coating treatment in Table 1, samples that underwent water coating treatment are indicated as "Yes", and samples that did not undergo salt water coating treatment are indicated as "No". Note that the atmosphere during wiping was air.

[0042] [Table 1] TIFF0007574972000002.tif233121

[0043] Each sample of the obtained Zn-Al-Mg-Si plated steel sheet was sheared to a size of 10 x 20 mm. The plating layer of the sample after shearing was observed from the surface direction of the plated steel sheet using a scanning electron microscope to confirm the presence or absence of a Zn-Al-MgZn2 ternary eutectic structure. If a structure consisting of three phases, Zn phase, Al phase, and MgZn2 alloy phase, was found when the composition analysis was performed by EDS during observation, and if the Zn phase, Al phase, and MgZn2 alloy phase were confirmed when the same surface was analyzed by XRD, then the Zn-Al-MgZn2 ternary eutectic structure was present and "present" was recorded in Table 1. If a structure consisting of three phases, Zn phase, Al phase, and MgZn2 alloy phase, was not found when the composition analysis was performed by EDS during observation, and if any of the Zn phase, Al phase, and MgZn2 alloy phase was not confirmed when the same surface was analyzed by XRD, then the Zn-Al-MgZn2 crystalline structure was not present and "absent" was recorded in Table 1.

[0044] The plating layer of the sample after shearing was observed from the surface direction of the plated steel sheet using a scanning electron microscope to observe the state of the Mg2Si alloy phase present in the surface layer and inside of the plating layer and evaluate its number density. The number density of the Mg2Si alloy phase present in the surface layer and inside of the plating layer was evaluated from a backscattered electron image (5000x) observed when irradiated with an electron beam at an accelerating voltage of 7.0 kV. The number density of the Mg2Si alloy phase present in the inside of the plating layer was evaluated from a backscattered electron image (5000x) observed when irradiated with an electron beam at an accelerating voltage of 15.0 kV.

[0045] The plating layer of the sample after shearing was observed from the surface direction of the plated steel sheet using a scanning electron microscope to observe the state of the SiO2 oxide phase present inside the plating layer and evaluate the number density. The SiO2 oxide phase present inside the plating layer was evaluated from the backscattered electron image (5000x) observed when irradiated with an electron beam at an accelerating voltage of 15.0 kV.

[0046] [Chemical conversion treatment] Next, the chemical conversion treatability of the obtained Zn-Al-Mg-Si-plated steel sheets was evaluated. Each sample was sheared to a size of 30 x 30 mm, and then phosphating was performed for 90 seconds under the same conditions. After observing the surface direction of the plated steel sheet using a scanning electron microscope, the state of phosphate crystal scabbing (degree of exposure of the plated surface under chemical conversion) was observed from the secondary electron image (800 times) obtained by observing it, and was evaluated as follows. In Table 1, the following is shown: "◎" when there is no phosphate crystal scabbing and no exposure of the plated steel sheet surface; "○" when there is very little phosphate crystal scabbing and very little exposure of the plated steel sheet surface; "△" when there is very little phosphate crystal scabbing and very little exposure of the plated steel sheet surface; and "×" when there is phosphate crystal scabbing and the plated surface is exposed. The evaluation of ◎ or ◯ was passed, and △ or × was failed.

[0047] [Bulging under the coating from the sheared edge after painting] Next, the suppression of under-coating blistering from the sheared edge of the painted Zn-Al-Mg-Si-plated steel sheet was evaluated. Each sample was sheared to a size of 80 x 80 mm, phosphate-treated under the same conditions, and electrocoated (the thickness of the coating was constant at 15 μm), and then sheared to a size of 50 x 50 mm to prepare a sheared edge. The above samples were then subjected to 45 cycles of corrosion testing according to JASO M609-91, after which the maximum width of under-coating blistering from the sheared edge was evaluated. The blister width was shown in Table 1 as "◎" when it was less than 1.0 mm, "○" when it was 1.0 mm or more but less than 1.5 mm, "△" when it was 1.5 mm or more but less than 2.0 mm, and "×" when it was 2.0 mm or more. The evaluations of ◎ or ◯ were considered to be pass, and △ or × were considered to be fail.

[0048] [Corrosion resistance of processed and dissimilar joints] Next, the corrosion resistance of the processed and dissimilar joints of the Zn-Al-Mg-Si-plated steel sheets was evaluated. Each sample was sheared to a size of 70 × 120 mm, and mechanically joined at two points to the Al alloy sheared to a size of 40 × 90 mm by mechanical clinching (5 mmφ), to give a processed part, and a processed dissimilar joint sample of the Zn-Al-Mg-Si-plated steel sheet and the Al alloy was prepared. At this time, the phosphate treatment was performed under the same conditions except for the joint surface, and then the electrodeposition coating was performed (the thickness of the coating was constant at 15 μm) and coated. Then, a corrosion test was performed by the N-VDA test on the processed dissimilar joint sample. The corrosion amount of the Al alloy after the corrosion test was performed for 12 weeks was evaluated. The amount of Al corrosion was calculated by immersing the processed dissimilar joint sample in a 60 mass% nitric acid aqueous solution at room temperature to remove the corrosion products mainly composed of aluminum, and calculating the difference between the weight before the test and the weight after the corrosion products were removed, in accordance with ISO8407:2021. If the corrosion amount was 5 g / m 2 If it is less than 5g / m, mark it as "◎" 2 More than 10g / m 2 If it is less than 10g / m, mark it as "○" 2 More than 15g / m 2 If it is less than 15g / m, it will be marked as "△". 2 The above cases are indicated as "X" in Table 1. A rating of ◎ or ◯ was considered to be a pass, while a rating of △ or × was considered to be a fail.

[0049] As shown in Table 1, the plating composition defined in the present invention has a number density of Mg2Si alloy phase of 100,000 / mm2 when observed at an accelerating voltage of 7.0 kV. 2 Less than 500 particles / mm when observed at an accelerating voltage of 15.0 kV 2 The above-mentioned invention examples had excellent chemical conversion treatability, sufficiently suppressed blistering under the coating film from the sheared edge, and excellent corrosion resistance at the joint between the processed and dissimilar materials. In other words, it was found that the presence of a small amount of Mg2Si alloy phase in the surface layer of the plating layer and a large amount in the interior of the plating layer is advantageous for chemical conversion treatability, suppression of blistering under the coating film from the sheared edge, and corrosion resistance at the joint between the processed and dissimilar materials. In particular, the number density of SiO2 when observed at an accelerating voltage of 15.0 kV was 150,000 particles / mm 2That is, the invention examples, which have a large amount of SiO2 inside the plating layer, showed more favorable evaluation results. In contrast, the comparative examples, which are outside the scope of the present invention, showed inferior results in any of the following: chemical conversion treatability, suppression of blistering under the coating film from the sheared end, and corrosion resistance of the processed and dissimilar joint parts, compared to the invention examples. [Industrial Applicability]

[0050] ADVANTAGE OF THE PRESENT DISCLOSURE According to the present invention, there is provided a Zn-Al-Mg-Si plated steel sheet which has excellent chemical conversion treatability, which satisfactorily suppresses under-coat blistering from the edges, and which has excellent corrosion resistance at dissimilar joints in contact with an aluminum alloy at a processed portion.

Claims

[Claim 1] A steel sheet having a base steel sheet and a plating layer formed on at least one surface of the base steel sheet, The plating layer has a composition, in mass%, of Mg: 0.50 to 3.00%, Al: 0.10 to 3.00%, Si: 0.010 to 0.20%, and Fe: 0.30% or less, with the balance being Zn and unavoidable impurities; and Zn-Al-MgZn. 2 A ternary eutectic structure; In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 7.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 On the ternary eutectic structure, needle-like Mg with a long side length of 0.5 μm or more is 2 The number density of the Si alloy phase is 100,000 pieces / mm 2 Less than (0 pieces / mm 2 (including In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 On the ternary eutectic structure, needle-like Mg with a long side length of 0.5 μm or more is 2 The number density of the Si alloy phase is 500 pieces / mm 2 There are more than In a backscattered electron image at a magnification of 5000 times obtained by irradiating the surface of the plating layer with an electron beam at an accelerating voltage of 15.0 kV using a scanning electron microscope, the Zn-Al-MgZn 2 On the ternary eutectic structure, needle-like SiO having a long side length of 0.5 μm or more is 2 The oxide phase has a density of 100,000 particles / mm 2 The Zn-Al-Mg-Si plated steel sheet is characterized in that the above-mentioned components are present.

Citation Information

Patent Citations

  • Plated steel

    WO2018139619A1

  • Plated steel

    WO2018139620A1

  • Production of hot-dip zn-mg-al coated steel sheet

    JP1992147955A

  • Non-removable coating type lubricated plated steel sheet excellent in workability

    JP2004338397A

  • Highly corrosion-resistant hot-dip plating steel sheet and manufacturing method therefor