Plating solution purification filters

A filter with controlled activated carbon properties efficiently removes decomposition products from plating solutions, addressing uneven plating issues by minimizing chlorine elution and additive loss, ensuring high-quality finishes.

JP7576006B2Active Publication Date: 2024-10-30KURARAY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021112350
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-27
Filing Date
2021-07-06
Publication Date
2024-10-30
Estimated Expiration
2039-12-24

AI Technical Summary

Technical Problem

Existing filters for purifying plating solutions, particularly acidic copper foil solutions, fail to efficiently remove decomposition products from additives while suppressing the removal of necessary additives and elution of chlorine, leading to uneven plating finishes.

Method used

A filter containing activated carbon with specific iodine adsorption amounts (930 to 1300 mg/g) and controlled chloride ion concentrations (6.0 to 9.0 mg/g) is used to remove decomposition products while minimizing the elution of chlorine and additives, ensuring high-quality plating finishes.

Benefits of technology

The filter effectively removes decomposition products from plating solutions, suppresses chlorine elution, and maintains the integrity of additives, resulting in high-quality plating finishes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576006000004
    Figure 0007576006000004
  • Figure 0007576006000005
    Figure 0007576006000005
  • Figure 0007576006000006
    Figure 0007576006000006
Patent Text Reader

Abstract

To provide an activated carbon containing filter for purifying a plating solution capable of efficiently removing decomposition products generated from additives from the plating solution.SOLUTION: A filter for purifying a plating solution has a molded body 6 containing an adsorbent comprising activated carbon and having an iodine adsorption capacity per unit mass of 930-1,300 mg / g. A chloride ion concentration of filtered water collected after filtering raw water having a chloride ion concentration of 6.0-9.0 mg / L, a pH of 6.9-7.5, and an electrical conductivity of 90-130 μS / cm for one minute is less than or equal to the chloride ion concentration of the raw water.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a filter for refining a plating solution and an adsorbent for refining a plating solution. [Background technology]

[0002] Filters containing activated carbon are widely used for purifying liquids, not limited to water purification applications. For example, Patent Document 1 discloses an activated carbon-containing filter used for purifying an alkali-resistant plating solution.

[0003] On the other hand, in addition to the plating components, various additives are added to the plating solution to improve the plating finish. For example, polymer organic compounds such as polyethylene glycol, polyvinyl alcohol, and gelatin are added as additives to the plating solution for electrolytic plating. It is known that these polymer organic compounds gradually decompose in the solution each time electrolytic plating is performed, turning into low molecular weight decomposition products that are impurities. If the decomposition products increase in the plating solution, problems will occur in the plating finish, so it is necessary to remove the decomposition products.

[0004] For example, Patent Document 2 discloses a method of using an activated carbon-containing filter to remove decomposition products from a plating solution and reuse the plating solution.

[0005] However, according to the investigations of the present inventors, when an acidic copper foil plating solution is used, and the decomposition products are adsorbed and removed using an activated carbon-containing filter, plating is sometimes defective in the plating finish, such as uneven plating.

[0006] As a result of investigating the cause of this defect, the inventors found that a high chlorine concentration in the acidic copper foil plating solution promotes the dissolution of the anode metal and metallic copper in the plating solution, resulting in uneven plating, and that chlorine dissolves from the activated carbon-containing filter into the regenerated plating solution.

[0007] Furthermore, it was found that the activated carbon-containing filter removes not only decomposition products but also necessary additives consisting of high molecular weight organic compounds from the regenerated plating solution, which also causes defects in the plating finish.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a filter for purifying a plating solution, which can efficiently remove decomposition products generated from additives from a plating solution while suppressing removal of the additives, and can suppress elution of chlorine into the plating solution, and to provide an activated carbon adsorbent for obtaining the filter for purifying a plating solution. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2012-61390 A [Patent Document 2] JP 2005-240108 A Summary of the Invention

[0010] As a result of extensive investigations, the present inventors have found that the above object can be achieved by the following invention.

[0011] A plating solution purification filter according to one aspect of the present invention includes a molded body containing an adsorbent made of activated carbon and having an iodine adsorption amount per unit mass of 930 to 1300 mg / g, and the chloride ion concentration of filtrate collected after filtering raw water having a chloride ion concentration of 6.0 to 9.0 mg / L, a pH of 6.9 to 7.5, and an electrical conductivity of 90 to 130 μS / cm for 1 minute is equal to or lower than the chloride ion concentration of the raw water.

[0012] An adsorbent for purifying a plating solution according to another aspect of the present invention is an adsorbent for purifying a plating solution made of activated carbon, the adsorbent having an iodine adsorption amount per unit mass of 1000 to 1400 mg / g, an ash content of the activated carbon being 0.5 mass% or less, and a chloride content of the activated carbon being 0.0030 mass% or less. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a perspective view of a mold for preparing a molded body of the filter for refining a plating solution according to this embodiment. [Diagram 2] FIG. 2 is a perspective view showing an example of a molded body of this embodiment obtained using the mold frame of FIG. [Diagram 3] FIG. 3 is a diagram for explaining how to cut out a sample when measuring the specific surface area, etc., of the activated carbon in the molded body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these.

[0015] (Filter for refining plating solution) The filter for purifying a plating solution of this embodiment includes a molded body containing an adsorbent made of activated carbon and having an iodine adsorption amount per unit mass of 930 to 1300 mg / g, and the chloride ion concentration of filtrate collected after filtering raw water having a chloride ion concentration of 6.0 to 9.0 mg / L, a pH of 6.9 to 7.5, and an electrical conductivity of 90 to 130 μS / cm for 1 minute is equal to or lower than the chloride ion concentration of the raw water.

[0016] With such a configuration, it is possible to efficiently remove decomposition products generated from the additives from the plating solution while suppressing removal of the additives, and it is also possible to suppress the elution of chlorine into the plating solution.

[0017] This is believed to be because, by specifying the lower limit of the iodine adsorption amount per unit mass of the molded body, the removal performance of decomposition products generated from the additives from the plating solution can be ensured, and, by specifying the upper limit of the iodine adsorption amount, removal of the additives from the plating solution can be suppressed.

[0018] In addition, it is believed that dissolution of chlorine into the plating solution can be suppressed by controlling the chloride ion concentration of the filtrate obtained by filtering raw water using the plating solution purification filter of this embodiment to a predetermined value or less.

[0019] The iodine adsorption amount per unit mass of the molded body included in the plating solution purification filter of this embodiment (hereinafter also referred to as "molded body iodine adsorption amount") is 930 to 1300 mg / g. If the molded body iodine adsorption amount is less than 930 mg / g, the decomposition products cannot be sufficiently removed from the plating solution, which adversely affects the plating formed. On the other hand, if the molded body iodine adsorption amount is more than 1300 mg / g, not only the decomposition products but also the additives are removed from the plating solution, and the plating cannot be formed sufficiently. The molded body iodine adsorption amount is preferably 940 mg / g or more, more preferably 950 mg / g or more. In addition, the molded body iodine adsorption amount is preferably 1290 mg / g or less, more preferably 1200 mg / g or less. In this embodiment, the molded body iodine adsorption amount is measured and calculated by the method of determining "iodine adsorption performance" specified in JIS K 1474:2014 (activated carbon test method) as described in the examples described later.

[0020] In the plating solution purification filter of this embodiment, the chloride ion concentration of the filtrate (hereinafter simply referred to as "filtrate") collected after filtering the raw water for 1 minute using the filter is equal to or lower than the chloride ion concentration of the raw water. If the chloride ion concentration of the filtrate is higher than that of the raw water, chlorine will be dissolved in the plating solution from which decomposition products have been removed by filtration, which will have an adverse effect on the plating formed. However, according to the plating solution purification filter of this embodiment, the adverse effect on the plating caused by chlorine can be suppressed. The difference between the chloride ion concentration of the filtrate and that of the raw water (the value obtained by subtracting the chloride ion concentration of the raw water from the chloride ion concentration of the filtrate) is preferably -0.5 mg / L or less. In this embodiment, the chloride ion concentrations of the raw water and the filtrate are measured by an ion chromatography method described in the examples described later.

[0021] Here, the reason why the chloride ion concentration of the filtered water is higher than that of the raw water is due to chlorine or chlorides (hereinafter referred to as "chlorine, etc.") contained in the activated carbon constituting the molded body. Activated carbon, particularly that made from plant-based carbonaceous materials such as coconut shells, contains a certain amount of chlorine, etc. as impurities. The chlorine, etc. contained in the activated carbon can be reduced by washing the activated carbon with an acid to reduce impurities other than chlorine, etc., and then subjecting it to a heat treatment. However, if the activated carbon contains more chlorine, etc. than its adsorption capacity allows, the chloride ion concentration of the filtered water may be higher than that of the raw water.

[0022] In the filter for purifying a plating solution according to the present embodiment, the electrical conductivity of the filtrate collected after filtering the raw water for 1 minute using the filter is preferably equal to or less than the electrical conductivity of the raw water plus 5 μS / cm (the value obtained by subtracting the electrical conductivity of the raw water from the electrical conductivity of the filtrate is equal to or less than 5 μS / cm). The electrical conductivity of the filtrate increases due to impurities such as metal components and chlorine eluted from the molded body. If the electrical conductivity of the filtrate is higher than the value obtained by adding 5 μS / cm to the electrical conductivity of the raw water, metal components eluted from the activated carbon, chlorine, etc. will be eluted into the plating solution from which decomposition products have been removed by filtration, which may adversely affect the plating formed. The difference between the electrical conductivity of the filtrate and the electrical conductivity of the raw water (the value obtained by subtracting the electrical conductivity of the raw water from the electrical conductivity of the filtrate) is more preferably equal to or less than 3 μS / cm, and even more preferably equal to or less than 1 μS / cm. There is no particular limit to the lower limit of the electrical conductivity of the filtrate, but if the electrical conductivity is too low, the cost of the molded body will be excessively high. Therefore, the difference between the electrical conductivity of the filtrate and that of the raw water is preferably -7 μS / cm or more, more preferably -6 μS / cm or more. In this embodiment, the electrical conductivity of the raw water and the filtrate is measured using a pH meter "F-74" and a ToupH electrode "9615S-10D" (both manufactured by Horiba Advanced Techno Co., Ltd.).

[0023] Here, the raw water used in the evaluation of the chloride ion concentration and the electrical conductivity has a chloride ion concentration of 6.0 to 9.0 mg / L, a pH of 6.9 to 7.5, and an electrical conductivity of 90 to 130 μS / cm. This raw water can be purified water obtained by filtering tap water using activated carbon for water purification. The chloride ion concentration, pH, and electrical conductivity of the purified water are measured, and if all of the items are within the above ranges, the purified water can be used as is as the raw water for evaluation. If the chloride ion concentration of the purified water is lower than the above range, it can be increased by adding sodium chloride (NaCl), and if the chloride ion concentration of the purified water is higher than the above range, it can be decreased by adding ion-exchanged water. If the electrical conductivity of the purified water is lower than the above range, it can be increased by adding sodium sulfate (Na2SO4), and if the electrical conductivity of the purified water is higher than the above range, it can be decreased by adding ion-exchanged water. As the activated carbon for water purification used for adjusting the raw water, a commercially available product can be used.

[0024] The plating solution purification filter of this embodiment preferably has a methylene blue circulation adsorption number of 4 to 12. The methylene blue circulation adsorption number refers to the number of times (the number of times methylene blue is added plus 1) that 2 L of an aqueous methylene blue solution with an initial concentration of about 120 mg / L is circulated through the plating solution purification filter, and if the concentration of the aqueous methylene blue solution 30 minutes after the start of the circulation is 2 mg / L or less, methylene blue is added so that the initial concentration is reached, and circulation is continued, until the concentration of the aqueous methylene blue solution 30 minutes after the addition of methylene blue exceeds 2 mg / L.

[0025] If the number of times of circulation of methylene blue is less than 4, the decomposition products cannot be sufficiently removed from the plating solution, which adversely affects the plating formed. On the other hand, if the number of times of circulation of methylene blue is more than 12, not only the decomposition products but also the additives are removed from the plating solution, and the plating cannot be formed sufficiently. The number of times of circulation of methylene blue is preferably 5 times or more, more preferably 6 times or more. In addition, the number of times of circulation of methylene blue is preferably 11 times or less, more preferably 10 times or less. In this embodiment, the number of times of circulation of methylene blue is measured by the method described in the examples below.

[0026] In the plating solution purification filter of this embodiment, the ratio of the volume of pores having a diameter of 1.0 nm or more and 1.5 nm or less of the activated carbon measured by the MP method to the total pore volume of the activated carbon measured at a pore volume calculation relative pressure of 0.990 (hereinafter referred to as "1 nm pore volume ratio") is preferably 2.3% or more. If the 1 nm pore volume ratio is less than 2.3%, decomposition products cannot be sufficiently removed from the plating solution, which has an adverse effect on the plating formed. The 1 nm pore volume ratio is preferably 2.8% or more, more preferably 3.0% or more. In this embodiment, the 1 nm pore volume ratio is measured by the method described in the Examples below.

[0027] In the plating solution purification filter of this embodiment, the average pore diameter of the activated carbon measured by the MP method is preferably 1.70 nm or more and 1.92 nm or less. If the average pore diameter of the activated carbon is less than 1.70 nm, the decomposition products cannot be sufficiently removed from the plating solution, which adversely affects the plating formed. On the other hand, if the average pore diameter of the activated carbon is larger than 1.92 nm, not only the decomposition products but also the additives are removed from the plating solution, and the plating cannot be formed sufficiently. The average pore diameter of the activated carbon is preferably 1.71 nm or more, more preferably 1.74 nm or more. In addition, the average pore diameter of the activated carbon is preferably 1.91 nm or less, more preferably 1.88 nm or less. In this embodiment, the average pore diameter of the activated carbon is measured by the method described in the examples described later.

[0028] (activated carbon) The activated carbon used as an adsorbent in the molded body of the filter for refining a plating solution of the present embodiment preferably has an iodine adsorption amount per unit mass of 1000 to 1400 mg / g, an ash content of 0.5 mass% or less, and a chloride content of 0.0030 mass% or less.

[0029] If the iodine adsorption amount per unit mass of activated carbon (hereinafter also referred to as "activated carbon iodine adsorption amount") is less than 1000 mg / g, even if a filter for purifying a plating solution made using this activated carbon is used, the decomposition products cannot be sufficiently removed from the plating solution, which adversely affects the plating formed. On the other hand, if the activated carbon iodine adsorption amount is greater than 1400 mg / g, not only the decomposition products but also the additives are removed from the plating solution by using a filter for purifying a plating solution made using this activated carbon, and the plating cannot be formed sufficiently. The activated carbon iodine adsorption amount is preferably 1050 mg / g or more, more preferably 1060 mg / g or more. In addition, the activated carbon iodine adsorption amount is preferably 1390 mg / g or less, more preferably 1380 mg / g or less. In this embodiment, the activated carbon iodine adsorption amount is measured and calculated by the same method as the above-mentioned molded body iodine adsorption amount.

[0030] If the ash content of the activated carbon exceeds 0.5% by mass, the ash will dissolve into the plating solution filtered using a plating solution purification filter made using the activated carbon, adversely affecting the plating formed. In order to suppress the dissolution of the ash into the plating solution, the ash content of the adsorbent is preferably 0.4% by mass or less, more preferably 0.3% by mass or less.

[0031] If the chloride content of the activated carbon exceeds 0.0030% by mass, chloride will dissolve into the plating solution filtered using a plating solution purification filter made using this activated carbon, adversely affecting the plating formed. In order to suppress the dissolution of chloride into the plating solution, the chloride content of the activated carbon is preferably 0.0029% by mass or less, and more preferably 0.0020% by mass or less.

[0032] The activated carbon of the present embodiment may be, for example, activated carbon obtained by subjecting a carbonaceous material to at least one of carbonization and activation.

[0033] When carbonization of a carbonaceous material is required, it can be performed, for example, at about 400 to 800°C, preferably 500 to 800°C, and more preferably 550 to 750°C, while blocking oxygen or air. As the activation method, either a gas activation method or a chemical activation method can be adopted, or both may be combined, and the gas activation method, which leaves less impurities, is particularly preferred. The gas activation method can be performed by reacting the carbonized carbonaceous material with an activation gas (for example, water vapor, carbon dioxide gas, etc.) at, for example, about 750 to 1100°C, preferably 800 to 980°C, and more preferably 850 to 950°C. In consideration of the safety of the work and the reactivity of the carbonaceous material, the activation gas is preferably a water vapor-containing gas containing 10 to 40% by volume of water vapor. The activation time and the temperature rise rate are not particularly limited, and can be appropriately selected depending on the type, shape, and size of the carbonaceous material selected.

[0034] The carbonaceous material is not particularly limited, and examples thereof include plant-based carbonaceous materials (e.g., plant-derived materials such as wood, sawdust, charcoal, fruit shells such as coconut shells and walnut shells, fruit seeds, pulp manufacturing by-products, lignin, and blackstrap molasses), mineral-based carbonaceous materials (e.g., mineral-derived materials such as peat, lignite, brown coal, bituminous coal, anthracite, coke, coal tar, coal pitch, petroleum distillation residue, and petroleum pitch), synthetic resin-based carbonaceous materials (e.g., synthetic resin-derived materials such as phenolic resins, polyvinylidene chloride, and acrylic resins), and natural fiber-based carbonaceous materials (e.g., natural fibers such as cellulose, and regenerated fibers such as rayon). These carbonaceous materials can be used alone or in combination of two or more. Among these carbonaceous materials, coconut shells and phenolic resins are preferred from the viewpoint of obtaining a molded body having the above-mentioned characteristics, and coconut shells are more preferred.

[0035] The activated carbon after activation may be washed to remove ash and chemicals, especially when using plant-based carbonaceous materials such as coconut shells or mineral-based carbonaceous materials. An acid is used for washing, and hydrochloric acid is preferred as the acid because of its high washing efficiency. After pickling, the acid is thoroughly washed away with water.

[0036] The shape of the activated carbon in this embodiment may be any of powder, particulate, fibrous (fiber, woven fabric (cloth), felt), etc., and can be appropriately selected depending on the application, but a particulate shape with high adsorption performance per volume is preferred.

[0037] The particle size of the activated carbon in this embodiment is not particularly limited, but the 50% particle size (D50) in the cumulative particle size distribution based on volume is preferably about 120 to 170 μm, more preferably about 125 to 165 μm, and even more preferably about 130 to 160 μm. If the activated carbon has a particle size in such a range, it is easy to obtain a molded body that can efficiently remove decomposition products generated from the additives from the plating solution while suppressing the removal of the additives. In this embodiment, the above-mentioned D50 value is a value measured by a laser diffraction / scattering method, and can be measured, for example, by a wet particle size distribution measuring device (Microtrac MT3300EX II) manufactured by Nikkiso Co., Ltd.

[0038] (binder) The molded body of this embodiment preferably contains a fibrous binder. The fibrous binder is not particularly limited as long as it can be shaped by entangling the activated carbon, can be mixed with the activated carbon after pickling, and has acid resistance to enable the filter to be used in an acidic plating solution, and can be widely used regardless of whether it is a synthetic product or a natural product. Examples of such binders include acrylic fibers, polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, cellulose fibers, nylon fibers, aramid fibers, and pulp. The fiber length of the fibrous binder is preferably 4 mm or less.

[0039] These fibrous binders may be used in combination of two or more kinds. It is particularly preferable to use polyacrylonitrile fiber or cellulose pulp as a binder. This can further increase the density and strength of the molded body and suppress the deterioration of performance.

[0040] In this embodiment, the water permeability of the fibrous polymer binder is about 10 to 150 mL in terms of CSF value. In this embodiment, the CSF value is a value measured in accordance with JIS P 8121-2:2012 (Pulp-Freeness Test Method-Part 2: Canadian Standard Freeness Method). The CSF value can be adjusted, for example, by fibrillating the binder.

[0041] If the CSF value of the fibrous polymer binder is less than 10 mL, liquid permeability may not be achieved and pressure loss may increase, while if the CSF value exceeds 150 mL, the powdered activated carbon may not be sufficiently retained, resulting in a molded body with low strength and poor adsorption performance.

[0042] The mixture ratio of the activated carbon and the fibrous binder in the molded body of this embodiment is preferably about 4.0 to 6.0 parts by mass of the fibrous binder per 100 parts by mass of the activated carbon in terms of the adsorption effect of decomposition products in the plating solution, moldability, etc. If the amount of the fibrous binder is less than 4.0 parts by mass, there is a risk that the molded body cannot be molded because sufficient strength cannot be obtained. Also, if the amount of the fibrous binder exceeds 6.0 parts by mass, there is a risk that the adsorption performance decreases. More preferably, it is desirable to mix 4.5 to 5.5 parts by mass of the fibrous binder.

[0043] (Modification of plating solution purification filter) The filter for refining a plating solution according to the present embodiment may be a cylindrical filter having a center core in addition to the molded body. The cylindrical shape has the advantage of being able to reduce the resistance to liquid passage.

[0044] The core that can be used in this embodiment is not particularly limited as long as it can be inserted into the hollow part of a cylindrical molded body and reinforce the molded body, but for example, a trical pipe, a netron pipe, a ceramic filter, a cylindrical nonwoven fabric laminated pipe, etc. are preferable. Furthermore, a nonwoven fabric or the like can be wrapped around the outer periphery of the core.

[0045] In addition, the filter for refining a plating solution of the present embodiment may have a nonwoven fabric wrapped around the outer periphery of a cylindrical molded body, or may have gaskets adhered to the end faces on both sides of the molded body.

[0046] (How to use filters for refining plating solutions) The plating solution purification filter of the present embodiment is used by immersing it in a plating solution tank that contains a plating solution. By circulating the plating solution through the filter, it is possible to adsorb and remove decomposition products generated from the additives while suppressing removal of the additives in the plating solution.

[0047] (Method of manufacturing molded body) The molded body included in the filter for refining a plating solution according to the present embodiment can be manufactured by any method, and is not particularly limited. The slurry suction method is preferred in terms of efficient manufacturing.

[0048] As an example, the method for producing a cylindrical molded body according to this embodiment will be described in detail below, but the present invention is not limited to this.

[0049] Specifically, for example, a cylindrical molded body can be obtained by a manufacturing method including a slurry preparation step of dispersing powdered activated carbon and a fibrous binder in water to prepare a slurry, a suction filtration step of filtering the slurry while suctioning to obtain a premolded body, a drying step of drying the premolded body to obtain a dried molded body, and, if necessary, a grinding step of grinding the outer surface of the molded body.

[0050] (Slurry preparation process) In this embodiment, in the slurry preparation step, a slurry is prepared by dispersing powdered activated carbon and a fibrous binder in a solvent so that, for example, the fibrous binder is 4.5 to 5.5 parts by mass relative to 100 parts by mass of activated carbon, and the solid content concentration is 4.0 to 6.0 mass% (particularly preferably 4.5 to 5.5 mass%). The solvent is not particularly limited, but it is preferable to use water or the like. If the solid content concentration of the slurry is too high, there is a problem that the dispersion is likely to become non-uniform and the molded body is likely to have spots. On the other hand, if the solid content concentration is too low, not only does the molding time increase and the productivity decrease, but the density of the molded body increases, and clogging is likely to occur due to the capture of turbid components.

[0051] (Suction filtration process) Next, in the suction filtration step, for example, as shown in Fig. 1, a core as described above is attached to a cylindrical molding frame 1 having a large number of small suction holes 3 on the surface of a core body 2 and flanges 4, 4' attached to both ends, and the core is immersed in the slurry contained in a container, and the slurry is filtered while being sucked from the inside of the frame 1 through a filtrate outlet 5, thereby attaching the slurry to the frame 1. As a suction method, a conventional method such as a method of sucking using a suction pump or the like can be used. The preform 7 attached to the frame 1 is compressed to a predetermined diameter.

[0052] (drying process) After the preform 7 is molded by the suction filtration process, the flanges 4, 4' at both ends of the mold 1 are removed, and the core 2 is pulled out to obtain the preform 7 having a hollow cylindrical shape. In the drying process, the preform 7 removed from the mold 1 is dried in a dryer or the like to obtain the molded body 6 (the molded body of this embodiment) shown in Fig. 2.

[0053] The drying temperature is, for example, about 100 to 150°C (particularly, 110 to 130°C), and the drying time is, for example, about 4 to 24 hours (particularly, 8 to 16 hours). If the drying temperature is too high, the fibrous binder is likely to be altered or melted, resulting in a decrease in the filtering performance and a decrease in the strength of the molded body 6. If the drying temperature is too low, the drying time may be long or the drying may be insufficient.

[0054] (Grinding process) If necessary, after the drying step, a grinding step can be performed to further adjust the outer diameter of the filter or to reduce unevenness on the outer peripheral surface. The grinding means used in this embodiment is not particularly limited as long as it can grind (or polish) the outer surface of the dried molded body 6, and a conventional grinding method can be used, but from the viewpoint of grinding uniformity, a method using a grinding machine that rotates and grinds the molded body 6 itself is preferred.

[0055] The grinding step is not limited to the method using a grinding machine, and may be performed, for example, by grinding the molded body 6 fixed to a rotating shaft with a fixed flat grinding wheel. In this method, the generated grinding swarf tends to accumulate on the grinding surface, so it is effective to perform grinding while blowing air.

[0056] The molded body thus obtained can be used as the filter for purifying a plating solution of the present embodiment. For example, after the molded body is produced by the above-mentioned production method, it can be cut into a desired size and shape depending on the amount of plating solution to be processed, etc., to obtain a filter for purifying a plating solution. Furthermore, if necessary, a core may be inserted into the hollow part of the molded body, a cap may be attached to the tip part of the molded body, or a nonwoven fabric may be wrapped around the outer periphery of the molded body.

[0057] (Adsorbent for refining plating solution) The adsorbent for purifying a plating solution according to another embodiment of the present invention is an adsorbent for purifying a plating solution made of activated carbon, and has an iodine adsorption amount per unit mass of 1000 to 1400 mg / g, an ash content of the activated carbon of 0.5 mass% or less, and a chloride content of the activated carbon of 0.0030 mass% or less. The reasons for specifying the iodine adsorption amount, the ash content, and the chloride content are the same as the reasons for specifying these items of the activated carbon described above.

[0058] By using the adsorbent for purifying a plating solution according to this embodiment, it is possible to efficiently remove decomposition products generated from the additives from the plating solution while suppressing removal of the additives, and it is also possible to suppress the elution of chlorine and ash into the plating solution. The adsorbent for a plating solution according to this embodiment can be used in the above-mentioned filter for purifying a plating solution.

[0059] As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.

[0060] A plating solution purification filter according to one embodiment of the present invention includes a molded body containing an adsorbent made of activated carbon and having an iodine adsorption amount per unit mass of 930 to 1,300 mg / g, and the chloride ion concentration of filtrate collected after filtering raw water having a chloride ion concentration of 6.0 to 9.0 mg / L, a pH of 6.9 to 7.5, and an electrical conductivity of 90 to 130 μS / cm for 1 minute is equal to or lower than the chloride ion concentration of the raw water.

[0061] With this configuration, it is possible to provide a filter for refining a plating solution that can efficiently remove decomposition products generated from the additives while suppressing removal of the additives, and can also suppress the elution of chlorine into the plating solution.

[0062] The filter for purifying a plating solution may have an electric conductivity of the filtered water equal to or less than the electric conductivity of the raw water plus 5 μS / cm, thereby making it possible to suppress the elution of metal components and the like into the plating solution and to form a high-quality plating.

[0063] In the above-mentioned plating solution refining filter, the molded body may contain a fibrous binder, which makes the molded body less likely to lose its shape and enables efficient removal of decomposition products generated from the additives from the plating solution while stably suppressing removal of the additives over a long period of time.

[0064] In the above-mentioned plating solution refining filter, the activated carbon may be made from coconut shell as a raw material, thereby making it possible to produce the plating solution refining filter at low cost.

[0065] The plating solution purification filter may have a methylene blue circulation adsorption number of 4 to 12. This makes it possible to efficiently remove decomposition products generated from the additives from the plating solution while suppressing removal of the additives.

[0066] The plating solution purification filter may have a ratio of the volume of pores having a diameter of 1.0 nm or more and 1.5 nm or less of the activated carbon measured by the MP method to the total pore volume of the activated carbon measured at a pore volume calculation relative pressure of 0.990 of 2.3% or more, thereby making it possible to efficiently remove decomposition products generated from the additives from the plating solution while suppressing removal of the additives.

[0067] In the plating solution purification filter, the activated carbon may have an average pore size of 1.70 nm or more and 1.92 nm or less as measured by an MP method, which makes it possible to efficiently remove decomposition products generated from the additives from the plating solution while suppressing removal of the additives.

[0068] An adsorbent for purifying a plating solution according to another embodiment of the present invention is an adsorbent for purifying a plating solution made of activated carbon, the adsorbent having an iodine adsorption amount per unit mass of 1000 to 1400 mg / g, an ash content of the activated carbon being 0.5 mass% or less, and a chloride content of the activated carbon being 0.0030 mass% or less.

[0069] With this configuration, it is possible to provide an adsorbent for use in purifying a plating solution, which is capable of efficiently removing decomposition products generated from the additives from the plating solution while suppressing removal of the additives, and which is capable of suppressing elution of chlorine into the plating solution, in order to obtain a filter for purifying a plating solution. EXAMPLES

[0070] The present invention will be described in more detail below based on examples, but these examples are not intended to limit the present invention in any way.

[0071] First, the methods for producing the activated carbon, molded body, and filter prepared in each example shown in Tables 1 to 3 will be described.

[0072] [Raw materials for molded bodies] (granular activated carbon) The raw material for granular activated carbons 1 to 11 was coconut shells. The coconut shell char carbonized at 400°C to 600°C was activated with steam at 900°C to 950°C. The activation time was adjusted so as to achieve the target amount of iodine adsorption. The activated carbon after activation was named granular activated carbon 11.

[0073] The activated carbon was washed with dilute hydrochloric acid, then washed with ion-exchanged water, and dried at 120° C. to obtain granular activated carbon. The washed and dried activated carbon was named granular activated carbon 7-9.

[0074] The washed and dried activated carbon was further heat-treated in LPG combustion gas with a heat treatment temperature of 700°C and a water vapor partial pressure of about 40%. The heat-treated activated carbon was named granular activated carbon 1-6 and 10.

[0075] (Activated carbon fiber) Phenol resin is the raw material of the fibrous activated carbon 1. Phenolic resin fibers ("KT-2800" manufactured by Gun-ei Chemical Industry Co., Ltd.) were heat-treated in LPG combustion gas at 980°C to obtain the fibrous activated carbon 1 (2 denier, 800,000 fibers).

[0076] (fibrous binder) As the fibrous binder, "Fibrillated acrylic pulp Bi-PUL / F" manufactured by Nippon Exlan Kogyo Co., Ltd. was used.

[0077] [Manufacturing of molded bodies] (Slurry using granular activated carbon) Granular activated carbons 1 to 10 were pulverized in a ball mill and then classified using a JIS standard sieve with an upper mesh of 80 mesh and a lower mesh of 325 mesh to obtain powdered activated carbons having the particle size (D50) shown in Table 2.

[0078] To 2.0 kg of the powdered activated carbon, 0.11 kg (CSF=55 mL) of the fibrous binder was added in terms of solid content, and the mixture was stirred and dispersed in tap water to prepare 30 L of a slurry.

[0079] (Slurry using fibrous activated carbon) 1 kg of fibrous activated carbon 1 was added to 0.055 kg (CSF = 55 mL) of the above fibrous binder in terms of solid content and 100 L of tap water, and the mixture was placed in a small beater and beaten to form a slurry so that the density of the molded body for measuring the beaten density was 0.22 g / mL.

[0080] The density of the molded body for measuring the beaten density, which was made from the slurry after beating, was measured as follows. A 300-mesh wire net was wrapped around the central axis (core) of a mold (frame) having an outer diameter of 40 mm and an outer diameter flange interval of 50 mm, and having a large number of small suction holes (diameter 3 mm, pitch 5 mm) as shown in Figure 1, so that the outer diameter was 18 mm. The slurry was sucked using this mold to prepare a cylindrical molded body for measuring the beaten density, and the density (beaten density) of the molded body was calculated from the weight and dimensions after drying.

[0081] (Slurry molding) The obtained slurry was sucked into a mold (frame) having an outer diameter of 63 mm, a center axis (core) diameter of 30 mm, and a flange-to-flange length of 245 mm, as shown in Figure 1, and equipped with a center axis filter (MF filter manufactured by Asahi Textile Industries Co., Ltd., nominal mesh size 30 μm, inner diameter 30 mm, outer diameter 33 mm, length 245 mm) until the outer diameter of the preform molded body obtained by sucking the slurry became approximately 65 mm, which is approximately 2 mm larger than the outer diameter of the mold.

[0082] The obtained preform was then compressed and molded (rolling molding) by pressing it with a plate while rotating it until it had the same outer diameter as the mold, and then removed from the mold and dried to complete a cylindrical molded body as shown in Figure 2. A nonwoven fabric (a spunbond nonwoven fabric "Elves T0703WDO" manufactured by Unitika Ltd.) was wrapped around the outer periphery of the completed molded body in one layer, and packings made by punching out a 2 mm thick foamed polyethylene sheet into a doughnut shape with an outer diameter of 63 mm and an inner diameter of 30 mm were attached to both ends of the molded body with a 0.5 mm thick hot melt adhesive, and the length was adjusted to 250 mm to complete a filter for purifying plating solution. This molded body or filter was used in Tests No. 1 to 12.

[0083] Next, the methods for evaluating the activated carbon and molded bodies prepared in each Example shown in Tables 1 to 3, and the methods for evaluating the filtrate obtained in each Example will be described.

[0084] [Ash and chloride content in activated carbon, iodine adsorption capacity of activated carbon] The amount of iodine adsorption (activated carbon iodine adsorption amount) of the activated carbon before mixing with the binder was measured according to the measurement method for "iodine adsorption performance" specified in JIS K 1474:2014 (activated carbon test method). The ash and chloride contents in the activated carbon were also measured according to the method specified in the above JIS.

[0085] [Measurement of metal (Na, K) content in activated carbon] 10 mL of concentrated nitric acid (1.38) was added to 0.1 g of a sample of activated carbon before mixing with the binder, and microwaves were applied using a parallel scale-up microwave synthesis device (CEM's "Microwave MARS6") to produce an activated carbon decomposition liquid.

[0086] The element contents in the decomposition liquid obtained were measured using a multi-type ICP emission spectrometer (Shimadzu Corporation, "ICPE-9820"). Based on the element contents obtained, the element contents in the activated carbon were calculated. The Na and K contents shown in Table 1 are values ​​per 1 kg of activated carbon calculated in this way.

[0087] [Measurement of activated carbon particle size] The particle size (D50) of each activated carbon after grinding in a ball mill was measured by the laser diffraction measurement method described below. That is, the activated carbon to be measured was placed in ion-exchanged water together with a surfactant, ultrasonic vibration was applied to create a uniform dispersion, and the particle size distribution was measured using a particle size distribution measuring device (Microtrac MT3300EX-II manufactured by Microtrac-Bell). The surfactant used was "Polyoxyethylene (10) octylphenyl ether" manufactured by Wako Pure Chemical Industries, Ltd. The analysis conditions are shown below.

[0088] (Analysis conditions) Number of measurements: Average of 3 measurements Measurement time: 30 seconds Distribution display: volume Particle size classification: Standard Calculation mode: MT3000II Solvent name: WATER Upper measurement limit: 2000μm, lower measurement limit: 0.021μm Remaining ratio: 0.00 Passage ratio: 0.00 Remaining ratio setting: Disabled Particle Permeability: Absorption Particle Refractive Index: N / A Particle shape: N / A Solvent refractive index: 1.333 DV value: 0.0882 Transmittance (TR):0.800~0.930 Enhanced Filter: Disabled Flow rate: 70% Ultrasonic output: 40W Ultrasonic time: 180 seconds

[0089] [Measurement of specific surface area, pore volume, and average pore diameter of activated carbon in molded body] Before the attachment of the peripheral nonwoven fabric and packing, the molded body was cut with a cutter knife at a position 115 mm from the end face in the longitudinal direction to a volume of about 6 mL, as shown in Figure 3. The cut sample was placed in a crucible and heated at 700°C in a nitrogen atmosphere for 1 hour, and then cooled to room temperature in a nitrogen atmosphere to prepare a sample for measuring the specific surface area and pore volume. Using this sample, the specific surface area and pore volume of the activated carbon in the molded body were calculated by the following method.

[0090] Specific surface area S1(m 2 / g) was determined by measuring the nitrogen adsorption isotherm at 77 K using a high-precision fully automatic gas adsorption apparatus (Microtrack-Bel Corporation, "BELSORP-mini") and using the BET method.

[0091] The total pore volume V1 (mL / g) was determined from the amount of nitrogen adsorbed using the above-mentioned high-precision fully automatic gas adsorption apparatus. Specifically, the amount of nitrogen adsorbed (V) at a pore volume calculation relative pressure of 0.990 measured using the above-mentioned high-precision fully automatic gas adsorption apparatus was converted to the volume of liquid nitrogen (Vp) using the following formula (1), and the obtained value of Vp was taken as the total pore volume V1 (mL / g). In formula (1), Mg is the molecular weight of the adsorbate (nitrogen) (28.013), ρg (g / cm 3 ) is the density of the adsorbate (nitrogen) (0.808g / cm 3 ). Vp = V × Mg / (22414 × ρg) … (1)

[0092] The average pore diameter D1 (nm) is calculated by multiplying the total pore volume V1 (mL / g) and the specific surface area S1 (m 2 / g) according to the following formula (2). D1 = (V1 / S1) × 4 × 1000 … (2)

[0093] The nitrogen gas adsorption isotherm was analyzed by the MP method, and the total pore volume (mL / g) of pores with diameters in the range of 1.0 to 1.5 nm was calculated. NGCB-BEL.t was used as the standard curve.

[0094] [Molded iodine adsorption amount] A sample was cut out at the same position and size as the sample used to measure the specific surface area of ​​the activated carbon in the molded body. The cut out sample was cut into sample pieces of different sizes and dried at 115°C for 3 hours. After drying, the weight of the sample cooled in a desiccator was measured, and each sample piece was broken up with a spatula to remove lumps, and used as a sample for measuring the iodine adsorption amount of the molded body. Using these samples, the iodine adsorption amount of the molded body was measured according to the measurement method for "iodine adsorption performance" specified in JIS K 1474:2014 (Test method for activated carbon).

[0095] [Methylene blue (MB) circulation times] The cylindrical molded body wrapped with nonwoven fabric was cut to a thickness of 16.3 mm, and gaskets were attached to both ends with hot melt to prepare a sample filter for measuring the MB circulation frequency. The gasket was made by punching out a 2 mm thick foamed polyethylene sheet into a doughnut shape with an outer diameter of 63 mm and an inner diameter of 30 mm. The aqueous solution for measuring the MB circulation frequency (MB aqueous solution) was made by adding methylene blue (MB) to ion-exchanged water to a concentration of approximately 120 mg / L. The column in which the sample filter was set was a homemade one with an inner diameter of 70 mm, with a structure that allowed both ends of the sample filter to be sealed with ribs.

[0096] A sample filter was set on the column, and 2 L of MB aqueous solution was circulated through the sample at OUT-IN at 20°C and a flow rate of 0.56 L / min. If the MB concentration in the MB aqueous solution 30 minutes after the start of the flow was 2 mg / L or less, further MB was added so that the concentration was about 120 mg / L. This operation was repeated until the MB concentration 30 minutes after the MB addition exceeded 2 mg / L. The number of repetitions (the number of MB additions plus 1) until the MB concentration 30 minutes after the start of the flow or the addition of MB exceeded 2 ppm was defined as the MB circulation number.

[0097] The pump used for circulating the solution was a "Digital Pump 07522-20" manufactured by Yamato Scientific Co., Ltd. The concentration of MB in the MB aqueous solution was measured using an ultraviolet-visible spectrophotometer (Shimadzu Corporation's "UV-1800") at a wavelength of 665 nm, after diluting the MB aqueous solution with ion-exchanged water.

[0098] [Raw water] The raw water for filtration was prepared by filtering tap water with activated carbon for water purification and adjusting the water temperature to 20±3° C. The pH of the raw water was 6.9 to 7.5. The chloride ion concentration and electrical conductivity of the raw water used in each example were as shown in Table 3.

[0099] [Measurement of chloride ion concentration in raw water and filtered water] A filter for purifying plating solution, which includes a molded body, a nonwoven fabric wrapped around the outer circumference of the molded body, and packings attached to both ends of the molded body, was set in a plastic housing (Advantec Co., Ltd. "1PA"). Raw water was passed through at a flow rate of 10 L / min. 1 minute after the raw water was filtered and the filtrate started to come out of the plastic housing outlet, 100 ml of the filtrate was sampled and the chloride ion concentration was measured using an ion chromatograph (Thermo Fisher Scientific Co., Ltd. "INTEGRION") under the following conditions. 100 ml of unfiltered raw water was also sampled and the chloride ion concentration was measured in the same manner. If the chloride ion concentration of the filtered water was equal to or lower than the chloride ion concentration of the raw water, the chlorine elution judgment was "○" (OK), and if the chloride ion concentration of the filtered water was higher than the chloride ion concentration of the raw water, the chlorine elution judgment was "×" (NOT OK).

[0100] (Ion chromatographic conditions) Columns: AS23 4×250mm and AS23 4×50mm Suppressor: AERS 500 Carbonate 4mm Eluent: 4.5M sodium carbonate + 0.8mM sodium bicarbonate solution (ultrapure water)

[0101] [Measurement of electrical conductivity of raw water and filtered water] The electrical conductivity of the filtered water and raw water sampled for measuring the chloride ion concentration was measured using a pH meter ("LAQUA F-74" and "ToupH electrode 9615S-10D" manufactured by Horiba Advanced Techno Co., Ltd.).

[0102] [Polyethylene glycol (PEG) removal performance evaluation] The PEG removal performance evaluation was carried out to evaluate the filter's ability to remove decomposition products from the plating solution. In the PEG removal performance evaluation test, the plating solution was replaced with ion-exchanged water, the additive (high molecular weight organic compound) added to the plating solution was replaced with polyethylene glycol 20,000 (PEG20000), and the decomposition products (low molecular weight organic compounds) generated from the additives in the plating solution were replaced with polyethylene glycol 400 (PEG400).

[0103] To evaluate the PEG removal performance, a sample filter similar to the sample filter used to measure the MB circulation number was used.

[0104] Two types of PEG aqueous solutions were used: PEG20000 or PEG400 were added to ion-exchanged water so that the TOC concentration was approximately 1,650 mg / L.

[0105] A sample filter was set on the column, and 5 L of the aqueous PEG solution was circulated through the sample at 20°C and a flow rate of 0.5 L / min. The TOC concentration in the aqueous PEG solution was measured 3 hours after the start of the flow, and the removal rates of PEG20000 and PEG400 from the aqueous PEG solution before the flow were calculated.

[0106] Since it is preferable for the plating solution purification filter of the present invention to remove only decomposition products without removing additives as much as possible, a removal rate of 25% or less for PEG20000, which corresponds to additives, was deemed to pass, and a removal rate of 25% or more for PEG400, which corresponds to decomposition products, was deemed to pass. Those that satisfied both the removal rate of 25% or less for PEG20000 and the removal rate of 25% or more for PEG400 were given the removal performance rating of "○" (acceptable), and those that did not were given the removal performance rating of "×" (not acceptable).

[0107] The pump used for circulating the liquid was "Digital Pump 07522-20" manufactured by Yamato Scientific Co., Ltd. The TOC concentration in the PEG aqueous solution was measured using a total organic carbon meter ("TOC-Lcsh ASI-L" manufactured by Shimadzu Corporation).

[0108] [Plating finish judgment] Using the plating solution filtered through a plating refinement filter, plate-shaped nickel test pieces were copper-plated, and the finished product was visually inspected. Products that could be used as plated products were rated as "Good", products that could be used as plated products were rated as "Good", and products that were unusable due to uneven color or thickness were rated as "Poor".

[0109] The measurement and evaluation results for each of the above items are shown in Tables 1 to 3. Table 1 shows the measurement and evaluation results for the activated carbon before crushing or beating. Table 2 shows the measurement and evaluation results for the filter and the activated carbon in the filter. Table 3 shows the measurement results for the raw water and the filtrate, an evaluation of the filter performance, and an evaluation of the plating finish.

[0110] [Table 1]

[0111] [Table 2]

[0112] [Table 3]

[0113] (Consideration) The filter for purifying a plating solution of this embodiment (an example of the present invention) was able to efficiently remove PEG400 from a PEG solution while suppressing the removal of PEG20000, and was also able to suppress the elution of chlorine into the PEG solution, demonstrating excellent removal performance. Furthermore, when plating was performed using a plating solution filtered through the filter for purifying a plating solution of this embodiment, the result was excellent in the finish.

[0114] In contrast, the filter for refining a plating solution of the Comparative Example was inferior in terms of removal performance or suppression of chlorine elution. Furthermore, when plating processing was performed using the plating solution filtered through the filter for refining a plating solution of the Comparative Example, the finish was inferior.

[0115] From the above, it was confirmed that the filter for purifying a plating solution of the present invention can efficiently remove decomposition products generated from additives from the plating solution while suppressing the removal of additives from the plating solution, and can also suppress the elution of chlorine into the plating solution. In addition, when the filter for purifying a plating solution of the present invention is used, the finished quality of the plated product obtained is good, and therefore it was confirmed that the filter for purifying a plating solution of the present invention is useful as a filter for purifying a plating solution.

[0116] This application is based on Japanese Patent Application No. 2018-245928, filed on December 27, 2018, the contents of which are incorporated herein by reference.

[0117] In order to express the present invention, the present invention has been described adequately and sufficiently through the embodiments with reference to specific examples, but it should be recognized that those skilled in the art can easily change and / or improve the above-mentioned embodiments. Therefore, unless the changes or improvements made by those skilled in the art are at a level that departs from the scope of the claims described in the claims, the changes or improvements are interpreted as being included in the scope of the claims. [Industrial Applicability]

[0118] The present invention has wide industrial applicability in the technical fields relating to filters for purifying plating solutions and adsorbents for purifying plating solutions.

Claims

1. A filter for purifying a plating solution, The present invention is provided with a molded body containing an adsorbent made of activated carbon and having an iodine adsorption amount per unit mass of 930 to 1300 mg / g, raw water having a chloride ion concentration of 6.0 to 9.0 mg / L, a pH of 6.9 to 7.5, and an electrical conductivity of 90 to 130 μS / cm is filtered for 1 minute, and the chloride ion concentration of filtrate collected is equal to or lower than the chloride ion concentration of the raw water; The activated carbon has a chloride content of 0.0030% by mass or less, A plating solution purification filter in which the number of times of methylene blue circulation adsorption is 4 to 12 times, which is the number of times (the number of times methylene blue was added plus 1) that a cycle of circulating and passing 2 L of an aqueous methylene blue solution having an initial concentration of 120 mg / L through the plating solution purification filter and continuing circulation and passing the solution if the concentration of the aqueous methylene blue solution 30 minutes after the start of passing the solution is 2 mg / L or less, is repeated until the concentration of the aqueous methylene blue solution 30 minutes after the addition of the methylene blue exceeds 2 mg / L.

2. 2. The filter for refining a plating solution according to claim 1, wherein the electrical conductivity of the filtrate is equal to or less than the electrical conductivity of the raw water plus 5 μS / cm.

3. 3. The filter for refining a plating solution according to claim 1, wherein the molded body contains a fibrous binder.

4. 4. The filter for refining a plating solution according to claim 1, wherein a ratio of a volume of pores having a diameter of 1.0 nm or more and 1.5 nm or less of the activated carbon measured by an MP method to a total pore volume of the activated carbon measured at a pore volume calculation relative pressure of 0.990 is 2.3% or more.

5. The filter for refining a plating solution according to any one of claims 1 to 4, wherein the activated carbon has an average pore diameter measured by an MP method of 1.70 nm or more and 1.92 nm or less.

Citation Information

Patent Citations

  • Production of activated carbon and activated carbon raw material

    JP1987052113A

  • Plating apparatus and plating method

    JP2005240108A

  • Method and apparatus for highly purifying activated carbon

    JP2008007387A

  • Molded adsorption body and water purification material

    JP2011255310A

  • Filter for purification

    JP2012061390A