Turning tool and manufacturing method thereof

By integrating an HPHT single-crystal diamond substrate with a CVD single-crystal diamond layer facing the base and using brazing, the cutting tool achieves enhanced adhesive strength and processing accuracy, overcoming stress and adhesion issues in previous designs.

JP7576198B1Active Publication Date: 2024-10-30DISCO CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024065823
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-10-30
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

Existing cutting tools using CVD single-crystalline diamond layers face issues with stress relief and processing accuracy due to stress accumulation during epitaxial growth, and HPHT single-crystalline diamond substrates have poor adhesive strength with brazing materials.

Method used

A cutting tool design that integrates an HPHT single-crystal diamond substrate with a CVD single-crystal diamond layer deposited on it, where the CVD layer faces the base, and the cutting edge is bonded using a brazing material to enhance adhesive strength and processing accuracy.

Benefits of technology

The design achieves high adhesive strength and improved processing accuracy, addressing the limitations of previous tools by stabilizing the CVD layer and enhancing the bond with the base.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576198000001_ABST
    Figure 0007576198000001_ABST
Patent Text Reader

Abstract

Provided is a cutting tool that has excellent machining accuracy as a cutting tool and can obtain high adhesive strength with a base, and a method for manufacturing the cutting tool. The cutting tool includes a base 30 and a cutting edge 20 brazed to the base. The cutting edge includes a HPHT single crystal diamond substrate 21 and a CVD single crystal diamond layer 22 deposited on the HPHT single crystal diamond substrate, and the cutting edge and the base are bonded together such that the CVD single crystal diamond layer of the cutting edge faces the base.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cutting tool for grinding and cutting a workpiece, and a method for manufacturing the cutting tool. [Background technology]

[0002] Diamond has the hardest hardness of any substance and is used in machining tools for various materials such as silicon. In recent years, cutting tools with single crystal diamond as the cutting edge have been attracting attention.

[0003] Single crystal diamonds include natural diamonds and synthetic diamonds. Most natural diamonds are type Ia, and contain nitrogen in the lattice or between the lattices. Although type IIa diamonds do exist, there is a large variation in the impurity content and crystal structure, and the quality and performance are not constant, making the supply unstable. Furthermore, the price of natural diamonds fluctuates depending on the amount of diamonds mined, so there are issues with stable supply, and they are expensive and difficult to obtain. On the other hand, synthetic diamonds can be produced with a consistent quality more consistently than natural diamonds, and the supply is stable.

[0004] Therefore, in recent years, synthetic diamonds that are inexpensive and have high durability have been studied. For example, Patent Document 1 proposes a tool using single crystal diamond that has both high hardness and high toughness, is easy to process when making tools, is less likely to crack or chip than tools using natural products or high-temperature high-pressure synthetic Ib products, and has a long life and high chipping resistance when cutting. Patent Document 1 also discloses a technology in which CVD single crystal diamond is epitaxially grown by chemical vapor deposition (hereinafter, referred to as "CVD") on a seed substrate manufactured by high pressure and high temperature (hereinafter, referred to as "HPHT"), and the CVD single crystal diamond layer separated from the seed substrate is used.

[0005] Patent Document 2 discloses a tool using a single crystal diamond suitable for diamond products, which suppresses the stress accumulated between the epitaxially grown single crystal and the substrate. In order to solve this problem, the invention described in Patent Document 2 considers alleviating the stress caused by depositing single crystal diamond on the side as well as the main surface of the HPHT substrate by CVD. The document states that the stress on the CVD single crystal diamond layer can be alleviated by forming a carbonaceous layer on the side of the HPHT substrate. Patent Document 2 also discloses that the HPHT single crystal diamond substrate and the CVD single crystal diamond layer deposited thereon are separated, and the CVD single crystal diamond layer is used for a tool.

[0006] On the other hand, Patent Document 3 discloses a technique of using a HPHT single crystal diamond substrate to improve the toughness and / or wear resistance of a tool. In particular, the tool is disclosed in which at least a portion of the HPHT diamond tool piece contains a ratio of aggregate nitrogen centers to C-nitrogen centers of more than 30%. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2014 / 003110 [Patent Document 2] JP 2015-34114 A [Patent Document 3] Special Publication No. 2019-523741 Summary of the Invention [Problem to be solved by the invention]

[0008] It is known that the surface of a CVD single crystal diamond layer is relatively rough because stress with the substrate cannot be avoided during epitaxial growth. For this reason, the inventions described in Patent Documents 1 and 2 are concerned with the relaxation of stress in a CVD single crystal diamond layer deposited on a HPHT single crystal diamond substrate.

[0009] However, even if the CVD single crystal diamond layer described in Patent Document 1 and Patent Document 2 is used for a tool, it cannot be said that the stress is sufficiently relieved. Even if the method discussed in these documents is used, there is a limit to the stress relief, and stress remains in the CVD single crystal diamond. In particular, in the case of cutting tools, since high processing accuracy is required for the work material in recent years, further study is required.

[0010] It is also known that CVD single-crystalline diamond layers are more difficult to process than HPHT single-crystalline diamond substrates, and as mentioned above, CVD single-crystalline diamond layers tend to have poorer processing accuracy due to the effects of stress during epitaxial growth.

[0011] In addition, the cutting edge of the cutting tool needs to be polished after use to maintain processing accuracy, so a thick plate is better. However, obtaining a thick single crystal diamond using HPHT is time-consuming and expensive.

[0012] On the other hand, in paragraph 0019 of Patent Document 3, it is described that when the ratio of aggregated nitrogen center to C-nitrogen center is more than 30%, aggregated nitrogen center reduces the lattice distortion of diamond compared with the diamond crystal lattice that consists of only C-center.This is because both the time and temperature of annealing affect the ratio of aggregated nitrogen center to C-center.

[0013] Here, paragraph 0014 of Patent Document 3 discloses that a diamond tool is formed by brazing a diamond tool piece to a carrier. However, since the surface of the HPHT single crystal diamond substrate is smooth, it is difficult to obtain a strong adhesive force even when brazed.

[0014] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a cutting tool that is excellent in machining accuracy as a cutting tool and that can obtain high adhesive strength with a base, and a method for manufacturing the cutting tool. [Means for solving the problem]

[0015] Conventionally, as disclosed in Patent Documents 1 to 3, cutting tools using either a CVD single crystal diamond layer or an HPHT single crystal diamond substrate have been used, making it difficult to combine the advantages of both.

[0016] From the viewpoint of improving grinding accuracy and good processability, the inventors first used HPHT single crystal diamond substrates and investigated whether they could achieve high adhesive strength by conventional brazing. Although silver brazing or Cu brazing is used for brazing, which is the process of bonding the cutting edge and the base, it seems that it would be good to investigate brazing materials that can further improve adhesive strength.

[0017] However, since single crystal diamond is not a metal, it is not easy to improve the adhesive strength by brazing, especially in the case of HPHT single crystal diamond substrates. This is presumably because single crystal diamond is not only chemically stable but also thermally stable, so that the constituent elements are unlikely to interdiffuse near the bonding interface between the brazing material and single crystal diamond.

[0018] Therefore, the inventors came up with the idea of ​​improving the adhesive strength physically, rather than metallurgically, and after further investigation, came up with the idea of ​​using the CVD single crystal diamond layer as a cutting edge, without separating it from the HPHT single crystal diamond substrate as in the conventional method.

[0019] In addition, problems such as crystal quality and the difficulty of processing the cutting edge itself have been considered to be issues. This is thought to be because when a CVD single-crystalline diamond layer is deposited on a HPHT single-crystalline diamond substrate by epitaxial growth, stress is applied, resulting in a relatively large amount of surface unevenness. Therefore, the inventors came up with the idea of ​​bonding a CVD single-crystalline diamond layer deposited on a HPHT single-crystalline diamond substrate to a base.

[0020] Here, it has been known that various properties of single crystal diamonds formed by depositing a CVD single crystal diamond layer on a HPHT single crystal diamond substrate are deteriorated due to internal stress, and therefore the use of single crystal diamonds formed by depositing a CVD single crystal diamond layer on a HPHT single crystal diamond substrate for cutting tools has been avoided.

[0021] However, the present inventors have dared to use a cutting edge made by depositing a CVD single crystal diamond layer on an HPHT single crystal diamond substrate, which has been avoided in the past. Furthermore, the present inventors have bonded the cutting edge to the base by brazing so that the CVD single crystal diamond layer faces the base. As a result, a cutting tool using a cutting edge made of single crystal diamond with high grinding accuracy and adhesive strength to the base has been obtained, and the present invention has been completed. The present invention, which has been made based on these findings, is as follows.

[0022] (1) A cutting tool having a base and a cutting edge brazed to the base, the cutting edge comprises a HPHT single crystal diamond substrate and a CVD single crystal diamond layer deposited on the HPHT single crystal diamond substrate; The cutting edge and the base are bonded together so that the CVD single crystal diamond layer on the cutting edge faces the base. A bit tool characterized by the above.

[0023] (2) The bit tool according to (1) above, wherein the HPHT single crystal diamond substrate has a thickness of 0.3 to 3.0 mm.

[0024] (3) The cutting tool according to (1) or (2) above, wherein the CVD single crystal diamond layer has a thickness of 0.1 to 2.0 mm.

[0025] (4 to 5) The cutting tool according to any one of (1) to (3) above, wherein the CVD single-crystalline diamond layer is transparent or yellow in color.

[0026] (6 to 9) The bit tool according to any one of (1) to (5) above, wherein the surface vicinity region of the CVD single crystal diamond layer exhibits a color different from that of the region other than the surface vicinity region of the CVD single crystal diamond layer.

[0027] (10) A method for manufacturing a cutting tool having a base and a cutting edge brazed to the base, comprising the steps of: a CVD single crystal diamond layer deposition step of depositing a CVD single crystal diamond layer on a pre-prepared HPHT single crystal diamond substrate by a CVD method in an atmosphere gas containing an additive gas composed of at least one of oxygen, nitrogen, and / or nitrogen oxide; A manufacturing method for a cutting tool, comprising: a cutting edge bonding step of bonding a cutting edge formed by depositing a CVD single crystalline diamond layer on an HPHT single crystal diamond substrate by a CVD single crystalline diamond layer deposition step to a base by brazing so that the CVD single crystalline diamond layer faces the base.

[0028] (11) The method for producing a cutting tool according to (10) above, wherein during a time period from the last 20 to 0.5% of the process time of the CVD single-crystalline diamond layer deposition step onwards, the amount of additive gas introduced is increased to 2 to 200 times the amount of additive gas introduced during a time period other than the last 20 to 0.5% of the process time.

[0029] (12) The method for producing a cutting tool as set forth in (10) above, wherein the additive gas is introduced only during the final 20 to 0.5% or more of the process time of the CVD single-crystalline diamond layer deposition step.

[0030] (13) A method for producing a bit tool as set forth in any one of (10) to (12) above, comprising a grinding and flattening step of grinding and flattening a deposition surface of the CVD single-crystalline diamond layer deposited in the CVD single-crystalline diamond layer deposition step so that the deposition surface becomes at least partially parallel to a surface of the HPHT single-crystalline diamond substrate.

[0031] (14) The bit tool according to any one of (1) to (9) above, wherein a plurality of protrusions are formed on the surface of the CVD single crystalline diamond layer, and the height difference from the lowest to the highest of the protrusions is 0.05 mm or more.

[0032] (15) The bit tool according to any one of (1) to (9) above, wherein the area of ​​a surface of the CVD single crystal diamond layer that is parallel to the HPHT single crystal diamond substrate is 30 to 95% of the surface area of ​​the CVD single crystal diamond layer.

[0033] (16) The bit tool according to any one of (1) to (9) above, wherein the interval between the convex portions of abnormal growth is at least half the width of the CVD single crystal diamond layer. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is a perspective view of a cutting tool according to the present embodiment. [Diagram 2] FIG. 2 is an exploded perspective view of the cutting tool according to the present embodiment. [Diagram 3] FIG. 3 is a perspective view of a cutting edge constituting the cutting tool according to the present embodiment. [Figure 4] Figure 4 is a process perspective view showing the manufacturing process of the bit tool according to this embodiment, where Figure 4(a) is a perspective view of a pre-prepared HPHT single crystal diamond substrate, Figure 4(b) is a perspective view of the HPHT single crystal diamond substrate on which a CVD single crystal diamond layer has been deposited by the CVD method, and Figure 4(c) is a perspective view of the cutting edge of the HPHT single crystal diamond substrate on which the CVD single crystal diamond layer has been deposited, with the CVD single crystal diamond layer bonded to a base. [Diagram 5] FIG. 5 is a profile showing the relationship between gas type and deposition time (%), illustrating one example of deposition conditions for CVD single-crystalline diamond in the manufacturing process for the cutting tool according to this embodiment. [Figure 6]FIG. 6 is a schematic cross-sectional view of a cutting edge manufactured by the manufacturing method for a bit tool according to this embodiment, showing the state before and after grinding and flattening treatment is performed to make the surface of the cutting edge parallel to the HPHT single crystal diamond substrate of the cutting edge. FIG. 6(a) is a schematic cross-sectional view of the cutting edge before grinding and FIG. 6(b) is a schematic cross-sectional view of the cutting edge after grinding and flattening treatment has been performed. [Figure 7] Figure 7 is an optical microscope photograph of the cutting edge of the bit tool according to this embodiment, with Figure 7(a) being the HPHT single crystal diamond substrate before the CVD single crystal diamond layer was deposited in Example 2, and Figure 7(b) being the CVD single crystal diamond layer deposited on the HPHT single crystal diamond substrate in Example 2. [Figure 8] Figure 8 shows photographs of the cutting edge of Example 2, in which the CVD single-crystalline diamond layer was deposited under deposition conditions in which the amount of nitrogen introduced was increased from 0.05 volume parts to 0.20 volume parts when the amount of hydrogen introduced was 100 volume parts for the final 5 hours of the total deposition time. Figure 8(a) is an optical microscope photograph of the cutting edge, and Figure 8(b) is an SEM photograph of the cutting edge after grinding and flattening. [Figure 9] Figure 9 shows photographs of the cutting edge of Example 3, in which the CVD single-crystalline diamond layer was deposited under deposition conditions in which the amount of nitrogen introduced was increased from 0.10 volume parts to 0.50 volume parts when the amount of hydrogen introduced was 100 volume parts for the final 3 hours of the total deposition time. Figure 9(a) is an optical microscope photograph of the cutting edge, and Figure 9(b) is an SEM photograph of the cutting edge after grinding and flattening. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail with reference to the accompanying drawings. The present invention is not limited to the following embodiments. In addition, the present invention may be implemented in a form in which the respective embodiments are combined.

[0036] 1. Tool bits (1) Overview of tool bits Fig. 1 is a perspective view of the cutting tool 1 according to this embodiment. Fig. 2 is an exploded perspective view of the cutting tool 1 according to this embodiment. The cutting tool 1 shown in Figs. 1 and 2 is composed of a cutting edge 20 and a base 30 to which the cutting edge 20 is fixed by brazing material. This may be used as the cutting tool 1 as is, but depending on the grinding device, the cutting edge portion 10 composed of the cutting edge 20 and the base 30 to which the cutting edge 20 is fixed may be detachably attached to a shank 34 by a fastening bolt 38.

[0037] The shank 34 is made of stainless steel and formed into a square column shape as shown in Fig. 1, with a tapered mounting part 341 provided at its tip (lower end). It may be cylindrical, and may have any shape according to the specifications of the grinding device (not shown). A female screw hole 343 is formed in a mounting surface 342 of the mounting part 341 as shown in Fig. 2.

[0038] The base 30 is formed of a hard material such as tungsten carbide, and includes a mounting part 301 having a mounting surface 301a that is detachably mounted on the shank 34, and a tip mounting part 302 to which the cutting edge 20 is brazed. Note that, although the illustrated embodiment shows an example in which the mounting part 301 and the tip mounting part 302 that constitute the base 30 are integrally molded, the mounting part 301 and the tip mounting part 302 may be formed separately and the two parts may be brazed together.

[0039] The base 30 thus formed has a tip mounting portion 302 to which the cutting edge 20 is brazed, which protrudes from the front surface 301b of the mounting portion 301, and the cutting edge 20 is brazed to the tip mounting surface 302a, which is the front surface of the tip mounting portion 302, using a brazing material such as silver-tin.

[0040] The distance between the front surface 301b of the mounting portion 301 constituting the base 30 and the chip mounting surface 302a is set to, for example, 5 mm in the illustrated embodiment. It may be about 3 to 10 mm, and is not particularly limited.

[0041] The thickness of the cutting edge 20 is set to 2 mm in the illustrated embodiment. It may be about 0.5 to 5 mm. A bolt insertion hole 303 is provided in the mounting portion 301 of the base 30. The fastening bolt 38 is inserted into the bolt insertion hole 303 and screwed into the bolt insertion hole 303 formed in the shank 34, whereby the base 30 can be attached to the shank 34. The cutting tool 1 configured as above, or the shank 34 to which the cutting tool 1 is attached, is attached to a grinding device (not shown).

[0042] (2) Cutting edge 3 is a perspective view of a cutting edge portion 10 constituting the cutting tool according to this embodiment. The cutting edge 20 according to the present invention is a single crystal diamond, and is composed of an HPHT single crystal diamond substrate 21 and a CVD single crystal diamond layer 22 deposited on the HPHT single crystal diamond substrate. The cutting edge 20 and the base 30 are brazed with a brazing material 23 so that the CVD single crystal diamond layer 22 constituting the cutting edge portion 10 and the base 30 face each other.

[0043] The HPHT single crystal diamond substrate 21 is of type Ib or type IIa, with type Ib being preferred. From the viewpoint of grinding and polishing the cutting edge of the cutting tool after use and reusing it, the plate thickness is preferably 0.3 mm or more, more preferably 0.5 mm or more, and may be 1.5 mm or more. There is no particular upper limit, but as a manufacturable range, it may be 3.0 mm or less, or may be 2.0 mm or less.

[0044] From the viewpoint of deposition by the CVD method, it is not preferable for the CVD single-crystalline diamond layer 22 to be thicker than necessary from the viewpoint of cost. Therefore, in this embodiment, the upper limit is preferably 2.0 mm or less. The lower limit is sufficient as long as the thickness is thick enough to form the irregularities described below, so that it is sufficient to have a thickness of 0.05 mm or more, and preferably 0.10 mm or more.

[0045] When the HPHT single crystal diamond substrate 21 is thick, the CVD single crystal diamond layer 22 may be thin. When the HPHT single crystal diamond substrate 21 is thin, the CVD single crystal diamond layer 22 may be thick. Since it generally takes a long time to thicken the HPHT single crystal diamond substrate 21, the CVD single crystal diamond may be thick. When the CVD single crystal diamond layer 22 is thick, at least the CVD single crystal diamond layer 22 or its surface is of low quality, and the CVD single crystal diamond may have large irregularities on its surface.

[0046] Considering the life of the cutting edge, it is better to have a thicker HPHT single crystal diamond substrate 21. In this case, the CVD single crystal diamond layer 22 may be thin within the above-mentioned range, so long as the unevenness is formed to such an extent that peeling from the base 30 is suppressed.

[0047] The surface of the CVD single crystal diamond layer 22 is rougher than that of the HPHT single crystal diamond substrate 21. Therefore, stronger adhesion is possible compared to the case where the HPHT single crystal diamond substrate 21 is directly brazed to the base 30. The reason why strong adhesion is possible is presumed to be detailed as follows. Since the brazing material 23 is molten at the time of bonding, the molten brazing material 23 penetrates into the recesses of the CVD single crystal diamond layer 22. Therefore, compared to a smooth surface, the surface with irregularities has a larger specific surface area, so that the contact area between the brazing material 23 and the CVD single crystal diamond layer 22 after solidification increases, and stronger adhesion is possible. The irregularities will be described later.

[0048] In order for the CVD single crystal diamond layer 22 to be more firmly bonded to the base 30, it is better for the crystal quality of the CVD single crystal diamond layer 22 to be inferior. Conventionally, the CVD single crystal diamond layer 22 epitaxially deposited on the HPHT single crystal diamond substrate 21 has been peeled off from the HPHT single crystal diamond substrate 21 and used alone. For this reason, conventionally, the HPHT single crystal diamond substrate on which the CVD single crystal diamond layer 22 is deposited has not been used as it is for tools or the like.

[0049] However, in the cutting tool according to this embodiment, in order to strengthen the brazing to the base 30, the CVD single-crystalline diamond layer 22 is configured based on a technical idea that is the exact opposite of the conventional one. In other words, it is preferable to use a CVD single-crystalline diamond layer 22 with a rough surface and with the same or lower crystal quality as the HPHT single-crystalline diamond substrate 21. The color of the CVD single-crystalline diamond layer 22 may be transparent or yellow. Yellow is preferable.

[0050] The nitrogen contained in the cutting edge 20 strengthens the bond between the homoepitaxial growth interface between the HPHT single crystal diamond substrate 21 and the CVD single crystal diamond layer 22, and reduces crystal stress caused by deposition. Furthermore, the nitrogen incorporated into the diamond crystals leads to a deterioration in the quality of the diamond crystals, and when deposition of the CVD single crystal diamond layer 22 is completed, the entire CVD single crystal diamond layer 22 or the surface of the CVD single crystal diamond layer 22 becomes rough. As a result, the bond strength with the brazing material 23 increases, and peeling from the base 30 can be suppressed.

[0051] In the present invention, the surface vicinity region of the CVD single crystalline diamond layer 22 may have a different color from the other regions of the CVD single crystalline diamond layer 22. That is, even if the CVD single crystalline diamond layer 22 is deposited under deposition conditions aiming at high quality as in the past, if the crystal quality of the surface vicinity region is deteriorated, the surface vicinity region and the other regions will have different colors. If the color of the surface vicinity region of the CVD single crystalline diamond layer 22 is darker than the color of the other regions, the crystal quality of the bonding surface of the CVD single crystalline diamond layer 22 will be more deteriorated, and the unevenness and holes on the surface will be more prominently formed, and the bonding by brazing will be stronger. In addition, the crystal quality of the CVD single crystalline diamond layer 22 will be deteriorated due to the inclusion of nitrogen compared to a crystal without the inclusion of nitrogen, making it easier to machine the cutting edge itself.

[0052] In the present invention, as described above, although the colours of these regions are different in a preferred embodiment, the amount of nitrogen is increased during deposition to deteriorate the crystal quality of the near-surface region of the CVD single-crystalline diamond layer 22. For this reason, the colour of the near-surface region of the CVD single-crystalline diamond layer 22 may be a deeper yellow than the colour of the other regions, or may have changed to a colour other than yellow, such as purple or brown. Naturally, although at least the near-surface region of the CVD single-crystalline diamond layer 22 has a colour different from the other regions, it is not colourless.

[0053] The darker the yellow, the higher the nitrogen content and the poorer the crystal quality. The yellow can be distinguished, for example, based on the GIA COLOR SCALE D to Z. If it is darker than Z, it can be judged by a dark color scale distinguished as a fancy color. Fancy colors include dark yellow, green, red, green, orange, pink, blue, purple, navy blue, and black. The grades are classified in order of lightness into faint, very light, light, fancy light, fancy, fancy dark, and fancy deep. In the present invention, the darker the color, the poorer the crystal quality, so the brazing becomes stronger and the peeling between the base 30 and the cutting edge 20 can be suppressed. The color classification can be done visually.

[0054] The crystal quality of the CVD single-crystalline diamond layer 22 may be defined by the half-width of the Raman spectrum. When the Raman spectrum of the CVD single-crystalline diamond layer 22 is used to define the crystal quality, the FWHM, which is the half-width of the peak of the CVD single-crystalline diamond layer 22, is set to 1.0 to 5.0 cm. -1 Furthermore, the peak shift amount may be determined by shifting the peak of a natural diamond of type Ia containing an extremely small amount of nitrogen or an artificial diamond of type IIa to 1333.0 cm. -1 The peak shift amount of the CVD single crystal diamond layer 22 is −1.0 to +1.0 cm -1The surface of the CVD single-crystalline diamond layer 22 that satisfies at least any one or all of these conditions is rough, and the adhesive strength of the brazing material is improved. In some cases, if holes are formed, even stronger adhesion is possible.

[0055] In the present invention, the "near-surface region of the CVD single-crystalline diamond layer" refers to a depth of up to 0.1 mm from the surface of the CVD single-crystalline diamond layer 22. For example, when the thickness of the CVD single-crystalline diamond layer 22 is 0.1 mm, the crystal quality of the entire CVD single-crystalline diamond layer 22 is poor.

[0056] Furthermore, the CVD single crystalline diamond layer 22 constituting the cutting edge 20 may have a roughened surface to form recesses 22-1 or protrusions 22-2, as shown in Fig. 6(b), for example. The recesses 22-1 may be formed as recesses 22-1 when holes are formed in the flat surface of the CVD single crystalline diamond layer 22. The protrusions 22-2 correspond to the tops of the abnormally grown portions. The formation of the protrusions 22-2 also forms the recesses 22-1 at the same time.

[0057] In this embodiment, the greater the height difference 50 from the bottom end of the recess 22-1 to the top end of the protrusion 22-2, the greater the specific surface area of ​​the CVD single-crystalline diamond layer 22, and the brazing material flows into the recess 22-1 when melted, enabling stronger adhesion. When grinding is performed for smoothing after depositing the CVD single-crystalline diamond layer 22, the height difference is the difference between the bottom end of the recess 22-1 and the highest point of the protrusion 22-2 after grinding flattening. The height difference 50 is preferably more than 0.05 mm and not more than 0.5 mm, and most preferably more than 0.1 mm. The height difference can be obtained by observing the cross section of the cutting edge 20 with an optical microscope.

[0058] Furthermore, if the interval 60 between the protrusions 22-2 on the surface after grinding as shown in FIG. 6(b) is 1 / 2 or more of the width 70 of the CVD single crystalline diamond layer 22, the cutting edge 20 can be stably placed on the base 30. More preferably, the interval 60 is 3 / 5 or more of the width 70, and most preferably 7 / 10 or more. As shown in FIG. 6(b), the tip of the protrusion 22-2 becomes flat when grinding is performed. In this case, the interval 60 may be measured on the parallel surface 22-4 with the portion 22-3 near the outside of the cutting edge 20 as a reference, as shown in FIG. 6(b).

[0059] In addition, as shown in Fig. 6(b), it is preferable that the surface of the CVD single crystal diamond layer 22 has a surface 22-4 parallel to the HPHT single crystal diamond substrate 21. The presence of such parallel surface 22-4 allows for stable mounting on the base 30. The area of ​​surface 22-4 parallel to the HPHT single crystal diamond substrate present on the surface of the CVD single crystal diamond layer is preferably 30 to 95% of the surface area of ​​the CVD single crystal diamond layer.

[0060] When the area ratio is 30-49% and the parallel faces 22-4 are biased toward the end of the CVD single crystalline diamond layer, it is preferable that the cutting edge 20 be placed more stably. In this case, it is preferable that the interval 60 between the protrusions 22-2 is within the above-mentioned range.

[0061] As described above, in the past, after the CVD single-crystalline diamond layer 22 is deposited on the HPHT single-crystalline diamond substrate 21, the CVD single-crystalline diamond layer 22 is separated from the HPHT single-crystalline diamond substrate 21, and the CVD single-crystalline diamond layer 22 is used as a cutting edge. This is because the CVD single-crystalline diamond layer 22 deposited on the HPHT single-crystalline diamond substrate 21 is likely to be damaged during processing because the CVD single-crystalline diamond layer 22 maintains a state in which stress is applied to the CVD single-crystalline diamond layer 22. In addition, since the quality of the CVD single-crystalline diamond layer 22 is different from the crystal quality of the HPHT single-crystalline diamond substrate 21, it is difficult to achieve processing accuracy equivalent to that of the HPHT single-crystalline diamond substrate 21. Therefore, in the past, the HPHT single-crystalline diamond substrate 21 and the CVD single-crystalline diamond layer 22 had to be separated.

[0062] However, since it takes a long time to deposit a thick single crystal diamond by CVD, and the separation process also takes time, the cost is undeniably high. On the other hand, if only the HPHT single crystal diamond substrate 21 is used for the cutting edge 20, the adhesive strength with the brazing material 23 will be inferior because the HPHT single crystal diamond substrate 21 is of high quality.

[0063] In consideration of these circumstances, the cutting tool 1 of the present invention is able to solve the above-mentioned problems by using single crystal diamond, which has a CVD single crystal diamond layer 22 deposited on an HPHT single crystal diamond substrate 21, as the cutting edge 20, which was previously avoided.

[0064] 2. Manufacturing method of tool bits The manufacturing method of the cutting tool according to the present invention will be described with reference to Fig. 4. Fig. 4 is a perspective view showing the manufacturing process of the cutting tool according to this embodiment.

[0065] The manufacturing method of the bit tool according to the present invention comprises a CVD single crystal diamond layer deposition step of depositing a CVD single crystal diamond layer 22 on an HPHT single crystal diamond substrate 21 by a CVD method, and a cutting edge bonding step of brazing the cutting edge 20, on which the CVD single crystal diamond layer 22 has been deposited on the HPHT single crystal diamond substrate 21 by the CVD single crystal diamond layer deposition step, to a base 30 using a braze 23 so that the CVD single crystal diamond layer 22 and the base 30 face each other. The steps will be described below in order with reference to FIG.

[0066] (1) CVD single-crystalline diamond layer deposition process As shown in FIG. 4(a), a HPHT single crystal diamond substrate 21 manufactured by a conventional method is prepared. Then, as shown in FIG. 4(b), a CVD single crystal diamond layer 22 is deposited on the HPHT single crystal diamond substrate 21 to form a cutting edge 20. In the manufacturing method according to the present invention, for example, a microwave plasma CVD device is used to deposit the CVD single crystal diamond layer 22 by epitaxial growth. There is no particular limitation as long as it is a conventional CVD method such as microwave CVD or direct current plasma CVD. The deposition conditions are, for example, a deposition temperature of 700 to 1300°C, an atmosphere of about 50 to 300 Torr, and an additive gas composed of at least one of oxygen, nitrogen, and / or nitrogen oxides in addition to hydrogen or methane as the main gas.

[0067] Furthermore, from the viewpoint of improving the adhesive strength with the brazing material 23, the CVD single crystalline diamond layer 22 constituting the present invention preferably has many projections and recesses formed on its surface at the end of deposition.

[0068] Furthermore, it is preferable to deposit with a larger amount of additive gas than in the past, in order to deteriorate the crystal quality of the CVD single crystal diamond layer 22. For example, in the past, when a CVD single crystal diamond layer was deposited with an additive gas introduction amount of less than 0.1 parts by volume, assuming that hydrogen constituting the main gas is 100 parts by volume, if the additive gas introduction amount is increased to 0.1 to 2.0 parts by volume as in this embodiment, the adhesive strength of the brazing material is improved and interface damage at the HPHT single crystal diamond substrate 21 is also suppressed.

[0069] The atmosphere gas in the CVD single-crystalline diamond layer deposition step may contain, in addition to hydrogen and methane as the main gases, additive gases such as nitrogen, oxygen, and nitrogen oxides. When the atmosphere gas is composed of these mixed gases, the amount of each gas introduced is calculated with the amount of hydrogen introduced being 100 parts by volume. The amount of methane and additive gas introduced that constitute the main gas may be methane introduced amount: additive gas introduced amount = 10.0 to 2.0 parts by volume: 0.0 to 2.0 parts by volume, and is preferably 10.0 to 2.0 parts by volume: 0.01 to 2.0 parts by volume. The volume ratio of the amount of additive gas introduced to the amount of methane introduced may be 0.00 to 40.00%. When the amount of additive gas introduced is increased midway through the CVD single-crystalline diamond layer deposition step, it may be 0.00 to 2.00% at first, and may be increased to 0.50 to 40.00% midway. This volume ratio is a ratio (%) obtained by multiplying the value obtained by dividing the amount of additive gas introduced by the amount of methane introduced by 100.

[0070] In the case where the crystal quality of the CVD single-crystalline diamond layer 22 is significantly deteriorated, it is preferable to increase the proportion of the added gas. 3 The methane input is 5m 3 The amount of added gas introduced was 0.05 m 3 In this case, the amount of methane introduced: the amount of added gas introduced = 5 parts by volume: 0.05 parts by volume, and the volume ratio is 5: 0.05. The added gas is preferably at least one of oxygen, nitrogen, and / or an oxide of nitrogen, and more preferably nitrogen, NO2, or NO.

[0071] In addition, in order to further deteriorate the crystal quality of the surface of the CVD single-crystalline diamond layer 22, it is preferable to increase the additive gas concentration in a time range of 20.0 to 0.5% of the deposition time of the CVD single-crystalline diamond layer 22, the time range being the time range up to the end of the deposition time, and to increase the additive gas concentration in the time range to 2 to 200 times the additive gas concentration in the time range other than the time range. For example, when the deposition time is 50 hours, the additive gas concentration in the atmospheric gas is 10 hours, which is 20% of the deposition time, and the additive gas concentration increases to 2 to 200 times the previous concentration from 10 hours before the end of deposition. For example, the temperature profile shown in FIG. 5 may be used.

[0072] In this embodiment, the atmospheric gas conditions at the start of the CVD single-crystalline diamond layer deposition process may be referred to as the "first stage", and the atmospheric gas conditions in the time region after the additive gas is newly introduced or the amount of additive gas introduced is increased may be referred to as the "second stage". In Fig. 5, 0 to 80% of the volume time (%) is the first stage, and 80 to 100% is the second stage.

[0073] In the manufacturing method according to the present invention, the amount of additive gas introduced may not be increased from the second stage, but may be increased from the first stage and maintained until the end. In this case, the crystal quality of the entire CVD single-crystalline diamond layer 22 will be poor. Therefore, if the volume ratio of the amount of additive gas introduced to the amount of methane introduced is 1.1% or more from the beginning of the CVD single-crystalline diamond layer deposition process, the concentration of the additive gas does not need to be increased midway. Naturally, even if the volume ratio is within this range, the concentration of the additive gas may be increased midway.

[0074] Furthermore, when the CVD single crystalline diamond layer deposition step is started in an atmosphere to which no additive gas is added, the additive gas may be introduced only during the aforementioned time period.

[0075] In this embodiment, the additive gas may be introduced or the amount of additive gas introduced may be increased at any timing. By doing so, even if a high-quality CVD single-crystalline diamond layer 22 is deposited halfway, the crystal quality of the surface of the CVD single-crystalline diamond layer 22 will be poor, and large irregularities will cause differences in height on the surface of the CVD single-crystalline diamond layer 22. This makes it possible to suppress peeling from the base 30.

[0076] The cutting tool according to this embodiment is manufactured so that the quality of the CVD single crystalline diamond layer 22 deteriorates. For this reason, abnormal growth occurs in places on the deposition surface of the CVD single crystalline diamond layer 22. In this embodiment, even if there are places where abnormal growth occurs, it is better to form irregularities on the growth surface to suppress peeling from the base 30. However, if the places where abnormal growth occurs are left as they are, it may not be possible to stably braze to the base 30.

[0077] Therefore, the manufacturing method of the bit tool according to this embodiment may include a grinding and flattening step for grinding and flattening the deposition surface of the CVD single crystalline diamond layer 22 before the cutting edge bonding step described below. The grinding and flattening step is a step for grinding and flattening the abnormally grown portion 22-2 so that the deposition surface of the CVD single crystalline diamond layer 22 is partially parallel to the surface of the HPHT single crystalline diamond substrate 21. The grinding and flattening step allows the cutting edge 20 and the base 30 to be joined at parallel surfaces 22-4, enabling extremely strong brazing.

[0078] FIG. 6 is a schematic cross-sectional view of the cutting edge manufactured by the manufacturing method of the cutting tool according to this embodiment, showing the state before and after grinding flattening treatment so that the surface of the cutting edge is parallel to the HPHT single crystal diamond substrate of the cutting edge, FIG. 6(a) is a schematic cross-sectional view of the cutting edge before grinding flattening treatment, and FIG. 6(b) is a schematic cross-sectional view of the cutting edge after grinding flattening treatment. As shown in FIG. 6(a), the deposition surface of the CVD single crystal diamond layer 22 may have an abnormal growth portion 22-2. For this reason, in the manufacturing method of the cutting tool according to this embodiment, the grinding flattening treatment may grind the convex portion 22-2, which is the abnormal growth portion, on a parallel line 40 to the surface of the HPHT single crystal diamond substrate 21, as shown in FIG. 6, for example. The grinding flattening treatment at least partially forms a surface parallel to the surface of the HPHT single crystal diamond substrate 21.

[0079] The area of ​​such parallel faces is appropriately adjusted depending on the number, locations and growth rate of the protrusions 22-2 formed in the CVD single crystal diamond layer. In the grinding flattening step, it is sufficient to perform the minimum amount of grinding required to obtain a face parallel to the face of the HPHT single crystal diamond substrate 21.

[0080] Here, in this embodiment, "minimum grinding to obtain a surface parallel to the base" means minimum grinding to obtain a parallel surface to the extent that the cutting edge 20 does not tilt when the cutting edge 20 is placed on the base 30. That is, for example, if the convex portion 22-2 is biased toward the end of the CVD single crystalline diamond layer, it is necessary to grind all of the abnormally grown portions to prevent the cutting edge 20 from tilting when placed on the base 30.

[0081] However, the protrusions 22-2 are often present over the entire surface of the CVD single crystalline diamond layer. Therefore, as shown in Fig. 6(b), by grinding the vicinity of the apex of the protrusions 22-2, the cutting edge 20 will not tilt when placed on the base 30, and the cutting edge 20 can be placed stably.

[0082] As a more preferable "minimum grinding to obtain a surface parallel to the base", for example, grinding may be performed so that the interval 60 of the protrusions 22-2 on the ground surface as shown in FIG. 6(b) is 1 / 2 or more of the width 70 of the CVD single crystalline diamond layer 22 as described above. By such grinding, the cutting edge 20 can be stably placed on the base 30. More preferably, the interval 60 is 3 / 5 or more of the width 70, and most preferably 7 / 10 or more. As shown in FIG. 6(b), grinding makes the tip of the protrusion 22-2 flat. In this case, the interval 60 may be measured on the flat part based on the part 22-3 near the outside of the cutting edge 20 as shown in FIG. 6(b).

[0083] As one guideline, grinding of the surface of the CVD single crystalline diamond layer 22 may be carried out so as to obtain such a gap 60. Even after the surface of the CVD single crystalline diamond layer 22 is ground, the height difference 50 of the surface of the CVD single crystalline diamond layer 22 is preferably within the above-mentioned range.

[0084] In the CVD single-crystalline diamond layer 22, the convex portions 22-2, which are abnormally grown portions, are ground away in a grinding and flattening step, so that, as shown in Figure 6(b), a surface 22-4 parallel to the surface of the HPHT single-crystalline diamond substrate 21 is formed. The area of ​​the parallel surface 22-4 is preferably 30 to 95% of the area of ​​the HPHT single-crystalline diamond substrate.

[0085] Furthermore, when the CVD single-crystalline diamond layer deposition step is carried out as described above, the cutting edge may be covered with polycrystalline CVD diamond and / or diamond-like carbon (hereinafter, appropriately referred to as "DLC"). A step of removing this DLC by grinding may be carried out before the cutting edge bonding step described below.

[0086] The grinding in the flattening step and the DLC removal step may be performed by a general grinding machine. The grinding conditions are not particularly limited.

[0087] (2) Blade tip bonding process Finally, as shown in Fig. 4(c), the manufacturing method according to the present invention includes a cutting edge bonding step of bonding the cutting edge 20, formed by depositing a CVD single crystalline diamond layer 22 on an HPHT single crystalline diamond substrate 21 in a CVD single crystalline diamond layer deposition step, to a base 30 by brazing. In the cutting edge bonding step, the cutting edge 20 and the base 30 are bonded by brazing so that the CVD single crystalline diamond layer 22 of the cutting edge 20 and the base 30 face each other.

[0088] As the brazing material 23 used for brazing, general brazing materials such as silver brazing, copper brazing, etc. Also, as long as the temperature of the bit tool does not become high during use or during the grinding process of the cutting edge 20 described later, a high-temperature solder having a higher melting point than the temperature during use or the grinding process may be used.

[0089] Furthermore, brazing may be performed while applying ultrasonic waves in order to improve the adhesive strength of the cutting edge 20. By applying ultrasonic waves, the wettability between the brazing material 23 and the cutting edge 20 is improved, thereby further improving the adhesive strength.

[0090] The details of the blade tip bonding process are as follows. First, the brazing material 23 is placed on the base 30 at the location where the blade tip 20 is to be bonded. Alternatively, the brazing material 23 is bonded in advance to a predetermined position, and then the blade tip 20, which is formed by growing the CVD single crystal diamond layer 22 on the HPHT single crystal diamond substrate 21, is placed on the base 30 at the position where the brazing material 23 is placed, or at the position where the brazing material 23 is to be bonded. The blade tip 20 is placed on the base 30 so that the CVD single crystal diamond layer 22 of the blade tip 20 faces the base 30 (mounting process). After that, the brazing material 23 is melted at a temperature about 20 to 30° C. higher than the melting point of the brazing material 23, and cooled to bond the blade tip 20 and the base 30. EXAMPLES

[0091] The present embodiment will be described with reference to the following examples. The present invention is not limited to the following examples. Examples 1 to 3 will be described in detail below, but Examples 4 to 16 are the same as Examples 1 to 3 except for the CVD conditions, and therefore will not be described.

[0092] Example 1 First, a Ib-type HPHT single crystal diamond substrate (manufactured by Element Chic, model number: MXP L3010) with a size of 3 mm and a thickness of 1.0 mm was prepared. The color was fancy yellow. CVD single crystal diamond was deposited on this substrate using a microwave plasma CVD apparatus. Hydrogen and methane were used as the main gases, and nitrogen was used as the additive gas. The hydrogen introduction amount was 100 parts by volume, and the methane introduction amount: nitrogen introduction amount = 5.0 parts by volume: 0.10 parts by volume were introduced into the apparatus. The CVD single crystal diamond layer was deposited for 45 hours under deposition conditions of a temperature of 1000°C and a pressure of 100 torr, and a CVD single crystal diamond layer with a film thickness of 0.5 mm was deposited. The "volume ratio (%) of methane to additive gas," which is the ratio (%) obtained by dividing the amount of additive gas introduction by the amount of methane introduction and multiplying it by 100, was 2.00%.

[0093] After deposition, the periphery of the cutting edge was covered with DLC with large irregularities, so the DLC was removed by grinding in the same manner as in the past. In other words, in Example 1, after forming the CVD single-crystalline diamond layer, as shown in Figure 6, no abnormal growth was observed, so a surface parallel to the surface of the HPHT single-crystalline diamond substrate was obtained without performing a grinding flattening process on the growth surface. The area of ​​this surface was 95% of the area of ​​the HPHT single-crystalline diamond substrate. In addition, when the cross section of the cutting edge of Example 1 was observed with an optical microscope, the height difference 50 shown in Figure 6 was 0.05 mm.

[0094] The color of the deposited CVD single crystal diamond layer was visually confirmed to be “fancy yellow” in terms of GIA grade, which is the same yellow color as the Ib type HPHT single crystal diamond substrate. -1Using the Raman spectrum as a standard, the full width at half maximum (FWHM) and the peak shift were calculated from the Raman spectrum. -1 The peak shift is +0.10 cm -1 It was.

[0095] (3) Blade tip bonding process using brazing Thereafter, the CVD single crystal diamond layer and the CVD single crystal diamond layer were placed in a predetermined position on a base so as to face each other. A silver solder had been attached to a predetermined position on the base. The base on which the cutting edge was placed was then heated to 1000°C in air to melt the silver solder, and naturally cooled to room temperature. The cutting edge was then attached to the base to obtain a cutting tool.

[0096] Example 2 CVD single-crystalline diamond was deposited on a pre-prepared Ib-type HPHT single-crystalline diamond substrate (Element Chic, model number: MXP L3010) with a size of 3 mm and a thickness of 1.0 mm, using a microwave plasma CVD apparatus. Hydrogen and methane were used as the main gases, and nitrogen was used as the additive gas. The hydrogen introduction amount was 100 parts by volume, and the methane introduction amount:nitrogen introduction amount=5.0 parts by volume:0.05 parts by volume. The CVD single-crystalline diamond layer was deposited for 45 hours under deposition conditions of a temperature of 1000°C and a pressure of 100 torr. The "volume ratio (%) of methane to additive gas", which is the ratio (%) obtained by dividing the amount of additive gas introduction by the amount of methane introduction and multiplying it by 100, was 1.00%.

[0097] For the next 5 hours, deposition was continued under deposition conditions of temperature 1000°C, pressure 100 torr, and the amount of hydrogen introduced was 100 volume parts, while the amount of methane introduced: the amount of nitrogen introduced was 5.0 volume parts:0.20 volume parts, depositing a CVD single-crystalline diamond layer with a thickness of 0.6 mm. The "volume ratio (%) of methane to added gas", which is the ratio (%) obtained by dividing the amount of added gas introduced by the amount of methane introduced and multiplying it by 100, was 4.00%.

[0098] After deposition, the periphery of the cutting edge was covered with DLC with large irregularities, so the DLC was removed by grinding in the same manner as in the past. That is, in Example 2, after forming the CVD single-crystalline diamond layer 22, as shown in Figure 6, a process of grinding and flattening the abnormally grown areas was carried out. By this process, the area of ​​the surface parallel to the surface of the HPHT single-crystalline diamond substrate 21 was 95% of the area of ​​the HPHT single-crystalline diamond substrate 21. Furthermore, when the cross section of the cutting edge of Example 2 was observed with an optical microscope, the height difference 50 shown in Figure 6 was 0.06 mm.

[0099] The color of the deposited CVD single crystal diamond layer was observed by visual inspection of the cross section, and the color of the central part of the plate thickness of the CVD single crystal diamond layer was fancy light yellow, and the color of the surface of the CVD single crystal diamond layer was fancy dark yellow. -1 Using the Raman spectrum as a standard, the full width at half maximum (FWHM) of the peak and the peak shift were calculated. -1 The peak shift is +0.15 cm -1 It was.

[0100] Figure 7 is an optical microscope photograph of the cutting edge of the cutting tool according to this embodiment, where Figure 7(a) is the HPHT single crystal diamond substrate before the CVD single crystal diamond layer is deposited in Example 2, and Figure 7(b) is the CVD single crystal diamond layer deposited on the HPHT single crystal diamond substrate in Example 2. It can be seen that the CVD single crystal diamond layer in Figure 7(b) is a darker color (yellow) compared to the color of the HPHT single crystal diamond substrate in Figure 7(a). The actual color is as described above.

[0101] (3) Blade tip bonding process using brazing Then, the HPHT single crystal diamond substrate on which the CVD single crystal diamond layer was laminated was machined into a predetermined shape, and the obtained cutting edge was placed at a predetermined position on a base so that the CVD single crystal diamond layer faced the base. A silver solder had been attached to a predetermined position on the base. The base on which the cutting edge was placed was then heated to 1000°C in air to melt the silver solder, and naturally cooled to room temperature, and the cutting edge was attached to the base to obtain a cutting tool.

[0102] 2. Example 3 A microwave plasma CVD apparatus was used for the same HPHT single crystal diamond substrate as in Example 2. Hydrogen and methane were used as main gases, and nitrogen was used as additive gas. The hydrogen introduction amount was 100 parts by volume, and methane introduction amount: nitrogen introduction amount = 5.0 parts by volume: 0.10 parts by volume. Deposition was performed for 40 hours under deposition conditions of a temperature of 1000°C and a pressure of 100 torr. The "volume ratio (%) of methane to additive gas", which is the ratio (%) obtained by dividing the amount of additive gas introduction by the amount of methane introduction and multiplying it by 100, was 2.00%.

[0103] For the next three hours, deposition was continued under deposition conditions of a temperature of 1000°C and a pressure of 100 torr, with the amount of methane introduced: the amount of nitrogen introduced being 5.0 parts by volume:0.50 parts by volume, resulting in the deposition of a CVD single-crystalline diamond layer with a thickness of 0.7 mm. The "volume ratio (%) of methane to added gas", which is the ratio (%) obtained by dividing the amount of added gas introduced by the amount of methane introduced and multiplying it by 100, was 10.00%.

[0104] In Example 3, as in Example 2, the edge was covered with DLC with large irregularities after deposition, so the DLC was removed by grinding in the same manner as in the past. That is, after forming the CVD single-crystalline diamond layer 22, Example 3 also underwent a process of grinding and flattening the abnormally grown areas as shown in Figure 6. As a result of this process, the area of ​​the surface parallel to the surface of the HPHT single-crystalline diamond substrate 21 was 50% of the area of ​​the HPHT single-crystalline diamond substrate 21. When the cross section of the edge of Example 3 was observed with an optical microscope, the height difference 50 shown in Figure 6 was 0.20 mm.

[0105] The color of the deposited CVD single crystal diamond layer was visually inspected on the cross section, and the color of the central part of the plate thickness of the CVD single crystal diamond layer was fancy yellow, and the color of the surface of the CVD single crystal diamond layer was fancy deep yellow. -1 Using the Raman spectrum as a standard, the full width at half maximum (FWHM) and the peak shift were calculated from the Raman spectrum. -1 The peak shift is +0.18 cm -1 It was.

[0106] In Examples 4 to 17, a CVD single crystal diamond layer 22 was deposited on an HPHT single crystal diamond substrate under the conditions shown in Table 1 below. Other conditions were the same as in Example 2, and cutting tools were manufactured using the same method. The colors of the CVD single crystal diamond are as shown in Table 1. Also, in these Examples, the FWHM, which is the peak half-width obtained from the Raman spectrum of the CVD single crystal diamond layer 22, was 1.0 to 5.0 cm. -1 The peak shift amount of the CVD single crystal diamond layer 22 was −1.0 to +1.0 cm -1 It was.

[0107] In Examples 4 to 17, after forming the CVD single crystal diamond layer 22, the abnormally grown portions were ground and flattened as shown in Fig. 6. As a result of this process, the area of ​​the surface parallel to the surface of the HPHT single crystal diamond substrate 21 was 50 to 95% of the area of ​​the HPHT single crystal diamond substrate. Furthermore, when the cross section of the cutting edge was observed with an optical microscope, the height difference 50 shown in Fig. 6 was 0.05 to 0.20 mm.

[0108] 5. Comparative Example 1 A cutting edge obtained under conditions in which the deposition conditions of the CVD single crystal diamond layer 22 in Example 1 were changed to those of Comparative Example 1 in Table 1 was placed at a predetermined position on a base so that the HPHT single crystal diamond substrate faced the base, and a bit tool was manufactured in the same manner as in Example 1.

[0109] 6. Comparative Example 2 A cutting tool was manufactured in the same manner as in Example 1, except that the CVD single crystal diamond layer was separated by laser cutting from the cutting edge obtained under the same deposition conditions as in Comparative Example 1, and the surface of the separated CVD single crystal diamond layer opposite to the separated surface was joined to a base. Examples and comparative examples including those mentioned above are as shown in Table 1 below.

[0110] 7. Evaluation The cutting tools of Examples 1 to 17 and Comparative Examples 1 and 2 obtained as described above were evaluated for (1) the height difference of the growth surface of the CVD single crystal diamond layer, (2) the presence or absence of peeling of the cutting edge, and (3) the substrate processing accuracy.

[0111] (1) Height difference on the growth surface of the CVD single crystal diamond layer The cross section of the cutting edge manufactured as described above was observed with an optical microscope, and the height difference was measured by depth measurement. The height difference was the difference between the lowest point and the highest point after grinding and flattening. If the height difference was less than 0.05 mm, it was evaluated as "poor", if the height difference was more than 0.05 mm and 0.1 mm or less, it was evaluated as "good", and if it was more than 0.1 mm, it was evaluated as "best".

[0112] (2) Presence or absence of peeling on the cutting edge After the above processing, it was visually confirmed whether the cutting edge had peeled off from the base. If no peeling of the cutting edge was observed, it was rated as "good", and if the cutting edge was peeled off, it was rated as "poor".

[0113] (3) Circuit board processing accuracy The Cu electrode on the Si substrate was ground using the cutting tool manufactured as described above. The ground surface was observed under an optical microscope, and if there were no lines, it was evaluated as "good", and if lines were observed, it was evaluated as "bad". The evaluation results are shown in Table 1.

[0114] [Table 1]

[0115] As is clear from Table 1, all of the present examples were rated "best" or "good." On the other hand, in Comparative Example 1, since the HPHT single crystal diamond substrate and the base were bonded, the unevenness of the cutting edge was small and the cutting edge peeled off from the base. In Comparative Example 2, since the CVD single crystal diamond layer was bonded to the base, no peeling of the cutting edge was observed, but the processing accuracy was poor.

[0116] The cutting edge produced in this embodiment will be described using a photograph. Figure 8 is a photograph of the cutting edge of Example 2, which is deposited under the deposition conditions of the CVD single-crystalline diamond layer 22, with the amount of nitrogen introduced increased from 0.05 to 0.20 volume parts when the amount of hydrogen introduced is 100 volume parts, for the last 5 hours of the total deposition time, Figure 8(a) is an optical microscope photograph of the cutting edge, and Figure 8(b) is an SEM photograph of the cutting edge after grinding and flattening. Figure 9 is a photograph of the cutting edge of Example 3, which is deposited under the deposition conditions of the CVD single-crystalline diamond layer 22, with the amount of nitrogen introduced increased from 0.10 to 0.50 volume parts when the amount of hydrogen introduced is 100 volume parts, for the last 3 hours of the total deposition time, Figure 9(a) is an optical microscope photograph of the cutting edge, and Figure 9(b) is an SEM photograph of the cutting edge after grinding and flattening. Note that both Figure 8 and Figure 9 are photographs taken from the CVD single-crystalline diamond layer 22 side.

[0117] As shown in Example 2 in Fig. 8, when the amount of nitrogen introduced during the 5 hours from the end of the deposition time (the last 10% of the process time of the CVD single crystal diamond layer deposition process, which is the second stage in Table 1) is increased from 0.05 volume parts in the first stage to 0.2 volume parts in the second stage, four times the amount of hydrogen introduced, assuming that the amount of hydrogen introduced is 100 volume parts, an in-plane height difference was formed on the surface of the CVD single crystal diamond layer 22. Also, in Example 2, as shown in Fig. 8(b), in order to obtain a surface 22-4 parallel to the HPHT single crystal diamond substrate 21 in the CVD single crystal diamond layer 22, a grinding flattening process was performed on 95% of the area of ​​the CVD single crystal diamond layer 22. The height difference in Example 2 was 0.60 mm.

[0118] As shown in FIG. 9, in Example 3, when the amount of nitrogen introduced during the 3 hours from the end of the deposition time (a time period of about 7% of the process time of the CVD single-crystalline diamond layer deposition process) is increased by 5 times from 0.10 to 0.50 volume parts when the amount of hydrogen introduced is 100 volume parts, it was found that the in-plane height difference of the upper surface of the cutting edge 20 increases. In Example 2, in order to obtain a parallel surface with the HPHT single-crystalline diamond substrate 21 in the CVD single-crystalline diamond layer 22, it was necessary to perform grinding and flattening treatment over a range of 95% of the area of ​​the CVD single-crystalline diamond layer. In Example 3, as shown in FIG. 9(b), in order to obtain a parallel surface 22-4 with the HPHT single-crystalline diamond substrate 21 in the CVD single-crystalline diamond layer 22, grinding and flattening treatment was performed over a region of 50% of the area of ​​the CVD single-crystalline diamond layer. In addition, the height difference after the grinding and flattening treatment was 0.20 mm. [Explanation of symbols]

[0119] 1 Tool 10 Cutting edge 20 Cutting Edge 21 HPHT single crystal diamond substrate 22 CVD single crystal diamond layer 22-1 Recess 22-2 Convex part (abnormal growth area) 22-3 The outer part of the cutting edge 22-4 (HPHT single crystal diamond substrate) Parallel surface 23 Brazing material 30 Foundations 301 Mounting part 302 Tip attachment part 34 Shank 40 Parallel line (to HPHT single crystal diamond substrate) 50 height difference [Industrial Applicability]

[0120] The cutting tool according to the present invention is widely used in super-finishing grinding of metals, such as aluminum, and is particularly suitable for planarizing grinding of composite semiconductor substrates for electrodes constituting TSVs (Through-Silicon Vias), which are through-silicon electrodes.

Claims

1. A tool having a base and a cutting edge brazed to the base, The cutting edge is a HPHT single crystal diamond substrate; a CVD single crystal diamond layer deposited on the HPHT single crystal diamond substrate, the CVD single crystal diamond layer having the same or lower crystal quality and a rougher surface compared to the HPHT single crystal diamond; The cutting edge and the base are bonded together so that the CVD single crystal diamond layer of the cutting edge faces the base. A bit tool characterized by the above.

2. 2. The bit tool according to claim 1, wherein the HPHT single crystal diamond substrate has a thickness of 0.3 to 3.0 mm.

3. 3. The cutting tool according to claim 1, wherein the CVD single crystal diamond layer has a thickness of 0.1 to 2.0 mm.

4. 3. The tool according to claim 1, wherein the CVD single crystal diamond layer is transparent or yellow in colour.

5. The tool according to claim 3 , wherein the CVD single crystal diamond layer is transparent or yellow in colour.

6. 3. The cutting tool according to claim 1, wherein a near-surface region of the CVD single-crystalline diamond layer exhibits a colour different from a region other than the near-surface region of the CVD single-crystalline diamond layer.

7. 4. The cutting tool according to claim 3, wherein a near-surface region of the CVD single crystal diamond layer exhibits a colour different from a region other than the near-surface region of the CVD single crystal diamond layer.

8. 5. The cutting tool according to claim 4, wherein a near-surface region of the CVD single crystal diamond layer exhibits a colour different from a region other than the near-surface region of the CVD single crystal diamond layer.

9. 6. The cutting tool according to claim 5, wherein a near-surface region of the CVD single crystal diamond layer exhibits a colour different from a region other than the near-surface region of the CVD single crystal diamond layer.

10. A manufacturing method of a cutting tool including a base and a cutting edge brazed to the base, a CVD single crystal diamond layer deposition step of depositing a CVD single crystal diamond layer on a pre-prepared HPHT single crystal diamond substrate by a CVD method in an atmosphere gas containing an additive gas composed of at least one of oxygen, nitrogen, and / or an oxide of nitrogen; a cutting edge bonding step of bonding the cutting edge formed by depositing the CVD single crystal diamond layer on the HPHT single crystal diamond substrate by the CVD single crystal diamond layer depositing step to the base by brazing so that the CVD single crystal diamond layer faces the base; A manufacturing method of a bit tool comprising:

11. The method of manufacturing a bit tool according to claim 10, wherein, during a time period from the last 20 to 0.5% of the process time of the CVD single-crystalline diamond layer deposition step onwards, the amount of added gas introduced is increased to 2 to 200 times the amount of added gas introduced during a time period other than the last 20 to 0.5% of the process time.

12. The method for manufacturing a cutting tool according to claim 10, wherein the additive gas is introduced only during a time period from the last 20% to 0.5% or later of the process time of the CVD single-crystalline diamond layer deposition process.

13. The method for manufacturing a bit tool according to any one of claims 10 to 12, further comprising a grinding and flattening step of grinding and flattening a deposition surface of the CVD single-crystalline diamond layer deposited in the CVD single-crystalline diamond layer deposition step so that the deposition surface is at least partially parallel to a surface of the HPHT single-crystalline diamond substrate.

Citation Information

Patent Citations

  • Diamond cutting tool and manufacture thereof

    JP1993253757A

  • Tool for brazing synthetic diamond in gas phase and its production

    JP1995196379A

  • Throw-away tip and cutting tool

    JP2004291110A

  • Single crystal diamond and producing method thereof

    JP2006315942A

  • Diamond composite, diamond joint body, single crystal diamond and tool including the same

    JP2015034114A